Composition, reactive diluent, curable composition, and method for producing composition
The composition with a specific diglycidyl ether and controlled chlorine content addresses impurity reduction and performance maintenance in epoxy resin curable compositions for electronic materials, achieving enhanced insulation reliability and heat resistance for electronic applications.
Patent Information
- Application Number
- PCT/JP2024/012686
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Curable compositions containing epoxy resins for electronic material applications face challenges in reducing impurity content, particularly chlorine, to prevent electrical short circuits and improve insulation reliability, while maintaining performance and viscosity adjustment.
A composition with a specific diglycidyl ether, represented by a specific formula, is developed, which has a total chlorine content of 900 ppm or less, using a method involving the reaction of an alkanediol with epichlorohydrin and subsequent purification with solid sodium hydroxide and water to adjust reaction temperature and chlorine levels, incorporating a branched alkylene group for improved heat resistance and viscosity reduction.
The resulting composition exhibits excellent insulation reliability, dielectric properties, and heat resistance, suitable for electronic material applications such as semiconductor encapsulants, with a balanced performance and low viscosity, effectively addressing the impurity reduction and performance maintenance issues.
Smart Images

Figure JP2024012686_03102024_PF_FP_ABST
Abstract
Description
Composition, reactive diluent, curable composition and method for producing the composition
[0001] The present invention relates to a composition, a reactive diluent, a curable composition and a method for making the composition.
[0002] BACKGROUND ART Curable compositions containing epoxy resins have excellent physical properties such as electrical insulation, heat resistance, moisture resistance, and dimensional stability, and therefore can be used in a variety of applications.
[0003] In liquid molding such as casting molding, liquid epoxy resins, typified by bisphenol A epoxy resins, can be used. However, since such liquid epoxy resins often have high viscosity, a reactive diluent for epoxy resins may be used to adjust the viscosity of the curable composition and to impart physical properties. For example, diglycidyl ether is one of the commonly used reactive diluents.
[0004] For example, Patent Document 1 discloses a short-chain aliphatic compound having a glycidyloxymethyl group at a geminal position.
[0005] Patent Document 2 discloses a diglycidyl ether represented by a specific general formula.
[0006] Patent Document 3 discloses a method for producing high-purity fatty acid glycidyl ethers with a low chlorine content, characterized in that when an alcohol is reacted with epichlorohydrin in the presence of a solid alkali metal hydroxide to produce a glycidyl ether, the reaction is carried out in the presence of pulverized solid alkali metal hydroxide in the reaction mixture.
[0007] US Patent No. 004481348 International Publication No. 98 / 39314 Japanese Unexamined Patent Publication No. Hei 1-151567
[0008] Curable compositions containing epoxy resins are widely used in electronic components such as semiconductor encapsulants, LED encapsulants, printed circuit boards, build-up boards, and resist inks, conductive adhesives such as conductive pastes and other adhesives, liquid encapsulants such as underfills, liquid crystal sealants, coverlays for flexible substrates, adhesive films for build-up, die bonding films, non-conductive films, matrices for composite materials, paints, stereolithography resins, photoresist materials, and developer materials. Among these, in electronic material applications such as semiconductors and printed wiring boards, technological innovations in these applications have led to increasing demands for higher performance encapsulants, substrate materials, and the like.
[0009] When epoxy resins are used in electronic materials, a reduction in the impurity content is required. For example, a reduction in the impurity content is also required for reactive diluents for epoxy resins used in electronic materials. Reducing the impurity content is thought to result in excellent insulation reliability, as it can avoid problems such as electrical short circuits in electronic components and migration between electronic circuit wiring. Furthermore, with regard to the diglycidyl ethers contained in reactive diluents used in electronic materials, it is required to use a suitable diglycidyl ether from the viewpoint of reducing the viscosity of the epoxy resin without impairing the performance of the epoxy resin.
[0010] The problem to be solved by the present invention is to provide a composition which contains a specific diglycidyl ether, has a reduced total chlorine content, and has excellent insulation reliability.
[0011] The present invention includes the following aspects: [1] A composition comprising a chlorine-containing compound and a diglycidyl ether represented by the following formula (1), wherein the total chlorine content is 900 ppm or less:
[0012]
[0013] (In formula (1), X represents an alkylene group having 9 to 11 carbon atoms.) [2] The composition according to [1], wherein the alkylene group in X of formula (1) is a branched alkylene group. [3] The composition according to [1] or [2], wherein the diglycidyl ether is at least one of diglycidyl ethers represented by the following formula (1-1) and the following formula (1-2):
[0014]
[0015] [4] A reactive diluent for an epoxy resin, comprising the composition according to any one of [1] to [3]. [5] A curable composition, comprising the reactive diluent according to [4]. [6] A method for producing a composition comprising a chlorine-containing compound and a diglycidyl ether represented by the following formula (1), wherein the total chlorine content of the composition is 900 ppm or less, the method comprising: a crude diglycidyl ether production step of reacting an alkanediol having 9 to 11 carbon atoms with epichlorohydrin to obtain a crude diglycidyl ether containing the diglycidyl ether represented by the following formula (1); and a purification step of purifying the obtained crude diglycidyl ether, wherein in the crude diglycidyl ether production step, solid sodium hydroxide and water are added in portions to adjust the reaction temperature and the total chlorine content.
[0016]
[0017] (In formula (1), X represents an alkylene group having 9 to 11 carbon atoms.)
[0018] According to the present invention, it is possible to provide a composition which contains a specific diglycidyl ether, has a reduced total chlorine content, and has excellent insulation reliability.
[0019] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail. The present invention is not limited to the following description, and can be practiced with various modifications within the scope of the gist. In this specification, ppm means ppm by mass.
[0020] <Composition> The composition of the present embodiment is a composition containing a chlorine-containing compound and a diglycidyl ether represented by the following formula (1), and has a total chlorine content of 900 ppm or less.
[0021]
[0022] (In formula (1), X represents an alkylene group having 9 to 11 carbon atoms.) By including the above-described structure, the composition of this embodiment has excellent insulation reliability. Furthermore, the composition of this embodiment also tends to have an excellent balance between dielectric properties, coefficient of linear thermal expansion, and heat resistance. The above properties are required when the composition of this embodiment is used as an electronic material. Examples of electronic material applications include semiconductor encapsulation materials.
[0023] <Total Chlorine Amount> The total chlorine amount refers to the chlorine content relative to the total amount of the composition. The total chlorine amount is measured by combustion microcoulometric titration (JIS K2170-2013 Appendix A). The composition of the present embodiment contains a chlorine-containing compound, and the total chlorine amount is 900 ppm or less. A total chlorine amount of 900 ppm or less results in excellent insulation reliability. From the above viewpoints, the total chlorine amount is preferably 600 ppm or less, more preferably 500 ppm or less, and even more preferably 400 ppm or less. Furthermore, for stable and low-cost production, the total chlorine amount may be more than 0 ppm, may be 1 ppm or more, or may be 10 ppm or more.
[0024] The reason why the composition of this embodiment contains a chlorine-containing compound is presumed to be as follows: When a diglycidyl ether is produced by the condensation reaction of an alkanediol with epichlorohydrin, a compound having a terminal group containing a carbon-chlorine bond in the molecule is produced as a by-product. In particular, in the case of a diglycidyl ether having a branched alkylene group with a large number of carbon atoms, the reactivity and selectivity are reduced compared to linear compounds due to the steric bulkiness around the reaction site or the influence of electron donating properties, and by-products such as compounds having a terminal group containing a carbon-chlorine bond and polymeric condensates of epichlorohydrin tend to be produced more easily. It is presumed that these chlorine-containing by-products are mixed into the composition of this embodiment.
[0025] (Diglycidyl ether represented by formula (1)) The composition of the present embodiment contains the diglycidyl ether represented by formula (1). When the diglycidyl ether represented by formula (1) is contained in a reactive diluent used in electronic material applications, it can reduce the viscosity of the epoxy resin without impairing the performance of the epoxy resin.
[0026] In the formula (1), the alkylene group X may be linear or branched. However, a branched alkylene group is preferred from the viewpoint of reducing the viscosity of the epoxy resin without impairing its performance. Generally, thermoplastic resins such as polyesters having branched alkylene groups tend to have low glass transition temperatures (Tg) and therefore poor heat resistance. For this reason, it has been thought that reactive diluents having branched alkylene groups are difficult to use in applications such as semiconductor encapsulation. In contrast, in this embodiment, the diglycidyl ether represented by formula (1), in which X is a branched alkylene group having 9 to 11 carbon atoms, has a high Tg in thermosetting resins such as epoxy resins. Therefore, the diglycidyl ether has excellent heat resistance and can be suitably used in applications such as semiconductor encapsulation that can withstand soldering during mounting of electronic components on electronic boards.
[0027] In formula (1), X represents an alkylene group having 9 to 11 carbon atoms, preferably an alkylene group having 9 to 10 carbon atoms, and more preferably an alkylene group having 9 carbon atoms.
[0028] From the viewpoint of lowering the viscosity of the epoxy resin without impairing the performance of the epoxy resin, the diglycidyl ether is preferably at least one of the diglycidyl ethers represented by the following formula (1-1) and the following formula (1-2).
[0029]
[0030] The composition of this embodiment has a concentration of the diglycidyl ether represented by formula (A), calculated by the following calculation method using values measured under the gas chromatographic analysis conditions below, of preferably 94.5% or more, and more preferably 95.0% or more. The composition of this embodiment may have a concentration of the diglycidyl ether represented by formula (A), calculated by the following calculation method using values measured under the gas chromatographic analysis conditions below, of less than 100.0%.
[0031] [Gas chromatograph analysis conditions] Analytical apparatus: 7890A Gas Chromatography System manufactured by Agilent Technologies Analytical column: HP-5 manufactured by Agilent Technologies (length 30 m × inner diameter 0.32 mm × film thickness 0.25 μm, packing: (5%-phenyl)-methylpolysiloxane) Heating conditions: After holding at 50°C for 5 minutes, heat from 50°C to 320°C at 10°C / min, and hold at 320°C for 28 minutes Sample introduction temperature: 320°C Carrier gas: nitrogen Column gas flow rate: 0.5 mL / min Detector and detection temperature: flame ionization detector (FID), 320°C Control mode: constant flow Split ratio: 50 Sample injection conditions: 1.0 μL
[0032] [Method for calculating diglycidyl ether concentration (DGE concentration)] The diglycidyl ether concentration (DGE concentration) was calculated using the following formula (A) from the total area value of diglycidyl ether peaks detected at retention times of 25.5 to 26.9 minutes under the above measurement conditions (DGE detected peak area value) and the total area value of all peaks detected at retention times of 0.0 to 60.0 minutes (total detected peak area value): DGE concentration (%) = (DGE detected peak area value / total detected peak area value) × 100 (A)
[0033] <Reactive Diluent for Epoxy Resin> The reactive diluent for epoxy resin of this embodiment includes the composition of this embodiment. The composition of this embodiment can be suitably used as a reactive diluent for epoxy resin. By using the composition of this embodiment as a reactive diluent for epoxy resin, a resin with excellent insulating reliability suitable for electronic components and the like can be obtained. The diglycidyl ether contained in the composition of this embodiment can reduce the viscosity of the epoxy resin without impairing the performance of the epoxy resin. Furthermore, by using the composition of this embodiment as a reactive diluent for epoxy resin, the obtained resin has excellent dielectric properties, coefficient of linear thermal expansion, heat resistance, and the like. The reactive diluent for epoxy resin of this embodiment may include a known reactive diluent in addition to the composition of this embodiment.
[0034] <Curable Composition> The curable composition of this embodiment contains the reactive diluent for the epoxy resin of this embodiment. The curable composition of this embodiment can be prepared, for example, by mixing a curing agent, a curing accelerator, and the like with an epoxy resin composition containing an epoxy resin and the reactive diluent for the epoxy resin of this embodiment. By including the reactive diluent for the epoxy resin containing the composition of this embodiment, the curable composition of this embodiment can obtain a resin that is suitable for electronic components and the like and has excellent insulation reliability, dielectric properties, coefficient of linear thermal expansion, heat resistance, and the like.
[0035] <Method for Producing Composition> The method for producing the composition of this embodiment is a method for producing the composition of this embodiment. The method for producing the composition of this embodiment is a method for producing a composition containing a chlorine-containing compound and a diglycidyl ether represented by the following formula (1), wherein the total chlorine content of the composition is 900 ppm or less, and the method includes a crude diglycidyl ether production step of reacting an alkanediol having 9 to 11 carbon atoms with epichlorohydrin to obtain a crude diglycidyl ether containing the diglycidyl ether represented by the following formula (1), and a purification step of purifying the obtained crude diglycidyl ether, wherein the reaction temperature and the total chlorine content are adjusted by adding solid sodium hydroxide and water in portions in the crude diglycidyl ether production step.
[0036]
[0037] (In formula (1), X represents an alkylene group having 9 to 11 carbon atoms.) In X of formula (1), the alkylene group is preferably a branched alkylene group.
[0038] (Crude diglycidyl ether production step) The crude diglycidyl ether production step is a step in which an alkanediol having 9 to 11 carbon atoms is reacted with epichlorohydrin to obtain a crude diglycidyl ether containing the diglycidyl ether represented by formula (1). In addition, in the crude diglycidyl ether production step, the reaction temperature and the total chlorine content are adjusted by adding solid sodium hydroxide and water in portions.
[0039] In the crude diglycidyl ether production step, a crude diglycidyl ether containing the diglycidyl ether represented by formula (1) may be obtained by reacting an alkanediol having 9 to 11 carbon atoms with epichlorohydrin in the presence of solid sodium hydroxide, water, and a phase transfer catalyst.
[0040] Examples of the phase transfer catalyst include quaternary ammonium salts and quaternary phosphonium salts. Examples include tetraethylammonium chloride, tetra-n-butylammonium bromide, tetrabutylammonium sulfate, and ethyltriphenylphosphonium bromide, with tetra-n-butylammonium bromide being preferred. The amount of the phase transfer catalyst used is preferably 0.5 mmol to 10.0 mmol, and more preferably 3.0 mmol to 7.0 mmol, relative to 1.0 mol of epichlorohydrin.
[0041] The amount of solid sodium hydroxide used is not particularly limited, but is preferably 1.0 mol to 12.0 mol in total, more preferably 1.5 mol to 10.0 mol, even more preferably 2.0 mol to 8.0 mol, and particularly preferably 3.0 mol to 6.0 mol, relative to 1.0 mol of the alkanediol having 9 to 11 carbon atoms.
[0042] The amount of water used is not particularly limited, but is preferably 0.5 mol to 1.0 mol in total, more preferably 0.6 mol to 0.95 mol, and even more preferably 0.7 mol to 0.90 mol, per 1.0 mol of the alkanediol having 9 to 11 carbon atoms.
[0043] In the crude diglycidyl ether production step, solid sodium hydroxide and water are added in portions to adjust the reaction temperature, hydroxide ion concentration in the reaction solution, and total chlorine content. This allows the total chlorine content in the resulting composition to be effectively suppressed. Therefore, it is easy to keep the total chlorine content in the resulting composition at 900 ppm or less. When aqueous sodium hydroxide is added instead of solid sodium hydroxide and water, it tends to be difficult to adjust the reaction temperature, hydroxide ion concentration in the reaction solution, and total chlorine content.
[0044] The number of divided additions is preferably 3 to 10 times, and more preferably 4 to 8 times, for both the number of times solid sodium hydroxide is added and the number of times water is added. The time required for all divided additions to be completed (hereinafter referred to as the "divided addition time") is preferably 1 to 5 hours, and more preferably 2 to 4 hours. By adding solid sodium hydroxide and water three or more times, the hydroxide ion concentration in the reaction solution can be appropriately suppressed and the progression of side reactions can be inhibited. By adding solid sodium hydroxide and water ten or less times, excessive addition work can be prevented. By adding the divided addition time for one hour or more, the hydroxide ion concentration in the reaction solution can be appropriately suppressed and the progression of side reactions can be inhibited. By adding the divided addition time for five hours or less, excessive addition work can be prevented. In the crude diglycidyl ether production step, it is preferable to add solid sodium hydroxide and water in multiple divided additions, for example, in amounts within the above-mentioned preferred ranges. In the divided addition, solid sodium hydroxide and water may be added simultaneously or separately. Separate addition is preferred. When solid sodium hydroxide and water are added separately in the divided addition, the order may be such that solid sodium hydroxide is added first and then water is added, or the reverse order may be used. From the viewpoint of adjusting the reaction temperature, the hydroxide ion concentration in the reaction solution, and the total amount of chlorine, the order of adding solid sodium hydroxide first and then water is preferred. More preferably, divided addition in which solid sodium hydroxide is added first and then water is added is one cycle, and this cycle is repeated. When the cycle is repeated, it is preferably repeated 3 to 10 times, and more preferably repeated 4 to 8 times.
[0045] The reaction temperature is preferably 35°C to 49°C. A reaction temperature of 35°C or higher can promote the reaction with good selectivity even in alkanediols having branched alkylene groups with a large carbon number. A reaction temperature of 49°C or lower can suppress the progression of side reactions. From the above perspective, the reaction temperature is more preferably 38°C to 48°C, and even more preferably 40°C to 47°C. By maintaining the reaction temperature within the above range, the total amount of chlorine in the resulting composition can be effectively suppressed. Furthermore, performing divided addition makes it easier to maintain the reaction temperature within the above range.
[0046] It is presumed that by adding solid sodium hydroxide and water in separate portions, it is possible to prevent the hydroxide ion concentration in the reaction solution from exceeding the predetermined level, and as a result, it is possible to control the reaction temperature below a certain level.
[0047] It is preferable to further stir the reaction solution after the divided addition of solid sodium hydroxide and water. This allows the reaction to proceed further. The stirring time is preferably 1 hour to 12 hours, more preferably 2 hours to 10 hours, and even more preferably 4 hours to 8 hours. The preferred, more preferred, and even more preferred temperatures of the reaction solution during stirring are the same as the reaction temperatures described above.
[0048] In the alkanediol having 9 to 11 carbon atoms as a raw material, the alkane is preferably a branched alkane. Examples of the alkanediol having 9 to 11 carbon atoms include 2,4-dialkyl-1,5-pentanediol and 2,2-dialkyl-1,3-propanediol. Examples of the 2,4-dialkyl-1,5-pentanediol include 2-methyl-4-propyl-1,5-pentanediol, 2-isopropyl-4-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-ethyl-4-propyl-1,5-pentanediol, 2-ethyl-4-isopropyl-1,5-pentanediol, 2,4-dipropyl-1,5-pentanediol, 2-isopropyl-4-propyl-1,5-pentanediol, and 2,4-diisopropyl-1,5-pentanediol. Of the above, 2,4-diethyl-1,5-pentanediol is preferred.
[0049] Examples of 2,2-dialkyl-1,3-propanediols include 2-methyl-2-pentyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-ethyl-2-(2-methylpropyl)-1,3-propanediol, 2,2-dipropyl-1,3-propanediol, 2-methyl-2-hexyl-1,3-propanediol, 2-ethyl-2-pentyl-1,3-propanediol, and 2-ethyl-2-(3-methylbutyl)- Examples include 1,3-propanediol, 2-propyl-2-butyl-1,3-propanediol, 2-isopropyl-2-butyl-1,3-propanediol, 2-methyl-2-heptyl-1,3-propanediol, 2-ethyl-2-hexyl-1,3-propanediol, 2-propyl-2-pentyl-1,3-propanediol, 2-isopropyl-2-(3-methylbutyl)-1,3-propanediol, and 2,2-dibutyl-1,3-propanediol. Of these, 2-butyl-2-ethyl-1,3-propanediol is preferred.
[0050] The alkanediol having 9 to 11 carbon atoms may be a commercially available product or may be produced according to a known method. Examples of commercially available products include Kyowadiol PD-9 (manufactured by KH Neochem Co., Ltd.) and Butyl Ethyl Propanediol (manufactured by KH Neochem Co., Ltd.). Examples of known methods include the method described in WO 98 / 39314.
[0051] The amount of epichlorohydrin used is preferably 1.0 mol to 12.0 mol, more preferably 1.5 mol to 10.0 mol, still more preferably 2.0 mol to 8.0 mol, and particularly preferably 3.0 mol to 6.0 mol, per 1.0 mol of the alkanediol having 9 to 11 carbon atoms.
[0052] One embodiment of the crude glycidyl ether production process is shown below in (1) to (5). (1) An alkanediol, 1.0 mol to 12.0 mol of epichlorohydrin per 1.0 mol of alkanediol, and 0.5 mmol to 10.0 mmol of phase transfer catalyst per 1.0 mol of epichlorohydrin are charged into a reactor. (2) 1.0 mol to 12.0 mol of solid sodium hydroxide per 1.0 mol of alkanediol is added to the reactor in three to ten equal portions over a period of one to five hours. Simultaneously or separately, (3) 0.5 mol to 1.0 mol of water per 1 mol of alkanediol is added to the reactor in three to ten equal portions over a period of one to five hours. (4) After the addition of sodium hydroxide and water in portions is complete, the reaction solution is further stirred for one to twelve hours. (5) During the steps (2) to (4), the temperature of the reaction solution is maintained at 35°C to 49°C. When the divided additions of steps (2) and (3) are each considered to be one step, the order of these steps is preferably such that the divided addition step of step (2) comes after the divided addition step of step (3), from the viewpoint of adjusting the reaction temperature, the hydroxide ion concentration in the reaction solution, and the total amount of chlorine. The order of the divided addition step of step (2) and the divided addition step of step (3) is also preferably the same when these steps are repeated.
[0053] (Purification Step) The purification step is a step of purifying the obtained crude diglycidyl ether. The purification of the crude diglycidyl ether may be carried out by extracting the obtained crude diglycidyl ether and then distilling it. The extraction may be carried out, for example, by filtering the crude diglycidyl ether and then adding chloroform to the filtrate. The distillation may be carried out, for example, by distillation under reduced pressure. The distillation conditions can be adjusted as appropriate.
[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. In the examples, the apparatus and conditions used for sample preparation and physical property analysis are as follows:
[0055] [GC (Gas Chromatography Analysis)] Analytical apparatus: 7890A Gas Chromatography System manufactured by Agilent Technologies Analytical column: HP-5 manufactured by Agilent Technologies (length 30 m × inner diameter 0.32 mm × film thickness 0.25 μm, packing: (5%-phenyl)-methylpolysiloxane) Heating conditions: After holding at 50°C for 5 minutes, heat from 50°C to 320°C at 10°C / min, and hold at 320°C for 28 minutes Sample introduction temperature: 320°C Carrier gas: nitrogen Column gas flow rate: 0.5 mL / min Detector and detection temperature: flame ionization detector (FID), 320°C Control mode: constant flow Split ratio: 50 Sample injection conditions: 1.0 μL
[0056] [Calculation of diglycidyl ether concentration (DGE concentration)] The diglycidyl ether concentration was calculated using the following formula (A) from the total area value of the peaks of diglycidyl ethers such as BEPG-DGE (DGE represented by formula (1-2)), an isomer of BEPG-DGE, and PD9-DGE (DGE represented by formula (1-1)) detected at a retention time of 25.5 to 26.9 minutes under the above measurement conditions (DGE detected peak area value) and the total area value of all peaks detected at a retention time of 0.0 to 60.0 minutes (total detected peak area value). DGE concentration (%) = (DGE detected peak area value / total detected peak area value) × 100 (A)
[0057] [GC-MS (Gas Chromatography Mass Spectrometry)] GC analyzer: 6890N manufactured by Agilent Technologies MS analyzer: Jms-K9 ultraQuad GC / MS manufactured by JEOL Corporation GC analytical column: HP-5 manufactured by Agilent Technologies (length 30 m × inner diameter 0.32 mm × film thickness 0.25 μm, packing: (5%-phenyl)-methylpolysiloxane) Heating conditions: After holding at 50°C for 5 minutes, heat from 50°C to 320°C at 10°C / min, and hold at 320°C for 28 minutes Sample introduction temperature: 320°C Carrier gas: Helium Column gas flow rate: 0.5 mL / min Control mode: Constant flow Split ratio: 50 Sample injection conditions: 1.0 μL MS measurement mode: CI Interface temperature: 250° C. Ion source temperature: 150° C. Ionization gas: isobutane Mass spectra of the peaks of BEPG-DGE and PD9-DGE detected at a retention time of 22.0 to 24.0 minutes under the above measurement conditions were confirmed.
[0058] [ 1 H NMR spectrum (500 MHz)] Apparatus: JNM-ECA500 manufactured by JEOL Corporation Standard: tetramethylsilane (0.00 ppm)
[0059] [ 13 C NMR spectrum (126 MHz)] Apparatus: JNM-ECA500 manufactured by JEOL Corporation Standard: tetramethylsilane (0.00 ppm)
[0060] [Measurement of total chlorine content] Apparatus: Mitsubishi Chemical Analytic Co., Ltd. NSX-2100 Argon gas flow rate: 100 ml / min Oxygen gas flow rate: 300 ml / min Heater temperature at inlet: 900°C Heater temperature at outlet: 1000°C Chlorine measurement - potentiometric titration End point: 290-315 mV
[0061] [Epoxy equivalent, crosslink density] Test method: ISO 3001 (tetraethylammonium bromide-perchloric acid method) Crosslink density (calculated value): The reciprocal of the epoxy equivalent [g / eq] measured by the above method was taken as the crosslink density [eq / g].
[0062] [Dielectric loss tangent, relative dielectric constant] Apparatus: Precision LCR meter E4980A manufactured by Agilent Technologies Test method: Compliant with IEC62631-2-1 Test dimensions: 60 x 60 x t3 (mm) Frequency: 1 MHz Test temperature: 23°C
[0063] [Glass transition temperature, coefficient of linear thermal expansion] Apparatus: Rigaku Corporation TMA8311 Test method: JIS K 7197 Test dimensions: 10 × 5 × t3 (mm) Heating rate: 5°C / min Measurement temperature range: room temperature to 300°C Measurement mode: compression (load 49 mN) Atmosphere: nitrogen gas flow (100 mL / min)
[0064] [Oven] Equipment: Constant temperature incubator DKM600 manufactured by Yamato Scientific Co., Ltd.
[0065] The abbreviations have the following meanings: PD-9: 2,4-diethyl-1,5-pentanediol BEPG: 2-butyl-2-ethyl-1,3-propanediol PD9-DGE: 2,4-diethyl-1,5-pentanediol diglycidyl ether BEPG-DGE: 2-butyl-2-ethyl-1,3-propanediol diglycidyl ether 16HD-DGE: 1,6-hexanediol diglycidyl ether [Epogose (registered trademark) HD(D), electronic materials grade, manufactured by Yokkaichi Chemical Co., Ltd.] BPA: bisphenol A epoxy resin [jER (registered trademark) 828, manufactured by Mitsubishi Chemical Corporation] MH700: 4-methylhexahydrophthalic anhydride / hexahydrophthalic anhydride mixture (molar ratio 70:30) [Rikacid (registered trademark) MH-700, manufactured by New Japan Chemical Co., Ltd.] TBP-DEPS: tetrabutylphosphonium O,O-diethylphosphorodithioate [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.] EPH: epichlorohydrin [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 99%] TBNB: tetra-n-butylammonium bromide [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.] NaOH: sodium hydroxide [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 97%, granular solid] CDCl 3 : deuterated chloroform [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., containing 0.03% tetramethylsilane]
[0066] Example 1: Preparation of a Composition Containing PD9-DGE (Composition A) Kyowadiol PD-9 (a mixture of PD-9 and BEPG, with a GC area ratio of PD-9 / BEPG of 95 / 5) manufactured by KH Neochem Co., Ltd. was used as the alkanediol. 305 g (1.90 mol) of alkanediol, 705 g (7.62 mol) of EPH, and 8.60 g (26.7 mmol) of TBNB were charged to a reaction flask. Next, while stirring the charged solution at 250 rpm using a mechanical stirrer equipped with a stirring blade, the liquid temperature in the reaction flask was maintained at 45±1°C in a water bath, and 50.8 g (1.25 mol) of NaOH was added. Subsequently, 5.08 g (0.282 mol) of water was added, yielding a cloudy, heterogeneous mixture. No increase in the liquid temperature in the reaction flask was observed. The heterogeneous mixture was stirred at 250 rpm for 30 minutes while maintaining the temperature at 45±1°C, and 50.8 g (1.27 mol) of NaOH was added again. Then, 5.08 g (0.282 mol) of water was added. The same procedure was repeated a total of six times, and a total of 305 g (7.63 mol) of NaOH and 30.5 g (1.69 mol) of water were added to the reaction flask over three hours. This mixture was stirred at 250 rpm for an additional six hours while maintaining the temperature at 45±1°C, yielding a heterogeneous reaction mixture. This mixture was filtered to remove insoluble matter. 100 g of chloroform was added to the filtrate to extract the product, which was then washed with 1,000 g of water. The product after water washing was then purified by distillation under reduced pressure to obtain Composition A. Composition A had a boiling point of 145-150°C / 0.9 kPa, and the isolated yield was 49% (based on alkanediol). The DGE concentration, total chlorine content, epoxy equivalent, and crosslink density of the resulting composition A are shown in Table 1.
[0067] Then, GC-MS (CI), 1 H-NMR, and 13 C-NMR analysis was performed. The analytical results are shown below. GC-MS (CI) m / z: 273 (GC-MS retention time: 22.5-22.7 min, BEPG-DGE, MH + ), 273 (GC-MS retention time; 23.0-23.5 minutes, PD9-DGE, MH + ). 1 H NMR (CDCl3 , 500MHz) δ 3.68 (m, 2H, glycidyl group), 3.40 (m, 2H, glycidyl group), 3.36 (m, 4H, CH 2 CHCH 2 O), 3.12 (m, 2H, glycidyl group), 2.78 (m, 2H, glycidyl group), 2.60 (m, 2H, glycidyl group), 1.60 (m, 2H, CH 2 CHCH 2 O), 1.46-1.28 (m, 4H, CH 3 CH 2 ), 1.25 (m, 2H, CH 2 CHCH 2 O), 0.88 (t, 6H, CH 3 CH 2 ). 13 C NMR (CDCl 3 , 126MHz) δ74.6, 71.6, 51.0, 44.2, 37.4, 32.8, 24.3, 10.9.
[0068] Example 2 Production of a composition containing BEPG-DGE (Composition B) Composition B was obtained in the same manner as in Example 1, except that the alkanediol was changed to BEPG manufactured by KH Neochem Co., Ltd. The boiling point of Composition B was 146 to 152°C / 0.8 kPa, and the isolated yield was 29% (based on the alkanediol). The DGE concentration, total chlorine content, epoxy equivalent, and crosslink density of the obtained Composition B are shown in Table 1.
[0069] Then, GC-MS (CI), 1 H-NMR, and 13 C-NMR analysis was performed. The analytical results are shown below. GC-MS (CI) m / z: 273 (GC-MS retention time: 22.5-22.7 min, BEPG-DGE, MH + ), 273 (GC-MS retention time: 23.0-23.5 min, BEPG-DGE isomer MH + ). 1 H NMR (CDCl 3, 500MHz) δ 3.68 (m, 2H, glycidyl group), 3.40 (m, 2H, glycidyl group), 3.36 (m, 4H, CH 2 CHCH 2 O), 3.12(m, 2H, glycidyl group), 2.78 (m, 2H, glycidyl group), 2.60 (m, 2H, glycidyl group), 1.60 (m, 2H, CH 2 CHCH 2 O), 1.46-1.28 (m, 4H, CH 3 CH 2 ), 1.25 (m, 2H, CH 2 CHCH 2 O), 0.88 (t, 6H, CH 3 CH 2 ). 13 C NMR (CDCl 3 , 126MHz) δ74.6, 71.6, 51.0, 44.2, 37.4, 32.8, 24.3, 10.9.
[0070] Comparative Example 1 Preparation of a Composition Containing PD9-DGE (Composition C) The same alkanediol as in Example 1 was used. 305 g (1.90 mol) of alkanediol, 705 g (7.62 mol) of EPH, and 8.60 g (26.7 mmol) of TBNB were charged into a reaction flask. Next, while stirring the charged liquid at 250 rpm using a mechanical stirrer equipped with a stirring blade, the liquid temperature in the reaction flask was maintained at 45°C using a water bath. 305 g (7.63 mol) of NaOH and 5.08 g (1.69 mol) of water were simultaneously added, causing the liquid temperature in the reaction flask to rapidly rise to 50°C. Cooling in the water bath for 1 hour and 15 minutes yielded a cloudy heterogeneous mixture with a liquid temperature of 45°C in the reaction flask. The heterogeneous mixture was stirred at 250 rpm for 6 hours while maintaining the temperature at 45±1°C, yielding a heterogeneous reaction liquid. This was filtered to remove insoluble matter. 100 g of chloroform was added to this filtrate to extract the product, which was then washed with 1,000 g of water. The product after water washing was then purified by distillation under reduced pressure to obtain composition C. The boiling point of composition C was 145 to 150°C / 0.9 kPa, and the isolated yield was 49% (based on alkanediol). The DGE concentration, total chlorine content, epoxy equivalent, and crosslink density of the obtained composition C are shown in Table 1.
[0071] Comparative Example 2 Analysis of a composition containing 16HD-DGE (composition D) Analysis was performed on Epogose (registered trademark) HD(D) manufactured by Yokkaichi Synthetic Co., Ltd., which is composition D. The DGE concentration, total chlorine content, epoxy equivalent, and crosslink density of composition D are shown in Table 1.
[0072] Examples 3-4, Comparative Examples 3-4 Preparation and Evaluation of Curable Compositions 1-4 To 100 parts by mass of the epoxy resin composition listed in Table 2, the curing agent MH700 was added in an equimolar amount relative to the epoxy groups in the epoxy resin composition, and 1 part by mass of the curing accelerator TBP-DEPS was added to obtain a mixture. This mixture was degassed by stirring under reduced pressure at room temperature (approximately 25°C) for 30 minutes to prepare Curable Compositions 1-4. Each curable composition, along with a 3 mm-thick U-shaped silicone rubber spacer, was sandwiched between two glass substrates that had been previously treated with a fine heat-resistant TFE coating (manufactured by Fine Chemical Japan Co., Ltd.). The curable composition sandwiched between the two glass substrates was then heated in an oven at 100°C for 2 hours (pre-curing), and then heated to 150°C and heated for 5 hours (main curing). After gradual cooling, the glass substrates were removed, yielding each cured product with a thickness of 3 mm. The cured products were evaluated for dielectric constant, dielectric loss tangent, glass transition temperature (Tg), and coefficient of linear thermal expansion (CTE). Each physical property was measured according to the following procedures. The results are shown in Table 2.
[0073] [Dielectric constant, dielectric loss tangent] The dielectric loss tangent tanδ and capacitance Cp were measured when a voltage of 1 V and 1 MHz was applied to a test piece sandwiched between the electrodes of the holder, and the capacitance Cp of air measured under the same conditions was also measured. 0 Divide by to get the relative permittivity ε r The dielectric loss tangent tanδ or relative dielectric constant ε r The lower the value, the better the dielectric properties.
[0074] [Glass transition temperature (Tg)] The thermal properties of the test piece were measured by thermomechanical analysis (TMA), and tangents were drawn to the curves before and after the obtained TMA curve, and Tg was determined from the intersection of these tangents. When Tg is high, the glass state can be maintained even at high temperatures during soldering of electronic substrates, and the heat resistance is excellent, making it suitable for use as a semiconductor encapsulant, for example.
[0075] [Coefficient of Linear Thermal Expansion (CTE)] Thermomechanical analysis (TMA) of the test piece was measured, and the CTE was determined from the slope of the obtained TMA curve in the section from 50° C. to 100° C. The lower the CTE, the more excellent the dimensional stability.
[0076]
[0077] As shown in Table 1, Compositions A and B, which are compositions containing a chlorine-containing compound and a diglycidyl ether represented by formula (1) and have a total chlorine content of 900 ppm or less, have a total chlorine content sufficiently lower than the halogen-free grade threshold (900 ppm or less) desired in the electronic materials field, and are found to have excellent insulation reliability. On the other hand, Composition C of Comparative Example 1, which was produced by a conventionally known production method (WO98 / 39314) and has a total chlorine content not less than 900 ppm, has a total chlorine content higher than the threshold (900 ppm or less), and is considered to have significantly lower insulation reliability. Therefore, it is considered difficult to use it for, for example, semiconductor encapsulation applications.
[0078]
[0079] As shown in Table 2, the curable composition 1 (Example 3) to which the composition A obtained in Example 1 was added as a reactive diluent had a lower dielectric constant and CTE than the curable composition 3 (Comparative Example 3) to which the composition C obtained in Comparative Example 1, which was produced by a conventionally known production method (WO98 / 39314), was added as a reactive diluent.
[0080] As shown in Table 2, the curable composition 1 (Example 3) to which the composition A obtained in Example 1 was added as a reactive diluent had lower relative permittivity, dielectric loss tangent, and CTE than the curable composition 4 (Comparative Example 4) to which the conventionally known composition D of Comparative Example 2 was added as a reactive diluent.
[0081] As shown in Table 2, curable composition 2 (Example 4) to which composition B obtained in Example 2 was added as a reactive diluent had lower relative permittivity, dielectric loss tangent, and CTE than curable composition 4 (Comparative Example 4) to which composition D of the conventionally known Comparative Example 2 was added as a reactive diluent.
[0082] Furthermore, as shown in Table 1, the crosslink density of the reactive diluent (Example 1: Composition A) was 0.86 times that of the conventionally known reactive diluent (Comparative Example 2: Composition D), indicating that Example 1 had a low crosslink density. In contrast, as shown in Table 2, the difference in Tg between curable composition 4 (Comparative Example 4) to which a conventionally known reactive diluent (Comparative Example 2: Composition D) was added and curable composition 1 (Example 3) to which a reactive diluent (Example 1: Composition A) was added was 2°C, which was equivalent. Also, as shown in Table 1, the crosslink density of the reactive diluent (Example 2: Composition B) was 0.86 times that of the conventionally known reactive diluent (Comparative Example 2: Composition D), indicating that Example 2 had a low crosslink density. In contrast, as shown in Table 2, the Tg of curable composition 2 (Example 4) to which a reactive diluent (Example 2: Composition B) was added was 6°C higher than that of curable composition 4 (Comparative Example 4) to which a conventionally known reactive diluent (Comparative Example 2: Composition D) was added.
[0083] This application is based on a Japanese patent application (Patent Application No. 2023-058088) filed with the Japan Patent Office on March 31, 2023, the contents of which are incorporated herein by reference.
[0084] The composition of the present invention has industrial applicability as a reactive diluent for epoxy resins, a curable composition, a method for producing a composition, and the like.
Claims
1. A composition comprising a chlorine-containing compound and a diglycidyl ether represented by the following formula (1), wherein the total chlorine content is 900 ppm or less. (In formula (1), X represents an alkylene group having 9 to 11 carbon atoms.) 2. The composition according to claim 1, wherein in said X of said formula (1), said alkylene group is a branched alkylene group.
3. The composition according to claim 1, wherein the diglycidyl ether is at least one of diglycidyl ethers represented by the following formula (1-1) and the following formula (1-2):
4. A reactive diluent for epoxy resins comprising the composition of claim 1.
5. A curable composition comprising the reactive diluent of claim 4.
6. A method for producing a composition containing a chlorine-containing compound and a diglycidyl ether represented by the following formula (1), wherein the total chlorine content of the composition is 900 ppm or less, the method comprising: a crude diglycidyl ether production step of reacting an alkanediol having 9 to 11 carbon atoms with epichlorohydrin to obtain a crude diglycidyl ether containing the diglycidyl ether represented by the following formula (1); and a purification step of purifying the obtained crude diglycidyl ether, wherein the reaction temperature and the total chlorine content are adjusted by adding solid sodium hydroxide and water in portions in the crude diglycidyl ether production step. (In formula (1), X represents an alkylene group having 9 to 11 carbon atoms.)
Citation Information
Patent Citations
Glycidyl ether and method for producing the same
JP2005029487A
Production method of glycidyl ethers
JP2016193874A
Glycidyl ether of gem-bis(hydroxymethyl) hydrocarbons
US4481348A
Diglycidyl ethers
WO1998039314A1