Polycarbonate resin composition and molded article thereof
The polycarbonate resin composition, featuring specific aliphatic and aromatic dihydroxy compounds, addresses the issue of scratches by providing self-healing and maintaining mechanical strength, resulting in durable and aesthetically superior molded articles.
Patent Information
- Application Number
- PCT/JP2024/013074
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Polycarbonate resin products suffer from scratches that impair their aesthetic appearance over time, and existing solutions like hard coat treatments compromise physical properties such as brittleness and increase production complexity.
A polycarbonate resin composition incorporating specific aliphatic and aromatic dihydroxy compounds in specific ratios, forming carbonate structural units that provide self-healing properties while maintaining mechanical strength and heat resistance.
The composition achieves excellent self-healing, heat resistance, and mechanical strength, enabling the production of molded articles with improved durability and appearance retention.
Smart Images

Figure JP2024013074_03102024_PF_FP_ABST
Abstract
Description
Polycarbonate resin composition and molded article thereof
[0001] The present invention relates to a polycarbonate resin composition and molded articles such as injection molded articles and extrusion molded articles made from this polycarbonate resin composition.
[0002] Polycarbonate resins have excellent mechanical strength, electrical properties, transparency, etc., and are used in a variety of fields, including electrical and electronic equipment and automobiles.
[0003] However, polycarbonate resin has the drawback that it is more susceptible to scratches than glass, which can easily damage the aesthetic appearance of finished products. To overcome this drawback, polycarbonate resins with improved surface hardness and scratch resistance have been developed (Patent Documents 1, 2, and 3). However, the polycarbonate resins described in Patent Documents 1 to 3 are not completely scratch-resistant, and scratches gradually accumulate over time during use, damaging the aesthetic appearance.
[0004] One possible solution to this problem is to apply a hard coat to the polycarbonate resin to further improve its surface hardness, but it is generally known that applying a hard coat not only increases the number of steps required for commercialization, but also adversely affects the physical properties of the polycarbonate resin, such as making it brittle.
[0005] In recent years, so-called self-healing polymers have been reported, which are materials that do not resist scratches but naturally heal when scratches occur. Self-healing polymers maintain their beauty for a long time because scratches disappear over time even if they occur. However, no self-healing polycarbonate has been proposed so far.
[0006] JP 2021-102739 A JP 2021-88651 A Japanese Patent No. 5802495 A
[0007] An object of the present invention is to provide a polycarbonate resin composition having excellent heat resistance and mechanical strength, which are inherently required of polycarbonate resins, and also having self-repairing properties, and a molded article thereof.
[0008] The present inventors have found that by preparing a polycarbonate resin composition containing carbonate structural units derived from a specific aliphatic dihydroxy compound and carbonate structural units derived from a specific aromatic dihydroxy compound in a specific ratio, it is possible to maintain the excellent physical properties of polycarbonate resins, such as heat resistance and mechanical strength, while retaining the property of being able to erase scratches by heat. The gist of the present invention resides in the following [1] to
[14] .
[0009] [1] A polycarbonate resin composition comprising carbonate structural units (X) derived from an aliphatic dihydroxy compound represented by at least one of the group consisting of the following formulas (1), (2), and (8), and carbonate structural units (Y) derived from an aromatic dihydroxy compound represented by the following formula (3), wherein the content of the carbonate structural units (X) is 10% by mass or more and less than 26% by mass, and the content of the carbonate structural units (Y) is more than 74% by mass and 90% by mass or less, based on 100% by mass of all carbonate structural units in the polycarbonate resin composition.
[0010]
[0011] (In formulas (1) and (2), m is an integer of 2 or more.)
[0012]
[0013] (In formula (8), A represents a divalent linking group having no cyclic structure, which is composed of 1 to 15 carbon atoms, 0 to 1 oxygen atom, and a hydrogen atom, and multiple As in formula (8) are the same. B represents a divalent linking group having no cyclic structure, which is composed of 1 to 40 carbon atoms and a hydrogen atom. n is an integer from 2 to 100.)
[0014]
[0015] (In formula (3), W 1 ~W 4 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms. 5 is -CR 1 R 2 - (R 1and R 2 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms, or a cycloalkylidene group having 3 to 10 carbon atoms.
[0016] [2] The polycarbonate resin composition according to [1], wherein the polycarbonate resin composition contains a copolymer polycarbonate resin containing the carbonate structural unit (X) and the carbonate structural unit (Y).
[0017] [3] The polycarbonate resin composition according to [1] or [2], wherein the polycarbonate resin composition is a mixture of a polycarbonate resin containing the carbonate structural unit (X) and a polycarbonate resin containing the carbonate structural unit (Y).
[0018] [4] The polycarbonate resin composition according to any one of [1] to [3], wherein the content of the carbonate structural unit (X) in 100% by mass of all carbonate structural units in the polycarbonate resin composition is less than 20% by mass.
[0019] [5] The polycarbonate resin composition according to any one of [1] to [4], wherein the aromatic dihydroxy compound represented by formula (3) is an aromatic dihydroxy compound represented by the following formula (4) and / or the following formula (5):
[0020]
[0021] [6] The polycarbonate resin composition according to any one of [1] to [5], wherein the aliphatic dihydroxy compound represented by the formula (8) is an aliphatic polyester polyol represented by the following formula (9):
[0022]
[0023] (In formula (9), n is an integer of 2 to 100.)
[0024] [7] The polycarbonate resin composition according to any one of [1] to [6], wherein the glass transition temperature of the polycarbonate resin composition is 110°C or lower.
[0025] [8] The polycarbonate resin composition according to any one of [1] to [7], wherein the number average molecular weight of the aliphatic dihydroxy compound represented by at least one of the group consisting of the formula (1), the formula (2), and the formula (8) is 20,000 or less.
[0026] [9] The polycarbonate resin composition according to any one of [1] to [8], wherein the polycarbonate resin composition has a tensile modulus of 100 MPa or more and 3000 MPa or less.
[0027]
[10] The polycarbonate resin composition according to any one of [1] to [9], wherein the viscosity average molecular weight (Mv) of the polycarbonate resin composition is in the range of 13,000 to 32,000.
[0028]
[11] A molded article comprising the polycarbonate resin composition according to any one of [1] to
[10] .
[0029]
[12] An injection-molded article comprising the polycarbonate resin composition according to any one of [1] to
[10] .
[0030]
[13] An extrusion-molded product comprising the polycarbonate resin composition according to any one of [1] to
[10] .
[0031] According to the present invention, it is possible to provide a polycarbonate resin composition having excellent self-repairing properties, heat resistance, and mechanical strength, and a molded article thereof. The polycarbonate resin composition of the present invention has good self-repairing properties, heat resistance, and mechanical strength, and therefore can be widely used in industrial fields such as automobile interior parts.
[0032] The present invention will be described in detail below with reference to embodiments and examples. The present invention should not be construed as being limited to the embodiments and examples shown below. In this specification, unless otherwise specified, the word "to" is used to mean that the numerical values before and after it are included as the lower and upper limits.
[0033] [Polycarbonate Resin Composition] The polycarbonate resin composition of the present invention comprises a carbonate structural unit (X) (hereinafter sometimes simply referred to as "carbonate structural unit (X)") derived from an aliphatic dihydroxy compound represented by at least one of the group consisting of the following formula (1), the following formula (2), and the following formula (8) (hereinafter sometimes referred to as "specific aliphatic dihydroxy compound of the present invention"), and a carbonate structural unit (Y) (hereinafter sometimes simply referred to as "carbonate structural unit (Y)") derived from an aromatic dihydroxy compound represented by the following formula (3) (hereinafter sometimes referred to as "aromatic dihydroxy compound (3)"), wherein the content of the carbonate structural unit (X) is 10% by mass or more and less than 26% by mass, and the content of the carbonate structural unit (Y) is more than 74% by mass and 90% by mass or less, based on 100% by mass of all carbonate structural units in the polycarbonate resin composition.
[0034]
[0035] (In formulas (1) and (2), m is an integer of 2 or more.)
[0036]
[0037] (In formula (8), A represents a divalent linking group having no cyclic structure, which is composed of 1 to 15 carbon atoms, 0 to 1 oxygen atom, and a hydrogen atom, and multiple As in formula (8) are the same. B represents a divalent linking group having no cyclic structure, which is composed of 1 to 40 carbon atoms and a hydrogen atom. n is an integer from 2 to 100.)
[0038]
[0039] (In formula (3), W 1 ~W 4 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms. 5 is -CR 1 R 2 - (R 1 and R 2are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms, or a cycloalkylidene group having 3 to 10 carbon atoms.
[0040] Hereinafter, the contents of the carbonate structural unit (X), the carbonate structural unit (Y) and other carbonate structural units are all expressed as weight percentages relative to 100% by mass of all carbonate structural units in the polycarbonate resin composition.
[0041] By configuring the polycarbonate resin composition of the present invention, the carbonate structural unit (X) derived from the specific aliphatic dihydroxy compound of the present invention forms a soft segment, and the carbonate structural unit (Y) derived from the aromatic dihydroxy compound (3) represented by the formula (3) forms a hard segment, thereby exhibiting self-repairing properties that allow scratches caused by heat to disappear while maintaining the shape. That is, the soft segment derived from the carbonate structural unit (X) provides excellent self-repairing properties. Furthermore, the hard segment derived from the carbonate structural unit (Y) provides excellent heat resistance and mechanical strength. Therefore, it is possible to obtain a polycarbonate resin composition and molded article that have self-repairing properties while maintaining heat resistance and mechanical strength.
[0042] <Carbonate Structural Unit (X)> The carbonate structural unit (X) contained in the polycarbonate resin composition of the present invention is a carbonate structural unit derived from the specific aliphatic dihydroxy compound of the present invention.
[0043] From the viewpoint of polymerizability, A in the formula (8) is preferably a linear or branched alkylene group having 1 to 6 carbon atoms. The branched chain is preferably a branched alkylene group having 1 to 6 carbon atoms and containing a methyl group. B in the formula (8) is preferably a linear alkylene group having 1 to 10 carbon atoms.
[0044] The aliphatic polyester polyol represented by the formula (8) is preferably an aliphatic polyester polyol represented by the following formula (9) from the viewpoints of availability and polymerizability.
[0045] (n is an integer from 2 to 100.)
[0046] The aliphatic polyester polyol represented by the above formula (9) is preferably a biomass-derived aliphatic polyester polyol synthesized by condensing 3-methyl-1,5-pentanediol with sebacic acid produced from plant-derived raw materials. Whether or not the aliphatic polyester polyol is produced from plant-derived resources can be determined, for example, by radiocarbon ( 14 This can be confirmed by measuring the concentration of C).
[0047] The number average molecular weight of the specific aliphatic dihydroxy compound of the present invention is desirably 20,000 or less. The upper limit of the number average molecular weight of the specific aliphatic dihydroxy compound of the present invention is more preferably 10,000 or less, particularly preferably 5,000 or less. If the number average molecular weight of the specific aliphatic dihydroxy compound of the present invention is not more than the above upper limit, the compatibility with the aromatic dihydroxy compound (3) is good, and polymerization failure due to poor compatibility can be prevented. On the other hand, there is no particular restriction on the lower limit of the number average molecular weight of the specific aliphatic dihydroxy compound of the present invention, but from the viewpoint of achieving both self-repairability and heat resistance, it is usually 200 or more, preferably 400 or more. Therefore, it is preferable that m in the above formulas (1) and (2) and n in the above formula (8) are numbers that satisfy the above-mentioned preferred range of number average molecular weight.
[0048] The number average molecular weight of the specific aliphatic dihydroxy compound of the present invention is 1 It can be calculated by a measurement method using H-NMR.
[0049] <Carbonate Structural Unit (Y)> The carbonate structural unit (Y) contained in the polycarbonate resin composition of the present invention is a carbonate structural unit derived from an aromatic dihydroxy compound (3).
[0050] In the formula (3), W 1 ~W 4 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms.
[0051] In the present invention, the number of carbon atoms in a group such as an alkyl group refers to the number of carbon atoms in the entire group, including the carbon atoms of the substituent, when the alkyl group has a substituent. Regarding an aryl group having 6 to 12 carbon atoms, when the aryl group has a substituent, the number of carbon atoms is the sum of the number of carbon atoms of the substituent and the number of carbon atoms of the aryl group.
[0052] W 1 ~W 4 The alkyl group having 1 to 10 carbon atoms represented by the formula (I) may be unsubstituted or may have a substituent. It may also be linear, branched, or cyclic. Examples of the substituent that the alkyl group may have include a halogen atom, a nitro group, a cyano group, a hydroxyl group, an aryl group, an alkoxy group, an aryloxy group, a carboxyl group, an alkoxycarbonyl group, an acyl group, and an acyloxy group.
[0053] In the formula (3), W 1 ~W 4 Specific examples of the alkyl group having 1 to 10 carbon atoms include: a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group; a methylethyl group, a methylpropyl group, a methylbutyl group, a methylpentyl group, a methylhexyl group, a methylheptyl group, a methyloctyl group, and a methylnonyl group; a dimethylethyl group, a dimethylpropyl group, a dimethylbutyl group, a dimethylpentyl group, a dimethylhexyl group, a dimethylheptyl group, and a dimethyloctyl group; a trimethylpropyl group, a trimethylbutyl group, a trimethylpentyl group, a trimethylhexyl group, and a trimethylheptyl group; an ethylbutyl group, an ethylpentyl group, an ethylhexyl group, an ethylheptyl group, and an ethyloctyl group; cyclohexyl group, methylcyclohexyl group, dimethylcyclohexyl group, trimethylcyclohexyl group, tetramethylcyclohexyl group, ethylcyclohexyl group, diethylcyclohexyl group, methylethylcyclohexyl group, and the like.
[0054] W 1 ~W 4The aryl group having 6 to 12 carbon atoms represented by the formula (I) may be unsubstituted or may have a substituent. Examples of the substituent that the aryl group may have include a halogen atom, a nitro group, a cyano group, a hydroxyl group, an alkyl group, an alkoxy group, an aryloxy group, a carboxyl group, an alkoxycarbonyl group, an acyl group, and an acyloxy group.
[0055] In the formula (3), W 1 ~W 4 Specific examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a tolyl group, and a naphthyl group.
[0056] In the formula (3), W 5 is -CR 1 R 2 - (R 1 and R 2 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms, or a cycloalkylidene group having 3 to 10 carbon atoms.
[0057] W 5 Represented by "-CR 1 R 2 R in "-" 1 and R 2 The hydrogen atom, alkyl group having 1 to 10 carbon atoms, or aryl group having 6 to 12 carbon atoms is W 1 ~W 4 The same is true in
[0058] W 5 The cycloalkylidene group having 3 to 10 carbon atoms represented by the formula (I) may have a branched structure and may be unsubstituted or may have a substituent. The substituent that the cycloalkylidene group may have is the same as that of the above-mentioned W 1 ~W 4 The substituents are the same as those that the alkyl group may have.
[0059] W 5 Specific examples of the cycloalkylidene group having 3 to 10 carbon atoms represented by the formula (I) include a cyclopentylidene group and a cyclohexylidene group.
[0060] Among these, W 1 ~W 4are each independently a hydrogen atom or a methyl group, and W 5 is -CR 1 R 2 - (R 1 and R 2 are each independently a hydrogen atom or a methyl group, and W 1 ~W 4 are each independently a hydrogen atom or a methyl group, and W 5 is a 2,2-propylidene group (-CR 1 R 2 -R 1 and R 2 is a methyl group).
[0061] Specific examples of the aromatic dihydroxy compound represented by formula (3) include 2,2-bis(4-hydroxyphenyl)propane (=bisphenol A) (hereinafter may be abbreviated as "BPA") represented by formula (4) below, and 2,2-bis(4-hydroxy-3-methylphenyl)propane (=bisphenol C) (hereinafter may be abbreviated as "BPC") represented by formula (5) below.
[0062]
[0063] <Containment Form of Carbonate Structural Unit (X) and Carbonate Structural Unit (Y)> The polycarbonate resin composition of the present invention may contain the carbonate structural unit (X) and the carbonate structural unit (Y) in the above-mentioned content ratio of the carbonate structural unit (X) and the carbonate structural unit (Y), and there are no particular limitations on the containing form of the carbonate structural unit (X) and the carbonate structural unit (Y). Usually, the carbonate structural unit (X) and the carbonate structural unit (Y) are contained in the polycarbonate resin.
[0064] The polycarbonate resin composition of the present invention may be a polycarbonate resin mixture (blend) of a polycarbonate resin containing the carbonate structural unit (X) and a polycarbonate resin containing the carbonate structural unit (Y), or may contain a copolymer-type polycarbonate resin containing both the carbonate structural unit (X) and the carbonate structural unit (Y).
[0065] The polycarbonate resin composition of the present invention may be a mixture of a polycarbonate resin containing the carbonate structural unit (X) or the carbonate structural unit (Y) and a copolymer polycarbonate resin containing the carbonate structural unit (X) and the carbonate structural unit (Y), or a mixture of a polycarbonate resin containing the carbonate structural unit (X), a polycarbonate resin containing the carbonate structural unit (Y), and a copolymer polycarbonate resin containing the carbonate structural unit (X) and the carbonate structural unit (Y). Furthermore, the polycarbonate resin composition of the present invention may be a mixture of a polycarbonate resin containing the carbonate structural unit (X) and a polycarbonate resin containing the carbonate structural unit (Y), or may contain a polycarbonate resin containing neither the carbonate structural unit (X) nor the carbonate structural unit (Y) in addition to the copolymer polycarbonate resin containing the carbonate structural units (X) and (Y).
[0066] In the present invention, the term "polycarbonate resin composition" includes the concepts of both "a polycarbonate resin mixture containing a plurality of polycarbonate resins" and "a copolymer polycarbonate resin."
[0067] When the polycarbonate resin composition of the present invention contains the carbonate structural unit (X) and the carbonate structural unit (Y) as a copolymer polycarbonate resin containing the carbonate structural unit (X) and the carbonate structural unit (Y), the polycarbonate resin composition of the present invention is referred to as a "polycarbonate resin."
[0068] When the polycarbonate resin composition of the present invention is a mixture of a polycarbonate resin containing the carbonate structural unit (X) and a polycarbonate resin containing the carbonate structural unit (Y), it is usually referred to as a "polycarbonate resin composition." The same applies to the above-mentioned other containing forms.
[0069] In the present invention, the term "polycarbonate resin composition" includes cases where a single copolymer polycarbonate resin contains the carbonate structural unit (X) and the carbonate structural unit (Y). In Examples 1 to 8 and Comparative Examples 1 to 3 described below, a single copolymer polycarbonate resin is produced, and therefore is referred to as a "polycarbonate resin" (the "polycarbonate resin" of the present invention), but this is also included in the polycarbonate resin composition of the present invention.
[0070] <Content of Each Carbonate Structural Unit (X) and Carbonate Structural Unit (Y)> The polycarbonate resin composition of the present invention contains the carbonate structural unit (X) and the carbonate structural unit (Y), and contains the carbonate structural unit (X) in an amount of 10% by mass or more and less than 26% by mass, and the carbonate structural unit (Y) in an amount of more than 74% by mass and 90% by mass or less, thereby enabling the composition to have good self-repairing properties, heat resistance, and mechanical strength.
[0071] The content of the carbonate structural unit (X) in the polycarbonate resin composition of the present invention is 10% by mass or more, preferably 13% by mass or more, and more preferably 16% by mass or more, from the viewpoint of self-repairing property. On the other hand, from the viewpoints of heat resistance and mechanical strength, the content of the carbonate structural unit (X) is less than 26% by mass, preferably less than 20% by mass, more preferably 19% by mass or less, and even more preferably 18.5% by mass or less.
[0072] The content of the carbonate structural unit (Y) in the polycarbonate resin composition of the present invention is more than 74% by mass, preferably 80% by mass or more, more preferably 81% by mass or more, and even more preferably 81.5% by mass or more, from the viewpoint of heat resistance and mechanical strength. On the other hand, from the viewpoint of self-repairing property, the content of the carbonate structural unit (Y) is 90% by mass or less, preferably 87% by mass or less, and more preferably 84% by mass or less.
[0073] The polycarbonate resin composition of the present invention may contain only one type of carbonate structural unit (X), or may contain two or more types. That is, it may contain two or more types of carbonate structural units (X) derived from the specific aliphatic dihydroxy compound of the present invention. One type of molecular weight grade may be used, or two or more types of molecular weight grades may be used. Furthermore, the polycarbonate resin composition may contain only one type of carbonate structural unit (Y), or may contain two or more types. That is, it may contain two or more types of carbonate structural units (Y) derived from the aromatic dihydroxy compound (3).
[0074] As described above, the contents of the carbonate structural units (X) and (Y) are each expressed as a weight percentage relative to 100% by mass of all carbonate structural units in the polycarbonate resin composition. Specifically, the contents of the carbonate structural units (X) and (Y) in the polycarbonate resin composition of the present invention can be determined as the proportion of carbonate units derived from each dihydroxy compound, i.e., the proportion of carbonate units derived from the specific aliphatic dihydroxy compound of the present invention and the proportion of carbonate units derived from the aromatic dihydroxy compound (3), in all carbonate units derived from all dihydroxy compounds used in the production of the polycarbonate resin composition of the present invention.
[0075] The content of each carbonate structural unit (X) and (Y) in the polycarbonate resin composition is 1 The same applies to other carbonate structural units described below.
[0076] When the carbonate structural unit (X) comprises any one of a carbonate structural unit derived from an aliphatic dihydroxy compound represented by formula (1), a structural unit derived from an aliphatic dihydroxy compound represented by formula (2), and a carbonate structural unit derived from an aliphatic dihydroxy compound represented by formula (8), the content of the carbonate structural unit (X) is the proportion of the amount of the one structural unit relative to 100% by mass of all carbonate structural units in the polycarbonate resin composition of the present invention. When the carbonate structural unit (X) comprises two or more of a carbonate structural unit derived from an aliphatic dihydroxy compound represented by formula (1), a structural unit derived from an aliphatic dihydroxy compound represented by formula (2), and a carbonate structural unit derived from an aliphatic dihydroxy compound represented by formula (8), the content of the carbonate structural unit (X) is the proportion of the combined amount of these two structural units relative to 100% by mass of all carbonate structural units in the polycarbonate resin composition of the present invention. The same applies when the polycarbonate resin composition of the present invention contains all of the carbonate structural units derived from the aliphatic dihydroxy compound represented by formula (1), the aliphatic dihydroxy compound represented by formula (2), and the aliphatic dihydroxy compound represented by formula (8). Similarly, when the polycarbonate resin composition contains two or more carbonate structural units derived from the aliphatic dihydroxy compound represented by formula (1), two or more carbonate structural units derived from the aliphatic dihydroxy compound represented by formula (2), or two or more carbonate structural units derived from the aliphatic dihydroxy compound represented by formula (8), the content of the carbonate structural unit (X) is the proportion of the total amount of these structural units. The same applies to the carbonate structural unit (Y).
[0077] <Other Carbonate Structural Units> The polycarbonate resin composition of the present invention may contain other carbonate structural units than the carbonate structural unit (X) and the carbonate structural unit (Y), i.e., carbonate structural units derived from aromatic and / or aliphatic dihydroxy compounds other than the specific aliphatic dihydroxy compound of the present invention and the aromatic dihydroxy compound (3) (hereinafter, these may be referred to as "other dihydroxy compounds"), within the scope of not impairing the object of the present invention.
[0078] Other carbonate structural units may also be contained as copolymer polycarbonate resins with the carbonate structural unit (X) and / or the carbonate structural unit (Y), and polycarbonate resins comprising other carbonate structural units may be mixed with polycarbonate resins containing the carbonate structural unit (X) and / or the carbonate structural unit (Y).
[0079] When the polycarbonate resin composition of the present invention contains other carbonate structural units, the content of the other carbonate structural units in 100% by mass of all carbonate structural units in the polycarbonate resin composition is preferably 10% by mass or less, particularly 5% by mass or less, and especially 2% by mass or less. When the polycarbonate resin composition contains other carbonate structural units, it may be possible to obtain improving effects such as a decrease in water absorption due to the other carbonate structural units, but if the content is too high, the effects of the present invention, such as improved self-repairability, heat resistance, and mechanical strength, which are achieved by containing the carbonate structural units (X) and (Y), may be impaired.
[0080] The polycarbonate resin composition of the present invention may contain only one type of other carbonate structural unit, or may contain two or more types.
[0081] <Other Components> The polycarbonate resin composition of the present invention may contain, as necessary, other components in addition to the polycarbonate resin containing the carbonate structural unit (X) and / or the carbonate structural unit (Y), as long as the other components do not significantly impair the desired physical properties. Examples of the other components include polycarbonate resins that do not contain the carbonate structural unit (X) and the carbonate structural unit (Y), resins other than polycarbonate resins, various resin additives, etc.
[0082] Examples of other resins that may be contained in the polycarbonate resin composition of the present invention include thermoplastic polyester resins such as polyethylene terephthalate resin, polytrimethylene terephthalate, and polybutylene terephthalate resin; styrene-based resins such as polystyrene resin, high impact polystyrene resin (HIPS), acrylonitrile-styrene copolymer (AS resin), acrylonitrile-styrene-acrylic rubber copolymer (ASA resin), and acrylonitrile-ethylene propylene rubber-styrene copolymer (AES resin); polyolefin resins such as polyethylene resin and polypropylene resin; polyamide resin; polyimide resin; polyetherimide resin; polyurethane resin; polyphenylene ether resin; polyphenylene sulfide resin; polysulfone resin; polymethacrylate resin, etc. One type of other resin may be contained, or two or more types may be contained in any combination and ratio.
[0083] Examples of resin additives include heat stabilizers, antioxidants, mold release agents, light stabilizers (HALS), flame retardants, antistatic agents, antifogging agents, lubricants, antiblocking agents, flow improvers, plasticizers, dispersants, antibacterial agents, dyes, pigments, etc. These resin additives may be contained alone or in any combination and ratio of two or more.
[0084] <Tensile Modulus of Polycarbonate Resin Composition> The tensile modulus of the polycarbonate resin composition of the present invention is not particularly limited, but from the viewpoint of mechanical strength, it is preferably 100 MPa or more and 3000 MPa or less, particularly 500 MPa or more and 2500 MPa or less. The tensile modulus of the polycarbonate resin composition of the present invention is measured for a test sample prepared by hot pressing to obtain a square pressed piece having a thickness of 0.5 mm and a length and width of 70 mm, and then cutting it with scissors to a thickness of 0.5 mm, a length of 70 mm, and a width of 10 mm, by the method described in the Examples section below.
[0085] <Viscosity Average Molecular Weight of Polycarbonate Resin Composition> The viscosity average molecular weight of the polycarbonate resin composition of the present invention is not particularly limited, but from the viewpoint of mechanical strength, it is preferably from 13,000 to 32,000, particularly from 17,000 to 30,000. The viscosity average molecular weight of the polycarbonate resin composition of the present invention is measured by the method described in the Examples section below.
[0086] <Glass Transition Temperature of Polycarbonate Resin Composition> The glass transition temperature of the polycarbonate resin composition of the present invention is not particularly limited, but is preferably −10° C. or higher and 120° C. or lower, more preferably 0° C. or higher and 110° C. or lower, and even more preferably 10° C. or higher and 100° C. or lower. The glass transition temperature of the polycarbonate resin composition of the present invention is measured by the method described in the Examples section below.
[0087] [Method for producing polycarbonate resin composition] <Method for producing polycarbonate resin> The polycarbonate resin constituting the polycarbonate resin composition of the present invention can be produced by a conventionally known polymerization method, and the polymerization method is not particularly limited. Examples of the polymerization method include interfacial polymerization, melt transesterification, pyridine method, ring-opening polymerization of a cyclic carbonate compound, and solid-phase transesterification of a prepolymer. Among these, the melt transesterification and interfacial polymerization are preferred. Below, particularly preferred methods among these are specifically described.
[0088] (Interfacial Polymerization Method) In the interfacial polymerization method, a starting dihydroxy compound and a carbonate-forming compound are reacted in the presence of an organic solvent inert to the reaction and an aqueous alkaline solution, usually at a pH of 9 or higher, and then interfacial polymerization is carried out in the presence of a polymerization catalyst to obtain a polycarbonate resin. If necessary, a molecular weight modifier (end terminator) may be present in the reaction system, and an antioxidant may be present to prevent oxidation of the starting dihydroxy compound.
[0089] The organic solvent inert to the reaction is not particularly limited, and examples thereof include chlorinated hydrocarbons such as dichloromethane, 1,2-dichloroethane, chloroform, monochlorobenzene, and dichlorobenzene; aromatic hydrocarbons such as benzene, toluene, and xylene; etc. One type of organic solvent may be used, or two or more types may be used in any combination and ratio.
[0090] The alkaline compound contained in the alkaline aqueous solution is not particularly limited, but examples thereof include alkali metal compounds and alkaline earth metal compounds such as sodium hydroxide, potassium hydroxide, lithium hydroxide, and sodium bicarbonate. Among these, sodium hydroxide and / or potassium hydroxide are preferred. The alkaline compounds may be used alone or in any combination and ratio of two or more.
[0091] Although there are no limitations on the concentration of the alkali compound in the alkaline aqueous solution, the alkali compound is usually used at a concentration of 5 to 10 mass % in order to control the pH of the alkaline aqueous solution to 10 to 12. For example, when blowing in phosgene, the alkali compound is usually used in an amount of 1.9 mol or more, preferably 2.0 mol or more, and usually 3.2 mol or less, preferably 2.5 mol or less, per mol of the starting dihydroxy compound in order to control the pH of the aqueous phase to 10 to 12, preferably 10 to 11.
[0092] By using a starting dihydroxy compound containing the specific aliphatic dihydroxy compound of the present invention and the aromatic dihydroxy compound (3), a copolymer polycarbonate resin containing a carbonate structural unit (X) and a carbonate structural unit (Y) can be produced. By using the specific aliphatic dihydroxy compound of the present invention, a polycarbonate resin containing a carbonate structural unit (X) can be produced. By using the aromatic dihydroxy compound (3), a polycarbonate resin containing a carbonate structural unit (Y) can be produced. When producing a polycarbonate resin containing the above-mentioned other carbonate structural units, one or more dihydroxy compounds other than the specific aliphatic dihydroxy compound of the present invention and the aromatic dihydroxy compound (3) can be used.
[0093] As the carbonate-forming compound, a carbonyl halide is preferably used, and among these, phosgene is preferably used. The method using phosgene is particularly called the phosgene method.
[0094] The polymerization catalyst is not particularly limited, but examples thereof include aliphatic tertiary amines such as trimethylamine, triethylamine, tributylamine, tripropylamine, and trihexylamine; alicyclic tertiary amines such as N,N'-dimethylcyclohexylamine and N,N'-diethylcyclohexylamine; aromatic tertiary amines such as N,N'-dimethylaniline and N,N'-diethylaniline; quaternary ammonium salts such as trimethylbenzylammonium chloride, tetramethylammonium chloride, and triethylbenzylammonium chloride; pyridine; guanine; salts of guanidine; etc. One type of polymerization catalyst may be used, or two or more types may be used in any combination and ratio.
[0095] The molecular weight modifier is not particularly limited, and examples thereof include phenols having a monovalent phenolic hydroxyl group; aliphatic alcohols such as methanol and butanol; mercaptan; and phthalimide. Among these, phenols are preferred. Specific examples of phenols include phenol, o-n-butylphenol, m-n-butylphenol, p-n-butylphenol, o-isobutylphenol, m-isobutylphenol, p-isobutylphenol, o-t-butylphenol, m-t-butylphenol, p-t-butylphenol, o-n-pentylphenol, m-n-pentylphenol, p-n-pentylphenol, o-n-hexylphenol, m-n-hexylphenol, p-n-hexylphenol, p-t-octylphenol, o-cyclohexylphenol, m-cyclohexylphenol, p-cyclohexylphenol, o-phenylphenol, m-phenylphenol, p-phenylphenol, o-n-nonylphenol, m-n-nonylphenol, and p-n-nonylphenol. Examples of suitable phenols include o-cumylphenol, m-cumylphenol, p-cumylphenol, o-naphthylphenol, m-naphthylphenol, p-naphthylphenol, 2,5-di-t-butylphenol, 2,4-di-t-butylphenol, 3,5-di-t-butylphenol, 2,5-dicumylphenol, 3,5-dicumylphenol, p-cresol, bromophenol, tribromophenol, monoalkylphenols having a linear or branched alkyl group having an average of 12 to 35 carbon atoms at the ortho, meta, or para position, 9-(4-hydroxyphenyl)-9-(4-methoxyphenyl)fluorene, 9-(4-hydroxy-3-methylphenyl)-9-(4-methoxy-3-methylphenyl)fluorene, and 4-(1-adamantyl)phenol. Among these, p-t-butylphenol, p-phenylphenol, and p-cumylphenol are preferred. The molecular weight modifier may be used alone or in any combination of two or more in any ratio.
[0096] The amount of the molecular weight modifier used is not particularly limited, but is, for example, usually 0.5 mol or more, preferably 1 mol or more, and usually 50 mol or less, preferably 30 mol or less, per 100 mol of the starting dihydroxy compound.
[0097] The antioxidant is not particularly limited, but examples thereof include hindered phenol-based antioxidants. Specific examples thereof include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesitylene-2,4, 6-tolyl)tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4- hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, and the like.
[0098] Among these, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Commercially available phenolic antioxidants include "Irganox (registered trademark) 1010" and "Irganox (registered trademark) 1076" manufactured by BASF, and "Adekastab (registered trademark) AO-50" and "Adekastab (registered trademark) AO-60" manufactured by ADEKA. One type of antioxidant may be used, or two or more types may be used in any combination and ratio.
[0099] The amount of antioxidant used is not particularly limited, but is, for example, usually 0.001 part by mass or more, preferably 0.01 part by mass or more, more preferably 0.1 part by mass or more, and usually 1 part by mass or less, preferably 0.5 parts by mass or less, relative to 100 parts by mass of the starting dihydroxy compound. If the amount of antioxidant used is less than the lower limit of the above range, the antioxidant effect may be insufficient. If the amount of antioxidant used exceeds the upper limit of the above range, gas may be more likely to be generated during injection molding.
[0100] During the reaction, the order in which the reaction substrates (reaction raw materials), reaction solvent (organic solvent), catalyst, additives, etc. are mixed is arbitrary as long as the desired polycarbonate resin is obtained, and an appropriate order may be arbitrarily set. For example, when phosgene is used as the carbonate-forming compound, the molecular weight modifier can be mixed at any time between the reaction of the raw material dihydroxy compound with phosgene (phosgenation) and the start of the polymerization reaction.
[0101] The reaction temperature is not particularly limited, but is usually 0 to 40° C. The reaction time is not particularly limited, but is usually several minutes (for example, 10 minutes) to several hours (for example, 6 hours).
[0102] (Melt transesterification method) In the melt transesterification method, for example, a transesterification reaction is carried out between a carbonate ester and a starting dihydroxy compound. The starting dihydroxy compound is the same as that in the interfacial polymerization method.
[0103] The carbonate ester may be, for example, a compound represented by the following formula (6), and examples thereof include diaryl carbonates, dialkyl carbonates, biscarbonates of dihydroxy compounds, monocarbonates of dihydroxy compounds, and carbonates of dihydroxy compounds such as cyclic carbonates.
[0104]
[0105] In the formula (6), R 11 and R 12 R each independently represents an alkyl group or an aryl group. 11 and R 12 The alkyl group and aryl group represented by the following formula (7) may be unsubstituted or may have a substituent. The substituent that these substituents may have is represented by R 13 , R 14 The substituents are the same as those that the aryl group in R 11 and R 12 The number of carbon atoms in the alkyl group represented by R is preferably 1 to 30. 11 and R 12 The aryl group represented by the formula (I) preferably has 6 to 30 carbon atoms, and more preferably 6 to 12 carbon atoms.
[0106] Below, R 11 and R 12 However, when the group is an alkyl group, it is called a dialkyl carbonate, and when the group is an aryl group, it is called a diaryl carbonate.
[0107] Among them, from the viewpoint of reactivity with dihydroxy compounds, R 11 and R 12 is preferably each independently an aryl group which may have a substituent. The carbonate ester is more preferably a diaryl carbonate represented by the following formula (7) which may have a substituent.
[0108]
[0109] In the formula (7), R 13 and R 14are each independently a halogen atom, a nitro group, a cyano group, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, a carboxylic acid group, an alkoxycarbonyl group having 2 to 20 carbon atoms, or an acyloxy group having 1 to 20 carbon atoms. p and q are each independently an integer of 0 to 5.
[0110] The alkoxycarbonyl group is —C(═O)—OR 20 (R 20 is an alkyl group. Specific examples include a methoxycarbonyl group and an ethoxycarbonyl group. An acyloxy group is a group represented by the formula -O-C(=O)-R 21 (R 21 is a hydrogen atom, an alkyl group, or an aryl group. Specific examples include a formyloxy group and an acetyloxy group. p and q are each independently preferably an integer of 0 to 3, and more preferably an integer of 0 to 2.
[0111] Specific examples of the carbonate ester represented by formula (6) and / or formula (7) include dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, and di-t-butyl carbonate; diphenyl carbonate (hereinafter sometimes abbreviated as "DPC"); bis(4-methylphenyl)carbonate, bis(4-chlorophenyl)carbonate, bis(4-fluorophenyl)carbonate, bis(2-chlorophenyl)carbonate, bis(2,4-difluorophenyl)carbonate, bis(4-nitrophenyl)carbonate, bis(2-nitrophenyl)carbonate, bis(methylsalicylphenyl)carbonate, and diaryl carbonates such as ditolyl carbonate. Of these, diphenyl carbonate is preferred. These carbonate esters may be used alone or in any combination and ratio of two or more.
[0112] The carbonate ester may be substituted with a dicarboxylic acid or a dicarboxylic acid ester, preferably in an amount of 50 mol % or less, more preferably 30 mol % or less. Typical dicarboxylic acids or dicarboxylic acid esters include terephthalic acid, isophthalic acid, diphenyl terephthalate, diphenyl isophthalate, etc. When substituted with such a dicarboxylic acid or dicarboxylic acid ester, a polyester carbonate is obtained.
[0113] The ratio of the starting dihydroxy compound to the carbonate ester may be any ratio as long as the desired polycarbonate resin is obtained; however, it is preferable to use an excess of these carbonate esters relative to the starting dihydroxy compound when polymerizing them with the dihydroxy compound. The amount of carbonate ester used is preferably 1.01 to 1.30 mol, more preferably 1.01 to 1.20 mol, per mol of the dihydroxy compound. If this molar ratio is too small, the resulting polycarbonate resin will have more terminal OH groups, which tends to deteriorate the thermal stability of the resin. On the other hand, if this molar ratio is too large, the transesterification reaction rate will decrease, making it difficult to produce a polycarbonate resin having the desired molecular weight, or the amount of carbonate ester remaining in the resin will increase, which may cause an odor during molding or when the molded product is formed.
[0114] When producing a polycarbonate resin by the melt transesterification method, a transesterification catalyst is usually used. The transesterification catalyst is not particularly limited, and conventionally known catalysts can be used. For example, it is preferable to use an alkali metal compound and / or an alkaline earth metal compound. A basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound may be used in combination as an auxiliary. One type of transesterification catalyst may be used, or two or more types may be used in any combination and ratio.
[0115] In the melt transesterification method, the reaction temperature is not particularly limited, but is usually 100 to 300° C. The pressure during the reaction is not particularly limited, but is usually a reduced pressure of 2 Torr or less. Specifically, the melt polycondensation reaction may be carried out under the above conditions while removing by-products.
[0116] In the presence of an alkali catalyst, the polycarbonate resin composition of the present invention is significantly affected by thermal history and oxidation, leading to deterioration of the color. Therefore, the reaction temperature is preferably 300° C. or lower. To prevent oxygen leakage from the equipment due to excessive pressure reduction, it is preferable to select reduced pressure conditions with a lower limit of about 0.05 Torr.
[0117] The reaction can be carried out in either a batch or continuous manner. In the batchwise manner, the order of mixing the reaction substrates (reaction raw materials), catalyst, additives, etc. is arbitrary as long as the desired polycarbonate resin is obtained, and an appropriate order may be arbitrarily set.
[0118] In the melt transesterification method, a catalyst deactivator may be used as needed. As the catalyst deactivator, any compound that neutralizes the transesterification catalyst may be used. Examples thereof include sulfur-containing acidic compounds and their derivatives, phosphorus-containing acidic compounds and their derivatives, etc. One type of catalyst deactivator may be used, or two or more types may be used in any combination and ratio.
[0119] The amount of the catalyst deactivator used is not particularly limited, but is usually 0.5 equivalents or more, preferably 1 equivalent or more, more preferably 3 equivalents or more, relative to the transesterification catalyst, and usually 50 equivalents or less, preferably 10 equivalents or less, more preferably 8 equivalents or less. The amount of the catalyst deactivator used is usually 1 ppm or more and 100 ppm or less, preferably 50 ppm or less, relative to the polycarbonate resin.
[0120] <Method for Producing Polycarbonate Resin Composition> When the polycarbonate resin composition of the present invention is a mixture of a polycarbonate resin containing a carbonate structural unit (X) and a polycarbonate resin containing a carbonate structural unit (Y), or a mixture of a polycarbonate resin containing the carbonate structural unit (X) and / or the carbonate structural unit (Y) and a copolymer polycarbonate resin containing the carbonate structural unit (X) and the carbonate structural unit (Y), or when the polycarbonate resin composition of the present invention contains two or more polycarbonate resins, such as a mixture containing a polycarbonate resin containing neither the carbonate structural unit (X) nor the carbonate structural unit (Y), there are no particular limitations on the method for producing the polycarbonate resin composition of the present invention by mixing a plurality of polycarbonate resins, for example, two polycarbonate resins, polycarbonate resin (a) and polycarbonate resin (b). Examples of the method include the following methods 1) to 4). 1) A method of melt-kneading polycarbonate resin (a) and polycarbonate resin (b); 2) A method of melt-kneading molten polycarbonate resin (a) and molten polycarbonate resin (b); 3) A method of mixing polycarbonate resin (a) and polycarbonate resin (b) in a solution state; 4) A method of dry-blending polycarbonate resin (a) and polycarbonate resin (b). Each method will be described below.
[0121] 1) A method of melt-kneading polycarbonate resin (a) and polycarbonate resin (b): Pellets or powder particles of polycarbonate resin (a) and pellets or powder particles of polycarbonate resin (b) are melt-kneaded using a mixing device such as a kneader, a twin-screw extruder, a single-screw extruder, etc. Pellets or powder particles of polycarbonate resin (a) and pellets or powder particles of polycarbonate resin (b) may be mixed in advance in a solid state and then kneaded, or one of them may be melted first in the mixing device, and the other polycarbonate resin may be added thereto and kneaded.
[0122] The temperature during kneading is not particularly limited, but is preferably 200°C or higher, more preferably 220°C or higher, and even more preferably 230°C or higher. Also, 320°C or lower is preferred, and 300°C or lower is particularly preferred. If the kneading temperature is low, the polycarbonate resin (a) and the polycarbonate resin (b) are not mixed completely, which is undesirable because there is a risk of variations in hardness and impact resistance when a molded product is produced. If the kneading temperature is too high, the color tone of the polycarbonate resin composition may deteriorate, which is undesirable.
[0123] 2) A method of melt-kneading a molten polycarbonate resin (a) and a molten polycarbonate resin (b): The molten polycarbonate resin (a) and the molten polycarbonate resin (b) are mixed using a mixing device such as a stirring tank, a static mixer, a kneader, a twin-screw extruder, a single-screw extruder, etc. In this case, if the polycarbonate resin is obtained by, for example, a melt polymerization method, it may be introduced into the mixing device in a molten state without being cooled or solidified.
[0124] 3) A method of mixing polycarbonate resin (a) and polycarbonate resin (b) in a solution state: This method involves dissolving polycarbonate resin (a) and polycarbonate resin (b) in an appropriate solvent to form a solution, mixing them in the solution state, and then isolating them as a polycarbonate resin composition. Pellets or powder of polycarbonate resin (a) and pellets or powder of polycarbonate resin (b) may be mixed in advance in a solid state and then dissolved in an appropriate solvent to form a solution. Alternatively, one of the polycarbonate resins may be first dissolved in an appropriate solvent to form a solution, and the other polycarbonate resin may be added to form a solution.
[0125] Suitable solvents include, for example, aliphatic hydrocarbons such as hexane and n-heptane; chlorinated aliphatic hydrocarbons such as dichloromethane, chloroform, carbon tetrachloride, dichloroethane, trichloroethane, tetrachloroethane, dichloropropane, and 1,2-dichloroethylene; aromatic hydrocarbons such as benzene, toluene, and xylene; substituted aromatic hydrocarbons such as nitrobenzene and acetophenone; and cyclic ethers such as tetrahydrofuran. Among these, chlorinated hydrocarbons such as dichloromethane or chlorobenzene are preferably used. These solvents can be used alone or in combination with other solvents.
[0126] Examples of the mixing device include a stirring tank, a static mixer, etc. The mixing temperature is not particularly limited as long as the polycarbonate resin (a) and the polycarbonate resin (b) are dissolved, and the mixing is usually carried out at a temperature equal to or lower than the boiling point of the solvent used.
[0127] 4) Method of dry blending polycarbonate resin (a) and polycarbonate resin (b): This method involves dry blending pellets or powder of polycarbonate resin (a) with pellets or powder of polycarbonate resin (b) using a tumbler, a super mixer, a Henschel mixer, a Nauta mixer, or the like.
[0128] Among the above methods 1) to 4), methods 1) and 2) in which the polycarbonate resin (a) and the polycarbonate resin (b) are melt-kneaded, and method 4) in which the polycarbonate resin (a) and the polycarbonate resin (b) are dry-blended are preferred.
[0129] In producing the polycarbonate resin composition, in any of the above methods, pigments, dyes, mold release agents, heat stabilizers, etc. may be added as appropriate within the range that does not impair the object of the present invention.
[0130] [Molded Article] The molded article of the present invention contains the polycarbonate resin composition of the present invention and is obtained using the polycarbonate resin composition of the present invention. To produce a molded article from the polycarbonate resin composition of the present invention, a conventional extrusion molding machine or injection molding machine is used.
[0131] The molding temperature when molding the polycarbonate resin composition of the present invention is preferably 160°C or higher, more preferably 180°C or higher, and even more preferably 200°C or higher. It is also preferably 320°C or lower, more preferably 300°C or lower. If the molding temperature is too low, the melt viscosity increases, the flowability decreases, and moldability may decrease. If the molding temperature is too high, the polycarbonate resin composition may become discolored, and the color tone of the resulting molded product may also deteriorate, which is undesirable. Furthermore, polycarbonate resin compositions containing structural units derived from aliphatic dihydroxy compounds, such as carbonate structural units (X), may decompose at high temperatures.
[0132] When injection molding or extrusion molding is carried out, pigments, dyes, mold release agents, heat stabilizers, etc. may be added to the polycarbonate resin composition of the present invention as appropriate within the range that does not impair the object of the present invention.
[0133] <Injection-molded article> The injection-molded article of the present invention contains the polycarbonate resin composition of the present invention and is obtained using the polycarbonate resin composition of the present invention. A conventional injection molding machine is used to produce an injection-molded article from the polycarbonate resin composition of the present invention.
[0134] When an injection molding machine or the like is used, the mold temperature is preferably 120°C or lower, more preferably 90°C or lower. Also, it is preferably 20°C or higher, more preferably 30°C or higher. If the mold temperature is too high, the cooling time during molding must be extended, which may lengthen the production cycle of molded articles and reduce productivity. If the mold temperature is too low, the melt viscosity of the polycarbonate resin composition may become too high, making it impossible to obtain uniform molded articles, and problems such as unevenness on the surface of the molded articles may occur, which is undesirable.
[0135] <Extrusion Molded Article> The extrusion molded article of the present invention contains the polycarbonate resin composition of the present invention and is obtained using the polycarbonate resin composition of the present invention. To produce an extrusion molded article from the polycarbonate resin composition of the present invention, a conventional extrusion molding machine is used. The extrusion molding machine is generally equipped with a T-die, a round die, or the like, and extrusion molded articles of various shapes can be obtained. Examples of the extrusion molded article include sheets, films, plates, tubes, pipes, and the like. Of these, sheets or films are preferred.
[0136] <Uses> Molded articles of the polycarbonate resin composition of the present invention have excellent self-repairing properties, heat resistance, and mechanical strength, and can be used in various fields including vehicle interiors.
[0137] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0138] [Measurement and Evaluation Methods] The physical properties of the polycarbonate resins obtained in the following examples and comparative examples were measured and evaluated by the following methods.
[0139] (1) Glass transition temperature (Tg) was measured using a differential scanning calorimeter (DSC6220 manufactured by SII). The obtained polycarbonate resin was used as a measurement sample without drying. An aluminum sample pan containing approximately 10 mg of the measurement sample was heated from 30°C to 300°C at a temperature increase rate of 20°C / min with a nitrogen gas flow rate of 50 mL / min, and further cooled to -120°C at a temperature decrease rate of 40°C / min. The sample was then heated again to 300°C at a temperature increase rate of 20°C / min. The differential scanning calorimetry curve obtained from the second temperature increase was analyzed as the measurement curve. The glass transition temperature (Tg) was analyzed in accordance with JIS K7121-1987. The extrapolated glass transition onset temperature was determined as the temperature at the intersection of a straight line extending the low-temperature baseline toward the high-temperature side and a tangent drawn at the point where the gradient of the stepwise change in the glass transition curve is maximum. The extrapolated glass transition temperature was taken as the glass transition temperature (Tg).
[0140] (2) Viscosity Average Molecular Weight (Mv) A polycarbonate resin was dissolved in methylene chloride (concentration: 6.0 g / L), and the intrinsic viscosity (intrinsic viscosity) [η] (unit: dL / g) at 20°C was determined using an Ubbelohde viscosity tube (manufactured by Moritomo Rika Kogyo Co., Ltd.), and the viscosity average molecular weight (Mv) was calculated using Schnell's viscosity formula (the following formula): η = 1.23 × 10 -4 Mv 0.83
[0141] (3) Tensile Modulus The obtained polycarbonate resin was dried at 100°C for at least 3 hours. Using a 0.5 mm thick, 70 mm long, and 70 mm wide SUS spacer, 4 g of the dried polycarbonate resin was preheated in a heat press at a temperature of 200-240°C for 4 minutes, pre-pressed at 2 MPa for 1 minute, and then pressurized at 10 MPa for 1 minute. The spacer was then removed and cooled at room temperature to produce a pressed piece with a thickness of 0.5 mm. This pressed piece was cut with scissors to obtain a rectangular test sample with a thickness of 0.5 mm, a length of 70 mm, and a width of 10 mm. The obtained test sample was subjected to a tensile test using a benchtop precision universal testing machine, AUTOGRAPH AGS-X (Shimadzu Corporation), with an initial chuck distance of 45 mm and an initial tensile speed of 1 mm / min. The tensile modulus was measured five times at displacements of 0 to 0.3 mm, and the average value was used as the result. A higher tensile modulus indicates better mechanical strength.
[0142] (4) Self-healing property The test piece obtained by the above-mentioned heat pressing was scratched using a pencil hardness tester (manufactured by Toyo Seiki) with a load of 750 g applied with a 4H pencil having a lead length of 5 to 6 mm. This was placed in a dryer (manufactured by Tokyo Rikakikai Co., Ltd.) and heated at 100 ° C for 6 hours. The difference in scratches between the sample left at room temperature and the heated sample was evaluated visually and by touch with the fingers. If the scratches on the heated sample had disappeared, it was judged as "○", if the dents in the scratches were recognized to have decreased by touch with the fingers, it was judged as "△", and if the dents in the scratches were not recognized to have decreased by touch with the fingers, it was judged as "×". If it was judged as "○" or "△", it was judged to have self-healing property.
[0143] (5) Heat Resistance In the self-repairing property test described above, if the test piece remained unchanged after heating, it was judged as "Good", if it became slightly cloudy, it was judged as "Good", and if it became cloudy, it was judged as "Poor". If it was judged as "Good" or "Good", it was judged to have heat resistance.
[0144] [Raw Materials] The compounds used in the following examples and comparative examples are abbreviated as follows. The compounds used were manufactured by the following manufacturers.
[0145] <Dihydroxy Compounds> PO3G500: Polytrimethylene ether glycol, number average molecular weight 562 (manufactured by ALLESSA, trade name: VELVETOL (registered trademark)) PO3G1000: Polytrimethylene ether glycol, number average molecular weight 1069 (manufactured by ALLESSA, trade name: VELVETOL (registered trademark)) PO3G2700: Polytrimethylene ether glycol, number average molecular weight 2743 (manufactured by ALLESSA, trade name: VELVETOL (registered trademark)) PTMG1000: Polytetramethylene ether glycol, number average molecular weight 991 (manufactured by Mitsubishi Chemical Corporation) PTMG3000: Polytetramethylene ether glycol, number average molecular weight 2840 (manufactured by Mitsubishi Chemical Corporation) P-2050: Aliphatic polyester polyol represented by the formula (9), number average molecular weight 1965 (manufactured by Kuraray Co., Ltd., trade name: Kuraray Polyol) BPA: 2,2-bis(4-hydroxyphenyl)propane (=bisphenol A) (manufactured by Mitsubishi Chemical Corporation) BPC: 2,2-bis(4-hydroxy-3-methylphenyl)propane (=bisphenol C) (manufactured by Honshu Chemical Co., Ltd.)
[0146] <Carbonate ester> DPC: diphenyl carbonate (manufactured by Mitsubishi Chemical Corporation)
[0147] <Polymerization catalyst> Cesium carbonate (Kishida Chemical Co., Ltd.)
[0148] Example 1 A raw material mixture was prepared by adding 15.5 g (about 5.6 mmol) of PO3G2700, 84.5 g (about 0.370 mol) of BPA, 84.6 g (about 0.402 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst to a glass reactor having an internal volume of about 570 mL and equipped with a reactor stirrer, a reactor heating device, and a reactor pressure adjusting device, so that the amount of cesium carbonate was 1.00 μmol per 1 mol of the total dihydroxy compounds.
[0149] Next, the pressure inside the glass reactor was reduced to about 100 Pa, and then the pressure was returned to atmospheric pressure with nitrogen. This operation was repeated three times to purge the inside of the reactor with nitrogen. After nitrogen purge, the external temperature of the reactor was increased to 220°C, and the internal temperature of the reactor was gradually increased to dissolve the mixture. Thereafter, the stirrer was rotated at 100 rpm. Then, the pressure inside the reactor was reduced from 101.3 kPa (760 Torr) to 13.3 kPa (100 Torr) absolute pressure over 40 minutes, while distilling off phenol, which was by-produced in the oligomerization reaction of the dihydroxy compound and DPC inside the reactor.
[0150] Subsequently, the pressure inside the reactor was maintained at 13.3 kPa, and a transesterification reaction was carried out for 65 minutes while further distilling off phenol. Thereafter, the temperature outside the reactor was raised to 260°C over 15 minutes, and the pressure inside the reactor was reduced from 13.3 kPa (100 Torr) to 399 Pa (3 Torr) absolute pressure over a further 40 minutes, and the distilled phenol was removed from the system. The absolute pressure inside the reactor was then reduced to about 60 Pa (about 0.4 Torr), and a polycondensation reaction was carried out. The rotation speed of the agitator was reduced over the course of the reaction, and the polycondensation reaction was terminated when the agitator of the reactor reached a predetermined stirring power.
[0151] Next, the reactor interior was restored to an absolute pressure of 101.3 kPa with nitrogen, and then the gauge pressure was increased to 0.1 MPa. The polycarbonate resin was extracted in the form of strands from the bottom of the reactor. The strand-like polycarbonate resin was then pelletized using a rotary cutter. The content ratios of the carbonate structural unit (X) and the carbonate structural unit (Y) in the obtained copolymeric polycarbonate resin, calculated from the amounts of the raw material dihydroxy compounds charged, are shown in Table 1. The obtained polycarbonate resin was evaluated according to the above procedures. The results are shown in Table 1.
[0152] Example 2 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 19.7 g (approximately 7.2 mmol) of PO3G2700, 80.3 g (approximately 0.352 mol) of BPA, 80.7 g (approximately 0.377 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 1.
[0153] Example 3 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 32.5 g (approximately 11.9 mmol) of PO3G2700, 87.5 g (approximately 0.383 mol) of BPA, 89.0 g (approximately 0.415 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 1.
[0154] Example 4 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 17.9 g (approximately 6.5 mmol) of PO3G2700, 82.1 g (approximately 0.320 mol) of BPC, 70.7 g (approximately 0.330 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of the total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 1.
[0155] Example 5 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 19.4 g (approximately 18.6 mmol) of PO3G1000, 80.6 g (approximately 0.353 mol) of BPA, 83.6 g (approximately 0.390 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 1.
[0156] Example 6 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 17.6 g (approximately 31.4 mmol) of PO3G500, 82.4 g (approximately 0.361 mol) of BPA, 88.2 g (approximately 0.412 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 1.
[0157] Example 7 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 20.3 g (approximately 7.1 mmol) of PTMG3000, 79.8 g (approximately 0.350 mol) of BPA, 81.7 g (approximately 0.381 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the cesium carbonate content being 1.0 μmol per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 1.
[0158] Example 8 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 29.2 g (approximately 14.8 mmol) of P-2050, 87.5 g (approximately 0.383 mol) of BPA, 90.4 g (approximately 0.422 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of all dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 1.
[0159] Comparative Example 1 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 2.35 g (approximately 0.85 mmol) of PO3G2700, 97.7 g (approximately 0.428 mol) of BPA, 96.4 g (approximately 0.450 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 2.
[0160] Comparative Example 2 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 32.7 g (approximately 33.0 mmol) of PTMG1000, 84.0 g (approximately 0.368 mol) of BPA, 91.1 g (approximately 0.425 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 2.
[0161] Comparative Example 3 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 46.5 g (approximately 16.9 mmol) of PO3G2700, 73.5 g (approximately 0.322 mol) of BPA, 76.2 g (approximately 0.356 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 2.
[0162] Comparative Example 4 The procedure described in Example 1 was repeated, except that a raw material mixture was prepared using 35.4 g (approximately 62.9 mmol) of PO3G500, 81.4 g (approximately 0.356 mol) of BPA, 94.3 g (approximately 0.440 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, with the addition of 1.0 μmol of cesium carbonate per mol of total dihydroxy compounds. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 2.
[0163] Comparative Example 5 Bisphenol A polycarbonate (manufactured by Mitsubishi Engineering-Plastics Corporation, trade name NOVAREX (registered trademark) 7022J) was evaluated according to the above procedures. The results are shown in Table 2.
[0164] Comparative Example 6 A raw material mixture was prepared by adding 100 g (approximately 0.390 mol) of BPC, 86.1 g (approximately 0.402 mol) of DPC, and a 0.04 wt % aqueous solution of cesium carbonate as a catalyst, so that the cesium carbonate concentration was 1.5 μmol per mol of total dihydroxy compounds. The procedure described in Example 1 was repeated, except that the external temperature of the reactor after heating from 220°C was changed from 260°C to 250°C, and 40 minutes after the end of pressure reduction, the temperature was raised to 285°C over 10 minutes, and the reaction was continued at 285°C until the end of polymerization. The resulting polycarbonate resin was evaluated using the procedures described above. The results are shown in Table 2.
[0165]
[0166]
[0167] Example 9 4.2 g of the polycarbonate resin (PC1) produced in Comparative Example 4 and 2.8 g of bisphenol A polycarbonate (manufactured by Mitsubishi Engineering-Plastics Corporation, trade name NOVAREX (registered trademark) 7022J) (PC2) were dissolved in 60 mL of methylene chloride and dried at room temperature for 12 hours to volatilize the methylene chloride. The solution was then dried at 100°C for 1 hour in a hot air dryer. The dried polycarbonate resin composition was hot-pressed using the method described above to obtain a test piece measuring 0.5 mm in thickness, 70 mm in length, and 70 mm in width. The content ratios of the carbonate structural unit (X) and the carbonate structural unit (Y) in this polycarbonate resin composition are shown in Table 3. This polycarbonate resin composition was evaluated using the procedures described above. The results are shown in Table 3. The viscosity average molecular weight (Mv) and glass transition temperature were evaluated using the test piece after hot pressing.
[0168]
[0169] [Discussion] The above results reveal the following. Table 1 shows that in Examples 1 to 8, the content of the carbonate structural unit (X) was 10% by mass or more but less than 26% by mass, and the content of the carbonate structural unit (Y) was more than 74% by mass but less than 90% by mass, and therefore, the self-repairing property, heat resistance, and mechanical strength all achieved good results. Comparative Example 1, which contains both the carbonate structural unit (X) and the carbonate structural unit (Y) but has too little carbonate structural unit (X), does not have self-repairing property. Comparative Examples 2, 3, and 4, which have too much carbonate structural unit (X), have poor heat resistance. Comparative Examples 5 and 6 are typical BPA polycarbonate resin and BPC polycarbonate resin, respectively, and do not have self-repairing property. From Table 3, it can be seen that the polycarbonate resin composition of the present invention is not limited to a copolymer polycarbonate resin, and may also be a mixture of two types of polycarbonate resins containing the carbonate structural unit (X) and the carbonate structural unit (Y) as long as the composition contains the carbonate structural unit (X) and the carbonate structural unit (Y) in a predetermined content ratio.
[0170] From the above, it can be seen that the polycarbonate resins of Examples 1 to 9, which are the polycarbonate resin compositions of the present invention, are superior in self-repairing property, heat resistance, and mechanical strength compared to the polycarbonate resins of Comparative Examples 1 to 5.
[0171] Although the present invention has been described in detail using specific embodiments, it will be apparent to those skilled in the art that various modifications are possible within the scope of the invention. This application is based on Japanese Patent Application No. 2023-054759 filed on March 30, 2023, and is incorporated by reference in its entirety.
Claims
1. A polycarbonate resin composition comprising a carbonate structural unit (X) derived from an aliphatic dihydroxy compound represented by at least one of the group consisting of the following formulas (1), (2), and (8), and a carbonate structural unit (Y) derived from an aromatic dihydroxy compound represented by the following formula (3), wherein the content of the carbonate structural unit (X) is 10% by mass or more and less than 26% by mass, and the content of the carbonate structural unit (Y) is more than 74% by mass and 90% by mass or less, based on 100% by mass of all carbonate structural units in the polycarbonate resin composition. (In formulas (1) and (2), m is an integer of 2 or more.) (In formula (8), A represents a divalent linking group having no cyclic structure, which is composed of 1 to 15 carbon atoms, 0 to 1 oxygen atom, and a hydrogen atom, and the multiple As in formula (8) are the same. B represents a divalent linking group having no cyclic structure, which is composed of 1 to 40 carbon atoms and a hydrogen atom. n is an integer from 2 to 100.) (In formula (3), W 1 ~W 4 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms. 5 is -CR 1 R 2 - (R 1 and R 2 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 12 carbon atoms, or a cycloalkylidene group having 3 to 10 carbon atoms.
2. The polycarbonate resin composition according to claim 1, which comprises a copolymer polycarbonate resin containing the carbonate structural unit (X) and the carbonate structural unit (Y).
3. The polycarbonate resin composition according to claim 1, which is a mixture of a polycarbonate resin containing the carbonate structural unit (X) and a polycarbonate resin containing the carbonate structural unit (Y).
4. The polycarbonate resin composition according to claim 1, wherein the content of the carbonate structural unit (X) is less than 20 mass% based on 100 mass% of all carbonate structural units in the polycarbonate resin composition.
5. The polycarbonate resin composition according to claim 1, wherein the aromatic dihydroxy compound represented by formula (3) is an aromatic dihydroxy compound represented by the following formula (4) and / or the following formula (5):
6. The polycarbonate resin composition according to claim 1, wherein the aliphatic dihydroxy compound represented by the formula (8) is an aliphatic polyester polyol represented by the following formula (9): (In formula (9), n is an integer from 2 to 100.) 7. The polycarbonate resin composition according to claim 1, wherein the glass transition temperature of the polycarbonate resin composition is 110°C or lower.
8. The polycarbonate resin composition according to claim 1, wherein the aliphatic dihydroxy compound represented by at least one of the group consisting of formulas (1), (2), and (8) has a number average molecular weight of 20,000 or less.
9. The polycarbonate resin composition according to claim 1, wherein the polycarbonate resin composition has a tensile modulus of elasticity of 100 MPa or more and 3,000 MPa or less.
10. The polycarbonate resin composition according to claim 1, wherein the viscosity average molecular weight (Mv) of the polycarbonate resin composition is in the range of 13,000 to 32,000.
11. A molded article comprising the polycarbonate resin composition according to any one of claims 1 to 10.
12. An injection-molded article comprising the polycarbonate resin composition according to any one of claims 1 to 10.
13. An extrusion molded article comprising the polycarbonate resin composition according to any one of claims 1 to 10.
Citation Information
Patent Citations
Thermoplastic molding composition and manufacture therefor
JP1979127455A
Polycarbonate-polyether block copolymer, polymer blend and intermediate
JP1987079222A
Polyester / polycarbonate and treatment thereof
JP1989126326A
Production of copolymerized polycarbonate
JP1995149888A
Optical quality copolycarbonate containing polyoxyalkylene carbonate units
JP2002522584A
Cited By
Polycarbonate resin composition
WO2025159177A1