Metal resin composite body and method for producing same
The metal-resin composite with carbodiimide-modified polyolefin and thermal fusion achieves strong bonding across a wide temperature range, addressing the weakness of conventional composites by maintaining high adhesive strength at high temperatures and facilitating easy separation at room temperature.
Patent Information
- Application Number
- PCT/JP2024/013016
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional metal-resin composites experience a decrease in adhesive strength at high temperatures, limiting their effectiveness in applications requiring strong bonding over a wide temperature range.
A metal-resin composite is developed using a carbodiimide-modified polyolefin with carbodiimide groups, which is thermally fused with a metal member, providing enhanced adhesive strength at both room temperature and high temperatures, such as 100°C, while allowing easy separation at room temperature.
The composite exhibits superior adhesive strength at high temperatures and easy peelability at room temperature, balancing performance across temperature ranges and maintaining structural integrity during deformation.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Metal-resin composite and method for producing the same
[0001] The present invention relates to a metal-resin composite having excellent adhesive strength between a metal member and a polymer composition, particularly excellent adhesive strength at high temperatures, and a method for producing the same.
[0002] BACKGROUND ART Composites of metals and thermoplastic resins such as polyolefin resins typified by polyethylene and polypropylene are used in a variety of fields, including home appliances, machine parts, electrical parts, and automobile parts.
[0003] In general, polyolefin resins do not contain polar groups in their molecules and therefore have poor adhesive strength to metals. Therefore, as disclosed in Patent Document 1, a method of grafting an unsaturated carboxylic acid such as maleic acid onto polyolefins to improve their affinity with polar resins is widely used.
[0004] Japanese Patent Application Publication No. 50-4144
[0005] However, when used in various fields, sufficient adhesive strength is required over a wide temperature range, and conventional adhesive techniques have the problem of reduced adhesive strength, particularly at high temperatures.
[0006] Therefore, an object of the present invention is to provide a metal-resin composite in which the metal member and the polymer composition have sufficient adhesive strength over a wide temperature range.
[0007] The present invention relates to the following items [1] to
[14] . [1] A metal resin composite comprising a layer (AL) made of a metal member (A) and a layer (BL) made of a polymer composition (B) satisfying the following requirements (i) and (ii): (i) A carbodiimide-modified polyolefin formed by reacting a polyolefin (a) having a group reactive with a carbodiimide group with a carbodiimide group-containing compound (b). (ii) The carbodiimide group is contained in an amount of 0.1 to 50 mmol per 100 g of the polymer composition (B). [2] The metal resin composite according to the above item [1], wherein the content of the carbodiimide-modified polyolefin in the polymer composition (B) is 1% by mass to 40% by mass. [3] The polymer composition (B) further comprises a polymer composition having a density of 0.890 g / cm 3[4] The metal resin composite according to [3] above, wherein the content of the high-density polymer (c) in the polymer composition (B) is 60% by mass to 99% by mass. [5] The polymer composition (B) has a density of 0.890 g / cm or more. 3 [6] The metal resin composite according to any one of the above [1] to [4], wherein the content of the low-density polymer (d) having a density of less than 0.900 g / cm is 10 mass% or less. 3The metal resin composite according to any one of [1] to [5] above, wherein at least a portion of the space between the layer (AL) and the layer (BL) is heat-fused. [7] The metal resin composite according to any one of [1] to [6] above, wherein at least a portion of the space between the layer (AL) and the layer (BL) is heat-fused. [8] The metal resin composite according to [1] to [7] above, wherein at least a portion of the space between the layer (AL) and the layer (BL) is in contact. [9] The metal resin composite according to [8] above, wherein the adhesive strength between the layer (AL) and the layer (BL) at 100°C is greater than the adhesive strength at room temperature.
[10] The metal resin composite according to [3] or [4] above, wherein the high-density polymer (c) comprises a polymer (c-1) having no polar functional group.
[11] The metal resin composite according to [3] or [4] above, wherein the high-density polymer (c) comprises a polymer (c-2) having a polar functional group.
[12] The metal-resin composite according to any one of [1] to
[11] above, wherein the number of carbodiimide groups per molecule of the carbodiimide group-containing compound (b) is 5 or more.
[13] The metal-resin composite according to any one of [1] to
[12] above, wherein the metal member (A) is aluminum.
[14] The method for producing a metal-resin composite according to [7] or [8] above, comprising the steps of contacting a melt of a polymer composition (B) satisfying the following requirements (i) and (ii) with the surface of a layer (AL) made of a metal member (A), and cooling the melt of the layer (AL) made of the polymer composition (B) that has contacted the surface of the layer (AL) made of the metal member (A). (i) The composite comprises a carbodiimide-modified polyolefin formed by reacting a polyolefin (a) having a group reactive with a carbodiimide group with a carbodiimide group-containing compound (b). (ii) The polymer composition (B) contains 0.1 to 50 mmol of carbodiimide groups per 100 g of the polymer composition (B).
[0008] According to the present invention, by using a specific polymer composition containing a carbodiimide group, sufficient adhesive strength can be obtained with a metal member, and a metal resin composite can be provided in which the metal member and the polymer composition have sufficient adhesive strength over a wide temperature range.
[0009] The present invention will be described in further detail below. In this disclosure, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the upper and lower limits. In the numerical ranges described in stages in this disclosure, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in this disclosure, the upper or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In this disclosure, when a composition contains multiple substances corresponding to each component, the amount of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified.
[0010] (Metal Resin Composite) The metal resin composite of the present invention comprises a layer (AL) made of a metal member (A) and a layer (BL) made of a polymer composition (B) described below. In the metal resin composite of the present invention, preferably, at least a portion between the layer (AL) and the layer (BL) is heat-sealed. In the metal resin composite of the present invention, preferably, at least a portion between the layer (AL) and the layer (BL) is in contact with each other.
[0011] Metal-resin composites may be deformed in high-temperature environments (e.g., 100°C) to facilitate metal processing, and may be required to exhibit high adhesive strength that prevents unexpected peeling during deformation. On the other hand, metal-resin composites are widely recycled, and may be required to have adhesive strength that allows easy peeling of the metal and resin while maintaining adhesive strength near room temperature. In other words, metal-resin composites may be required to have higher adhesive strength at high temperatures such as 100°C than at room temperature. According to one embodiment of the present invention, not only is adhesive strength excellent, but peeling of the metal and resin can be performed relatively easily at room temperature, and higher adhesive strength can be exhibited in high-temperature environments such as 100°C than at room temperature.
[0012] <Metal Member (A)> The metal member (A) constituting the metal-resin composite of the present invention is not particularly limited as long as it is a member composed of a metal, and alloys and oxides of various metals such as iron, nickel, chromium, cobalt, gold, silver, copper, tin, lead, and aluminum can be used. Iron and aluminum are preferred because they exhibit better adhesion to the layer (BL) composed of the polymer composition (B). Aluminum is preferred because it exhibits particularly good adhesion to the layer (BL) composed of the polymer composition (B).
[0013] The shape of the metal member (A) is not particularly limited, and various shapes can be adopted depending on the use of the metal-resin composite. The surface of the metal member (A) according to the present invention may be subjected to a corona treatment or an ozone treatment.
[0014] <Polymer Composition (B)> The polymer composition (B) constituting the layer (BL) constituting the metal resin composite of the present invention satisfies the following requirements (i) to (ii).
[0015] <Requirement (i)> The polymer composition (B) according to the present invention contains a carbodiimide-modified polyolefin formed by reacting a polyolefin (a) having a group reactive with a carbodiimide group with a carbodiimide group-containing compound (b).
[0016] The content of the carbodiimide-modified polyolefin in the polymer composition (B) is preferably 1% by mass to 40% by mass, more preferably 3% by mass to 35% by mass, and even more preferably 5% by mass to 30% by mass. When the content of the carbodiimide-modified polyolefin is within the above range, the balance between the adhesive strength at room temperature and the adhesive strength in a high-temperature environment (e.g., 100°C) tends to be excellent.
[0017] The density of the carbodiimide-modified polyolefin (measured in accordance with JIS K7112) is preferably 0.890 to 0.970 g / cm 3 and more preferably 0.890 to 0.950 g / cm 3 and more preferably 0.890 g to 0.940 g / cm 3When the density of the carbodiimide-modified polyolefin is within the above range, the balance between the adhesive strength at room temperature and the adhesive strength in a high-temperature environment (e.g., 100°C) tends to be excellent. This is presumably because the components are less likely to melt in a high-temperature environment.
[0018] [Polyolefin (a)] The polyolefin (a) can be obtained by introducing a compound (m) having a group reactive with a carbodiimide group into a polyolefin. The polyolefin (a) may be used alone or in combination of two or more types.
[0019] Compounds (m) having a group reactive with a carbodiimide group include compounds having a group containing an active hydrogen atom reactive with a carbodiimide group. Specific examples include compounds having a group derived from a carboxylic acid, an amine, an alcohol, a thiol, or the like. Among these, compounds having a group derived from a carboxylic acid are preferably used, and unsaturated carboxylic acids and / or their derivatives are particularly preferred. In addition to compounds having a group containing an active hydrogen atom, compounds having a group that can be easily converted into a group containing an active hydrogen atom by water or the like can also be preferably used. Specific examples include compounds having an epoxy group or a glycidyl group.
[0020] The compound (m) having a group reactive with a carbodiimide group may be one type alone or two or more types.
[0021] The unsaturated carboxylic acid and / or derivative thereof used as the compound (m) having a group reactive with a carbodiimide group can be an unsaturated compound having one or more carboxylic acid groups, preferably an unsaturated compound having one or more carboxylic acid anhydride groups, and a derivative thereof. Examples of the unsaturated group include a vinyl group, a vinylene group, and an unsaturated cyclic hydrocarbon group. Specific examples of the compound include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, norbornene dicarboxylic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid, as well as their acid anhydrides and derivatives (e.g., acid halides, amides, imides, and esters). Specific examples of the compound include malenyl chloride, malenylimide, maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride, dimethyl maleate, monomethyl maleate, diethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconic acid, dimethyl tetrahydrophthalate, dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glycidyl (meth)acrylate, aminoethyl methacrylate, and aminopropyl methacrylate.
[0022] When an unsaturated carboxylic acid and / or a derivative thereof is used as the compound (m) having a group reactive with a carbodiimide group, it may be used alone or in combination of two or more. Among these, maleic anhydride, (meth)acrylic acid, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride, hydroxyethyl (meth)acrylate, glycidyl methacrylate, and aminopropyl methacrylate are preferred. Furthermore, dicarboxylic anhydrides such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride are particularly preferred.
[0023] As a method for introducing the compound (m) having a group reactive with a carbodiimide group into a polyolefin, a well-known method can be adopted. For example, a method for graft copolymerizing the compound (m) having a group reactive with a carbodiimide group onto the polyolefin main chain, or a method for radical copolymerizing an olefin with the compound (m) having a group reactive with a carbodiimide group can be exemplified.
[0024] The following will specifically explain the graft copolymerization and the radical copolymerization separately.
[0025] <Graft Copolymerization> The polyolefin (a) having a group reactive with a carbodiimide group can be obtained by graft copolymerizing a compound (m) having a group reactive with a carbodiimide group onto the polyolefin main chain.
[0026] (Polyolefin Main Chain) The polyolefin used as the polyolefin main chain is a polymer primarily composed of an aliphatic α-olefin having 2 to 20 carbon atoms, a cyclic olefin, or a non-conjugated diene, preferably a polymer primarily composed of an aliphatic α-olefin having 2 to 10 carbon atoms, and more preferably aliphatic α-olefin having 2 to 8 carbon atoms. These olefins may be used alone or in combination of two or more. In the case of a copolymer, the content of the olefin serving as a comonomer is not particularly limited as long as the effects of the present invention are obtained, but is typically 50 mol% or less, preferably 40 mol% or less, and more preferably 30 mol% or less. Among polyolefins within this range, crystalline polyolefins such as polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, and copolymers of these α-olefins are preferred, with polyethylene, polypropylene, or propylene-ethylene copolymers being more preferred. Furthermore, both isotactic and syndiotactic structures can be used, and there are no particular restrictions on the stereoregularity.
[0027] The polyolefin used in the present invention may be a polymer obtained using only fossil fuel-derived olefins such as fossil fuel-derived propylene as a raw material, a polymer obtained using only biomass-derived olefins such as biomass-derived propylene as a raw material, or a polymer obtained using a mixture of fossil fuel-derived olefins and biomass-derived olefins as a raw material, or may be a mixture of two or more of these polymers.
[0028] Here, fossil fuels refer to petroleum, coal, natural gas, shale gas, and other substances that have been fossilized by the volume and pressure of the remains of plants and animals over hundreds of millions of years, and fossil fuel-derived olefins are olefins obtained from these fossil fuels. 14 Since the time has passed much longer than the half-life of the C isotope, 5,730 years, it is unlikely that carbon from fossils will be present. 14 C is not detected.
[0029] Biomass refers to any renewable natural raw material and its residue, whether plant-derived or animal-derived, including fungi, yeast, algae, and bacteria, and biomass-derived olefins refer to olefins obtained from this biomass. Biomass-derived carbon refers to carbon derived from 14 Contains a certain amount of C isotope (10 -12 (Proportion of the same).
[0030] The density of the polyolefin used for graft modification (measured in accordance with JIS K7112) is not particularly limited as long as the effects of the present invention can be obtained, but it is usually 0.8 to 1.10 g / cm 3 , preferably 0.8 to 1.05 g / cm 3 , more preferably 0.8 to 1.00 g / cm 3 The melt flow rate (MFR) at 230°C under a load of 2.16 kg according to ASTM D1238 is not particularly limited as long as the effects of the present invention are obtained, but is usually 0.01 to 500 g / 10 min, preferably 0.05 to 200 g / 10 min, and more preferably 0.1 to 100 g / 10 min. If the density and MFR are within these ranges, the density and MFR of the graft copolymer after modification will also be approximately the same, making it easy to handle.
[0031] The crystallinity of the polyolefin used for graft modification is not particularly limited as long as the effects of the present invention can be obtained, but is usually 2% or more, preferably 5% or more, and more preferably 10% or more. If the crystallinity is in this range, the graft copolymer after modification will be excellent in handleability.
[0032] The number average molecular weight (Mn) of the polyolefin used for graft modification, as measured by gel permeation chromatography (GPC), is preferably 5,000 to 500,000, and more preferably 10,000 to 100,000. A number average molecular weight (Mn) within this range provides excellent handleability. For ethylene-based polyolefins, the number average molecular weight can be determined in polyethylene terms if the comonomer content is 10 mol% or less, or in ethylene-propylene terms (based on an ethylene content of 70 mol%) if the comonomer content is 10 mol% or more.
[0033] The polyolefins described above can be produced by any known method, for example, by polymerization using a titanium catalyst, a vanadium catalyst, a metallocene catalyst, etc. The polyolefins used for graft modification may be in the form of either a resin or an elastomer, and both isotactic and syndiotactic structures can be used, with no particular limitation on stereoregularity. Commercially available polymers can also be used as they are.
[0034] (Graft Polymerization Method) When the polyolefin (a) having a group reactive with a carbodiimide group is obtained by graft copolymerization, the polyolefin that becomes the above-mentioned graft main chain is graft copolymerized with a compound (m) having a group reactive with a carbodiimide group, and further with other ethylenically unsaturated monomers and the like as necessary, in the presence of a radical initiator.
[0035] The method for grafting the compound (m) having a group reactive with a carbodiimide group onto the polyolefin main chain is not particularly limited, and any conventionally known graft polymerization method such as a solution method or a melt-kneading method can be used.
[0036] The graft amount of the compound (m) having a group reactive with a carbodiimide group is usually 0.05 to 20 mass%, preferably 0.05 to 10 mass%, more preferably 0.05 to 5 mass%, and even more preferably 0.05 to 3 mass%, based on 100 mass% of the polyolefin (a). The graft amount of the compound (m) is the net graft amount measured after removing the free compound (m) from the polyolefin (a). The graft amount is 13 C-NMR, 1 The acid value can be measured by known means such as H-NMR measurement. When a monomer having an acidic functional group, such as an unsaturated carboxylic acid or an anhydride thereof, is used as the compound (m), the acid value can also be used as a measure of the amount of functional group introduced into the polyolefin (a). When maleic anhydride is used, the acid value can be measured by an infrared spectrophotometer, usually at 1780 to 1790 cm ―1The amount of grafting can also be determined based on the absorption spectrum of the carbonyl group of maleic anhydride detected in the vicinity.
[0037] <Radical copolymerization> The polyolefin (a) having a group reactive with a carbodiimide group can also be obtained by radical copolymerization of an olefin with a compound (m) having a group reactive with a carbodiimide group. The olefin may be the same as the olefin used to form the polyolefin that serves as the graft main chain, and the compound (m) having a group reactive with a carbodiimide group is also as described above.
[0038] The method for copolymerizing the olefin with the compound (m) having a group reactive with a carbodiimide group is not particularly limited, and any conventionally known radical copolymerization method can be used.
[0039] (Configuration of Polyolefin (a)) The content of the residue of the compound (m) having a group reactive with a carbodiimide group in the polyolefin (a) having a group reactive with a carbodiimide group is usually 0.1 to 10 mass%, preferably 0.1 to 8.0 mass%, and more preferably 0.1 to 6.0 mass%. If the content of the residue of the compound (m) having a group reactive with a carbodiimide group is within the above range, it is preferable because the polyolefin (a) can be suitably crosslinked with the carbodiimide group-containing compound (b) to produce the polymer composition (B).
[0040] The density of the polyolefin (a) having a group reactive with a carbodiimide group (measured in accordance with JIS K7112) is preferably 0.890 to 0.970 g / cm 3 and more preferably 0.890 to 0.950 g / cm 3 and more preferably 0.890 g to 0.940 g / cm 3 When the density of the polyolefin (a) is within the above range, the density of the polymer composition (B) described below is easily achieved, and there is a tendency for the balance between the adhesive strength at room temperature and the adhesive strength in a high-temperature environment (e.g., 100°C) to be excellent. This is presumably because a decrease in adhesive strength due to melting of the components in a high-temperature environment is less likely to occur.
[0041] The melt flow rate (MFR, in accordance with ASTM D1238, 230°C, 2.16 kg load) of the polyolefin (a) having a group reactive with a carbodiimide group is not particularly limited as long as the effects of the present invention can be obtained, but is usually 0.01 to 500 g / 10 min, preferably 0.05 to 200 g / 10 min, and more preferably 0.01 to 150 g / 10 min.
[0042] (Carbodiimide Group-Containing Compound (b)) The carbodiimide group-containing compound (b) is a polycarbodiimide having a repeating unit represented by the following general formula (1): The carbodiimide group-containing compound (b) may be a single compound or a combination of two or more compounds.
[0043] -N=C=N-R 1 ...(1) [In the formula, R 1 represents a divalent organic group having 2 to 40 carbon atoms.] Polycarbodiimides can be produced by carrying out a decarboxylation condensation reaction of an organic diisocyanate, such as an aliphatic diisocyanate, an aromatic diisocyanate, or an alicyclic diisocyanate, in the presence of a condensation catalyst, either without a solvent or in an inert solvent. For example, diisocyanates such as hexamethylene diisocyanate, 4,4-diphenylmethane diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, xylylene diisocyanate, cyclohexane-1,4-diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and isophorone diisocyanate can be used alone or in combination. In the decarboxylation condensation reaction, the degree of polymerization of the polycarbodiimide can be adjusted by selecting the catalyst, reaction temperature, end-capping agent, etc. The degree of polymerization is usually 2 to 40, preferably 4 to 20. Examples of the end-capping agent that can be used include monoisocyanates such as phenyl isocyanate, tolyl isocyanate, and naphthyl isocyanate, as well as active hydrogen compounds such as methanol, ethanol, diethylamine, cyclohexylamine, succinic acid, benzoic acid, and ethyl mercaptan. Examples of the condensation catalyst that can be used include alcoholates of titanium, hafnium, zirconium, sodium, calcium, and the like, and organic phosphorus compounds such as phosphorene oxide.
[0044] The polystyrene-equivalent number average molecular weight (Mn) of the carbodiimide group-containing compound (b) determined by gel permeation chromatography (GPC) is not particularly limited as long as the effects of the present invention can be obtained, but is usually 400 to 500,000, preferably 700 to 10,000, and more preferably 1,000 to 8,000. When the number average molecular weight (Mn) is within this range, the polymer composition (B) has excellent adhesive strength, which is preferable.
[0045] The carbodiimide group-containing compound (b) may contain a monocarbodiimide in a polycarbodiimide, and may be used alone or in combination of a plurality of compounds.
[0046] As the carbodiimide group-containing compound (b), commercially available carbodiimide group-containing compounds can be used as they are, such as Carbodilite (registered trademark) HMV-8CA, HMV-15CA, and Carbodilite (registered trademark) LA1 manufactured by Nisshinbo Chemical Inc.
[0047] The more the number of carbodiimide groups in one molecule of carbodiimide compound, the more reaction points with polyolefin (a) there are, so that it can adhere more firmly to the metal layer.For this reason, the number of carbodiimide groups in one molecule of carbodiimide group-containing compound (b) is preferably 5 or more, more preferably 10 or more.In addition, the upper limit of the number of carbodiimide groups in one molecule of carbodiimide group-containing compound (b) is not particularly limited as long as the effect of the present invention can be obtained, but as the number of carbodiimide groups in one molecule increases, the amount of carbodiimide compound added increases, and the raw material cost increases, so that in consideration of cost, it is usually 30.
[0048] The carbodiimide group content in the carbodiimide group-containing compound (b) is 13 It can be measured by C-NMR, IR, titration, etc., and can be determined as the carbodiimide group equivalent. 13 C-NMR: 130-142 ppm, IR: 2130-2140 cm 1It is possible to observe a peak attributable to the carbodiimide group.
[0049] 13 C-NMR measurement is carried out, for example, as follows. That is, 0.35 g of a sample is heated and dissolved in 2.0 ml of hexachlorobutadiene. After filtering this solution through a glass filter (G2), 0.5 ml of deuterated benzene is added and the solution is placed in an NMR tube with an inner diameter of 10 mm. Then, using a JEOL GX-500 NMR measurement apparatus, the sample is heated and dissolved in 2.0 ml of hexachlorobutadiene. 13 C-NMR measurement is performed with an accumulation count of 10,000 or more.
[0050] (Reaction of polyolefin (a) having a group reactive with a carbodiimide group with carbodiimide group-containing compound (b)) The polyolefin having a carbodiimide group contained in polymer composition (B) is obtained by reacting polyolefin (a) having a group reactive with a carbodiimide group with carbodiimide group-containing compound (b) preferably at a temperature of 230° C. or higher. Specifically, polymer composition (B) can be obtained by melt-kneading, such as melt modification, but is not limited to this method.
[0051] An example of melt mixing is shown below. The method for reacting a polyolefin (a) having a group reactive with a carbodiimide group with a carbodiimide group-containing compound (b), preferably at 230°C or higher, is not particularly limited, but examples include a method in which the polyolefin (a) having a group reactive with a carbodiimide group and the carbodiimide group-containing compound (b) are charged and kneaded in, for example, a Henschel mixer, a V-type blender, a tumbler blender, a ribbon blender, or the like, and then melt-kneaded in a single-screw extruder, a multi-screw extruder, a kneader, a Banbury mixer, or the like. Among these, the use of a device with excellent kneading performance, such as a multi-screw extruder, a kneader, or a Banbury mixer, is preferred, since it allows the adhesive polymer composition (B) to be obtained in which the components are more uniformly dispersed and reacted.
[0052] The polyolefin (a) having a group reactive with a carbodiimide group and the carbodiimide group-containing compound (b) can be supplied either by premixing them and then supplying them from a hopper, or by supplying some of the components from the hopper and then supplying the other components from a supply port located anywhere between the vicinity of the hopper and the tip of the extruder.
[0053] The temperature at which the components are melted and kneaded can be equal to or higher than the highest melting point of the components to be mixed, but specifically, the melt-kneading is usually carried out at a temperature in the range of 180 to 320°C, preferably 230 to 300°C, and more preferably 235 to 280°C.
[0054] The reaction rate between the polyolefin (a) and the carbodiimide group-containing compound (b) can be evaluated by the following method.
[0055] After preparing heat-pressed sheets for the polyolefin (a) (reference) having a group reactive with a carbodiimide group and the polymer composition containing a polyolefin having a carbodiimide group, infrared absorption is measured using an infrared absorption analyzer. From the obtained chart, the difference between the absorbance attributable to the group reactive with the carbodiimide group in the polyolefin (a), the absorbance attributable to the group reactive with the carbodiimide group in the polyolefin (a), and the absorbance attributable to the group reactive with the carbodiimide group in the polymer composition is compared, and the reaction rate can be calculated using the following formula (2). When maleic anhydride is used as the group reactive with the carbodiimide group, the absorbance attributable to the group reactive with the carbodiimide group in the polyolefin (a) is 1790 cm -1 Absorbance in the vicinity can be used.
[0056] Reaction rate (%) = {X / Y} × 100 (2) X: difference between the absorbance attributable to groups reactive with carbodiimide groups in the polyolefin (a) and the absorbance attributable to groups reactive with carbodiimide groups in the polymer composition Y: absorbance attributable to groups reactive with carbodiimide groups in the polyolefin (a) The reaction rate of the polymer composition (B) determined by the above method is usually in the range of 40 to 100%, preferably 60 to 100%, and more preferably 80 to 100%.
[0057] <Requirement (ii)> The polymer composition (B) contains carbodiimide groups in an amount of 0.1 to 50 mmol per 100 g of the polymer composition (B).
[0058] The polymer composition (B) according to the present invention contains a carbodiimide-modified polyolefin having carbodiimide groups, and the amount of the carbodiimide groups is 0.1 to 50 mmol, preferably 0.2 to 40 mmol, and more preferably 0.5 to 30 mmol per 100 g of the polymer composition (B). When the amount of carbodiimide groups in the polymer composition (B) is within the above range, the polymer composition (B) has excellent adhesive strength to the metal member (A) at room temperature and under high-temperature conditions (e.g., 100°C), and crosslinking of the polyolefin (a) can be suppressed, which is preferable.
[0059] The content of carbodiimide groups in the polymer composition is 13 It can be measured by C-NMR, IR, titration, etc., and can be determined as the carbodiimide group equivalent. 13 C-NMR: 130-142 ppm, IR: 2130-2140 cm 1 It is possible to observe a peak attributable to the carbodiimide group. 13 The C-NMR measurement is carried out, for example, by the measurement method described above for the carbodiimide group content in the carbodiimide group-containing compound (b) and the measurement method described in the Examples.
[0060] The polymer composition (B) according to the present invention is produced by reacting the carbodiimide groups (NCN) of the polycarbodiimide with the compound (m) having a group reactive with the carbodiimide group, as described above, and some of the carbodiimide groups are consumed during the reaction, and the carbodiimide group residues connected to the polyolefin group as the same molecular chain contribute to the adhesion to the polymer (α) having an NH group at the molecular end. If the content of the carbodiimide groups exceeds the above range, excess free carbodiimide groups will be present relative to the polyolefin (a) having a group reactive with the carbodiimide group, and the adhesion performance to the metal member (A) and moldability will be reduced.
[0061] Although carbodiimide groups are converted to urea groups by absorbing water, even urea groups exhibit high reactivity with semi-aromatic polyamides. Therefore, the polymer composition (B) according to the present invention may contain polyolefins in which carbodiimide groups have been converted to urea groups by, for example, water in the atmosphere, which is one of the preferred embodiments of the present invention.
[0062] The polymer composition (B) further has a density of 0.890 g / cm 3 It is preferable that the polymer composition (B) contains a high-density polymer (c) having a density of 0.900 g / cm or more. It is also preferable that the density of the polymer composition (B) is 0.900 g / cm or more. It is also preferable that the content of a low-density polymer (d) having a density of less than 0.890 g / cm in the polymer composition (B) is 10 mass% or less.
[0063] The content of the high-density polymer (c) in the polymer composition (B) is preferably 60% by mass to 99% by mass.
[0064] The high-density polymer (c) preferably contains a polymer (c-1) having no polar functional group, and also preferably contains a polymer (c-2) having a polar functional group.
[0065] Examples of the polymer (c-2) having a polar functional group include the polymers exemplified in the "other layers" described below (excluding polyolefins), as well as polymers used in the "polyolefin layer (Z-1)" in which a monomer having a polar group (e.g., a carbonyl group, a hydroxyl group, an ether-bonding group, etc.) is copolymerized with a polyolefin.
[0066] The polymer (c-1) having no polar functional group is a polyolefin, and examples thereof include the polymers (1) to (12) given below under "Specific examples of polyolefins."
[0067] To the polymer composition (B) of the present invention, it is also possible to add known additives used in the field of polyolefins, such as tackifiers, process stabilizers, heat stabilizers, heat aging agents, fillers, etc.
[0068] In the present invention, it is particularly preferable to blend a tackifier for the purpose of imparting tackiness. Examples of tackifiers include rosin derivatives, terpene resins, petroleum resins, and hydrogenated versions of these. Among these, hydrogenated terpene resins and hydrogenated petroleum resins are preferred. The tackifier is not particularly limited as long as it exhibits the effects of the present invention, but it is preferable to blend, for example, 0 to 30% by mass of the tackifier relative to 100% by mass of the polymer composition (B).
[0069] <<Metal Resin Composite>> The metal resin composite of the present invention comprises a layer (AL) made of the metal member (A) and a layer (BL) made of the polymer composition (B).
[0070] In one embodiment of the present invention, the metal-resin composite is characterized in that the adhesive strength between the metal member (A) and the polymer composition (B) at 100°C is higher than the adhesive strength at 23°C.
[0071] The metal-resin composite of the present invention may have, in addition to the layer (AL) made of the metal member (A) and the layer (BL) made of the polymer composition (B), another layer (X) on the surface of the layer (BL) made of the polymer composition (B).
[0072] <Other Layer (X)> The other layer (X) that may constitute the metal-resin composite of the present invention is a layer different from the layer (BL) of the polymer composition (B). The polymer forming the other layer (X) is not particularly limited as long as it achieves the effects of the present invention, but examples include polyolefins, polyketones, polyesters, aliphatic polyamides, semi-aromatic polyamides, liquid crystal polymers, polysaccharide derivatives, polyethers, polyurethanes, ethylene-vinyl alcohol copolymers, polyvinyl alcohols, ionomers, ethylene-acrylic acid copolymers, ethylene-vinyl acetate copolymers, polycarbonates, polyphenylene sulfides, polyphenylene ethers, polyacetals, polysulfones, polyarylates, polyaryletherketones, polyimides, and modified fluororesins. Such polymers may be used alone or in combination of two or more. Furthermore, such polymers may be polymers having acidic functional groups such as carbonyl groups, carboxy groups, and sulfonic acid groups.
[0073] (Polyolefin Layer (Z-1)) One of the preferred examples of the layer (Z) constituting the metal resin composite of the present invention is to have a polyolefin layer (Z-1).
[0074] The polyolefin layer (Z-1) comprises a polyolefin. Examples of such polyolefins include homopolymers and copolymers of α-olefins having 2 to 20 carbon atoms. The polyolefins may be composed of one type alone or two or more types. Specific examples of α-olefins include ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene. Furthermore, the polyolefin may be copolymerized with a small amount, for example, 10 mol % or less, of a monomer other than the α-olefin. Examples of such other monomers include, but are not limited to, a polar group (e.g., a carbonyl group, a hydroxyl group, an ether bond, etc.) and a monomer having a polymerizable carbon-carbon double bond in the molecule.
[0075] Specific examples of polyolefins include, for example, (1) ethylene homopolymers (the production method may be either a low-pressure method or a high-pressure method), (2) ethylene-propylene copolymers of 99 to 80 mol% ethylene and 1 to 20 mol% propylene, preferably ethylene-propylene copolymers of 95 to 85 mol% ethylene and 5 to 15 mol% propylene, (3) ethylene-1-butene copolymers of 99 to 80 mol% ethylene and 1 to 20 mol% 1-butene, preferably ethylene-1-butene copolymers of 95 to 85 mol% ethylene and 5 to 15 mol% 1-butene, (4) ethylene-1-octene copolymers of 99 to 80 mol% ethylene and 1 to 20 mol% 1-octene, preferably ethylene-1-octene copolymers of 97 to 85 mol% ethylene and 3 to 15 mol% 1-octene, (5) ethylene-based copolymers such as copolymers of ethylene and 10 mol% or less of other α-olefins (excluding propylene, 1-butene, and 1-octene) or vinyl monomers (for example, vinyl acetate, ethyl acrylate, etc.); (6) propylene homopolymers; (7) random copolymers of propylene and 30 mol% or less of other α-olefins, preferably random copolymers of propylene and 20 mol% or less of other α-olefins; (8) block copolymers of propylene and 40 mol% or less of other α-olefins; (9) 1-butene homopolymers; (10) random copolymers of 1-butene and 10 mol% or less of other α-olefins; (11) 4-methyl-1-pentene homopolymers; (12) random copolymers of 4-methyl-1-pentene and 20 mol% or less of other α-olefins.
[0076] Among these, preferred are homopolymers and copolymers such as (2) ethylene-propylene copolymers of 95 to 85 mol % of ethylene and 5 to 15 mol % of propylene, (3) ethylene-1-butene copolymers of 95 to 85 mol % of ethylene and 5 to 15 mol % of 1-butene, (4) ethylene-1-octene copolymers of 97 to 85 mol % of ethylene and 3 to 15 mol % of 1-octene, (5) ethylene-based copolymers such as copolymers of ethylene and 10 mol % or less of other α-olefins (excluding propylene, 1-butene, and 1-octene) or vinyl monomers (e.g., vinyl acetate, ethyl acrylate, etc.), (6) propylene homopolymers, (7) random copolymers of propylene and 20 mol % or less of other α-olefins, and (8) block copolymers of propylene and 40 mol % or less of other α-olefins.
[0077] <Configuration of Laminate> The metal-resin composite of the present invention may be a laminate. The laminate of the present invention has a layer (AL) made of a metal member (A) and a layer (BL) made of a polymer composition (B) that is in contact with the layer (AL) at least partially made of the metal member (A). The first laminate is preferably a laminate in which a layer (Z), preferably a polyolefin layer (Z-1), and a layer (AL) are laminated via a layer (BL). When the layer designation is omitted, a laminate having a three-type three-layer structure of Z / BL / AL and a three-type five-layer structure of AL / BL / Z / BL / AL or Z / BL / AL / BL / Z are more preferred, but are not limited thereto.
[0078] The thickness of the layer (AL) made of the metal member (A) is usually 0.005 to 3 mm, preferably 0.01 to 0.5 mm. The thickness of the layer (BL) made of the polymer composition (B) is usually 0.005 to 3 mm, preferably 0.01 to 0.5 mm. The thickness of the layer (Z) is usually 0.01 to 100 mm, preferably 0.03 to 2 mm. The thickness of the laminate having a three-type three-layer structure of X / Y / Z is usually 0.02 to 106 mm, preferably 0.05 to 3 mm. When there are multiple layers (AL) made of the metal member (A), multiple layers (BL) made of the polymer composition (B), and multiple layers (Z), the thickness of each layer can be determined by referring to the above.
[0079] <Metal Resin Composite Manufacturing Method> As the method for manufacturing the metal resin composite of the present invention, various known manufacturing methods can be used, but one of the manufacturing methods includes a step of contacting a melt of the polymer composition (B) with the surface of the layer (AL) made of the metal member (A), and a step of cooling the layer (BL) made of the melt of the polymer composition (B) that has contacted the surface of the layer (AL) made of the metal member (A). One aspect of this method includes forming the polymer composition (B) into a layer in advance, specifically, bonding the layer made of the metal member (A) and the layer (BL) made of the polymer composition (B) obtained by pre-molding, and then heating and melting the layer (BL) made of the polymer composition (B), and then cooling the layer (BL) to produce a metal resin composite.
[0080] In the method for producing a metal resin composite of the present invention, the method for bringing the melt of the polymer composition (B) into contact can be any of various known methods. Specifically, there can be employed a method of injection molding the melt of the polymer composition (B) onto the surface of the layer (AL) consisting of the metal member (A), a method of previously fitting the layer (AL) consisting of the metal member (A) in a mold and then closing the mold to inject the polymer composition (B), a method of extrusion coating the surface of the layer (AL) consisting of the metal member (A) with the polymer composition (B), and a method of hot pressing a film of the polymer resin composition (B) onto the surface of the layer (AL) consisting of the metal member (A).
[0081] <Uses of Metal-Resin Composite> The metal-resin composite of the present invention can be used, for example, for food packaging applications such as food containers and beverage containers, for medicine packaging applications such as cosmetic bottles and shampoo bottles, for industrial materials such as automobile parts, fuel pipes, gas pipes, hot water pipes, ink tubes and liquid transport tubes, and for building materials such as decorative sheets, without being particularly limited thereto.
[0082] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way as long as it does not depart from the gist of the invention.
[0083] [Various Measurement Methods] In the present examples, measurements were carried out according to the following methods.
[0084] [Melt Flow Rate (MFR)] Measurement was carried out in accordance with ASTM D1238 at 230°C under a load of 2.16 kg.
[0085] [Density] The density was measured in accordance with JIS K7112.
[0086] [Number Average Molecular Weight of Carbodiimide Group-Containing Compound] The number average molecular weight of the carbodiimide group-containing compound was measured by GPC (gel permeation chromatography) using tetrahydrofuran as a solvent (mobile phase) at a column temperature of 40°C (polystyrene equivalent, Mw: weight average molecular weight, Mn: number average molecular weight). The molecular weight of the standard polystyrene was 580≦Mw≦7×10 6 For the polymer, polystyrene PS-1 manufactured by Agilent Technologies Inc. (formerly Polymer Laboratories Limited) was used.
[0087] [Carbodiimide Group Content] The carbodiimide group content was calculated from the charged amount.
[0088] [Graft Amount of Maleic Anhydride] The graft amount of maleic anhydride was measured by the following method using FT-IR.
[0089] For FT-IR measurement, the sample was heat-pressed at 250°C for 3 minutes to prepare a sheet, and then measured by a transmission method using an infrared spectrophotometer (manufactured by JASCO Corporation, FT-IR410 model) at 1790 cm -1 The infrared absorption spectrum was measured at a resolution of 2 cm. -1 The number of integrations was set to 32.
[0090] [Reaction rate (%) between polyolefin (a) and carbodiimide group-containing compound (b)] The reaction rate (%) is the graft amount of maleic anhydride measured for the adhesive polymer composition and the polyolefin (a) by FT-IR (the absorbance (at 1790 cm) derived from maleic anhydride in the polymer composition). -1 ) and the absorbance due to maleic anhydride in polyolefin (a), calculated according to the above formula (2).
[0091] [Metal Member] In the examples and comparative examples, the following aluminum sheets were used.
[0092] Aluminum sheet having a thickness of 200 μm and a width of 15 mm [Resin member] In the comparative example, the following resins were used.
[0093] EVOH (EVAL F101A, manufactured by Kuraray Co., Ltd.) 200 μm thick, 15 mm wide Polyamide 6 (Amilan CM1021XF, manufactured by Toray Industries, Inc.) 200 μm thick, 15 mm wide PET (Mitsui PET J125, manufactured by Mitsui Chemicals, Inc.) [Production of Resin Composite] A metal member or a resin member and a polymer composition were superimposed in a layer structure of metal member or resin member / resin composition / metal member or resin member, and then a three-layer resin composite (laminate) was produced in a press molding machine set at a temperature of 200° C. under the conditions of preheating for 6 minutes, pressing at a pressure of 3.9 MPa for 4 minutes, and cooling for 3 minutes.
[0094] [Adhesion Strength of Resin Composite] The obtained resin composite was cut into a width of 15 mm, and the adhesive strength (unit: N / 15 mm) at the interface between the member and the layer made of the polymer composition (including carbodiimide-modified polypropylene, etc.) was measured using a tensile tester using the 180° peel method in an atmosphere of room temperature (23°C) and an atmosphere of 100°C. In addition, the obtained resin composite was retorted in hot water at 121°C for 30 minutes, and the adhesive strength was measured in an atmosphere of room temperature in the same manner as above. The crosshead speed was 300 mm / min.
[0095] [Polyolefins Used] The polyolefins used in the examples and comparative examples are listed below. Unless otherwise specified, all of the polyolefins used were commercially available products.
[0096] (1) PP-1: Polypropylene (random PP, MFR: 7 g / 10 min, density: 0.910 g / cm 3 (2) MAH-PP-2: Maleic anhydride modified polypropylene (MFR: 6 g / 10 min, density: 0.890 g / cm 3, maleic anhydride graft amount: 0.15%, manufactured by Mitsui Chemicals, Inc.) Example 1 Production of Polyolefin (a) Having a Group Reactive with a Carbodiimide Group 100 parts by weight of PP-1 were mixed with 1 part by weight of maleic anhydride (manufactured by Wako Pure Chemical Industries, Ltd., hereinafter abbreviated as MAH) and 0.25 parts by weight of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3 (manufactured by NOF Corporation, trade name Perhexyne (registered trademark) 25B), and the mixture was extruded using a twin-screw kneader (manufactured by The Japan Steel Works, Ltd., TEX-30, L / D: 40, vacuum vent used) at a cylinder temperature of 220°C, a screw rotation speed of 200 rpm, and a discharge rate of 80 g / min to obtain maleic acid-modified polypropylene (hereinafter abbreviated as MAH-PP-1). The density of MAH-PP-1 was 0.915 g / cm 3 It was.
[0097] The obtained MAH-PP-1 was dissolved in xylene, and then the obtained xylene solution was poured into acetone to reprecipitate and purify MAH-PP-1. The graft amount of maleic anhydride was measured by FT-IR and was found to be 0.7 wt%.
[0098] <Production of Polymer Composition (B-1)> 90 parts by weight of PP-1, 10 parts by weight of the MAH-PP-1 produced above, and 1.7 parts by weight of a carbodiimide group-containing compound (manufactured by Nisshinbo Chemical Inc., trade name Carbodilite (registered trademark) HMV-8CA, carbodiimide group equivalent 278, number average molecular weight 2100, number of carbodiimide groups per molecule 9) were mixed and extruded using a twin-screw kneader (manufactured by The Japan Steel Works, Ltd., TEX-30, L / D=40, vacuum vent used) at a cylinder temperature of 250°C, a screw rotation speed of 200 rpm, and a discharge rate of 80 g / min, to produce a polymer composition (B-1) containing carbodiimide-modified polypropylene (CDI-PP-1).
[0099] The resulting polymer composition (B-1) had an MFR (230°C, 2.16 kg load) of 3 g / 10 min and a density of 0.910 g / cm 3 According to the FT-IR analysis, CDI-PP-1 exhibited a maleic anhydride peak (1790 cm -1) had disappeared, the ratio of the difference (X) between the absorbance attributable to the group reactive with the carbodiimide group in MAH-PP-1 and the absorbance attributable to the group reactive with the carbodiimide group in CDI-PP-1 to the absorbance (Y) attributable to the group reactive with the carbodiimide group in MAH-PP-1 was 1, and therefore the reaction rate between MAH-PP-1 and the carbodiimide group-containing compound was 100%. The carbodiimide group content was 6.01 mmol (calculated from the charged amount) per 100 g of the polymer composition (B-1). Furthermore, the polymer composition (B-1) contained 88.5 mass% of PP-1 and 11.5 mass% of carbodiimide-modified polypropylene (CDI-PP-1). The density of the carbodiimide-modified polypropylene (CDI-PP-1) was 0.909 g / cm 3 there were.
[0100] <Production of Metal Resin Composite and Measurement of Adhesion Strength> A metal resin composite was produced using the obtained polymer composition (B-1) by the method described above, and then the adhesion strength of the metal resin composite was measured by the method described above.
[0101] The results are shown in Table 1. [Example 2] A resin composite was obtained in the same manner as in Example 1, except that the amount of the carbodiimide group-containing compound added was adjusted to change the carbodiimide group content to 0.61 mmol (calculated from the charged amount) per 100 g of polymer composition (B-2). The results are shown in Table 1. The polymer composition (B-2) contained 98.8 mass % of PP-1 and 1.2 mass % of carbodiimide-modified polypropylene (CDI-PP-2). The density of polymer composition (B-2) was 0.910 g / cm 3 The density of the carbodiimide-modified polypropylene (CDI-PP-2) was 0.909 g / cm 3Example 3 A resin composite was obtained in the same manner as in Example 1, except that the amount of the carbodiimide group-containing compound added was adjusted to change the carbodiimide group content to 11.8 mmol (calculated from the charged amount) per 100 g of polymer composition (B-3). The results are shown in Table 1. The polymer composition (B-3) contained 77.5 mass % of PP-1 and 22.5 mass % of carbodiimide-modified polypropylene (CDI-PP-3). The density of the polymer composition (B-3) was 0.910 g / cm 3 The density of the carbodiimide-modified polypropylene (CDI-PP-3) was 0.909 g / cm 3 The results are shown in Table 1. [Comparative Example 1] A resin composite was obtained in the same manner as in Example 1, except that MAH-PP-2 was used instead of the polymer composition (B-1) used in Example 1. The results are shown in Table 1. [Comparative Example 2] A resin composite was obtained in the same manner as in Example 1, except that EVOH was used as the adherend. The results are shown in Table 1. [Comparative Example 3] A resin composite was obtained in the same manner as in Example 1, except that polyamide 6 was used as the adherend. The results are shown in Table 1. [Comparative Example 4] A resin composite was obtained in the same manner as in Example 1, except that PET was used as the adherend. The results are shown in Table 1.
[0102]
[0103] As shown in Table 1, the metal resin composites using the polymer compositions containing carbodiimide-modified polypropylene obtained in Examples 1 to 3 and having a carbodiimide group content within a predetermined range had excellent adhesive strength at room temperature and even at a high temperature of 100°C, and also had higher adhesive strength at a high temperature of 100°C than at room temperature. In contrast, the metal resin composite using the polymer composition not containing carbodiimide groups obtained in Comparative Example 1 had low adhesive strength at a high temperature of 100°C.
[0104] According to the present invention, by using a carbodiimide-modified polyolefin that can be bonded to a wide variety of resins, it is possible to provide a lightweight metal resin composite that has sufficient adhesive strength between a metal member and a polymer composition.
[0105] The metal-resin composite of the present invention can be used in a variety of applications, including food packaging applications such as food containers and beverage containers, pharmaceutical packaging applications such as cosmetic bottles and shampoo bottles, industrial packaging applications such as semiconductor trays, industrial material applications such as automobile parts, fuel pipes, gas pipes, hot water pipes, ink tubes, and liquid transport tubes, and building material applications such as decorative sheets.
Claims
1. A metal resin composite comprising a layer (AL) made of a metal member (A) and a layer (BL) made of a polymer composition (B) that satisfies the following requirements (i) and (ii): (i) a carbodiimide-modified polyolefin formed by reacting a polyolefin (a) having a group reactive with a carbodiimide group with a carbodiimide group-containing compound (b); and (ii) the polymer composition (B) contains 0.1 to 50 mmol of carbodiimide groups per 100 g of the polymer composition (B).
2. The metal resin composite according to claim 1, wherein the content of the carbodiimide-modified polyolefin in the polymer composition (B) is 1% by mass to 40% by mass.
3. The polymer composition (B) further has a density of 0.890 g / cm 3 The metal-resin composite according to claim 1 , comprising the above-mentioned high-density polymer (c).
4. The metal resin composite according to claim 3, wherein the content of the high density polymer (c) in the polymer composition (B) is 60% by mass to 99% by mass.
5. The density of the polymer composition (B) is 0.890 g / cm 3 The metal resin composite according to claim 1 , wherein the content of the low density polymer (d) is less than 10 mass %.
6. The density of the polymer composition (B) is 0.900 g / cm 3 The metal-resin composite according to claim 1 .
7. The metal-resin composite according to claim 1, wherein at least a portion of said layer (AL) and said layer (BL) is heat-sealed.
8. The metal-resin composite according to claim 7, characterized in that at least a portion of said layer (AL) and said layer (BL) are in contact with each other.
9. The metal resin composite according to claim 7 or 8, characterized in that the adhesive strength between the layer (AL) and the layer (BL) at 100°C is greater than the adhesive strength at room temperature.
10. The metal resin composite according to claim 3, wherein the high density polymer (c) comprises a polymer (c-1) having no polar functional group.
11. The metal-resin composite according to claim 3, wherein the high-density polymer (c) includes a polymer (c-2) having a polar functional group.
12. The metal resin composite according to claim 1, wherein the number of carbodiimide groups in one molecule of said carbodiimide group-containing compound (b) is 5 or more.
13. The metal-resin composite according to claim 1, wherein the metal member (A) is aluminum.
14. A method for producing a metal resin composite according to claim 7 or 8, comprising the steps of: bringing a melt of a polymer composition (B) that satisfies the following requirements (i) and (ii) into contact with the surface of a layer (AL) made of a metal member (A); and cooling the melt of the layer (BL) made of the polymer composition (B) that has been in contact with the surface of the layer (AL) made of the metal member (A). (i) The polymer composition (B) comprises a carbodiimide-modified polyolefin formed by reacting a polyolefin (a) having a group reactive with a carbodiimide group with a carbodiimide group-containing compound (b). (ii) The polymer composition (B) contains 0.1 to 50 mmol of carbodiimide groups per 100 g of the polymer composition.
Citation Information
Patent Citations
JP1975004144A
Novel compatibilizer and polar polymer composition using this compatibiliser
JP2005307157A
Polyarylene sulfide resin composition, molded article, composite structure, and manufacturing method
JP2019111790A
Hot melt adhesive resin laminate and laminate
JP2019137853A
Composite body
JP2022127843A