Composite positive electrode active material, positive electrode comprising same, and lithium battery
The composite cathode active material, featuring a layered lithium transition metal oxide core and olivine-based second core with a carbon-based shell, addresses side reactions and thermal stability issues, resulting in improved performance and safety for lithium batteries.
Patent Information
- Application Number
- PCT/KR2024/003730
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Existing high-capacity lithium batteries face issues with side reactions and thermal stability due to interactions between composite cathode active materials and electrolytes, limiting their performance and safety.
A composite cathode active material is developed, comprising a first lithium transition metal oxide core with a layered crystal structure and high Ni content, a second lithium transition metal oxide with an olivine-based structure, and a shell of metal oxide and carbon-based material, which reduces surface reactions and enhances thermal stability.
The composite cathode active material improves conductivity and thermal stability, leading to enhanced high-temperature cycle characteristics and thermal safety of lithium batteries.
Smart Images

Figure KR2024003730_03102024_PF_FP_ABST
Abstract
Description
Composite cathode active material, cathode and lithium battery containing the same
[0001] The present invention relates to a composite cathode active material, a cathode including the same, and a lithium battery.
[0002] To accommodate the miniaturization and high-performance of various devices, lithium batteries are becoming increasingly important not only for their miniaturization and weight reduction, but also for their high energy density. In other words, high-capacity lithium batteries are becoming increasingly important.
[0003] Existing high-capacity composite cathode materials have been plagued by side reactions with the electrolyte and poor thermal stability. Composite cathode materials that offer high capacity, suppress side reactions with the electrolyte, and exhibit superior thermal stability are currently being explored.
[0004] One aspect is to provide a novel composite cathode active material with excellent thermal stability while reducing surface side reactions with the electrolyte.
[0005] Another aspect is to provide a positive electrode comprising the above composite positive electrode active material.
[0006] Another aspect is to provide a lithium battery comprising the above positive electrode.
[0007] According to one aspect,
[0008] A first core (1) comprising a first lithium transition metal oxide st core);
[0009] A second core (2) comprising a second lithium transition metal oxide nd core); and
[0010] A shell disposed along the surface of at least one of the first core and the second core;
[0011] The above shell comprises at least one first metal oxide; and a first carbon-based material;
[0012] The first metal oxide is disposed within the first carbon-based material matrix,
[0013] The above first metal oxide has the chemical formula M a Ob (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되며, 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이며,
[0014] The first lithium transition metal oxide and the second lithium transition metal oxide have different particle sizes,
[0015] The first lithium transition metal oxide has a layered crystal structure and a Ni content of 60 mol% or more,
[0016] A composite cathode active material is provided in which a second lithium transition metal oxide has an olivine crystal structure.
[0017] According to another aspect
[0018] anode current collector; and
[0019] A positive electrode is provided, which includes a positive electrode active material layer disposed on one or both sides of the positive electrode current collector and including the composite positive electrode active material and a binder.
[0020] According to another aspect,
[0021] The above positive electrode; the negative electrode; and the electrolyte disposed between the positive electrode and the negative electrode,
[0022] A lithium battery is provided, wherein the first electrode, the second electrode, or a combination thereof is an electrode according to claim 17.
[0023] According to one aspect, the high-temperature cycle characteristics and thermal safety of a lithium battery employing such a composite cathode active material are improved by reducing the side reaction of the composite cathode active material with the electrolyte and improving the conductivity and thermal stability.
[0024] Figure 1 is a cross-sectional schematic diagram of a dry electrode positive electrode active material according to one embodiment.
[0025] Figure 2 is a cross-sectional schematic diagram of a dry electrode positive electrode active material according to one embodiment.
[0026] Figure 3 is a scanning electron microscope image of the surface of the composite positive electrode active material prepared in Example 1.
[0027] Figure 4 is a graph showing the specific capacities of positive electrode active materials according to Examples 1 to 4.
[0028] Figure 5 is a graph showing the cycle characteristics of lithium batteries each employing the positive electrode active materials prepared in Example 1 and Comparative Examples 1-3.
[0029] Figure 6 is a schematic diagram of a lithium battery according to an embodiment.
[0030] Figure 7 is a schematic diagram of a lithium battery according to an embodiment.
[0031] Figure 8 is a schematic diagram of a lithium battery according to an embodiment.
[0032] Various embodiments are illustrated in the accompanying drawings. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. Like reference numerals in the drawings indicate like elements.
[0033] When a component is referred to as being "on" another component, it can be understood that it is either directly on top of the other component or that other components may be intervening between them. Conversely, when a component is referred to as being "directly on" another component, no intervening components are present.
[0034] Although the terms "first," "second," "third," etc. may be used herein to describe various components, elements, regions, layers, and / or zones, these components, elements, regions, layers, and / or zones should not be limited by these terms. These terms are used only to distinguish one component, element, region, layer, or zone from another component, element, region, layer, or zone. Thus, a first component, element, region, layer, or zone described below may be referred to as a second component, element, region, layer, or zone without departing from the teachings of this specification.
[0035] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms including "at least one," unless the content clearly dictates otherwise. "At least one" should not be construed as limiting to the singular. As used herein, the term "and / or" includes any and all combinations of one or more of the listed items. The terms "comprises" and / or "comprising" as used in the detailed description specify the presence of stated features, regions, integers, steps, operations, components, and / or ingredients, but do not preclude the presence or addition of one or more other features, regions, integers, steps, operations, components, ingredients, and / or groups thereof.
[0036] Spatially relative terms such as "below," "under," "bottom," "above," "above," and "top" may be used herein to readily describe the relationship of one component or feature to another. It will be understood that spatially relative terms are intended to encompass different orientations of the device when in use or operation in addition to the orientations depicted in the drawings. For example, if the device in the drawings were turned over, a component described as "below" or "below" another component or feature would then be oriented "above" the other component or feature. Thus, the exemplary term "below" can encompass both the above and below orientations. The device can be arranged in other orientations (rotated 90 degrees or otherwise rotated), and the spatially relative terms used herein can be interpreted accordingly.
[0037] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains. Furthermore, it will be understood that terms defined in commonly used dictionaries should be interpreted to have a meaning consistent with their meaning within the context of the relevant art and the present disclosure, and not in an idealized or overly formal sense.
[0038] Exemplary embodiments are described herein with reference to cross-sectional drawings that are schematic representations of idealized embodiments. As such, variations from the shapes depicted are to be expected, for example, as a result of manufacturing techniques and / or tolerances. Therefore, the embodiments described herein should not be construed as limited to the specific shapes of regions as depicted herein, but should encompass variations in shapes resulting from, for example, manufacturing. For example, regions depicted or described as flat may typically have rough and / or non-linear features. Moreover, angles depicted as sharp may be rounded. Therefore, the regions depicted in the drawings are schematic in nature, and their shapes are not intended to depict the precise shapes of the regions, nor are they intended to limit the scope of the claims.
[0039] "Group" means a group in the periodic table of elements according to the International Union of Pure and Applied Chemistry ("IUPAC") Group 1-18 classification system.
[0040] In this specification, “particle size” refers to the average diameter of spherical particles, and refers to the average major axis length of non-spherical particles. Particle size can be measured using a particle size analyzer (PSA). “Particle size” refers to the average particle size, for example. “Average particle size” refers to the median particle diameter, D50, for example.
[0041] D50 is the size of the particle corresponding to 50% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.
[0042] D90 is the size of the particle corresponding to 90% of the cumulative volume, calculated from the particle side with a smaller particle size in the particle size distribution measured by laser diffraction.
[0043] D10 is the size of the particle corresponding to 10% of the cumulative volume, calculated from the particle side with a small particle size in the particle size distribution measured by laser diffraction.
[0044] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0045] In this disclosure, “alloy” means a mixture of two or more metals.
[0046] In the present disclosure, “electrode active material” means an electrode material capable of undergoing lithiation and delithiation.
[0047] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.
[0048] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0049] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to an electrode active material.
[0050] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from an electrode active material.
[0051] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.
[0052] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.
[0053] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.
[0054] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during a discharge process.
[0055] While specific implementations have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently anticipated or unforeseen may occur to the applicant or those skilled in the art. Accordingly, the appended claims, as filed and as amended, are intended to encompass all such alternatives, modifications, variations, improvements, and substantial equivalents.
[0056]
[0057] Hereinafter, composite cathode active materials, cathodes including the same, and lithium batteries according to exemplary embodiments will be described in more detail.
[0058] [Composite cathode active material]
[0059] A composite cathode active material according to an embodiment of the present invention comprises a first core (1) including a first lithium transition metal oxide st core); a second core (2) comprising a second lithium transition metal oxide nd core); and a shell disposed along the surface of at least one of the first core and the second core; wherein the shell comprises at least one first metal oxide; and a first carbon-based material, wherein the first metal oxide is disposed within the first carbon-based material matrix, and the first metal oxide is represented by the chemical formula M a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되며, 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이며, 상기 제1 리튬전이금속산화물과 상기 제2 리튬전이금속산화물이 서로 다른 입경을 가지며, 제1 리튬전이금속산화물이 층상 결정 구조를 가지며 Ni 함량이 60mol% 이상이며, 제2 리튬전이금속산화물이 올리빈계 결정 구조를 가질 수 있다.
[0060] Referring to FIG. 1, the composite cathode active material (100) includes a first core (10), a second core (20), and a shell (30) that is continuously or discontinuously disposed along the surface of at least one of the first core (10) and the second core (20). The shell (20) may cover all or part of the first core (10) and the second core (20). The shell (30) includes a first metal oxide (31) and a first carbon-based material (32). The composite cathode active material (100) is, for example, a dry composite cathode active material that is not impregnated, dissolved, or dispersed in a process solvent during the cathode manufacturing process, or a wet composite cathode active material that is impregnated, dissolved, or dispersed in a process solvent during the cathode manufacturing process. The composite cathode active material (100) is, for example, a dry composite cathode active material that includes a process solvent or does not come into contact with a process solvent during the cathode manufacturing process, or a wet composite cathode active material that includes a process solvent or comes into contact with a process solvent during the cathode manufacturing process.
[0061] The composite cathode active material (100) may include, for example, a first core (10) / shell (30) and / or a second core (10) / shell (30). The first core (10) and the second core (20) may have, for example, different particle sizes. The first core (10) / shell (30) and the second core (20) / shell (30) may have different particle sizes.
[0062] The composite cathode active material (100) has a mixed structure of a first core (10) / shell (30) structure and a second core (10) / shell (30) structure, so that the composite density and specific capacity can be improved. For example, the first core (10) / shell (30) structure and the second core (10) / shell (30) structure included in the composite cathode active material (100) have different particle sizes of the first core (10) and the second core (20), so that the second core (10) / shell (30) is arranged in the gap between a plurality of first cores (10) / shells (30), so that the composite density and specific capacity of the entire composite cathode active material (100) can be improved. By improving the composite density and specific capacity of the composite cathode active material (100), the capacity characteristics of a lithium battery including such a composite cathode active material (100) can be improved. In addition, since the shell (30) included in the composite cathode active material (100) includes the first carbon-based material (32), the conductivity and thermal stability of the composite cathode active material (100) can be improved. As the conductivity and thermal stability of the composite cathode active material (100) are improved, a lithium battery including such a composite cathode active material (100) can have improved capacity characteristics and high-temperature cycle characteristics.
[0063] The particle size of the first core (10) may be, for example, a large-diameter cathode active material having a larger particle size than that of the second core (20). The particle size of the first core (10) may be, for example, a large-diameter lithium transition metal oxide having a larger particle size than that of the second core (20). The second core (20) may be, for example, a small-diameter cathode active material having a smaller particle size than that of the first core (10). The second core (20) may be, for example, a small-diameter lithium transition metal oxide having a smaller particle size than that of the first core (10). For example, the first lithium transition metal oxide included in the first core (10) may be a large-diameter cathode active material, and the second lithium transition metal oxide included in the second core (20) may be a small-diameter cathode active material. For example, the second lithium transition metal oxide having a smaller average particle size than that of the first lithium transition metal oxide may be arranged in the pores between the first lithium transition metal oxides. By disposing the second lithium transition metal oxide, which is a small-diameter particle, in the gaps between the first lithium transition metal oxide, which is a large-diameter particle, the ionic conductivity and electronic conductivity of the positive electrode including the composite positive electrode active material (100) can be improved simultaneously. In addition, the energy density of the positive electrode including the composite positive electrode active material (100) can be further improved. Consequently, the energy density of the lithium battery including the composite positive electrode active material (100) can be improved and the cycle characteristics can be enhanced.
[0064] The first lithium transition metal oxide and the second lithium transition metal oxide may have, for example, a bimodal particle size distribution in the particle size distribution. For example, the composite cathode active material (100) may have a bimodal particle size distribution having two peaks in the particle size distribution obtained using a particle size analyzer (PSA) or the like. The bimodal particle size distribution may have a first peak corresponding to the first lithium transition metal oxide and a second peak corresponding to the second lithium transition metal oxide.
[0065] The particle size ratio of the first lithium transition metal oxide and the second lithium transition metal oxide may be, for example, 3:1 to 40:1, 3:1 to 30:1, 3:1 to 20:1, 3:1 to 10:1, or 3:1 to 5:1. When the first lithium transition metal oxide and the second lithium transition metal oxide have particle size ratios within this range, the energy density and cycle characteristics of a lithium battery including the composite positive electrode active material (100) may be further improved.
[0066] The particle size of the first lithium transition metal oxide may be, for example, greater than 10 μm to 30 μm, 11 μm to 25 μm, 11 μm to 20 μm, or 11 μm to 15 μm. The particle size of the first lithium transition metal oxide may be, for example, a median particle diameter (D50).
[0067] The particle size of the second lithium transition metal oxide may be, for example, 1 μm to 10 μm, 1 μm to 9 μm, 1 μm to 8 μm, 1 μm to 5 μm, or 1 μm to 4 μm.
[0068] The particle size of the first lithium transition metal oxide may be, for example, a median particle diameter (D50). When the first lithium transition metal oxide and the second lithium transition metal oxide have an average particle diameter in this range, the energy density and / or cycle characteristics of a lithium battery including the composite positive electrode active material (100) may be further improved. The particle sizes of the first lithium transition metal oxide and the second lithium transition metal oxide are measured using, for example, a laser diffraction or dynamic light scattering measuring device. The particle size is measured using, for example, a laser scattering particle size distribution meter (for example, Horiba LA-920), and is the value of the median particle size (D50) when 50% is accumulated from the small particle side in volume conversion. Alternatively, the particle sizes of the first lithium transition metal oxide and the second lithium transition metal oxide may be measured from a scanning electron microscope (SEM) image or an optical microscope.
[0069] The weight ratio of the first lithium transition metal oxide and the second dry electrode active material may be, for example, 90:10 to 60:40, 85:15 to 65:35, 80:20 to 65:35, or 75:25 to 65:35. When the first lithium transition metal oxide and the second lithium transition metal oxide have a weight ratio within this range, the energy density and / or cycle characteristics of a lithium battery including the composite positive electrode active material may be further improved.
[0070] The first core (10) may include a first lithium transition metal oxide, and the second core (20) may include a second lithium transition metal oxide.
[0071] The first lithium transition metal oxide may have, for example, a layered crystal structure and an Ni content of 60 mol% or more, and the second lithium transition metal oxide may have, for example, an olivine-based crystal structure. The first lithium transition metal oxide may have, for example, a layered crystal structure and an Ni content of 60 mol% or more, so that a composite cathode active material including the first lithium transition metal oxide can easily realize high-capacity characteristics. The second lithium transition metal oxide may have, for example, an olivine-based crystal structure, so that a composite cathode active material including the second lithium transition metal oxide can easily realize thermal stability characteristics. A composite cathode active material including both the first lithium transition metal oxide and the second lithium transition metal oxide can simultaneously have high-capacity characteristics and thermal stability characteristics.
[0072] The first core (10) may include, for example, a compound selected from among lithium transition metal oxides represented by the following chemical formulas 1 to 6. The first lithium transition metal oxide may be represented by a chemical formula selected from among the following chemical formulas 1 to 6:
[0073] <Chemical Formula 1>
[0074] Li a Ni x Co y M z O 2-b A b
[0075] In the above chemical formula 1,
[0076] 1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0≤y≤0.3, 0 <z≤0.3, 및 x+y+z=1이고,
[0077] M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof,
[0078] A is F, S, Cl, Br or a combination thereof,
[0079] <Chemical Formula 2>
[0080] LiNi x Co y Mn z O2
[0081] <Chemical Formula 3>
[0082] LiNi x Co y Al z O2
[0083] In the above chemical formulas 2 and 3, 0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1이며,
[0084] <Chemical Formula 4>
[0085] LiNi x Co y Mn z Al w O2
[0086] In the above chemical formula 4, 0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1이며,
[0087] <Chemical Formula 5>
[0088] Li a Co x M y O 2-b A b
[0089] In the above chemical formula 5,
[0090] 1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1,
[0091] M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof,
[0092] A is F, S, Cl, Br or a combination thereof,
[0093] <Chemical Formula 6>
[0094] Li a Ni x Mn y M' z O 2-b A b
[0095] In the above chemical formula 6,
[0096] 1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고,
[0097] M' is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof,
[0098] A is F, S, Cl, Br or a combination thereof.
[0099] The second core (10) may include a compound selected from among lithium transition metal oxides represented by, for example, the following chemical formulas 7 and 8. The second lithium transition metal oxide may be represented by a chemical formula selected from the following chemical formulas 7 and 8:
[0100] <Chemical Formula 7>
[0101] Li a M1 x M2 y PO 4-b X b
[0102] In the above chemical formula 7, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며,
[0103] M1 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr) or a combination thereof,
[0104] M2 is magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y) or a combination thereof, and X is O, F, S, P or a combination thereof.
[0105] <Chemical Formula 8>
[0106] Li a M3 z PO4
[0107] In the above chemical formula 8, 0.90≤a≤1.1, 0.9≤z≤1.1,
[0108] M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.
[0109] The composite cathode active material (100) includes a first core (10) / shell (30) and / or a second core (20) / shell (30), and the shell (30) may be arranged continuously or discontinuously along the surface of the first core (10) or the second core (20). The composite cathode active material (100) includes a mixed structure of the first core (10) / shell (30) and the second core (20) / shell (30), and the shell (30) may be arranged continuously or discontinuously along the surface of the first core (10) and the second core (20).
[0110] The shell (30) can be more uniformly disposed on the first core (10) or the second core (20) by including the first metal oxide (31) disposed on the first carbon-based material matrix (32). The shell (30) can be more uniformly disposed on the first core (10) or the second core (20) without agglomeration by being introduced onto the first core (10) or the second core (20) from a composite including the first metal oxide (31) disposed on the first carbon-based material matrix (32), for example. The shell uniformly disposed on the first core (10) or the second core (20) can effectively block contact between the core and the electrolyte, thereby preventing side reactions due to contact between the first core (10) or the second core (20) and the electrolyte. In addition, by suppressing ion mixing by contact between the first core (10) or the second core (20) and the electrolyte, the formation of a resistance layer on the surface of the first core (10) or the second core (20) can be suppressed. In addition, by introducing the shell (30) onto the first core (10) or the second core (20), the elution of transition metal ions from the first core (10) or the second core (20) including the transition metal can be suppressed. The first carbon-based material (32) may be, for example, a crystalline carbon-based material. The first carbon-based material (32) may be, for example, a carbon-based nanostructure. The first carbon-based material (32) may be, for example, a carbon-based two-dimensional nanostructure. The first carbon-based material (32) may be, for example, graphene. For example, a shell including graphene and / or a matrix thereof has flexibility, so that it can easily accommodate changes in the volume of the composite cathode active material (100) during charge and discharge, thereby suppressing the occurrence of cracks within the composite cathode active material (100). Since graphene has high electronic conductivity, the interfacial resistance between the composite cathode active material (100) and the electrolyte is reduced. Therefore, despite the introduction of a shell including graphene, an increase in the internal resistance of the lithium battery can be suppressed.In contrast, conventional carbon-based materials that do not include the first metal oxide (31) are easily aggregated, making it difficult to uniformly arrange them on the core of the dry electrode active material. In addition, since the first carbon-based material matrix (32) is derived from, for example, a graphene matrix, it has a relatively low density and high porosity compared to conventional carbon-based materials derived from graphite-based materials.
[0111] The composite cathode active material (100) has a mixed structure of a first core (10) / shell (30) and a second core (10) / shell (30). The shell (30) includes a first metal oxide (31), and the metal included in the first metal oxide (31) may be, for example, one or more selected from among Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide (31) may be, for example, Al2O z (0 <z<3), NbO x (0 <x<2.5), MgO x (0 <x<1), Sc2O z (0 <z<3), TiO y (0 <y<2), ZrO y (0 <y<2), V2O z (0 <z<3), WO y (0 <y<2), MnO y (0 <y<2), Fe2O z (0 <z<3), Co3O w (0 <w<4), PdO x (0 <x<1), CuO x (0 <x<1), AgO x (0 <x<1), ZnO x (0 <x<1), Sb2O z (0 <z<3), 및 SeO y(0 <y<2) 중에서 선택된 하나 이상일 수 있다. 제1 탄소계 재료 메트릭스(32) 내에 이러한 제1 금속산화물(31)이 배치됨에 의하여 제1 코어(10) 또는 제2 코어(20) 상에 배치된 쉘(30)의 균일성이 향상되고, 복합양극활물질(100)의 내전압성(high-voltage resistance)이 더욱 향상된다. 쉘(30)은 예를 들어 제1 금속산화물(31)로서 Al2O x (0 <x<3)를 포함한다.
[0112] The shell (30) may further include one or more second metal oxides. The second metal oxides may be, for example, of the chemical formula M. a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시될 수 있으며, 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이다. 제2 금속산화물은 예를 들어 상기 제1 금속산화물(31)과 동일한 금속을 포함할 수 있다. 제2 금속산화물의 a 와 c의 비율인 c / a가 상기 제1 금속산화물(31)의 a 와 b의 비율인 b / a에 비하여 더 큰 값을 가질 수 있다. 예를 들어, c / a > b / a. The second metal oxide can be arranged in the first carbon-based material matrix (32). The second metal oxide is selected from, for example, Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2. The first metal oxide (31) is, for example, a reduction product of the second metal oxide. The first metal oxide (31) is obtained by reducing part or all of the second metal oxide. Therefore, the first metal oxide (31) has a lower oxygen content and a lower oxidation number of the metal than the second metal oxide. For example, the shell is Al2O, which is the first metal oxide (31). x(0 <x<3) 및 제2 금속산화물인 Al2O3를 포함한다.
[0113] The shell includes, for example, at least one selected from a first metal oxide (31) and a second metal oxide, and the particle size of at least one selected from the first metal oxide (31) and the second metal oxide may be, for example, 0.1 nm to 100 nm, 0.5 nm to 100 nm, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or 10 nm to 30 nm. Since the first metal oxide (31) and / or the second metal oxide have particle sizes in the nano-range, they may be more uniformly distributed within the first carbon-based material matrix (32). If the particle size of at least one of the first metal oxide (31) and the second metal oxide increases excessively, the thickness of the shell may increase, thereby increasing the internal resistance of the composite negative electrode active material. If the particle size of one or more of the first metal oxide (31) and the second metal oxide is excessively reduced, uniform dispersion may be difficult.
[0114] The shell (30) may include a first metal oxide (31) and / or a second metal oxide, and may include a first carbon-based material (32). The first carbon-based material (32) may be arranged in a direction protruding from the surface of the first metal oxide (31) and / or the second metal oxide. The first carbon-based material (32) may be arranged in a direction protruding from the surface of the first metal oxide (31) and / or the second metal oxide by growing directly from the surface of the first metal oxide (31) and / or the second metal oxide. The first carbon-based material (32) arranged in a direction protruding from the surface of the first metal oxide (31) and / or the second metal oxide is, for example, a carbon-based two-dimensional nanostructure, a carbon-based flake, or graphene.
[0115] The thickness of the shell (30) is, for example, 0.1 nm to 5 ㎛, 0.5 nm to 5 ㎛, 1 nm to 5 ㎛, 1 nm to 1 ㎛, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 20 nm. When the shell has a thickness in this range, the electronic conductivity of the dry electrode including the dry electrode active material can be further improved and the internal resistance can be further reduced.
[0116] The content of the shell may be, for example, 0.01 wt% to 5 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 2 wt%, or 0.01 wt% to 1 wt% of the total weight of the composite cathode active material (100). The content of the first metal oxide (31) may be, for example, 0.006 wt% to 3 wt%, 0.06 wt% to 1.8 wt%, 0.006 wt% to 1.2 wt%, or 0.006 wt% to 0.6 wt% of the total weight of the composite cathode active material (100). When the composite cathode active material (100) includes the shell (30) and the first metal oxide (31) in these content ranges, the cycle characteristics of the lithium battery are further improved.
[0117] The shell (30) may have a single-layer structure or a multi-layer structure. The multi-layer structure may have, for example, a two-layer structure, a three-layer structure, or a four-layer structure. The multi-layer structure may have, for example, different types of metals in the first metal oxide (31) contained in each layer.
[0118] The composite cathode active material (100) may further include, for example, a third metal doped on the first core (10) or the second core (20) or a third metal oxide coated on the first core (10) or the second core (20). In addition, the shell (30) may be disposed on the third metal doped on the first core (10) or the second core (20) or the third metal oxide coated on the first core (10) or the second core (20). For example, a third metal may be doped onto the surface of a compound, for example, a first lithium transition metal oxide or a second lithium transition metal oxide, included in the first core (10) or the second core (20), or a third metal oxide may be coated on the surface of a compound, for example, a first lithium transition metal oxide or a second lithium transition metal oxide, included in the first core (10) or the second core (20), and then a shell (30) may be disposed on the third metal and / or the third metal oxide. The composite cathode active material (100) includes, for example, a core; an intermediate layer disposed on the first core (10) or the second core (20); and a shell (30) disposed on the intermediate layer, wherein the intermediate layer may include a third metal or a third metal oxide. The third metal is one or more metals selected from Al, Zr, W, and Co, and the third metal oxide may be Al2O3, Li2O-ZrO2, WO2, CoO, Co2O3, Co3O4, or a combination thereof.
[0119] The shell (30) disposed along the surface of the first core (10) or the second core (20) may be, for example, a dry coating layer. The shell (30) may be introduced onto the first core (10) or the second core (20) by, for example, a dry method such as milling. The shell (30) disposed along the surface of the first core (10) or the second core (20) may include, for example, at least one selected from a composite including a first metal oxide (31) and a first carbon-based material (32), for example, graphene, and a milling result of the composite. The first metal oxide (31) is disposed within a matrix of the first carbon-based material (32), for example, a graphene matrix.
[0120] The shell (30) is manufactured from a composite including, for example, a first metal oxide (31) and a first carbon-based material (32), for example, graphene. The composite may further include a second metal oxide in addition to the first metal oxide (31). The composite may include, for example, two or more types of the first metal oxide (31). The composite may include, for example, two or more types of the first metal oxide (31) and two or more types of the second metal oxide.
[0121] The content of one or more of the composite and the milling result thereof may be, for example, 5 wt% or less, 3 wt% or less, 2 wt% or less, 1 wt% or less, or 0.5 wt% or less of the total weight of the composite cathode active material (100). The content of one or more of the composite and the milling result thereof may be 0.01 wt% to 5 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 1 wt%, 0.02 wt% to 1 wt%, or 0.05 wt% to 1 wt% of the total weight of the composite cathode active material (100). When the dry electrode active material includes one or more of the composite and the milling result thereof in this range, the cycle characteristics of a lithium battery including the dry electrode active material are further improved.
[0122] The composite may include at least one selected from a first metal oxide (31) and a second metal oxide. The particle size of at least one selected from the first metal oxide (31) and the second metal oxide may be 0.1 nm to 100 nm, 0.5 nm to 100 nm, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or 10 nm to 30 nm. Since the first metal oxide and / or the second metal oxide have particle sizes in this nano-range, they can be more uniformly distributed within the first carbon-based material matrix of the composite. Therefore, the composite can be uniformly coated on the core without agglomeration to form a shell. In addition, since the first metal oxide and / or the second metal oxide have particle sizes in this range, they can be more uniformly arranged on the core. Therefore, the withstand voltage characteristics can be more effectively exhibited by uniformly disposing the first metal oxide and / or the second metal oxide on the core. The particle size of the first metal oxide and / or the second metal oxide is measured using, for example, a measuring device such as a laser diffraction method or a dynamic light scattering method. The particle size is measured using, for example, a laser scattering particle size distribution meter (for example, Horiba LA-920), and is a value of the median particle size (D50) when 50% is accumulated from the small particle side in volume conversion. The uniformity deviation of at least one selected from the first metal oxide and / or the second metal oxide may be 3% or less, 2% or less, or 1% or less. The uniformity can be obtained, for example, by XPS. Therefore, at least one selected from the first metal oxide and the second metal oxide may have a deviation of 3% or less, 2% or less, or 1% or less and may be uniformly distributed within the composite.
[0123] The composite includes a first carbon-based material (32). The first carbon-based material (32) has, for example, a branched structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide may be distributed within the branched structure of the first carbon-based material. The branched structure of the first carbon-based material (32) includes, for example, a plurality of first carbon-based material (32) particles that are in contact with each other. The first carbon-based material (32) may provide various conductive paths by having a branched structure. The first carbon-based material (32) may be, for example, graphene. The graphene may have, for example, a branched structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide may be distributed within the branched structure of the graphene. The branched structure of the graphene includes, for example, a plurality of graphene particles that are in contact with each other. The graphene may provide various conductive paths by having a branched structure.
[0124] The first carbon-based material (32) has, for example, a spherical structure, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the first carbon-based material (32) may be 50 nm to 300 nm. There may be a plurality of first carbon-based materials (32) having a spherical structure. Since the first carbon-based material (32) has a spherical structure, the composite may have a rigid structure. The first carbon-based material (32) may be, for example, graphene. Graphene has, for example, a spherical structure, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the graphene may be 50 nm to 300 nm. There may be a plurality of graphene having a spherical structure. Since the graphene has a spherical structure, the composite may have a rigid structure.
[0125] The first carbon-based material (32) has, for example, a spiral structure in which a plurality of spherical structures are connected, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the spiral structure. The size of the spiral structure of the first carbon-based material (32) may be 500 nm to 100 μm. Since the first carbon-based material (32) has a spiral structure, the composite may have a rigid structure. The first carbon-based material (32) may be, for example, graphene. Graphene has, for example, a spiral structure in which a plurality of spherical structures are connected, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the spiral structure. The size of the spiral structure of the graphene may be 500 nm to 100 μm. Since the graphene has a spiral structure, the composite may have a rigid structure.
[0126] The first carbon-based material (32) has, for example, a cluster structure in which a plurality of spherical structures are aggregated, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the cluster structure. The size of the cluster structure of the first carbon-based material (32) may be 0.5 mm to 10 cm. Since the first carbon-based material (32) has a cluster structure, the composite may have a rigid structure. The first carbon-based material (32) may be, for example, graphene. Graphene has, for example, a cluster structure in which a plurality of spherical structures are aggregated, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure of the cluster structure. The size of the cluster structure of the graphene may be 0.5 mm to 10 cm. Since the graphene has a cluster structure, the composite may have a rigid structure.
[0127] The composite may be, for example, a faceted-ball structure, and at least one selected from a first metal oxide and a second metal oxide may be distributed within or on the surface of the structure. Since the composite is a faceted-ball structure, the composite can be easily coated on the irregular surface unevenness of the core.
[0128] The composite may be, for example, a planar structure, and at least one selected from a first metal oxide and a second metal oxide may be distributed within or on the surface of the structure. Since the composite is such a two-dimensional planar structure, the composite can be easily coated on the irregular surface unevenness of the core.
[0129] The first carbon-based material (32) may extend from the first metal oxide by a distance of 10 nm or less and may include at least 1 to 20 carbon-based material layers. For example, by stacking a plurality of first carbon-based material layers, the first carbon-based material (32) having a total thickness of 12 nm or less may be disposed on the first metal oxide. For example, the total thickness of the first carbon-based material (32) may be 0.6 nm to 12 nm. The first carbon-based material (32) may be, for example, graphene. The graphene may extend from the first metal oxide by a distance of 10 nm or less and may include at least 1 to 20 graphene layers. For example, by stacking a plurality of graphene layers, graphene having a total thickness of 12 nm or less may be disposed on the first metal oxide. For example, the total thickness of the graphene may be 0.6 nm to 12 nm.
[0130] The shell may further include, for example, a second carbon-based material (33) that is distinct from the first carbon-based material (32). The shell may further include, for example, the second carbon-based material (33) that is fibrous carbon having an aspect ratio of 10 or more. Therefore, the conducting path of the composite cathode active material (100) may become longer. The second carbon-based material (33) may form a three-dimensional conducting network between the plurality of composite cathode active materials (100), thereby reducing the internal resistance of the cathode including the composite cathode active material (100). By fixing the fibrous carbon on the composite cathode active material (100), a uniform and stable three-dimensional conducting network may be formed between the plurality of composite cathode active materials (100). Therefore, since the composite cathode active material (100) includes the second carbon-based material, the high-rate characteristics of a lithium battery including the composite cathode active material (100) may be improved. In contrast, a simple mixture of the first core (10) or the second core (20) and the second carbon-based material, fibrous carbon, makes it difficult to form a uniform three-dimensional conductive network between a plurality of first core (10) or second core (20) particles due to aggregation of the fibrous carbon, etc. The second carbon-based material (33) may be disposed on the surface of the composite cathode active material (100).
[0131] Referring to FIG. 2, the composite cathode active material (100) includes a first core (10); a second core (20), and a shell (30) that is continuously or discontinuously disposed along the surface of the first core (10) or the second core (20). The shell (30) may cover all or part of the first core (10) or the second core (20). The shell (30) includes a first metal oxide (31), a first carbon-based material (31), and a second carbon-based material (33). The second carbon-based material (33) may protrude from the surface of the composite cathode active material (100). The second carbon-based material (33) may effectively provide a conductive network between a plurality of composite cathode active materials (100). The second carbon-based material (33) may be easily coated on the first core (10) or the second core (20) by being disposed within the matrix of the first carbon-based material (32). The first carbon-based material (32) matrix can act as a binder that binds the first core (10) or the second core (20) and the second carbon-based material (33). Therefore, in the absence of the first carbon-based material (32) matrix, the second carbon-based material (33) may not be easily attached onto the first core (10) or the second core (20), or the second carbon-based material (33) may be easily detached from the first core (10) or the second core (20) during the process of manufacturing the slurry for the positive electrode. In the case where a binder is added to bind the first core (10) or the second core (20) and the second carbon-based material (33), the internal resistance of the composite positive electrode active material (100) may increase because the first core (10) or the second core (20) is covered with an insulating binder. In order to carbonize the binder, when the second carbon-based material (33) and the core coated with the binder are subjected to high-temperature heat treatment, the first core (10), the second core (20), and the second carbon-based material (33) may deteriorate during the heat treatment process.
[0132] The aspect ratio of the second carbon-based material may be 10 or greater or 20 or greater. The aspect ratio of the second carbon-based material may be, for example, 10 to 100,000, 10 to 80,000, 10 to 50,000, 10 to 10,000, 10 to 5000, 10 to 1000, 10 to 500, 10 to 100, or 10 to 50. The aspect ratio of the second carbon-based material is, for example, a ratio of the length of a major axis passing through the center of the second carbon-based material, i.e., the second carbon-based material, to the length of a minor axis passing through the center of the second carbon-based material and perpendicular to the major axis, i.e., the diameter of the second carbon-based material.
[0133] The diameter of the second carbon-based material may be, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the second carbon-based material may be, for example, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. If the diameter of the second carbon-based material is excessively large, the absolute number of strands per volume may decrease, resulting in a minimal effect in reducing internal resistance. If the diameter of the second carbon-based material is excessively small, uniform dispersion may be difficult.
[0134] The length of the second carbon-based material may be, for example, 1000 μm or less, 100 μm or less, 50 μm or less, 10 μm or less, 5 μm or less, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the second carbon-based material may be, for example, 100 nm to 1000 μm, 100 nm to 500 μm, 100 nm to 100 μm, 100 nm to 50 μm, 100 nm to 10 μm, 100 nm to 5 μm, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, or 100 nm to 300 nm. The length of the second carbon-based material may be, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 100 μm, 500 nm to 50 μm, 500 nm to 10 μm, 500 nm to 5 μm, or 500 nm to 2 μm. As the length of the second carbon-based material increases, the internal resistance of the electrode may decrease. If the length of the second carbon-based material is too short, it may be difficult to provide an effective conductive path.
[0135] The second carbon-based material may include, for example, carbon nanofibers, carbon nanotubes, or a combination thereof.
[0136] The carbon nanotube may include, for example, a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof.
[0137] The primary structure of a carbon nanotube is a single carbon nanotube unit. A carbon nanotube unit has a graphite sheet in the shape of a cylinder with a nano-sized diameter and an sp2 bonding structure. Depending on the angle and structure of the graphite sheet, it can exhibit the properties of a conductor or a semiconductor. Carbon nanotube units can be classified into single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), and multi-walled carbon nanotubes (MWCNTs) depending on the number of bonds forming the wall. The thinner the wall of a carbon nanotube unit, the lower the resistance.
[0138] The carbon nanotube primary structure may include, for example, a single-walled carbon nanotube (SWCNT), a double-walled carbon nanotube (DWCNT), a multi-walled carbon nanotube (MWCNT), or a combination thereof. The diameter of the carbon nanotube primary structure may be, for example, 1 nm or more or 2 nm or more. The diameter of the carbon nanotube primary structure may be, for example, 20 nm or less or 10 nm or less. The diameter of the carbon nanotube primary structure may be, for example, 1 nm to 20 nm, 1 nm to 15 nm, or 1 nm to 10 nm. The length of the carbon nanotube primary structure may be, for example, 100 nm or more or 200 nm or more. The length of the carbon nanotube primary structure can be, for example, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the carbon nanotube primary structure can be, for example, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, 100 nm to 400 nm, 100 nm to 300 nm, or 200 nm to 300 nm. The diameter and length of the carbon nanotube primary structure can be measured from scanning electron microscope (SEM) or transmission electron microscope (TEM) images. Alternatively, the diameter and / or length of the carbon nanotube primary structure can be measured by laser diffraction.
[0139] A carbon nanotube secondary structure is a structure formed by assembling carbon nanotube primary structures, wholly or partially, into a bundle or bundle shape. The carbon nanotube secondary structure may include, for example, a bundle-type carbon nanotube, a rope-type carbon nanotube, or a combination thereof. The diameter of the carbon nanotube secondary structure may be, for example, 2 nm or more, or 3 nm or more. The diameter of the carbon nanotube secondary structure may be, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure may be, for example, 2 nm to 50 nm, 2 nm to 30 nm, or 2 nm to 20 nm. The length of the carbon nanotube secondary structure can be, for example, 500 nm or more, 700 nm or more, 1 μm or more, or 10 μm or more. The length of the carbon nanotube secondary structure can be, for example, 1000 μm or less, 500 μm or less, or 100 μm or less. The length of the carbon nanotube secondary structure can be, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 200 μm, 500 nm to 100 μm, or 500 nm to 50 μm. The diameter and length of the carbon nanotube secondary structure can be measured from a scanning electron microscope (SEM) image or an optical microscope. Alternatively, the diameter and / or length of the carbon nanotube secondary structure can be measured by laser diffraction.
[0140] The carbon nanotube secondary structure can be converted into a carbon nanotube primary structure by dispersing it in a solvent, etc., and then used to manufacture a composite cathode active material (100).
[0141] The content of the second carbon-based material may be, for example, 0.1 wt% to 50 wt%, 1 wt% to 40 wt%, or 5 wt% to 30 wt% based on the total weight of the first carbon-based material and the second carbon-based material. When the composite cathode active material (100) includes the first carbon-based material and the second carbon-based material in this range, a conduction path is more effectively secured within the composite cathode active material (100), so that the internal resistance of the composite cathode active material (100) can be further reduced. As a result, the cycle characteristics of a lithium battery including the composite cathode active material (100) can be further improved. The content of the second carbon-based material may be, for example, 0.001 wt% to 5 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 1 wt%, 0.01 wt% to 0.5 wt%, or 0.01 wt% to 0.1 wt% of the total weight of the composite cathode active material (100). When the composite cathode active material (100) includes the second carbon-based material in this range, a conduction path is secured within the composite cathode active material (100), so that the internal resistance of the composite cathode active material (100) can be further reduced. As a result, the cycle characteristics of a lithium battery including the composite cathode active material (100) can be further improved.
[0142] The shell (30) includes a first metal oxide (31) and a first carbon-based material (32), the first core (10) includes a first lithium transition metal oxide, and the first core (20) includes a second lithium transition metal oxide. The first carbon-based material and the transition metal of the first lithium transition metal oxide or the second lithium transition metal oxide can be chemically bound, for example, through a chemical bond. The carbon atom (C) of the first carbon-based material and the transition metal (Me) of the first lithium transition metal oxide or the second lithium transition metal oxide can be chemically bound, for example, through a CO-Me bond (for example, a CO-Ni bond or a CO-Co bond) mediated by an oxygen atom. The first carbon-based material disposed in the shell (30) and the first lithium transition metal oxide disposed in the first core or the second lithium transition metal oxide disposed in the second core are chemically bonded through a chemical bond, thereby forming a composite between the first core or the second core and the shell. Therefore, the composite cathode active material (100) is distinguished from a simple physical mixture or blend of the first carbon-based material and the first lithium transition metal oxide and / or the second lithium transition metal oxide. The first metal oxide and the first carbon-based material may also be chemically bonded through a chemical bond. Here, the chemical bond is, for example, a covalent bond or an ionic bond.
[0143]
[0144] [anode]
[0145] According to another embodiment, a positive electrode includes: a positive electrode current collector; and a positive electrode active material layer disposed on one or both sides of the positive electrode current collector and including the composite positive electrode active material described above.
[0146]
[0147] [Anode: Anode current collector]
[0148] The cathode current collector may include, for example, a metal layer.
[0149] The material constituting the metal layer may be any metal or alloy that does not react with lithium, i.e., does not form an alloy or compound with lithium, and has conductivity. The metal layer may be formed of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel (SUS), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The metal layer may have a form selected from, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through-holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field may be used.
[0150] The cathode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. By having such a structure, the cathode current collector can reduce the weight of the electrode and consequently improve the energy density of the all-solid-state secondary battery.
[0151] The cathode current collector may include, for example, a metal layer; and an interlayer disposed between the metal layer and the cathode active material layer. The interlayer may include, for example, a carbon-based conductive material.
[0152] The interlayer is, for example, directly disposed on one or both surfaces of the metal layer. Therefore, no other layer may be disposed between the metal layer and the interlayer. By directly disposing the interlayer on one or both surfaces of the metal layer, the bonding strength between the metal layer and the positive electrode active material layer can be further enhanced.
[0153] The thickness of the intermediate layer is, for example, 0.01 to 30%, 0.1 to 30%, 0.5 to 30%, 1 to 25%, 1 to 20%, 1 to 15%, 1 to 10%, 1 to 5%, or 1 to 3% of the thickness of the metal layer. The thickness of the intermediate layer is, for example, 10 nm to 5 ㎛, 50 nm to 5 ㎛, 200 nm to 4 ㎛, 500 nm to 3 ㎛, 500 nm to 2 ㎛, 500 nm to 1.5 ㎛, or 700 nm to 1.3 ㎛. When the intermediate layer has a thickness in this range, the bonding force between the metal layer and the positive electrode active material layer is further enhanced, and an increase in interfacial resistance is suppressed.
[0154] The intermediate layer may include, for example, a carbon-based conductive material. The carbon-based conductive material included in the intermediate layer may be selected from among the carbon-based conductive materials used in the positive electrode active material layer. The intermediate layer may include the same carbon-based conductive material as the carbon-based conductive material used in the positive electrode active material layer. By including a carbon-based conductive material in the intermediate layer, the intermediate layer may be, for example, a conductive layer.
[0155] The intermediate layer may additionally include, for example, a binder. By additionally including a binder in the intermediate layer, the bonding strength between the metal layer and the positive electrode active material layer may be further enhanced. The binder included in the intermediate layer may be, for example, a conductive binder or a non-conductive binder. The conductive binder may be, for example, an ion-conductive binder and / or an electron-conductive binder. A binder having both ion-conductive and electron-conductive properties may be classified as either an ion-conductive binder or an electron-conductive binder.
[0156] The binder included in the intermediate layer may be selected from among the binders used in the positive electrode active material layer. The intermediate layer may include the same binder as the binder used in the positive electrode active material layer. The binder included in the intermediate layer is, for example, a fluorinated binder. The fluorinated binder included in the intermediate layer is, for example, polyvinylidene fluoride (PVDF). The intermediate layer may be, for example, a binding layer including a binder. The intermediate layer may be, for example, a conductive layer including a binder and a carbon-based conductive material.
[0157] The intermediate layer can be disposed on the metal layer, for example, dry or wet. The intermediate layer can be disposed on the metal layer dry, for example, by deposition such as CVD or PVD. The intermediate layer can be disposed on the metal layer wet, for example, by spin coating, dip coating, or the like. The intermediate layer can be disposed on the metal layer, for example, by depositing a carbon-based conductive material on the metal layer by deposition. A dry-coated intermediate layer is made of the carbon-based conductive material and may not include a binder. The intermediate layer can be disposed on the metal layer, for example, by coating a composition comprising a carbon-based conductive material, a binder, and a solvent on the surface of the metal layer and drying it. The intermediate layer can have a single-layer structure or a multi-layer structure including a plurality of layers. The multi-layer structure can be a two-layer structure, a three-layer structure, a four-layer structure, etc.
[0158]
[0159] For example, the anode may be a dry anode or a wet anode.
[0160] The positive electrode active material layer included in the dry positive electrode may be a dry positive electrode film manufactured according to a dry manufacturing method and including a composite positive electrode active material having the core / shell structure described above. By including the dry positive electrode film in the positive electrode, the internal resistance of the dry positive electrode is reduced and the mechanical properties are improved. The dry positive electrode film may be disposed on a positive electrode current collector through a lamination process.
[0161] [Positive: Dry positive electrode]
[0162] The dry cathode film includes a dry binder. A dry binder is, for example, a binder that is not impregnated, dissolved, or dispersed in a process solvent during the manufacturing process of the dry cathode film. A dry binder is, for example, a binder that does not contain or come into contact with a process solvent during the manufacturing process of the dry cathode film. The dry binder is, for example, a fibrillated binder or a fibrous binder. The fibrillated binder or the fibrous binder can serve as a matrix that supports and binds the electrode active material and other components included in the electrode active material layer. The fibrillated binder or the fibrous binder can be confirmed to have a fibrous form, for example, in a scanning electron microscope image of a cross-section of the electrode. The fibrillated binder or the fibrous binder has an aspect ratio of, for example, 10 or more, 20 or more, 50 or more, or 100 or more.
[0163] The dry binder may be, but is not limited to, any binder used in the manufacture of a dry positive electrode, such as, but not limited to, polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexapropylene (PVDF-HFP) copolymer, polyvinylidene fluoride (PVDF), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, cellulose, polyvinylpyrrolidone, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or copolymers thereof. The dry binder may particularly include a fluorinated binder. Fluorinated binders include, for example, polytetrafluoroethylene (PTFE), polyvinylidene fluoride-hexapropylene (PVDF-HFP) copolymer, or polyvinylidene fluoride (PVDF).
[0164] Glass transition temperature (T) of dry binderg ) can be, for example, -30°C to 150°C, 15°C to 150°C, 15°C to 130°C, 50°C to 130°C, 100°C to 130°C or 120°C to 130°C. The glass transition temperature (T) of the dry binder g ) can be, for example, -30°C to 150°C, -30°C to 100°C, -30°C to 50°C, -30°C to 15°C, -30°C to -10°C, or -30°C to -20°C. The glass transition temperature of polytetrafluoroethylene (PTFE) is, for example, 120°C to 130°C. Since the dry binder has a glass transition temperature in this range, a fiberized binder or a fibrous binder can be more easily obtained during the dry anode manufacturing process.
[0165] The content of the dry binder is, for example, 0.1 to 5 wt%, 0.5 to 5 wt%, or 1 to 5 wt% based on the total weight of the dry positive electrode film. By including the dry binder in this range in the dry positive electrode film, the bonding strength of the dry positive electrode film is improved, and the dry positive electrode film can maintain a high energy density.
[0166] The dry cathode film may further include, for example, a dry conductive material. A dry conductive material is a conductive material that is not impregnated, dissolved, or dispersed in a process solvent during the manufacturing process of the dry cathode film. A dry conductive material is a conductive material that does not include or come into contact with a process solvent during the manufacturing process of the dry cathode film. The dry conductive material includes, for example, a carbon-based conductive material. The carbon-based conductive material includes, for example, a fibrous carbon-based material having an aspect ratio of 10 or greater, a particulate carbon-based material having an aspect ratio of less than 10, or a combination thereof.
[0167] The fibrous carbon-based material having an aspect ratio of 10 or more includes, but is not limited to, carbon fibers, carbon nanotubes, carbon nanobelts, etc., and any material used as a carbon-based conductive material in the relevant technical field may be used. The fibrous carbon-based material having an aspect ratio of 10 or more may be selected from the second carbon-based materials described above. The fibrous carbon-based material conductive material is distinguished from the second carbon-based material forming part of the composite cathode active material in that it is simply mixed with the composite cathode active material.
[0168] Particulate carbon-based materials having an aspect ratio of less than 10 include, but are not limited to, carbon black, acetylene black, Ketjen black, natural graphite, artificial graphite, etc., and any material used as a carbon-based conductive material in the relevant technical field may be used. The aspect ratio of the particulate carbon-based material is, for example, 1 to 7, 1 to 5, 1 to 3, or 1 to 2.
[0169] The content of the dry conductive material included in the dry positive electrode film is, for example, 0.1 to 5 wt%, 0.5 to 5 wt%, or 1 to 5 wt% based on the total weight of the dry positive electrode film. By including the dry conductive material in this range in the dry positive electrode film, the conductivity of the dry positive electrode film is improved, and the cycle characteristics of a lithium battery including the dry positive electrode film can be improved.
[0170] Dry cathode films are, for example, self-standing films. Dry cathode films can maintain a film form without a support, for example. Therefore, dry cathode films can be prepared as separate self-standing films and then placed on a current collector. Since dry cathode films are manufactured through a dry process, they do not contain any intentionally added process solvents. For example, they do not contain residual processing solvents. While trace amounts of unintended solvents may remain in the dry cathode film, these solvents are not intentionally added process solvents. Therefore, dry cathode films are distinguished from wet electrode films, which are manufactured by mixing components and a process solvent, and then drying to remove some or all of the process solvent.
[0171] The tensile strength of the dry positive electrode film can be, for example, 500 kPa or more, 700 kPa or more, or 1000 kPa or more at 25°C. The tensile strength of the dry positive electrode film can be, for example, 500 kPa to 5000 kPa, 700 kPa to 5000 kPa, or 1000 kPa to 5000 kPa at 25°C. When the dry positive electrode film has a tensile strength in this range, the structural stability of the dry positive electrode film can be improved. Therefore, the dry positive electrode film can maintain a stable three-dimensional conductive network during the charge and discharge process, thereby improving the reversibility of the electrode reaction. When the dry positive electrode film has a high tensile strength in this range, the mechanical strength of the dry positive electrode film can be improved. Since the dry cathode film has improved mechanical strength, local deterioration due to volume change during charge and discharge of an electrode including the dry cathode film and a lithium battery including the same can be suppressed. As a result, the cycle characteristics of the lithium battery can be improved.
[0172] [Positive: Wet Positive]
[0173] The positive electrode active material layer included in the wet positive electrode may be a wet positive electrode active material layer manufactured according to a wet manufacturing method and including the composite positive electrode active material described above. For example, the wet positive electrode active material layer may be disposed on the positive electrode current collector by coating a composition including the composite positive electrode active material including the core / shell structure described above, a wet binder, a wet conductive agent, and a solvent on the surface of the positive electrode current collector and drying the composition.
[0174] Wet conductive materials include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any material used as a conductive material in the relevant technical field may be used.
[0175] As wet binders, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the above polymers, styrene butadiene rubber polymers, etc. are used, and as solvents, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but are not necessarily limited to these, and any solvent used in the relevant technical field may be used.
[0176] It is also possible to form pores inside the positive electrode by adding a plasticizer or a pore forming agent to the positive electrode active material composition.
[0177] The content of the composite cathode active material, wet conductive agent, wet binder, and solvent used in the wet cathode may be at levels typically used in lithium batteries. Depending on the intended use and configuration of the lithium battery, one or more of the wet conductive agent, wet binder, and solvent may be omitted.
[0178] The wet binder content included in the wet positive electrode may be 0.1 to 10 wt% or 0.1 to 5 wt% of the total weight of the positive electrode active material layer. The composite positive electrode active material content included in the wet positive electrode may be 90 wt% to 99 wt% or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.
[0179] The composite cathode active material described above includes a first lithium transition metal oxide and a second lithium transition metal oxide in the first core and the second core, respectively, and includes a first metal oxide and a first carbon-based material in a shell disposed on the surface of the first core or the second core.
[0180] The cathode active material layer may additionally include a conventional cathode active material in addition to the dry cathode active material having the core / shell structure described above. Any conventional cathode active material commonly used in the art may be used without limitation.
[0181] The cathode active material may be, for example, one or more of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof, and a specific example thereof is Li a A 1-b B b D2 (in the above formula, 0.90 ≤ a ≤ 1, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α(In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above equation, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α F2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn dGeO2 (in the above formula, 0.90 ≤ a ≤ 1, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (wherein 0.90 ≤ a ≤ 1, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:
[0182] In the chemical formula representing the compound described above, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.
[0183] It is also possible to use a compound having a coating layer added to the surface of the above-mentioned compound, or it is also possible to use a mixture of the above-mentioned compound and a compound having a coating layer added. The coating layer added to the surface of the above-mentioned compound includes, for example, a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element of the coating element. The compound forming the coating layer is amorphous or crystalline. The coating elements included in the coating layer are Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The method for forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method includes, for example, spray coating and dipping. Since specific coating methods are well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0184]
[0185] [Lithium battery]
[0186] According to another embodiment, a lithium battery may include the above-described positive electrode; negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode.
[0187] The cycle characteristics of a lithium battery are improved by having the above-described positive electrode having reduced internal resistance and improved mechanical properties.
[0188] The lithium battery may include, for example, a dry positive electrode, a dry negative electrode, or a dry positive electrode and a dry negative electrode. The lithium battery may include, for example, a dry positive electrode and a wet negative electrode, or a dry positive electrode and a dry negative electrode, or a wet positive electrode and a dry negative electrode.
[0189]
[0190] [Lithium Battery: Electrolyte]
[0191] A lithium battery includes an electrolyte, which may include, for example, a liquid electrolyte, a solid electrolyte, or a combination thereof.
[0192] Liquid electrolytes are, for example, organic electrolytes. Organic electrolytes are prepared by dissolving lithium salts in organic solvents.
[0193] Any organic solvent used in the relevant technical field may be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0194] Lithium salts are all possible if they are used as lithium salts in the relevant technical field. Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (where x and y are natural numbers), LiCl, LiI, or mixtures thereof.
[0195] The solid electrolyte may include, for example, an inorganic solid electrolyte, an organic solid electrolyte, an organic-inorganic composite solid electrolyte, or a combination thereof.
[0196] The solid electrolyte may include, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer-based solid electrolyte, or a combination thereof.
[0197] The solid electrolyte may be, but is not limited to, boron oxide, lithium oxynitride, etc., and any solid electrolyte used in the relevant technical field may be used. The solid electrolyte may be formed on the cathode by, for example, sputtering or a separate solid electrolyte sheet may be laminated on the cathode.
[0198] Oxide solid electrolytes include, for example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0≤x<1, 0≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li3+x La3M2O 12 (M = Te, Nb, or Zr, 0≤x≤10), Li 3+x La3Zr 2-y M y O 12 (M doped LLZO, M=Ga, W, Nb, Ta, Al or a combination thereof, 0≤x≤10, 0 <y<2), Li7La3Zr 2-x Ta x O 12 (0 <x<2, LLZ-Ta), 또는 이들의 조합을 포함한다. 산화물계 고체전해질은 예를 들어 가넷계(Garnet-type) 고체전해질이다. 산화물계 고체전해질은 소결법 등에 의하여 제작된다.
[0199] Oxide-based solid electrolytes include, for example, Li7La3Zr2O 12 (LLZO), Li 6.5 La3Zr 1.5 Ta 0.5 O 12 , Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Li 0.34 La 0.51 TiO 2.94 , Li 1.07 Al 0.69 Ti 1.46 (PO4)3, 50Li4SiO4-50Li2BO3, 90Li3BO3-10Li2SO4, Li 2.9 PO 3.3 N 0.46 , or a combination thereof.
[0200] Sulfide-based solid electrolytes include, for example, Li2S-P2S5, Li2S-P2S5-LiX, where X is a halogen element, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n, m, n are positive numbers, Z is one of Ge, Zn or Ga, Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q , p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga In, Li 7-x PS 6-x Cl x , 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , at least one selected from 0≤x≤2. The sulfide-based solid electrolyte is manufactured by treating starting materials such as Li2S and P2S5 by a melting rapid cooling method or a mechanical milling method. In addition, heat treatment may be performed after such treatment. The sulfide-based solid electrolyte may be amorphous, crystalline, or a mixture thereof.
[0201] The sulfide-based solid electrolyte may include, for example, an argyrodite type solid electrolyte represented by the following chemical formula 9:
[0202] <Chemical Formula 9>
[0203] Li + 12-n-x A n+ X 2- 6-x Y - x
[0204] In the above formula, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb, or Ta, X is S, Se, or Te, Y is Cl, Br, I, F, CN, OCN, SCN, or N3, and 1≤n≤5, 0≤x≤2.
[0205] Sulfide-based solid electrolyte is Li 7-x PS 6-x Cl x, 0≤x≤2, Li 7-x PS 6-x Br x , 0≤x≤2, and Li 7-x PS 6-x I x , may be an argyrodite-type compound including at least one selected from 0≤x≤2. In particular, the sulfide-based solid electrolyte included in the solid electrolyte may be an argyrodite-type compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.
[0206] The polymer-based solid electrolyte may be, for example, a solid electrolyte comprising an ion-conducting polymer and a lithium salt, a solid electrolyte comprising an ionic liquid polymer and a lithium salt, or a combination thereof.
[0207] An ion-conducting polymer is a polymer that contains an ion-conducting repeating unit in its main chain or side chain. The ion-conducting repeating unit is a unit having ion conductivity, and may be, for example, an alkylene oxide unit, a hydrophilic unit, etc. The ion-conducting polymer may contain, for example, an ether monomer, an acrylic monomer, a methacrylic monomer, a siloxane monomer, or a combination thereof as the ion-conducting repeating unit. The ion-conducting polymer may be, for example, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyethyl methacrylate, polydimethylsiloxane, polyacrylic acid, polymethacrylic acid, polymethyl acrylate, polyethyl acrylate, poly-2-ethylhexyl acrylate, polybutyl methacrylate, poly-2-ethylhexyl methacrylate, polydecylacrylate, polyethylenevinylacetate, or a combination thereof. The ion-conducting polymer can be, for example, polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyvinyl sulfone, or a combination thereof.
[0208] Polymeric ionic liquids (PILs) include, for example, i) one or more cations selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazole and mixtures thereof, and ii) BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, (CF3SO2)2N-, Cl-, Br-, I-, BF4-, SO4 - , PF6-, ClO4-, CF3SO3-, CF3CO2-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, NO3 - , Al2Cl7 - , AsF6 - , SbF6 - , CF3COO - , CH3COO - , CF3SO3 - , (CF3SO2)3C - , (CF3CF2SO2)2N - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , SF5CF2SO3 - , SF5CHFCF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (O(CF3)2C2(CF3)2O)2PO -And may contain repeating units comprising one or more anions selected from (CF3SO2)2N-. The ionic liquid polymer may be, for example, poly(diallyldimethylammonium)TFSI, poly(1-allyl-3-methylimidazolium trifluoromethanesulfonylimide), poly(N-methyl-N-propylpiperidinium bis(trifluoromethanesulfonyl)imide)), or a combination thereof.
[0209] Lithium salts include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(1≤x≤20, 1≤y≤20), LiCl, LiI or a combination thereof.
[0210]
[0211] Dry anode: manufacturing method
[0212] A method for manufacturing a dry anode according to another embodiment is provided.
[0213] A method for manufacturing a dry cathode comprises the steps of providing a dry cathode film; and the steps of disposing the dry cathode film on one or both sides of a cathode current collector.
[0214] The step of providing a dry positive electrode film includes a step of preparing a dry mixture by dry mixing the above-described composite positive electrode active material, dry conductive material, and dry binder; and a step of preparing a dry positive electrode film by molding the dry mixture.
[0215] First, a dry mixture is prepared by dry mixing the composite cathode active material, dry conductive agent, and dry binder described above. For example, a dry mixture is prepared by dry mixing the composite cathode active material, dry conductive agent, and dry binder.
[0216] Dry mixing means mixing without a process solvent. A process solvent is, for example, a solvent used in the preparation of an electrode slurry. The process solvent is not limited to, but includes, water, NMP, etc., and is not limited to, any process solvent used in the preparation of an electrode slurry. Dry mixing can be performed using a stirrer at a temperature of, for example, 15°C to 65°C and a rotation speed of 10 to 10,000 rpm. Dry mixing can be performed using a stirrer for, for example, 1 to 200 minutes.
[0217] Dry mixing may be performed, for example, more than once. First, a composite positive electrode active material, a dry conductive material, and a dry binder may be subjected to a first dry mixing to prepare a first dry mixture. The first dry mixing may be performed, for example, at a temperature of 25 to 65°C, at a rotation speed of 10 to 2000 rpm or less, for a time of 15 minutes or less. Subsequently, the first dry mixture may be additionally subjected to a second dry mixing to prepare a second mixture. The second dry mixing may be performed, for example, at a temperature of 25 to 65°C, at a rotation speed of 3000 to 9000 rpm, for a time of 10 to 60 minutes. By the second dry mixing, a dry mixture including a fibrillated dry binder may be obtained.
[0218] The stirrer is, for example, a kneader. The stirrer includes, for example, a chamber; one or more rotating shafts disposed inside the chamber and rotating; and blades rotatably coupled to the rotating shafts and disposed in the longitudinal direction of the rotating shafts. The blades may be, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersion blade, and a screw blade. By including the blades, an electrode active material, a dry conductive material, and a dry binder can be effectively mixed without a solvent to produce a dough-like mixture.
[0219] Dry binders include, for example, vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the aforementioned polymers, and styrene butadiene rubber-based polymers. The dry binder may be selected from among the dry binders used in the above-described dry positive electrode films.
[0220] Dry conductive materials include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver; and conductive polymers such as polyphenylene derivatives. Any material used as a conductive material in the relevant technical field may be used. The conductive material is, for example, a carbon-based conductive material. The dry conductive material may be selected from among the dry conductive materials used in the above-described dry positive electrode film.
[0221] It is also possible to form pores inside the electrode plate by adding a plasticizer or pore former to the dry mixture.
[0222] The content of the above-described composite positive electrode active material, dry binder, and dry conductive material used in the dry positive electrode film is at a level typically used in lithium batteries.
[0223] The dry cathode film uses a composite cathode active material including the first core / shell and / or second core / shell structures described above as a composite cathode active material. The composite cathode active material refers to the composite cathode active material described above. The dry cathode film uses a dry cathode active material as a dry cathode active material.
[0224] Next, the dry mixture is molded to prepare a dry cathode film.
[0225] The prepared dry mixture can be fed into an extrusion device and extruded into a sheet or film form. The pressure during extrusion is, for example, 4 MPa to 100 MPa.
[0226] Next, an electrode current collector is provided in which an intermediate layer is disposed on one or both sides of a metal layer.
[0227] The step of providing an electrode current collector having an intermediate layer disposed on one or both sides of a metal layer includes, for example, a step of providing a metal layer; and a step of disposing the intermediate layer on one or both sides of the metal layer.
[0228] The metal layer of the positive electrode collector refers to the positive electrode collector section described above. The metal layer of the positive electrode collector is, for example, aluminum foil. The negative electrode collector is, for example, copper foil.
[0229] The step of disposing an intermediate layer on one or both sides of the metal layer includes dry coating and / or wet coating. Dry coating involves, for example, coating a carbon-based conductive material and / or a precursor thereof on one or both sides of a positive electrode current collector by vapor deposition or the like. The vapor deposition is performed at a temperature ranging from room temperature to high temperature and a pressure ranging from normal pressure to vacuum. The intermediate layer disposed by dry coating may not include a binder if it is made of a carbon-based material. Wet coating involves, for example, coating a composition comprising a carbon-based conductive material and a binder on one or both sides of the positive electrode current collector. The composition includes, for example, a carbon-based conductive material, a binder, and a process solvent. For details on the carbon-based conductive material and binder, refer to the electrode section described above. The process solvent may be selected from solvents used in the preparation of the positive electrode slurry. The process solvent is removed by drying after the composition is coated on the electrode current collector. The coating method may include, but is not limited to, spin coating, dip coating, or the like, and any coating method used in the art may be used.
[0230] Next, the dry cathode films are simultaneously or sequentially placed on one or both sides of the electrode collector to manufacture a dry cathode.
[0231] A rolling step may be added during and / or after placing the dry cathode film on one or both sides of the cathode collector.
[0232] Rolling can be performed using, but is not limited to, a roll press or a flat plate press. The pressure during rolling is, for example, 1.0 to 10.0 ton / cm. If the pressure during rolling is excessively high, cracks may occur in the positive electrode current collector. If the pressure during rolling is excessively low, the bonding strength between the positive electrode current collector and the dry positive electrode film may be reduced.
[0233]
[0234] [Wet Anode: Manufacturing Method]
[0235] A method for manufacturing a wet anode according to another embodiment is provided.
[0236] The wet positive electrode manufacturing method includes the steps of preparing a positive electrode active material slurry by mixing the above-described composite positive electrode active material, wet conductive material, wet binder, and solvent; directly coating the prepared positive electrode active material slurry on a positive electrode current collector; and drying the positive electrode current collector coated with the positive electrode active material slurry to form a positive electrode active material layer, thereby manufacturing a wet positive electrode.
[0237] Alternatively, the above-mentioned positive electrode active material slurry is cast on a separate support, and then the film obtained by peeling off the support is laminated on the positive electrode current collector to manufacture a wet positive electrode having a positive electrode active material layer formed thereon.
[0238] For the composite cathode active material, wet conductive agent, wet binder and solvent included in the cathode active material slurry, refer to the description described above.
[0239] Lithium Batteries: Manufacturing Methods
[0240] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not limited to these methods and may vary depending on the required conditions.
[0241] First, one or both of the positive electrode and the negative electrode can be manufactured according to the above-described dry electrode manufacturing method. Alternatively, when one of the positive electrode and the negative electrode is manufactured using the above-described dry electrode manufacturing method, the other electrode can be manufactured using the above-described wet manufacturing method. For example, the other electrode can be manufactured by manufacturing an electrode slurry containing an electrode active material, a conductive material, a binder, and a solvent, coating the manufactured electrode slurry on an electrode current collector, and drying it. The manufactured dry positive electrode or wet positive electrode can include the above-described composite positive electrode active material.
[0242] Next, a separator to be inserted between the positive and negative electrodes is prepared.
[0243] Any separator commonly used in lithium batteries can be used. For example, a separator with low resistance to ion migration and excellent electrolyte absorption capacity is used. The separator may be selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be in the form of a nonwoven or woven fabric. For lithium-ion batteries, a rollable separator, such as polyethylene or polypropylene, is used, while for lithium-ion polymer batteries, a separator with excellent organic electrolyte absorption capacity is used.
[0244] The separator is manufactured by the following exemplary methods, but is not limited to these methods and may be adjusted according to required conditions.
[0245] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated and dried on the electrode to form a separator. Alternatively, the separator composition is cast on a support and dried, and then a separator film peeled from the support is laminated on the electrode to form a separator.
[0246] The polymer used in separator manufacturing is not particularly limited; any polymer used as a binder for electrode plates can be used. Examples include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof.
[0247] Next, the electrolyte is prepared. Refer to the lithium battery section described above for the electrolyte.
[0248] As shown in Fig. 6, the lithium battery (1) includes a positive electrode (3), a negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An organic electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0249] As shown in Fig. 7, the lithium battery (1) includes a positive electrode (3), a negative electrode (2), and a separator (4). The separator (4) is placed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may have, for example, a cylindrical shape, a thin film shape, etc.
[0250] As shown in Fig. 8, a lithium battery (1) includes a positive electrode (3), a negative electrode (2), and a separator (4). A separator (4) is placed between the positive electrode (3) and the negative electrode (2) to form a battery structure. A battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. An organic electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.
[0251] A pouch-type lithium battery corresponds to the lithium batteries of FIGS. 6 to 8, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with an organic electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0252] Lithium batteries are used in electric vehicles (EVs) due to their excellent cycle life and high-rate characteristics. For example, they are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). They are also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.
[0253] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0254] [Composite cathode active material: manufacturing method]
[0255] Another embodiment of a method for manufacturing a composite cathode active material comprises the steps of: providing a first core and a second core; providing a composite; and mechanically milling the first core, the second core, and the composite to manufacture a composite cathode active material, wherein the composite comprises at least one first metal oxide; and a first carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, and the first metal oxide is represented by the chemical formula M. a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되며, 상기 M은 원소주기율표 2족 내지 16족 중에서 선택된 하나 이상의 금속이다.
[0256] As a first core, for example, the first lithium transition metal oxide described above is provided. The first lithium transition metal oxide may have a layered crystal structure and an Ni content of 60 mol% or more, for example. The first lithium transition metal oxide may be a compound represented by any of the chemical formulae 1 to 6 described above.
[0257] As a second core, for example, the second lithium transition metal oxide described above is provided. The second lithium transition metal oxide may have, for example, an olivine-based crystal structure. The second lithium transition metal oxide may be, for example, a compound represented by the chemical formulae 7 to 8 described above.
[0258] A composite is provided. The step of providing the composite includes, for example, the step of supplying a reaction gas consisting of a carbon source gas to a structure including a metal oxide and performing a heat treatment to provide the composite. The step of providing the composite includes, for example, M a O c(0 <a≤3, 0<c≤4, a가 1, 2 또는 3인 경우, b가 정수임)로 표시되는 1 종 이상의 제2 금속산화물에 탄소 공급원 기체로 이루어진 반응 가스를 공급하고 열처리하여 복합체를 제조하는 단계를 포함하며, 상기 M은 원소주기율표 제2 족 내지 제13 족, 제15 족 및 제16 족 중에서 선택된 하나 이상의 금속이다.
[0259] The carbon source gas is a gas composed of a compound represented by the following chemical formula 10, or at least one mixed gas selected from the group consisting of a compound represented by the following chemical formula 10, a compound represented by the following chemical formula 11, and an oxygen-containing gas represented by the following chemical formula 12.
[0260] <Chemical Formula 10>
[0261] C n H (2n+2-a) [OH] a
[0262] In the above chemical formula 10, n is 1 to 20, a is 0 or 1;
[0263] <Chemical Formula 11>
[0264] C n H 2n
[0265] In the above chemical formula 11, n is 2 to 6;
[0266] <Chemical Formula 12>
[0267] C x H y O z
[0268] In the above chemical formula 12, x is 0 or an integer from 1 to 20, y is 0 or an integer from 1 to 20, and z is 1 or 2.
[0269] The compound represented by Chemical Formula 10 and the compound represented by Chemical Formula 11 are at least one selected from the group consisting of methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Chemical Formula 12 includes, for example, carbon dioxide (CO2), carbon monoxide (CO), water vapor (H2O), or a mixture thereof.
[0270] M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물에 탄소 공급원 기체로 이루어진 반응 가스를 공급하고 열처리하는 단계 이후에 질소, 헬륨 및 아르곤으로 이루어진 군으로부터 선택된 하나 이상의 불활성 기체를 이용한 냉각 단계를 더 거칠 수 있다. 냉각 단계는 상온(20 내지 25℃)으로 조절하는 단계를 말한다. 탄소 공급원 기체는 질소, 헬륨, 아르곤으로 이루어진 군으로부터 선택된 하나 이상의 불활성 기체를 포함할 수 있다.
[0271] In the manufacturing method of the composite, the process of growing carbon-based materials, such as graphene, depending on the gas phase reaction can be performed under various conditions.
[0272] According to the first condition, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 메탄을 공급하고 열처리온도(T)까지 승온처리한다. 열처리 온도(T)까지의 승온 시간은 10 분 내지 4 시간이고 열처리온도(T)는 700 ℃ 내지 1100 ℃ 범위이다. 열처리온도(T)에서 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 시간 내지 8 시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 시간 내지 5 시간이다.
[0273] According to the second condition, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 수소를 공급하고 열처리온도(T)까지 승온 처리한다. 열처리 온도(T)까지의 승온 시간은 10 분 내지 4 시간이고 열처리온도(T)는 700 ℃ 내지 1100 ℃ 범위이다. 열처리온도(T)에서 일정 반응 시간 동안 열처리한 후 메탄 가스를 공급하고 잔여 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 시간 내지 8 시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 냉각하는 과정에서 질소를 공급한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 시간 내지 5 시간이다.
[0274] According to the third condition, for example, M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물이 배치된 반응기에 먼저 수소를 공급하고 열처리온도(T)까지 승온 처리한다. 열처리 온도(T)까지의 승온 시간은 10 분 내지 4 시간이고 열처리온도(T)는 700 ℃ 내지 1100 ℃ 범위이다. 열처리온도(T)에서 일정 반응 시간 동안 열처리한 후 메탄과 수소의 혼합 가스를 공급하고 잔여 반응 시간 동안 열처리를 실시한다. 반응시간은 예를 들어 4 시간 내지 8 시간이다. 열처리된 결과물을 상온으로 냉각시켜 복합체를 제조한다. 냉각하는과정에서 질소를 공급한다. 열처리온도(T)에서 상온까지 냉각하는 과정에 걸치는 시간은 예를 들어 1 시간 내지 5 시간이다.
[0275] In the process of manufacturing a composite, if the carbon source gas contains water vapor, a composite having very good conductivity can be obtained. The content of water vapor in the gas mixture is not limited and is, for example, 0.01% to 10% by volume based on 100% by volume of the total carbon source gas. The carbon source gas is, for example, methane; a mixed gas containing methane and an inert gas; or a mixed gas containing methane and an oxygen-containing gas.
[0276] The carbon source gas can be, for example, methane; a mixture of methane and carbon dioxide; or a mixture of methane, carbon dioxide, and water vapor. In the mixture of methane and carbon dioxide, the molar ratio of methane to carbon dioxide is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. In the mixture of methane, carbon dioxide, and water vapor, the molar ratio of methane, carbon dioxide, and water vapor is about 1:0.20 to 0.50:0.01 to 1.45, about 1:0.25 to 0.45:0.10 to 1.35, or about 1:0.30 to 0.40:0.50 to 1.0.
[0277] The carbon source gas is, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas may not include an inert gas such as nitrogen.
[0278] The heat treatment pressure can be selected considering the heat treatment temperature, the composition of the gas mixture, and the desired amount of carbon coating. The heat treatment pressure can be controlled by adjusting the amount of the incoming gas mixture and the amount of the outgoing gas mixture. The heat treatment pressure is, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more. The heat treatment pressure is, for example, 0.5 atm to 10 atm, 1 atm to 10 atm, 2 atm to 10 atm, 3 atm to 10 atm, 4 atm to 10 atm, or 5 atm to 10 atm.
[0279] The heat treatment time is not particularly limited and can be appropriately adjusted depending on the heat treatment temperature, the pressure during the heat treatment, the composition of the gas mixture, and the desired amount of carbon coating. For example, the reaction time at the heat treatment temperature is, for example, 10 minutes to 100 hours, 30 minutes to 90 hours, or 50 minutes to 40 hours. For example, as the heat treatment time increases, the amount of carbon deposited, for example, the amount of graphene (carbon), increases, and thus the electrical properties of the composite may improve. However, this trend may not necessarily be directly proportional to time. For example, after a certain period of time, carbon deposition, for example, graphene deposition, may no longer occur or the deposition rate may decrease.
[0280] Through the gas phase reaction of the carbon source gas described above, M is produced even at relatively low temperatures. a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물 및 그 환원 생성물인 M a O b(0 <a≤3, 0<b<4, a는 1, 2, 또는 3이며, b 는 정수가 아님)로 표시되는 제1 금속산화물 중에서 선택된 하나 이상에 균일한 탄소계 재료의 코팅 예를 들어 그래핀 코팅을 제공함에 의하여 복합체가 얻어진다.
[0281] The composite is a matrix of carbon-based materials having one or more structures selected from, for example, a spherical structure, a spiral structure in which multiple spherical structures are connected, a cluster structure in which multiple spherical structures are aggregated, and a sponge structure, for example, a graphene matrix and M arranged within the graphene matrix. a O b (0 <a≤3, 0<b<4, a는 1, 2, 또는 3이며, b 는 정수가 아님)로 표시되는 제1 금속산화물 및 M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3이면, c는 정수임)로 표시되는 제2 금속산화물 중에서 선택된 하나 이상을 포함한다.
[0282] Next, the first lithium transition metal oxide, the second lithium transition metal oxide, and the composite are mechanically milled to manufacture a composite cathode active material. A Nobilta mixer, etc. can be used during the milling. The rotation speed of the mixer during the milling is, for example, 1000 rpm to 5000 rpm. The milling time is, for example, 5 minutes to 100 minutes. The average particle diameter (D50) of the composite used for the mechanical milling of the first lithium transition metal oxide, the second lithium transition metal oxide, and the composite is, for example, 50 nm to 200 nm, 100 nm to 300 nm, or 200 nm to 500 nm. The milling method in the mechanical milling step is not particularly limited, and any method usable in the art as a method of contacting the first lithium transition metal oxide, the second lithium transition metal oxide, and the composite using a machine may be used.
[0283]
[0284] The present invention is further described in detail through the following examples and comparative examples. However, these examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0285] (Manufacture of composites)
[0286] Manufacturing example: Al2O3@Gr composite
[0287] Al2O3 particles (average particle diameter: approximately 15 nm) were placed inside the reactor, and then CH4 was supplied into the reactor at approximately 300 sccm and 1 atm for approximately 30 minutes, and the temperature inside the reactor was raised to 1000°C.
[0288] Then, heat treatment was performed by maintaining the temperature for 7 hours. Then, the internal temperature of the reactor was adjusted to room temperature (20 to 25°C) to produce Al2O3 particles and its reduction product, Al2O z (0 <z<3) 입자가 그래핀에 매립된 복합체를 얻었다.
[0289] The alumina content of the composite was 60 wt%.
[0290]
[0291] (Manufacture of composite cathode active material)
[0292] Manufacturing Example 1: Manufacturing of NCA91 coated with Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) and LFP coated with Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) (weight ratio 90:10)
[0293] LiNi with an average particle size (D50) of 14 ㎛ 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91), LiFePO4 (hereinafter referred to as LFP) having an average particle size (D50) of 3.5 μm, and the composite prepared in Manufacturing Example were milled using a Nobilta Mixer (Hosokawa, Japan) at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes to obtain a composite cathode active material. The weight ratio of the total weight of NCA91 and LFP to the composite prepared in Manufacturing Example 1 was 99.64:0.36. In addition, the weight ratio of NCA91 to LFP was 90:10.
[0294]
[0295] Manufacturing Example 2: Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated NCA91 and Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated LFP (weight ratio 80:20)
[0296] LiNi with an average particle size (D50) of 14 ㎛ 0.91 Co 0.05 Al 0.04O2 (hereinafter referred to as NCA91), LiFePO4 (hereinafter referred to as LFP) having an average particle size (D50) of 3.5 μm, and the composite prepared in Manufacturing Example were milled using a Nobilta Mixer (Hosokawa, Japan) at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes to obtain a composite cathode active material. The weight ratio of the total weight of NCA91 and LFP to the weight of the composite prepared in Manufacturing Example 1 was 99.64:0.36. In addition, the weight ratio of NCA91 to LFP was 80:20.
[0297]
[0298] Manufacturing Example 3: Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated NCA91 and Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated LFP (weight ratio 75:25)
[0299] LiNi with an average particle size (D50) of 14 ㎛ 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91), LiFePO4 (hereinafter referred to as LFP) having an average particle size (D50) of 3.5 μm, and the composite prepared in Manufacturing Example were milled using a Nobilta Mixer (Hosokawa, Japan) at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes to obtain a composite cathode active material. The weight ratio of the total weight of NCA91 and LFP to the composite prepared in Manufacturing Example 1 was 99.64:0.36. In addition, the weight ratio of NCA91 to LFP was 75:25.
[0300]
[0301] Manufacturing Example 4: Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated NCA91 and Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated LFP (weight ratio 50:50)
[0302] LiNi with an average particle size (D50) of 14 ㎛ 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91), LiFePO4 (hereinafter referred to as LFP) having an average particle size (D50) of 3.5 μm, and the composite prepared in Manufacturing Example were milled at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes using a Nobilta Mixer (Hosokawa, Japan) to obtain a composite cathode active material. The weight ratio of the total weight of NCA91 and LFP to the weight of the composite prepared in Manufacturing Example 1 was 99.64:0.36. In addition, the weight ratio of NCA91 to LFP was 50:50.
[0303]
[0304] Manufacturing Example 5: Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated NCA91 and Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated LFP (weight ratio 20:80)
[0305] LiNi with an average particle size (D50) of 14 ㎛ 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91), LiFePO4 (hereinafter referred to as LFP) having an average particle size (D50) of 3.5 μm, and the composite prepared in Manufacturing Example were milled using a Nobilta Mixer (Hosokawa, Japan) at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes to obtain a composite cathode active material. The weight ratio of the total weight of NCA91 and LFP to the composite prepared in Manufacturing Example 1 was 99.64:0.36. In addition, the weight ratio of NCA91 to LFP was 20:80.
[0306]
[0307] Manufacturing Example 6: Al2O3@Gr composite 0.36 wt% (alumina 0.36 wt%) coated NCA91 and LFP
[0308] LiNi with an average particle size (D50) of 14 ㎛ 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91) and the composite prepared in the manufacturing example were milled at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes using a Nobilta Mixer (Hosokawa, Japan) to obtain a 0.36 wt% Al2O3@Gr composite (0.36 wt% alumina) coated NCA91. Thereafter, LiFePO4 (hereinafter referred to as LFP) having an average particle diameter (D50) of 3.5 μm was added to the 0.36 wt% Al2O3@Gr composite (0.36 wt% alumina) coated NCA91, and then milled at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes using a Nobilta Mixer (Hosokawa, Japan) to obtain a composite cathode active material. The weight ratio of NCA91 to the weight of the composite manufactured in Manufacturing Example 1 was 99.64:0.36. In addition, the weight ratio of NCA91 to LFP was 90:10.
[0309]
[0310] Comparative Manufacturing Example 1: NCA91 and LFP
[0311] LiNi with an average particle size (D50) of 14 ㎛ 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91) and LiFePO4 (hereinafter referred to as LFP) having an average particle size (D50) of 3.5 ㎛ were milled using a Nobilta Mixer (Hosokawa, Japan) at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes to obtain a composite cathode active material. The weight ratio of NCA91 to LFP was 90:10.
[0312] Comparative Manufacturing Example 2: NCA91
[0313] LiNi with an average particle size (D50) of 14 ㎛ without additional milling0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91) was prepared.
[0314]
[0315] Comparative Manufacturing Example 3: Manufacturing of Carbon-Coated NCA91 and Carbon-Coated LFP
[0316] Carbon-coated NCA91 and carbon-coated LFP were manufactured by adding 0.36 wt% of carbon black to NCA91 with an average particle size (D50) of 14 μm and LPF with an average particle size (D50) of 3.5 μm, respectively, in a Thinky mixer and milling at a rotation speed of 1000 to 2000 rpm for about 2 to 5 minutes. The weight ratio of the total weight of NCA91 and LFP to the weight of the composite manufactured in Manufacturing Example 1 was 99.64:0.36. In addition, the weight ratio of NCA91 to LFP was 90:10.
[0317] .
[0318] Comparative Manufacturing Example 4: Manufacturing of Gr-coated NCA91 and Gr-coated LFP (weight ratio 90:10)
[0319] LiNi with an average particle size (D50) of 14 ㎛ 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91), LiFePO4 (hereinafter referred to as LFP) having an average particle size (D50) of 3.5 ㎛, and graphene were milled using a Nobilta Mixer (Hosokawa, Japan) at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes to obtain a composite cathode active material. The weight ratio of the total weight of NCA91 and LFP to the weight of the composite prepared in Preparation Example 1 was 99.64:0.36. In addition, the weight ratio of NCA91 to LFP was 90:10.
[0320]
[0321] (Manufacturing of lithium batteries (half cells))
[0322] Example 1
[0323] (Manufacture of dry cathode film and dry cathode)
[0324] The dry composite cathode active material, dry carbon conductive material, and polytetrafluoroethylene (PTFE) as a dry binder manufactured in Manufacturing Example 1 were placed in a blade mixer at a weight ratio of 96:2:2, and then primary dry mixing was performed at a speed of 1200 rpm at 25°C for 10 minutes to prepare a first dry mixture in which the dry cathode active material, dry conductive material, and dry binder were uniformly mixed. The dry carbon conductive material used was a mixture of carbon nanotubes (CNT) and Ketjen Black (ECP) at a weight ratio of 7:3.
[0325] Next, to allow the fiberization of the binder to proceed, the first dry mixture was further mixed for a second time using a blade mixer at 25°C for 25 minutes at a speed of 4000 rpm to prepare a second dry mixture.
[0326] No separate solvent was used in the preparation of the first dry mixture and the second dry mixture.
[0327] The prepared second dry mixture was fed into an extruder and extruded to prepare a sheet-shaped dry cathode film self-standing film. The pressure during extrusion was 60 MPa.
[0328] A rolled dry electrode film self-supporting membrane was prepared by rolling the prepared dry positive electrode film self-supporting membrane. The pressure during rolling was 3.5 ton / cm. 2 The thickness of the dry anode film was approximately 200 ㎛.
[0329] A cathode current collector was prepared in which a carbon layer was coated on one side of a 25 ㎛ thick aluminum film.
[0330] The carbon layer was prepared by coating a composition containing a carbon conductive material (Danka black) and polyvinylidene fluoride (PVDF) and then drying. The thickness of the carbon layer disposed on one surface of the positive electrode collector was approximately 1 μm.
[0331] A dry cathode was manufactured by placing a rolled dry cathode film on one side of a cathode current collector.
[0332] (Manufacturing of coin cells)
[0333] Using the positive electrode manufactured above, a coin cell was manufactured using lithium metal as a counter electrode, a PTFE separator, and a solution of 1.3 M LiPF6 dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (3:4:3 volume ratio) as an electrolyte.
[0334] Example 2
[0335] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Manufacturing Example 2 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0336] Example 3
[0337] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Manufacturing Example 3 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0338] Example 4
[0339] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Manufacturing Example 4 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0340] Example 5
[0341] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Manufacturing Example 5 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0342] Example 6
[0343] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Manufacturing Example 6 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0344] Comparative Example 1
[0345] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Comparative Manufacturing Example 1 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0346] Comparative Example 2
[0347] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Comparative Manufacturing Example 2 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0348] Comparative Example 3
[0349] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Comparative Manufacturing Example 3 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0350] Comparative Example 4
[0351] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Comparative Manufacturing Example 4 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0352] Comparative Example 5
[0353] A dry electrode film, a dry positive electrode, and a coin cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material manufactured in Comparative Manufacturing Example 4 was used instead of the composite positive electrode active material manufactured in Manufacturing Example 1.
[0354] Evaluation Example 1: SEM, HR-TEM, and SEM-EDS Analysis
[0355] Scanning electron microscopy, high-resolution transmission electron microscopy, and EDS (Energy-dispersive X-ray spectroscopy) analyses were performed on the composite cathode active material manufactured in Manufacturing Example 1.
[0356] SEM-EDS analysis was performed using Philips' FEI Titan 80-300. Figure 3 is a scanning electron microscope image of the composite cathode active material prepared in Manufacturing Example 1.
[0357] Referring to FIG. 3, it was confirmed that a composite including graphene was arranged on a large-diameter NCA91 core and a small-diameter LFP core in the composite cathode active material manufactured in Example 1.
[0358]
[0359] Evaluation Example 2: Specific Capacity and Compound Density Evaluation
[0360] The specific capacity and composite density of the composite positive electrode active materials manufactured in Manufacturing Examples 1 to 5 were measured.
[0361] The specific capacity of the composite cathode active material was measured by dividing the charge (current x time, mAh) obtained by discharging coin cells containing the composite cathode active materials manufactured in Manufacturing Examples 1 to 5 in the range of 3.0 to 4.3 V for 5 hours by the weight of the cathode active material. The composite density was calculated by measuring the weight and volume (area x thickness) of the cathode electrode.
[0362] The specific capacities and composite densities of the composite positive electrode active materials manufactured in Manufacturing Examples 1 to 5 are shown in Table 1 below.
[0363]
[0364] Al2O3@Gr composite coating NCA contentAl2O3@Gr composite coating LFP contentSpecific capacity (mAh / g)Composite density (g / cc)Manufacturing example 19010201.13.61Manufacturing example 28020197.23.60Manufacturing example 37525196.23.59Manufacturing example 45050185.53.57Manufacturing example 52080173.83.54
[0365]
[0366] As shown in Table 1, it was confirmed that the specific capacity and composite density increased as the content of Al2O3@Gr composite coating NCA in the composite cathode active material increased.
[0367]
[0368] Evaluation Example 3: Evaluation of high-temperature (40°C) charge / discharge characteristics
[0369] The lithium batteries manufactured in Examples 1 to 6 and Comparative Examples 1 to 5 were charged at a constant current of 0.1 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Li) during discharge (formation cycle).
[0370] The lithium battery, which had undergone a Mars cycle, was charged at a constant current of 0.5 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Subsequently, the battery was discharged at a constant current of 0.5 C rate until the voltage reached 2.8 V (vs. Li) (1 st cycle). These cycles are 50 th The cycle was repeated under the same conditions.
[0371] In all charge / discharge cycles, a 10-minute pause was provided after each charge / discharge cycle. During the high-temperature charge / discharge experiment, 1 st Charging capacity in cycle, 1 st Discharge capacity in cycles, 1 st Efficiency in cycles, electrode density and 50 th The results of measuring the capacity retention rate [%] in the cycle are shown in Table 2 below.
[0372] Also, during the high temperature charge and discharge experiment, 1 stFrom cycle 50 th The results of measuring the capacity retention rate [%] of each cycle up to the cycle are shown in Fig. 4. The capacity retention rate is defined by the following mathematical equation 1.
[0373] <Mathematical Formula 1>
[0374] Capacity retention rate at each cycle [%] = [Discharge capacity at each cycle / 1] st Discharge capacity in cycles] Х 100
[0375]
[0376] Evaluation Example 4: Gas Emission Measurement
[0377] The amount of gas generated when the lithium batteries manufactured in Examples 1 to 6 and Comparative Examples 1 to 5 were left at 130°C for 1 hour was measured.
[0378] Specifically, the positive electrode in a charged state was placed in a pouch, sealed, and then the weight was measured. After 1 hour at 130°C, the density of the pouch with the gas generated from the positive electrode added was measured, and the weight change value obtained was converted into volume to calculate the amount of gas generated according to Archimedes' principle.
[0379] The measurement results are shown in Table 2 below.
[0380]
[0381] Cathode active materialInitial charge capacity (mAh / g)Initial discharge capacity (mAh / g)Initial efficiency (%)Electrode density (g / cc)Retention rate (%@50) th)Gas generation amount (cc / g)Example 1 Composite coating NCA91+ Composite coating LFP(90:10)226.7200.488.43.61949.96Example 2 Composite coating NCA91+ Composite coating LFP(80:20)219.9196.189.13.694.29.82Example 3 Composite coating NCA91+ Composite coating LFP(75:25)216.1193.889.73.5995.19.78Example 4 Composite coating NCA91+ Composite coating LFP(50:50)197.4182.592.53.5796.59.62Example 5 Composite coating NCA91+ Composite coating LFP(20:80)176.4169.094.83.5497.29.38Example 6Composite coating NCA91+ LFP(90:10)227.5198.687.33.6693.510.12Comparative example 1NCA91+ LFP(90:10)231.2201.1873.6491.210.09Comparative example 2NCA91234.4203.686.93.6789.710.10Comparative example 3Carbon coating NCA91+Carbon coating LFP(90:10)227.6199.887.83.690.811.20Comparative example 4Graphene coating NCA91+Graphene coating LFP(90:10)227.6200.187.93.6292.510.23
[0382] As shown in Table 2, the lithium batteries of Examples 1 to 6 had improved high-temperature life characteristics compared to the lithium batteries of Comparative Examples 1 to 4.
[0383] The lithium batteries of Examples 1 to 3 had relatively reduced gas generation compared to the lithium battery of Example 6.
[0384] The lithium batteries of Examples 1 to 3 had relatively superior initial capacities and electrode densities compared to the lithium batteries of Examples 4 and 5.
[0385] <Explanation of symbols>
[0386] 1 lithium battery 2 cathode
[0387] 3 positive electrode 4 separator
[0388] 5 Battery case 6 Cap assembly
[0389] 7 Battery structure 8 Electrode tab
[0390] 10 1st core 20 2nd core
[0391] 30 Shell 31 First metal oxide
[0392] 32 First carbon-based material 33 Second carbon-based material
[0393] 100 composite cathode active materials
Claims
1. A first core (1) comprising a first lithium transition metal oxide st core); A second core (2) comprising a second lithium transition metal oxide nd core); and A shell disposed along the surface of at least one of the first core and the second core; The above shell comprises at least one first metal oxide; and a first carbon-based material; The first metal oxide is disposed within the first carbon-based material matrix, The above first metal oxide has the chemical formula M a O b (0 <a≤3, 0<b<4, a가 1, 2, 또는 3 이면, b는 정수가 아님)로 표시되며, 상기 M은 원소주기율표 2족 내지 13족, 제15족 및 16족 중에서 선택된 하나 이상의 금속이며, The first core and the second core have different particle sizes, The first lithium transition metal oxide has a layered crystal structure and a Ni content of 60 mol% or more, A composite cathode active material in which a second lithium transition metal oxide has an olivine crystal structure.
2. In paragraph 1, A composite cathode active material, wherein the particle size of the first lithium transition metal oxide included in the first core is larger than the particle size of the second lithium transition metal oxide included in the second core.
3. In paragraph 1, The particle size distribution of the first lithium transition metal oxide and the second lithium transition metal oxide has a bimodal particle size distribution, A composite cathode active material, wherein the particle size ratio of the first lithium transition metal oxide to the second lithium transition metal oxide is 3:1 to 40:
1.
4. In paragraph 1, The particle size of the first lithium transition metal oxide is greater than 10 μm to 30 μm, A composite cathode active material, wherein the particle size of the second lithium transition metal oxide is 1 µm to 10 µm.
5. In paragraph 1, A composite cathode active material, wherein the weight ratio of the first lithium transition metal oxide to the second lithium transition metal oxide is 90:10 to 60:
40.
6. In paragraph 1, The above first lithium transition metal oxide is a composite cathode active material represented by a chemical formula selected from the following chemical formulas 1 to 6: <Chemical Formula 1> Li a Ni x Co y M z O 2-b A b In the above chemical formula 1, 1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0≤y≤0.3, 0 <z≤0.3, 및 x+y+z=1이고, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof, A is F, S, Cl, Br or a combination thereof, <Chemical Formula 2> LiNi x Co y Mr z O2 <Chemical Formula 3> LiNi x Co y Al z O2 In the above chemical formulas 2 and 3, 0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2 및 x+y+z=1이며, <Chemical Formula 4> LiNi x Co y Mr z Al w O2 In the above chemical formula 4, 0.8≤x≤0.95, 0≤y≤0.2, 0 <z≤0.2, 0<w≤0.2, 및 x+y+z+w=1이며, <Chemical Formula 5> Li a Co x M y O 2-b A b In the above chemical formula 5, 1.0≤a≤1.2, 0≤b≤0.2, 0.9≤x≤1, 0≤y≤0.1, and x+y=1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof, A is F, S, Cl, Br or a combination thereof, <Chemical Formula 6> Li a Ni x Mr y M' z O 2-b A b In the above chemical formula 6, 1.0≤a≤1.2, 0≤b≤0.2, 0 <x≤0.3, 0.5≤y<1, 0<z≤0.3, 및 x+y+z=1이고, M' is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, A is F, S, Cl, Br or a combination thereof.
7. In paragraph 1, A composite cathode active material, wherein the second lithium transition metal oxide is represented by a chemical formula selected from the following chemical formulas 7 and 8: <Chemical Formula 7> Yes a M1 x M2 y PO 4-b X b In the above chemical formula 7, 0.90≤a≤1.1, 0≤x≤0.9, 0≤y≤0.5, 0.9 <x+y<1.1, 0≤b≤2 이며, M1 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr) or a combination thereof, M2 is magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y) or a combination thereof, and X is O, F, S, P or a combination thereof, <Chemical Formula 8> Li a M3 z PO4 In the above chemical formula 8, 0.90≤a≤1.1, 0.9≤z≤1.1, M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.
8. In paragraph 1, The above shell is a composite positive electrode active material arranged along the surfaces of the first core and the second core.
9. In paragraph 1, The metal contained in the first metal oxide is at least one metal selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se, The above first metal oxide is Al2O z (0 <z<3), NbO x (0 <x<2.5), MgO x (0 <x<1), Sc2O z (0 <z<3), TiO y (0 <y<2), ZrO y (0 <y<2), V2O z (0 <z<3), WO y (0 <y<2), MnO y (0 <y<2), Fe2O z (0 <z<3), Co3O w (0 <w<4), PdO x (0 <x<1), CuO x (0 <x<1), AgO x (0 <x<1), ZnO x (0 <x<1), Sb2O z (0 <z<3), 및SeO y (0 <y<2) 중에서 선택되는 하나 이상인, 복합양극활물질.
10. In paragraph 1, The above shell further comprises a second metal oxide, The second metal oxide has the chemical formula M a O c (0 <a≤3, 0<c≤4, a가 1, 2, 또는 3 이면, c는 정수임)로 표시되며, The second metal oxide contains the same metal as the first metal oxide, The ratio of a and c of the second metal oxide, c / a, has a larger value than the ratio of a and b of the first metal oxide, b / a, A composite cathode active material in which the second metal oxide is disposed within the first carbon-based material matrix.
11. In paragraph 10, The second metal oxide is selected from Al2O3, NbO, NbO2, Nb2O5MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2, A composite cathode active material wherein the first metal oxide is a reduction product of the second metal oxide.
12. In paragraph 1, A composite cathode active material, wherein the thickness of the shell is 0.1 nm to 5 μm, and the shell has a single-layer structure or a multi-layer structure.
13. In paragraph 1, A composite cathode active material, wherein the weight of the shell is 0.01 to 5 wt% based on the total weight of the composite cathode active material.
14. In paragraph 1, Further comprising a third metal doped on the first core or the second core or a third metal oxide coated on the first core or the second core, The shell is placed on the third metal oxide, A composite cathode active material, wherein the third metal oxide is an oxide of at least one third metal selected from Al, Zr, W, and Co.
15. In paragraph 1, The above shell further comprises a second carbon-based material, The above second carbon-based material includes a fibrous carbon-based material having an aspect ratio of 10 or more, The second carbon-based material comprises carbon nanofibers, carbon nanotubes, or a combination thereof, The above carbon nanotube comprises a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof. A composite cathode active material in which the above carbon nanotube primary structure is a single carbon nanotube unit chain.
16. In paragraph 1, The first carbon-based material and the transition metal of the first lithium transition metal oxide or the transition metal of the second lithium transition metal oxide are chemically bound through a chemical bond, The carbon atom (C) of the first carbon-based material and the transition metal (Me) of the first lithium transition metal oxide or the transition metal (Me) of the second lithium transition metal oxide are chemically bonded (bound) through a CO-Me bond via an oxygen atom, A composite cathode active material in which the first metal oxide is chemically bound to the first carbon-based material through a chemical bond.
17. Anode current collector; and A positive electrode comprising a positive electrode active material layer disposed on one or both sides of the positive electrode current collector and including a composite positive electrode active material according to any one of claims 1 to 16.
18. In paragraph 17, The above cathode current collector includes a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a polymer, and the polymer comprises polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, An anode, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
19. In paragraph 17, The above anode is a dry anode or a wet anode.
20. The anode according to Article 17; cathode; and A lithium battery comprising an electrolyte disposed between the positive electrode and the negative electrode.
Citation Information
Patent Citations
Cathode active material of lithium secondary battery for high power characteristic, and lithium secondary battery comprising thereof
KR1020120113007A
Positive electrode active material for rechargeable lithium battery, manufacturing method of the same, and rechargeable lithium battery including the same
KR1020150093451A
Image signal encoding / decoding method and apparatus using efficient motion vector predictor
KR1020200085667A
Photovoltaic plant anomaly monitoring and analysis method, device and system through image processing
KR1020240082431A
Positive electrode active material compositiom for secondary battery and secondary battery comprising the same
KR102227302B1
Cited By
Rechargeable lithium metal battery system
US20260221491A1