Release sheet-provided resin film

The resin film with a release sheet, incorporating large-sized particles and controlled resin composition, addresses the issues of repellency and quality in resin films by enhancing peeling resistance and coating quality, achieving improved releasability and handling properties.

WO2024204522A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012608
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Resin films with large-sized particles relative to their thickness face issues with repellency and quality deterioration due to pinholes and depressions, leading to poor releasability and coating quality, with existing solutions failing to effectively address these problems.

Method used

A resin film with a release sheet containing a resin composition of epoxy resin, thermoplastic resin, and large-sized particles exceeding twice the average resin thickness, with a specific particle size distribution and content, along with controlled peeling resistance and complex viscosity, to suppress expansion and improve releasability.

Benefits of technology

The solution achieves a resin film with enhanced peeling resistance, improved coating quality, and reduced repellency, ensuring good releasability and quality, while maintaining handling properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012608_03102024_PF_FP_ABST
    Figure JP2024012608_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a resin film in which, although having on one surface of a release sheet a resin containing particles having a particle size sufficiently large with respect to the thickness of the resin film, releasability from the release sheet is excellent, and expansion of repelling is inhibited, and which has good quality. This release sheet-provided resin film has, on one surface of a release sheet, a resin composition containing components [A]-[D], contains 10-30 mass% of particles of [D] in the resin composition, and has the following property (I). [A] An epoxy resin. [B] A thermoplastic resin. [C] A curing agent. [D] Particles including large-particle-size particles having a particle size exceeding 2A with respect to the average resin thickness A of the resin film. [I] The release resistance [X] (mN / 20 mm) of the surface of the release sheet coated with the resin in the release sheet and the complex viscosity [Y] (MPa·S) of the resin composition at 25°C exist in a region satisfying formulas (1)-1 to (1)-4.
Need to check novelty before this filing date? Find Prior Art

Description

Resin film with release sheet

[0001] The present invention relates to a resin film with a release sheet containing large particles.

[0002] Resin films with release sheets (hereinafter referred to as "resin films") obtained by thinly spreading resin have traditionally been widely used in electronic components, automobiles, adhesives, pharmaceutical components, and the like, taking advantage of their ease of handling and processability. In recent years, as components have become smaller, thinner, and lighter, thinner resin films have also been required. However, during resin film molding, there have been issues with the formation of pinholes, which are very small holes, on the resin-coated surface, and with the occurrence of repellency, a phenomenon in which resin particles on the surface repel each other, creating holes or depressions, resulting in a deterioration in the quality of the resin film. Patent Document 1 describes an adhesive film for semiconductors and proposes specifying the surface energy of the substrate to which the resin is coated in order to provide a resin film that combines good thin-film coating properties and easy peelability and suppresses pinholes and repellency. While specifying the film thickness to be 10 μm or less, it also describes the use of a particulate filler, with a maximum particle diameter of 25 μm or less.

[0003] Furthermore, in recent years, as products have become increasingly multifunctional, competition to differentiate products through new functions and added value has intensified, making it a new important issue to impart functionality to the resin film itself.

[0004] Various technologies have been proposed to solve the above problems. Broadly speaking, there are methods that process the surface of a resin film, such as sputtering or surface treatment, and methods that add functional fillers to the resin itself. The latter, in particular, allows for different functionalities to be obtained depending on the type and size of the filler applied, making it possible to add a wide range of functions to the resin film.

[0005] Furthermore, when a filler is present in a resin film, particularly if the filler contains volatile components, voids are likely to occur, resulting in swelling and peeling, making it difficult to coat the resin uniformly and with high quality. Furthermore, when the filler is particulate, fillers with a particle size smaller than the resin thickness are generally blended. However, when resin films are laminated for the purpose of imparting functionality such as thermal conductivity, particulate fillers with a particle size larger than the resin thickness may also be blended. The blending of such particulate fillers with a large particle size can easily cause pinholes and repellency originating from the filler when or after the resin is placed on a release sheet, resulting in a deterioration in the quality of the resin film. Patent Document 2 proposes specifying the B / C ratio (the ratio of the B roll (coating roll) speed to the C roll (back roll) speed) using a reverse roll coater method in order to provide a high-quality resin film containing coarse particles with a particle size larger than the resin thickness.

[0006] JP 2012-162680 A JP 2016-160367 A

[0007] If a resin containing particles with a particle size larger than the thickness of the resin is used as the particles to be incorporated into the resin film, not only does the aforementioned repelling occur when the resin is placed on one side of a release sheet, but the repelling also increases over time, tending to deteriorate the quality of the resin film. Therefore, it is necessary to increase the viscosity of the resin to reduce its fluidity or to change the surface properties of the release sheet to make it easier to retain the resin. However, increasing the viscosity of the resin to make it easier to retain on the release sheet results in poor releasability of the resin from the release sheet. The invention described in Patent Document 1 achieves both good thin-film coatability and releasability from the substrate, and while it describes the use of a particulate filler with a maximum diameter exceeding twice the film thickness, it considers a composition containing particles with a maximum diameter within twice the film thickness to be a more preferred embodiment, and does not address or address the specific issues that arise when particles with a particle size sufficiently large relative to the film thickness are used. Patent Document 2 discloses the use of particles containing coarse particles exceeding 2A μm for a resin thickness of A μm in the resin film. However, Patent Document 2 does not describe or suggest the problem of the above-mentioned repellency that may occur due to coarse particles. Furthermore, Patent Document 2 teaches that in a composition that can produce a high-quality resin film, the amount of particles containing coarse particles used is small, and the content of the coarse particles is 2 mass% or less for one of the two types of particles used, and while it teaches to avoid a composition with a sufficiently high content of coarse particles, it does not disclose any technology necessary to obtain a high-quality resin film using a resin that contains coarse particles in excess of the above amount in the composition.

[0008] In other words, it cannot be said that the prior art documents recognized the problem of repellency, which occurs specifically when a resin film contains particles with a particle size larger than the thickness of the resin film, and they did not specifically disclose a method for suppressing this problem. As a result, it was difficult to obtain a resin film that suppresses the expansion of repellency, has good quality, and has good releasability from the release sheet.

[0009] In view of the above circumstances, the problem to be solved by the present invention is to provide a resin film that has good quality and exhibits good releasability from a release sheet, with the expansion of repellency suppressed, even though a resin containing particles with a particle size sufficiently large relative to the thickness of the resin film is placed on one side of the release sheet.

[0010] The present invention, which solves the above-mentioned problems, has the following configuration. Here, in the present invention, particles having a particle size more than twice the average resin thickness A of the resin composition arranged on one side of the release sheet, i.e., particles having a particle size exceeding 2A (2×A), are referred to as large-particle-size particles. 1. A resin film with a release sheet, in which a resin composition containing the following components [A] to [D] is arranged on one side of the release sheet, wherein the particles of [D] are contained in the resin composition at 10 to 30 mass %, and the resin film has the following property (I): [A] epoxy resin [B] thermoplastic resin [C] curing agent [D] particles containing large-particle-size particles having a particle size exceeding 2A with respect to the average resin thickness A of the resin film. (I) The peel resistance [X] (mN / 20 mm) of the surface of the release sheet to which the resin is applied and the complex viscosity [Y] (MPa s) of the resin composition at 25°C are in a range satisfying the following formulas (1)-1 to (1)-4.

[0011]

[0012] 2. The resin film with a release sheet according to the above 1, wherein the particles [D] have a particle size distribution in which the content of the large-diameter particles is 10 to 30% of the total amount of particles [D] on a number basis. 3. The resin film with a release sheet according to the above 1 or 2, wherein the particles [D] are inorganic particles. 4. The resin film with a release sheet according to any one of the above 1 to 3, wherein the shape of the particles [D] is spherical. 5. The resin film with a release sheet according to any one of the above 1 to 4, wherein the average resin thickness A of the resin film is 50 μm or less. 6. The resin film with a release sheet according to any one of the above 1 to 5, which has the following property (II) and property (III): (II) The resin coverage of the resin film with a release sheet immediately after coating is 95% or more, and the magnification ratio of the repellency on the resin film with a release sheet, as expressed by the following formula (2), is 6 times or less.

[0013]

[0014] (III) The peeling rate of the resin composition from the release sheet is 95% or more.

[0015] According to the present invention, a resin film with a release sheet can be obtained in which a resin containing a predetermined amount of large-diameter particles having an average resin thickness A exceeding 2A is disposed on one side of a release sheet, and the resin film has good quality with suppressed expansion of repellency and good releasability from the release sheet.

[0016] The epoxy resin [A] used in the resin film with a release sheet of the present invention is not particularly limited and may be liquid or solid. Examples thereof include amine-type epoxy resins, bisphenol-type epoxy resins, phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, resorcinol-type epoxy resins, phenol aralkyl-type epoxy resins, naphthol-type epoxy resins, dicyclopentadiene-type epoxy resins, epoxy resins having a biphenyl skeleton, isocyanate-modified epoxy resins, tetraphenylethane-type epoxy resins, and triphenylmethane-type epoxy resins.

[0017] Among these, it is preferable to use amine-type epoxy resins and bisphenol-type epoxy resins, which have an excellent balance between heat resistance and adhesiveness. These epoxy resins may be self-curing when heated, or may contain a curing agent, a curing accelerator, or the like.

[0018] As the amine-type epoxy resin, a trifunctional or tetrafunctional amine-type epoxy resin is preferably used, and examples thereof include tetraglycidyldiaminodiphenylmethane, triglycidylaminophenol, triglycidylaminocresol, tetraglycidylxylylenediamine, halogen- or alkinol-substituted products thereof, and hydrogenated products thereof.

[0019] These epoxy resins may be used alone or in combination. The combination of a glycidylamine type epoxy resin and a bifunctional glycidyl ether type epoxy resin is particularly preferred because it has both heat resistance and moisture absorption resistance.

[0020] The bisphenol type epoxy resin is a bisphenol compound in which two phenolic hydroxyl groups are glycidylated, and examples thereof include bisphenol A type, bisphenol F type, bisphenol AD ​​type, bisphenol S type, halogen- or alkyl-substituted products, hydrogenated products, etc. Furthermore, not only monomers but also high molecular weight compounds having multiple repeating units can be suitably used.

[0021] The thermoplastic resin [B] used in the resin film with a release sheet of the present invention is not particularly limited, but when the epoxy resin [A] is in a liquid state, it dissolves in the epoxy resin during preparation of the resin composition and forms the resin composition together with the epoxy resin. Specific compounds of the thermoplastic resin [B] that are preferably used include polyethersulfone, polysulfone, polyimide, polyetherimide, polycarbonate, polyetherethersulfone, polyvinyl formal, and polymethyl methacrylate.

[0022] The curing agent [C] for the resin used in the resin film with release sheet of the present invention may be any compound having an active group capable of reacting with an epoxy group. Examples of the curing agent include aromatic amines, dicyandiamide, and dibasic acid dihydrazides, either singly or in mixtures. Of these, aromatic amines are preferred, and specific examples thereof include metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, and metaxylenediamine.

[0023] These curing agents may be used alone or in combination as appropriate. Aromatic amines are particularly preferred because they can impart heat resistance to the cured resin.

[0024] The [D] particles used in the resin film with release sheet of the present invention are large-sized particles having a particle size exceeding 2A relative to the average resin thickness A of the resin film, and the particles are at least partially insoluble in the epoxy resin composition. Hereinafter, large-sized particles having a particle size exceeding 2A relative to the average resin thickness A of the resin film may be abbreviated as [D] particles. Examples of these particles include metal particles, rubber particles, thermoplastic resin particles, inorganic particles, and any type of particle can be used. Generally, particles that are insoluble in the epoxy resin composition and can exist as particles in the cured resin are used. Examples of materials include acrylic, polyamide, polyimide, polyaramid, polyester, polycarbonate, polyphenylene sulfide, polybenzimidazole, polyetherimide, polysulfone, polyethersulfone, polyetheretherketone, polyacetylene, polyaniline, polypyrrole, polythiophene, polyisothianaphthene, polyethylenedioxythiophene, carbon, silica, titania, alumina, zirconia, tungsten trioxide, vanadium pentoxide, barium titanate, potassium titanate, and various metal fine particles. These particles may also be a combination of any two or more materials. Examples include particles in which a core of an inorganic or organic material is coated with a metal material.

[0025] In this embodiment, multiple types of particles may be used simultaneously, and a particulate filler that does not contain large-diameter particles may also be used in addition to the particles [D]. Note that the presence or absence of large-diameter particles is evaluated separately for each particle component.

[0026] The particles [D] are contained in an amount of 10 to 30% by mass relative to the total resin composition. The amount of particles contained in the resin composition is preferably 25% by mass or less. The particle shape is preferably spherical to prevent deterioration of the quality of the resin film. In the present invention, 40 particles are examined under a microscope, and particles are considered to be spherical when 90% or more of the particles have a circularity of 1.1 or less. Circularity can be determined by dividing the maximum radius of the particles by the minimum radius in accordance with JIS B 0621:1984. The particles according to the present invention include large-sized particles, but whether or not they are large-sized particles is determined by their relationship with the thickness of the resin disposed on one side of the release sheet in the resin film. Particles with a diameter exceeding 2A (unit: μm, etc.) relative to the average resin thickness A (unit: μm, etc.) are considered large-sized particles. In the present invention, the content of large particles among the [D] particles can exhibit functionality even if it is 1% or more of the total amount of [D] particles in the particle size distribution expressed on a number basis, but in order to exhibit sufficient effects, it is preferably 10% or more, and the upper limit is preferably 30% or less. The preferred upper limit of the content of large particles is more preferably 25% or less, and even more preferably 20% or less.

[0027] The content of large particles (>2A) referred to here can be determined from data on 2,000 or more particles that can be observed by magnifying the resin film 300 times and microscopically examining any position. If the content of large particles in the particles according to the present invention is less than 10% by number of the total amount of [D] particles, it may be difficult to obtain sufficient functionality from the particles when the resin film is laminated. Furthermore, if the content of large particles in the particles according to the present invention is more than 30% by number of the total amount of [D] particles, the probability of particles coming into contact with each other in the resin film may increase, which may deteriorate the quality of the resin film.

[0028] The particle size used in determining the particle size distribution, i.e., the particle size of the individual particles counted in the present invention, is the average diameter of the maximum and minimum diameters of the individual particles that can be observed by microscope, and the particle size distribution is calculated using particles with an average diameter of 1 μm or more. In addition, the density of the [D] particles is 1.0 g / cm 3 2.0g / cm or more 3 It is preferable that:

[0029] In order to obtain particles of a predetermined particle size, classification may be carried out using a dry classification device (for example, TTSP Separator (manufactured by Hosokawa Micron Corporation)) if necessary.

[0030] Furthermore, the particles used in the present invention are preferably those that can be dispersed in a resin by a normal mixing operation.

[0031] In addition to the above components, the resin composition used in the resin film of the present invention may contain one or more liquid thermosetting resins other than epoxy resins, curing accelerators, flame retardants, and silane coupling agents as needed.

[0032] Next, characteristic (I) will be described. The relationship between the peel resistance [X] of the surface on which the resin is disposed in the release sheet according to the present invention and the complex viscosity [Y] of the resin composition at 25°C exists in a region that satisfies the following formulas (1)-1 to (1)-4.

[0033]

[0034] Furthermore, it is more preferable that the relationship between the peel resistance [X] of the surface on which the resin is disposed in the release sheet according to the present invention and the complex viscosity [Y] of the resin composition at 25°C exists in a region that satisfies the following formulas (1)-1, (1)-2', (1)-3, and (1)-4'.

[0035]

[0036] The peel resistance [X] of the surface of the release sheet on which the resin is placed is a value obtained by measuring as follows. A rectangular release sheet 250 mm wide and 90 mm long is fixed to a flat surface, and an adhesive consisting of an acrylic emulsion is applied to the surface. The thickness of the applied adhesive is adjusted to 125 μm in a wet state immediately after application. Immediately after application, the adhesive is baked and dried by heating at 100°C for 120 seconds. Next, a PET film is applied to the adhesive-coated surface of the dried release sheet. This application is performed, for example, by moving a 7.5 kg rubber roller back and forth once, utilizing the weight of the rubber roller. Next, the sheet is heated at 23°C and 50% RH. After leaving it for 30 minutes under the atmosphere of , a test piece of 20 mm in width and 250 mm in length was cut out, and the test piece was subjected to 180° peel peeling in accordance with the method specified in JIS Z 0237:2009 "Test methods for adhesive tapes and adhesive sheets", except that the peeling speed was changed to 1000 mm / min, and the simple average value of the force at this time was taken as the peel resistance.

[0037] The complex viscosity [Y] of the resin composition at 25°C refers to the complex viscosity at 25°C read from the viscoelastic curve obtained by measuring using a dynamic viscoelasticity measuring device (e.g., ARES-G2 manufactured by TA Instruments) with parallel plates, simply raising the temperature from 10°C at a rate of 2°C / min, at a frequency of 77.25 Hz, and with a plate spacing of 0.5 mm. Each of the formulas (1) is obtained from a semi-logarithmic Y-axis graph, with peel resistance [X] on the X-axis and complex viscosity [Y] on the Y-axis, with the Y-axis being a logarithmic scale. In formulas (1)-2, (1)-2', (1)-4, and (1)-4', the coefficient in the exponent part of the exponential function e represents the slope of the semi-logarithmic Y-axis graph represented by the above formula. The coefficient in the exponent part of such an exponential function e may be expressed as follows, using E, which represents a power of 10: For example, "-7E-04" indicates -0.0007, and represents the slope of the Y-axis semi-logarithmic graph expressed by the above formula.

[0038] As described above, the resin composition used in the present invention contains particles [D] as an essential component, and it is preferable that, in the particle size distribution expressed on a number basis, 75% or less of the particles have a particle size larger than the average resin thickness A of the resin disposed on one side of the release sheet. In this case, when the release sheet is turned face down, a difference in height occurs between the resin present above the particles and the resin present to the side of the particles, making them more susceptible to the expansion force of the resin composition. This makes repellent particles more likely to occur and to expand over time. To suppress the formation and expansion of repellent particles, it is preferable to increase the peel resistance [X] of the release sheet to a certain extent. A low peel resistance [X] of the release sheet is considered preferable because it is easier to peel it from the resin film. However, since large-sized particles are used in the present invention, if the peel resistance [X] is too low, the force holding the resin composition on the release sheet is reduced and the expansion force of the resin composition is increased, resulting in the formation of more repellent particles, the expansion of repellent particles over time is accelerated, and the quality of the resin film is deteriorated. Furthermore, the present invention has found that in order to suppress the expansion force of the resin composition and thereby suppress the generation and spread of repellency, it is preferable to increase the complex viscosity [Y] of the resin composition to a certain extent. Considering conventional common technical knowledge, in a composition containing particles with a large particle size, it is first thought that the occurrence of tearing between resins due to the above-mentioned difference in height can be prevented by using a resin composition with a low complex viscosity [Y]. However, the present invention has found that if the complex viscosity [Y] of the resin composition is too low, the resin composition becomes more likely to flow and the expansion force increases, making repellency more likely to occur, accelerating the spread of repellency over time and deteriorating the quality of the resin film.

[0039] Furthermore, since a higher adsorptive force of the [D] particles to the resin composition increases their affinity to the resin composition and can suppress the generation and expansion of repellency, the adsorptive force of the [D] particles is preferably 0.3 mN / m to 17.8 mN / m, more preferably 0.5 mN / m to 10 mN / m, and even more preferably 1.0 mN / m to 5 mN / m. Note that the adsorptive force is measured by applying an adhesive to the probe side of a Si cantilever of an AFM (e.g., a scanning probe microscope SPM manufactured by Bruker), attaching the particles, and leaving them to stand for 1 hour to fix them, contacting them with a sapphire substrate cleaned with ethanol, and measuring the adhesion time at 0 seconds, a loading speed of 300 nm / s, room temperature, and a humidity of 20% to 40%.

[0040] On the other hand, if the peel resistance [X] of the release sheet is increased too much, the releasability of the resin from the release sheet will be poor, and if the complex viscosity [Y] of the resin composition is increased beyond a certain value, the resin will harden, making it difficult to handle when placed on the release sheet and also poorly releasable from the release sheet. Therefore, in order to obtain an excellent resin film that achieves both quality and releasability, it is necessary to appropriately control the peel resistance [X] of the release sheet and the complex viscosity [Y] of the resin composition.

[0041] Specifically, by setting the peel resistance [X] of the release sheet to 500 mN / 20 mm or more, the expansion force of the resin composition can be suppressed and the expansion of the resin repelling can be suppressed. Furthermore, by setting the peel resistance [X] of the release sheet to 4000 mN / 20 mm or less, the releasability of the resin from the release sheet can be improved. On the other hand, specifically, by setting the complex viscosity [Y] of the resin composition at 25 °C to 0.01 MPa s or more, the expansion force of the resin composition can be suppressed and the expansion of the repelling on the resin film can be suppressed, and it is preferably 0.08 MPa s or more. Furthermore, by setting the complex viscosity [Y] to 2.1 MPa s or less, good handling properties can be maintained when placing the resin on the release sheet. From this perspective, it is more preferable to set the complex viscosity [Y] to 1 MPa s or less.

[0042] In addition to the above conditions, the balance between the peel resistance [X] of the release sheet and the complex viscosity [Y] of the resin composition at 25°C is important. For example, within the above-mentioned ranges of peel resistance [X] and complex viscosity [Y], if the peel resistance [X] is 500 mN / 20 mm and the complex viscosity [Y] is 0.01 MPa s, the release sheet cannot fully suppress the expansion force of the resin composition, causing increased repelling and deteriorating quality. On the other hand, for example, within the above-mentioned ranges of peel resistance [X] and complex viscosity [Y], if the peel resistance [X] is 4000 mN / 20 mm and the complex viscosity [Y] is 2.1 MPa s, the releasability of the resin from the release sheet will be poor. However, in a semi-logarithmic graph in which the X axis represents peel resistance [X] and the Y axis represents complex viscosity [Y], the Y axis is a logarithmic scale, and within the ranges defined by the above-mentioned ranges of peel resistance [X] and complex viscosity [Y], the range Y≧0.14e excludes the range in which both peel resistance [X] and complex viscosity [Y] are small values ​​and the range in which both peel resistance [X] and complex viscosity [Y] are large values. -7E-04X (1)-3, and Y≦3.00e -7E-04X When a combination of [X] and [Y] that satisfies both of (1)-4 is obtained, a resin film having sufficiently good quality and good peelability can be obtained. -7E-04X (1)-3, and Y≦1.40e -7E-04X It is more preferable to have a combination of [X] and [Y] that satisfies both of (1)-4.

[0043] The average resin thickness A of the resin film with release sheet of the present invention is preferably 50 μm or less. This thickness is determined by: In the state of a resin film in which the resin is coated on a release sheet, the temperature is lowered to below the glass transition point of the resin to create a glassy state; the average thickness of the resin film is determined at 10 arbitrarily selected points using a micrometer (e.g., a MDC-25MX Coolantproof Micrometer manufactured by Mitutoyo); and the difference is calculated from the average thickness of the resin film at 10 arbitrarily selected points measured on a separately measured release sheet (the resin may be removed from the resin film with release sheet). The average resin thickness A is the difference between the average thickness of the resin film measured as described above (N=10) and the average thickness of the release sheet measured previously (N=10). By setting the average resin thickness A to 50 μm or less, the resin film can be used to manufacture thin, lightweight parts, even when laminated. The lower limit of the average resin thickness A is not particularly limited, but a value of 5 μm or more is preferred. That is, the large particles contained in the particles [D] preferably have a diameter of 10 μm or more, and the maximum diameter of the large particles is preferably 120 μm or less.

[0044] The resin film with a release sheet of the present invention preferably has a property (II) in which the magnification of the repellency on the resin film with a release sheet, as shown in the following formula (2), is 95% or more immediately after coating and is 6 times or less.

[0045]

[0046] In the present invention, the resin coverage rate of a resin film with a release sheet can be determined by measuring the area of ​​the resin composition covering the release sheet in an observation range of the resin film, with the unit area being an arbitrarily selected square area of ​​10 mm x 10 mm, under microscope observation of the surface of the resin film from the resin film side at a magnification of 50 times, and calculating the ratio of this area to the unit area.

[0047] The magnification rate of repellency can be determined by observing the surface of a resin film obtained by coating a release sheet with the resin composition at a magnification of 200 times and observing one arbitrarily selected repellent area at a fixed point, and calculating the ratio of the area of ​​the repellent area immediately after coating to the area of ​​the repellent area 24 hours after coating, and can be expressed by the above formula (2). The area ratios are obtained by observing 10 arbitrarily selected repellent areas, and the average value is used as the magnification rate of repellency.

[0048] The magnification ratio of the repelling is preferably 6 times or less. If it exceeds 6 times, when the resin film with a release sheet is attached to a substrate, uncoated areas will be generated, which will become defects and the required properties will not be obtained. The magnification ratio is preferably 4 times or less, and more preferably 3 times or less.

[0049] Here, the parameter related to property (II) can also be confirmed by using the same release sheet and resin composition as the target resin film with a release sheet, applying the resin composition to the release sheet using a knife coater, and measuring by the above-mentioned method immediately after coating and 24 hours after coating.

[0050] Furthermore, the resin film with a release sheet of the present invention preferably has a characteristic (III) of 95% or more of the resin composition peeling from the release sheet. The peeling rate of the resin composition from the release sheet is measured as follows. The resin film is cut into strips 25 mm wide and 300 mm long to prepare test pieces. Next, an evaluation tape (e.g., Damlon Tape No. 3201R, manufactured by Nitto Denko Corporation) having the same shape as the cut test piece and an adhesive strength of 8.1 N / 25 mm is attached to the side of the test piece where the resin is located, by rolling a 2 kg rubber roller back and forth once. A stainless steel support is attached to the side of the test piece where the evaluation tape is attached using double-sided tape. Next, the support is attached to a tensile tester, and the evaluation tape is peeled off at a 90° angle relative to the longitudinal direction of the test piece at a tensile speed of 10,000 mm / min in an atmosphere of 25°C and 50% RH. The entire test piece after peeling is photographed, and the image is binarized to measure the area of ​​the resin composition that does not cover the release sheet. This is then divided by the area of ​​the entire test piece to determine the peel rate. The resin film with a release sheet according to the present invention preferably has a peel rate of 95%, and particularly preferably 98% or higher, as characteristic (III). If the peel rate is less than 95%, uncoated areas, which can be defects, may occur when the resin film with a release sheet is attached to a substrate and the release sheet is peeled off.

[0051] Furthermore, in the present invention, it is preferable that both of the above characteristics (II) and (III) are satisfied.

[0052] The upper and lower limits of the above-mentioned ranges can be combined in any way.

[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0054] 1. Raw Materials <[A] Epoxy Resin> Tetraglycidyldiaminodiphenylmethane, "Sumiepoxy (registered trademark)" ELM434 (manufactured by Sumitomo Chemical Co., Ltd.) Bisphenol F type liquid epoxy resin ("EPICLON (registered trademark)" 830, manufactured by DIC Corporation).

[0055] <[B] Thermoplastic resin> Polyethersulfone, "Virantage (registered trademark)" VW-10700RFP (manufactured by Solvay).

[0056] <[C] Curing Agent> 3,3'-Diaminodiphenyl sulfone [3,3'-DAS] (manufactured by Mitsui Fine Chemicals, Inc.).

[0057] <Particles> [D] Inorganic particles: Average particle size of 32 μm, median diameter on a volume basis of 40 μm, adsorptive power of 2.4 mN / m, density of 1.4 g / cm 3 Of the 40 particles examined under a microscope, 9.5% had a circularity of 1.1 or less.

[0058] <Particulate filler (not containing large particles)> Polyamide particles, "Orgasol (registered trademark) 1002D" (manufactured by Arkema Co., Ltd.), not containing particles exceeding 54 μm.

[0059] <Release Sheet> For the release sheet, silicone was used as the release agent, and the composition of the silicone, the amount of coating, and the conditions for drying and heat treatment after coating on the release paper were adjusted to use release paper with the peel resistance shown in Table 1.

[0060] 2. Evaluation Method Each evaluation was carried out with n=1 unless otherwise specified.

[0061] <Peel Resistance> A rectangular release sheet measuring 250 mm wide and 90 mm long is fixed to a flat surface, and an adhesive consisting of an acrylic emulsion is applied to the surface. The coating thickness is adjusted to 125 μm in a wet state immediately after application. Immediately after application, the adhesive is baked and dried by heating at 100°C for 120 seconds. Next, a PET film is attached to the adhesive-coated surface of the dried release sheet. This attachment is performed by moving a 7.5 kg rubber roller back and forth once, utilizing the weight of the rubber roller. Next, after leaving the sample in an atmosphere of 23°C and 50% RH for 30 minutes, a test piece measuring 20 mm wide and 250 mm long is cut out from the test piece. A 180° peel peel is performed on the test piece according to the method specified in JIS Z 0237:2009 "Test Methods for Adhesive Tapes and Adhesive Sheets," except that the peel speed is changed to 1000 mm / min. The simple average value of the force at this time is taken as the peel resistance.

[0062] <Complex Viscosity> This refers to the complex viscosity at 25°C read from a viscoelastic curve obtained by measuring using a dynamic viscoelasticity measuring device (ARES-G2: manufactured by TA Instruments) with parallel plates, simply raising the temperature from 10°C at a temperature increase rate of 2°C / min, at a frequency of 77.25 Hz, a plate spacing of 0.5 mm, and a strain of 0.17%.

[0063] <Resin Coverage of Resin Film with Release Sheet Immediately After Coating> The surface of the resin film is observed from the resin film side at a magnification of 50 times, and the area of ​​the resin composition covering the release sheet is measured in an arbitrarily selected 10 mm × 10 mm square area of ​​the resin film as a unit area, and the resin coverage rate is calculated by taking the ratio of this area to the unit area.

[0064] <Magnification ratio of repellents on a resin film with a release sheet> The surface of a resin film obtained by coating a release sheet with a resin composition was examined under a microscope at a magnification of 200 times, and one arbitrarily selected repellent area was observed at a fixed point. The ratio of the area of ​​the repellent area immediately after coating to the area of ​​the repellent area 24 hours after coating was calculated using the following formula (2). The area ratios were obtained for 10 arbitrarily selected repellents, and the average value was calculated.

[0065]

[0066] <Release Rate of Resin Composition from Release Sheet> The resin film was cut into strips 25 mm wide and 300 mm long to prepare test specimens. Next, an evaluation tape having the same shape as the cut test specimen, 25 mm wide and 300 mm long, was attached to the side of the test specimen where the resin was located by rolling a 2 kg rubber roller back and forth once. A stainless steel support was attached to the surface of the test specimen to which the evaluation tape was attached using double-sided tape. Next, the support was attached to a tensile tester, and the evaluation tape was peeled off in the longitudinal direction of the test specimen at a tensile speed of 10,000 mm / min in an atmosphere of 25°C and 50% RH. The entire test piece after peeling is photographed, and the image is binarized to measure the area of ​​the release sheet that is not covered by the resin composition. The peel rate is calculated by dividing this area by the area of ​​the entire test piece.

[0067] 3. Preparation of Resin Film with Release Sheet: Using a knife coater, the resin composition was applied to one side of a release sheet to obtain a resin film with a release sheet. The average resin thickness A was 27 μm. [D] The proportion of large particles with a particle size exceeding 2A (μm) (i.e., exceeding 54 μm) in the inorganic particles was 11.8%.

[0068] [Examples 1 to 7] Resin compositions were obtained by kneading compounds having the compositions shown in Table 1 as raw materials in a kneader. The obtained resin compositions were placed on one side of a release sheet to obtain resin films with a release sheet. The peel resistance [X] of the release sheet, the complex viscosity [Y] of the resin composition at 25°C, the resin coverage of the resin film with a release sheet immediately after coating, the expansion rate of repellency, and the peel rate of the resin composition from the release sheet were as shown in Table 1.

[0069] [Comparative Example 1] A resin film with a release sheet was obtained in the same manner as in Example 2, except that the same release sheet as in Example 4 was used and the peel resistance [X] was set relatively low as shown in Table 1. In Comparative Example 1, the complex viscosity [Y] was Y≧0.14e -7E-04X (1)-3 was not satisfied. The resin coverage rate, the expansion rate of repellency, and the peel rate of the resin composition from the release sheet were evaluated under the same conditions as in Examples 1 to 7, and the results are shown in Table 1.

[0070] [Comparative Example 2] A resin film with a release sheet was obtained in the same manner as in Example 3, except that the same release sheet as in Example 4 was used and the peel resistance [X] was set relatively low as shown in Table 1. In Comparative Example 2, the complex viscosity [Y] was Y≧0.14e -7E-04X (1)-3 was not satisfied. The resin coverage rate, the expansion rate of repellency, and the peel rate of the resin composition from the release sheet were evaluated under the same conditions as in Examples 1 to 7, and the results are shown in Table 1.

[0071] [Comparative Example 3] A resin film with a release sheet was obtained in the same manner as in Example 7, except that the same release sheet as in Example 7 was used and the number of parts by mass of the thermoplastic resin [B] was set low as shown in Table 1. In Comparative Example 3, the complex viscosity [Y] was Y≧0.14e -7E-04X (1)-3 was not satisfied. The resin coverage rate, the expansion rate of repellency, and the peel rate of the resin composition from the release sheet were evaluated under the same conditions as in Examples 1 to 7, and the results are shown in Table 1.

[0072]

[0073] The present invention is suitably used for parts that require thermal conductivity and are obtained by laminating resin films, but the scope of application is not limited to these.

Claims

1. A resin film with a release sheet, in which a resin composition containing the following components [A] to [D] is disposed on one side of the release sheet, the particles of [D] are contained in the resin composition at 10 to 30% by mass, and the resin film has the following characteristic (I): [A] epoxy resin, [B] thermoplastic resin, [C] hardener, [D] particles containing large particles having a particle size exceeding 2A with respect to the average resin thickness A of the resin film (I) The peel resistance [X] (mN / 20 mm) of the surface of the release sheet on which the resin is applied and the complex viscosity [Y] (MPa s) of the resin composition at 25°C are in a range that satisfies the following formulas (1)-1 to (1)-4.

2. The resin film with release sheet according to claim 1, wherein the content of the large particles in the particles [D] is 10 to 30% of the total amount of the particles [D] on a number basis.

3. The resin film with a release sheet according to claim 1 or 2, wherein the particles [D] are inorganic particles.

4. A resin film with a release sheet according to claim 1 or 2, wherein the particles [D] have a spherical shape.

5. The resin film with a release sheet according to claim 1 or 2, wherein the average resin thickness A of the resin film is 50 μm or less.

6. The resin film with a release sheet according to claim 1 or 2, which has the following characteristics (II) and (III): (II) The resin coverage of the resin film with a release sheet immediately after coating is 95% or more, and the magnification of the repellency on the resin film with a release sheet, as shown in the following formula (2), is 6 times or less. (III) The peeling rate of the resin composition from the release sheet is 95% or more.

7. The resin film with a release sheet according to claim 3, which has the following characteristics (II) and (III): (II) The resin coverage of the resin film with a release sheet immediately after coating is 95% or more, and the magnification of the repellency on the resin film with a release sheet, as shown in the following formula (2), is 6 times or less. (III) The peeling rate of the resin composition from the release sheet is 95% or more.

Citation Information

Patent Citations

  • Adhesive film for semiconductor, adhesive sheet, semiconductor wafer, and semiconductor device

    JP2012162680A

  • Resin film and method for producing the same

    JP2016160367A

  • Insulating sheet, method of manufacturing the same, and rotary electric machine

    JP2022083529A

  • Prepreg and production method therefor