Recycled polyarylene sulfide resin composition and method for producing same
The recycled polyarylene sulfide resin composition, incorporating specific olefin resins and additives, addresses the issues of mold releasability and deposits in recycled resin pellets, allowing for increased recycled material usage and improved processing efficiency.
Patent Information
- Application Number
- PCT/JP2024/013422
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-03
AI Technical Summary
Recycled polyarylene sulfide resin pellets suffer from decomposition of the matrix polymer, deterioration of additives, and micronization of fillers during the recycling process, leading to poor mold releasability and increased risk of mold deposits during molding, limiting their effective use and efficiency.
A recycled polyarylene sulfide resin composition is developed by incorporating an olefin resin with a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, fatty acid derivatives, and silicone compounds, along with an elastomer having a reactive functional group, to improve mold releasability and prevent mold deposits, allowing for increased usage of recycled material without compromising mold release properties.
The composition enhances mold releasability, reduces the need for mold release agents, and effectively suppresses mold deposits, enabling the use of higher proportions of recycled material while maintaining excellent physical properties and work efficiency.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000041_0000
Abstract
Description
Recycled polyarylene sulfide resin composition and its manufacturing method
[0001] The present invention relates to a recycled polyarylene sulfide resin composition and a method for producing the same.
[0002] Toward the creation of a sustainable recycling-based society, technologies for recycling and utilizing plastic waste have been investigated (for example, Patent Document 1). Polyarylene sulfide resins have excellent heat resistance, mechanical properties, chemical resistance, dimensional stability, and flame retardancy, and are therefore widely used as materials for electrical and electronic equipment components, automobile components, chemical equipment components, etc. Therefore, recycling and utilizing materials containing polyarylene sulfide resins can help create a sustainable recycling-based society.
[0003] Japanese Patent Application Laid-Open No. 2022-103152
[0004] Incidentally, when molding a resin material containing polyarylene sulfide resin, a method of injection molding or extrusion molding a pellet-shaped resin material (hereinafter simply referred to as "pellets") can be generally employed. Furthermore, as a method of obtaining pellets, for example, a method of mixing a polyarylene sulfide resin with other components, such as inorganic fillers as necessary, and melt-kneading and extruding the mixture using a single-screw or twin-screw extruder to obtain pellets can be employed. When recycling materials containing polyarylene sulfide resin, molded products or items discharged after a long period of residence in a cylinder during molding (hereinafter collectively referred to as "recycled products") are crushed and re-pelletized to form recycled pellets (hereinafter also referred to as "repellet"). However, recycled pellets may have decomposed matrix polymers, deteriorated additives, and refined fillers due to shear stress during crushing of the recycled products and thermal history resulting from undergoing one or more molding processes. In such cases, changes in fluidity, crystallinity, polarity, etc. may occur compared to virgin materials that have not undergone a molding process. When such recycled pellets are used alone or as a mixture with virgin material in molding, mold release may be worse than when virgin material alone is used. Reducing the amount of recycled pellets used to prevent poor mold release results in only small amounts of recycled material being effectively used. While applying a mold release agent to the mold used during molding can improve mold release, this can be problematic when the recycled pellet mix ratio is high or when injection molding molded products with a large contact area with the mold. Furthermore, blending additional components into the recycled material can easily result in mold deposits (MD) during molding, depending on the type and amount of the components, which can lead to mold contamination.
[0005] An object of the present invention is to provide a recycled polyarylene sulfide resin composition that exhibits excellent mold releasability while suppressing the generation of mold deposits during molding, and a method for producing the same.
[0006] The present invention has the following aspects. [1] A recycled polyarylene sulfide resin composition (Y) comprising 100 parts by mass of a recycled material (X) that is a pulverized product containing a polyarylene sulfide resin, and a total of 0.1 to 3.0 parts by mass of a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound. [1a] A recycled polyarylene sulfide resin composition (Y) comprising 100 parts by mass of a recycled material (X) containing a polyarylene sulfide resin, and a total of 0.1 to 3.0 parts by mass of a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound. [2] The recycled polyarylene sulfide resin composition (Y) according to [1] or [1a], wherein the recycled material (X) contains an elastomer having a reactive functional group in an amount of 1% by mass or more relative to the total amount of the recycled material (X). [3] The recycled polyarylene sulfide resin composition (Y) according to [1], [1a], or [2], wherein the recycled material (X) contains an elastomer containing structural units derived from an α-olefin and structural units derived from a glycidyl ester of an α,β-unsaturated acid. [4] The recycled polyarylene sulfide resin composition (Y) according to any one of [1] to [3], wherein the recycled material (X) contains an elastomer having a reactive functional group, and the compound (A) contains 95% by mass or more of (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa s relative to the total amount of the compound (A). [5] The recycled polyarylene sulfide resin composition (Y) according to [1], wherein the recycled material (X) does not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass% relative to the total amount of the recycled material (X).[6] A method for producing a recycled polyarylene sulfide resin composition (Y), comprising melt-kneading 100 parts by mass of a recycled material (X) that is a pulverized product containing a polyarylene sulfide resin, and a total of 0.1 to 3.0 parts by mass of a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a silicone-based compound. [6a] A method for producing a recycled polyarylene sulfide resin composition (Y), comprising melt-kneading 100 parts by mass of a recycled material (X) containing a polyarylene sulfide resin, and a total of 0.1 to 3.0 parts by mass of a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a silicone-based compound. [7] The method for producing a recycled polyarylene sulfide resin composition (Y) according to [6] or [6a], further comprising selecting a compound (A) prior to melt-kneading, wherein the selection of compound (A) is: if the recycled material (X) contains 1% by mass or more of an elastomer having a reactive functional group relative to the total amount of the recycled material (X), selecting (A-1) a compound (A) containing a total of 95% by mass or more of an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C relative to the total amount of the compound (A); if the recycled material (X) does not contain an elastomer having a reactive functional group or the content of the elastomer having a reactive functional group is less than 1% by mass relative to the total amount of the recycled material (X), selecting (A-1) a compound (A) containing one or more selected from an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, relative to the total amount of the compound (A). [8] A polyarylene sulfide resin composition (Z) comprising the recycled polyarylene sulfide resin composition (Y) according to any one of [1] to [5] and a virgin polyarylene sulfide resin or a virgin polyarylene sulfide resin composition (V).[9] The polyarylene sulfide resin composition (Z) according to [8], wherein the content of the recycled polyarylene sulfide resin composition (Y) is 50 mass% or more relative to the total amount of the recycled polyarylene sulfide resin composition (Y) and the virgin polyarylene sulfide resin or virgin polyarylene sulfide resin composition (V).
[10] A method for improving the release properties of recycled polyarylene sulfide resin or recycled polyarylene sulfide resin composition, comprising: pellets (P) containing polyarylene sulfide resin and / or pulverized articles (X) containing polyarylene sulfide resin; and (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C.; (A-2) a fatty acid derivative; and (A-3) a compound (A) containing one or more selected from silicone-based compounds. The method for improving release properties comprises melt-kneading the total amount of compound (A) to 0.1 to 3.0 parts by mass relative to a total of 100 parts by mass of the pellets (P) containing polyarylene sulfide resin and the pulverized articles (X) containing polyarylene sulfide resin, to form pellets (Y) for recycled polyarylene sulfide resin composition. [10a] A method for improving the releasability of a recycled material (X) containing a polyarylene sulfide resin during recycling, the method comprising melt-kneading the recycled material (X) containing a polyarylene sulfide resin with a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, so that the total amount of compound (A) is 0.1 to 3.0 parts by mass per 100 parts by mass of the recycled material (X) containing a polyarylene sulfide resin.
[11] The method for improving the releasability according to
[10] or [10a], wherein the pellets (P) containing a polyarylene sulfide resin are obtained by recycling an article containing a polyarylene sulfide resin or a polyarylene sulfide resin composition. [11a] The method for improving releasability according to
[10] or [10a], wherein the recycled material (X) containing a polyarylene sulfide resin is a pulverized product or a repellet of an article containing a polyarylene sulfide resin.
[12] Use of compound (A) for improving the mold releasability of recycled polyarylene sulfide resin or recycled polyarylene sulfide resin composition, comprising pellets (P) containing polyarylene sulfide resin and / or pulverized product (X) of an article containing polyarylene sulfide resin, and (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a compound (A) containing one or more selected from a silicone-based compound. The total amount of compound (A) is 0.1 to 3.0 parts by mass relative to a total of 100 parts by mass of pellets (P) containing polyarylene sulfide resin and pulverized product (X) containing polyarylene sulfide resin. Use of compound (A), comprising forming pellets (Y) for recycled polyarylene sulfide resin composition. [12a] Use of a compound (A) for improving the releasability during recycling of a recycled material (X) containing a polyarylene sulfide resin, the recycled material (X) containing a polyarylene sulfide resin, and (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a compound (A) containing one or more selected from a silicone-based compound, the compound (A) being melt-kneaded so that the total amount of the compound (A) is 0.1 to 3.0 parts by mass per 100 parts by mass of the recycled material (X) containing a polyarylene sulfide resin.
[13] The use of the compound (A) according to
[12] or [12a], wherein the pellets (P) containing a polyarylene sulfide resin are obtained by recycling an article containing a polyarylene sulfide resin or a polyarylene sulfide resin composition. [13a] The use of the compound (A) according to
[12] or [12a], wherein the recycled material (X) containing a polyarylene sulfide resin is a pulverized product or a repellet of an article containing a polyarylene sulfide resin.
[0007] According to the present invention, a recycled polyarylene sulfide resin composition having excellent mold releasability and a method for producing the same can be provided. Specifically, a recycled polyarylene sulfide resin composition having excellent mold releasability while suppressing the generation of mold deposits during molding and a method for producing the same can be provided.
[0008] Fig. 1 is a diagram illustrating a double cylindrical test piece for measuring mold release resistance during molding, (a) is a top view, (b) is a bottom view, (c) is a perspective view, and (d) is a dimensional drawing. Fig. 2 is a schematic diagram of a molded body used for evaluating mold deposits, with the upper side being a top view and the lower side being a cross-sectional view.
[0009] An embodiment of the present disclosure will be described in detail below, but the scope of the present disclosure is not limited to the embodiment described herein, and various modifications can be made without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Furthermore, when multiple upper and lower limit values are described for a specific parameter, any of these upper and lower limit values can be combined to form a suitable numerical range. The expression "X to Y" indicating a numerical range means "X or more and Y or less." If a specific description described for one embodiment also applies to other embodiments, that description may be omitted in other embodiments.
[0010] [First embodiment: Recycled polyarylene sulfide resin composition (Y)] The recycled polyarylene sulfide resin composition (Y) according to the present disclosure comprises 100 parts by mass of a recycled material (X) (hereinafter also referred to as "recycled material (X)") containing a polyarylene sulfide resin, and 0.1 to 3.0 parts by mass in total of a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound. By containing 100 parts by mass of recycled material (X) and 0.1 to 3.0 parts by mass of compound (A), the generation of mold deposits during molding of the recycled polyarylene sulfide resin composition (Y) is suppressed, while the releasability from the mold is improved. The recycled polyarylene sulfide resin composition (Y ) can be used alone or as a mixture with virgin material for molding. However, with the above configuration, even when the content of recycled polyarylene sulfide resin composition (Y) is high (the proportion of recycled polyarylene sulfide resin composition (Y) is 50% or more), the number of times a mold release agent needs to be applied to the mold during molding of the recycled polyarylene sulfide resin composition (Y) can be reduced. As a result, the amount of recycled material used can be increased and work efficiency can be improved. Furthermore, even when producing molded products with a large contact area with the mold, excellent mold releasability from the mold can be achieved, expanding the options for part shapes to which recycled materials can be applied. Since mold deposits are suppressed, molded products with excellent appearance can be obtained.
[0011] (Recycled Material (X)) In the first embodiment, the recycled material (X) is a pulverized product of an article containing a polyarylene sulfide resin. In this specification, "recycle" means pulverizing an article (recycled product) such as a molded body and regenerating it as a raw material for use in manufacturing a molded body, "recycled material" means a material to be recycled and used, and "pulverized product of an article containing a polyarylene sulfide resin" means a pulverized product of an article (recycled molded product) containing a polyarylene sulfide resin. In contrast, raw materials not used in manufacturing a molded body (raw materials that have not undergone a molding process) are referred to as "virgin materials," and virgin materials of polyarylene sulfide resins are referred to as "virgin polyarylene sulfide resins." Furthermore, virgin materials of polyarylene sulfide resin compositions are referred to as "virgin polyarylene sulfide resin compositions." The recycled product (recycled product) may be a molded product, or may be one that was discharged after being retained in a cylinder for a long period of time during molding. Examples include defective products generated during the manufacturing process of molded products, parts other than the product obtained during injection molding (e.g., runners, sprues, etc.), unused products, and chunks of polyarylene sulfide resin material used for purging during molding. In one embodiment, the recycled material (X), which is a pulverized product of an article containing polyarylene sulfide resin, may be a resin-containing material recycled from an article containing virgin polyarylene sulfide resin, or may be a resin-containing material recycled from an article containing recycled polyarylene sulfide resin. As described above, "virgin polyarylene sulfide resin" refers to a polyarylene sulfide resin that has never undergone a molding process. Polyarylene sulfide resin that has not undergone a molding process does not have a thermal history during molding. In contrast, recycled polyarylene sulfide resin has a thermal history of being heated at high temperatures during the manufacturing stage of the recycled molded product.
[0012] The polyarylene sulfide resin is a resin having a repeating unit represented by the following general formula (I): -(Ar-S)- (I) (where Ar represents an arylene group).
[0013] The arylene group is not particularly limited, but examples thereof include a p-phenylene group, an m-phenylene group, an o-phenylene group, a substituted phenylene group, a p,p'-diphenylene sulfone group, a p,p'-biphenylene group, a p,p'-diphenylene ether group, a p,p'-diphenylene carbonyl group, and a naphthalene group.
[0014] The polyarylene sulfide resin can be a homopolymer using the same repeating unit represented by the general formula (I) above, or a copolymer containing different repeating units. A preferred homopolymer has a p-phenylene group as the arylene group, that is, a p-phenylene sulfide group as the repeating unit. This is because homopolymers having a p-phenylene sulfide group as the repeating unit have extremely high heat resistance and exhibit high strength, high rigidity, and high dimensional stability over a wide temperature range. By using such homopolymers, molded articles with excellent physical properties can be obtained.
[0015] As the copolymer, a combination of two or more different arylene sulfide groups among the above-mentioned arylene group-containing arylene sulfide groups can be used. Among these, a combination containing a p-phenylene sulfide group and an m-phenylene sulfide group is preferred from the viewpoint of obtaining a molded product with high physical properties such as heat resistance, moldability, and mechanical properties. A polymer containing 70 mol% or more of p-phenylene sulfide groups is more preferred, and a polymer containing 80 mol% or more is even more preferred. The polyarylene sulfide resin containing phenylene sulfide groups is a polyphenylene sulfide resin (PPS resin).
[0016] Polyarylene sulfide resins are generally known to have a substantially linear molecular structure without branching or crosslinking, or a structure with branching or crosslinking, depending on the production method thereof. In one embodiment, from the viewpoint of improving the toughness of a molded article, it is more preferable that the polyarylene sulfide resin does not contain a structure with a crosslinking structure.
[0017] The melt viscosity of the recycled material (X) is not limited as long as it does not impair the effects of the present disclosure, and is preferably 310°C and a shear rate of 1200 sec. -1The melt viscosity measured by the method may be 5 to 300 Pa·s, or may be 8 to 250 Pa·s.
[0018] The recycled material (X) may contain other components contained in the recycled molded product. In one embodiment, the content of the polyarylene sulfide resin in the recycled material (X) is preferably 30 to 99% by mass, more preferably 50 to 95% by mass, based on the total amount of the recycled material (X). In one embodiment, the content of the polyarylene sulfide resin in the thermoplastic resin (excluding elastomers) contained in the recycled material (X) is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, based on the total amount of the thermoplastic resin (excluding elastomers).
[0019] Other components that may be contained in the recycled material (X) include, for example, elastomers, organic or inorganic fillers, and other additives that are generally added to thermoplastic resins (for example, flame retardants, colorants such as dyes and pigments, stabilizers such as antioxidants and ultraviolet absorbers, lubricants, crystallization accelerators, crystal nucleating agents, etc.).
[0020] Examples of the elastomer include an olefin-based elastomer, a styrene-based elastomer, a polyester-based elastomer, and the like, which may be grafted. It is preferable that the composition contains one or more selected from these, and it is more preferable that the composition contains an olefin-based elastomer.
[0021] The elastomer may be an elastomer having a reactive functional group, such as an acid-modified elastomer modified with an acid or acid anhydride, such as (meth)acrylic acid or maleic anhydride; an elastomer using a copolymerizable monomer having a glycidyl group or an epoxy group (glycidyl (meth)acrylate, etc.); or an epoxy-modified elastomer obtained by epoxidizing the unsaturated bond of an elastomer.
[0022] Examples of olefin-based elastomers include copolymers of α-olefins and copolymers of α-olefins and copolymerizable monomers. The α-olefin is preferably one or more selected from α-olefins having 2 to 13 carbon atoms (e.g., ethylene, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, etc.). Examples of copolymers of α-olefins and copolymerizable monomers include, but are not limited to, α-olefin-unsaturated carboxylic acid alkyl ester copolymers and olefin-based copolymers containing structural units derived from α-olefins and structural units derived from glycidyl esters of α,β-unsaturated acids. Examples of glycidyl esters of α,β-unsaturated acids include, but are not limited to, acrylic acid glycidyl ester, methacrylic acid glycidyl ester, and ethacrylic acid glycidyl ester. Specific preferred examples of the olefin-based elastomer include ethylene propylene rubber (EPR), ethylene-glycidyl methacrylate copolymer (E-GMA), ethylene-glycidyl methacrylate-methyl acrylate copolymer (E-GMA-MA), etc. The olefin-based elastomer may be contained alone or in combination of two or more kinds.
[0023] Examples of styrene-based elastomers include block copolymers composed of a polymer block mainly composed of a vinyl aromatic compound such as styrene and a polymer block mainly composed of an unhydrogenated and / or hydrogenated conjugated diene compound. Specific preferred examples of styrene-based elastomers include styrene-butadiene rubber (SBR) and styrene-ethylene-butylene-styrene block copolymer (SEBS). Furthermore, the styrene-based elastomer may be a modified copolymer into which a functional group (epoxy group, carboxy group, acid anhydride group, etc.) has been introduced. Examples of modified copolymers include epoxidized styrene-diene copolymers in which the unsaturated bond of the diene has been epoxidized (e.g., epoxidized styrene-diene-styrene block copolymers or hydrogenated polymers thereof). The styrene-based elastomers may be used alone or in combination of two or more.
[0024] Examples of polyester-based elastomers include block copolymers having an aromatic polyester such as polyethylene terephthalate or polybutylene terephthalate as a hard segment and a polyether such as polyethylene glycol or polytetramethylene glycol, or an aliphatic polyester such as polyethylene adipate, polybutylene adipate or polycaprolactone as a soft segment. One type of polyester-based elastomer may be contained alone, or two or more types may be contained in combination.
[0025] Elastomers are sometimes blended with virgin materials to improve impact resistance, etc. However, in recycled materials, at least a portion of the chemical structure may change due to shearing during crushing of the recycled product or thermal history due to undergoing one or more molding processes, which can cause deterioration in mold releasability. In particular, if the elastomer has reactive functional groups, mold releasability may be further impaired when molding a recycled polyarylene sulfide resin composition. However, with the recycled polyarylene sulfide resin composition (Y) according to the present disclosure, mold releasability during molding can be improved even when the recycled material (X) contains an elastomer (especially an elastomer having reactive functional groups). In one embodiment, the recycled material (X) may contain an elastomer having reactive functional groups. In another embodiment, the recycled material (X) does not contain an elastomer having reactive functional groups, or the content of the elastomer may be less than 5% by mass, less than 1% by mass, or less than 0.01% by mass relative to the total amount of the recycled material (X).
[0026] The term "reactive functional group" as used herein refers to a functional group that has a high affinity (reactivity) with a metal material at the melting temperature of the resin. Examples of reactive functional groups include glycidyl groups, epoxy groups, carboxyl groups, hydroxyl groups, acid anhydride groups, salts of carboxyl groups, carboxylic acid ester groups, amide groups, amino groups, isocyanate groups, isothiocyanate groups, acetoxy groups, silanol groups, alkoxysilane groups, alkynyl groups, oxazoline groups, thiol groups, and sulfonic acid groups. In one embodiment, the elastomer may include an olefin-based elastomer, a styrene-based elastomer, or a polyester-based elastomer containing one or more groups selected from the group consisting of glycidyl groups, epoxy groups, carboxyl groups, hydroxyl groups, acid anhydride groups, salts of carboxyl groups, carboxylic acid ester groups, amide groups, and amino groups, isocyanate groups, isothiocyanate groups, acetoxy groups, silanol groups, alkoxysilane groups, alkynyl groups, oxazoline groups, thiol groups, and sulfonic acid groups.
[0027] In one embodiment, the recycling material (X) may contain, as the elastomer having a reactive functional group, one or more selected from an olefin-based elastomer containing a structural unit derived from an α-olefin and a structural unit derived from a glycidyl ester of an α,β-unsaturated acid, and a styrene-based elastomer containing an epoxidized styrene-diene copolymer in which the unsaturated bond of the diene has been epoxidized.
[0028] In one embodiment, the reclaimed material (X) may include an elastomer including structural units derived from an α-olefin and structural units derived from a glycidyl ester of an α,β-unsaturated acid. In one embodiment, the reclaimed material (X) may include an elastomer including a glycidyl ester of methacrylic acid.
[0029] In one embodiment, when the elastomer has a reactive functional group, the content of the reactive functional group may be 0.1 to 10 mass %, or may be 0.5 to 8 mass %, of the total amount of the elastomer. The content of the reactive functional group can be calculated from the manufacturer's catalog value of the copolymer composition and the molecular weight of the functional group.
[0030] In one embodiment, the content of the elastomer is preferably 1% by mass or more, more preferably 1 to 20% by mass, and even more preferably 2 to 15% by mass, based on the total amount of the recycled material (X). In one embodiment, the recycled material (X) may contain the elastomer having a reactive functional group in an amount of 1% by mass or more, 2% by mass or more, or 3 to 10% by mass, based on the total amount of the recycled material (X).
[0031] In another embodiment, the content of the elastomer can be less than 1% by mass, less than 0.8% by mass, or even 0% by mass, based on the total amount of the recycling material (X).
[0032] Examples of organic or inorganic fillers include fibrous fillers such as glass fibers, carbon fibers, zinc oxide fibers, titanium oxide fibers, wollastonite, silica fibers, silica-alumina fibers, alumina fibers, zirconia fibers, boron nitride fibers, silicon nitride fibers, boron fibers, potassium titanate fibers, stainless steel fibers, aluminum fibers, titanium fibers, copper fibers, brass fibers, polyamides, high molecular weight polyethylene, aramids, fluororesins, polyester resins, and acrylic resins, and other high-melting point organic fibrous substances; carbon black, graphite, silica, quartz powder, glass beads, Examples of fillers include milled glass fiber, glass balloons, glass powder, talc (granular), silicates such as calcium silicate, aluminum silicate, and diatomaceous earth, metal oxides such as iron oxide, titanium oxide, zinc oxide, and granular alumina, metal carbonates such as calcium carbonate and magnesium carbonate, metal sulfates such as calcium sulfate and barium sulfate, and powdery and granular fillers such as silicon carbide, silicon nitride, boron nitride, and various metal powders; and plate-like fillers such as mica, glass flakes, talc (plate-like), mica, kaolin, clay, alumina (plate-like), and various metal foils. In terms of mechanical strength, heat resistance, etc., it is preferable to contain an inorganic filler.
[0033] The content of the organic or inorganic filler in the material to be recycled (X) is preferably 10 to 70% by mass, more preferably 15 to 65% by mass, and even more preferably 20 to 60% by mass.
[0034] The method for producing the recycled material (X), which is a pulverized product of an article containing a polyarylene sulfide resin, is not limited, and for example, it can be obtained by pulverizing a molded product of a polyarylene sulfide resin (preferably a molded product of a virgin polyarylene sulfide resin) using a known pulverizer.
[0035] Examples of the recycled molded article that can be used as the raw material for the recycled material (X) include defective products generated during the manufacturing process of molded articles, parts other than the product obtained during injection molding (e.g., runners, sprues, etc.), unused products, and chunks of polyethylene sulfide resin material used for purging during molding, and it is preferable that the recycled molded article contains one or more selected from these. In one embodiment, the recycled molded article can be an injection molded article.
[0036] The average particle size of the particles after pulverizing the recycled molded article is not limited, and for example, the volume-based cumulative 50% diameter (D50) measured by a laser diffraction scattering method is preferably 0.3 to 20 mm, more preferably 0.4 to 15 mm, even more preferably 1 to 10 mm, and more preferably 1 to 3 mm.
[0037] (Compound (A)) Examples of compound (A) include (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C (hereinafter also referred to as "(A-1) olefin resin"), (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, and it is preferable to contain one or more selected from these. By containing compound (A), the releasability of the recycled polyarylene sulfide resin composition (Y) from a mold during molding is improved.
[0038] In one embodiment, the content of one or more selected from (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa s, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound is preferably 95 mass% or more in total, and more preferably 98 mass% or more in total, based on the total amount of compound (A). It is even more preferable that compound (A) consists of one or more selected from these.
[0039] Examples of the olefin resin (A-1) having a melt viscosity of 0.1 to 8.0 Pa s at 140°C include polyolefin resins having a degree of polymerization of about 500 to 1000 and 1 to 10 (preferably 1 to 4) carbon atoms, and specific examples include polyethylene resins, polypropylene resins, and ethylene-olefin copolymers having a degree of polymerization of 500 to 1000. These olefin resins (A-1) may be used alone or in combination of two or more. Among these, it is preferable to contain a polyethylene resin and / or a polypropylene resin, and it is more preferable to contain a polyethylene resin.
[0040] The melt viscosity of the (A-1) olefin resin at 140°C is 0.1 to 8.0 Pa·s, preferably 0.5 to 7.0 Pa·s, more preferably 1.0 to 6.5 Pa·s, and particularly preferably 2.0 to 6.0 Pa·s. (A-1) Olefin resins having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C have good dispersibility in the recycled material (X) and are easily dispersed uniformly. As a result, good release properties can be easily improved. Furthermore, since the (A-1) olefin resin is less likely to decompose during molding, it is easy to reduce volatile components derived from the (A-1) olefin resin, and mold deposits (MD) can be reduced. The melt viscosity at 140°C can be measured using a B-type viscometer (for example, the "RB-80H" manufactured by Toki Sangyo Co., Ltd.) based on JIS K7117.
[0041] The (A-2) fatty acid derivative is a substituted saturated fatty acid and / or unsaturated fatty acid having at least one carboxyl group, or a compound obtained by a chemical reaction between a saturated fatty acid and / or an unsaturated fatty acid and another compound. Examples of the (A-2) fatty acid derivative include fatty acid salts, fatty acid esters, and fatty acid amides, and it is preferable to include at least one selected from these.
[0042] Examples of fatty acid salts include fatty acid metal salts, such as lithium salts, calcium salts, magnesium salts, zinc salts, and aluminum salts of fatty acids (preferably saturated or unsaturated C8-35 fatty acids, more preferably saturated or unsaturated C10-20 fatty acids). Examples of saturated or unsaturated C8-35 fatty acids include saturated fatty acids such as lauric acid (dodecanoic acid), isodecanoic acid, tridecylic acid, myristic acid (tetradecanoic acid), pentadecylic acid, palmitic acid (hexadecanoic acid), margaric acid (heptadecanoic acid), stearic acid (octadecanoic acid), isostearic acid, tuberculostearic acid (nonadecanoic acid), 2-hydroxystearic acid, arachidic acid (icosanoic acid), behenic acid (docosanoic acid), lignoceric acid (tetradocosanoic acid), cerotic acid (hexadocosanoic acid), montanic acid (octadocosanoic acid), and melissic acid. and unsaturated fatty acids such as myristoleic acid (tetradecenoic acid), palmitoleic acid (hexadecenoic acid), oleic acid (cis-9-octadecenoic acid), elaidic acid (trans-9-octadecenoic acid), ricinoleic acid (octadecadienoic acid), vaccenic acid (cis-11-octadecenoic acid), linoleic acid (octadecadienoic acid), linolenic acid (9,11,13-octadecatrienoic acid), elestearic acid (9,11,13-octadecatrienoic acid), gadoleic acid (icosanoic acid), erucic acid (docosanoic acid), and nervonic acid (tetradocosanoic acid). These fatty acid metal salts may be used alone or in combination of two or more. Among these, from the viewpoints of cost and availability, zinc salts, calcium salts, or aluminum salts of fatty acids having less than 22 carbon atoms, such as lauric acid, myristic acid, palmitic acid, stearic acid, and oleic acid, are preferred, with calcium stearate and magnesium stearate being more preferred.
[0043] Examples of fatty acid esters include esters of aliphatic alcohols and fatty acids, with esters of polyhydric alcohols and fatty acids being preferred. Examples of polyhydric alcohols include glycol, polyglycol, glycerin, polyglycerin, propylene glycol, pentaerythritol, sorbitol, mannitol, and the like. Examples of fatty acids include saturated or unsaturated C8-35 fatty acids (preferably C10-20 fatty acids), and examples thereof include the fatty acids described above for the fatty acid metal salts. These fatty acid esters may be used alone or in combination of two or more. Among these, from the standpoints of cost and availability, esters of one or more selected from glycol, propylene glycol, and pentaerythritol with one or more fatty acids selected from fatty acids having less than 22 carbon atoms, such as lauric acid, myristic acid, palmitic acid, stearic acid, and oleic acid, are preferred, with pentaerythritol stearates such as pentaerythritol tristearate and pentaerythritol tetrastearate being more preferred.
[0044] Examples of fatty acid amides include C8-35 fatty acid amides and alkylene fatty acid amides. Examples of C8-35 fatty acid amides include oleic acid amide, stearic acid amide, erucic acid amide, behenic acid amide, ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, and ethylene bislauric acid amide. Examples of alkylene fatty acid amides include methylene bisstearic acid amide and ethylene bisstearic acid amide. These fatty acid amides may be used alone or in combination of two or more. Of these, ethylene bisstearic acid amide is more preferred from the viewpoints of cost and availability.
[0045] Examples of the silicone compound (A-3) include silicone oil and silicone resin. The silicone compound (A-3) may be used alone or in combination of two or more. Among these, silicone oil is more preferred from the viewpoints of cost and availability.
[0046] Research by the present inventors has revealed that when the recycled material (X) contains an elastomer having a reactive functional group, the releasability can be further improved by selecting and using, from the above-mentioned compound (A), a compound (A) having a high content of (or consisting of) (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s.
[0047] In one embodiment, when the recycled material (X) contains an elastomer having a reactive functional group (preferably the content of the elastomer having a reactive functional group is preferably 1% by mass or more, more preferably 3 to 10% by mass, relative to the total amount of the recycled material (X)), from the viewpoint of further improving releasability, the compound (A) preferably contains (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, more preferably 95% by mass or more, or 98% by mass or more, of the (A-1) olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, relative to the total amount of the compound (A), and even more preferably consists of (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C.
[0048] In one embodiment, when the recycled material (X) contains an elastomer having a reactive functional group (preferably the content of the elastomer having a reactive functional group is preferably 1% by mass or more, more preferably 3 to 10% by mass, based on the total amount of the recycled material (X)), the compound (A) preferably contains (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140°C in an amount of 95% by mass or more, based on the total amount of the compound (A), and does not contain (A-2) a fatty acid derivative or (A-3) a silicone-based compound, or the content of (A-2) a fatty acid derivative and (A-3) a silicone-based compound is less than 5% by mass in total, based on the total amount of the compound (A).
[0049] In one embodiment, the recycled material (X) includes an elastomer containing structural units derived from an α-olefin and structural units derived from a glycidyl ester of an α,β-unsaturated acid, and the compound (A) contains 95% by mass or more (preferably 98% by mass or more, and more preferably 98% by mass or more, of an olefin resin (A-1) having a melt viscosity at 140°C of 0.1 to 8.0 Pa s) relative to the total amount of the compound (A).
[0050] In another embodiment, when the recycled material (X) does not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass%, preferably less than 0.8 mass%, of the total amount of the recycled material (X), the compound (A) may contain one or more selected from the above-mentioned (A-1) olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) fatty acid derivative, and (A-3) silicone-based compound, and from the viewpoint of easier improvement of releasability, it preferably contains one or more selected from (A-1) olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C and (A-2) fatty acid ester.
[0051] In one embodiment, compound (A) may be an organic substance that is solid or liquid at room temperature (20 to 25°C). Organic substances that are solid or liquid at room temperature (20 to 25°C) may be melt-kneaded with the recycling material (X) during re-pelletization. The resulting re-pellet contains compound (A) in the matrix of the recycling material (X). In this specification, room temperature (20 to 25°C) preferably means 25°C. In another embodiment, compound (A) may be an organic substance that is solid at room temperature (20 to 25°C) and has a melting point of 50 to 135°C (preferably 55 to 130°C, more preferably 70 to 125°C, 90 to 120°C). The melting point is a value measured according to the DSC method (method described in JIS K7121).
[0052] (Content) The content of compound (A) is 0.1 to 3.0 parts by mass relative to 100 parts by mass of the recycled material (X), preferably 0.15 to 2.5 parts by mass, more preferably 0.2 to 2.0 parts by mass, even more preferably 0.3 to 1.5 parts by mass, and particularly preferably 0.4 to 1.2 parts by mass. By making the content 0.1 parts by mass or more relative to 100 parts by mass of the recycled material (X), the releasability from the mold when molding the recycled material (X) can be improved. By making the content 3.0 parts by mass or less, the occurrence of mold deposits (MD) can be suppressed. The total coating amount of compound (A) may be 0.4 parts by mass, 0.8 parts by mass, or 1.2 parts by mass within the range of 0.1 to 3.0 parts by mass relative to 100 parts by mass of the recycled material (X), and these may be the upper and / or lower limits.
[0053] (Other Additives) The recycled polyarylene sulfide resin composition (Y) may contain additives as needed. Examples of the additives include the same components as those that may be contained in the recycled material (X) described above.
[0054] (Mold Release Resistance) In one embodiment, the recycled polyarylene sulfide resin composition (Y) preferably has a molded product with a mold release resistance of 410 N or less, more preferably 405 N or less, and even more preferably 400 N or less. The mold release resistance value is the double cylinder mold release resistance value, and refers to the resistance when releasing the double cylindrical molded product shown in FIG. 1 from the mold. FIG. 1(a) is a top view of the double cylindrical molded product, FIG. 1(b) is a bottom view of the double cylindrical molded product, FIG. 1(c) is a perspective view of the double cylindrical molded product, and FIG. 1(d) is a dimensional diagram of the double cylindrical molded product, with the dimensions in FIGS. 1(a) and 1(d) being in mm. The gate size of the double cylindrical molded product is 5 mm x 2.5 mm.
[0055] The double cylindrical molded product shown in Figure 1 has a double cylindrical shape with a first cylinder 1 on the inside and a second cylinder 2 on the outside, and the first cylinder 1 and the second cylinder 2 are connected at four points by a 4 mm axis. The first cylinder 1 has a height of 20 mm, an outer diameter of 18 mm, and an inner diameter of 9 mm, while the second cylinder 2 has a height of 40 mm, an outer diameter of 40 mm, and an inner diameter of 30 mm. The thickness of the side surface of the first cylinder 1 is 4.5 mm, and the thickness of the bottom and side surfaces of the second cylinder 2 is 5 mm. The second cylinder 2 is a bottomed cylinder, but has an opening at the portion of the first cylinder 1.
[0056] (Mold Adhesion) In one embodiment, the recycled polyarylene sulfide resin composition (Y) preferably has a mold adhesivity of 100 μg or less, more preferably 90 μg or less, and even more preferably 80 μg or less, measured under the following conditions. A molded article having the dimensions and shape shown in FIG. 2 is continuously molded for 4 hours (1,000 times) using the injection molding machine and conditions described below. The total weight of the vent portion and cavity portion removed from the mold is measured before and after continuous molding. The change in the total weight of the vent portion and cavity portion before and after continuous molding is calculated as the weight (μg) of the adhesivity to the mold. Injection molding machine: FANUC ROBOSHOT S2000i30A Cylinder temperature: 340°C Injection time: 2 seconds Cooling time: 10 seconds Mold temperature: 140°C
[0057] (Uses) The recycled polyarylene sulfide resin composition (Y) can be suitably used as a resin composition for injection molding or a resin composition for extrusion molding.
[0058] [Second embodiment: Method for producing recycled polyarylene sulfide resin composition (Y)] The method for producing recycled polyarylene sulfide resin composition (Y) according to this embodiment includes melt-kneading 100 parts by mass of recycled material (X) containing polyarylene sulfide resin and 0.1 to 3.0 parts by mass of compound (A), together with additives used as needed. In the second embodiment, recycled material (X) is a pulverized product containing polyarylene sulfide resin. The compound (A) and additives, as well as the amounts of each component, are the same as in the first embodiment, and therefore will not be described here.
[0059] (Melt-Kneading Step) The melt-kneading temperature is equal to or higher than the melting point of the recycling material (X), and is usually 280 to 360°C, preferably 290 to 350°C.
[0060] The mixing method is not particularly limited as long as it can uniformly mix the recycled material (X) and the compound (A), and examples thereof include a melt-kneading method using a conventional melt-kneading device such as a single-screw or twin-screw extruder. After melt-kneading and extruding the components, the resulting recycled polyarylene sulfide resin composition (Y) can be processed into a desired form such as powder, flakes, or pellets.
[0061] (Compound (A) Selection Step) In one embodiment, the method for producing the recycled polyarylene sulfide resin composition (Y) preferably includes a step of selecting the compound (A) prior to melt-kneading in order to further improve the releasability of the recycled polyarylene sulfide resin composition (Y). As described above, when the recycled material (X) contains an elastomer having a reactive functional group, the compound (A) can be further improved in releasability by selecting and using a compound (A) that has a high content of (or consists of) an olefin resin (A-1) having a melt viscosity at 140°C of 0.1 to 8.0 Pa s.
[0062] In one embodiment, the step of selecting the compound (A) comprises: when the recycled material (X) contains an elastomer having a reactive functional group in an amount of 1% by mass or more (preferably 2% by mass or more, more preferably 3 to 10% by mass) relative to the total amount of the recycled material (X), selecting (A-1) a compound (A) containing an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa s; preferably selecting (A-1) a compound (A) containing an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa s; When the recycled material (X) does not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1% by mass, preferably less than 0.8% by mass, of the total amount of the recycled material (X), a compound (A) is selected that contains one or more selected from (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound in a total amount of 95% by mass or more relative to the total amount of the compound (A) (preferably consisting of one or more selected from these), preferably a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s and (A-2) a fatty acid ester, more preferably a compound (A) containing one or more selected from a C1-4 olefin resin such as a polyethylene resin, an ethylene copolymer, or a polypropylene resin; and a C8-35 fatty acid ester such as pentaerythritol tristearate or pentaerythritol tetrastearate.
[0063] [Third embodiment: Method for manufacturing a molded article containing recycled polyarylene sulfide resin composition (Y)] The recycled polyarylene sulfide resin composition (Y) can be molded and processed by known methods such as injection molding, profile / solidification extrusion, press molding, and spinning. The recycled polyarylene sulfide resin composition (Y) has excellent mold releasability, so the number of times a mold release agent is applied to the mold during molding can be reduced. Furthermore, even when producing a molded article with a large contact area with the mold, the excellent mold releasability from the mold allows for a wider range of part shape options.
[0064] In one embodiment, a method for producing a molded article containing the recycled polyarylene sulfide resin composition (Y) includes continuously injecting or extruding the recycled polyarylene sulfide resin composition (Y) into a mold together with other thermoplastic resins and additives as needed, and applying a release agent to the mold, where the release agent may be applied to the mold once for every 10 or more injections or extrusions. The release agent applied to the mold is not limited and can be selected from known release agents.
[0065] The recycled polyarylene sulfide resin composition (Y) has excellent releasability from a mold, so even when a molded article with a large contact area with the mold is injection molded or extrusion molded, the number of times a mold release agent is applied to the mold can be reduced.
[0066] [Fourth embodiment: Polyarylene sulfide resin composition (Z)] The above-mentioned recycled polyarylene sulfide resin composition (Y) can be mixed with other thermoplastic resins as needed to be used as a molding material. Examples of other thermoplastic resins include virgin polyarylene sulfide resins, and preferably virgin polyarylene sulfide resins or virgin polyarylene sulfide resin compositions.
[0067] In one embodiment, the polyarylene sulfide resin composition (Z) preferably contains a recycled polyarylene sulfide resin composition (Y) and a virgin polyarylene sulfide resin or a virgin polyarylene sulfide resin composition (V). By including the recycled polyarylene sulfide resin composition (Y), recycled materials can be effectively utilized, and a resin composition with excellent mold releasability can be obtained. Furthermore, the occurrence of mold deposits during molding can be suppressed. By including a virgin polyarylene sulfide resin or a virgin polyarylene sulfide resin composition (V), the excellent physical properties of the polyarylene sulfide resin can be reinforced. As described above, the "virgin polyarylene sulfide resin composition" refers to a virgin material of the polyarylene sulfide resin composition. In order to increase the amount of recycled material used, the content of the recycled polyarylene sulfide resin composition (Y) is preferably 50% by mass or more, more preferably 50 to 99.99% by mass, and even more preferably 60 to 100% by mass, of the total amount of the recycled polyarylene sulfide resin composition (Y) and the virgin polyarylene sulfide resin or virgin polyarylene sulfide resin composition (V). The polyarylene sulfide resin composition (Z) has excellent releasability from a mold even when the content of the recycled polyarylene sulfide resin composition (Y) is high.
[0068] Examples of the polyarylene sulfide resin contained in the virgin polyarylene sulfide resin or virgin polyarylene sulfide resin composition (V) include those described for the recycled material (X) in the first embodiment. From the viewpoint of quality control, it is preferable that the composition be the same as that of the polyarylene sulfide resin in the recycled material (X). The virgin polyarylene sulfide resin composition, like the recycled material (X), can contain other components such as compound (A), elastomer, organic or inorganic filler, release agent, other additives generally added to thermoplastic resins (e.g., flame retardants, colorants such as dyes and pigments, stabilizers such as antioxidants and UV absorbers, lubricants, crystallization accelerators, crystal nucleating agents, etc.). Details of the other components are as described in the first embodiment. In one embodiment, from the viewpoint of quality control, it is preferable that the virgin polyarylene sulfide resin composition has the same composition as the recycled polyarylene sulfide resin composition (Y) (e.g., the type and content of additives are the same). In one embodiment, when the recycled polyarylene sulfide resin composition (Y) does not contain an elastomer having a reactive functional group, it is preferable that the virgin polyarylene sulfide resin or virgin polyarylene sulfide resin composition (V) also does not contain an elastomer having a reactive functional group. In this case, the virgin polyarylene sulfide resin or virgin polyarylene sulfide resin composition (V) may or may not contain compound (A). When compound (A) is contained, the type thereof is not limited. In another embodiment, when the recycled polyarylene sulfide resin composition (Y) contains an elastomer having a reactive functional group, it is preferable that the virgin polyarylene sulfide resin or virgin polyarylene sulfide resin composition (V) also contains an elastomer having a reactive functional group, and it is more preferable that the type and content of the elastomer are the same. In this case, the virgin polyarylene sulfide resin or the virgin polyarylene sulfide resin composition (V) preferably contains the compound (A), and it is more preferable to select (A-1) an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa s.
[0069] The melt viscosity of the virgin polyarylene sulfide resin is not particularly limited as long as it is within a range that does not impair the effects of the present disclosure. However, from the viewpoint of the balance between mechanical properties and fluidity, it is preferable to use a melt viscosity of 310°C and a shear rate of 1200 sec. -1 The melt viscosity measured by is preferably 300 Pa·s or less, more preferably 250 Pa·s or less.
[0070] The method for producing the polyarylene sulfide resin composition (Z) is not limited, and the recycled polyarylene sulfide resin composition (Y) and another thermoplastic resin (preferably a virgin polyarylene sulfide resin) may be dry blended, or may be melt-kneaded using a conventionally known melt-kneading device such as a single-screw or twin-screw extruder, or may be mixed in the hopper (material supply member) of an injection molding machine.
[0071] The method for producing a molded article containing the polyarylene sulfide resin composition (Z) can be carried out in the same manner as the method for producing a molded article containing the recycled polyarylene sulfide resin composition (Y) described in the third embodiment.
[0072] (Uses) The polyarylene sulfide resin composition (Z) can be suitably used as a resin composition for injection molding or a resin composition for extrusion molding.
[0073] [Fifth embodiment: method for improving mold releasability] A method for improving the mold releasability of recycled polyarylene sulfide resin or recycled polyarylene sulfide resin composition according to the present disclosure includes melt-kneading pellets (P) containing polyarylene sulfide resin and / or pulverized product (X) of an article containing polyarylene sulfide resin with one or more compounds (A-1) selected from an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, so that the total amount of compound (A) is 0.1 to 3.0 parts by mass relative to a total of 100 parts by mass of pellets (P) containing polyarylene sulfide resin and pulverized product (X) containing polyarylene sulfide resin, to form pellets (Y) for the recycled polyarylene sulfide resin composition.
[0074] "For recycled polyarylene sulfide resin compositions" means that the polyarylene sulfide resin composition is prepared by crushing articles such as molded bodies (recycled products) and regenerating them as raw materials for use in producing molded bodies, or is intended to be used as such raw materials.
[0075] The method for improving mold releasability according to the fifth embodiment can also be expressed as follows. That is, this method for improving mold releasability is a method for improving the mold releasability during recycling of a recycled material (X) containing a polyarylene sulfide resin, and includes a recycled material (X) containing a polyarylene sulfide resin, and (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a compound (A) containing one or more selected from a silicone-based compound. The method includes melt-kneading the recycled material (X) containing a polyarylene sulfide resin so that the total amount of the compound (A) is 0.1 to 3.0 parts by mass relative to 100 parts by mass of the recycled material (X). According to the method of this embodiment, the mold releasability can be improved when recycling the recycled material (X). Furthermore, the occurrence of mold deposits at that time can be suppressed. In the fifth embodiment, the recycled material (X) may be pellets (P) (for example, virgin pellets or repellets) containing a polyarylene sulfide resin, or may be a pulverized product of an article containing a polyarylene sulfide resin or a composition thereof. In one embodiment, the recycled material (X) is preferably a pulverized product or repellet of an article containing a polyarylene sulfide resin or a composition thereof.
[0076] In this specification, "improving mold releasability" means that the mold releasability from a mold during molding of the recycled polyarylene sulfide resin composition is improved compared to when compound (A) is not blended. In one embodiment, the method for improving mold releasability is preferably a method that can improve mold releasability while suppressing the occurrence of mold deposits. "Improving mold releasability during recycling" means that, when the recycled material (X) is virgin pellets containing a polyarylene sulfide resin, the virgin pellets are molded once to obtain a molded product, and then the molded product is crushed into a crushed product or further formed into a repellet, and the mold releasability is improved when the crushed product or repellet is molded. When the recycled material (X) is a crushed product or repellet of an article containing a polyarylene sulfide resin, the mold releasability is improved when the crushed product or repellet is molded.
[0077] When the recycled material (X) is a pulverized product of an article containing a polyarylene sulfide resin, the "pulverized product of an article containing a polyarylene sulfide resin" refers to a pulverized product of an article (molded article to be recycled) containing a polyarylene sulfide resin, as described above. The recycled article (recycled article) may be a molded article, or may be an article that has been retained in a cylinder for a long period of time during molding and then discharged. Examples of the recycled article include defective products generated during the manufacturing process of molded articles, parts other than the product obtained during injection molding (e.g., runners, sprues, etc.), unused products, and chunks of polyarylene sulfide resin material used for purging during molding.
[0078] When the recycled material (X) is a pellet (P) containing a polyarylene sulfide resin, the pellet (P) may be a virgin pellet or a recycled pellet. That is, the polyarylene sulfide resin contained in the pellet (P) containing a polyarylene sulfide resin may be a virgin polyarylene sulfide resin or a recycled polyarylene sulfide resin. When the polyarylene sulfide resin contained in the pellet (P) containing a polyarylene sulfide resin is a virgin polyarylene sulfide resin, a predetermined amount of the above-mentioned compound (A) is blended with the pellet (P) containing the virgin polyarylene sulfide resin, melt-kneaded, and re-pelletized to obtain a compound (A)-containing virgin pellet (P1). In this case, the blending amount of the compound (A) is 0.04 to 3.0 parts by mass per 100 parts by mass of the pellet (P) containing the virgin polyarylene sulfide resin. The compound (A)-containing virgin pellets (P1) can be used as a raw material for a recycled polyarylene sulfide resin composition. That is, the virgin pellets (P1) are once molded into a molded body by a known method such as injection molding or extrusion molding (or discharged after a long residence time in a cylinder during molding), and then crushed and repelletized to form a recycled polyarylene sulfide resin composition. The virgin pellets (P1) have excellent mold releasability when first molded, and also have excellent mold releasability when molded when recycled as pellets (Y) for a recycled polyarylene sulfide resin composition.
[0079] When the polyarylene sulfide resin contained in the pellets (P) containing polyarylene sulfide resin is a recycled polyarylene sulfide resin, a predetermined amount of the above-mentioned compound (A) is blended with the pellets (P) containing recycled polyarylene sulfide resin, melt-kneaded, and re-pelletized to obtain recycled pellets (P2) containing compound (A). The recycled pellets (P2) containing compound (A) can be used as a recycled polyarylene sulfide resin composition. In this case, the amount of compound (A) blended is 0.04 to 3.0 parts by mass per 100 parts by mass of the pellets (P) containing recycled polyarylene sulfide resin. The pellets (P) containing recycled polyarylene sulfide resin are obtained by pulverizing an article containing polyarylene sulfide resin into pellets.
[0080] The shape of the pellets (P) containing the polyarylene sulfide resin is not particularly limited, and may be any shape such as a cylindrical (approximately cylindrical) shape or a spherical shape.
[0081] In one embodiment, the pellets (P) containing the polyarylene sulfide resin are preferably recycled (recycled material) from an article containing a polyarylene sulfide resin or a polyarylene sulfide resin composition. That is, the recycled material (X) containing the polyarylene sulfide resin is preferably a pulverized product or repellet of an article containing the polyarylene sulfide resin.
[0082] Details of the types and amounts of the "polyarylene sulfide resin" and "compound (A)," as well as the compounding method, are the same as those described in the section on the recycled polyarylene sulfide resin composition (Y) and its manufacturing method in the first embodiment.
[0083] [Sixth embodiment: Use of compound (A)] The use of compound (A) according to the present disclosure is the use of compound (A) for improving the demolding properties of recycled polyarylene sulfide resin or recycled polyarylene sulfide resin composition, and includes melt-kneading pellets (P) containing polyarylene sulfide resin and / or pulverized articles containing polyarylene sulfide resin (X) with compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a silicone-based compound so that the total amount of compound (A) is 0.1 to 3.0 parts by mass relative to a total of 100 parts by mass of pellets (P) containing polyarylene sulfide resin and pulverized articles containing polyarylene sulfide resin (X), to form pellets (Y) for the recycled polyarylene sulfide resin composition.
[0084] The use of the compound (A) according to the sixth embodiment can also be expressed as follows. That is, the use of this compound (A) is the use of the compound (A) to improve the releasability during recycling of a recycled material (X) containing a polyarylene sulfide resin, and the polyarylene sulfide resin is recycled as a material (X), and (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa s at 140 ° C., (A-2) a fatty acid derivative, and (A-3) a compound (A) containing one or more selected from a silicone-based compound, and melt-kneading the total amount of the compound (A) to 100 parts by mass of the recycled material (X) to 0.1 to 3.0 parts by mass. By using the compound (A) of this embodiment, the releasability when recycling the recycled material (X) can be improved. In addition, the occurrence of mold deposits at that time can be suppressed.
[0085] In the sixth embodiment, the recycled material (X) may be pellets (P) (e.g., virgin pellets or repellets) containing a polyarylene sulfide resin, or may be a pulverized product of an article containing a polyarylene sulfide resin or a composition thereof. In one embodiment, the recycled material (X) is preferably a pulverized product or repellet of an article containing a polyarylene sulfide resin or a composition thereof. The terms "improving releasability during recycling" and "pellets (P) containing a polyarylene sulfide resin" are as described in the section on the method for improving releasability in the fifth embodiment. When the recycled material (X) is a pulverized product of an article containing a polyarylene sulfide resin, the "pulverized product of an article containing a polyarylene sulfide resin" is as described in the fifth embodiment. When the recycled material (X) is pellets (P) containing a polyarylene sulfide resin, the pellets (P) may be virgin pellets or repellets. The "pellets (P)" are as described in the fifth embodiment. In one embodiment, the pellets (P) containing the polyarylene sulfide resin are preferably recycled (recycled material) from an article containing a polyarylene sulfide resin or a polyarylene sulfide resin composition. That is, the recycled material (X) is preferably a pulverized or re-pelletized article containing the polyarylene sulfide resin. Details of the types and amounts of the "polyarylene sulfide resin" and "compound (A)," as well as the blending method, are the same as those described in the section on the recycled polyarylene sulfide resin composition (Y) and its manufacturing method in the first embodiment.
[0086] The present invention will be explained in more detail below by showing examples, but the interpretation of the present invention is not limited to these examples.
[0087] [Materials] (Recycling material (X1): crushed injection-molded product) An injection-molded product of a resin composition (virgin PPS resin composition (V1) used in Reference Example 1 described later) containing 65 mass% polyphenylene sulfide resin (manufactured by Kureha Corporation, Fortron (registered trademark) KPS), 30 mass% glass fiber, and 4 mass% elastomer (composition: E-GMA-MA (glycidyl methacrylate content: 3 mass%)), with the remainder being additives, was crushed in a mechanical crusher to obtain crushed injection-molded product (recycling material) (X1).
[0088] (Recycled material (X2): crushed injection-molded product) An injection-molded product of a resin composition (containing 69 mass % of polyphenylene sulfide resin (manufactured by Kureha Corporation, Fortron (registered trademark) KPS), 30 mass % of glass fiber, and the remainder being additives (containing no elastomer component; the virgin PPS resin composition (V2) used in Reference Example 2 described later)) was crushed in a mechanical crusher to obtain crushed injection-molded product (recycled material) (X2).
[0089] (Recycled material (X3): crushed injection-molded product) An injection-molded product of a resin composition containing 0.4 parts by mass of compound (A1) per 100 parts by mass of the virgin PPS resin composition (V1) used in Reference Example 1 described later was crushed using a mechanical crusher to obtain crushed injection-molded product (recycled material) (X3).
[0090] Compound (A1): polyethylene resin (manufactured by Sanyo Chemical Industries, Ltd., "SANWAX 161-P", melting point 103°C, melt viscosity at 140°C 4.3 Pa s) Compound (A2): pentaerythritol stearate (manufactured by NOF Corporation, "UNISTAR H476", melting point 63°C) The melting points of compound (A1) and compound (A2) and the melt viscosity at 140°C of compound (A1) were measured by the following method. (Melting Point) Using a DSC device (differential scanning calorimeter, DSC-Q1000, manufactured by TA Instruments), the melting point (Tm) was measured by the DSC method (method described in JIS K7121) under conditions of a nitrogen atmosphere and a heating rate of 10°C / min. (Viscosity at 140°C) The viscosity was measured at 140°C using a Brookfield viscometer (RB-80H manufactured by Toki Sangyo Co., Ltd.) in accordance with JIS K7117 (1999).
[0091] [Examples 1 to 6] The pulverized material of the injection-molded product and compound (A1) or compound (A2) shown in Table 1 were dry-blended in the content ratios shown in Table 1. This was fed into a twin-screw extruder with a cylinder temperature of 320°C and melt-kneaded to obtain pellets (repellet) of the recycled polyarylene sulfide resin composition (Y) of Examples 1 to 6.
[0092] [Example 7] The recycled material (X3) was charged into a twin-screw extruder having a cylinder temperature of 320°C and melt-kneaded to obtain pellets (repellet) of the recycled polyarylene sulfide resin composition (Y) of Example 7.
[0093] [Example 8] Recycled material (X1), the virgin PPS resin composition (V1) used in Reference Example 1 described later, and compound (A1) were dry-blended in the content ratios shown in Table 2. This was fed into a twin-screw extruder with a cylinder temperature of 320°C and melt-kneaded to obtain pellets (repellet) of the recycled polyarylene sulfide resin composition (Y) of Example 8.
[0094] Comparative Example 1 Pellets (repellet) of the recycled polyarylene sulfide resin composition of Comparative Example 1 were obtained in the same manner as in Examples 1 to 6, except that compound (A1) or (A2) was not added.
[0095] [Comparative Examples 2 and 3] The recycled material (X1) and the compound (A1) were dry-blended in the content ratios shown in Table 2. This was fed into a twin-screw extruder with a cylinder temperature of 320°C and melt-kneaded to obtain pellets (repellet) of the recycled polyarylene sulfide resin composition (Y) of Comparative Examples 2 and 3.
[0096] [Reference Examples 1 and 2] The following virgin polyarylene sulfide resin compositions (virgin materials) were used in Reference Examples 1 and 2. Virgin PPS resin composition (V1): 65 mass% polyphenylene sulfide resin (manufactured by Kureha Corporation, Fortron (registered trademark) KPS), 30 mass% glass fiber, and 4 mass% elastomer (composition: E-GMA-MA (glycidyl methacrylate content: 3 mass%)), the balance being a resin composition containing additives. Virgin PPS resin composition (V2): 69 mass% polyphenylene sulfide resin (manufactured by Kureha Corporation, Fortron (registered trademark) KPS), and 30 mass% glass fiber, the balance being a resin composition containing additives (no elastomer component).
[0097] [Mold Release Resistance] Using the repellets of the Examples and Comparative Examples and the virgin materials of Reference Examples 1 and 2, the mold release resistance was measured by the following method. The results are shown in Tables 1 and 2. When the mold release resistance is 410 N or less, the mold release property is excellent, when it is 405 N or less, the mold release property is even better, and when it is 400 N or less, the mold release property is even better. Using an injection molding machine, a double cylindrical molded product as shown in FIG. 1 was molded under the following conditions, and the force when the molded piece (test piece) was ejected from the mold was measured, and the measured value was taken as the mold release resistance value. Pressure sensor: "Indirect type in-mold sensor" (Model: 9221A) manufactured by Nippon Kistler Co., Ltd. Injection molding machine: "EC60Ni1.5A" manufactured by Toshiba Machine Co., Ltd. Cylinder temperature: 320°C Injection time: 12 seconds Cooling time: 45 seconds Mold temperature: 150°C
[0098] [Evaluation of Mold Adhesion] Using the repellets of the Examples and Comparative Examples and the virgin materials of Reference Examples 1 and 2, mold adhesion was measured using the following method. The results are shown in Tables 1 and 2. A nested mold with a detachable vent and cavity was used. Using each repellet and the virgin material of Reference Example, molded articles having the dimensions and shape shown in Figure 2 were continuously molded for 4 hours (1,000 times) using the injection molding machine and conditions below. The total weight of the vent and cavity removed from the mold was measured before and after continuous molding. The change in the total weight of the vent and cavity before and after continuous molding was calculated as the weight (μg) of adhesion to the mold. Injection molding machine: FANUC ROBOSHOT S2000i30A Cylinder temperature: 340°C Injection time: 2 seconds Cooling time: 10 seconds Mold temperature: 140°C When the amount of mold adhesion is 100 μg or less, there is an effect of suppressing mold deposits, when it is 90 μg or less there is an excellent effect of suppressing mold deposits, and when it is 80 μg or less there is an even better effect of suppressing mold deposits.
[0099]
[0100] As shown in Tables 1 and 2, the recycled polyarylene sulfide resin compositions (Y) of Examples 1 to 6 containing 100 parts by weight of recycled material (X1) or (X2) and 0.1 to 3.0 parts by weight of compound (A1) or (A2) have a release resistance of 410 N or less, demonstrating excellent release properties. Comparing Examples 2 and 4, when recycled material (X1) containing an elastomer having a reactive functional group is used, compound (A) containing an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C can be used as compound (A), resulting in a release resistance of 400 N or less, achieving even better release properties.
[0101] As shown in Examples 5 and 6, when a recycled material (X2) that does not contain an elastomer having a reactive functional group is used, the release resistance is 270 N or less in both cases where compound (A) contains a fatty acid ester and where compound (A) contains an olefin resin having a melt viscosity at 140°C of 0.1 to 8.0 Pa·s, and even better release properties can be achieved.
[0102] Comparing Examples 1 to 4 with Reference Example 1, and comparing Examples 5 and 6 with Reference Example 2, the recycled material raw materials (X1) and (X2) of Examples 1 to 6 have mold release resistance that is the same as or lower than that of virgin material, and can be molded with good mold releasability from a mold that is the same as or higher than that of virgin material.
[0103] In contrast, the recycled polyarylene sulfide resin of Comparative Example 1 has a mold release resistance exceeding 410 N, and is poor in mold release properties.
[0104] Comparison of Example 7 and Comparative Example 1 shows that by adding compound (A1) to a virgin PPS resin composition in an amount within the specified range, excellent releasability, with a release resistance of 410 N or less, can be achieved even without adding compound (A1) when producing recycled pellets.
[0105] Comparison of Example 8 and Comparative Example 1 shows that blending recycled material with virgin material can achieve excellent mold release properties with a mold release resistance of 410 N or less. In addition, the amount of material adhering to the mold can be reduced.
[0106] As shown in Tables 1 and 2, the recycled polyarylene sulfide resin compositions (Y) of Examples 1 to 8 had mold deposits of 80 g or less, and were more effective in suppressing mold deposits. In contrast, the recycled polyarylene sulfide resin of Comparative Example 3 had mold deposits of more than 100 g, resulting in the generation of large amounts of mold deposits.
[0107] The recycled polyarylene sulfide resin composition (Y) of this embodiment has excellent mold releasability, and can be suitably used as resin pellets for injection molding or extrusion molding, and has industrial applicability.
Claims
1. A recycled polyarylene sulfide resin composition (Y) comprising: 100 parts by mass of a recycled material (X) containing a polyarylene sulfide resin; and 0.1 to 3.0 parts by mass in total of a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound.
2. The recycled polyarylene sulfide resin composition (Y) according to claim 1, wherein the recycled material (X) contains an elastomer having a reactive functional group in an amount of 1 mass% or more based on the total amount of the recycled material (X).
3. The recycled polyarylene sulfide resin composition (Y) according to claim 1 or 2, wherein the recycled material (X) comprises an elastomer comprising a structural unit derived from an α-olefin and a structural unit derived from a glycidyl ester of an α,β-unsaturated acid.
4. The recycled polyarylene sulfide resin composition (Y) according to claim 1 or 2, wherein the recycled material (X) contains an elastomer having a reactive functional group, and the compound (A) contains (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C in an amount of 95 mass% or more relative to the total amount of the compound (A).
5. The recycled polyarylene sulfide resin composition (Y) according to claim 1, wherein the recycled material (X) does not contain an elastomer having a reactive functional group, or the content of the elastomer having a reactive functional group is less than 1 mass% based on the total amount of the recycled material (X).
6. A method for producing a recycled polyarylene sulfide resin composition (Y), comprising melt-kneading 100 parts by mass of a recycled material (X) containing a polyarylene sulfide resin with a total of 0.1 to 3.0 parts by mass of a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound.
7. The method for producing recycled polyarylene sulfide resin composition (Y) according to claim 6, further comprising selecting a compound (A) prior to melt-kneading, wherein the selection of compound (A) comprises: selecting (A-1) a compound (A) containing a total of 95% by mass or more of an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C relative to the total amount of compound (A) when the recycled material (X) contains an elastomer having a reactive functional group at 1% or more by mass relative to the total amount of the recycled material (X); and selecting (A-1) a compound (A) containing a total of 95% by mass or more of one or more selected from an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound relative to the total amount of compound (A) when the recycled material (X) does not contain an elastomer having a reactive functional group or the content of the elastomer having a reactive functional group is less than 1% by mass relative to the total amount of the recycled material (X).
8. A polyarylene sulfide resin composition (Z) comprising the recycled polyarylene sulfide resin composition (Y) according to claim 1 or 2 and a virgin polyarylene sulfide resin or a virgin polyarylene sulfide resin composition (V).
9. The polyarylene sulfide resin composition (Z) described in claim 8, wherein the content of the recycled polyarylene sulfide resin composition (Y) is 50 mass% or more based on the total amount of the recycled polyarylene sulfide resin composition (Y) and the virgin polyarylene sulfide resin or virgin polyarylene sulfide resin composition (V).
10. A method for improving the releasability during recycling of a polyarylene sulfide resin-containing recycled material (X), comprising melt-kneading the polyarylene sulfide resin-containing recycled material (X) with one or more compounds (A) selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, so that the total amount of compound (A) is 0.1 to 3.0 parts by mass per 100 parts by mass of the polyarylene sulfide resin-containing recycled material (X).
11. The method for improving releasability according to claim 10, wherein the recycling material (X) containing a polyarylene sulfide resin is a ground product or a repellet of an article containing a polyarylene sulfide resin.
12. Use of a compound (A) for improving the releasability of a recycled material (X) containing a polyarylene sulfide resin during recycling, comprising melt-kneading the recycled material (X) containing a polyarylene sulfide resin with a compound (A) containing one or more selected from (A-1) an olefin resin having a melt viscosity of 0.1 to 8.0 Pa·s at 140°C, (A-2) a fatty acid derivative, and (A-3) a silicone-based compound, such that the total amount of compound (A) is 0.1 to 3.0 parts by mass per 100 parts by mass of the recycled material (X) containing a polyarylene sulfide resin.
13. Use of the compound (A) according to claim 12, wherein the regenerating material (X) containing a polyarylene sulfide resin is a ground product or a repellet of an article containing a polyarylene sulfide resin.
Citation Information
Patent Citations
Polyphenylene sulfide resin composition
JP1998077408A
Production of polymer blend by recycling high performance polymer
JP1999140221A
Resin composition and tabular insert-molded body
WO2014103814A1
Polyarylene sulfide resin composition
WO2018101399A1
Method for producing glass fiber-reinforced recycled polyphenylene sulfide resin composition, and molded article obtained by molding glass fiber-reinforced recycled polyphenylene sulfide resin composition
WO2023002903A1
Cited By
Method for producing recycled polyarylene sulfide resin composition, and recycled polyarylene sulfide resin composition
JPWO2025094875A1
Method for producing recycled polyarylene sulfide resin composition, and recycled polyarylene sulfide resin composition
WO2025094875A1