Cathode active material for lithium secondary battery, method for preparing same, and lithium secondary battery comprising same

The development of a nickel-containing layered lithium transition metal oxide with specific particle size and composition addresses the limitations of small-diameter single particle cathode materials, enhancing energy density and electrochemical performance in lithium-ion batteries.

WO2024205105A1PCT designated stage expired Publication Date: 2024-10-03POSCO HLDG INC +1

Patent Information

Application Number
PCT/KR2024/003436
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium-ion batteries face challenges with small-diameter single particle cathode materials, which have low rolling density and limited electrode energy density, while increasing particle size compromises lithium ion diffusion and electrochemical characteristics.

Method used

A nickel-containing layered lithium transition metal oxide with an average particle diameter of 5 to 8 μm, composed of single particles and quasi-single particles, is developed, incorporating grain growth promoting elements like Zr, Al, or B, and a coating layer, to enhance mechanical strength and electrochemical performance.

Benefits of technology

The solution improves electrode energy density, charge/discharge efficiency, and battery lifespan by optimizing particle size and structure, while maintaining high capacity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024003436_03102024_PF_FP_ABST
    Figure KR2024003436_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a cathode active material for a lithium secondary battery, as a nickel-containing layered lithium transition metal oxide, comprising: single particles having an average particle diameter (D50) of 5-8 μm and composed of one primary particle, and spherical quasi-single particles composed of a plurality of primary particles, the cathode active material satisfying equation 1 below. [Equation 1] 1.2 μm ≤ D50 - D50p ≤ 1.8 μm. In equation 1, D50 is the average particle diameter (D50) of the cathode active material before nine tons of pressure are applied, and D50p is the average particle diameter (D50) of the cathode active material after nine tons of pressure are applied.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material for lithium secondary batteries, method for producing the same, and lithium secondary batteries comprising the same

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same, and more specifically, to a positive electrode active material for a single-particle lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same.

[0002]

[0003] As electric vehicles expand to achieve carbon neutrality and demand for energy storage devices such as ESS for renewable energy sources surges, lithium-ion batteries are becoming an irreplaceable, core energy storage device. In particular, the characteristics of lithium-ion batteries are significantly influenced by their cathode materials, making cathode material research a significant part of lithium-ion battery research.

[0004] Among cathode materials, active research is being conducted on NCM cathode materials, which are nickel-based cathode active materials with a layered structure and doped with cobalt and manganese. Previously, secondary particle active materials formed by agglomeration of primary particles have been extensively studied. However, these secondary particle active materials have large surface areas and low particle strength, leading to problems such as cracking and reduced lifespan due to gas generation. Therefore, development is underway on single-particle cathode materials composed of a single primary particle, primarily produced for small-particle cathode materials with an average particle diameter of approximately 3 to 5 μm in bimodal cathode materials.

[0005] The above-mentioned small-diameter single particles possess excellent mechanical particle strength characteristics, resulting in excellent service life and stability. However, the small particle size results in a low rolling density, which limits the ability to increase electrode energy density.

[0006] To address this issue, attempts have been made to increase electrode energy density by increasing the particle size of single particles. However, indiscriminately increasing the particle size of a single particle leads to a longer lithium ion migration path, which degrades electrochemical characteristics (capacity, charge / discharge efficiency, and output characteristics) related to lithium diffusion.

[0007]

[0008] One object of the present invention is to provide a single-particle series positive electrode active material for a lithium secondary battery, which has excellent rolling density to improve electrode energy density, good capacity and charge / discharge efficiency characteristics, and excellent strength to improve battery life characteristics, a method for producing the same, and a lithium secondary battery including the same.

[0009]

[0010] One embodiment of the present invention provides a positive electrode active material for a lithium secondary battery, which is a nickel-containing layered lithium transition metal oxide, having an average particle diameter (D50) of 5 to 8 μm, including a single particle composed of one primary particle and a spherical quasi-single particle composed of multiple primary particles, and satisfying the following formula 1.

[0011] [Formula 1]

[0012] 1.2 μm ≤ D50 - D50 p ≤ 1.8 μm

[0013] In the above equation 1, D50 is the average particle diameter (D50) of the positive electrode active material before applying a pressure of 9 tons, and D50 p is the average particle diameter (D50) of the positive electrode active material after applying a pressure of 9 tons.

[0014] The average number of primary particles in the above quasi-single particle may be 8 or less.

[0015] The average aspect ratio of the primary particles in the above quasi-single particles may be 1.1 or more.

[0016] The above-mentioned positive electrode active material for a lithium secondary battery may have a compression density of 3.61 g / cc or more after applying a pressure of 9 tons.

[0017] The above-mentioned positive electrode active material for lithium secondary batteries has a BET specific surface area of ​​0.55 m 2 / g can be less.

[0018] The above lithium transition metal oxide may further include a grain growth promoting element such as Zr, Al, B or a combination thereof.

[0019] The content of the above-mentioned growth promoting element may be 0.1 to 1 mol% based on the total mole number of transition metals.

[0020] The above positive electrode active material may further include a coating layer including Co, Al or a combination thereof on the lithium transition metal oxide.

[0021] The above lithium transition metal oxide can be represented by the following chemical formula 1.

[0022] [Chemical Formula 1]

[0023] Li a [Ni x Co y Mn z M1 w1 M2 w2 ]O2

[0024] In the above chemical formula 1, 0.8≤a≤1.2, 0.60≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0≤w1≤0.01, 0≤w2≤0.2, x+y+z+w1+w2=1, M1 is Zr, Al, B or a combination thereof, and M2 is Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof.

[0025]

[0026] Another embodiment of the present invention provides a method for manufacturing a cathode active material for a lithium secondary battery, comprising the steps of: preparing a nickel-containing transition metal precursor; forming a mixture including the transition metal precursor and a lithium raw material and then firing the mixture to form a lithium transition metal oxide having a larger number of primary particles; post-firing the lithium transition metal oxide; and pulverizing the post-firing lithium transition metal oxide to form a lithium transition metal oxide including a single particle composed of one primary particle and a spherical quasi-single particle composed of a plurality of primary particles, wherein the main-firing temperature is higher than the post-firing temperature, and the main-firing time is shorter than the post-firing time.

[0027] The transition metal precursor prepared in the step of preparing the above transition metal precursor or the lithium transition metal oxide formed in the step of forming the lithium transition metal oxide in which the number of primary particles has grown by the above main firing may further include a grain growth promoting element such as Zr, Al, B or a combination thereof.

[0028] The content of the above-mentioned growth promoting element may be 0.1 to 1 mol% based on the total mole number of transition metals in the transition metal precursor or the lithium transition metal oxide.

[0029]

[0030] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.

[0031] Another embodiment of the present invention provides a lithium secondary battery including the positive electrode.

[0032]

[0033] A cathode active material for a lithium secondary battery according to one embodiment of the present invention has an average particle diameter in a range larger than that of conventional small-diameter single particles, thereby improving electrode energy density, and includes quasi-single particles composed of multiple primary particles in addition to single particles composed of one primary particle, thereby satisfying Equation 1 described below, thereby evenly improving the capacity, charge / discharge efficiency, and life characteristics of the battery.

[0034]

[0035] Figure 1 is a SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Example 1.

[0036] Figure 2 is a SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Example 2.

[0037] Figure 3 is a SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Example 3.

[0038] Figure 4 is a SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Example 4.

[0039] Figure 5 is an SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Comparative Example 1.

[0040] Figure 6 is an SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Comparative Example 2.

[0041] Figure 7 is an SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Comparative Example 3.

[0042] Figure 8 is an SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Comparative Example 4.

[0043] Figure 9 is an SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Comparative Example 5.

[0044] Figure 10 is an SEM image of a positive electrode active material for a lithium secondary battery manufactured according to Comparative Example 6.

[0045]

[0046] The terms first, second, and third, etc., are used to describe, but are not limited to, various parts, components, regions, layers, and / or sections. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.

[0047] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.

[0048] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.

[0049] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.

[0050] Also, unless otherwise stated, % means weight%, and 1 ppm is 0.0001 weight%.

[0051] In this specification, the term "combination(s) thereof" described in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including any one or more selected from the group consisting of said components.

[0052] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0053]

[0054] 1. Positive active material

[0055] One embodiment of the present invention provides a positive electrode active material for a lithium secondary battery, which is a nickel-containing layered lithium transition metal oxide, having an average particle diameter (D50) of 5 to 8 μm, including a single particle composed of one primary particle and a spherical quasi-single particle composed of multiple primary particles, and satisfying the following formula 1.

[0056] [Formula 1]

[0057] 1.2 μm ≤ D50 - D50 p ≤ 1.8 μm

[0058] In the above equation 1, D50 is the average particle diameter (D50) of the positive electrode active material before applying a pressure of 9 tons, and D50 p is the average particle diameter (D50) of the positive electrode active material after applying a pressure of 9 tons.

[0059]

[0060] A cathode active material for a lithium secondary battery according to one embodiment of the present invention is composed of single-particle series particles.

[0061] In this specification, the term “single particle” is used to distinguish it from the secondary particle type positive electrode active material particle formed by the agglomeration of tens to hundreds of primary particles that have been commonly used in the past, and is a concept that includes a single particle composed of one primary particle and an aggregate particle of 30 or fewer primary particles. The “secondary particle” refers to an aggregate, i.e., a secondary structure, formed by the physical or chemical bonding between primary particles without an intentional agglomeration or assembly process for the primary particles.

[0062] The above “primary particle” refers to the smallest particle unit that can be distinguished as a single lump when observing the cross-section of the positive electrode active material through a scanning electron microscope (SEM), and may be composed of a single crystal grain or multiple crystal grains.

[0063] Since the cathode active material for a lithium secondary battery according to one embodiment of the present invention is composed of single-particle series particles, the particle strength is increased, which can suppress particle breakage during rolling, and the occurrence of cracks between primary particles during repeated charging and discharging can be prevented, and the specific surface area is small, which can reduce the amount of gas generated due to side reactions with the electrolyte.

[0064]

[0065] The positive electrode active material for a lithium secondary battery according to one embodiment of the present invention may have an average particle diameter (D50) of 5 to 8 μm, and more specifically, 5.2 to 8 μm, 5.5 to 8 μm, or 6 to 8 μm.

[0066] In this specification, the average particle diameter (D50) can be defined as the particle diameter corresponding to 50% of the volume accumulation amount in the particle diameter distribution curve. The average particle diameter (D50) can be measured using, for example, the laser diffraction method. The laser diffraction method can generally measure particle diameters from the submicron range to several millimeters, and can obtain results with high reproducibility and high resolution.

[0067] When the average particle size of the positive electrode active material is sufficiently large, as in the above range, the tap density can be further improved compared to conventional small-diameter single particles, and as a result, the electrode energy density can be significantly improved. However, if the average particle size of the positive electrode active material is excessively large, the lithium ion migration path can become longer, which can deteriorate electrochemical characteristics such as capacity and output. Therefore, the upper limit is set as above.

[0068]

[0069] However, if the average particle diameter (D50) is increased to the above range using only a single particle composed of one primary particle, there is a problem in that the movement path of lithium ions within the particle becomes longer, resulting in a decrease in electrochemical characteristics such as capacity and charge / discharge efficiency.

[0070] Accordingly, a cathode active material for a lithium secondary battery according to one embodiment of the present invention includes both a single particle composed of one primary particle and a spherical quasi-single particle composed of multiple primary particles. In the present specification, “single particle” means a single particle composed of one primary particle, and “quasi-single particle” means a single particle composed of multiple primary particles. Since the cathode active material includes some quasi-single particles in addition to single particles, the deterioration of the electrochemical properties mentioned above can be minimized, and the rolling density can be further maximized. In the present specification, the spherical shape does not necessarily have to be a sphere, and is a concept including a pseudo-sphere.

[0071]

[0072] In addition, the positive electrode active material for a lithium secondary battery according to one embodiment of the present invention satisfies the following equation 1.

[0073] [Formula 1]

[0074] 1.2 μm ≤ D50 - D50 p ≤ 1.8 μm

[0075] In the above equation 1, D50 is the average particle diameter (D50) of the positive electrode active material before applying a pressure of 9 tons, and D50 p is the average particle diameter (D50) of the positive electrode active material after applying a pressure of 9 tons.

[0076] If the Equation 1 value of the positive electrode active material is too small, the particle strength may be excellent, but the capacity and charge / discharge efficiency characteristics may be poor. If the Equation 1 value of the positive electrode active material is too large, the particle strength may be poor, resulting in poor cycle life characteristics.

[0077] At this time, the average number of primary particles in the quasi-single particle composed of the plurality of primary particles may be 8 or less, and more specifically, may be 2 to 8 or 3 to 8.

[0078] In this specification, the “average number of primary particles in a quasi-single particle” can be obtained by taking 2D images of 25 μm × 20 μm observed in a SEM (scanning electron microscope) image at 5,000x magnification at 5 points per sample, and then deriving the arithmetic mean of the number of primary particles observed with the naked eye for each of at least 5 random single particles per point. It should be noted that in this specification, the “average number of primary particles in a quasi-single particle” refers to the average number of primary particles observed in a SEM image of a 2D image, not the average number of primary particles contained in a single particle in an actual three-dimensional reality.

[0079] If the average number of primary particles in a quasi-single particle is too large, the voids formed between the primary particles will also increase proportionally, which may cause particle breakage due to repeated shrinkage and expansion of primary particles with different orientations during the rolling process or charge / discharge process. In other words, the particle strength may be degraded, and as a result, the life characteristics may deteriorate. However, if the average number of primary particles in a quasi-single particle is too small, it will become similar to a single particle, which may lengthen the lithium ion diffusion distance within the particle, resulting in deterioration of the capacity and charge / discharge efficiency characteristics.

[0080] Additionally, the average aspect ratio of the primary particles in the quasi-single particles may be 1.1 or more, and more specifically, 1.1 to 2.5.

[0081] In this specification, “aspect ratio” may be defined as the ratio of the length of the longest side to the length of the shortest side of a particle, and “average aspect ratio” may be defined as the arithmetic mean of the aspect ratios derived by measuring the lengths of the shortest and longest sides using software during the SEM image measurement process for particle shape analysis for at least 10 particles. The reason why the average aspect ratio of the primary particles is 1.1 or more and the shape of the primary particles is closer to a rod shape than a perfect sphere is because the surface energy is different depending on the crystal plane and the crystal tends to grow in the direction of the thermodynamically stable 003 plane. The larger the aspect ratio, the advantage of increasing particle strength is that, however, if the average aspect ratio of the primary particles is too large, there may be a problem of reduced capacity and efficiency due to an increase in the lithium diffusion distance.

[0082] The value of the above formula 1 can be more easily implemented in the target range according to the present invention when the positive electrode active material of the single particle series includes single particles and quasi-single particles, and the average number of primary particles in the quasi-single particles and the average aspect ratio of the primary particles in the quasi-single particles are appropriately controlled.

[0083]

[0084] The above-mentioned positive electrode active material for a lithium secondary battery may have a compression density of 3.61 g / cc or more after applying 9 tons of pressure. The above-mentioned physical property corresponds to the rolling density of the active material during electrode manufacturing, and thus, having such a high compression density can improve the electrode energy density.

[0085] In this specification, the compression density after applying 9 tons of pressure to the active material can be measured by loading 3g of the active material sample into a pellet with a diameter of 13mm, applying 9 tons of pressure using a hydraulic press from Caver, and then measuring the change in height of the pellet before and after applying the pressure. The specific calculation formula is as follows.

[0086]

[0087] [Calculation Formula 1]

[0088] Density after applying 9 tons of pressure = Weight of active material sample (3g) / (Φ*(1.3cm / 2) 2 *(Height change before and after pressure application)

[0089]

[0090] In the above calculation formula 1, Φ represents pi.

[0091]

[0092] The above-mentioned positive electrode active material for lithium secondary batteries has a BET specific surface area of ​​0.55 m 2 / g or less. When the specific surface area of ​​the active material is sufficiently small, the side reaction between the active material and the electrolyte is reduced, which can improve the battery life characteristics.

[0093] In this specification, the specific surface area of ​​the active material can be measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020) for the active material powder.

[0094]

[0095] Meanwhile, the lithium transition metal oxide may contain nickel in an amount of 60 mol% or more, and more specifically, 70, 80, or 90 mol% or more, based on the total moles of transition metals. With such a high nickel content, high-capacity characteristics can be realized.

[0096]

[0097] The lithium transition metal oxide may further include a grain growth promoting element such as Zr, Al, B, or a combination thereof. By further including a grain growth promoting element in the lithium transition metal oxide, the sintering temperature for forming the lithium transition metal oxide can be lowered, thereby preventing crystal defects such as an increase in the cation mixing ratio due to high-temperature sintering, and the average particle diameter of single particles can be efficiently increased during the sintering process.

[0098] The content of the above grain growth promoting element may be 0.1 to 1 mol% based on the total mole number of transition metals, and more specifically, 0.3 to 1 mol%. More specifically, the content of Zr may be 0.1 to 0.3 mol% based on the total mole number of transition metals. In addition, the content of Al may be 0.3 to 1.0 mol% based on the total mole number of transition metals. In addition, the content of B may be 0.1 to 0.8 mol%.

[0099] When the content of the growth-promoting element satisfies the above range, the effect of adding the growth-promoting element described above and the effect of preventing deterioration of electrochemical properties due to excessive addition can be equally implemented.

[0100]

[0101] The above-described positive electrode active material may further include a coating layer comprising Co, Al, or a combination thereof on the lithium transition metal oxide. By further including a coating layer having the above-described composition, the positive electrode active material can suppress side reactions with the electrolyte, improve the structural stability of the active material, and further improve battery life characteristics.

[0102]

[0103] The above lithium transition metal oxide can be represented by the following chemical formula 1.

[0104] [Chemical Formula 1]

[0105] Li a [Ni x Co y Mn z M1 w1 M2 w2 ]O2

[0106] In the above chemical formula 1, 0.8≤a≤1.2, 0.60≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0≤w1≤0.01, 0≤w2≤0.2, x+y+z+w1+w2=1, M1 is Zr, Al, B or a combination thereof, and M2 is Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof.

[0107] In the lithium transition metal oxide of the above chemical formula 1, lithium may be included in a content corresponding to a, that is, 0.8≤a≤1.2. If a is too small, the capacity may be reduced, and if a is too large, the strength of the sintered positive electrode active material may be increased, making pulverization difficult, and the amount of gas generated may increase due to an increase in lithium byproducts. Considering the effect of improving the capacity characteristics of the positive electrode active material according to the control of the lithium content and the sinterability balance during the production of the active material, the lithium may be included in a content of 0.9≤a≤1.1 more preferably.

[0108] In the lithium transition metal oxide of the above chemical formula 1, nickel may be included in an amount corresponding to x, that is, 0.6≤x<1, 0.6≤x≤0.97, 0.80≤x≤0.97, or 0.90≤x≤0.97. If the nickel amount is too low, it may be difficult to achieve high capacity of the battery, and if the nickel amount is too high, the battery life and safety may be reduced due to a decrease in the structural stability of the active material.

[0109] In the lithium transition metal oxide of the above chemical formula 1, cobalt may be included in an amount corresponding to y, i.e., 0≤y≤0.4, 0≤y≤0.2, or 0≤y≤0.1. If the cobalt amount is too low, it may be difficult to simultaneously achieve sufficient rate characteristics and high powder density of the active material. If the cobalt amount is too high, the overall cost of the raw material may increase and the reversible capacity may decrease.

[0110] In the lithium transition metal oxide of the above chemical formula 1, manganese may be included in a content corresponding to z, i.e., 0≤z≤0.4. If the manganese content is too low, the production cost may increase and the stability of the active material may decrease. If the manganese content is too high, the capacity and output characteristics of the battery may decrease.

[0111] In the lithium transition metal oxide of the above chemical formula 1, M1 may be included in a content corresponding to w1, that is, 0≤w1≤0.01. At this time, M1 is a grain growth promoting element, and is Zr, Al, B, or a combination thereof.

[0112] In the lithium transition metal oxide of the above chemical formula 1, M2 may be included in a content corresponding to w2, that is, 0≤w2≤0.2. At this time, M2 is another doping element, such as Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr, or a combination thereof.

[0113]

[0114] 2. Method for manufacturing positive electrode active material

[0115] Another embodiment of the present invention provides a method for manufacturing a cathode active material for a lithium secondary battery, comprising the steps of: preparing a nickel-containing transition metal precursor; forming a mixture including the transition metal precursor and a lithium raw material and then firing the mixture to form a lithium transition metal oxide having a larger number of primary particles; post-firing the lithium transition metal oxide; and pulverizing the post-firing lithium transition metal oxide to form a lithium transition metal oxide including a single particle composed of one primary particle and a spherical quasi-single particle composed of a plurality of primary particles, wherein the main-firing temperature is higher than the post-firing temperature, and the main-firing time is shorter than the post-firing time.

[0116] Hereinafter, a method for manufacturing a positive electrode active material for a lithium secondary battery according to another embodiment of the present invention will be described step by step.

[0117]

[0118] First, a nickel-containing transition metal precursor is prepared.

[0119] The above transition metal precursor may be a transition metal hydroxide or a transition metal oxide.

[0120] The above transition metal hydroxide may be prepared by a coprecipitation reaction by adding a complexing agent-containing solution and a pH adjusting agent-containing solution to a transition metal-containing solution including, for example, a nickel raw material and optionally, a cobalt raw material or a manganese raw material, as a precursor of a positive electrode active material.

[0121] The above transition metal oxide may be manufactured by calcining a transition metal hydroxide in an oxygen or air atmosphere at a temperature of 250 to 650°C.

[0122] At this time, the average particle diameter (D50) of the transition metal precursor may be 5 μm or more. When the average particle diameter of the transition metal precursor satisfies the above range, a single-particle lithium transition metal oxide having a medium particle diameter as targeted by the present invention can be easily obtained.

[0123] The above nickel raw material is not particularly limited as long as it is used in the art for manufacturing a positive electrode active material precursor. For example, the nickel raw material may be a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, fatty acid nickel salt, nickel halide, or a combination thereof, but is not limited thereto.

[0124] The above cobalt raw material is not particularly limited as long as it is used in the manufacture of a cathode active material precursor in the art. For example, the cobalt raw material may be a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, CoSO 4, It may be, but is not limited to, CoSO4ㆍ7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O or a combination thereof.

[0125] The manganese raw material is not particularly limited as long as it is used in the art for manufacturing a precursor of a cathode active material. For example, the manganese raw material may be a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof, and specifically, may be a manganese salt such as MnSO4, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylic acid salt, manganese citrate, and manganese fatty acid salt, manganese oxide such as Mn2O3, MnO2, and Mn3O4, oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.

[0126] The above transition metal-containing solution may be prepared by adding a nickel raw material and optionally a cobalt raw material or a manganese raw material to a solvent, specifically, water, or a mixture of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water.

[0127] The above complexing agent-containing solution performs the function of forming a complex, and may include, but is not limited to, NH3, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3 or a combination thereof as the complexing agent. Meanwhile, the complexing agent-containing solution may be used in the form of an aqueous solution, and at this time, water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water may be used as the solvent.

[0128] The above pH adjusting agent-containing solution acts as a precipitant or pH adjusting agent, and may include an alkaline compound such as a hydroxide of an alkali metal or alkaline earth metal, such as NaOH, KOH, or Ca(OH)2, a hydrate thereof, or a combination thereof. Meanwhile, the pH adjusting agent-containing solution may also be used in the form of an aqueous solution, and at this time, water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that can be uniformly mixed with water may be used as the solvent. At this time, the pH adjusting agent-containing solution may be added in an amount such that the pH of the reaction solution becomes 11 to 13.

[0129] The above coprecipitation reaction can be performed under an inert atmosphere such as nitrogen or argon, can be performed at a temperature of 30 to 70°C, and can be performed at a pH of 11 to 13.

[0130] Through the above process, nickel-cobalt-manganese (doped element) hydroxide particles are generated and precipitated within the reaction solution. The precipitated precursor particles can be separated, washed, and dried using conventional methods to obtain the precursor. The precursor may be a secondary particle formed by the agglomeration of primary particles.

[0131] At this time, the molar ratio of nickel, cobalt, and manganese in the precursor can be controlled by controlling the concentration of nickel raw material, cobalt raw material, and manganese raw material.

[0132] Meanwhile, the doping element may also be doped during the preparation stage of the positive electrode active material precursor. In this case, the doping raw material may be additionally added to a transition metal-containing solution and a co-precipitation reaction may be performed to dope the precursor with the doping element.

[0133]

[0134] Next, a mixture containing the above transition metal precursor and lithium raw material is formed and then fired to form a lithium transition metal oxide with a grown number of primary particles.

[0135] More specifically, a single particle of lithium transition metal oxide composed of a plurality of primary particles can be formed through the above-described primary particle formation.

[0136] Afterwards, the grown lithium transition metal oxide is post-calcined.

[0137] The method for manufacturing an active material according to one embodiment of the present invention divides the firing into two stages as described above, and at this time, the main firing temperature is higher than the post-firing temperature, and the main firing time is shorter than the post-firing time.

[0138] High-temperature, short-term post-firing allows for the growth of primary particles within a single particle to an appropriate range. Low-temperature, long-term post-firing induces crystal rearrangement, relieving the increased internal stress during high-temperature post-firing and reducing nickel cation mixing.

[0139] More specifically, as a conventional method for manufacturing single particles, a single-stage firing method using high-temperature, long-term firing had problems such as nickel cation mixing and the generation of Rocksalt impurities. On the other hand, a manufacturing method according to one embodiment of the present invention can prevent the above problems through high-temperature, short-term main firing and low-temperature, long-term post-firing, and can induce the final active material to include single particles composed of a single particle and multiple primary particles by appropriately growing the number of primary particles within the single particle.

[0140] At this time, the main firing temperature may be 850 to 900°C, and the main firing time may be 5 to 9 hours. In addition, the post-firing temperature may be 760 to 820°C, and the post-firing time may be 9 to 12 hours. When the main firing temperature and time, and the post-firing temperature and time satisfy the above ranges, the active material composition and properties targeted by the present invention can be more easily achieved.

[0141] The lithium raw material may be lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it can be dissolved in water. Specifically, the lithium raw material may be, but is not limited to, Li2CO3, LiNO3, LiNO2, LiOH, LiOHㆍH2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a combination thereof.

[0142] The above firing can be performed under an oxygen or air atmosphere. When firing under the above atmosphere, the local oxygen partial pressure increases, which can improve the crystallinity of the positive electrode active material.

[0143] Meanwhile, other doping elements can be doped during the lithium transition metal oxide formation stage. In this case, other doping raw materials can be added during the formation of the mixture and then calcined to dope other doping elements into the lithium transition metal oxide.

[0144]

[0145] Meanwhile, the transition metal precursor prepared in the step of preparing the transition metal precursor or the lithium transition metal oxide formed in the step of forming the lithium transition metal oxide in which the number of primary particles has grown by the main firing may further include a grain growth promoting element such as Zr, Al, B or a combination thereof. That is, the grain growth promoting element may be doped in the step of forming the transition metal precursor or may be doped in the step of forming the lithium transition metal oxide as the active material.

[0146] At this time, the content of the grain growth promoting element may be 0.1 to 1 mol% based on the total mole number of transition metals in the transition metal precursor or the lithium transition metal oxide, and more specifically, may be 0.3 to 1 mol%. More specifically, the content of Zr may be 0.1 to 0.3 mol% based on the total mole number of transition metals in the transition metal precursor or the lithium transition metal oxide. In addition, the content of Al may be 0.3 to 1.0 mol% based on the total mole number of transition metals in the transition metal precursor or the lithium transition metal oxide. In addition, the content of B may be 0.1 to 0.8 mol%.

[0147] The technical significance of introducing the pressure growth promoting element and controlling its content as described above is omitted as it is the same as described above.

[0148]

[0149] Next, the post-calcined lithium transition metal oxide is pulverized to form a lithium transition metal oxide including a single particle composed of one primary particle and a spherical quasi-single particle composed of multiple primary particles.

[0150] In this way, a positive electrode active material according to the present invention can be obtained.

[0151]

[0152] Optionally, as needed, after the step of forming a lithium transition metal oxide including a single particle composed of the above-described one primary particle and a spherical single particle composed of a plurality of primary particles, a step of forming a coating layer including Co, Al or a combination thereof may be further included.

[0153] More specifically, a coating layer can be formed by mixing the lithium transition metal oxide of the single particle with a Co raw material, an Al raw material, or a combination thereof, and then heat-treating the mixture. The technical significance of forming the coating layer is as described above, and thus is omitted.

[0154]

[0155] 3. Cathode ray and lithium secondary battery

[0156] Another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the positive electrode active material described above.

[0157] Another embodiment of the present invention provides a lithium secondary battery comprising the positive electrode. More specifically, the lithium secondary battery may include a positive electrode; a negative electrode; a separator; and an electrolyte.

[0158] In addition, the lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0159]

[0160] Specifically, the positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and including the positive electrode active material described above.

[0161] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0162] The above-described positive electrode active material layer may include a binder and / or a conductive material together with the above-described positive electrode active material.

[0163] At this time, the binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one kind alone or a mixture of two or more kinds thereof may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0164] And, the conductive material is used to provide conductivity to the electrode, and in the battery to be constructed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types among these may be used, but the present invention is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.

[0165] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above positive electrode active material is used.

[0166] Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, including the positive electrode active material described above and optionally a binder, a conductive agent, or a solvent, on a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, binder, and conductive agent are as described above.

[0167] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0168] Alternatively, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.

[0169]

[0170] The above negative electrode may include a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0171] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0172] The negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material. As an example, the negative electrode active material layer may be manufactured by applying a composition for forming a negative electrode active material layer comprising the negative electrode active material and optionally a binder and a conductive material onto a negative electrode current collector and drying the composition, or by casting the negative electrode forming composition onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling the film off from the support.

[0173] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples thereof include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, and Al alloy; metallic oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.

[0174] The above binder and conductive material may be the same as those described above for the positive electrode.

[0175]

[0176] The above separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without any particular restrictions. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.

[0177]

[0178] The above electrolyte may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0179] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.

[0180] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.

[0181] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0182] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.

[0183]

[0184] Another embodiment of the present invention provides a battery module including the lithium secondary battery as a unit cell and a battery pack including the same.

[0185] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as power tools; electric vehicles including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or power storage systems.

[0186]

[0187] Hereinafter, embodiments of the present invention will be described in more detail through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.

[0188]

[0189] Example 1

[0190] (1) Manufacturing of positive electrode active material

[0191] (Preparation of transition metal hydroxide) According to the general coprecipitation method, (Ni) with an average particle size (D50) of 7 μm 0.96 Co 0.03 Mn 0.01 )(OH)2 transition metal hydroxide was prepared.

[0192] (Preparation of transition metal oxide) 500 g of the above transition metal hydroxide, ZrO-20.993 g corresponding to 0.15 mol% of Zr and Al(OH)32.096 g corresponding to 0.5 mol% of Al based on 100 mol% of the total transition metal of the transition metal hydroxide as a grain growth accelerator were mixed, and then calcined at 500°C for 4 hours in an air atmosphere, followed by a dehydration reaction to produce a transition metal oxide precursor containing Zr and Al.

[0193] (After calcination), 83.963 g of LiOH·H2O as a lithium raw material was mixed with 150 g of the above transition metal oxide precursor so that the Li / Me molar ratio was 1.02, and then the main calcination was performed at 850°C for 6.7 hours, followed by post-calcination at 790°C for 9.8 hours to manufacture a lithium transition metal oxide.

[0194] (After disintegration), the post-calcined lithium transition metal oxide was disintegrated.

[0195] (Coating) After that, 0.560 g of LiOH·H2O, 22.504 g of Co(OH), and 30.189 g of Al(OH) were mixed with 130 g of the above-mentioned disintegrated lithium transition metal oxide, and heat-treated at 650 to 700°C for 15 hours to produce a positive electrode active material having a coating layer containing 2 mol% of Co and 0.2 mol% of Al formed on the surface.

[0196] (2) Lithium secondary battery manufacturing

[0197] The slurry for manufacturing the electrode plate was mixed with the above-mentioned positive electrode active material: conductive material (carbon black, denka black): binder (PVDF, KF1100) = = 96.5 : 1.5 : 2 wt%, and the viscosity was adjusted so that the solid content was approximately 30% by adding NMP (N-Methyl-2-pyrrolidone). The manufactured slurry was coated on a 15 μm thick Al foil using a doctor blade, and then dried and rolled. The electrode loading amount was 15.0 mg / cm 2 and the rolling density (25 ℃, 20 kN) was 3.6 g / cm 3 It was.

[0198] The electrolyte was 1M LiPF6in EC:DMC:EMC=3:4:3 (vol%), with 3.0 vol% VC added to the total amount of the electrolyte, and a coin cell was manufactured using a PP separator and a lithium negative electrode (200 μm, Honzo metal).

[0199]

[0200] Examples 2 to 4 and Comparative Example 1

[0201] A cathode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the sintering temperature and time of the main sintering and post-sintering were different in the sintering step as shown in Table 1 below.

[0202]

[0203] Comparative Example 2, Comparative Examples 4 to 6

[0204] In the transition metal hydroxide preparation step, a transition metal hydroxide having an average particle diameter (D50) of 4 μm was prepared, and in the sintering step, as shown in Table 1 below, the sintering temperature and time of the main sintering and post-sintering were changed, and the cathode active material and lithium secondary battery were manufactured in the same manner as in Example 1.

[0205]

[0206] Comparative Example 3

[0207] According to the general precipitation method, the average particle size (D50) is 13 μm (Ni 0.96 Co 0.03 Mn 0.01 )(OH)2 transition metal hydroxide was prepared.

[0208] Afterwards, 71.992 g of LiOH·H2O was mixed with 150 g of the above transition metal hydroxide so that the Li / Me molar ratio was 1.06, and then calcined at 750°C for 12 hours, followed by pulverization, washing, and drying to produce a lithium transition metal oxide.

[0209] Afterwards, 130 g of the above lithium transition metal oxide was mixed with 0.371 g of H3BO3, and heat-treated at 250 to 300°C for 6 hours to manufacture a positive electrode active material having a coating layer containing 0.45 mol% of B formed on the surface.

[0210] Thereafter, a lithium secondary battery was manufactured in the same manner as in Example 1.

[0211]

[0212] Table 1 below summarizes the manufacturing methods of examples and comparative examples.

[0213] ClassificationPrecursorAverage particle size (D50, μm)Main firing temperature (℃)Main firing time (h)Post-firing temperature (℃)Post-firing time (h)Example 178506.77909.8Example 278604.97909.8Example 378606.77909.8Example 478608.87909.8Comparative example 178403.87909.8Comparative example 248303.87409.8Comparative example 31375012--Comparative example 478406.78609.8Comparative example 57850127908Comparative example 6787012--

[0214] Experimental Example 1: Observation of SEM images of active materials

[0215] SEM (scanning electron microscope) images of the positive electrode active materials manufactured according to the examples and comparative examples were observed, and these are shown in the order of Examples 1 to 4 and Comparative Examples 1 to 6 in Figures 1 to 7, respectively.

[0216] Referring to FIGS. 1 to 9, it was confirmed that the active materials of Examples 1 to 4 and Comparative Examples 1 to 2 and 4 to 6 were not in the form of aggregates of tens to hundreds of primary particles classified as conventional secondary particle shapes, but rather in the form of single particles. On the other hand, it was confirmed that Comparative Example 3 had the conventionally general secondary particle shape.

[0217] In addition, it was confirmed that in the cases of Examples 1 to 4, both single particles composed of one primary particle and quasi-single particles composed of multiple primary particles were included, with a particle size at the level of an intermediate particle size.

[0218] On the other hand, in the case of Comparative Example 1, it was confirmed that the number of primary particles in the quasi-single particles was significantly greater. In addition, in the case of Comparative Example 2, it was confirmed that the particle size was smaller than that of the examples.

[0219]

[0220] Experimental Example 2: Evaluation of the properties of positive electrode active materials

[0221] The properties of the positive electrode active materials manufactured according to the examples and comparative examples were evaluated, and the results are shown in Table 2 below. The experimental method is as follows.

[0222] (1) Measurement of average particle diameter (D50)

[0223] For the active material powder, the particle size corresponding to 50% of the cumulative volume was measured using the laser diffraction method.

[0224] (2) Evaluation of Equation 1

[0225] [Formula 1] = D50 - D50 p The value expressed as was evaluated.

[0226] In the above equation 1, D50 is the average particle diameter (D50) of the positive electrode active material before applying a pressure of 9 tons, and D50 p is the average particle diameter (D50) of the positive electrode active material after applying a pressure of 9 tons.

[0227] (3) Average number of primary particles in a single particle

[0228] A 2D image of (25 μm) × (20 μm) observed on a SEM (scanning electron microscope) image at 5,000x magnification was taken at 5 points per sample, and the arithmetic mean value of the number of primary particles observed with the naked eye for each of at least 5 random single particles per point was derived.

[0229] (4) Compression density evaluation (9 tons)

[0230] Density was evaluated after applying 9 tons of pressure. Specifically, 3 g of active material sample was loaded onto a pellet with a diameter of 13 mm, and then 9 tons of pressure was applied using a hydraulic press from Caver. The change in height of the pellet before and after applying the pressure was measured, and the specific calculation formula is as follows.

[0231] [Calculation Formula 1]

[0232] Density after applying 9 tons of pressure = Weight of active material sample (3g) / (Φ*(1.3cm / 2) 2 *(Height change before and after pressure application)

[0233] In the above calculation formula 1, Φ represents pi.

[0234] (5) BET surface area evaluation

[0235] The specific surface area was measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020).

[0236] Average particle size (D50, μm) Formula 1 (μm) Average number of primary particles in a single particle Compressed density (9 ton, g / cc) Specific surface area (m 2 / g)Example 17.011.6573.630.344Example 26.181.5263.620.326Example 36.341.2873.630.414Example 46.411.2743.620.523Comparative Example 17.012.0203.600.561Comparative Example 24.132.34-3.500.83Comparative Example 313.643.26> 1003.770.57Comparative Example 46.121.1323.580.372Comparative Example 56.031.1833.590.365Comparative Example 66.241.1223.580.345

[0237] Referring to Table 2, in the case of Examples 1 to 4 in which the precursor particle size, main firing and post-firing temperature and time were appropriately controlled during the production of the active material, it was confirmed that the average particle size of the active material, the value of Equation 1, the average number of primary particles in the quasi-single particle, the compressed density, and the specific surface area were all appropriately obtained within the target range of the present invention. On the other hand, in the case of Comparative Example 1, it was confirmed that the main firing temperature was too low, resulting in too many average primary particles in the single particle. Accordingly, it was confirmed that the value of Equation 1 was too large, resulting in weak strength and too large specific surface area.

[0238] In Comparative Example 2, it was confirmed that the average particle diameter of the obtained active material was too small because the particle diameter of the precursor was too small, and the value of Equation 1 was too large, resulting in weak strength and a too large specific surface area. In addition, it was confirmed that the compression density was also deteriorated because the average particle diameter of the active material was too small.

[0239] In the case of Comparative Example 3, it was confirmed that the value of Equation 1 was too large, so the strength was weak and the specific surface area was large, as it was a secondary particle active material that was commonly used in the past.

[0240] In the case of Comparative Example 4, it was confirmed that the post-firing temperature was higher than the main firing temperature, and thus the value of Equation 1 was too small.

[0241] In the case of Comparative Example 5, it was confirmed that the post-firing time was shorter than the main firing time, and thus the value of Equation 1 was too small.

[0242] In the case of Comparative Example 6, it was confirmed that the value of Equation 1 was too small as it was performed only with a high-temperature, long-term single-stage firing rather than a two-stage firing.

[0243]

[0244] Experimental Example 3: Evaluation of Battery Electrochemical Characteristics

[0245] (1) Initial charge and discharge capacity, initial efficiency evaluation

[0246] After fabricating half-cells of lithium secondary batteries, they were aged at 25°C for 12 hours and then subjected to charge-discharge tests. To evaluate the initial capacity, the cells were charged to a reference capacity of 200 mAh / g at a constant current of 0.1C to 4.25 V, then switched to constant voltage and charged until the end current reached 0.05 C. After a 10-minute rest period after charging, the cells were discharged to 2.5 V at a constant current of 0.1C, using a reference capacity of 200 mAh / g.

[0247] (2) Evaluation of high temperature lifespan (45℃, 50 cycles)

[0248] The high-temperature life retention rate was measured at 45℃, by charging to 4.25 V with a constant current of 0.5 C, then switching to a constant voltage and charging until the end current reached 0.05 C. After a 10-minute rest time after charging, the battery was discharged at a constant current of 1.0 C until the voltage reached 2.5 V. 50 charge / discharge cycles were performed under these charge / discharge conditions, and the capacity retention rate of the 50th cycle was calculated compared to the first cycle.

[0249] (3) Evaluation of high temperature resistance increase rate (45℃, 50 cycles)

[0250] The high temperature resistance increase rate was measured by charging the battery to 4.25 V at a constant current of 0.5 C at 45 °C, then switching to a constant voltage and charging until the end current reached 0.05 C. After a 10-minute rest time after charging, the battery was discharged at a constant current of 1.0 C until the voltage reached 2.5 V. 50 charge / discharge cycles were performed under these charge / discharge conditions, and the resistance increase rate of the 50th cycle compared to the first cycle was calculated.

[0251] Classification Charge capacity (mAh / g, 0.1C) Discharge capacity (mAh / g, 0.1C) Initial efficiency (%) High temperature life maintenance rate (%, 50 cycles) High temperature resistance increase rate (%, 50 cycles) Example 1242.0210.687.093.087.1 Example 2241.2206.685.792.786.2 Example 3240.4206.285.892.990.5 Example 4241.8208.786.393.7570.1 Comparative example 1241.8212.387.891.1100.3 Comparative example 2243.4216.789.091.576.1 Comparative example 3243.9218.489.585.0135.3Comparative Example 4237.7202.085.092.585.3Comparative Example 5239.5204.585.492.790.5Comparative Example 6235.6200.585.191.586.0

[0252] Referring to Table 3, in the case of Examples 1 to 4 where the average particle size of the active material, the value of Equation 1, the average number of primary particles in the quasi-single particles, the specific surface area, etc. were appropriately controlled, it was confirmed that the capacity, initial efficiency, high-temperature lifespan maintenance rate, and high-temperature resistance increase rate of the battery were all excellent. On the other hand, in the case of Comparative Example 1 where the average number of primary particles in the quasi-single particles was too large, it was confirmed that the high-temperature lifespan characteristics were poor as a result of the poor particle strength.

[0253] In the case of Comparative Example 2, which had an average particle size in the small particle size range, the capacity and initial efficiency were good, but it was confirmed that the high-temperature lifespan retention rate was inferior to that of the example. In addition, a deterioration in electrode energy density was predicted.

[0254] In the case of Comparative Example 3 of conventional secondary particles, the capacity and initial efficiency were good, but it was confirmed that the high-temperature life characteristics were significantly reduced as a result of the particle strength being inferior as a secondary particle.

[0255] In the case of Comparative Examples 4 to 6, it was confirmed that the value of Equation 1 was too small, resulting in excellent particle strength but poor battery capacity and initial efficiency.

[0256]

[0257] Although the preferred embodiments of the present invention have been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the patent claims, the detailed description of the invention, and the attached drawings, and it is obvious that this also falls within the scope of the present invention.

[0258] Accordingly, the actual scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A nickel-containing layered lithium transition metal oxide, The average particle diameter (D50) is 5 to 8 μm, It includes a single particle composed of one primary particle and a spherical quasi-single particle composed of multiple primary particles, A cathode active material for a lithium secondary battery satisfying the following equation 1: [Formula 1] 1.2 μm ≤ D50 - D50 p ≤ 1.8 μm In the above equation 1, D50 is the average particle diameter (D50) of the positive electrode active material before applying a pressure of 9 tons, and D50 p is the average particle diameter (D50) of the positive electrode active material after applying a pressure of 9 tons.

2. In paragraph 1, A positive electrode active material for a lithium secondary battery, wherein the average number of primary particles in the above-mentioned quasi-single particles is 8 or less.

3. In paragraph 1, A cathode active material for a lithium secondary battery, wherein the average aspect ratio of the primary particles in the above-mentioned quasi-single particles is 1.1 or more.

4. In paragraph 1, A cathode active material for a lithium secondary battery having a compression density of 3.61 g / cc or more after applying a pressure of 9 tons.

5. In paragraph 1, BET surface area is 0.55 m 2 / g or less cathode active material for lithium secondary batteries.

6. In paragraph 1, The above lithium transition metal oxide is a positive electrode active material for a lithium secondary battery containing nickel in an amount of 60 mol% or more based on the total mole number of transition metals.

7. In paragraph 1, The above lithium transition metal oxide is a cathode active material for a lithium secondary battery, further comprising a grain growth promoting element such as Zr, Al, B or a combination thereof.

8. In paragraph 7, A positive electrode active material for a lithium secondary battery, wherein the content of the above-mentioned growth promoting element is 0.1 to 1 mol% based on the total mole number of transition metals.

9. In paragraph 1, The positive electrode active material for a lithium secondary battery further comprises a coating layer containing Co, Al or a combination thereof on the lithium transition metal oxide.

10. In paragraph 1, The above lithium transition metal oxide is a positive electrode active material for a lithium secondary battery represented by the following chemical formula 1: [Chemical Formula 1] Li a [Ni x Co y Mr z M1 w1 M2 w2 ]O2 In the above chemical formula 1, 0.8≤a≤1.2, 0.60≤x<1, 0≤y≤0.4, 0≤z≤0.4, 0≤w1≤0.01, 0≤w2≤0.2, x+y+z+w1+w2=1, M1 is Zr, Al, B or a combination thereof, and M2 is Y, Mg, Ti, Nb, W, Sc, Si, V, Fe, Y, Mo, Ce, Hf, Ta, La, Sr or a combination thereof.

11. Step of preparing a nickel-containing transition metal precursor; A step of forming a mixture including the above transition metal precursor and lithium raw material and then firing the mixture to form a lithium transition metal oxide with a grown number of primary particles; A step of post-calcining the above lithium transition metal oxide; and A step of forming a lithium transition metal oxide including a single particle composed of one primary particle and a spherical single particle composed of multiple primary particles by crushing the above-mentioned post-calcined lithium transition metal oxide, A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein the main firing temperature is higher than the post-firing temperature and the main firing time is shorter than the post-firing time.

12. In paragraph 11, In the step of preparing the above transition metal precursor, A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein the average particle diameter (D50) of the above transition metal precursor is 5 μm or more.

13. In paragraph 11, A cathode active material for a lithium secondary battery, wherein the transition metal precursor prepared in the step of preparing the transition metal precursor or the lithium transition metal oxide formed in the step of forming the lithium transition metal oxide in which the number of primary particles has grown by the main firing further contains a grain growth promoting element such as Zr, Al, B or a combination thereof.

14. In paragraph 13, A positive electrode active material for a lithium secondary battery, wherein the content of the above-mentioned growth promoting element is 0.1 to 1 mol% based on the total mole number of transition metals in the above-mentioned transition metal precursor or the above-mentioned lithium transition metal oxide.

15. A positive electrode for a lithium secondary battery comprising the positive electrode active material of any one of claims 1 to 10.

16. A lithium secondary battery comprising the positive electrode for a lithium secondary battery of Article 15.

Citation Information

Patent Citations

  • Image signal encoding / decoding method and apparatus using efficient motion vector predictor

    KR1020200085667A

  • Semiconductor device

    KR1020230012669A

  • Screw fixer

    KR1020230092721A

  • Environment learning automation method for optinizing ai image analysis and apparatus therefor

    KR1020230166356A

  • Manufacturing method for hybrid photocatalyst disinfectant and hybrid photocatalytic disinfectant prepared thereby

    KR102176682B1

Cited By

  • Lithium ion secondary battery, positive electrode active material, preparation method and electric equipment

    CN119994146A