Conductive polymer dispersion liquid, method for producing conductive polymer dispersion liquid, and method for producing solid electrolytic capacitor
The conductive polymer dispersion, optimized with polyethylenedioxythiophene and polystyrene sulfonic acid, addresses the challenge of high ESR in solid electrolytic capacitors by adjusting weight and volume ratios and pH, resulting in improved performance for high-frequency digital equipment.
Patent Information
- Application Number
- PCT/JP2024/012856
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Solid electrolytic capacitors using conductive polymers face challenges in achieving low equivalent series resistance (ESR), which is essential for high-frequency digital equipment applications, as existing methods struggle to optimize the conductivity and viscosity of conductive polymer dispersions.
A conductive polymer dispersion is developed using polyethylenedioxythiophene doped with polystyrene sulfonic acid, with specific weight and volume ratios of the conductive polymer and additive, along with pH adjustment and concentration steps, to form a solid electrolyte layer with reduced ESR.
The method effectively reduces the initial ESR of solid electrolytic capacitors, maintaining high conductivity and preventing gelation, thereby enhancing their performance in high-frequency applications.
Smart Images

Figure JP2024012856_03102024_PF_FP_ABST
Abstract
Description
Conductive polymer dispersion, method for producing conductive polymer dispersion, and method for producing solid electrolytic capacitor
[0001] The present invention relates to a conductive polymer dispersion for forming a solid electrolyte of a solid electrolytic capacitor, a method for producing a conductive polymer dispersion, and a method for producing a solid electrolytic capacitor.
[0002] Electrolytic capacitors use valve metals such as tantalum or aluminum as anode and cathode foils. The anode foils are enlarged by shaping the valve metal into a sintered or etched foil, and the enlarged surface is coated with a dielectric film by anodizing or other processes. An electrolyte is interposed between the anode and cathode foils.
[0003] Electrolytic capacitors have the advantage of being able to increase the specific surface area by expanding the surface area of the anode foil, making it easier to achieve a larger capacitance than other types of capacitors. Electrolytic capacitors contain electrolyte in the form of an electrolytic solution. The contact area between the electrolyte and the dielectric film on the anode foil increases, making it easier to further increase the capacitance of electrolytic capacitors.
[0004] In recent years, solid electrolytic capacitors, which use a solid electrolyte with higher conductivity than the electrolyte solution, have also been attracting attention. Solid electrolytic capacitors use a solid electrolyte with higher conductivity than the electrolyte solution, and can achieve low equivalent series resistance (ESR). Known solid electrolytes include manganese dioxide and 7,7,8,8-tetracyanoquinodimethane (TCNQ) complex.
[0005] Additionally, conductive polymers derived from monomers with π-conjugated double bonds, such as poly(3,4-ethylenedioxythiophene) (PEDOT), which has excellent adhesion to dielectric films, are rapidly becoming popular as solid electrolytes. Conductive polymers use acid compounds such as polyanions as dopants to achieve high conductivity. Therefore, solid electrolytic capacitors have the advantage of low equivalent series resistance (ESR).
[0006] A solid electrolyte containing a conductive polymer is formed by applying or impregnating a conductive polymer dispersion between an anode body and a cathode body and then drying the dispersion medium. The conductive polymer dispersion is a dispersion of a conductive polymer, and for example, water is used as the dispersion medium to disperse the conductive polymer in water.
[0007] JP 2011-60980 A JP 2014-152320 A
[0008] Thus, solid electrolytic capacitors are easier to achieve a low ESR than electrolytic capacitors that use an electrolytic solution. However, electrolytic capacitors are increasingly being used in digital devices where information processing in the high frequency range of over several tens of kHz is becoming commonplace, and solid electrolytic capacitors that use conductive polymers as the electrolyte are also attracting attention. As solid electrolytic capacitors become more versatile, there is an even greater demand for lower ESR in solid electrolytic capacitors.
[0009] The present invention has been proposed to solve the above-mentioned problems, and an object of the present invention is to provide a conductive polymer dispersion for realizing a solid electrolytic capacitor with a low ESR, a method for producing the conductive polymer dispersion, and a method for producing a solid electrolytic capacitor.
[0010] In order to solve the above problems, the conductive polymer dispersion of this embodiment contains polyethylenedioxythiophene doped with polystyrene sulfonic acid as a conductive polymer, a dispersion medium for the conductive polymer, and an additive added to the dispersion medium, wherein the amount x (wt %) of the conductive polymer and the amount y (Vol %) of the additive fall within the range enclosed by the following relational expressions (1) to (4): y=-29x+100 (1) y=-34x+83 (2) x=1 (3) y=5 (4)
[0011] The additive may be a polyhydric alcohol.
[0012] The pH may be 3 or more and 6 or less.
[0013] The mass ratio of the polystyrene sulfonic acid (PSS) to the polyethylenedioxythiophene (PEDOT) may be PEDOT:PSS=less than 1:3.
[0014] Furthermore, in order to solve the above-described problems, the method for producing a conductive polymer of this embodiment includes an additive addition step of adding an additive, or an additive and an additional dispersion medium, to a conductive polymer dispersion liquid in which a conductive polymer is dispersed in a dispersion medium, wherein the conductive polymer is polyethylenedioxythiophene doped with polystyrene sulfonic acid, and in the additive addition step, the amount x (wt %) of the conductive polymer added and the amount y (Vol %) of the additive added are within the range surrounded by the relational expressions (1) to (4).
[0015] The mass ratio of the polystyrene sulfonic acid (PSS) to the polyethylenedioxythiophene (PEDOT) may be PEDOT:PSS=less than 1:3.
[0016] The method may include a pH adjustment step of adjusting the pH of the conductive polymer dispersion to 3 or more and 6 or less, and a concentration step of concentrating the conductive polymer dispersion after the pH adjustment step, wherein after the concentration step, in the additive addition step, the amount x (wt %) of the conductive polymer added and the amount y (Vol %) of the additive added may be adjusted to fall within the range surrounded by the relational expressions (1) to (4).
[0017] The concentration step may be a second concentration step, and may include a first concentration step, prior to the pH adjustment step, of concentrating the conductive polymer dispersion so that the concentration of the conductive polymer is in the range of less than 2.6 wt %, and the pH adjustment step may be performed after the first concentration step, and in the second concentration step, the conductive polymer dispersion may be further concentrated so that the concentration of the conductive polymer is in the range of 3.5 wt % or less.
[0018] The additive may be a polyhydric alcohol.
[0019] In order to solve the above-mentioned problems, the method for producing a conductive polymer according to the present embodiment uses the conductive polymer dispersion to form a solid electrolyte layer between an anode body and a cathode body.
[0020] According to the present invention, a solid electrolytic capacitor with low ESR can be realized.
[0021] 1 is a graph showing the relationship between the amount of PEDOT:PSS contained in a conductive polymer dispersion and the amount of additives. 2 is a scatter diagram showing the results of relational expressions (1) to (4) and each example and each comparative example.
[0022] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the embodiments described below.
[0023] (Conductive Polymer Dispersion) The conductive polymer dispersion is a dispersion for forming a solid electrolyte layer in a solid electrolytic capacitor. A solid electrolytic capacitor is a passive element that stores and discharges electric charge through capacitance. It consists of an anode foil and a cathode foil, each having a dielectric film formed thereon, facing each other, with a solid electrolyte layer interposed between the anode foil and the cathode foil. The solid electrolyte layer contains a conductive polymer. In addition to the solid electrolyte layer, the solid electrolytic capacitor may be impregnated with an electrolytic solution. A separator may also be inserted between the anode foil and the cathode foil to prevent short circuits between the anode foil and the cathode foil and to maintain the solid electrolyte layer.
[0024] The conductive polymer dispersion is a dispersion in which particles or powder of a conductive polymer to be contained in the solid electrolyte layer are dispersed. The conductive polymer is adhered between the anode foil and the cathode foil by immersing each of the anode foil, cathode foil, and separator in the conductive polymer dispersion and drying them. Alternatively, the conductive polymer may be adhered by first winding or stacking the anode foil and cathode foil with the separator interposed therebetween to prepare a capacitor element, and then immersing the capacitor element in the conductive polymer dispersion and drying it. In addition to immersion, the conductive polymer dispersion may be applied by dropwise application or spray application. The drying process may be repeated multiple times, or drying may be performed under reduced pressure.
[0025] The conductive polymer used is polyethylenedioxythiophene, also known as PEDOT, which is represented by the following chemical formula (1).
[0026] This PEDOT is doped with polystyrene sulfonic acid, also known as PSS. That is, the conductive polymer is polyethylenedioxythiophene doped with polystyrene sulfonic acid. Hereinafter, polyethylenedioxythiophene doped with polystyrene sulfonic acid will be referred to as PEDOT:PSS.
[0027] The number average molecular weight of PSS is 1,000 to 2,000,000, preferably 10,000 to 500,000. If the number average molecular weight is less than 1,000, the resulting conductive polymer will have insufficient conductivity and reduced dispersibility, which is undesirable, while if the number average molecular weight exceeds 2,000,000, the viscosity of the mixed liquid will increase, which is undesirable.
[0028] When the weight ratio of PSS to PEDOT is less than 1:3, the initial ESR can be reduced. When the weight ratio of PEDOT to PSS is 1:1.5 or more, the increase in viscosity of the conductive polymer dispersion can be suppressed. When the weight ratio of PEDOT to PSS is 1:2.5 or more, the initial ESR can be reduced while suppressing the increase in viscosity of the conductive polymer dispersion.
[0029] The dispersion medium for the conductive polymer dispersion may be any medium capable of dispersing conductive polymer particles or powder. The dispersion medium for the conductive polymer dispersion is typically water, but may also be an organic solvent or a mixture of an organic solvent and water. Examples of the organic solvent include polar solvents, alcohols, esters, hydrocarbons, carbonate compounds, ether compounds, chain ethers, heterocyclic compounds, and nitrile compounds.
[0030] Examples of polar solvents include N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide. Examples of alcohols include methanol, ethanol, propanol, and butanol. Examples of esters include ethyl acetate, propyl acetate, and butyl acetate. Examples of hydrocarbons include hexane, heptane, benzene, toluene, and xylene. Examples of carbonate compounds include ethylene carbonate and propylene carbonate. Examples of ether compounds include dioxane and diethyl ether. Examples of linear ethers include ethylene glycol dialkyl ether, propylene glycol dialkyl ether, polyethylene glycol dialkyl ether, and polypropylene glycol dialkyl ether. Examples of heterocyclic compounds include 3-methyl-2-oxazolidinone. Examples of nitrile compounds include acetonitrile, glutarodinitrile, methoxyacetonitrile, propionitrile, and benzonitrile.
[0031] The dispersion medium further contains an additive such as a polyhydric alcohol. Examples of the polyhydric alcohol include polyethylene glycol, 1-hexanol, ethylene glycol, diethylene glycol, triethylene glycol, glycerin, and combinations of two or more of these. Because the polyhydric alcohol has a high boiling point, it remains in the solid electrolyte layer even after the conductive polymer dispersion is dried.
[0032] Here, in the conductive polymer dispersion, the amount x (wt %) of the conductive polymer and the amount y (Vol %) of the additive fall within the range Er surrounded by the following relational expressions (1) to (4), as shown in Figure 1. The amount x (wt %) of the conductive polymer is the percentage of the weight of the conductive polymer relative to the total weight of the conductive polymer dispersion, and the amount y (Vol %) of the additive is the percentage of the volume of the conductive polymer relative to the total volume of the conductive polymer dispersion.
[0033] (Relationship) y = -29x + 100 (5 ≤ y ≤ 71, 1 ≤ x ≤ 3.3) ... (1) y = -34x + 83 (5 ≤ y ≤ 49, 1 ≤ x ≤ 2.3) ... (2) x = 1 (49 ≤ y ≤ 71) ... (3) y = 5 (2.3 ≤ x ≤ 3.3) ... (4)
[0034] In Figure 1, the lines indicated by relational formulas (2), (3), and (4) represent the boundary of the range in which the initial ESR of a solid electrolytic capacitor is favorable. The initial ESR refers to the value measured after a solid electrolytic capacitor is manufactured and aged to repair defects by applying a voltage, before it is energized and has not been exposed to a high-temperature or low-temperature environment. The line indicated by relational formula (1) represents the boundary at which aggregation occurs in the conductive polymer dispersion, even when the pH of the conductive polymer dispersion is 3 to 6. If the amount of ethylene glycol or the amount of PEDOT:PSS is greater than the line indicated by relational formula (1), aggregation occurs in the conductive polymer dispersion and gelation occurs.
[0035] It is more preferable that the amount x (wt %) of the conductive polymer and the amount y (Vol %) of the additive fall within a range Er surrounded by the following relational expressions (2a), (4a), (1), and (3) instead of the line segments indicated by relational expressions (2) and (4).
[0036] (Relationship)
[0037] In order to keep the amount x (wt%) of the conductive polymer and the amount y (Vol%) of the additive within the range Er enclosed by the relational expressions (1) to (4), it is sufficient to add an additive addition step to the manufacturing method of the conductive polymer dispersion, in which an additive, or an additive and an additional dispersion medium, is added to the initial conductive polymer dispersion composed of the conductive polymer and the dispersion medium. By adding the additive, or the additive and the additional dispersion medium in this additive addition step, the amount x (wt%) of the conductive polymer and the amount y (Vol%) of the additive are adjusted.
[0038] However, in order to perform this additive addition process, it may be necessary to first concentrate the initial PEDOT:PSS concentration of the conductive polymer dispersion. If the pH of the conductive polymer dispersion is 3 or less, concentrating the PEDOT:PSS concentration of the conductive polymer dispersion to 2.6 wt% or more will cause aggregation in the conductive polymer dispersion. Also, even if the pH of the conductive polymer dispersion is 3 to 6, concentrating the PEDOT:PSS concentration of the conductive polymer dispersion to 3.5 wt% or more will cause aggregation in the conductive polymer dispersion, as shown in relational expression (1).
[0039] Therefore, when concentrating the PEDOT:PSS concentration of a conductive polymer dispersion, a pH adjustment step is performed before the concentration step, in which the pH of the conductive polymer dispersion is adjusted to 3 or more and 6 or less. In the pH adjustment step, for example, ammonia is blown into the conductive polymer dispersion. The concentration step can be performed by any known method as long as it can concentrate the conductive polymer dispersion, and examples thereof include ultrafiltration. That is, the conductive polymer dispersion is forced through a semipermeable membrane by pressure or the like.
[0040] Preferably, a concentration step is added before the pH adjustment step to concentrate the conductive polymer dispersion to a PEDOT:PSS concentration of less than 2.6 wt%. That is, a first concentration step is performed, followed by a pH adjustment step, followed by a second concentration step. In the first concentration step, the PEDOT:PSS concentration of the conductive polymer dispersion is kept below 2.6 wt% so that the initial conductive polymer dispersion with a pH of approximately 1.9 does not gel, even if the pH adjustment step has not been performed. In the second concentration step, the conductive polymer dispersion is concentrated to a PEDOT:PSS concentration of 3.5 wt% or less because the pH adjustment step prevents gelation if the PEDOT:PSS concentration of the conductive polymer dispersion is 3.5 wt% or less.
[0041] By performing the first concentration step, then the pH adjustment step, and then the second concentration step, it is possible to suppress dedoping of polystyrene sulfonic acid that may occur during the pH adjustment step, thereby maintaining the high conductivity of the conductive polymer and further reducing the initial ESR of the solid electrolytic capacitor.
[0042] The initial conductive polymer dispersion preparation process before adjusting the amount x (wt %) of conductive polymer and the amount y (Vol %) of additive is, for example, as follows: First, a monomer constituting the conductive polymer and an acid or its alkali metal salt that releases a dopant constituting the conductive polymer are added, an oxidizing agent is added, and the mixture is stirred until chemical oxidation polymerization is complete. Next, residual monomers and impurities are removed by purification means such as ultrafiltration, cation exchange, and anion exchange. This yields a conductive polymer dispersion.
[0043] In addition, in the process of preparing this conductive polymer dispersion, for example, a monomer constituting the conductive polymer and an acid or its alkali metal salt that releases a dopant constituting the conductive polymer are added, a supporting electrolyte is added, and electrolytic oxidation polymerization is carried out by one of a constant potential method, a constant current method, and a potential sweep method while stirring, and then impurities and residual monomers are removed by a purification means such as ultrafiltration, cation exchange, and anion exchange. The conductive polymer is dispersed using, for example, ultrasound.
[0044] The conductive polymer dispersion may contain an organic binder, a surfactant, a dispersant, an antifoaming agent, a coupling agent, an antioxidant, an ultraviolet absorber, and the like.
[0045] A solid electrolytic capacitor in which a solid electrolyte layer is formed using such a conductive polymer dispersion improves the initial ESR regardless of its specific configuration. For example, a stacked configuration is adopted in which anode bodies and cathode bodies are alternately stacked with a separator sandwiched therebetween. In the stacked configuration, in addition to a flat plate configuration in which an exterior is omitted, for example, the capacitor element is covered with a laminate film, or is sealed by molding, dip coating, or printing with a resin such as a heat-resistant resin or an insulating resin.
[0046] Alternatively, a wound arrangement is employed in which the anode and cathode elements are alternately stacked with a separator sandwiched therebetween and wound. In the wound arrangement, for example, the capacitor element is inserted into a cylindrical outer case with a bottom, and the open end of the outer case is sealed with a sealing body by crimping. The sealing body is made of, for example, rubber or a laminate of rubber and a hard substrate. Examples of rubber include ethylene propylene rubber and butyl rubber.
[0047] The anode and cathode bodies are foils made of valve metals, such as aluminum, tantalum, niobium, niobium oxide, titanium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony. The purity of the anode foil is preferably 99.9% or higher, and that of the cathode foil is preferably 99% or higher. However, impurities such as silicon, iron, copper, magnesium, and zinc may be included. Furthermore, when the solid electrolytic capacitor is a flat type, a solid electrolyte layer may be formed on the anode foil so as to cover the dielectric film, and then a metal paste such as silver paste may be printed and dried. This silver layer corresponds to the cathode of the solid electrolytic capacitor.
[0048] The anode body has a porous structure on its surface, either as a sintered body made by sintering valve metal powder or as an etched foil made by etching a stretched foil. The porous structure consists of tunnel-like pits, spongy pits, or voids between densely packed powder particles. The porous structure is typically formed by direct current etching or alternating current etching, in which direct current or alternating current is applied in an acidic aqueous solution containing halogen ions, such as hydrochloric acid, or by vapor deposition or sintering metal particles or the like on the core. The cathode body may also have a porous surface, if necessary.
[0049] The dielectric film is the dielectric layer of a solid electrolytic capacitor and is typically an oxide film formed on the surface of the anode body. If the anode body is an aluminum foil, the dielectric film is an aluminum oxide layer formed by oxidizing the porous structure region. This dielectric film is formed by applying a voltage in a solution free of halogen ions, such as an aqueous solution of adipic acid or boric acid. A dielectric film may also be formed on the cathode foil as needed, and a layer made of a metal nitride, metal carbide, or metal carbonitride formed by vapor deposition, or a film containing carbon on the surface, may also be used.
[0050] Examples of separators include cellulose papers such as kraft, Manila hemp, esparto, hemp, and rayon, and mixtures thereof; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and derivatives thereof; polytetrafluoroethylene resins, polyvinylidene fluoride resins, vinylon resins; polyamide resins such as aliphatic polyamides, semi-aromatic polyamides, and wholly aromatic polyamides; polyimide resins; polyethylene resins; polypropylene resins; trimethylpentene resins; polyphenylene sulfide resins; acrylic resins; and polyvinyl alcohol resins. These resins can be used alone or in combination. If the shape of the solid electrolyte layer can be maintained by itself and the pair of electrodes can be separated by the solid electrolyte layer, the separator can be omitted from the capacitor element.
[0051] An electrolyte solution may be used in addition to the solid electrolyte layer. The solvent for the electrolyte solution is not particularly limited, and a protic organic polar solvent or an aprotic organic polar solvent can be used. Typical examples of protic polar solvents include monohydric alcohols, polyhydric alcohols, and oxyalcohol compounds, such as ethylene glycol or propylene glycol. Typical examples of aprotic polar solvents include sulfones, amides, lactones, cyclic amides, nitriles, and sulfoxides, such as sulfolane, γ-butyrolactone, ethylene carbonate, and propylene carbonate.
[0052] The solute contained in the electrolyte solution includes anionic and cationic components, typically organic acids such as adipic acid and benzoic acid or their salts, inorganic acids such as boric acid and phosphoric acid or their salts, or composite compounds of organic acids and inorganic acids such as borodisalicylic acid or their ionically dissociable salts, used alone or in combination of two or more. Examples of these salts of organic acids, salts of inorganic acids, and at least one salt of a composite compound of an organic acid and an inorganic acid include ammonium salts, quaternary ammonium salts, quaternized amidinium salts, amine salts, sodium salts, potassium salts, etc. Anionic acids and cationic bases may be added separately to the electrolyte solution as solute components.
[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0054] (Examples 1 to 16) Conductive polymer dispersions of Examples 1 to 16 and Comparative Examples 1 to 11 were prepared as follows. First, a conductive polymer dispersion composed of 1.2 wt % PEDOT:PSS and 98.8 wt % water was subjected to a dispersion treatment using ultrasound to disperse the conductive polymer. The weight ratio of PSS to PEDOT was PEDOT:PSS = 1:2.5. After the dispersion treatment, a first concentration step was performed using an ultrafiltration device. In the first concentration step, the conductive polymer dispersion was concentrated until the PEDOT:PSS content of the conductive polymer dispersion reached 2 wt %.
[0055] After the first concentration step, the process moved to a pH adjustment step, in which ammonia was added until the pH of the conductive polymer dispersion reached 4. After the pH adjustment step, the process moved to a second concentration step using an ultrafiltration device, in which the conductive polymer dispersion was concentrated until the PEDOT:PSS content reached 3.4 wt % relative to the conductive polymer dispersion. Here, for the conductive polymer dispersion of Comparative Example 11, when the conductive polymer dispersion was concentrated in the first concentration step without undergoing the pH adjustment step to pH = 4 until the PEDOT:PSS content reached 2.6 wt % relative to the conductive polymer dispersion, the conductive polymer dispersion of Comparative Example 11 gelled.
[0056] The conductive polymer dispersions of Examples 1 to 16 and Comparative Examples 1 to 10 that remained liquid without gelling were subjected to the additive addition step. Ethylene glycol was used as the additive in the additive addition step. In the additive addition step, ethylene glycol or ethylene glycol and water were added to the conductive polymer dispersion, and the amount x (wt%) of the conductive polymer and the amount y (Vol%) of the additive were adjusted for each of Examples 1 to 16 and Comparative Examples 1 to 10 to achieve various combinations.
[0057] The conductive polymer dispersions of Examples 1, 4, 9, 12, and 14 to 16 were prepared by adding ethylene glycol, while the conductive polymer dispersions of Examples 2, 3, 5 to 8, 10, 11, and 13 and Comparative Examples 1 to 10 were prepared by adding ethylene glycol and water. Note that in Comparative Example 11, 10 vol % ethylene glycol was added to the conductive polymer dispersion that remained gelled and stirred, but the dispersion remained gelled.
[0058] Solid electrolytic capacitors were fabricated using the conductive polymer dispersions of Examples 1 to 16 and Comparative Examples 1 to 10, and the initial ESR was measured. Aluminum foils were prepared as anode and cathode foils for the solid electrolytic capacitors. Both surfaces of the anode foil were subjected to an area enlargement treatment by AC etching. The anode foil was then transferred to a chemical conversion treatment process, where a dielectric film was formed on the anode foil.
[0059] Lead wires were connected to the anode and cathode foils, and the anode and cathode bodies were wound facing each other with a cellulose separator interposed between them. The wound assembly was then repaired and chemically converted. The wound assembly had a diameter of 8 mm, a height along the winding axis of 10 mm, a product rated voltage of 35 WV, and a capacitance of 150 μF.
[0060] The conductive polymer dispersions of Examples 1 to 16 and Comparative Examples 1 to 10 were impregnated into each wound body and dried at 125°C for 30 minutes. A solid electrolyte layer containing a conductive polymer was formed by drying the impregnated conductive polymer dispersion. The capacitor element with the solid electrolyte layer formed was then impregnated with an electrolyte solution. The solvent for the electrolyte solution was ethylene glycol, and 0.16 mol of ammonium azelaate per 1 kg of electrolyte solution was added as a solute.
[0061] The capacitor element with the solid electrolyte layer formed and impregnated with the electrolyte solution was housed in a cylindrical outer case with a bottom. A rubber seal was attached to the open end of the outer case and the case was sealed by crimping. Each solid electrolytic capacitor was subjected to an aging treatment by applying a voltage.
[0062] The initial ESR of the solid electrolytic capacitors using the conductive polymer dispersions of Examples 1 to 16 and Comparative Examples 1 to 10 was measured using an LCR meter (E4980A, manufactured by Agilent Technologies) with an AC current level set to 1.0 Vrms and a measurement frequency set to 100 kHz.
[0063] The amount x (wt %) of the conductive polymer, the amount y (Vol %) of the additive, and the ESR measurement results for the conductive polymer dispersions of Examples 1 to 16 and Comparative Examples 1 to 10 are shown in Tables 1 and 2 below. In the tables, the PEDOT:PSS concentration is the concentration of the conductive polymer relative to the conductive polymer dispersion, i.e., the amount x of the conductive polymer dispersion, and the EG ratio is the ratio of the additive relative to the conductive polymer dispersion, i.e., the amount y of the additive.
[0064] (Table 1)
[0065] (Table 2)
[0066] The results of Tables 1 and 2 above were plotted in Figure 2, which was created within Figure 1. Figure 2 is a scatter plot showing the results of relational expressions (1) to (4) and each example and comparative example. In Figure 2, the plots of black squares represent examples, and the plots of white squares represent comparative examples. The numerical values in parentheses adjacent to each plot are ESR values.
[0067] 2, the conductive polymer dispersions of Examples 1 to 16 were prepared so that the amount x (wt%) of conductive polymer and the amount y (Vol%) of additive fell within the range Er enclosed by the relational expressions (1) to (4). On the other hand, the conductive polymer dispersions of Comparative Examples 1 to 10 were prepared so that the amount x (wt%) of conductive polymer and the amount y (Vol%) of additive fell below the line segment of the relational expression (3) and fell outside the range Er. Note that Examples 2, 3, 6, 8, 11, 13, and 16 were prepared so that they fell on or near the line segment of the relational expressions (2a) and (4a).
[0068] 2, it was confirmed that the solid electrolytic capacitors produced using the conductive polymer dispersions of Examples 1 to 16 generally had lower initial ESR than the solid electrolytic capacitors produced using the conductive polymer dispersions of Comparative Examples 1 to 10. In other words, it was confirmed that a conductive polymer dispersion in which the amount x (wt %) of conductive polymer and the amount y (Vol %) of additive fall within the range Er enclosed by the relational expressions (1) to (4) reduces the initial ESR of the solid electrolytic capacitor.
[0069] In the conductive polymer dispersions of Comparative Examples 1 to 7, the amount x (wt %) of the conductive polymer and the amount y (Vol %) of the additive were small, and therefore, similarly to Comparative Example 11, gelation did not occur even when the initial conductive polymer dispersion was not concentrated, i.e., the concentration step and the pH adjustment step were omitted, and the additive addition step was performed and the amount x (wt %) of the conductive polymer and the amount y (Vol %) of the additive were adjusted.
[0070] For the conductive polymer dispersions of Comparative Examples 8 to 10, the line segment indicated by relational expression (1) was exceeded, and aggregation occurred in the conductive polymer dispersions, resulting in a significant deterioration in the initial ESR of the solid electrolytic capacitors. It was confirmed that the conductive polymer dispersions of Comparative Examples 8 to 10 gelled within a few minutes when left standing.
[0071] On the other hand, when the amount of conductive polymer x (wt%) and the amount of additive y (Vol%) are within the range Er, as in the conductive polymer dispersions of Examples 1 to 16, the initial conductive polymer dispersion must be concentrated. Therefore, unless the pH adjustment step is followed by the concentration step, the conductive polymer dispersion will gel, and the ESR of the solid electrolytic capacitor cannot be reduced. A solid electrolytic capacitor was fabricated using the gelled conductive polymer dispersion of Comparative Example 7, and the initial ESR was measured, finding that the ESR was 1.5 Ω.
[0072] (Examples 17 to 24) Solid electrolytic capacitors were also fabricated using the conductive polymer dispersions of Examples 17 to 24. The conductive polymer dispersions of Examples 17 to 24 differed from Examples 8, 9, 13, and 16 in the weight ratio of PSS to PEDOT in the conductive polymer dispersion. The weight ratio of PSS to PEDOT in Examples 8, 9, 13, and 16 was PEDOT:PSS = 1:2.5, while the weight ratio of PSS to PEDOT in Examples 17 to 20 was PEDOT:PSS = 1:2.7. The weight ratio of PSS to PEDOT in Examples 21 to 24 was PEDOT:PSS = 1:3.
[0073] Except for the difference in the weight ratio of PSS to PEDOT, the conductive polymer dispersions of Examples 17 and 21 had the same composition as Example 8 and were produced by the same manufacturing method and under the same manufacturing conditions; the conductive polymer dispersions of Examples 18 and 22 had the same composition as Example 9 and were produced by the same manufacturing method and under the same manufacturing conditions; the conductive polymer dispersions of Examples 19 and 23 had the same composition as Example 13 and were produced by the same manufacturing method and under the same manufacturing conditions; and the conductive polymer dispersions of Examples 20 and 24 had the same composition as Example 16 and were produced by the same manufacturing method and under the same manufacturing conditions.
[0074] Then, using the conductive polymer dispersions of Examples 17 to 24, solid electrolytic capacitors having the same configuration as Examples 8, 9, 13, and 16 were produced using the same manufacturing method and under the same manufacturing conditions as Examples 8, 9, 13, and 16. The initial ESR of the solid electrolytic capacitors using the conductive polymer dispersions of Examples 17 to 24 was also measured under the same conditions as Examples 8, 9, 13, and 16. The ESR measurement results for Examples 17 to 24, as well as Examples 8, 9, 13, and 16, are shown in Table 3 below.
[0075] (Table 3)
[0076] From the results of Examples 8, 9, 13, 16, and 17 to 24, it was confirmed that the initial ESR could be reduced even if the weight ratio of PSS to PEDOT was changed. In particular, the ESR reduction effect tended to be greater when the PEDOT:PSS ratio was less than 1:3.
Claims
1. A conductive polymer dispersion comprising: polyethylenedioxythiophene doped with polystyrenesulfonic acid as a conductive polymer; a dispersion medium; and an additive, wherein the amount x (wt%) of the conductive polymer and the amount y (Vol%) of the additive fall within the range enclosed by the following relational expressions (1) to (4): y = -29x + 100 ... (1) y = -34x + 83 ... (2) x = 1 ... (3) y = 5 ... (4) 2. The conductive polymer dispersion according to claim 1, wherein the additive is a polyhydric alcohol.
3. The conductive polymer dispersion according to claim 1 or 2, characterized in that the pH is 3 or more and 6 or less.
4. The conductive polymer dispersion according to claim 1 or 2, wherein a mass ratio of said polystyrene sulfonic acid (PSS) to said polyethylenedioxythiophene (PEDOT) is PEDOT:PSS=less than 1:
3.
5. A method for producing a conductive polymer dispersion comprising an additive addition step of adding an additive, or an additive and an additional dispersion medium, to a conductive polymer dispersion in which a conductive polymer is dispersed in a dispersion medium, the conductive polymer being polyethylenedioxythiophene doped with polystyrenesulfonic acid, and in the additive addition step, the amount x (wt%) of the conductive polymer added and the amount y (Vol%) of the additive added are within the range surrounded by the following relational expressions (1) to (4). y = -29x + 100 ... (1) y = -34x + 83 ... (2) x = 1 ... (3) y = 5 ... (4) 6. The method for producing a conductive polymer dispersion liquid according to claim 5, wherein a mass ratio of said polystyrene sulfonic acid (PSS) to said polyethylene dioxythiophene (PEDOT) is PEDOT:PSS=less than 1:
3.
7. A method for producing a conductive polymer dispersion according to claim 5, comprising: a pH adjustment step of adjusting the pH of the conductive polymer dispersion to 3 or more and 6 or less; and a concentration step of concentrating the conductive polymer dispersion after the pH adjustment step, wherein after the concentration step, in the additive addition step, the amount x (wt %) of the conductive polymer to be added and the amount y (Vol %) of the additive to be added are adjusted to be within the range surrounded by the relational expressions (1) to (4).
8. A method for producing a conductive polymer dispersion liquid according to claim 7, characterized in that the concentrating step is a second concentrating step, and includes a first concentrating step of concentrating the conductive polymer dispersion liquid to a concentration of the conductive polymer in the range of less than 2.6 wt % before the pH adjusting step, the pH adjusting step is performed after the first concentrating step, and in the second concentrating step, the conductive polymer dispersion liquid is further concentrated to a concentration of the conductive polymer in the range of 3.5 wt % or less.
9. The method for producing a conductive polymer dispersion liquid according to any one of claims 5 to 8, wherein the additive is a polyhydric alcohol.
10. A method for producing a solid electrolytic capacitor, comprising forming a solid electrolyte layer between an anode body and a cathode body using the conductive polymer dispersion liquid according to any one of claims 5 to 8.
Citation Information
Patent Citations
Solid electrolytic capacitor
JP2010087014A
Electrolytic capacitor and manufacturing method thereof
JP2013026536A
Production method of fluid dispersion for solid electrolytic capacitor, fluid dispersion for solid electrolytic capacitor, manufacturing method of solid electrolytic capacitor using the fluid dispersion and solid electrolytic capacitor
JP2013055308A
Solid electrolytic capacitor and method for manufacturing the same
JP2013131514A
Electrolytic capacitor
JP2017045868A