Foam sheet and pressure-sensitive adhesive tape

The multilayer foam sheet with enhanced stress relaxation and tensile strength addresses the trade-off in conventional foam sheets, preventing light unevenness and ensuring reworkability, making it suitable for large electronic device screens.

WO2024204824A1PCT designated stage expired Publication Date: 2024-10-03SEKISUI CHEMICAL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013335
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional foam sheets used in electronic devices, especially large screens, face a trade-off between stress relaxation properties and tensile strength, leading to potential light unevenness on displays and poor reworkability due to low tensile strength, which can result in breakage during the rework process.

Method used

A multilayer foam sheet with a base layer made of a foam layer and a surface layer, either foam or non-foam, laminated directly or via another layer, featuring a stress relaxation rate of 25% or more and a tensile strength of 1.6 MPa or more, with specific density, thickness, and gel fraction ranges to balance flexibility and mechanical strength.

Benefits of technology

The multilayer foam sheet effectively reduces stress transmission to liquid crystal panels, preventing light unevenness on large screens and ensuring excellent reworkability by maintaining tensile strength during peeling, thus enhancing the usability and reliability of foam sheets in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013335_03102024_PF_FP_ABST
    Figure JP2024013335_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A multilayered foam sheet which is a laminated foam sheet comprising a base layer comprising foam and a resin layer provided to at least one surface of the base directly or with another layer interposed therebetween, the resin layer being a foam or non-foam layer. The laminated foam sheet has a degree of stress relaxation of 25% or higher and a tensile strength of 1.6 MPa or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Foam sheets and adhesive tapes

[0001] The present invention relates to a foam sheet and an adhesive tape including the foam sheet.

[0002] Foam sheets are widely used as sealing materials or shock-absorbing materials in electronic devices such as mobile phones, cameras, displays, game consoles, electronic organizers, and personal computers. Foam sheets are also sometimes used inside electronic devices, for example, by applying an adhesive to at least one surface thereof to form adhesive tapes. Various types of foam sheets have been proposed for use in these applications. For example, Patent Document 1 discloses a multilayer foam sheet that has excellent step-conforming properties and reworkability, and includes a base layer made of a foam layer and a surface layer made of a foam layer or a resin film laminated on at least one surface of the base layer, and has a 25% compressive strength and a tensile breaking strength within a predetermined range.

[0003] Patent Document 2 discloses a multilayer foam sheet having excellent flexibility and mechanical strength in the shear direction, the multilayer foam sheet comprising a base layer made of a foam layer and a surface layer made of a foam layer or a resin film laminated on at least one surface of the base layer, the multilayer foam sheet having a low-shear elastic modulus and 25% compressive strength within a predetermined range. Patent Document 3 discloses a multilayer foam sheet having high impact resistance and flexibility, the multilayer foam sheet comprising a resin layer and foam layers on both surfaces of the resin layer, the resin layer having a thickness and 25% compressive strength within a predetermined range. Patent Document 4 discloses a multilayer foam sheet having excellent flexibility and mechanical strength in the shear direction, the multilayer foam sheet comprising a base layer made of a foam layer and a surface layer made of a foam layer or a resin film laminated on at least one surface of the base layer, the multilayer foam sheet having a low-shear elastic modulus and 25% compressive strength within a predetermined range.

[0004] JP 2022-131586 A JP 2022-064669 A International Publication No. 2022 / 030649 International Publication No. 2022 / 080219

[0005] Recently, with the increasing size of displays used in information terminals such as smartphones, tablets, and personal computers, as well as televisions, there has been an increasing demand for liquid crystal panels that provide images with a wide viewing angle. Because liquid crystal panels are sensitive to distortion, when the panel is attached to a housing with tape, distortion from the housing can be transmitted through the tape to the liquid crystal panel, resulting in uneven light in the screen display. Therefore, to prevent uneven light in the screen display due to the transmission of distortion from the housing, the foam tape used for attachment must be flexible and have high stress relaxation properties.

[0006] However, with conventional foam sheets, there is a trade-off between stress relaxation and tensile strength, and foams with stress relaxation have low tensile strength. This means that when dismantling a television or other object, the foam tape breaks during peeling, making it difficult to rework the product.

[0007] Therefore, an object of the present invention is to provide a foam sheet that, when used on a large screen of an electronic device, does not cause uneven light on the screen display and has excellent reworkability.

[0008] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, they have found that the above-mentioned problems can be solved by a multilayer foam sheet having a base layer made of a foam layer and a surface layer made of a foam layer or a resin film laminated directly or via another layer on at least one surface of the base layer, the multilayer foam sheet having a predetermined stress relaxation rate and tensile strength, and have completed the present invention. That is, the present invention provides the following [1] to [9].

[0009] [1] A multilayer foam sheet comprising a base layer made of a foam layer and a surface layer made of a foam layer or a non-foam layer laminated on at least one surface of the base layer directly or via another layer, wherein the stress relaxation rate of the multilayer foam sheet is 25% or more and the tensile strength of the multilayer foam sheet is 1.6 MPa or more. [2] The density of the foam sheet is 0.05 to 0.2 g / cm 3[3] The multilayer foam sheet according to [1], wherein the foam sheet has a thickness of 0.3 to 1.7 mm. [4] The multilayer foam sheet according to any one of [1] to [3], wherein the foam sheet has a 25% compressive strength of 150 kPa or less. [5] The multilayer foam sheet according to any one of [1] to [4], wherein, when the multilayer foam sheet has the surface layer on either side of the base layer, the ratio of the thickness of the base layer to the thickness of the surface layer is 5 or more, and when the multilayer foam sheet has the surface layer on both sides of the base layer, the ratio of the thickness of the base layer to the average thickness of the surface layer is 5 or more. [6] The density of the base layer is 0.04 to 0.14 g / cm 3 [7] The multilayer foam sheet according to any one of [1] to [5], wherein the gel fraction of the base layer is 13 to 50 mass% when the surface layer is made of a foam, and the gel fraction of the base layer is 13 to 75 mass% when the surface layer is made of a non-foam layer. [8] The multilayer foam sheet according to any one of [1] to [7], wherein the base layer comprises at least one selected from the group consisting of an olefin-based resin and a thermoplastic elastomer. [9] A pressure-sensitive adhesive tape comprising the multilayer foam sheet according to any one of [1] to [8], and an adhesive material on at least one surface of the multilayer foam sheet.

[0010] According to the present invention, it is possible to provide a foam sheet that does not cause uneven light in the display on the screen when used for a large screen of an electronic device, and that has excellent reworkability.

[0011] FIG. 1 is a schematic diagram showing a method for evaluating the retention performance of a foam sheet.

[0012] [Multilayer Foam Sheet] The multilayer foam sheet of the present invention comprises a base layer made of a foam layer and a surface layer made of a foam layer or a non-foam layer laminated on at least one side of the base layer, and has a stress relaxation rate of 25% or more and a tensile strength of 1.6 MPa or more. As a result, when the multilayer foam sheet is used, for example, on a large screen of an electronic device, it does not cause light unevenness in the screen display and has excellent reworkability. More specifically, when the multilayer foam sheet is used, for example, inside a thin electronic device, the multilayer foam sheet distributes stress caused by distortion of the housing in the plane direction of the multilayer foam sheet, reducing stress transmitted to the panel and effectively preventing light unevenness in the screen display. Furthermore, the tensile strength of 1.6 MPa or more prevents the multilayer foam sheet from breaking during peeling from an adherend such as a housing or panel during repair of the electronic device, and the multilayer foam sheet can be peeled off without leaving any part of the multilayer foam sheet on the adherend.

[0013] (Stress Relaxation Rate) The stress relaxation rate of the multilayer foam sheet of the present invention is 25% or more. If the stress relaxation rate is less than 25%, for example, when used on a large screen of an electronic device, light unevenness may occur in the display on the screen. From this viewpoint, the stress relaxation rate is preferably 26% or more, more preferably 30% or more, and even more preferably 35% or more. The stress relaxation rate is not particularly limited, but from the viewpoint of imparting a certain degree of stiffness to the multilayer foam sheet and facilitating excellent reworkability, it is preferably 80% or less, more preferably 75% or less, and even more preferably 70% or less. The desired level of stress relaxation rate can be achieved by adjusting the cell structure in the multilayer foam sheet, the expansion ratio, the types of resins constituting the base layer and the surface layer, etc. The stress relaxation rate can be measured by the method described in the Examples below.

[0014] (Tensile Strength) The tensile strength of the multilayer foam sheet of the present invention is 1.6 MPa or more. If the tensile strength is less than 1.6 MPa, the multilayer foam sheet may be damaged during rework, resulting in poor reworkability. From the viewpoint of facilitating good reworkability, the tensile strength is preferably 1.7 MPa or more, more preferably 1.75 MPa or more. Furthermore, from the viewpoint of imparting a certain degree of flexibility to the multilayer foam sheet and preventing light unevenness from occurring in the screen display when used on a large screen of an electronic device, the tensile strength is preferably 5 MPa or less, more preferably 4.5 MPa or less, and even more preferably 4 MPa or less. Note that the tensile strength of the multilayer foam sheet may be at least the above-mentioned lower limit in either the machine direction (MD) or the direction perpendicular to the machine direction (TD), but it is more preferable that both be at least the lower limit. Similarly, it is sufficient that either MD or TD is equal to or less than the upper limit value, but it is more preferable that both are equal to or less than the upper limit value. The tensile strength of the multilayer foam sheet can be measured by the method described in the Examples below.

[0015] (25% Compression Strength) The 25% compression strength of the multilayer foam sheet of the present invention is preferably 150 kPa or less, more preferably 150 kPa or less, more preferably 145 kPa or less, and even more preferably 60 kPa or less. When the 25% compression strength is equal to or less than the above upper limit, the multilayer foam sheet is imparted with good flexibility, and when used on a large screen of an electronic device, the occurrence of light unevenness in the screen display can be further reduced. Furthermore, from the viewpoint of imparting a certain degree of stiffness to the multilayer foam sheet and making it easier to ensure excellent reworkability, the 25% compression strength is preferably 10 kPa or more, more preferably 20 kPa or more, and even more preferably 30 kPa or more. The 25% compression strength of the multilayer foam sheet can be measured by the method described in the Examples below.

[0016] (Density) The density of the multilayer foam sheet of the present invention is preferably 0.05 to 0.2 g / cm 3 and more preferably 0.055 to 0.15 g / cm 3and more preferably 0.06 to 0.11 g / cm 3 When the density of the multilayer foam sheet is equal to or less than the upper limit, the multilayer foam sheet is endowed with good flexibility, and when used on a large screen of an electronic device, the occurrence of light unevenness in the display on the screen can be further reduced. When the density of the multilayer foam sheet is equal to or greater than the lower limit, the multilayer foam sheet can be endowed with appropriate mechanical strength. Note that the density referred to here means apparent density, and is a value measured in accordance with JIS K 7222 (2005).

[0017] In the multilayer foam sheet of the present invention, the density of the substrate layer made of the foam layer is preferably 0.03 to 0.15 g / cm 3 and more preferably 0.04 to 0.14 g / cm 3 and more preferably 0.05 to 0.085 g / cm 3 By setting the density of the base layer to these upper limits or less, the flexibility of the foam sheet is improved, and when used on a large screen of an electronic device, light unevenness in the display can be reduced. Furthermore, by setting the density of the base layer to these lower limits or more, the reworkability of the foam sheet is likely to be improved.

[0018] When the surface layer is a foam layer, the density of the foam layer should be higher than the density of the base layer, preferably 0.2 to 0.9 g / cm 3 and more preferably 0.22 to 0.83 g / cm 3 and more preferably 0.25 to 0.67 g / cm 3By setting the density of the surface foam layer to be equal to or less than these upper limits, the flexibility of the foam sheet is improved, and when used on a large screen of an electronic device, the foam sheet is more likely to conform to an adherend. Furthermore, by setting the density of the surface foam layer to be equal to or greater than these lower limits, the tensile strength of the multilayer foam sheet is improved, and the reworkability of the multilayer foam sheet is more likely to be improved. The density can be measured by the method described in the Examples. In the present invention, by adjusting the density of the base layer to a relatively low value as described above and making the surface layer a high-density foam layer or a non-foam layer as described above, it is possible to obtain a multilayer foam sheet that does not cause light unevenness in the screen display and has excellent reworkability when used on a large screen of an electronic device.

[0019] (Thickness) The thickness of the multilayer foam sheet of the present invention is preferably 0.3 to 1.7 mm, more preferably 0.32 to 1.5 mm, and even more preferably 0.5 to 1.2 mm. When the thickness is equal to or less than the above upper limit, the sheet can be easily used in thin electronic devices. When the thickness is equal to or greater than the above lower limit, the sheet can be imparted with a certain level of flexibility and tensile strength, and when used on a large screen of an electronic device, it is easy to obtain a multilayer foam sheet that does not cause light unevenness in the screen display and has excellent reworkability.

[0020] When the multilayer foam sheet of the present invention has a surface layer on either side of the base layer (typically a two-layer structure), the ratio of the thickness of the base layer to the thickness of the surface layer (hereinafter also referred to as "ratio 1") is preferably 5 or more, more preferably 5.5 or more, and even more preferably 7 or more. Furthermore, ratio 1 is preferably 120 or less, more preferably 110 or less, and even more preferably 105 or less. When the multilayer foam sheet of the present invention has a surface layer on both sides of the base layer (typically a three-layer structure), the ratio of the thickness of the base layer to the average thickness of the surface layer (hereinafter also referred to as "ratio 2") is preferably 5 or more, more preferably 5.5 or more, and even more preferably 7 or more. Furthermore, ratio 2 is preferably 120 or less, more preferably 110 or less, and even more preferably 105 or less. When these ratios are equal to or greater than the above-mentioned lower limits, the proportion of the base layer in the entire multilayer foam sheet is increased, and the stress relaxation rate of the multilayer foam sheet is equal to or greater than a certain level, which makes it possible to reduce the occurrence of uneven light on the display when used on a large screen of an electronic device. In addition, the multilayer foam sheet is imparted with a certain degree of flexibility, which facilitates good conformability to an adherend. Furthermore, when these ratios are equal to or less than the above upper limits, the proportion of the surface layer in the entire multilayer foam sheet is equal to or greater than a certain level, which provides the multilayer foam sheet with a certain degree of tensile strength and facilitates improved reworkability.

[0021] The thickness of the substrate layer in the multilayer foam sheet of the present invention is preferably 0.05 to 1.5 mm, more preferably 0.08 to 1.2 mm, and even more preferably 0.1 to 1 mm. When the thickness of the substrate layer is equal to or greater than the above-mentioned lower limit, the flexibility of the multilayer foam sheet is improved, and when used on a large screen of an electronic device, light unevenness in the screen display can be reduced. Furthermore, when the thickness of the substrate layer is equal to or less than the above-mentioned upper limit, the thickness of the multilayer foam sheet can be reduced, making it easier to use inside a thin electronic device.

[0022] The thickness of the surface layer in the multilayer foam sheet of the present invention is preferably 0.01 to 0.5 mm, more preferably 0.05 to 0.3 mm, and even more preferably 0.08 to 0.2 mm. In the case of a multilayer foam sheet having surface layers on both sides of a substrate, the thickness of at least one surface layer should be within the above range, and preferably both surface layers should be within the above range. Having a surface layer thickness equal to or greater than the above lower limit provides the multilayer foam sheet with a certain level of tensile strength, which facilitates improved reworkability. Having a surface layer thickness equal to or less than the above upper limit improves the flexibility of the multilayer foam sheet, making it less likely for uneven light to occur in the display when used on a large screen of an electronic device.

[0023] (Gel Fraction) When the surface layer of the multilayer foam sheet of the present invention is a foam layer, the gel fraction of the base layer is preferably 13 to 50% by mass, more preferably 13 to 45% by mass, and even more preferably 16 to 40% by mass. When the surface layer is a non-foam layer, the gel fraction is preferably 13 to 75% by mass, more preferably 13 to 70% by mass, and even more preferably 16 to 60% by mass. Having a gel fraction equal to or greater than the lower limit imparts a certain degree of stiffness to the foamable resin composition, facilitating appropriate foaming of the composition during the production process of the multilayer foam sheet. Having a gel fraction equal to or less than the upper limit prevents the foamable resin composition from becoming too hard, facilitating appropriate foaming of the composition. Therefore, a gel fraction within the above range can provide a multilayer foam sheet having an expansion ratio equal to or greater than a certain level, which facilitates the production of a multilayer foam sheet that is less likely to cause light unevenness in the display when used on a large screen of an electronic device.

[0024] (Average Cell Diameter) The multilayer foam sheet of the present invention preferably has an average cell diameter in the MD direction of 70 to 500 μm, more preferably 80 to 400 μm, and even more preferably 100 to 300 μm. The average cell diameter in the TD direction is preferably 60 to 450 μm, more preferably 70 to 350 μm, and even more preferably 90 to 250 μm. The average cell diameter in the ZD direction is preferably 40 to 350 μm, more preferably 50 to 300 μm, and even more preferably 60 to 220 μm. By having an average cell diameter equal to or greater than the above lower limit, the stress relaxation rate of the multilayer foam sheet is maintained at a certain level, thereby reducing the occurrence of light unevenness in the display when used on large screens of electronic devices. By having an average cell diameter equal to or less than the above upper limit, the thickness of the multilayer foam sheet can be reduced, making it more suitable for use in thin electronic devices. The average cell diameter can be measured by the method described in the Examples. The average cell diameter can be adjusted to a desired range by adjusting the type and amount of foaming agent used, etc. The average cell diameter can also be adjusted to a desired range by appropriately stretching the foamable resin composition during or after foaming to obtain a multi-layer foam sheet.

[0025] The multilayer foam sheet of the present invention preferably has a ratio of the average cell diameter in the MD direction to the average cell diameter in the ZD direction (MD / ZD) of 1.1 or more, more preferably 1.2 or more, and even more preferably 1.4 or more. The multilayer foam sheet also preferably has a ratio of the average cell diameter in the TD direction to the average cell diameter in the ZD direction (TD / ZD) of 1.02 or more, more preferably 1.03 or more, and even more preferably 1.1 or more. When at least one of MD / ZD and TD / ZD is equal to or greater than the above lower limit, the cells have a flattened shape, which facilitates increasing the stress relaxation rate of the multilayer foam sheet. The MD / ZD ratio is preferably 3 or less, more preferably 2.5 or less, and even more preferably 1.7 or less. The TD / ZD ratio is preferably 2.5 or less, more preferably 2.4 or less, and even more preferably 2.35 or less. When at least one of MD / ZD and TD / ZD is equal to or less than the upper limit, the cells do not become too flat, and the multilayer foam sheet is more likely to have excellent reworkability.

[0026] The substrate and surface layer made of a foam layer are described in more detail below. <Substrate Layer (Foam Layer)> The substrate layer in the multilayer foam sheet of the present invention is made of a foam layer. The type of resin constituting the substrate layer is not particularly limited, but thermoplastic resins are preferably used, including olefin-based resins, acrylic-based resins, polyurethane-based resins, and thermoplastic elastomers. These may be used alone or in combination of two or more. The substrate layer preferably contains at least one resin selected from the group consisting of olefin-based resins and thermoplastic elastomers, and more preferably contains an olefin-based resin. The use of an olefin-based resin or a thermoplastic elastomer improves foamability and other properties while ensuring the flexibility and mechanical strength of the substrate layer. The resin used in the substrate layer may be used alone or in combination of two or more. It is also preferable to use an olefin-based resin and a thermoplastic elastomer in combination.

[0027] Specific examples of olefin-based resins include polyethylene resin, polypropylene resin, ethylene-vinyl acetate copolymer, etc., and among these, at least one selected from polyethylene resin and ethylene-vinyl acetate copolymer is preferred. The use of polyethylene resin or ethylene-vinyl acetate copolymer facilitates increasing the stress relaxation rate of the multilayer foam sheet, making it less likely for light unevenness to occur in the screen display when used on a large screen of an electronic device. Furthermore, when an ethylene-vinyl acetate copolymer is used, the stress relaxation rate of the multilayer foam sheet can be increased even if the expansion ratio of the base layer is relatively low. Examples of polyethylene resins include polyethylene resins polymerized with a polymerization catalyst such as a Ziegler-Natta compound, a metallocene catalyst, or a chromium oxide compound, and preferably polyethylene resins polymerized with a metallocene catalyst are used.

[0028] (Metallocene Catalyst) Examples of metallocene catalysts include compounds such as bis(cyclopentadienyl) metal complexes having a structure in which a transition metal is sandwiched between π-electron unsaturated compounds. More specifically, examples include compounds in which one or more cyclopentadienyl rings or analogs thereof are present as ligands on a tetravalent transition metal such as titanium, zirconium, nickel, palladium, hafnium, or platinum. Such metallocene catalysts have uniform active site properties, with each active site having the same activity. Polymers synthesized using metallocene catalysts have high uniformity in molecular weight, molecular weight distribution, composition, composition distribution, etc., so when a sheet containing a polymer synthesized using a metallocene catalyst is crosslinked, the crosslinking proceeds uniformly. A uniformly crosslinked sheet is foamed uniformly, making it easier to stabilize its physical properties. Furthermore, the sheet can be stretched uniformly, allowing the foam to have a uniform thickness.

[0029] Examples of the ligand include a cyclopentadienyl ring and an indenyl ring. These cyclic compounds may be substituted with a hydrocarbon group, a substituted hydrocarbon group, or a hydrocarbon-substituted metalloid group. Examples of hydrocarbon groups include a methyl group, an ethyl group, various propyl groups, various butyl groups, various amyl groups, various hexyl groups, 2-ethylhexyl groups, various heptyl groups, various octyl groups, various nonyl groups, various decyl groups, various cetyl groups, and a phenyl group. The term "various" refers to various isomers including n-, sec-, tert-, and iso-. Alternatively, a cyclic compound polymerized as an oligomer may be used as the ligand. In addition to π-electron unsaturated compounds, monovalent anionic ligands such as chlorine and bromine, or divalent anionic chelating ligands, hydrocarbons, alkoxides, arylamides, aryloxides, amides, arylamides, phosphides, arylphosphides, and the like may also be used.

[0030] Examples of metallocene catalysts containing a tetravalent transition metal or ligand include cyclopentadienyltitanium tris(dimethylamide), methylcyclopentadienyltitanium tris(dimethylamide), bis(cyclopentadienyl)titanium dichloride, and dimethylsilyltetramethylcyclopentadienyl-t-butylamido zirconium dichloride. Metallocene catalysts, when combined with a specific cocatalyst (promoter), function as a catalyst during the polymerization of various olefins. Specific cocatalysts include methylaluminoxane (MAO) and boron-based compounds. The ratio of the cocatalyst to the metallocene catalyst is preferably 100,000 to 1,000,000 moles, and more preferably 50 to 5,000 moles.

[0031] Furthermore, linear low-density polyethylene is preferred as the polyethylene resin. The linear low-density polyethylene is more preferably a linear low-density polyethylene obtained by copolymerizing ethylene (for example, 75% by mass or more, preferably 90% by mass or more, based on the total amount of monomers) with a small amount of an α-olefin as needed. Specific examples of the α-olefin include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene. Of these, α-olefins having 4 to 10 carbon atoms are preferred. The density of the polyethylene resin, for example, the linear low-density polyethylene described above, is 0.870 to 0.925 g / cm from the viewpoint of flexibility. 3 is preferably 0.890 to 0.925 g / cm 3 More preferably, 0.910 to 0.925 g / cm 3 As the polyethylene resin, a plurality of polyethylene resins may be used, and a polyethylene resin having a density outside the above range may be added.

[0032] Examples of the ethylene-vinyl acetate copolymer used as the olefin resin include an ethylene-vinyl acetate copolymer containing 50% by mass or more of ethylene. Examples of the polypropylene resin include homopolypropylene and a propylene-α-olefin copolymer containing 50% by mass or more of propylene. These may be used alone or in combination of two or more. Specific examples of the α-olefin constituting the propylene-α-olefin copolymer include ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene. Of these, α-olefins having 6 to 12 carbon atoms are preferred.

[0033] Examples of the thermoplastic elastomer include olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, vinyl chloride-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, polyester-based thermoplastic elastomers, and polyamide-based thermoplastic elastomers. These thermoplastic elastomers may be used alone or in combination of two or more. Among these, olefin-based thermoplastic elastomers and styrene-based thermoplastic elastomers are preferred, and styrene-based thermoplastic elastomers are more preferred.

[0034] It is preferable that the thermoplastic elastomer have at least one temperature within a certain temperature range (-45 to 50°C) at which the loss tangent (tan δ) of dynamic viscoelasticity shows a maximum value. Having at least one temperature near room temperature at which the loss tangent (tan δ) of dynamic viscoelasticity shows a maximum value makes it easier to achieve a stress relaxation rate of 25% or more for the multilayer foam sheet. From this perspective, it is more preferable that the loss tangent (tan δ) of dynamic viscoelasticity shows a maximum value at least within a range of -40 to 40°C, and even more preferably within a range of -35 to 35°C. The tan δ of the multilayer foam sheet is the loss tangent measured at a measurement frequency of 10 Hz. Tan δ is the ratio (G'' / G') of the storage shear modulus (G') to the loss shear modulus (G''), and indicates how much energy a material absorbs (converts into heat) when it deforms. The temperature at which the loss tangent (tan δ) of the dynamic viscoelasticity of a thermoplastic elastomer shows a maximum value is usually the glass transition temperature (Tg) of the thermoplastic elastomer. The maximum value of the loss tangent (tan δ) of the thermoplastic elastomer is preferably 0.5 or more, more preferably 1.0 or more, and even more preferably 1.5 or more, and is usually 4.0 or less. The maximum value here is preferably a temperature within the range of -45 to 50°C.

[0035] Examples of olefin-based thermoplastic elastomers include blend-type, dynamically crosslinked-type, and polymerized-type elastomers. More specifically, examples include thermoplastic elastomers that use a thermoplastic crystalline polyolefin such as polypropylene or polyethylene for the hard segment and fully vulcanized or partially vulcanized rubber for the soft segment. Examples of the thermoplastic crystalline polyolefin include a homopolymer of an α-olefin having 1 to 4 carbon atoms or a copolymer of two or more α-olefins, with polyethylene or polypropylene being preferred. Examples of the soft segment component include butyl rubber, halobutyl rubber, EPDM, EPM, acrylonitrile / butadiene rubber, NBR, and natural rubber, with EPDM being preferred.

[0036] Further, olefin-based thermoplastic elastomers include block copolymer types. Block copolymer types include those having a crystalline block and a soft segment block, and more specifically, crystalline olefin block-ethylene-butylene copolymer-crystalline olefin block copolymer (CEBC) is exemplified. In CEBC, the crystalline olefin block is preferably a crystalline ethylene block, and examples of commercially available CEBCs include "DYNARON 6200P" manufactured by JSR Corporation. Examples of olefin-based thermoplastic elastomers include "Absortomer EP1001."

[0037] Examples of the styrene-based thermoplastic elastomer include block copolymers having a styrene polymer or copolymer block and a conjugated diene compound polymer or copolymer block. Examples of the conjugated diene compound include isoprene and butadiene. The styrene-based thermoplastic elastomer used in the present invention may or may not be hydrogenated. When hydrogenation is performed, the hydrogenation can be performed by a known method.

[0038] The styrene-based thermoplastic elastomer is usually a block copolymer, and examples thereof include styrene-isoprene block copolymer, styrene-isoprene-styrene block copolymer, styrene-butadiene block copolymer, styrene-butadiene-styrene block copolymer, styrene-ethylene / butylene-styrene block copolymer (SEBS), styrene-ethylene / propylene-styrene block copolymer (SEPS), styrene-ethylene / butylene block copolymer (SEB), styrene-ethylene / propylene block copolymer (SEP), styrene-ethylene / butylene-crystalline olefin block copolymer (SEBC), etc. As the above-mentioned styrene-based thermoplastic elastomer, a block copolymer is preferred, and among these, SEBS and SEBC are more preferred.

[0039] Commercially available styrene-based thermoplastic elastomers include those manufactured by JSR Corporation under the trade name "DYNARON 8600P" (styrene content: 15% by mass), "DYNARON 4600P" (styrene content: 20% by mass), and "DYNARON 1321P" (styrene content: 10% by mass), those manufactured by Kuraray Co., Ltd. under the trade name "HYBRAR 7311," and those manufactured by Asahi Kasei Corporation under the trade name "S.O.E. (registered trademark) S1609."

[0040] The resin constituting the base layer preferably uses an olefin-based resin and a thermoplastic elastomer in combination. Among these, a linear low-density polyethylene and a thermoplastic elastomer are preferably used in combination. Furthermore, when an olefin-based resin and a thermoplastic elastomer are used in combination, the mass ratio of the thermoplastic elastomer to the olefin-based resin is preferably 15 / 85 to 85 / 15, more preferably 20 / 80 to 80 / 20, and even more preferably 25 / 75 to 75 / 25. When the mass ratio is equal to or greater than the lower limit, the elastomer tends to provide a stress relaxation rate of the multilayer foam sheet above a certain level, thereby reducing the occurrence of light unevenness in the display when used on a large screen of an electronic device. Furthermore, when the mass ratio is equal to or less than the upper limit, appropriate foaming is facilitated, making it easier to obtain a base layer with a consistent expansion ratio.

[0041] [Additives] The base layer comprising the foam layer used in the present invention is preferably obtained by foaming a foamable resin composition containing the above-mentioned resin and a foaming agent. A thermally decomposable foaming agent is preferred as the foaming agent. As the thermally decomposable foaming agent, organic foaming agents and inorganic foaming agents can be used. Examples of organic foaming agents include azo compounds such as azodicarbonamide, azodicarboxylic acid metal salts (e.g., barium azodicarboxylate), and azobisisobutyronitrile; nitroso compounds such as N,N'-dinitrosopentamethylenetetramine; hydrazine derivatives such as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), and toluenesulfonylhydrazide; and semicarbazide compounds such as toluenesulfonylsemicarbazide. Examples of inorganic foaming agents include ammonium carbonate, sodium carbonate, ammonium bicarbonate, sodium bicarbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate. Among these, from the viewpoint of obtaining fine bubbles and from the viewpoints of economy and safety, azo compounds are preferred, and azodicarbonamide is more preferred. One type of thermal decomposition type foaming agent may be used alone, or two or more types may be used in combination.

[0042] The amount of foaming agent in the foamable resin composition for forming the base layer is preferably 1 to 20 parts by mass, more preferably 3 to 15 parts by mass, and even more preferably 5 to 10 parts by mass, per 100 parts by mass of the resin. By using a foaming agent in an amount of 1 part by mass or more, it is possible to impart a certain level of flexibility to the foam sheet. Furthermore, by using a foaming agent in an amount of 20 parts by mass or less, it is possible to prevent the foam layer from expanding more than necessary, thereby improving the mechanical strength of the foam layer.

[0043] The foamable resin composition may contain a decomposition temperature regulator. The decomposition temperature regulator is added to lower the decomposition temperature of the thermally decomposable foaming agent or to accelerate or adjust the decomposition rate, and specific examples of such compounds include zinc oxide, zinc stearate, and urea. The decomposition temperature regulator is added in an amount of, for example, 0.01 to 5 parts by mass per 100 parts by mass of the resin in order to adjust the surface condition of the foam layer, etc.

[0044] The foamable resin composition may contain an antioxidant. Examples of the antioxidant include phenol-based antioxidants such as 2,6-di-t-butyl-p-cresol, sulfur-based antioxidants, phosphorus-based antioxidants, and amine-based antioxidants. The antioxidant is blended in an amount of, for example, 0.01 to 5 parts by mass per 100 parts by mass of the resin.

[0045] In the base layer, the resin is a main component, and the content of the resin is, for example, 70 mass % or more, preferably 80 mass % or more, more preferably 90 mass % or more, based on the total amount of the foam layer. In addition to the above, the foamable resin composition may contain additives commonly used in foams, such as a heat stabilizer, a colorant, a flame retardant, an antistatic agent, and a filler, as necessary.

[0046] <Surface Layer> The surface layer is laminated on at least one surface of the base layer. That is, the surface layer may be laminated on one surface of the base layer, or may be laminated on both surfaces of the base layer. In particular, from the viewpoint of improving reworkability, it is preferable that the surface layer be laminated on both surfaces of the base layer. The surface layer is a foam layer or a non-foam layer. In the present invention, it is preferable that the surface layer is a non-foam layer. When the surface layer is a non-foam layer, the tensile strength of the multilayer foam sheet is improved, and excellent reworkability is easily imparted. On the other hand, when the surface layer is a foam layer, it is easy to improve conformability to the adherend.

[0047] In the surface layer, the type of resin constituting the non-foam layer is not particularly limited. Examples of resins constituting the non-foam layer include, similar to the resins of the base layer, olefin-based resins, acrylic-based resins, polyurethane-based resins, and thermoplastic elastomers. In addition to these, silicone-based resins, vinyl chloride-based resins, styrene-based resins, polyester-based resins, polyamide-based resins, and ionomer-based resins may also be used. In the surface layer, one type of resin may be used alone, or two or more types may be used in combination. Furthermore, when surface layers are laminated on both sides of the foam layer, the resins used in each of the two surface layers may be the same or different. However, from the viewpoints of productivity and the ease of making the physical properties of both layers the same or similar, it is preferable that the resins be the same.

[0048] The resin constituting the surface layer is preferably a thermoplastic resin, and the use of a thermoplastic resin allows the surface layer to be easily adhered to the base layer. Furthermore, among the above-mentioned resins, an olefin-based resin is preferred as the resin used for each surface layer. The use of an olefin-based resin can further improve the reworkability of the foam sheet. Furthermore, when an olefin-based resin or a thermoplastic elastomer is used for the base layer, the adhesion of the surface layer to the foam layer can be particularly improved.

[0049] Examples of olefin resins include polyethylene resins and polypropylene resins. Ethylene-vinyl acetate copolymers and ethylene-ethyl acrylate copolymers may also be used. Examples of polyethylene resins include low-density polyethylene (density: 0.930 g / cm 3 less than 0.930 g / cm 3 0.942g / cm or more 3 less than 0.942 g / cm 3The polyethylene resin may be a linear low-density polyethylene. Details of the linear low-density polyethylene are as described in the description of the base layer, and therefore, further details are omitted here. Details of the polypropylene resin are as described in the description of the base layer, and therefore, further details are omitted here.

[0050] The ethylene-vinyl acetate copolymer used in the surface layer is the same as that described in the description of the base layer, and therefore a detailed description thereof will be omitted. Furthermore, examples of the ethylene-ethyl acrylate copolymer include an ethylene-ethyl acrylate copolymer containing 50% by mass or more of ethylene-derived structural units.

[0051] The resin constituting the surface layer is preferably a polyethylene resin. In this case, at least one of the above-mentioned low-density polyethylene, medium-density polyethylene, and high-density polyethylene may be used, but linear low-density polyethylene is preferably used, and a combination of linear low-density polyethylene and high-density polyethylene is also preferred. The use of high-density polyethylene in addition to linear low-density polyethylene improves the tensile strength of the multilayer foam sheet, making it easier to impart excellent reworkability to the multilayer foam sheet.

[0052] In the surface layer, the resin is the main component, and the resin content is, for example, 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more, based on the total amount of each layer. In addition to the resin, the surface layer may contain additives such as antioxidants, heat stabilizers, colorants, flame retardants, antistatic agents, and fillers. The surface layer may be crosslinked. As described in Production Method 1 below, the surface layer is preferably crosslinked in conjunction with the crosslinking of the base layer, and therefore is preferably crosslinked by ionizing radiation.

[0053] When the surface layer is a foam layer, for example, a foamable resin composition obtained by blending a foaming agent and the like as described for the base layer with a resin that can be used in the surface layer described above may be foamed. The amount of foaming agent in the foamable resin composition for forming the surface layer is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 1 to 3 parts by mass, per 100 parts by mass of the resin. If the amount of foaming agent is within this range, it is easy to adjust the expansion ratio of the surface layer to the desired range described above.

[0054] (Adhesive Layer) In the present invention, the base layer and the surface layer may be laminated directly or via another layer. Examples of such another layer include an adhesive layer. Known adhesives, pressure-sensitive adhesives, etc. may be used as the adhesive layer. Alternatively, a double-sided pressure-sensitive adhesive tape having pressure-sensitive adhesive layers on both sides of the base material may be used. The adhesive layer may have a thickness that does not significantly affect the physical properties of the multilayer foam sheet, such as mechanical strength and flexibility. Therefore, the thickness of the adhesive layer that bonds the base layer and the surface layer is preferably thinner than the surface layer, and more preferably 1 / 2 or less of the thickness of the surface layer.

[0055] <Method for Producing Foam Sheet> (Production Method 1) The multilayer foam sheet of the present invention is not particularly limited, and can be produced, for example, by a method in which a plurality of layers made of a resin composition are laminated to obtain a multilayer laminate sheet, and then the multilayer laminate sheet is foamed (hereinafter also referred to as "Production Method 1"). In this specification, the term "resin composition" conceptually includes a case in which the resin composition is composed of only one type of resin.

[0056] More specifically, the manufacturing method 1 includes the following steps I to II: (I) a step of obtaining a multilayer laminate sheet having a layer made of a foamable resin composition and a surface layer formed on one or both sides of the layer; and (II) a step of obtaining a foam sheet by foaming the layer made of the foamable resin composition of the multilayer laminate sheet.

[0057] Each step is described below. (Step (I)) The method for obtaining the multilayer laminate sheet in step (I) is not particularly limited, but co-extrusion molding is preferred. Specifically, when surface layers are formed on both sides of a layer made of a foamable resin composition, the resin for forming the surface layer and other additives blended as needed are fed to the first and third extruders, respectively, and melt-kneaded to obtain a resin composition for forming the surface layer. The resin for forming the base layer, a foaming agent such as a thermally decomposable foaming agent, and additives blended as needed are fed to the second extruder and melt-kneaded to obtain a foamable resin composition for forming the base layer. Next, the resin compositions fed from the first to third extruders are merged so that the composition fed from the second extruder forms the middle layer, and the resulting mixture is extruded into a sheet using a T-die or the like to obtain a multilayer laminate sheet having a three-layer structure.

[0058] Furthermore, when a surface layer is formed on one side of a layer made of a foamable resin composition, the resin for forming the surface layer and other additives blended as necessary are fed into a first extruder and melt-kneaded to obtain a resin composition for forming the surface layer. The resin for forming the base layer, a foaming agent such as a thermally decomposable foaming agent, and other additives blended as necessary are fed into a second extruder and melt-kneaded to obtain a foamable resin composition for forming the base layer. The resin composition fed from the first extruder is then merged with the composition fed from the second extruder and extruded into a sheet using a T-die or the like to obtain a multilayer laminate sheet with a two-layer structure. In co-extrusion molding, either a feedblock method or a multi-manifold method may be used, but the feedblock method is preferred.

[0059] In step (I), it is preferable to further crosslink the multilayer laminate sheet obtained above. Although a crosslinking method may involve blending an organic peroxide in advance and heating the multilayer laminate sheet obtained in step (I) to crosslink it, it is preferable to crosslink the multilayer laminate sheet by irradiating it with ionizing radiation. Examples of ionizing radiation include electron beams and β rays, with electron beams being preferred. The dose of ionizing radiation is preferably 1 to 10 Mrad, more preferably 3.0 to 7 Mrad.

[0060] (Step (II)) In step (II), the multilayer laminate sheet obtained in step (I) is foamed to foam the layer comprising the foamable resin composition. The layer comprising the foamable resin composition may be foamed by treating it so that the foaming agent foams. When the foaming agent is a thermally decomposable foaming agent, the layer is foamed by heating the multilayer laminate sheet. The heating temperature may be equal to or higher than the temperature at which the thermally decomposable foaming agent decomposes, for example, about 150 to 320°C. The method for heating the multilayer laminate sheet is not particularly limited, and examples include a method of heating the multilayer laminate sheet with hot air, infrared radiation, a salt bath, or an oil bath, and these may be used in combination. The multilayer laminate sheet may also be appropriately stretched during or after foaming. Note that the above description has been given of an example in which the surface layer is a non-foam layer. However, when the surface layer is a foam, a foaming agent such as a thermally decomposable foaming agent may be blended as an additive in the resin composition for forming the surface layer, and foamed in step (II).

[0061] (Second manufacturing method) The foam sheet of the present invention can also be manufactured by another method. Specifically, there is a method (also referred to as a "second manufacturing method") in which a foam layer constituting a base layer is manufactured in advance, and a non-foam layer or a foam layer constituting a surface layer is superimposed on one or both sides of the foam layer and bonded to the foam layer.

[0062] In the second production method, a foam may be obtained by melt-kneading a resin for forming the base layer, a thermally decomposable foaming agent, and additives blended as necessary to obtain a foamable resin composition for forming the base layer, and then molding the foamable resin composition into a sheet (foamable resin composition sheet). The method for melt-kneading the foamable resin composition and molding it into a sheet is not particularly limited, but it is preferably carried out using an extruder.

[0063] The obtained foamable resin composition sheet is preferably further crosslinked before foaming, as described below. A crosslinking method may involve blending an organic peroxide in advance and heating the foamable resin composition sheet to crosslink it, but it is preferred to crosslink the foamable resin composition sheet by irradiating it with ionizing radiation. The type and dose of ionizing radiation are as described in the first production method above.

[0064] Next, the foamable resin composition sheet may be foamed. The layer made of the foamable resin composition may be treated so that the foaming agent foams. When the foaming agent is a thermally decomposable foaming agent, the multilayer laminate sheet is heated to foam it. The heating temperature and heating method are as described in the first production method. The foamable resin composition sheet may be appropriately stretched during or after foaming.

[0065] Then, a separately prepared resin film (non-foamed) or foam for forming the surface layer is superimposed on one or both sides of the foam layer constituting the base layer and bonded to obtain a multilayer foam sheet. Specifically, this may be achieved by applying heat and pressure using a press or the like to achieve thermocompression bonding. Alternatively, a pressure-sensitive adhesive, adhesive, or the like may be applied to the bonding surface between the foam layer and the surface layer, or a double-sided adhesive tape may be applied to bond them together using the pressure-sensitive adhesive, adhesive, double-sided adhesive tape, or the like.

[0066] [Adhesive Tape] The multilayer foam sheet of the present invention may be used in an adhesive tape using the multilayer foam sheet as a substrate. The adhesive tape comprises, for example, a multilayer foam sheet and an adhesive material provided on at least one surface of the multilayer foam sheet. The adhesive tape can be adhered to other members via the adhesive material. The adhesive tape may comprise a multilayer foam sheet having an adhesive material provided on both surfaces or one surface thereof, but is preferably one having an adhesive material provided on both surfaces.

[0067] The adhesive material may comprise at least a pressure-sensitive adhesive layer. It may be a single pressure-sensitive adhesive layer laminated on the surface of a multilayer foam sheet, or a double-sided pressure-sensitive adhesive sheet attached to the surface of a multilayer foam sheet. However, a single pressure-sensitive adhesive layer is preferred. The double-sided pressure-sensitive adhesive sheet comprises a substrate and pressure-sensitive adhesive layers provided on both sides of the substrate. The double-sided pressure-sensitive adhesive sheet is used to adhere one pressure-sensitive adhesive layer to the multilayer foam sheet and the other pressure-sensitive adhesive layer to another component. The pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is not particularly limited, and examples include acrylic pressure-sensitive adhesives, urethane pressure-sensitive adhesives, and rubber pressure-sensitive adhesives. A release sheet such as release paper may also be attached to the adhesive material. The thickness of the adhesive material is preferably 5 to 200 μm, more preferably 7 to 150 μm, and even more preferably 10 to 100 μm.

[0068] [Uses] The multilayer foam sheet of the present invention and the pressure-sensitive adhesive tape comprising the multilayer foam sheet are not particularly limited, but are preferably used inside electronic devices. For example, they can be disposed between two components and used as shock absorbers, sealants, etc. Examples of electronic devices include mobile phones, cameras, displays, game consoles, electronic organizers, and personal computers. As described above, the multilayer foam sheet of the present invention and the pressure-sensitive adhesive tape comprising the same have excellent reworkability. They can also exhibit the effect of preventing light unevenness in liquid crystal displays. Therefore, the multilayer foam sheet and the pressure-sensitive adhesive tape comprising the same are preferably used in displays, particularly large displays, and more specifically, displays of 20 inches or larger. The display may be either a liquid crystal display or an organic electroluminescence display, but is preferably a liquid crystal display. In particular, the multilayer foam sheet and the pressure-sensitive adhesive tape comprising the same exhibit greater effects when used in liquid crystal displays of 20 inches or larger. Furthermore, when the pressure-sensitive adhesive tape comprising the multilayer foam sheet is used in a display, the pressure-sensitive adhesive tape comprising the multilayer foam sheet is preferably used on the back surface or frame of the display.

[0069] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0070] [Measurement Methods] The methods for measuring and evaluating each physical property are as follows.

[0071] <Thickness of Base Layer and Surface Layer (Thickness of Each Layer After Foaming)> A cross section of the foam sheet was photographed using a digital microscope (manufactured by Keyence Corporation, product name VHX-900), and the thicknesses of the base layer and the surface layer were measured from the photographed image.

[0072] <Thickness of Multilayer Foam Sheet (Total Thickness After Foaming)> The total thickness of the base layer and the surface layer was defined as the thickness of the multilayer foam sheet.

[0073] <Expansion Ratio and Density> The specific volumes (unit: cc / g) of the multilayer foam sheet, the base layer, and the surface layer constituting the multilayer foam sheet before and after foaming were measured, and the expansion ratio was calculated by dividing the specific volume after foaming by the specific volume before foaming. The density was also calculated from the measured specific volumes.

[0074] <Average Cell Diameter> The foam constituting the base layer was cut into 50 mm squares, immersed in liquid nitrogen for 1 minute, and then cut in the thickness direction along each of the MD and TD. A 200x magnified photograph was taken using a digital microscope (Keyence Corporation, product name VHX-900). For the foam in the photographed image, the MD and ZD cell diameters and the TD and ZD cell diameters were measured for all bubbles present in a 2 mm long cut surface in each of the MD and TD, and this operation was repeated five times. The average values ​​of the cell diameters of all bubbles in each of the MD and TD were taken as the average cell diameters in MD and TD, and the average value of the cell diameters of all ZDs measured by the above operation was taken as the average cell diameter in ZD.

[0075] <Tensile strength> The multilayer foam sheets produced in each Example and Comparative Example were cut into a dumbbell shape No. 1 as specified in JIS K6251 4.1. These were used as samples and subjected to measurements of tensile strength in the MD direction at a measurement temperature of 23°C and a speed of 500 mm / min using a tensile tester (product name: Tensilon RTF235, manufactured by A&D Co., Ltd.).

[0076] <25% Compression Strength> The 25% compression strength of the multilayer foam sheet was measured by a method in accordance with JIS K 6767. The measurement temperature was 23°C.

[0077] <Stress Relaxation Rate> According to a method in accordance with JIS K 6767, a multilayer foam sheet was compressed to 25% of its total thickness and allowed to rest in that state for 15 minutes, and the 25% compression strength B after resting was measured. The 25% compression strength before resting was designated as A, and the stress relaxation rate was calculated according to the following formula. The measurement was carried out in an environment of 23°C and 50% RH. Stress relaxation rate (%) = (A - B) / A x 100

[0078] <Gel Fraction> A test piece of about 100 mg was taken from the base layer of the foam sheet, and the mass C (mg) of the test piece was precisely weighed. Next, this test piece was immersed in 30 cm of xylene at 120°C. 3 After immersion for 24 hours, the insoluble matter on the mesh was filtered through a 200-mesh wire netting and collected. The insoluble matter was dried in vacuum and the mass D (mg) of the insoluble matter was precisely weighed. The gel fraction (mass%) was calculated from the obtained value using the following formula: Gel fraction (mass%) = 100 × (D / C)

[0079] <Evaluation of Screen Unevenness> A double-sided adhesive tape having adhesive layers formed on both sides of a foam sheet was cut into 3 mm wide tapes, which were attached to the three vertical and upper horizontal edges of a 143 cm x 80 cm liquid crystal panel (65-inch TV). The 143 cm x 80 cm liquid crystal panel was then joined to a housing using the double-sided adhesive tape to obtain an evaluation sample, which was then left standing upright for 24 hours. After 24 hours of leaving the sample, the degree of light unevenness when the liquid crystal panel was displayed was checked, and the light unevenness on the screen was evaluated. The evaluation criteria were as follows: (Evaluation Criteria) A: No light unevenness was observed at the edge of the liquid crystal screen. B: Light unevenness was observed at the edge of the liquid crystal screen, but the area was less than 100 mm 2 C: Less than 100 mm at the edge of the LCD screen. 2 Light unevenness 12 having an area of ​​this magnitude or larger was observed.

[0080] <Reworkability> Acrylic plates were attached to both sides of a double-sided adhesive tape having adhesive layers formed on both sides of a foam sheet, and the tape was left to stand for 24 hours at 23° C. Thereafter, a cutter was inserted between the attached acrylic plates to split the foam sheet, and when the two halves of the foam sheet were peeled off from the acrylic plates, the evaluation was given as "A" if both foam sheets could be peeled off without tearing, "B" if only one of the foam sheets could be peeled off without tearing, and "C" if both foam sheets could not be peeled off.

[0081] <Retention Performance> A 20 mm square foam sheet was cut from each of the foam sheets produced in Example 1 and Comparative Example 1, and a pressure-sensitive adhesive was applied to both sides of the foam sheet to obtain a double-sided pressure-sensitive adhesive tape using the foam sheet as a substrate. This tape was used as a test specimen. Then, as shown in Figure 1, two stainless steel (SUS) jigs 11, each with a 30 mm square bottom and a T-shaped cross section, were prepared for each test specimen. The adhesive side of each test specimen 10 was attached to the bottom surface 11A of each jig, and each test specimen 10 was attached so that it was sandwiched between the two jigs 11. Next, each test specimen 10 in the attached state was placed in an oven, cured at 40°C for 30 minutes, and then cooled to room temperature (23°C). Thereafter, using a tensile tester (product name "Tensilon RTF235", manufactured by A&D Co., Ltd.), at a measurement temperature of 23°C, the gripping portions 11B of the two jigs 11 were gripped with the fixtures of the tensile tester, and the test pieces 10 sandwiched between the two jigs 11 were fixed to the tensile tester so that the adhesive surface of each test piece 10 was perpendicular to the tensile direction, and the retention time (minutes) when a tensile load of 76 N was continuously applied was measured. Also, test pieces were prepared in the same manner as when measuring the retention time (minutes), and the test pieces were attached to the jigs in the same manner and fixed to the tensile tester. After applying a tensile load of 76 N, the tensile load remaining on the test pieces was measured. The retention times measured by the above method and the tensile loads remaining on the test pieces 1 minute and 50 minutes after the start of application of the tensile load were as shown in Table 1.

[0082] The materials used in each of the examples and comparative examples are as follows.

[0083] <Resins> Polyolefin resin (a): Kernel KF283 (manufactured by Japan Polyethylene Corporation, linear low-density polyethylene resin) Polyolefin resin (b): HY350 (manufactured by Japan Polyethylene Corporation, high-density polyethylene) Polyolefin resin (c): 626H (manufactured by Tosoh Corporation, ethylene-vinyl acetate copolymer) Elastomer resin (a): S.O.E. (registered trademark) S1609 (manufactured by Asahi Kasei Corporation, hydrogenated styrene-based thermoplastic elastomer (SEBS)), tanδ 1.2, Tg = 19°C Elastomer resin (b): Hybrar 7311F (manufactured by Kuraray Co., Ltd., styrene-based thermoplastic elastomer), tanδ 1.5, Tg = -32°C Elastomer resin (c): "Absortomer EP1001" (manufactured by Mitsui Chemicals, Inc., α-olefin copolymer), tanδ 2.7, Tg = 30°C

[0084] <Additives> Foaming agent: thermal decomposition type foaming agent (azodicarbonamide) Foaming assistant: OW-212F (manufactured by Sakai Chemical Industry Co., Ltd., zinc oxide) Antioxidant: phenolic antioxidant (2,6-di-t-butyl-p-cresol)

[0085] [Method of Producing Multilayer Foam Sheets] The multilayer foam sheets of Examples 1 to 9 and Comparative Examples 1 to 6 were produced as follows. Example 1: A foamable resin composition for a base layer was produced by feeding a polyolefin resin (a), a foaming agent, a foaming aid, and an antioxidant into a second extruder according to the formulation in Table 1 and then melt-kneading at 130°C. The resin, foaming aid, and antioxidant for the surface layer were the same as those for the base layer. The polyolefin resin (a), a foaming aid, and an antioxidant were fed into a first and third extruders according to the formulation in Table 1 and then melt-kneaded at 130°C to produce resin compositions for surface layers 1 and 2. The foamable resin composition was co-extruded from the second extruder to a thickness of 320 μm, and the resin composition was co-extruded from the first and third extruders to a thickness of 210 μm each, to produce an unfoamed multilayer laminate sheet comprising a layer of the foamable resin composition for the base layer and layers of the resin composition for the surface layer laminated on both sides of the layer. Next, the multilayer laminate sheet was crosslinked by irradiating it with an electron beam at an acceleration voltage of 500 kV for 4.0 Mrad. Thereafter, the crosslinked multilayer laminate sheet was continuously fed into a foaming furnace maintained at 250°C by hot air and an infrared heater, where it was heated and foamed, and stretched to a target thickness in a stretching step, thereby obtaining a multilayer foam sheet of Example 1 in which foam layers having different stretch ratios were laminated.

[0086] Examples 2 to 9 Multilayer foam sheets were obtained in the same manner as in Example 1, except that the type of resin for forming each layer, the blending of each component, and the thickness of each co-extruded composition were changed as shown in Tables 1 to 3.

[0087] Example 10 A foam sheet of Example 9 in which a surface layer was laminated only on one side of a base layer was obtained in the same manner as in Example 1, except that no raw material was supplied to the third extruder, and the third extruder was not used, and the type of resin for forming each layer and the blending of each component were changed as shown in Table 3.

[0088] Comparative Examples 1 to 4 Single-layer foam sheets were obtained in the same manner as in Example 1, except that no raw materials were supplied to the first and third extruders, the first and third extruders were not used, the types of resins for forming each layer and the blending ratios of each component were changed as shown in Tables 1 and 2, and the gel fraction was not measured.

[0089] Comparative Examples 5 and 6 Single-layer foam sheets were obtained in the same manner as in Example 1, except that no raw materials were supplied to the first and third extruders, the first and third extruders were not used, and the types of resins for forming each layer and the blending ratios of each component were changed as shown in Table 3.

[0090]

[0091]

[0092]

[0093] As is clear from the above results, the multilayer foam sheets produced in the Examples, which satisfied the requirements of the present invention, did not exhibit light unevenness in the screen display and had excellent reworkability. In contrast, the foam sheets produced in Comparative Examples 1 and 2 had stress relaxation rates lower than the specified level, resulting in light unevenness in the screen display. Furthermore, the foam sheets produced in Comparative Examples 3 to 6 had tensile strengths lower than the specified level, failing to exhibit excellent reworkability. The multilayer foam sheet produced in Example 1 had a smaller residual load after 1 minute than the single-layer foam sheet produced in Comparative Example 1, indicating that stress relaxation was achieved in a short period of time. Furthermore, the residual load after 50 minutes was also small. From these results, it appears that the multilayer foam sheet according to the present invention distributes the strain applied to the adhesive throughout the foam sheet, resulting in a longer retention time, compared to the single-layer foam sheet.

[0094] 10 Test piece 11 Jig 11A Bottom surface of jig 11B Grip portion of jig

Claims

1. A multi-layer foam sheet comprising a base layer made of a foam layer, and a surface layer made of a foam layer or a non-foam layer laminated directly or via another layer on at least one side of the base layer, wherein the stress relaxation rate of the multi-layer foam sheet is 25% or more, and the tensile strength of the multi-layer foam sheet is 1.6 MPa or more.

2. The density of the foam sheet is 0.05 to 0.2 g / cm 3 2. The multi-layer foam sheet of claim 1 , 3. The multi-layer foam sheet according to claim 1 or 2, wherein the foam sheet has a thickness of 0.3 to 1.7 mm.

4. The multi-layer foam sheet according to claim 1 or 2, wherein the foam sheet has a 25% compressive strength of 150 kPa or less.

5. A multilayer foam sheet according to claim 1 or 2, wherein, when the multilayer foam sheet has the surface layer on either one side of the base layer, the ratio of the thickness of the base layer to the thickness of the surface layer is 5 or more, and, when the multilayer foam sheet has the surface layer on both sides of the base layer, the ratio of the thickness of the base layer to the average thickness of the surface layer is 5 or more.

6. The density of the base layer is 0.04 to 0.14 g / cm 3 The multilayer foam sheet according to claim 1 or 2, 7. The multilayer foam sheet according to claim 1 or 2, wherein the gel fraction of the base material layer is 13 to 50 mass % when the surface layer is made of a foam, and the gel fraction of the base material layer is 13 to 75 mass % when the surface layer is made of a non-foam layer.

8. The multi-layer foam sheet according to claim 1 or 2, wherein the substrate layer comprises at least one material selected from the group consisting of olefin-based resins and thermoplastic elastomers.

9. An adhesive tape comprising the multi-layer foam sheet according to claim 1 or 2 and an adhesive material on at least one surface thereof.

Citation Information

Patent Citations

  • Multilayer foam sheet and adhesive tape

    JP2022064669A

  • Multilayer foam sheet

    WO2022030649A1

  • Multilayer foam sheet and adhesive tape

    WO2022080219A1

  • Adhesive ape

    JP2019157010A

  • Foam composite sheet and adhesive tape

    JP2020138494A