Anti-frost hydrogel coating composition, method for manufacturing hydrogel coating film using same, and heat exchanger comprising same

The application of a hydrogel coating with an ionic monomer on heat exchanger surfaces addresses frost formation issues by lowering freezing temperatures and preventing ice growth, enhancing energy efficiency and reducing corrosion.

WO2024205002A1PCT designated stage expired Publication Date: 2024-10-03SAMSUNG ELECTRONICS CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/001338
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-01-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Heat exchangers operating in low-temperature environments face issues with frost formation on aluminum fins, leading to reduced thermal conductivity, increased corrosion, and higher energy consumption due to defrosting processes.

Method used

A hydrogel coating composition containing an ionic monomer, a crosslinking agent, and a polymerization initiator is applied to the heat exchanger surfaces, forming a superhydrophilic hydrogel film that lowers the freezing temperature and inhibits ice nucleation and growth.

Benefits of technology

The hydrogel coating effectively delays frost formation and growth, reducing energy consumption and extending the lifespan of heat exchangers by maintaining thermal efficiency in low-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024001338_03102024_PF_FP_ABST
    Figure KR2024001338_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an anti-frost hydrogel coating composition using an ionic monomer, a method for manufacturing an anti-frost hydrogel coating film, and a heat exchanger comprising the anti-frost hydrogel. The anti-frost hydrogel coating composition comprises: an ionic monomer; a cross-linking agent including two or more acrylic groups; a polymerization initiator; and a solvent, wherein the ionic monomer comprises at least one monomer among Zwitterionic monomers, cationic monomers, and anionic monomers.
Need to check novelty before this filing date? Find Prior Art

Description

Hydrogel coating composition for preventing corrosion, method for producing a hydrogel coating film using the same, and heat exchanger including the same

[0001] The present disclosure relates to a hydrogel coating composition for preventing frost formation comprising an ionic monomer, a method for producing a hydrogel coating film for preventing frost formation using the hydrogel coating composition for preventing frost formation, and a heat exchanger comprising the hydrogel for preventing frost formation.

[0002] Equipment such as heat exchangers, airplanes, and wind turbines that operate in low-temperature environments experience freezing as moisture condenses on their surfaces.

[0003] For example, aluminum fins used in heat exchangers, when operated in low-temperature environments, can experience freezing, where water vapor liquefies on the fin surface due to the temperature difference between the heat exchanger and the surrounding environment, and then the liquefied water freezes on the surface. This freezing phenomenon causes frost to form on the surface, acting as thermal resistance and lowering thermal conductivity. This not only reduces cooling and energy efficiency, but also accelerates corrosion, shortening the lifespan of the heat exchanger.

[0004] To address these issues, a common method is to remove the frost formed on the surface through a defrosting process that involves applying heat using a heater. However, this defrosting method has the disadvantage of consuming additional power.

[0005] Accordingly, research is being conducted to reduce the formation of frost on the surface by applying a water-repellent treatment to the heat exchanger, thereby increasing energy efficiency during the cooling process, and to reduce power consumption during the operation process by reducing the power consumption required for the defrosting process.

[0006] In relation to this, Korean Patent Publication No. 10-2022-0021234 discloses a configuration that reduces freezing temperature by imparting hydrophilicity to an aluminum metal surface using an ethylene glycol-based composition used in antifreeze, thereby reducing freezing on the metal surface.

[0007] One aspect of the present disclosure provides a hydrogel coating composition for preventing sagging using a superhydrophilic ionic monomer that has not previously been used for sagging purposes.

[0008] One aspect of the present disclosure provides a method for coating a superhydrophilic hydrogel capable of further lowering the freezing temperature of a substrate surface by using a hydrogel coating composition comprising an ionic monomer having superhydrophilicity.

[0009] One aspect of the present disclosure is to provide a heat exchanger having a superhydrophilic ionic polymer hydrogel coating on the surface of a fin to further enhance ice nucleation and ice growth prevention performance and an ice adhesion reduction effect, in order to lower the freezing temperature of the surface of a device operated in a low-temperature environment.

[0010] The technical tasks to be achieved in this document are not limited to the tasks mentioned above, and other tasks not mentioned will be clearly understood by those skilled in the art to which the present invention pertains from the description below.

[0011] A hydrogel coating composition for preventing condensation according to the invention comprises an ionic monomer, a crosslinking agent containing two or more acrylic groups, a polymerization initiator, and a solvent. The ionic monomer comprises at least one monomer selected from the group consisting of a zwitterionic monomer, a cationic monomer, and an anionic monomer.

[0012] The zwitterionic monomer according to the invention comprises an acrylic monomer comprising a zwitterionic functional group comprising at least one of phosphorylcholine, sulfobetaine, and carboxybetaine.

[0013] The zwitterionic monomer according to the invention comprises at least one of 2-methacryloyloxyethyl phosphorylcholine, 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propionate, and [2-(methacryloyloxy)ethyl]dimethyl-3-sulfopropyl)ammonium hydroxide.

[0014] The cationic monomer according to the invention includes an acrylic monomer having a trialkylammonium cationic group at a terminal.

[0015] The cationic monomer according to the invention comprises at least one of [2-(methacryloyloxy)ethyl]trimethylammonium chloride and trimethyl-3-[(1-oxoallyl)amino]propylammonium chloride.

[0016] The anionic monomer according to the invention includes an acrylic monomer having a sulfonate anion group at a terminal.

[0017] The anionic monomer according to the invention comprises at least one of 3-prop-2-enoyloxy propane-1-sulfonic acid, 3-(2-methylprop-2-enoyloxy)propane-1-sulfonic acid, and acrylic acid.

[0018] The ionic monomer according to the invention includes the cationic monomer and the anionic monomer.

[0019] The crosslinking agent comprising two or more acrylic groups according to the invention includes at least one of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, N,N'-methylenebisacrylamide, and trimethylolpropane triacrylate.

[0020] The concentration of the cross-linking agent according to the invention comprises 0.1 w / v% to 5.0 w / v%.

[0021] The polymerization initiator according to the invention comprises at least one of a thermal polymerization initiator and a photopolymerization initiator.

[0022] It further includes a reaction catalyst for activating the polymerization initiator according to the invention.

[0023] A method for producing a hydrogel coating film for preventing frost according to the invention comprises: applying a hydrogel coating composition for preventing frost, which comprises an ionic monomer, a crosslinking agent comprising two or more acrylic groups, a polymerization initiator, and a solvent, onto a substrate; and crosslinking and polymerizing the hydrogel coating composition for preventing frost, to form a hydrogel coating film for preventing frost, which comprises an ionic polymer, on the substrate. The ionic monomer comprises at least one monomer selected from the group consisting of a zwitterionic monomer, a cationic monomer, and an anionic monomer.

[0024] A method for manufacturing a hydrogel coating film for preventing staining according to the invention further includes, before applying the hydrogel coating composition for preventing staining on a substrate, surface-treating the substrate with a silane compound containing an acrylic group to form an intermediate adhesive layer.

[0025] The method for manufacturing a hydrogel coating film for preventing staining according to the invention comprises the ionic monomer comprising the cationic monomer and the anionic monomer in an equivalent ratio of 1:1.

[0026] A heat exchanger according to the invention comprises an anti-freezing coating composition capable of lowering the freezing temperature on the surface of at least one fin and tube, wherein the anti-freezing coating composition comprises an ionic monomer, a crosslinking agent containing two or more acrylic groups, a polymerization initiator, and a solvent, wherein the ionic monomer comprises at least one of a zwitterionic monomer, a cationic monomer, and an anionic monomer.

[0027] A heat exchanger according to the invention comprises a heat exchanger having fins, and includes a frost-preventing hydrogel coating film coated on the fins. The frost-preventing hydrogel coating film comprises an ionic polymer copolymer.

[0028] One aspect of the present disclosure provides a hydrogel coating composition for preventing sagging using a superhydrophilic ionic monomer that has not previously been used for sagging purposes.

[0029] One aspect of the present disclosure provides a method for coating a superhydrophilic hydrogel capable of further lowering the freezing temperature of a substrate surface by using a hydrogel coating composition comprising an ionic monomer having superhydrophilicity.

[0030] One aspect of the present disclosure is to provide a heat exchanger having a superhydrophilic ionic polymer hydrogel coating on the surface of a fin to further enhance ice nucleation and ice growth prevention performance and an ice adhesion reduction effect, in order to lower the freezing temperature of the surface of a device operated in a low-temperature environment.

[0031] FIG. 1 is a cross-sectional view of a substrate having a hydrogel coating film formed thereon for preventing corrosion according to one embodiment.

[0032] FIG. 2 is a cross-sectional view of a substrate having a hydrogel coating film and an intermediate adhesive layer formed thereon for preventing corrosion according to one embodiment.

[0033] Figure 3 is a schematic diagram of a hydrogel coating film including an ionic polymer according to one embodiment.

[0034] Figure 4 shows the water contact angle according to the substrate surface treatment in one embodiment.

[0035] Figure 5 shows the results of X-ray photoelectron spectroscopy (XPS) of the substrate before surface treatment in Experimental Example 1 and the surface of the substrate treated according to Manufacturing Examples 1 to 5.

[0036] Figure 6 shows the results of differential scanning calorimetry (DSC) measurements of a hydrogel coating film measured in two cycles in Experimental Example 2.

[0037] Figure 7 is the freezing temperature of the ionic polymer hydrogel analyzed through DSC of Figure 6.

[0038] Figure 8 shows the results of Fourier transform-infrared spectroscopy (FT-IR) analysis of free and bound water for ionic polymers of Experimental Example 3.

[0039] Figure 9 shows the results of a wind tunnel experiment conducted at -10°C on a general aluminum substrate and an aluminum substrate coated with hydrogel in Experimental Example 4.

[0040] Figure 10 shows the results of a wind tunnel experiment conducted at -30°C on a general aluminum substrate and an aluminum substrate coated with hydrogel in Experimental Example 4.

[0041] It should be understood that the various embodiments and terms used in this document are not intended to limit the technical features described in this document to specific embodiments, but rather to encompass various modifications, equivalents, or alternatives of the embodiments.

[0042] In connection with the description of the drawings, similar reference numerals may be used for similar or related components.

[0043] The singular form of a noun corresponding to an item may include one or more of said items, unless the relevant context clearly indicates otherwise.

[0044] In this document, each of the phrases "A or B", "at least one of A and B", "at least one of A or B", "A, B, or C", "at least one of A, B, and C", and "at least one of A, B, or C" may include any one of the items listed together in that phrase, or all possible combinations thereof.

[0045] The term "and / or" includes any combination of a plurality of related described elements or any one of a plurality of related described elements.

[0046] Terms such as "first," "second," or "first" or "second" may be used simply to distinguish one component from another, and do not qualify the components in any other respect (e.g., importance or order).

[0047] In addition, terms such as 'front', 'rear', 'top', 'bottom', 'side', 'left', 'right', 'upper', and 'lower' used in the present disclosure are defined based on the drawings, and the shape and position of each component are not limited by these terms.

[0048] The terms "include" or "have" are intended to specify the presence of a feature, number, step, operation, component, part or combination thereof described in this document, but do not preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts or combinations thereof.

[0049] When a component is said to be “connected,” “coupled,” “supported,” or “in contact with” another component, this includes not only cases where the components are directly connected, coupled, supported, or in contact, but also cases where the components are indirectly connected, coupled, supported, or in contact through a third component.

[0050] When we say that a component is "on" another component, this includes not only cases where the component is in contact with the other component, but also cases where there is another component between the two components.

[0051] "About," "substantially," etc. are used in the sense of or near to the numerical value when manufacturing and material tolerances inherent in the meanings mentioned are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures in which exact or absolute numerical values ​​are mentioned to aid understanding of the present invention.

[0052] Hereinafter, a hydrogel coating composition for preventing frost according to the present invention, a method for producing a hydrogel coating film for preventing frost, and a heat exchanger using the same are specifically described.

[0053] The present invention provides a hydrogel coating composition for preventing sagging, comprising an ionic monomer, a crosslinking agent, a polymerization initiator, and a solvent.

[0054] The hydrogel coating composition for preventing sagging according to the present invention can impart superhydrophilicity to the hydrogel coating by including an ionic monomer. Here, the ionic monomer refers to a polymer having an ionic functional group in the main chain or side chain of a molecule, and may include at least one monomer selected from the group consisting of a zwitterionic (+ / -) monomer, a cationic (+) monomer, and an anionic (-) monomer. For example, it may be preferable to include at least one zwitterionic (+ / -) monomer, or at least one cationic (+) monomer and one anionic (-) monomer, but the present invention is not limited thereto.

[0055] In one embodiment, the hydrogel coating composition may include an ionic monomer at a molar concentration of about 0.5 to 3 mol / L. If the molar concentration of the ionic monomer is too low, hydrogel formation may not occur due to insufficient monomer content, and if the molar concentration of the ionic monomer is too high, the hydrogel may have brittle mechanical properties, making it unsuitable for applications. Therefore, it is preferable to satisfy the above molar concentration.

[0056] In one embodiment, when the hydrogel coating composition comprises a zwitterionic monomer as the ionic monomer, a hydrogel coating can be formed comprising a zwitterionic polymer and / or a copolymer thereof polymerized with the zwitterionic monomer.

[0057] Zwitterionic monomers are neutral chemical compounds having both positive and negative charges, and comprising at least one zwitterionic group and at least one reactive group in the backbone or side chain of the molecule. Examples of the zwitterionic group include phosphoryl choline, sulfobetaine, and carboxybetaine.

[0058] For example, zwitterionic monomers may include 2-methacryloyloxyethyl phosphorylcholine (MPC) represented by the following chemical formula 1-1, 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propionate (CBMA) represented by the following chemical formula 1-2, and [2-(methacryloyloxy)ethyl]dimethyl-3-sulfopropyl)ammonium hydroxide (SBMA) represented by the following chemical formula 1-3.

[0059] [Chemical Formula 1-1]

[0060]

[0061] [Chemical Formula 1-2]

[0062]

[0063] [Chemical Formula 1-3]

[0064]

[0065] In one embodiment, when the hydrogel coating composition comprises a cationic monomer as the ionic monomer, a hydrogel coating can be formed comprising a cationic polymer and / or a copolymer thereof polymerized with the cationic monomer.

[0066] A cationic monomer is a monomer that has or can have a positive charge, and includes at least one cationic group in the main chain or side chain of the molecule. Specifically, the cationic monomer may be an acrylic monomer that includes a trialkylammonium cationic group at the terminal, and may also exist in solution together with an anionic salt such as a halide (chloride) salt.

[0067] For example, cationic monomers may include [2-(Methacryloyloxy)ethyl]trimethylammonium chloride (METAC) represented by the following chemical formula 2-1 and trimethyl-3-[(1-oxoallyl)amino]propylammonium chloride represented by the following chemical formula 2-2.

[0068] [Chemical Formula 2-1]

[0069]

[0070] [Chemical Formula 2-2]

[0071]

[0072] In one embodiment, when the hydrogel coating composition comprises an anionic monomer as the ionic monomer, a hydrogel coating can be formed comprising an anionic polymer and / or a copolymer thereof polymerized with the anionic monomer.

[0073] An anionic monomer refers to a monomer that has or can have a negative charge, and includes at least one anionic group in the main chain or side chain of the molecule. Specifically, the anionic monomer may be an acrylic monomer that includes a sulfonate anionic group at the terminal, and may also exist in solution together with a cationic salt, such as a potassium salt.

[0074] For example, the anionic monomer may include 3-prop-2-enoyloxypropane-1-sulfonic acid (3-Sulfopropyl acrylate; SPA) represented by the following chemical formula 3-1, 3-(2-methylprop-2-enoyloxy)propane-1-sulfonic acid (3-Sulfopropyl methacrylate; SPMA) represented by the following chemical formula 3-2, and acrylic acid (AAc).

[0075] [Chemical Formula 3-1]

[0076]

[0077] [Chemical Formula 3-2]

[0078]

[0079] In one embodiment, the hydrogel coating composition may simultaneously include cationic and anionic monomers as ionic monomers. In this case, a hydrogel coating may be formed that includes a similar zwitterionic polymer and / or a copolymer thereof in which the cationic and anionic monomers are polymerized. In this case, to balance the negative and positive charges, the cationic and anionic monomers are preferably included in an equivalent ratio of about 1:1.

[0080] The hydrogel coating composition according to the present invention comprises a crosslinking agent containing an acrylic group to induce gelation through crosslinking polymerization with an ionic monomer. Any acrylic crosslinking agent containing two or more acrylic groups may be used without particular limitation.

[0081] In one embodiment, the cross-linking agent may be included in a molar ratio of about 0.5 to 5 mol% based on the ionic monomer. In addition, the concentration of the cross-linking agent in the hydrogel coating composition is preferably 0.1 w / v% to 5.0 w / v%. If the molar ratio or concentration range of the cross-linking agent is exceeded, the hydrogel coating composition may become brittle and may form defects and be destroyed upon impact. On the other hand, if the molar ratio or concentration range of the cross-linking agent is below the range, cross-linking between polymers is not sufficiently formed, and the hydrogel is not formed in a solid hydrogel form but in a viscous liquid form. Therefore, by including the cross-linking agent within the molar ratio or concentration range described above, a hydrogel having excellent elongation and strength can be stably formed on a substrate.

[0082] For example, crosslinking agents containing two or more acrylic groups may include, but are not limited to, polyethylene glycol diacrylate (PEGDA) represented by the following chemical formula 4-1, polyethylene glycol dimethacrylate represented by the following chemical formula 4-2, N,N'-methylenebisacrylamide represented by the following chemical formula 4-3, and trimethylolpropane triacrylate represented by the following chemical formula 4-4.

[0083] [Chemical Formula 4-1]

[0084]

[0085] In the above chemical formula 4-1, n is an arbitrary integer.

[0086] [Chemical Formula 4-2]

[0087]

[0088] In the above chemical formula 4-2, n is an arbitrary integer.

[0089] [Chemical Formula 4-3]

[0090]

[0091] [Chemical Formula 4-4]

[0092]

[0093] The hydrogel coating composition according to the present invention comprises a polymerization initiator that forms radicals in the ionic monomer to polymerize the ionic monomer. The polymerization initiator does not polymerize into the polymer chain, but may or may not be present within the prepared polymer hydrogel.

[0094] The above polymerization initiator is a substance that forms radicals by external stimuli such as heat and / or light, and may include at least one selected from the group consisting of a thermal polymerization initiator and a photopolymerization initiator depending on the polymerization method.

[0095] As the above thermal polymerization initiator, one or more selected from the group of initiators consisting of persulfate-based initiators and azo-based initiators can be used. Specifically, examples of persulfate-based initiators include ammonium persulfate (APS), sodium persulfate (Na2S2O8), and potassium persulfate (K2S2O8), all of which are represented by the following chemical formula 5-1. Examples of azo-based initiators include 4,4-azobis-(4-cyanovaleric acid), 2,2-azobis-(2-amidinopropane) dihydrochloride, and 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, all of which are represented by the following chemical formula 5-2. dihydrochloride), 2-carbamoyl azoisobutylonitrile, and 2,2-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, but are not limited thereto.

[0096] [Chemical Formula 5-1]

[0097]

[0098] [Chemical Formula 5-2]

[0099]

[0100] The photopolymerization initiator may be used without any particular limitation as long as it is a compound that can form radicals by light such as ultraviolet (UV) light. Examples of the photopolymerization initiator include, but are not limited to, 2-Hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (IRGACURE 2959), 2-Hydroxy-2-methyl-1-phenyl-propan-1-one (DAROCUR 1173), IRGACURE 500, IRGACURE 754, IRGACURE OXE02, etc., represented by the following chemical formula 6.

[0101] [Chemical Formula 6]

[0102]

[0103] The polymerization initiator may be included in a molar ratio of 0.5 to 2.5 mol% based on the ionic monomer. If the molar ratio of the polymerization initiator is too low, the rate of radical generation may be slower than the rate of radical extinction, preventing polymerization from being initiated by radicals. However, if the molar ratio of the polymerization initiator is too high, there is a risk of deterioration of the mechanical properties of the hydrogel.

[0104] In addition, the hydrogel coating composition according to the present invention may further include a reaction catalyst for activating the polymerization initiator.

[0105] For example, when ammonium persulfate (APS) is used as a polymerization initiator, tetramethylethylenediamine (TEMED), represented by the following chemical formula 7, may be further included as a reaction catalyst to promote the reaction.

[0106] [Chemical Formula 7]

[0107]

[0108] In addition, the hydrogel coating composition according to the present invention includes a solvent. The solvent may be used without limitation in its composition as long as it can dissolve the above-described components. The solvent may be, for example, one or more selected from water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, and carbitol, and may be used in combination, with water being most preferred.

[0109] The above solvent may be included as a residual amount excluding the above-described components with respect to the total content of the above composition.

[0110] Hereinafter, a method for manufacturing a hydrogel coating film for preventing frostbite is described with reference to FIGS. 1 and 2. FIGS. 1 and 2 are cross-sectional views of a substrate on which a hydrogel coating film for preventing frostbite is formed.

[0111] Referring to FIG. 1, the anti-staining hydrogel coating film according to the present invention is manufactured by applying the anti-staining hydrogel coating composition on a substrate (100) and then crosslinking and polymerizing to form a hydrogel coating film (110).

[0112] The substrate (100) is a general inorganic material, preferably a metal material. Examples of the substrate (100) include, but are not limited to, aluminum, aluminum alloys, alumino-silicates such as silica, quartz, glass, clays, inorganic oxides such as silicon, copper, tin (SnO), talc, Fe2O3, TiO2, Cr2O3, steel, iron, etc.

[0113] Referring to FIG. 2, the method for manufacturing a hydrogel coating film for preventing frost according to the present invention may further include, before applying the hydrogel coating composition for preventing frost on a substrate (100), surface-treating the substrate (100) with a silane compound containing an acrylic group to form an intermediate adhesive layer (101).

[0114] In addition, before forming the intermediate adhesive layer (101), the surface of the substrate (100) may be treated with UV to clean it, and ozone treatment may be further included to form a hydroxyl group on the surface of the substrate (100) to facilitate bonding with silane.

[0115] The intermediate adhesive layer (101) can be formed to prevent the substrate (100) and the hydrogel (110) from being separated from each other due to swelling of the hydrogel.

[0116] In one embodiment, an intermediate adhesive layer (101) may be formed by surface-treating a substrate (100) using a silane-based compound containing an acrylic group as a silane coupling agent, thereby forming an acrylic group on the surface of the substrate (100). The acrylic group on the surface of the substrate (100) enables hydrogel grafting, which forms a strong chemical bond between the hydrogel coating film (110) and the surface of the substrate (100). Therefore, the hydrogel coating film (110) may be stably maintained on the surface of the substrate (100) through the acrylic group formed on the surface of the substrate.

[0117] In addition, silane increases the adhesion and affinity between polymers and inorganic, organic, metallic, and glass materials in composite systems, and can form an adhesive on the surface of a substrate with a simple heat treatment, making it versatile in various processes. In addition, wettability is required for a thin hydrogel to be formed on the surface of a substrate, and silane can be used to increase the wettability of the substrate, thereby facilitating the formation of a hydrogel coating film (110) on the surface of the substrate.

[0118] For example, silane compounds containing the acrylic group may include methacryloxypropyltrimethoxysilane (TMSPMA), (3-acryloxypropyl)trimethoxysilane, and methacryloxypropylmethyldimethoxysilane.

[0119] For example, the intermediate adhesive layer (101) can be formed by preparing a silane solution containing a silane compound containing an acrylic group and a solvent, immersing the substrate (100) in the silane solution, and then reacting at room temperature or by heat treatment. For example, the heat treatment can be performed at 60 to 100°C for 30 minutes to 3 hours, but is not limited thereto.

[0120] In one embodiment, a hydrogel coating composition for preventing adhesion is applied to a substrate (100) on which an intermediate adhesive layer (101) is formed or not formed.

[0121] The hydrogel coating composition for preventing staining comprises an ionic monomer, a crosslinking agent containing two or more acrylic groups, a polymerization initiator, and a solvent, and a detailed description thereof is omitted as it is the same as described above.

[0122] The application of the above hydrogel coating composition can be performed by methods such as dip coating, casting, and spray coating. At this time, the thickness of the hydrogel coating film can be appropriately adjusted as needed.

[0123] Next, the hydrogel coating composition for preventing the formation of the above-mentioned substance is crosslinked and polymerized to form a hydrogel coating film (110) containing an ionic polymer on a substrate (100) on which an intermediate adhesive layer (101) is formed or not formed.

[0124] In one embodiment, in order to crosslink and polymerize the hydrogel coating composition, curing may be induced by performing heat treatment and / or light irradiation to form a hydrogel coating film (110).

[0125] For example, when the hydrogel coating composition includes a thermal polymerization initiator as a polymerization initiator, the hydrogel coating composition can be cured through heat treatment to form a hydrogel coating film (110). At this time, the heat treatment can be performed in an oven at 60 to 100°C.

[0126] For example, when the hydrogel coating composition includes a photopolymerization initiator as a polymerization initiator, curing of the hydrogel coating composition can be induced through light irradiation to form a hydrogel coating film (110). At this time, the light irradiation may be irradiation with a light source in the UV range.

[0127] For example, when the hydrogel coating composition includes both a thermal polymerization initiator and a photopolymerization initiator as polymerization initiators, both heat treatment and light irradiation can be performed to induce curing of the hydrogel coating composition.

[0128] Fig. 3 is a schematic diagram of a hydrogel coating film (110) containing an ionic polymer. Referring to Fig. 3, the hydrogel coating film (110) contains free water and bound water surrounding the ionic polymer, and ionic monomers are linked to each other by a crosslinker to polymerize into an ionic polymer. The polymerization initiator does not polymerize to the ionic polymer chain, but may or may not be present within the hydrogel coating film (110).

[0129] In one embodiment, the ionic polymer may include at least one polymer selected from the group consisting of a zwitterionic polymer, a cationic polymer, an anionic polymer, and a pseudo-zwitterionic polymer. Here, a pseudo-zwitterionic polymer may mean that the hydrogel coating film (110) includes both a cationic polymer and an anionic polymer.

[0130] For example, the ionic polymer may include, but is not limited to, a zwitterionic polymer represented by the following chemical formula 8-1, a cationic polymer represented by the following chemical formula 8-2, and an anionic polymer represented by the following chemical formula 8-3.

[0131] [Chemical Formula 8-1]

[0132]

[0133] [Chemical Formula 8-2]

[0134]

[0135] [Chemical Formula 8-3]

[0136]

[0137] In the above chemical formulas 8-1 to 8-3, n is each independently an arbitrary integer, + means electrically cationic, and - means electrically anionic.

[0138] In addition, the cured hydrogel coating film (110) can achieve an appropriate moisture content (about 30 to 50 wt%) for maintaining physical properties and structure through an appropriate level of drying under constant temperature and humidity conditions.

[0139] In one embodiment, the hydrogel coating film (110) may be formed to a thickness of 10 nm to 1 mm, preferably 100 nm to 500 μm. When the above thickness range is satisfied, both optimal anti-icing performance and hydrogel coating stability may be excellent.

[0140] The hydrogel coating film for frost prevention according to the present invention can delay the formation and growth of frost on a substrate by lowering the freezing temperature. For example, the freezing temperature of the hydrogel coating film may be about -18.5°C or lower, preferably about -25°C or lower, and more preferably about -27°C or lower. The lower the freezing temperature of the hydrogel coating film, the better the anti-icing performance it can have.

[0141] The hydrogel coating film according to one embodiment can be used on the surface of a product requiring anti-icing performance without any particular limitations. The hydrogel coating film manufactured according to the present invention can be applied to, for example, heat exchanger fins; transport channels such as pipes and power lines; and the external surfaces of aircraft, satellites, spacecraft, and the like, but is not limited thereto.

[0142] Hereinafter, a heat exchanger having a fin material will be described as an example to which a hydrogel coating film for preventing corrosion according to the present invention is applied.

[0143] The heat exchanger includes an evaporator having a tube having channels formed inside to allow refrigerant to flow and a fin joined to the outer surface of the tube.

[0144] Additionally, the tubes may be arranged to be connected in a zigzag pattern in multiple rows to expand the heat exchange area between the refrigerant flowing inside the tubes and the outside air.

[0145] The above fins may be provided in multiple numbers, and the fin material may be an aluminum alloy. In addition, to improve the anti-icing performance of the heat exchanger, an anti-icing hydrogel according to the present invention may be coated on the fin material.

[0146] A detailed description of the above-mentioned hydrogel for preventing staining is omitted as it is the same as that described for the above-mentioned hydrogel coating composition for preventing staining and the method for producing a hydrogel coating film using the same.

[0147]

[0148] In one embodiment, the fins may be provided between a plurality of tubes so that the refrigerant flowing along the channels formed inside the tubes and the outside air can efficiently exchange heat. That is, the fins may be arranged so as to be in contact with the tubes in the heat exchange space.

[0149] In one embodiment, the pin may be provided along the outer circumferential surface of the first tube in the longitudinal direction of the tube. At this time, the shape of the pin is not particularly limited.

[0150] In one embodiment, the pin may be press-fitted to the tube. That is, the tube and the pin may be joined by pushing the pin into a hole smaller than the outer diameter of the tube.

[0151] A hydrogel coating composition for preventing sagging according to one embodiment comprises an ionic monomer, a crosslinking agent comprising two or more acrylic groups, a polymerization initiator, and a solvent. The ionic monomer comprises at least one monomer selected from the group consisting of a zwitterionic monomer, a cationic monomer, and an anionic monomer.

[0152] The above zwitterionic monomer may be an acrylic monomer including a zwitterionic functional group selected from the group consisting of phosphorylcholine, sulfobetaine, and carboxybetaine.

[0153] The above zwitterionic monomer may be selected from the group consisting of 2-methacryloyloxyethyl phosphorylcholine, 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propionate, and [2-(methacryloyloxy)ethyl]dimethyl-3-sulfopropyl)ammonium hydroxide.

[0154] The above cationic monomer may be an acrylic monomer containing a trialkylammonium cationic group at the terminal.

[0155] The cationic monomer may be selected from the group consisting of [2-(methacryloyloxy)ethyl]trimethylammonium chloride and trimethyl-3-[(1-oxoallyl)amino]propylammonium chloride.

[0156] The above anionic monomer may be an acrylic monomer containing a sulfonate anionic group at the terminal.

[0157] The above anionic monomer may be selected from the group consisting of 3-prop-2-enoyloxy propane-1-sulfonic acid, 3-(2-methylprop-2-enoyloxy)propane-1-sulfonic acid, and acrylic acid.

[0158] The above ionic monomer may include the above cationic monomer and the above anionic monomer.

[0159] The crosslinking agent including two or more acrylic groups may include at least one selected from the group consisting of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, N,N'-methylenebisacrylamide, and trimethylolpropane triacrylate.

[0160] The concentration of the crosslinking agent may be 0.1 w / v% to 5.0 w / v%.

[0161] The above polymerization initiator may include at least one selected from the group consisting of a thermal polymerization initiator and a photopolymerization initiator.

[0162] It may further include a reaction catalyst for activating the above polymerization initiator.

[0163] A method for manufacturing a hydrogel coating film for preventing frost according to one embodiment comprises: applying a hydrogel coating composition for preventing frost, which comprises an ionic monomer, a crosslinking agent comprising two or more acrylic groups, a polymerization initiator, and a solvent, onto a substrate; and crosslinking and polymerizing the hydrogel coating composition for preventing frost, to form a hydrogel coating film for preventing frost, which comprises an ionic polymer, on the substrate. The ionic monomer comprises at least one monomer selected from the group consisting of a zwitterionic monomer, a cationic monomer, and an anionic monomer.

[0164] Before applying the above-described hydrogel coating composition for preventing adhesion to a substrate, the method may further include surface-treating the substrate with a silane compound containing an acrylic group to form an intermediate adhesive layer.

[0165] The silane compound including the above acrylic group may include at least one compound selected from the group consisting of methacryloxypropyltrimethoxysilane, (3-acrylooxypropyl)trimethoxysilane, and methacryloxypropylmethyldimethoxysilane.

[0166] The above ionic polymer may include at least one polymer selected from the group consisting of a zwitterionic polymer, a cationic polymer, an anionic polymer, and a pseudo-zwitterionic polymer.

[0167] The above ionic monomer may include the cationic monomer and the anionic monomer in an equivalent ratio of 1:1.

[0168] The zwitterionic monomer may be selected from the group consisting of 2-methacryloyloxyethyl phosphorylcholine, 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propionate, and [2-(methacryloyloxy)ethyl]dimethyl-3-sulfopropyl)ammonium hydroxide. The cationic monomer may be selected from the group consisting of [2-(methacryloyloxy)ethyl]trimethylammonium chloride and trimethyl-3-[(1-oxoallyl)amino]propylammonium chloride. The anionic monomer may be selected from the group consisting of 3-prop-2-enoyloxypropane-1-sulfonic acid, 3-(2-methylprop-2-enoyloxy)propane-1-sulfonic acid, and acrylic acid.

[0169] According to one embodiment, a heat exchanger comprises a heat exchanger having fins, and includes a frost-preventing hydrogel coating film coated on the fins. The frost-preventing hydrogel coating film comprises an ionic polymer copolymer.

[0170] The above ionic polymer copolymer may include at least one selected from the group consisting of a zwitterionic functional group, a cationic functional group, and an anionic functional group.

[0171] According to the invention, a hydrogel can be formed using an ionic-based superhydrophilic material that has not previously been used for the purpose of preventing freezing, thereby providing an anti-freezing effect.

[0172] According to the invention, by coating a hydrogel containing an ionic polymer on the surface of a device operated in a low-temperature environment, it is possible to provide effects of suppressing ice nucleus formation, preventing ice growth, and reducing ice adhesion.

[0173] The effects that can be obtained from the present disclosure are not limited to the effects mentioned above, and other effects that are not mentioned can be clearly understood by a person having ordinary skill in the art to which the present disclosure belongs from the description below.

[0174] Hereinafter, the present invention will be described in more detail through examples. However, the following examples are intended to further illustrate the present invention, and the scope of the present invention is not limited by the following examples.

[0175] [Example]

[0176] (1) Substrate surface treatment (formation of intermediate adhesive layer)

[0177] (1-1) Preparation of aluminum substrate

[0178] After washing the aluminum substrate in the order of acetone, ethanol, and distilled water (DI water), the remaining solution on the surface of the substrate was removed and dried at 70°C to prepare an aluminum substrate (bare Al) before surface treatment.

[0179] (1-2) Preparation of silane solution

[0180] A silane solution was prepared by adding TMSPMA (3-[trimethoxysilyl]propyl methacrylate) to an acetic acid (0.01 vol%) aqueous solution at a concentration of approximately 1 mM to make 2 wt% (TMSPMA / acetic acid aqueous solution).

[0181] (1-3) Aluminum substrate surface treatment

[0182] Manufacturing Example 1: The cleaned aluminum substrate was further cleaned and ozone-treated using a UV / ozone cleaner to prepare an aluminum substrate (Al+UV / O3).

[0183] Manufacturing Example 2: The washed aluminum substrate (bare Al) was placed in the previously prepared silane solution and reacted at room temperature (RT) for 2 hours. Thereafter, the substrate was washed with ethanol to prepare an aluminum substrate (Al+TMSPMA) surface-treated with silane.

[0184] Manufacturing Example 3: The washed aluminum substrate (bare Al) was placed in the previously prepared silane solution and reacted at 70°C for 2 hours. Thereafter, the substrate was washed with ethanol to prepare an aluminum substrate surface-treated with silane (Al+TMSPMA @70°C).

[0185] Manufacturing Example 4: The ozone-treated aluminum substrate of Manufacturing Example 1 was placed in the previously prepared silane solution and reacted at room temperature (RT) for 2 hours. Thereafter, the substrate was washed with ethanol to prepare an ozone- and silane-surface-treated aluminum substrate (Al+UV / O3+TMSPMA).

[0186] Manufacturing Example 5: The ozone-treated aluminum substrate of Manufacturing Example 1 was placed in the previously prepared silane solution and reacted at 70°C for 2 hours. Thereafter, the substrate was washed with ethanol to prepare an ozone- and silane-surface-treated aluminum substrate (Al+UV / O3+TMSPMA @70°C).

[0187] (1-4) Experimental Example 1: Measurement of water contact angle on substrate and elemental analysis

[0188] In order to select an appropriate surface treatment process, the water contact angle was measured for the aluminum substrate before surface treatment (bare Al) and the substrate immediately after the surface treatment (Manufacturing Examples 1 to 5), as shown in Fig. 4, and the surface elements were analyzed through X-ray photoelectron spectroscopy (XPS), as shown in Fig. 5. Through this, it was possible to verify whether a silane reaction occurred on the substrate surface.

[0189] Referring to Fig. 4, the substrate (bare Al) before surface treatment showed a contact angle of about 100°, but after ozone treatment, the substrate (Manufacturing Example 1) had a contact angle that decreased to close to about 0° due to the formation of hydroxyl groups on the surface. After reacting with a silane solution (Manufacturing Examples 2 to 4), the contact angle increased significantly, showing a contact angle of at least 60°. This is because silicon elements, which exhibit relatively hydrophobicity, are distributed on the surface through the surface treatment process, and this confirms that the surface treatment was performed normally. In addition, when heat treatment is performed during silane treatment, the water contact angle tends to decrease, which confirms that wettability is imparted by the heat-treated silane.

[0190] In addition, referring to FIG. 5, it can be confirmed that the silane surface treatment was performed normally through the increase in the intensity of the shoulder peak and silicon peak derived from C=O in the carbon peak of the surface-treated substrate compared to the substrate without surface treatment.

[0191] (2) Preparation of hydrogel coating film

[0192] (2-1) Examples 1-1 to 1-5 and Comparative Example 1-1: Preparation of hydrogel coating composition

[0193] Ionic monomers or nonionic monomers (2 to 3 mol / L in molar concentration, PEGDA (Polyethylene glycol diacrylate, stabilized with MEHQ, Tokyo Chemical Industry; 1 mol% relative to monomer) and APS (ammonium persulfate, ≥98%, Sigma Aldrich, 1 mol% relative to monomer) as shown in Table 1 below were sequentially added to a vial at a molar ratio of 1:0.01:0.01, and stirred with water as a solvent to obtain a hydrogel coating composition.

[0194] Monomer type Ionic type Example 1-1 2-methacryloyloxyethyl phosphorylcholine (MPC) Zwitterionic Example 1-2 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propionate (CBMA) Zwitterionic Example 1-3 [2-(methacryloyloxy)ethyl]trimethylammonium chloride (METAC) Cationic Example 1-4 3-prop-2-enoyloxypropane-1-sulfonic acid (SPA) Anionic Example 1-5 METAC + SPA Cationic + Anionic Comparative Example 1-1 Oligo(ethylene glycol) methacrylate (OEGMA) Nonionic (neutral)

[0195] (2-2) Examples 2-1 to 2-5 and Comparative Example 2-1: Preparation of hydrogel coating film

[0196] The hydrogel coating compositions according to Examples 1-1 to 1-5 and Comparative Example 1-1 were each cast on the substrate according to Preparation 5, and then cured in an oven at 70°C for 30 minutes to produce hydrogel coating films according to Examples 2-1 to 2-5 and Comparative Example 2-1. Thereafter, the hydrogel coating films, after completion of curing, were dried under constant temperature and humidity conditions (4°C desiccator) for 10 to 14 hours to contain an appropriate amount of moisture (about 30 to 50 wt%).

[0197] (2-3) Experimental Example 2: Freezing Temperature Test using Differential Scanning Calorimetry (DSC)

[0198] In order to confirm the anti-icing performance of the hydrogel coating film in a low-temperature environment, the freezing temperature of the hydrogel coating film of Examples 2-1 to 2-5 and Comparative Example 2-1 was measured for 2 cycles using DSC, and the results are as shown in Figs. 6 and 7 and Table 2 below. Through this experiment, it was possible to confirm the point in time when ice nuclei formation inside the hydrogel begins.

[0199] Monomer type Polymer ionic type Freezing temperature (℃) Control (water) --- 18.07 Example 2-1 Example 1-1 MPC: Zwitterionic - 34.68 Example 2-2 Example 1-2 CBMA: Zwitterionic - 27.3 Example 2-3 Example 1-3 METAC: Cationic - 34.7 Example 2-4 Example 1-4 SPA: Anionic - 31.3 Example 2-5 Example 1-5 METAC+SPA: Pseudo zwitterionic - 28.4 Comparative Example 2-1 Comparative Example 1-1 OEGMA: Nonionic - 25.11

[0200] Referring to FIGS. 6 and 7 and Table 2 above, Example 2-1 (MPC) and Example 2-2 (CBMA), which were manufactured based on zwitterionic monomers, showed freezing temperatures of about -34.68°C and -27.3°C, respectively. Example 2-3 (METAC), which was manufactured based on cationic monomers, showed a freezing temperature of -34.7°C, and Example 2-4 (SPA), which was manufactured based on anionic monomers, showed a freezing temperature of -31.3°C. In addition, Example 2-5 (METAC+SPA), which includes a similar zwitterionic polymer manufactured using both cationic monomers METAC and anionic monomers SPA, showed a freezing temperature of about -28.4°C. That is, it was confirmed that when a hydrogel coating film including ionic polymers was formed, the freezing temperature was significantly lowered, resulting in excellent anti-icing performance. Meanwhile, Comparative Example 2-1 (OEGMA), manufactured based on a nonionic monomer, was confirmed to have a freezing temperature of -25.11℃, which is lower than that of water (DI water). This is believed to be due to the hydrophilicity of the hydrogel, which lowers the freezing temperature. However, it was confirmed that the freezing temperature was lowered further when an ionic monomer was used compared to when a nonionic monomer was used.

[0201] (2-4) Experimental Example 3: Analysis of the physical state of water inside the hydrogel

[0202] Analyzing the DSC results of Fig. 6, it can be confirmed that the hydrogel coating films according to Examples 2-1 to 2-5 have a higher fraction of bound water that freezes at temperatures of -20 to -30°C or lower than the fraction of free water that freezes at 0°C. This is believed to be due to the enhanced interaction with water molecules due to the zwitterionic cation and anion structures, thereby inhibiting hydrogen bonding between water molecules and the formation of hexagonal structures for ice nuclei formation.

[0203] In addition, in order to quantitatively confirm the basis of the excellent anti-icing performance of the hydrogel coating film according to the present invention, Fourier transform-infrared spectroscopy (FT-IR) analysis was performed, and the results are shown in Fig. 8. Through this analysis, water existing inside the zwitterionic hydrogel was separated according to its physical state and each fraction was calculated.

[0204] Referring to FIG. 8, the hydrogel coating film manufactured by the method according to the present invention has a 3,400 cm OH stretching of free water. -1 3,200 cm of bound water due to interaction with ions compared to the peak -1 It can be confirmed that the fraction of peak is dominant. That is, the content of bound water, which is completely bound by the electrostatic force originating from the ions of the ionic polymer functional group, increases, so that the hydrogel coating film containing the ionic polymer has a low freezing temperature (T c ) appears to have.

[0205] (2-5) Experimental Example 4: Surface formation and growth test through wind tunnel experiment

[0206] The substrate on which the hydrogel coating film of Examples 2-1 to 2-5 and Comparative Example 2-1 according to the present invention was formed was subjected to a constant humidity (RH 80%) and temperature (T s = -10℃ or T s = -30℃) was installed in a wind tunnel experimental device built in a chamber, and the time required for frost to form on the surface of the coating film and the frost thickness over time were measured, and the results are shown in Figs. 9 and 10.

[0207] Specifically, the experimental equipment was a modified version of a device used to measure actual heat exchangers, and consisted of a Peltier element, a water-cooled cooler, a CMOS camera, and an electron microscope. Surface temperature was controlled using the Peltier element and the water-cooled chamber cooler. Furthermore, the side of the substrate was observed using a CMOS camera, and the front was observed using an electron microscope.

[0208] The experimental environment was maintained at a constant external temperature and humidity chamber (wet and dry bulb temperature), and the surface temperature and wind volume were controlled using a wind tunnel experimental device. During the experiment, the external conditions were maintained at 5℃ and 3.6℃, ​​respectively, and the surface temperature (T s ) was set to -10℃ or -30℃, and the airflow was 1.3 CMM. In addition, the experiment was conducted for 3 hours, and the time required for the formation and growth of surface frost was measured by observing the sample surface with a camera to determine whether surface frost was formed and grown and the thickness of the frost.

[0209] First, at a humidity RH of 80% and a surface temperature of -10℃, a seeding experiment was conducted on a general aluminum substrate before hydrogel coating as a control (Bare) and a substrate coated with hydrogel according to Example 2-1 (MPC), Example 2-3 (METAC), Example 2-4 (SPA), and Comparative Example 2-1 (OEGMA), and the results are as shown in Fig. 9.

[0210] Referring to Figure 9, in Examples 2-1 (MPC), 2-3 (METAC), and 1-4 (SPA) containing ionic polymers, the formation of cysts was delayed compared to the control group, and the cyst thickness was also formed thinner compared to the control group. On the other hand, in Comparative Example 2-1 (OEGMA) containing non-ionic polymers, the growth rate of cysts was slower compared to the control group, but cyst formation began at an earlier time point than the control group, confirming that there was no effect of delaying implantation.

[0211] In addition, at a humidity RH of 80% and a surface temperature of -30°C, a test for implantation of a general aluminum substrate before hydrogel coating as a control (Bare) and a substrate coated with hydrogel according to Example 2-1 (MPC), Example 2-2 (CBMA), and Example 2-5 (METAC+SPA) was conducted, and the results are as shown in Fig. 10.

[0212] Referring to FIG. 10, it was confirmed that the growth rate of Example 2-1 (MPC), Example 2-2 (CBMA), and Example 2-5 (METAC+SPA) containing ionic polymers according to the present invention was slower than that of the control group.

[0213] Through these results, it appears that the hydrogel coating film manufactured by the method according to the present invention will exhibit excellent sex-inhibiting performance.

[0214] The above illustrates and describes specific embodiments. However, the invention is not limited to the above-described embodiments, and those skilled in the art will readily appreciate that various modifications and implementations can be made without departing from the spirit and scope of the invention as set forth in the claims below.

[0215] Description of the symbol

[0216] 100: Description

[0217] 101: Intermediate adhesive layer

[0218] 110: Hydrogel coating film

Claims

1. Ionic monomer; A crosslinking agent containing two or more acrylic groups; polymerization initiator; and Contains a solvent, A hydrogel coating composition for preventing ionic bonding, wherein the ionic monomer comprises at least one monomer selected from the group consisting of a zwitterionic monomer, a cationic monomer, and an anionic monomer.

2. In paragraph 1, A hydrogel coating composition for preventing staining, wherein the zwitterionic monomer is an acrylic monomer containing a zwitterionic functional group selected from the group consisting of phosphorylcholine, sulfobetaine, and carboxybetaine.

3. In paragraph 1, A hydrogel coating composition for preventing staining, wherein the zwitterionic monomer comprises at least one selected from the group consisting of 2-methacryloyloxyethyl phosphorylcholine, 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propionate, and [2-(methacryloyloxy)ethyl]dimethyl-3-sulfopropyl)ammonium hydroxide.

4. In paragraph 1, A hydrogel coating composition for preventing staining, wherein the cationic monomer is an acrylic monomer containing a trialkylammonium cationic group at a terminal.

5. In paragraph 1, A hydrogel coating composition for preventing staining, wherein the cationic monomer comprises at least one selected from the group consisting of [2-(methacryloyloxy)ethyl]trimethylammonium chloride and trimethyl-3-[(1-oxoallyl)amino]propylammonium chloride.

6. In paragraph 1, A hydrogel coating composition for preventing staining, wherein the anionic monomer is an acrylic monomer containing a sulfonate anion group at a terminal.

7. In paragraph 1, A hydrogel coating composition for preventing staining, wherein the anionic monomer comprises at least one selected from the group consisting of 3-prop-2-enoyloxy propane-1-sulfonic acid, 3-(2-methylprop-2-enoyloxy)propane-1-sulfonic acid, and acrylic acid.

8. In paragraph 1, The above ionic monomer is a hydrogel composition for a sex-resistant coating, comprising the cationic monomer and the anionic monomer.

9. In paragraph 1, A hydrogel coating composition for preventing staining, wherein the crosslinking agent containing two or more acrylic groups includes at least one selected from the group consisting of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, N,N'-methylenebisacrylamide, and trimethylolpropane triacrylate.

10. In paragraph 1, A hydrogel coating composition for preventing staining, wherein the concentration of the cross-linking agent is 0.1 w / v% to 5.0 w / v%.

11. In paragraph 1, A hydrogel coating composition for preventing sagging, wherein the polymerization initiator comprises at least one selected from the group consisting of a thermal polymerization initiator and a photopolymerization initiator.

12. In paragraph 1, A hydrogel coating composition for preventing condensation, further comprising a reaction catalyst for activating the polymerization initiator.

13. Applying a hydrogel coating composition for preventing ionic bonding, comprising an ionic monomer, a crosslinking agent containing two or more acrylic groups, a polymerization initiator, and a solvent, onto a substrate; and It comprises forming a hydrogel coating film including an ionic polymer on the substrate by crosslinking and polymerizing the hydrogel coating composition for preventing the above-mentioned properties; A method for producing a hydrogel coating film for preventing ionic contamination, wherein the ionic monomer comprises at least one monomer selected from the group consisting of a zwitterionic monomer, a cationic monomer, and an anionic monomer.

14. In paragraph 13, A method for producing a hydrogel coating film for preventing frost, further comprising, before applying the hydrogel coating composition for preventing frost on a substrate, surface-treating the substrate with a silane compound containing an acrylic group to form an intermediate adhesive layer.

15. In paragraph 13, A method for producing a hydrogel coating film for preventing staining, wherein the ionic monomer comprises the cationic monomer and the anionic monomer in an equivalent ratio of 1:1.

Citation Information

Patent Citations

  • Composition for protecting plant from frost and / or freeze and method of application thereof

    JP2011155975A

  • Frost formation-restraining treatment composition for heat exchanger fin material

    JP2012241073A

  • Mixture of surface-post-crosslinked superabsorbers having different surface-post-crosslinking characteristics

    JP2012509166A

  • Aluminum fin material

    JP2023037459A

  • Durable icephobic surfaces

    KR1020180020964A