Microporous polyolefin membrane

The polyolefin microporous film with controlled air permeability and coating thickness addresses heat resistance and coating curl issues in lithium-ion batteries, enhancing battery performance and safety by ensuring minimal curl and stable heat shrinkage.

WO2024205057A1PCT designated stage expired Publication Date: 2024-10-03TORAY BATTERY SEPARATOR FILM KOREA LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/002847
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Polyolefin-based separators for lithium-ion secondary batteries face challenges with heat resistance and coating curl during manufacturing, affecting battery performance and safety.

Method used

A high-strength polyolefin microporous film with a coating layer on one or both sides, where the air permeability increase rate relative to coating thickness is limited to 15 or less, ensuring excellent heat resistance and minimizing coating curl, thereby improving battery cycle characteristics and safety.

Benefits of technology

The solution enhances the heat resistance and mechanical strength of the polyolefin microporous film, reducing coating curl and improving the productivity and stability of lithium-ion secondary batteries by maintaining optimal heat shrinkage and internal resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTKR2024002847-APPB-IMG-000001
    Figure PCTKR2024002847-APPB-IMG-000001
  • Figure PCTKR2024002847-APPB-IMG-000002
    Figure PCTKR2024002847-APPB-IMG-000002
Patent Text Reader

Abstract

The present invention relates to a microporous polyolefin membrane and, more specifically, to a microporous polyolefin membrane comprising a porous polyolefin substrate and a coating layer formed on one surface or both surfaces of the substrate, wherein the permeability increase rate, due to coating, relative to the coating thickness satisfies 15 or less, thereby having excellent heat resistance and preventing coating curling.
Need to check novelty before this filing date? Find Prior Art

Description

polyolefin microporous membrane

[0001] The present invention relates to a polyolefin microporous film, and more particularly, to a polyolefin microporous film having excellent heat resistance and preventing the occurrence of coating curl.

[0002]

[0003] Lithium-ion secondary batteries are widely used as power sources for portable electronic devices such as mobile phones, laptops, and camcorders, as well as electric vehicles. The polyolefin-based microporous membrane used as a separator in lithium-ion secondary batteries is closely related to the battery's performance, including its lifespan, output, and safety. To achieve superior battery performance, the polyolefin-based microporous membrane must possess appropriate permeability, superior mechanical properties, and heat resistance.

[0004] Polyolefin-based substrates commonly used as separators are subjected to temperatures exceeding 110°C during the manufacturing process, which includes stretching. This process, in turn, causes shrinkage due to changes in thermal properties. To address this issue, a technique has been proposed to enhance heat resistance by forming a coating layer on one or both sides of the separator using a mixture of inorganic particles, binders, and additive polymers. However, this coating layer can sometimes cause coating curling, which can lead to problems during the battery assembly process.

[0005] Accordingly, a high-strength polyolefin microporous film with excellent heat resistance and minimal coating curling and a coating separator using the film are required.

[0006]

[0007] The present invention has as its technical object the provision of a high-strength polyolefin microporous film having excellent heat resistance and minimizing the occurrence of coating curl, and a separator using the same.

[0008]

[0009] The present invention provides a polyolefin microporous film comprising a porous polyolefin substrate and a coating layer formed on one or both sides of the substrate, and satisfying the following formula 1.

[0010] [Formula 1]

[0011] (ba) / ct ≤ 15

[0012] In the above formula,

[0013] a is the pre-coating penetration rate (sec / 100cc),

[0014] b is the penetration rate after coating (sec / 100cc),

[0015] ct is the coating thickness (um).

[0016]

[0017] The polyolefin microporous film according to the present invention exhibits excellent heat resistance and strength, while minimizing coating curling. Therefore, the productivity and stability of secondary batteries using the polyolefin microporous film according to the present invention as a separator can be improved.

[0018]

[0019] The present invention will be described in detail below. However, it is not limited to the following description, and each component may be modified or selectively mixed as needed. Therefore, it should be understood that all modifications, equivalents, and alternatives included within the spirit and technical scope of the present invention are included.

[0020]

[0021] <Polyolefin microporous membrane>

[0022] The polyolefin microporous film of the present invention comprises a porous polyolefin substrate and a coating layer formed on one or both sides of the substrate, and satisfies the following formula 1.

[0023] [Formula 1]

[0024] (ba) / ct ≤ 15

[0025] In the above formula,

[0026] a is the pre-coating penetration rate (sec / 100cc),

[0027] b is the penetration rate after coating (sec / 100cc),

[0028] ct is the coating thickness (um).

[0029] ba is the difference in air permeability before and after coating, indicating the rate of increase in air permeability due to coating. The rate of increase in air permeability relative to the coating thickness may be 15 or less, for example, 13 or less. When the rate of increase in air permeability relative to the coating thickness of a polyolefin microporous film satisfies the aforementioned range, the occurrence of coating curl can be minimized, and when used as a separator, the resistance is reduced, which can improve the cycle characteristics of secondary batteries.

[0030] The coating thickness of the above polyolefin microporous film may be 1 to 10 um, for example, 1 to 6 um. If the coating thickness is less than the above-mentioned range, thermal shrinkage may worsen, which may compromise the safety of the battery. If the coating thickness exceeds the above-mentioned range, thermal shrinkage may be stable, but the internal resistance of the battery may increase, which may result in a decrease in battery output and difficulty in securing space between electrodes.

[0031] The high heat shrinkage (150°C, 1 hour) of the above polyolefin microporous film may be 10% or less, for example 5% or less, in both the transverse and axial directions. If the high heat shrinkage exceeds the above-mentioned range, the safety of the battery may be compromised.

[0032] The coating curl of the above polyolefin microporous film may be 4.0 mm or less, for example, 2.0 mm or less. If the coating curl exceeds the above-mentioned range, defects may occur in the battery assembly process.

[0033] The above polyolefin microporous membrane may satisfy the following equation 2.

[0034] [Formula 2]

[0035] Protrusion strength / t ≥ 40

[0036] In the above formula,

[0037] The protrusion strength is the protrusion strength (gf) of the porous polyolefin substrate,

[0038] t is the thickness (um) of the porous polyolefin substrate.

[0039] The strength-to-thickness ratio (gf / t) of the porous polyolefin substrate may be 40 or more, for example, 45 or more. When the strength-to-thickness ratio of the porous polyolefin substrate satisfies the above-mentioned range, high strength can be maintained with a thin, microporous film.

[0040] The polyolefin microporous film of the present invention comprises a porous polyolefin substrate and a coating layer formed on one or both sides of the substrate.

[0041]

[0042] Porous polyolefin substrate

[0043] The polyolefin resin constituting the porous polyolefin substrate of the present invention may be any conventional polyolefin resin known in the relevant technical field without limitation. For example, it may include polyethylene resin, polypropylene resin, or a mixture thereof.

[0044] The content of polyethylene resin may be, for example, 50 mass% or more, or, in another example, 60 mass% or more, with respect to the total mass of the polyolefin resin. The polyethylene resin may have a viscosity average molecular weight (Mv) of, for example, 5.0×10 4 4.0×10 6 g / mol, or another example, 7.0×10 4 3.5×10 6 It can be g / mol. The polyethylene may be any of high-density polyethylene (HDPE), medium-density polyethylene (MDPE), or low-density polyethylene (LDPE) without limitation. Alternatively, two or more types of polyethylene having different viscosity-average molecular weights (Mv) or densities may be mixed.

[0045] The content of the polypropylene resin may be, for example, 50 mass% or less, or, for another example, 40 mass% or less, relative to the total mass of the polyolefin resin. The polypropylene resin may have a viscosity average molecular weight (Mv) of, for example, 7.0×10 4 3.2×10 6 g / mol, or another example 9.5×10 4 3.0×10 6 It can be g / mol. As the polypropylene, atactic polypropylene (Atactic PP), syndiotactic polypropylene (Syndiotactic PP), isotactic polypropylene (isotactic PP), etc. can be used without limitation. Alternatively, two or more types of polypropylene having different viscosity average molecular weights (Mv) or densities can be mixed.

[0046] To further enhance the properties as a separator, the polyolefin resin may further include a polyolefin imparting a shutdown function. Examples of polyolefins imparting a shutdown function include low-density polyethylene (LDPE) and polyethylene wax. The low-density polyethylene (LDPE) may be at least one selected from the group consisting of branched LDPE, linear LDPE, and ethylene / α-olefin copolymers produced using a single-site catalyst. The amount of the LDPE may be appropriately adjusted within a range known in the art.

[0047] If necessary, conventional additives known in the relevant field, such as antioxidants and pore forming agents, may be included within a range that does not impair the effects of the present invention.

[0048] The polyolefin microporous film according to the present invention may have a multilayer structure in which multiple layers of the porous polyolefin substrate are laminated.

[0049]

[0050] coating layer

[0051] The polyolefin microporous film of the present invention comprises the porous polyolefin substrate described above and a coating layer formed on one or both sides of the substrate.

[0052] The coating composition forming the above coating layer includes inorganic particles and a binder. The coating composition may further include a solvent.

[0053] Non-limiting examples of usable inorganic particles include alumina, barium sulfate, aluminum hydroxide, barium titanium oxide, magnesium oxide, magnesium hydroxide, clay, titanium oxide, glass powder, boehmite, etc. The above inorganic particles may be used alone or in combination of two or more.

[0054] The size of the above-mentioned inorganic particles is not limited, but may range from 0.001 to 10 μm. When the size of the inorganic particles satisfies the above-mentioned range, a film of uniform thickness can be formed and an appropriate porosity can be secured.

[0055] The above-mentioned inorganic particles may be included in an amount of 88 to 98.8 wt%, for example, 95.4 to 98.8 wt%, based on the total weight of the coating composition. If the content of the inorganic particles is less than the above-mentioned range, the content of the binder may become excessively large, which may result in a decrease in the pore size and porosity due to a decrease in the empty space formed between the inorganic particles, thereby causing a decrease in the final battery performance due to an increase in ionic resistance. On the other hand, if the content of the binder exceeds the above-mentioned range, the content of the binder may be too small, which may result in a weakening of the adhesive strength between the inorganic materials and a weakening of the adhesive strength between the separator and the electrode.

[0056] Non-limiting examples of usable binders include polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, Examples of the binder include cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxyl methyl cellulose, acrylonitrile-styrene-butadiene copolymer, and polyimide. The binders may be used alone or in combination of two or more.

[0057] The binder may be included in an amount of 0.5 to 5.0 wt%, for example, 0.5 to 2.2 wt%, based on the total weight of the coating composition. If the content of the binder is less than the above-mentioned range, it may result in weakening of the adhesion between the inorganic materials and weakening of the adhesion between the separator and the electrode, and if it exceeds the above-mentioned range, the pore size and porosity may decrease due to a decrease in the empty space formed between the inorganic particles, which may result in a decrease in the final battery performance due to an increase in ionic resistance.

[0058] The coating composition of the present invention may further include a thickener. The thickener may be a polymer material such as carboxymethyl cellulose (CMC), methyl cellulose (MC), polyacrylic acid (PAA), polyethylene oxide (PEO), or polyacrylimide (PAM).

[0059] The thickener may be included in an amount of 0.5 to 5.0 wt%, for example, 0.5 to 1.5 wt%, based on the total weight of the coating composition. If the content of the thickener is less than the above-mentioned range, the amount adsorbed on the surface of the inorganic particles is small, making it difficult to maintain uniform dispersion, which may worsen heat shrinkage resistance. If the content exceeds the above-mentioned range, the viscosity of the dispersed slurry may increase, and coagulation or curling may occur between the inorganic particles.

[0060] The coating composition of the present invention may further include additives commonly used in the relevant technical field. Examples of such additives include vinylene carbonate, propane sultone, nitrile compounds, fluorinated surfactants, and nonionic surfactants.

[0061] The coating composition of the present invention may contain the binder, the thickener, and the additive in an amount of 1.2 to 12.0 wt%, for example, 1.2 to 4.6 wt%, based on the total weight of the coating composition. If the total content of the binder, the thickener, and the additive is less than the above-mentioned range, heat shrinkage may occur significantly, and if it exceeds the above-mentioned range, curling may not be prevented.

[0062] For example, the coating composition of the present invention can be manufactured by adding inorganic particles to a solvent in which a binder is dissolved, and then crushing and pulverizing the inorganic particles using a ball mill method. Non-limiting examples of usable solvents include acetone, tetrahydrofuran, methylene chloride, chloroform, water, dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone (NMR), or mixtures of two or more thereof.

[0063]

[0064] Method for manufacturing polyolefin microporous membrane

[0065] The method for manufacturing the polyolefin microporous film of the present invention is not particularly limited, and may include, for example, (1) a step of melt-mixing polyolefin and a plasticizer to prepare a polyolefin solution, (2) a step of extruding the polyolefin solution and then cooling it to form a sheet-shaped article, (3) a first stretching step of stretching the sheet-shaped article to form a film, (4) a step of removing the plasticizer from the film, (5) a step of drying the film from which the plasticizer has been removed, (6) a second stretching step of re-stretching the dried film, (7) a step of heat-treating to prepare a porous polyolefin substrate, (8) a step of preparing a coating slurry, and (9) a step of forming a coating layer on one or both sides of the porous polyolefin substrate. Hereinafter, each manufacturing process will be described in detail.

[0066]

[0067] (1) Preparation process of polyolefin solution

[0068] A polyolefin solution is prepared by melt-mixing a polyolefin resin and a plasticizer. Conventional methods known in the art can be used without limitation for melt-mixing a composition comprising a polyolefin resin and a plasticizer. For example, a method of melt-mixing a polyolefin resin and a plasticizer at a temperature of 100 to 250°C using a twin-screw extruder can be used.

[0069] The content of the polyolefin resin is not particularly limited, and for example, it may be included in an amount of 20 to 50 wt% based on the total weight of the composition including the polyolefin resin and the plasticizer, and for another example, it may be included in an amount of 20 to 40 wt%.

[0070] In the present invention, a plasticizer may be used without limitation as a conventional component known in the relevant technical field, and for example, it may be any organic compound that forms a single phase with the polyolefin resin at the extrusion temperature.

[0071] Non-limiting examples of usable plasticizers include aliphatic or cyclic hydrocarbons such as liquid paraffin (or paraffin oil) such as nonane, decane, decalin, and liquid paraffin (LP); paraffin wax; phthalic acid esters such as dibutyl phthalate and dioctyl phthalate; fatty acids having 10 to 20 carbon atoms such as palmitic acid, stearic acid, oleic acid, linoleic acid, and linolenic acid; fatty acid alcohols having 10 to 20 carbon atoms such as palmitic alcohol, stearic alcohol, and oleic alcohol. The above plasticizers may be used alone or in combination of two or more.

[0072] Among the above plasticizers, liquid paraffin is harmless to the human body, has a high boiling point, and contains little volatile components, making it suitable for use as a plasticizer in wet processes.

[0073] The content of the plasticizer is not particularly limited, and may be included in an amount of, for example, 50 to 90 wt% based on the total weight of the composition including the polyolefin resin and the plasticizer, and may be included in an amount of, for example, 60 to 80 wt% based on the total weight of the composition including the polyolefin resin and the plasticizer.

[0074] In addition to the polyolefin resin described above, other resins, inorganic particles, additives, etc. that are common in the relevant technical field may be included.

[0075]

[0076] (2) Sheet-shaped product formation process

[0077] The polyolefin solution manufactured in the above step (1) is extruded through a die equipped with an extruder and cooled to form a sheet-shaped product.

[0078] When a polyolefin solution is extruded through a die and cooled to form a gel-like sheet, the surface pore size and the porosity ratio can be controlled, for example, by controlling the cooling rate. For example, the cooling can be performed at a rate of 40°C / min or more, for example, 100°C / min or more, in another example, 100 to 650°C / min, or in another example, 300 to 650°C / min. If the cooling rate is less than the above-mentioned range, the phase separation between the resin and the plasticizer, as well as the phase separation between polyethylene and polypropylene in the resin, may proceed excessively, resulting in uneven initial micropore formation, and as a result, it may be difficult to control the surface pore size and the porosity ratio within a certain range.

[0079] The cooling method is not particularly limited, and any method known in the relevant technical field, such as cooling by contact with a chill roll, cooling with cold air, or cooling by immersion in cold water, may be used.

[0080]

[0081] (3) First extension process

[0082] The sheet-shaped material obtained in the above step (2) is biaxially stretched at least once to form a film. The size and surface porosity of the surface and internal pores of the porous film are primarily controlled through stretching and heating in the first stretching process.

[0083] In the present invention, the first stretching process can be performed at a predetermined ratio using a conventional method in the relevant technical field, such as a tenter method, a roll method, an inflation method, a rolling method, or a combination of these methods. In the case of biaxial stretching, either simultaneous biaxial stretching or sequential stretching may be performed.

[0084] In the above first stretching process, the stretching ratio varies depending on the thickness of the sheet-shaped material, but for example, in biaxial stretching, it is appropriate to perform at least 2 times x 2 times or more in any direction, and for example, it can be performed in the range of 3 to 10 times.

[0085] In the first stretching process, the structure of the fibrils, pore size, and porosity can be controlled by controlling the stretching temperature and air volume, and in particular, the porosity ratio can be controlled to be low by maintaining the temperature and air volume of the hot air applied to both sides of the sheet as equal as possible.

[0086] In the first stretching process of the present invention, the stretching temperature may be, for example, in the range of 100 to 130°C, and as another example, in the range of 105 to 125°C. When stretching in the above range, stretching can be performed to have appropriate air permeability and mechanical strength without blocking the pores within the sheet. If the first stretching temperature exceeds the above-mentioned temperature range, the resin within the sheet may melt, causing the molecular chains to not be oriented by stretching and resulting in non-uniform pore sizes. On the other hand, if the first stretching temperature is lower than the above-mentioned temperature range, softening of the sheet may be insufficient, resulting in breakage during stretching and failure to achieve high stretching ratios.

[0087]

[0088] (4) Plasticizer removal process

[0089] The plasticizer is extracted from the stretched film using a washing solvent. Since the polyolefin phase is phase-separated from the plasticizer, removing the plasticizer results in a porous film with a multi-pore structure. Any conventional method known in the art can be used without limitation to remove the plasticizer.

[0090] In the present invention, any organic solvent capable of extracting the plasticizer may be used as the cleaning solvent without particular limitation. For example, halogenated hydrocarbons such as methylene chloride, 1,1,1-trichloroethane, and fluorocarbons, which have high extraction efficiency and are easy to dry; hydrocarbons such as n-hexane and cyclohexane; alcohols such as ethanol and isopropanol; and ketones such as acetone and 2-butanone, may be used. For example, when liquid paraffin is used as the plasticizer, methylene chloride may be used as the organic solvent.

[0091]

[0092] (5) Drying process

[0093] The polyolefin microporous membrane obtained by removing the plasticizer can be dried using a conventional drying method known in the art. Examples of such methods include a heat drying method and an air drying method.

[0094]

[0095] (6) Second extension process

[0096] Next, the dried film is again stretched at least in one direction. Through stretching and heating in the second stretching process, the pore size and surface porosity of the surface and interior of the porous film are secondarily adjusted, thereby producing a microporous film in its final form.

[0097] In the present invention, the second stretching process can be performed in the same manner as the first stretching process, such as by a tenter method, while heating the film. The stretching can be uniaxial stretching or biaxial stretching.

[0098] The temperature of the second stretching process may be, for example, in the range of the crystal dispersion temperature of the polyolefin resin constituting the microporous membrane or higher, and the crystal dispersion temperature + 40°C or lower, or, as another example, in the range of the crystal dispersion temperature + 10°C or higher, and the crystal dispersion temperature + 40°C or lower. The crystal dispersion temperature refers to a value obtained by measuring the temperature characteristics of dynamic viscoelasticity based on ASTM D4065. When the polyolefin resin is polyethylene, its crystal dispersion temperature is generally 90 to 100°C.

[0099] By controlling the second stretching temperature within the aforementioned range, it is possible to prevent a decrease in permeability and the occurrence of property deviation in the sheet width direction when stretching in the transverse direction (width direction: TD direction). By controlling the second stretching temperature within the aforementioned range, it is possible to suppress the occurrence of deviation in the width direction while simultaneously controlling the pore size and porosity of the surface and interior of the film within the range of the present invention. At a temperature exceeding the aforementioned range, it may be difficult to control the pore size and porosity within the range of the present invention due to excessive melting of the polyolefin resin, and at a temperature below the aforementioned range, the film may be easily broken by stretching due to insufficient softening, and uniform stretching may not be achieved, making it difficult to secure uniform surface and interior pore size and porosity.

[0100] Additionally, by controlling the temperature of the second stretching process within the aforementioned range, the polyolefin resin can be sufficiently softened, preventing film rupture and enabling uniform stretching. For example, the second stretching temperature may be in the range of 90 to 140°C, and in another example, in the range of 120 to 140°C.

[0101] The magnification in the uniaxial direction of the second stretching may be, for example, 1.0 to 1.8 times, and as another example, 1.2 to 1.6 times. For example, in the case of uniaxial stretching, the magnification is set to 1.0 to 1.8 times in the longitudinal direction (machine direction: MD direction) or TD direction. In the case of biaxial stretching, the magnification is adjusted to 1.0 to 1.8 times in the MD direction and the TD direction, respectively. In the case of biaxial stretching, the respective magnifications in the MD direction and the TD direction may be the same or different. By adjusting the magnification within the aforementioned range, it is possible to prevent deterioration in permeability, electrolyte absorbency, and compression resistance, and to prevent excessive thinning of fibrils and deterioration in heat shrinkage resistance.

[0102]

[0103] (7) Heat treatment process

[0104] Next, the re-stretched film is fixed and heat-treated. The heat-treatment method may be any conventional method known in the relevant technical field without limitation, and examples thereof include heat-setting treatment and / or heat-relaxing treatment.

[0105] In particular, by performing a heat fixation treatment, the crystal structure of the fibrils formed by the second stretching process is stabilized, so that a microporous membrane having the surface and internal pore sizes of the present invention, a uniform pore size distribution, and a small porosity ratio on both surfaces can be produced.

[0106] In the present invention, the heat-setting treatment is performed within a temperature range from above the crystal dispersion temperature to below the melting point of the polyolefin resin constituting the microporous membrane. At this time, the heat-setting treatment can be performed using a tenter method, a roll method, or a rolling method.

[0107] Thermal relaxation can be performed using tenter, roll, or compression methods, or can be performed using belt conveyors or floating rolls. Thermal relaxation can be performed, for example, at a relaxation rate of 20% or less in at least one direction, and, for other examples, at a relaxation rate of 10% or less.

[0108]

[0109] (8) Coating slurry manufacturing process

[0110] A dispersant is added to a solvent containing water as the main component, and then inorganic particles are added and stirred to produce a mixture. The mixture is dispersed and crushed using a bead mill disperser using ceramic beads having a particle size of 0.3 mm to 1.0 mm to produce a master batch solution, and at least one binder and other additives are added to produce a slurry.

[0111]

[0112] (9) Coating process

[0113] The method for applying the above coating slurry onto a porous polyolefin substrate is not particularly limited, and may include a dip coater method, a roll coater method, an air-knife coater method, a blade coater method, a rod coater method, a bar coater method, a comma coater method, a gravure coater method, a silk screen coater method, a die coater method, a microgravure coater method, etc. The coating speed can be controlled in a range of, for example, 30 to 200 m / min, such as 40 to 130 m / min. The coated porous polyolefin is dried by passing it through a multi-stage oven at a constant speed. The drying temperature can be 40 to 100°C. Water can be removed from the wet coating layer through thermal evaporation and the oven. The pressure and temperature of the oven are determined by the amount of moisture.

[0114] The above coating methods can be applied alone or in combination of two or more methods.

[0115]

[0116] Lithium-ion secondary battery

[0117] The present invention provides a secondary battery, for example, a lithium ion secondary battery, comprising the polyolefin microporous film described above.

[0118] The lithium ion secondary battery of the present invention can be manufactured according to conventional methods known in the art, except that the polyolefin microporous film according to the present invention is used as a separator. For example, the battery can be manufactured by interposing a separator between the positive electrode and the negative electrode and introducing a non-aqueous electrolyte.

[0119] The lithium ion secondary battery of the present invention includes a negative electrode, a positive electrode, a separator, and an electrolyte as battery components, wherein the components of the positive electrode, the negative electrode, the electrolyte, and other additives, if necessary, excluding the separator described above, are based on components of conventional lithium ion secondary batteries known in the relevant industry.

[0120] For example, the positive electrode can be manufactured using a conventional positive electrode active material for lithium ion secondary batteries known in the art, and non-limiting examples thereof include lithium transition metal composite oxides such as LiMxOy (M = Co, Ni, Mn, CoaNibMnc) (e.g., lithium manganese composite oxides such as LiMn2O4, lithium nickel oxides such as LiNiO2, lithium cobalt oxides such as LiCoO2 and those in which some of the manganese, nickel, and cobalt of these oxides are replaced with other conventional transition metals or aluminum, or vanadium oxides containing lithium, etc.), LiNPO4 (N = Fe, Mn, Co, Ni) having an olivine structure, or chalcogen compounds (e.g., manganese dioxide, titanium disulfide, molybdenum disulfide, etc.).

[0121] For example, the negative electrode can be manufactured using a conventional negative electrode active material for lithium ion secondary batteries known in the industry, and non-limiting examples thereof include materials capable of intercalating / deintercalating lithium ions, such as lithium metal or lithium alloy, coke, artificial graphite, natural graphite, organic polymer compound combustion bodies, carbon fiber, silicon-based, and tin-based materials.

[0122] The non-aqueous electrolyte comprises electrolyte components commonly known in the industry, such as electrolyte salts and electrolyte solvents.

[0123] The above electrolyte salt may be composed of a combination of (i) a cation selected from the group consisting of Li+, Na+, and K+ and (ii) an anion selected from the group consisting of PF6-, BF4-, Cl-, Br-, I-, ClO4-, AsF6-, CH3CO2-, CF3SO3-, N(CF3SO2)2-, and C(CF2SO2)3-, and among these, a lithium salt is preferable. Specific examples of the lithium salt include LiClO4, LiCF3SO3, LiPF6, LiBF4, LiAsF6, and LiN(CF3SO2)2. These electrolyte salts may be used alone or in combination of two or more.

[0124] The above electrolyte solvent may be a cyclic carbonate, a linear carbonate, a lactone, an ether, an ester, an acetonitrile, a lactam, or a ketone.

[0125] Examples of the cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), fluoroethylene carbonate (FEC), etc., and examples of the linear carbonates include diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), and methyl propyl carbonate (MPC), etc. An example of the lactone is gamma-butyrolactone (GBL), and examples of the ethers include dibutyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, 1,2-dimethoxyethane, 1,2-diethoxyethane, etc. Examples of the above esters include methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, butyl propionate, and methyl pivalate. In addition, examples of the lactam include N-methyl-2-pyrrolidone (NMP), and examples of the ketone include polymethylvinyl ketone. In addition, halogen derivatives of the above organic solvents may also be used, but are not limited thereto. In addition, glyme, diglyme, triglyme, and tetraglyme may also be used as the above organic solvents. These organic solvents may be used alone or in combination of two or more.

[0126]

[0127] Hereinafter, the present invention will be described in more detail through examples. However, the following examples are intended only to aid understanding of the present invention and are not intended to limit the scope of the present invention in any way.

[0128]

[0129] [Example 1-5]

[0130] According to Table 1 below, a porous polyolefin substrate and a coating composition were prepared, and a coating layer was formed on one surface of the substrate to prepare a polyolefin microporous film of each example. The physical properties of the polyolefin microporous film of each example were measured using the following method, and the results are shown in Table 1 below.

[0131]

[0132] [Comparative Example 1-4]

[0133] According to Table 2 below, a porous polyolefin substrate and a coating composition were prepared, and a coating layer was formed on one surface of the substrate to prepare a polyolefin microporous film of each comparative example. The physical properties of the polyolefin microporous film of each comparative example were measured using the same method as in the examples, and the results are shown in Table 2 below.

[0134]

[0135] thickness

[0136] The film thickness D (㎛) and coating thickness of the polyolefin microporous film were measured according to the JIS standard (K7130-1992).

[0137]

[0138] Protrusion strength

[0139] After cutting the polyolefin microporous membrane to 95 mm wide x 95 mm long to manufacture specimens, each specimen was placed on a 10 mm hole using a Kato Tech KES-G5 measuring device, and the puncture force (gf) was measured with a 1 mm probe.

[0140]

[0141] Speculation

[0142] Air permeability is the time (in seconds) required for 100 cc of air to pass through a coating film of a given area under a given pressure. The air permeability of the porous polyolefin substrate before coating and the polyolefin microporous film after coating were measured using an Oken-type air permeability tester (Asahi Seiko Co. Ltd., EGO-1T) according to the JISP8117 measurement method. The air permeability increase rate was calculated as the air permeability before coating (b) minus the air permeability after coating (a).

[0143]

[0144] heat shrink

[0145] After leaving the polyolefin microporous membrane in a hot air drying oven at 150°C for 60 minutes, the shrinkage rate (%) in the longitudinal and transverse directions was checked.

[0146]

[0147] curl

[0148] The longitudinal direction of the polyolefin microporous film is fixed inside a dry box (dew point -50±10℃), left for 3 minutes, and the transverse curl (bending of the film) is measured with a ruler (mm).

[0149]

[0150]

[0151]

[0152] Inorganic particles: Barium Sulfate

[0153] Dispersant: Carboxylic copolymer mixture

[0154] Thickener: Anionic acrylic series, acrylonitrile-acrylic acid-acrylamide mixture

[0155] Binder: Acrylic synthetic polymer

[0156] Additives: Nonionic surfactant, polyoxyalkylene

[0157]

[0158] As shown in Tables 1 and 2 above, the microporous membranes of Examples 1-5 that satisfy Equation 1 according to the present invention exhibited excellent properties across all measured items. On the other hand, in the case of the microporous membranes of Comparative Examples 1-4 that do not satisfy Equation 1 according to the present invention, the membranes were rolled up so that curl measurement was impossible (Comparative Examples 1, 3, 4), or curling occurred more severely than in the examples (Comparative Example 2), and the thermal shrinkage in the longitudinal and transverse directions was irregular and the coating layer was detached so that thermal shrinkage measurement was impossible (Comparative Example 3).

[0159]

[0160] The polyolefin microporous film according to the present invention exhibits excellent heat resistance and strength, while minimizing coating curling. Therefore, the productivity and stability of secondary batteries using the polyolefin microporous film according to the present invention as a separator can be improved.

Claims

1. A polyolefin microporous film comprising a porous polyolefin substrate and a coating layer formed on one or both sides of the substrate, and satisfying the following formula 1: [Formula 1] (ba) / ct ≤ 15 In the above formula, a is the pre-coating penetration rate (sec / 100cc), b is the penetration rate after coating (sec / 100cc), ct is the coating thickness (um).

2. A polyolefin microporous film having a coating thickness of 1 to 10 um in the first paragraph.

3. A polyolefin microporous film having a high heat shrinkage (150°C, 1 hour) of 10% or less in both the transverse and axial directions in the first paragraph.

4. A polyolefin microporous film having a coating curl of 4.0 mm or less in the first paragraph.

5. In paragraph 1, a polyolefin microporous film satisfying the following formula 2: [Formula 2] Protrusion strength / t ≥ 40 In the above formula, The protrusion strength is the protrusion strength (gf) of the porous polyolefin substrate, t is the thickness (um) of the porous polyolefin substrate.

6. A polyolefin microporous film in accordance with claim 1, wherein the coating composition forming the coating layer comprises 88 to 98.8 wt% of inorganic particles and 0.5 to 5.0 wt% of binder based on the total weight of the coating composition.

7. In the first paragraph, the coating composition forming the coating layer includes inorganic particles, a binder, a thickener, and an additive, A polyolefin microporous film comprising 1.2 to 12.0 wt% of the binder, the thickener, and the additive based on the total weight of the coating composition.

8. A lithium ion secondary battery comprising a polyolefin microporous film according to one of claims 1 to 7.

Citation Information

Patent Citations

  • Lithium ion battery diaphragm with high heat resistance and high adhesion and preparation method thereof

    CN113972441A

  • A method of manufacturing separator for electrochemical device and separator for electrochemical device manufactured thereby

    KR101816764B1

  • Laminated porous film and production method therefor

    KR1020160143665A

  • Cosmetic composition for shape restoration gel comprising Polymer

    KR1020230130371A

  • Battery separator and method for producing same

    KR102036519B1