High elongation modulus film coating liquid, and method for manufacturing high elongation film using coating liquid

The high elongation modulus film coating solution, using optimized acrylic oligomer and photoinitiator compositions, addresses the limitations of conventional films by achieving rapid recovery and enhanced properties, overcoming issues of slow recovery and high processing costs, and enabling efficient manufacturing without heat drying.

WO2024205066A1PCT designated stage expired Publication Date: 2024-10-03POLYNETRON CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/002967
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional elongation films, such as PPF and EPU, face issues with slow recovery time, high heat-curing equipment requirements, and high processing costs, which limit their commercialization and productivity, while also suffering from yellowing and reduced transparency over time.

Method used

A high elongation modulus film coating solution is developed using a specific composition of acrylic oligomer, photocurable mixed monomer, and photoinitiator, optimizing the mixing composition and content to achieve a breaking point, elongation in the 300% to 600% range, and rapid recovery speed without heat drying, utilizing aliphatic urethane acrylate, DMAA, NVP, and THFA, with a photoinitiator like 2-Hydroxy-2-methyl-1-phenyl-1-propanone, to create a film that can be manufactured on existing EPU film production lines.

Benefits of technology

The solution provides a high elongation modulus film with immediate recovery speed, improved elasticity, and enhanced physical properties, such as water resistance and adhesion, while eliminating the need for heat drying, thus addressing the limitations of existing films and meeting market demands for durability and customization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTKR2024002967-APPB-IMG-000001
    Figure PCTKR2024002967-APPB-IMG-000001
  • Figure PCTKR2024002967-APPB-IMG-000002
    Figure PCTKR2024002967-APPB-IMG-000002
  • Figure PCTKR2024002967-APPB-IMG-000003
    Figure PCTKR2024002967-APPB-IMG-000003
Patent Text Reader

Abstract

The present invention pertains to a high elongation modulus film coating liquid, and a method for manufacturing a high elongation film using the coating liquid. The coating liquid contains 40-69 wt% of an acrylic oligomer, 30-50 wt% of a photocurable mixed monomer, and 1-10 wt% of a photoinitiator. By optimizing the specific ingredients and contents of the acrylic oligomer, photocurable mixed monomer, and photoinitiator without a heat drying process, the high elongation modulus film coating liquid composed of the above ingredients provides a high elongation modulus film that exhibits a breaking point required by the market, an elongation in the range of 300%, and a restoration speed, or a high elongation modulus film that exhibits a restoration speed of 30 seconds or less while satisfying an elongation in the range of 600%.
Need to check novelty before this filing date? Find Prior Art

Description

High-elasticity modulus film coating solution and method for manufacturing high-elasticity film using the coating solution

[0001] The present invention relates to a high-elasticity modulus film coating solution and a method for manufacturing a high-elasticity film using the coating solution, and more particularly, to a high-elasticity modulus film coating solution that provides a high-elasticity modulus film that realizes a breaking point, an elongation in the range of 300%, and a recovery speed required in the market, or a high-elasticity modulus film that realizes a recovery speed of less than 30 seconds while satisfying an elongation in the range of 600%, by optimizing specific components and contents of an acrylic oligomer, a photocurable mixed monomer, and a photoinitiator without a heat-drying process, and a method for manufacturing a high-elasticity film using the coating solution.

[0002] Currently, the most commonly used flexible films in the market are PPF (Paint Protection Film) film and EPU (Elastic Poly Urethane) film.

[0003] PPF film, introduced in Korea less than 10 years ago, protects a car's paint from various minor external impacts. It can even be scratched with a car key, as long as the object is not sharp. In other words, even if you scrub with all your might with a scrubbing sponge, it won't cause even 0.1% damage to the paint. Therefore, unless you use a sharp knife, it's absolutely impossible to penetrate PPF film, ensuring complete protection.

[0004] Additionally, the transparency of the PPF film itself is lower than that of spray-on clear paint, and yellowing, which occurs over time as the adhesive inside the film changes due to ultraviolet rays, is also pointed out as a disadvantage.

[0005] Therefore, PPF films have limitations in commercialization due to the high cost of heat-curing equipment and processes, and in order to improve problems after construction, durable film performance such as non-yellowing, water-repellent, high gloss, and anti-contamination or anti-staining is required.

[0006] In this regard, Patent Document 1 discloses an invention relating to a photocurable paint composition and a molded article including a cured coating layer formed therefrom, and specifically, a molded article including a photocurable paint composition for a plastic substrate [e.g., polycarbonate (PC), polymethyl methacrylate (PMMA)], particularly an automobile headlamp molded article, and a cured coating layer formed therefrom, which comprises a multifunctional polyurethane acrylate having 5 or more functional groups, a mono- to di-functional polyurethane acrylate, a mono- to tri-functional acrylate, a photopolymerization initiator, and a triazine-based ultraviolet absorber, and has excellent physical properties such as adhesion to a plastic substrate, water resistance, moisture resistance, heat resistance, and cold and heat resistance, and particularly has excellent weather resistance.

[0007] On the other hand, EPU film is cheaper than PPF and is currently being used as an alternative film.

[0008] EPU film is a more elastic film than standard polyurethane. It boasts high transparency due to its high transmittance, heat resistance up to 250°C, and exceptional elasticity, allowing it to return to its original shape even after being crumpled or cut. Therefore, it can be easily applied to curved surfaces, covering the entire LCD of even edge-mounted phones.

[0009] Therefore, EPU film can be applied in various fields such as replacing PPF that protects vehicle bodies, or as a film for mobile phones or OLED packaging by blocking light inside tablet PCs and laptops.

[0010] In particular, PPF films and EPU films must be provided as customized products to suit the customer's desired size, thickness, characteristics, and high transmittance.

[0011] However, both PPF film and EPU film have elasticity and resilience, but have the problem of slow recovery time.

[0012] In addition, since conventional flexible films must undergo a process of ultraviolet curing and then heat drying during the manufacturing process, the manufacturing process is complex and there are problems with low productivity.

[0013] Accordingly, the inventors of the present invention have made efforts to solve the problems of the past, and as a result, in an elastic elongation film comprising an acrylic oligomer, a monomer, and an initiator, which is an aliphatic urethane acrylate having a functional group number of 2, the mixed composition and content of the acrylic oligomer, the monomer, and the initiator are optimized to provide a high elongation modulus film coating solution that realizes a breaking point, an elongation in the range of 300%, and an immediate recovery speed required in the market without a heat drying process, or a high elongation modulus film coating solution that realizes a recovery speed of less than 30 seconds while satisfying an elongation in the range of 600%, and has completed the present invention by providing a film capable of controlling elasticity and elongation in a hard type EPU film that can be manufactured in a current EPU film manufacturing line.

[0014] The purpose of the present invention is to provide a high-elasticity modulus film coating solution that provides a high-elasticity modulus film that realizes a breaking point, an elongation in the range of 300%, and a recovery speed required in the market, or a high-elasticity modulus film that realizes a recovery speed within 30 seconds while satisfying an elongation in the range of 600%, by optimizing the specific components and contents of an acrylic oligomer, a photocurable mixed monomer, and a photoinitiator without a heat-drying process, and a method for manufacturing a high-elasticity film using the coating solution.

[0015] The object of the present invention is to provide a photopolymerizable polymeric composition comprising 40 to 69 wt% of an acrylic oligomer, 30 to 50 wt% of a photocurable mixed monomer, and 1 to 10 wt% of a photoinitiator, wherein the photocurable mixed monomer comprises 10 to 90 wt% of a curing-improving monomer and 10 to 90 wt% of an elongation-improving monomer, wherein the curing-improving monomer comprises at least one selected from the group consisting of DMAA (N,N-dimethylacrylamide), NVP (N-vinyl pyrrolidone), NVC (N-vinyl caprolactam), ACMO (4-acryloylmorpholine), HDDA (1,6-hexanediol diacrylate), HEA (2-hydroxyethyl acrylate), and HPA (Hydroxypropyl acrylate), and wherein the elongation-improving monomer comprises PHEA (2-phenoxyethyl acrylate), PEGDA (poly(ethylene glycol) The present invention is achieved by providing a high elongation modulus film coating solution comprising at least one selected from the group consisting of diacrylate, IBOA (isobornyl olefin acid ester) and THFA (Tetrahydrofurfuryl acrylate), and providing a film having a breaking point of 35±5 mm, an elongation of 280±80%, and a recovery speed of 1 to 2 for a tensile force of 280 to 320 mm / min.

[0016] In addition, the object of the present invention is to provide a photopolymerizable polymeric composition comprising 40 to 50 wt% of an acrylic oligomer, 30 to 40 wt% of a photocurable mixed monomer, and 1 to 10 wt% of a photoinitiator, wherein the photocurable mixed monomer is composed of 10 to 90 wt% of a curing-improving monomer and 10 to 90 wt% of an elongation-improving monomer, and the curing-improving monomer is composed of at least one selected from the group consisting of DMAA (N,N-dimethylacrylamide), NVP (N-vinyl pyrrolidone), NVC (N-vinyl caprolactam), ACMO (4-acryloylmorpholine), HDDA (1,6-hexanediol diacrylate), HEA (2-hydroxyethyl acrylate), and HPA (Hydroxypropyl acrylate), and the elongation-improving monomer is selected from the group consisting of PHEA (2-phenoxyethyl acrylate), PEGDA (poly(ethylene glycol) The present invention can also be improved by providing a high elongation modulus film coating solution comprising at least one selected from the group consisting of diacrylate, IBOA (isobornyl olefin acid ester) and THFA (Tetrahydrofurfuryl acrylate), and providing a film having a breaking point of 60±5 mm, an elongation of 550±50%, and a recovery speed of 30 seconds or less for a tensile force of 280 to 320 mm / min.

[0017] According to a preferred feature of the present invention, the acrylic oligomer is composed of an aliphatic urethane acrylate having a weight average molecular weight of 15,000 to 25,000.

[0018] According to a more preferred feature of the present invention, the acrylic oligomer is composed of 60 to 90 wt% of aliphatic urethane acrylate having a viscosity of 45,000 to 60,000 cps at 60°C and 10 to 40 wt% of aliphatic urethane acrylate having a viscosity of 50,000 to 100,000 cps at 60°C.

[0019] According to a more preferred feature of the present invention, the photocurable mixed monomer is composed of 35 to 65 wt% of NVP (N-vinyl-2-pyrrolidone), 30 to 55 wt% of THFA (Tetrahydrofurfuryl acrylate), and 5 to 10 wt% of HEA (2-hydroxyethyl acrylate).

[0020] According to a further preferred feature of the present invention, the high elongation modulus film coating liquid further contains a mixed initiator, and the mixed initiator is composed of 80 to 90 wt% of 2-Hydroxy-2-methyl-1-phenyl-1-propanone and 10 to 20 wt% of 1-Hydro-cyclohexyl-phenyl-ketone.

[0021] In addition, the object of the present invention can be achieved by providing a method for manufacturing a high-elasticity film, characterized in that the method comprises the steps of pouring the high-elasticity modulus film coating liquid between two sheets of release film in the shape of the letter I, then using a laminating machine to stamp out a liquid coating film of 50 to 100 μm in thickness to manufacture a sample, and then curing the manufactured sample by irradiating it with light.

[0022] The high-elasticity modulus film coating liquid according to the present invention is provided as a coating liquid that exhibits elasticity, which is a basic film characteristic, without a heat drying process, so that it is easy to check changes in physical properties according to optimization of the components and contents of the coating liquid, and products can be provided to meet various market needs during manufacturing.

[0023] That is, the purpose of the present invention is to provide a high elongation modulus film that realizes a breaking point, elongation in the range of 300%, and recovery speed required in the market by optimizing the specific components and contents of an acrylic oligomer, a photocurable mixed monomer, and a photoinitiator, or a high elongation modulus film that realizes a recovery speed of 30 seconds or less while satisfying an elongation in the range of 600%.

[0024] Hereinafter, the present invention will be described in detail.

[0025] The present invention provides a high elongation modulus film coating solution that satisfies the properties required in the market by optimizing the mixed composition and content of the acrylic oligomer, the photocurable mixed monomer and the photoinitiator, in an elastic elongation film comprising an acrylic oligomer, which is an aliphatic urethane acrylate having a functional group number of 2, a photocurable mixed monomer and a photoinitiator.

[0026] An oligomer is a molecule formed by repeating several to several dozen atoms or groups of atoms (these are called constituent units) of one or more types, and its physical properties change depending on the increase or decrease of one or several constituent units. It is also called an oligomer. In addition, when an oligomer is exposed to UV, the photoinitiator in the resin receives UV energy and initiates a polymerization reaction, and combines with the monomer, which is the main component of the UV ink or UV resin, to instantaneously cause a polymerization polymerization reaction, and is a substance that determines water resistance and adhesiveness.

[0027] In this way, monomers and oligomers are in a liquid state because they have small molecular weights, and when polymerization occurs, they change into a solid state with a very large molecular weight. At this time, the resin in a liquid state before curing instantly changes into a solid state, which is called UV curing.

[0028] The types of oligomers include 1) epoxy acrylate, 2) polyester acrylate, 3) urethane acrylate, and 4) silicone acrylate, depending on the chemical composition of the functional group.

[0029] In the present invention, it is preferable to use a urethane acrylate oligomer having good water resistance, adhesiveness, and flexibility, and in particular, an aliphatic urethane acrylate having a functional group of 2 is used.

[0030] In addition, in an embodiment of the present invention

[0031] PN-MF5023: Aliphatic urethane acrylate (bifunctional), weight average molecular weight 15,000 to 25,000, viscosity at 60°C 45,000 to 60,000 cpm, refractive index 1.477±0.002

[0032] PN-MF2923: Aliphatic urethane acrylate (bifunctional), weight average molecular weight 15,000 to 25,000, viscosity at 60°C 50,000 to 100,000 cpm, refractive index 1.481±0.003

[0033] PN-MF1423: Aliphatic urethane acrylate (difunctional),

[0034] Satorum aliphatic urethane acrylate (bifunctional),

[0035] Asia Industrial Aliphatic Urethane Acrylate (Difunctional),

[0036] Entissa aliphatic urethane acrylate (bifunctional),

[0037] Using the difunctional aliphatic urethane acrylate, the optimal aliphatic urethane acrylate with two functional groups that satisfies the properties required by the market is determined through a combination of compositions.

[0038] Accordingly, the present invention provides, as a first preferred embodiment, a film comprising 40 to 69 wt% of an acrylic oligomer, which is an aliphatic urethane acrylate having a functional group number of 2, 30 to 50 wt% of a photocurable mixed monomer, and 1 to 10 wt% of a photoinitiator, having a breaking point of 35±5 mm, an elongation of 280±80%, and a recovery speed of 1 to 2 for a tensile force of 280 to 320 mm / min, wherein the recovery speed is at a level of "immediate recovery."

[0039] In the present invention, the restoration experiment was performed by pulling 200% (the sample was 100 mm) and releasing the right fixing device. If the restoration was close to the original length of 10 mm (tolerance 1 mm) within 1 to 2 seconds using a stopwatch, it was classified as “immediate restoration”. If the original length was restored within 1 minute, it was classified as “restored”. If it took more than 1 minute, it was classified as “no restoration”.

[0040] At this time, the acrylic oligomer is preferably a mixed oligomer containing 60 to 90 wt% of PN-MF2923 (bifunctional aliphatic urethane acrylate), more preferably, the acrylic oligomer is composed of 60 to 90 wt% of PN-MF2923 (bifunctional aliphatic urethane acrylate) and 10 to 40 wt% of PN-MF5023 (bifunctional aliphatic urethane acrylate), and most preferably, 90 wt% of PN-MF2923 (bifunctional aliphatic urethane acrylate) and 10 wt% of PN-MF5023 (bifunctional aliphatic urethane acrylate).

[0041] In addition, the present invention provides, as a second preferred embodiment, a coating solution capable of producing a high elongation modulus film comprising 40 to 50 wt% of an acrylic oligomer, which is an aliphatic urethane acrylate having a functional group number of 2, 30 to 40 wt% of a photocurable mixed monomer, and 1 to 10 wt% of a photoinitiator, having a breaking point of 60±5 mm, an elongation of 550±50%, and a recovery speed of 30 seconds or less for a tensile force of 280 to 320 mm / min.

[0042] In the high-elasticity modulus film coating liquid of the second embodiment, the acrylic oligomer is a mixed oligomer containing 60 to 90 wt% of PN-MF5023 (bifunctional aliphatic urethane acrylate), and more preferably, the acrylic oligomer is a mixed oligomer containing 60 to 90 wt% of PN-MF5023 (bifunctional aliphatic urethane acrylate) and 10 to 40 wt% of PN-MF2923 (bifunctional aliphatic urethane acrylate).

[0043] In an embodiment of the present invention, when a mixed oligomer containing 90 wt% of PN-MF5023 (bifunctional aliphatic urethane acrylate) and 10 wt% of PN-MF2923 (bifunctional aliphatic urethane acrylate) is used, the breaking point is 60±5 mm, the elongation is 550±50%, and the recovery speed is 30 seconds or less.

[0044] In the high-elasticity modulus film coating liquid of the first embodiment and the second embodiment of the present invention, a photopolymerizable monomer is used as a reactive diluent of an oligomer to provide workability to a resin mixture, and is polymerized by irradiation with a UV low-pressure mercury lamp or metal lamp to perform the role of a crosslinking agent between polymers. If it satisfies the following requirements: 1) it must have low viscosity and good physical properties, 2) it must have high reactivity (in the order of acrylate > ethacrylate > vinyl), 3) it must be odorless and non-toxic, 4) it must be able to be cured well in the air, 5) it must have good compatibility with oligomers and photoinitiators, and 6) it must have low volatility, it can be used.

[0045] Additionally, for applications requiring rapid curing or curing of surfaces in contact with air, acrylic monomers are preferred. Generally, multifunctional acrylates exhibit faster curing than monofunctional acrylates. Furthermore, ether-type monomers exhibit rapid reactivity because they contain active hydrogens.

[0046] In addition, curing on the surface is inhibited by polymerization by oxygen in the air. To reduce this polymerization inhibition effect, it is desirable to use a monomer having a reactive group such as an alkyl group, an unsaturated higher fatty acid group, a tetrahydrofurfulyl group, or a benzoyl ether group.

[0047] The type of monomer used in the embodiment of the present invention may include at least one selected from the group consisting of DMAA (N,N-dimethylacrylamide), NVP (N-vinyl pyrrolidone), NVC (N-vinyl caprolactam), ACMO (4-acryloylmorpholine), HDDA (1,6-hexanediol diacrylate), HEA (2-hydroxyethyl acrylate), and HPA (Hydroxypropyl acrylate), which are advantageous for improving curing.

[0048] In addition, as a monomer advantageous for improving elongation, at least one selected from the group consisting of PHEA (2-phenoxyethyl acrylate), PEGDA (poly(ethylene glycol) diacrylate), IBOA (isobornyl olefin acid ester), and THFA (Tetrahydrofurfuryl acrylate) is used.

[0049] The embodiments of the present invention can affect the curing reactivity or elongation improvement of the entire film coating solution depending on various monomers, and when a monomer is used alone, it results in a property biased toward one side, so it is preferable to use a mixed monomer.

[0050] Therefore, the monomer used in the coating solution according to the embodiment of the present invention is preferably a mixed monomer that has a good curing speed and can also affect elongation improvement, and more preferably, 10 to 90 wt% of a curing-improving monomer and 10 to 90 wt% of a elongation-improving monomer are mixed, and in the embodiment, a mixed monomer composed of 35 to 65 wt% of NVP (N-vinyl-2-pyrrolidone) having a weight average molecular weight of 111.14 g / mol, 30 to 55 wt% of THFA (Tetrahydrofurfuryl acrylate) having a weight average molecular weight of 156.18 g / mol, and 5 to 10 wt% of HEA (2-hydroxyethyl acrylate) is used.

[0051] In addition, in the high-elasticity modulus film coating liquid of the first embodiment and the second embodiment of the present invention, a photoinitiator is added to a UV resin (here, all paints, coatings, inks, coatings, adhesives, sealants, etc. that use ultraviolet rays are collectively referred to as such) and refers to a substance that absorbs energy from an ultraviolet lamp to initiate a polymerization reaction. Depending on the type of resin, the photoinitiator is contained in an amount of 1 to 10% and plays a role in initiating photopolymerization by applying energy necessary for photopolymerization of monomers, oligomers, and free radicals, thereby changing these substances into polymer materials after curing.

[0052] In the present invention, I-184 (1-Hydro-cyclohexyl-phenyl-ketone), I-1173 (2-Hydroxy-2-methyl-1-phenyl-1-propanone), TPO (Diphenyl(2, 4, 6-trimethylbenzoyl)-phosphine oxide) and I-819 (Phosphine oxide, phenyl bis (2, 4, 6-trimethylbenzoyl)) are used as photoinitiators.

[0053] In an embodiment of the present invention, an initiator in the form of a mixed initiator is used, which is composed of 80 to 90 wt% of I-1173 (2-Hydroxy-2-methyl-1-phenyl-1-propanone) and 10 to 20 wt% of I-184 (1-Hydro-cyclohexyl-phenyl-ketone).

[0054] The high elongation modulus film coating solution of the present invention is provided in a liquid form by containing the above composition in an organic solvent. At this time, the organic solvent may be an inert organic solvent that is commonly used, for example, alcohols such as methoxy propanol and isopropyl alcohol, ketones such as acetone, acetates such as ethyl acetate, or aromatic compounds such as toluene, which may be used alone or in combination. Preferably, alcohols such as methoxy propanol or isopropyl alcohol may be used as a single solvent.

[0055] In addition, the present invention provides a method for manufacturing a high-elasticity film, which comprises pouring the high-elasticity modulus film coating liquid in a I shape between two sheets of release film, using a laminating machine to stamp out a liquid coating film of 50 to 100 μm in thickness, and curing the stamped sample after irradiating it with light.

[0056] The above manufacturing method can be manufactured on the current EPU manufacturing line.

[0057] The above light irradiation can be cured at 500 mJ / cm2 using a UV low-pressure mercury lamp or metal lamp to provide an elastic, elongated film.

[0058] Furthermore, the present invention provides an EPU (Elastic Poly Urethane) film having elasticity and high elongation manufactured by the above manufacturing method, which is a high elongation film improved to a level that can be confirmed almost immediately.

[0059] Therefore, the high-elasticity film of the present invention can be used as a replacement for PPF films used to protect vehicle bodies, or as a film for electronic devices such as tablet PCs and laptops, or for OLED packaging. In particular, the high-elasticity film of the present invention can be provided as a customized product tailored to the customer's desired size, thickness, characteristics, and high transmittance.

[0060]

[0061] Hereinafter, the present invention will be described in more detail through examples. These examples are intended to explain the present invention more specifically, and the scope of the present invention is not limited to these examples.

[0062]

[0063] <Examples 1-2>

[0064] A coating solution containing an oligomer (PN-MF2923: aliphatic urethane acrylate (bifunctional)), a monomer, and an initiator was prepared, poured in a I shape between two sheets of release film, and a liquid coating film of 50 to 100 μm was stamped using a laminating machine. The stamped sample was cured after irradiating the sample with light to produce a film.

[0065] The above-mentioned punched sample was cut into width × length × thickness (10 mm × 10 mm × 100 um), one side was fixed on a measuring centimeter, and the opposite side was pulled at a speed of 300 mm / min to check the length (mm) when the film was broken (ruptured).

[0066] Once the breaking point was confirmed, the measurement value was increased to -0.2 mm and the time (sec) for the opposite fixed part to return to normal was checked.

[0067] When the original altar size of 10 mm returns to 90%, the measurement time is recorded. However, if it does not return, the length value returned after leaving it for 1 minute is recorded to record the physical properties.

[0068] The evaluation of the influence of the initiator on the properties of the elongation film according to the experimental results is shown in Table 1.

[0069]

[0070] From the results in Table 1 above, depending on the monomer and oligomer reactivity, an initiator selected from among 1-hydro-cyclohexyl-phenyl-ketone (I-184), phosphine oxide, phenyl bis (2, 4, 6-trimethylbenzoyl) (I-819), 2-hydroxy-2-methyl-1-phenyl-1-propanone (I-1173) and diphenyl (2, 4, 6-trimethylbenzoyl)-phosphine oxide (TPO) can be used.

[0071] Table 2 below shows the evaluation of the properties of the elongation film according to the monomer.

[0072]

[0073] From the above Table 2, depending on the selection of monomer, the results of the influence on the curability and elongation of the elongation film were confirmed, and it was confirmed that the influence on the curing reactivity was greater than the influence on the elongation. However, when a monomer is used alone, it may have properties that are biased to one side, so it is desirable to contain it as a mixed composition for a balanced result of elongation and curability, and at this time, it was confirmed that DMAA, NVP, NVC, ACMO, HDDA, HEA, and HPA are desirable for improving curability among the monomers, and PHEA, PEGDA, IBOA, and THFA are desirable for improving elongation.

[0074] Table 3 shows the evaluation of the physical properties of the elongation film according to the oligomer.

[0075]

[0076] From the results in Table 3 above, it was confirmed that the elongation and elastic properties significantly differed depending on the selection of oligomer. In addition, the film was superior in terms of elongation and curability compared to films using commonly used urethane acrylic oligomers.

[0077] From the above results, PN-MF5023 and PN-MF2923 were selected as the best aliphatic urethane acrylates, and the properties of films manufactured by combining these mixed oligomers are shown in Tables 4 and 5 below. Table 4 shows the property influence evaluation (1) of the elongation film according to the content control.

[0078]

[0079] As shown in the results of Table 4 above, it was confirmed that films manufactured according to the content of mixed oligomers consisting of 90 wt% PN-MF2923 and 10 wt% PN-MF5023 could achieve properties of immediate restoration and elongation of 300%.

[0080] And Table 5 shows the evaluation of the physical properties of the elongation film according to the content control (2).

[0081]

[0082] From the results in Table 5 above, the mixed oligomer is composed of 90 wt% of PN-MF5023 and 10 wt% of PN-MF2923, and in the case of films manufactured according to the content, the elongation of 600% was achieved while satisfying the requirement of a restoration speed of 30 seconds or less to the original state.

[0083]

[0084] Although the present invention has been described in detail above only with respect to the described specific examples, it will be apparent to those skilled in the art that various modifications and variations are possible within the technical scope of the present invention, and it is natural that such modifications and variations fall within the scope of the appended claims.

Claims

1. Contains 40 to 69 wt% of acrylic oligomer, 30 to 50 wt% of photocurable mixed monomer, and 1 to 10 wt% of photoinitiator. The above photocurable mixed monomer is composed of 10 to 90 wt% of a curing-enhancing monomer and 10 to 90 wt% of an elongation-enhancing monomer, The above curing-enhancing monomer is composed of at least one selected from the group consisting of DMAA (N,N-dimethylacrylamide), NVP (N-vinyl pyrrolidone), NVC (N-vinyl caprolactam), ACMO (4-acryloylmorpholine), HDDA (1,6-hexanediol diacrylate), HEA (2-hydroxyethyl acrylate), and HPA (Hydroxypropyl acrylate). The above-mentioned elongation-improving monomer is composed of at least one selected from the group consisting of PHEA (2-phenoxyethyl acrylate), PEGDA (poly(ethylene glycol) diacrylate), IBOA (isobornyl olefin acid ester), and THFA (Tetrahydrofurfuryl acrylate). A high elongation modulus film coating solution that provides a film having a breaking point of 35±5 mm, an elongation of 280±80%, and a recovery speed of 1 to 2 for a tensile force of 280 to 320 mm / min.

2. Contains 40 to 50 wt% of acrylic oligomer, 30 to 40 wt% of photocurable mixed monomer, and 1 to 10 wt% of photoinitiator. The above photocurable mixed monomer is composed of 10 to 90 wt% of a curing-enhancing monomer and 10 to 90 wt% of an elongation-enhancing monomer, The above curing-enhancing monomer is composed of at least one selected from the group consisting of DMAA (N,N-dimethylacrylamide), NVP (N-vinyl pyrrolidone), NVC (N-vinyl caprolactam), ACMO (4-acryloylmorpholine), HDDA (1,6-hexanediol diacrylate), HEA (2-hydroxyethyl acrylate), and HPA (Hydroxypropyl acrylate). The above-mentioned elongation-improving monomer is composed of at least one selected from the group consisting of PHEA (2-phenoxyethyl acrylate), PEGDA (poly(ethylene glycol) diacrylate), IBOA (isobornyl olefin acid ester), and THFA (Tetrahydrofurfuryl acrylate). A high elongation modulus film coating solution that provides a film having a breaking point of 60±5mm, an elongation of 550±50%, and a recovery speed of 30 seconds or less for a tensile force of 280 to 320 mm / min.

3. In claim 1 or 2, A high-elasticity modulus film coating solution characterized in that the above acrylic oligomer is composed of aliphatic urethane acrylate having a weight average molecular weight of 15,000 to 25,000.

4. In claim 1 or 2, A high elongation modulus film coating solution characterized in that the acrylic oligomer comprises 60 to 90 wt% of aliphatic urethane acrylate having a viscosity of 45,000 to 60,000 cps at 60°C and 10 to 40 wt% of aliphatic urethane acrylate having a viscosity of 50,000 to 100,000 cps at 60°C.

5. In claim 1 or 2, A high elongation modulus film coating solution characterized in that the photocurable mixed monomer is composed of 35 to 65 wt% of NVP (N-vinyl-2-pyrrolidone), 30 to 55 wt% of THFA (Tetrahydrofurfuryl acrylate), and 5 to 10 wt% of HEA (2-hydroxyethyl acrylate).

6. In claim 1 or 2, A high elongation modulus film coating solution characterized in that the above high elongation modulus film coating solution further contains a mixed initiator, and the mixed initiator is composed of 80 to 90 wt% of 2-Hydroxy-2-methyl-1-phenyl-1-propanone and 10 to 20 wt% of 1-Hydro-cyclohexyl-phenyl-ketone.

7. A method for manufacturing a high-elasticity film, characterized by comprising the steps of: pouring a high-elasticity modulus film coating solution manufactured through any one of claims 1 to 6 between two sheets of release film in the shape of the letter I, then using a laminating machine to stamp out a liquid coating film of 50 to 100 μm in thickness to manufacture a sample, and then curing the manufactured sample by irradiating it with light.

Citation Information

Patent Citations

  • Active energy ray-curable resin composition, cured film of the composition, and laminate having the cured film

    JP6123428B2

  • High-elongation ultraviolet-curable coating agent composition

    KR1020140074505A

  • Active energy ray-curable adhesive composition and method for producing laminate

    KR1020150079692A

  • UV-curable coating composition of high-elongation and dual-curable, and the coating method using it

    KR1020160076045A

  • Motorcycle and method for reducing exhaust gas

    KR1020230139463A