Electrode structure including polymer electrolyte, method for manufacturing same, and lithium battery including same
The integration of a polymer electrolyte with a crosslinked structure and metal salt on a nickel or chromium current collector addresses the reactivity issues in lithium metal batteries, enhancing durability and stability by preventing polymerization suppression and ensuring uniform lithium deposition, thus improving battery lifespan.
Patent Information
- Application Number
- PCT/KR2024/003732
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-12
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium metal thin film electrodes in lithium metal batteries have high reactivity with liquid electrolytes, leading to dendrite formation and reduced lifespan and stability due to the high reactivity of lithium, necessitating improvements in electrode structures for enhanced durability and stability.
An electrode structure incorporating a polymer electrolyte with a crosslinked structure containing a metal salt and polar functional groups, applied to a nickel, chromium, or zinc-based current collector, which prevents polymerization reaction suppression and promotes uniform lithium electrodeposition, thereby improving durability and lifespan.
The proposed electrode structure enhances the durability and high-temperature stability of lithium batteries by preventing polymerization reaction suppression and ensuring uniform lithium electrodeposition, leading to improved lifespan characteristics.
Smart Images

Figure KR2024003732_03102024_PF_FP_ABST
Abstract
Description
Electrode structure including polymer electrolyte, method for manufacturing same, and lithium battery including same
[0001] An electrode structure including a polymer electrolyte, a method for manufacturing the same, and a lithium battery including the same are presented.
[0002] Lithium secondary batteries are high-performance secondary batteries with the highest energy density among the currently commercialized secondary batteries and can be used in various fields such as electric vehicles.
[0003] Lithium metal films are used as anodes in lithium metal batteries. When these films are used as anodes, the high reactivity of lithium leads to a high reactivity with the liquid electrolyte during charge and discharge. Furthermore, dendrites can form on the lithium anode film, reducing the lifespan and stability of lithium metal batteries employing the film. Therefore, improvements are needed.
[0004] One aspect is to provide an electrode structure comprising a polymer electrolyte with improved durability and life characteristics.
[0005] Another aspect is to provide a lithium battery comprising the electrode structure described above.
[0006] Electrode current collector; and
[0007] A polymer electrolyte disposed on the electrode collector;
[0008] The above electrode collector contains nickel (Ni), chromium (Cr) or zinc (Zn),
[0009] The polymer electrolyte comprises a crosslinked structure including repeating units (A) derived from a first polymer and repeating units (B) derived from a second polymer, and a metal salt,
[0010] The first polymer comprises a polymer containing a polar functional group,
[0011] An electrode structure is provided in which the second polymer comprises a polyurethane-based polymer.
[0012] According to another aspect, the step of preparing an electrode collector;
[0013] A step of preparing a composition for forming a polymer electrolyte comprising a first polymer, a second polymer, a metal salt, and an initiator;
[0014] A step of applying the polymer electrolyte forming composition on the electrode current collector; and
[0015] It comprises a step of forming an electrode structure including a polymer electrolyte from an electrode current collector to which the composition for forming the polymer electrolyte is applied,
[0016] The above electrode collector contains nickel (Ni), chromium (Cr) or zinc (Zn),
[0017] The first polymer comprises a polymer containing a polar functional group,
[0018] A method for manufacturing an electrode structure is provided, wherein the second polymer comprises a polyurethane-based polymer.
[0019] According to another aspect, a lithium battery including the electrode structure described above is provided.
[0020] An electrode structure according to one embodiment includes an electrode current collector and a polymer electrolyte disposed on the electrode current collector, wherein the electrode current collector includes nickel or chromium metal, and the polymer electrolyte includes a metal salt, so that a polymerization reaction for forming a polymer electrolyte can be prevented from being inhibited by metal ions flowing out from the electrode current collector during the process of forming the polymer electrolyte. Accordingly, the durability and high-temperature stability of the electrode structure can be improved.
[0021] In addition, the electrode structure includes a polymer electrolyte containing a metal salt, and the metal salt can induce uniform electrodeposition of lithium. An electrode structure including such a polymer electrolyte can have improved life characteristics.
[0022] Figure 1 schematically illustrates an electrode structure including a polymer electrolyte according to an embodiment.
[0023] Figure 2 shows a cross-sectional view of a lithium battery according to an embodiment.
[0024] Figure 3 shows a cross-sectional view of a lithium battery according to an embodiment.
[0025] Figure 4 is a schematic diagram of a lithium battery according to an exemplary embodiment.
[0026] Figure 5 is a schematic diagram of a lithium battery according to an exemplary embodiment.
[0027] Figure 6 is a schematic diagram of a lithium battery according to an exemplary embodiment.
[0028] Hereinafter, an electrode structure including a polymer electrolyte according to one embodiment, a method for manufacturing the same, and a lithium battery including the same will be examined in more detail. These examples are provided solely as examples to more specifically illustrate the present invention, and it will be apparent to those skilled in the art that the scope of the present invention is not limited by these examples.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, the present specification, including its definitions, shall prevail.
[0030] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, suitable methods and materials are described herein. The singular expression "singular" includes plural expression unless the context clearly indicates otherwise.
[0031] In this specification, the terms "include" or "have" are intended to indicate the presence of a feature, number, step, operation, component, part, ingredient, material or combination thereof described in the specification, but should be understood to not preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials or combinations thereof.
[0032] The term "combination of these" in this specification means a mixture or combination of one or more of the described components.
[0033] As used herein, the term "and / or" is meant to include any and all combinations of one or more of the items described herein. As used herein, the term "or" means "and / or." The expressions "at least one," "one or more," or "one or more" preceding elements herein may supplement the entire list of elements and do not mean that they supplement individual elements described above.
[0034] In order to clearly represent various layers and regions in the drawings, the thicknesses are enlarged or reduced. The same drawing reference numerals are used for similar parts throughout the specification. When a layer, film, region, plate, etc. is referred to as being "on" or "above" another part throughout the specification, this includes not only cases where it is directly above the other part, but also cases where there is another part in between. The terms first, second, etc. may be used throughout the specification to describe various components, but the components should not be limited by the terms. The terms are used only to distinguish one component from another.
[0035] In this disclosure, “metal” includes both metals and metalloids such as silicon and germanium, in their elemental or ionic states.
[0036] In this disclosure, “alloy” means a mixture of two or more metals.
[0037] In the present disclosure, “positive electrode material” means a positive electrode material capable of undergoing lithiation and delithiation.
[0038] In the present disclosure, “negative electrode active material” means a negative electrode material capable of undergoing lithiation and delithiation.
[0039] In the present disclosure, “lithiation” and “lithiating” mean a process of adding lithium to a positive electrode active material or a negative electrode active material.
[0040] In the present disclosure, “delithiation” and “delithiate” mean a process of removing lithium from a positive electrode active material or a negative electrode active material.
[0041] In this disclosure, “charging” and “charging” mean a process of providing electrochemical energy to a battery.
[0042] In this disclosure, “discharging” and “discharging” mean the process of removing electrochemical energy from a battery.
[0043] In the present disclosure, “positive electrode” and “cathode” mean an electrode at which electrochemical reduction and lithiation occur during a discharge process.
[0044] In the present disclosure, “cathode” and “anode” mean electrodes where electrochemical oxidation and delithiation occur during the discharge process.
[0045] With reference to the attached drawings, exemplary polymer electrolytes and lithium batteries including the same will be described in more detail below.
[0046]
[0047] [Electrode structure]
[0048] Figure 1 schematically illustrates an electrode structure including a polymer electrolyte according to an embodiment.
[0049] Referring to FIG. 1, the electrode structure (10) includes an electrode current collector (110); and a polymer electrolyte (120) disposed on the electrode current collector (100), wherein the electrode current collector (100) includes nickel (Ni), chromium (Cr), or zinc (Zn), and the polymer electrolyte (120) includes a cross-linked structure (121) including a repeating unit (A) derived from a first polymer and a repeating unit (B) derived from a second polymer, and a metal salt (122) disposed inside the cross-linked structure (121), wherein the first polymer includes a polymer including a polar functional group, and the second polymer may include a polyurethane-based polymer. For example, the electrode structure (10) includes a polymer electrolyte including a metal salt (122), and the metal salt (122) may include a metal having a high affinity for lithium. In this case, the metal salt (122) acts as a nucleation site of lithium during charge and discharge, so that lithium metal can be more uniformly deposited on the electrode current collector (100) by the metal salt (122) included in the polymer electrolyte (120). In addition, when the polymer electrolyte (120) includes the metal salt (122), during the manufacturing process of the electrode structure (10), the metal in the electrode current collector (110) with a relatively high degree of ionization can flow into the polymer electrolyte in the form of metal ions. In this case, when the electrode structure (10) includes copper (Cu), Cu 2+ is leaked, Cu 2+It functions as a radical scavenger, thereby stopping the polymerization reaction of polymers included in the polymer electrolyte, which may reduce the durability of the polymer electrolyte (120). However, the electrode current collector (110) of the present invention includes nickel (Ni) or chromium (Cr) instead of copper, so that the polymerization reaction of polymers included in the polymer electrolyte can be performed more easily. Accordingly, the durability of the polymer electrolyte (120) and the adhesion to the electrode current collector (110) can be further improved.
[0050]
[0051] [Electrode structure: electrode collector]
[0052] According to one embodiment, the surface of the electrode current collector (110) may include nickel (Ni) or chromium (Cr) and may not include copper (Cu). In this case, during the manufacturing process of the electrode structure (10), the polymer electrolyte (120) may include copper ions (Cu 2+ ) may not be included. Accordingly, copper ions (Cu 2+ ) effectively prevents the polymerization reaction inhibition effect of the first polymer and the second polymer, and the polymerization reaction or crosslinking reaction of the first polymer and the second polymer can be performed more easily.
[0053] According to one embodiment, the electrode current collector (110) includes a base film and a metal layer disposed on one or both sides of the base film, the base film includes a metal or a polymer, the metal in the base film includes indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li) or an alloy thereof, the polymer in the base film includes polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, and the metal layer may include nickel (Ni) or chromium (Cr). According to another embodiment, the electrode current collector (110) may be made of nickel (Ni) or chromium (Cr).
[0054] For example, when the base film includes a polymer, the polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may melt when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator.
[0055] For example, when the base film includes a metal, the metal may include indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
[0056] For example, the metal layer may include nickel (Ni) or chromium (Cr). For example, the metal layer may include nickel (Ni) or chromium (Cr) and may not include copper (Cu). The metal layer may function as an electrochemical fuse and may be cut off in the event of overcurrent to prevent a short circuit. The limit current and maximum current may be controlled by adjusting the thickness of the metal layer. The metal layer may be plated or deposited on the base film.
[0057] For example, when the thickness of the metal substrate layer becomes thinner, the limit current and / or maximum current of the electrode current collector (110) decreases, so the stability of the lithium battery in the event of a short circuit can be improved. A lead tab may be added on the metal layer for external connection. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal substrate layer may melt, so that the metal layer may be electrically connected to the lead tab. In order to make the welding of the metal substrate layer and the lead tab more solid, a metal chip may be added between the metal layer and the lead tab. The metal chip may be a thin piece of the same material as the metal of the metal layer. The metal chip may be, for example, a metal foil, a metal mesh, etc. The metal chip may be, for example, aluminum foil, copper foil, SUS foil, etc. A lead tab can be welded to a metal piece / metal layer laminate or a metal piece / metal layer / base film laminate by placing a metal piece on a metal layer and then welding it to the lead tab. During welding, the base film, metal layer, and / or metal piece melts, so that the metal layer or the metal layer / metal piece laminate can be electrically connected to the lead tab. A metal piece (metal chip) and / or a lead tab can be added to a portion of the metal layer.
[0058] For example, the thickness of the base film can be, for example, 1 to 50 ㎛, 1.5 to 50 ㎛, 1.5 to 40 ㎛, or 1 to 30 ㎛. When the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film can be, for example, 100 to 300 ℃, 100 to 250 ℃ or less, or 100 to 200 ℃. When the base film has a melting point in this range, the base film can be melted during the process of welding the lead tab and easily bonded to the lead tab. In order to improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment can be performed on the base film. The thickness of the metal layer can be, for example, 0.01 to 3 ㎛, 0.1 to 3 ㎛, 0.1 to 2 ㎛, or 0.1 to ㎛. By having a metal layer with a thickness within this range, conductivity can be maintained while ensuring the stability of the negative electrode. The thickness of the metal piece can be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. By having a metal piece with a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having the electrode current collector (110) with this structure, the weight of the electrode can be reduced, and consequently, the energy density can be improved.
[0059] For example, the electrode current collector (110) may have a form selected from among, for example, a sheet, a foil, a film, a plate, a porous body, a mesoporous body, a body containing through holes, a polygonal ring body, a mesh body, a foam body, and a non-woven body, but is not necessarily limited to these forms, and any form used in the relevant technical field may be used.
[0060] For example, the electrode current collector (110) may have a reduced thickness compared to a conventional electrode current collector. Therefore, the electrode according to the present disclosure is distinguished from a conventional electrode including a thick film current collector, for example, by including a thin film current collector. Since the electrode according to one embodiment employs a thin film current collector having a reduced thickness, the thickness of the electrode active material layer in the electrode including the thin film current collector may relatively increase. As a result, the energy density of a lithium battery employing such an electrode may increase. The thickness of the electrode current collector (110) may be, for example, less than 15 um, 14.5 um or less, or 14 um or less. The thickness of the electrode current collector (110) may be, for example, 0.1 um to less than 15 um, 1 um to 14.5 um, 2 um to 14 um, 3 um to 14 um, 5 um to 14 um, or 10 um to 14 um.
[0061]
[0062] [Electrode structure: polymer electrolyte]
[0063] The polymer electrolyte (120) may include a cross-linked structure (121) comprising repeating units (A) derived from a first polymer and repeating units (B) derived from a second polymer, and a metal salt (122). In this case, the metal salt (122) may be arranged inside the cross-linked structure (121).
[0064] For example, the cross-linked structure (121) may refer to a structure in which the first polymer and the second polymer included in the polymer electrolyte (120) are cross-linked to form a cross-linked network. For example, the first polymer includes a polymer including a polar functional group, and lithium ions may move within the polymer electrolyte (120) along the polymer including the polar functional group. For example, the second polymer is a polyurethane-based polymer, and may impart elastic properties to the polymer electrolyte (120).
[0065] According to one embodiment, the polymer comprising a polar functional group included in the first polymer may include polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride-hexafluoropropylene copolymer, or any combination thereof.
[0066] According to one embodiment, the first polymer may further comprise one or more terminal double bonds. For example, the first polymer may further comprise two or more terminal double bonds. For example, the one or more terminal double bonds may include an allyl group, an acryl group, or a vinyl group. For example, the one or more terminal double bonds may include an acryl group. For example, when the first polymer further comprises a terminal double bond, the first polymer can more easily form a crosslinking network between the first polymer and / or the second polymer as a crosslinking agent. Accordingly, the durability of a crosslinked structure including a repeating unit (A) derived from the first polymer can be further improved.
[0067] In one embodiment, the first polymer may include polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene glycol diacrylate, polyethylene glycol methyl ether acrylate, polymethyl methacrylate, polyethyl methacrylate, polycaprolactone, polyethylene carbonate, polypropylene carbonate, or any combination thereof.
[0068] In one embodiment, the second polymer may include polyurethane, urethane acrylate, urethane methacrylate, perfluoropolyether urethane acrylate, perfluoropolyether urethane methacrylate, or any combination thereof.
[0069] According to one embodiment, the content of the repeating unit (A) derived from the first polymer in the crosslinked structure (121) may be 50 to 90 wt% with respect to the total weight of the crosslinked structure, and the content of the repeating unit (B) derived from the second polymer may be 10 to 50 wt% with respect to the total weight of the crosslinked structure. For example, the content of the repeating unit (A) derived from the first polymer in the crosslinked structure (121) may be 60 to 90 wt%, 70 to 90 wt%, 50 to 80 wt%, or 60 to 80 wt% with respect to the total weight of the crosslinked structure. For example, the content of the repeating unit (B) derived from the second polymer may be 10 to 40 wt%, 10 to 30 wt%, 20 to 50 wt%, or 20 to 30 wt% with respect to the total weight of the crosslinked structure.
[0070] The metal salt (122) may include a lithium-compatible metal salt. For example, the lithium-compatible metal salt may include a lithium-compatible metal. For example, since the metal salt (122) includes a lithium-compatible metal salt, the lithium metal including the electrode structure (10) including the polymer electrolyte (120) may have lithium more uniformly deposited by the metal salt (122) included in the polymer electrolyte (120) during charge and discharge. For example, the lithium-compatible metal ion and the lithium ion included in the lithium-compatible metal salt may form an alloy during charge and discharge, and the formed alloy may act as a nucleation site, thereby inducing uniform deposition of lithium.
[0071] According to one embodiment, the metal salt (122) may include gold (Au), silver (Ag), platinum (Pt), zinc (Zn), silicon (Si), magnesium (Mg), or any combination thereof. For example, the lithium-affinity metal may include gold (Au), silver (Ag), platinum (Pt), zinc (Zn), silicon (Si), magnesium (Mg), or any combination thereof. For example, the metal salt (122) may include silver (Ag). For example, when the metal salt (122) includes silver (Ag), silver (Ag) and lithium form a Li-Ag alloy during charge and discharge, and the formed Li-Ag alloy acts as a nucleation site, thereby inducing uniform deposition of lithium.
[0072] According to one embodiment, the metal salt may include AgNO3, AuCl3, Mg(NO3)2, Zn(NO3)2, etc.
[0073] According to one embodiment, the content of the metal salt may be 1 to 50 parts by weight relative to 100 parts by weight of the cross-linked structure. For example, the content of the metal salt may be 1 to 40 parts by weight, 1 to 30 parts by weight, 1 to 20 parts by weight, 5 to 50 parts by weight, or 5 to 20 parts by weight relative to 100 parts by weight of the cross-linked structure.
[0074] According to one embodiment, the polymer electrolyte further comprises a lithium salt. Here, the content of the lithium salt is 20 to 100 parts by weight based on 100 parts by weight of the cross-linked structure. For example, when the polymer electrolyte comprises a lithium salt, the polymer electrolyte may be a polymer solid electrolyte comprising a lithium salt. For example, when the polymer electrolyte comprises a lithium salt and an organic solvent, the polymer electrolyte may be a polymer gel electrolyte comprising a lithium salt as a liquid electrolyte.
[0075] The polymer solid electrolyte may include, for example, a lithium salt and the cross-linked structure described above. The polymer solid electrolyte may be, for example, a polymer electrolyte that does not include a liquid electrolyte.
[0076] According to one embodiment, the polymer solid electrolyte may further include a third polymer in addition to the cross-linked structure described above. For example, the third polymer may be polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polymethyl methacrylate (PMMA), poly(methylmethacrylate), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylatlacene-2-sulfonate 9,10-diphenylanthracene-2-sulfonate, DPASLi +) or a combination thereof, but is not limited thereto, and any polymer electrolyte used in the relevant technical field is possible.
[0077] For example, the lithium salt can be any one that can be used as a lithium salt in the relevant technical field. The lithium salt can be, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(x and y are each 1 to 20), LiCl, LiI or a mixture thereof.
[0078] According to one embodiment, the polymer electrolyte may further comprise a liquid electrolyte. For example, the polymer electrolyte may be a gel polymer electrolyte comprising the cross-linked structure described above and a liquid electrolyte. For example, the liquid electrolyte may be disposed within a cross-linked network formed by the cross-linked structure.
[0079] According to one embodiment, the liquid electrolyte may include an organic solvent or an ionic liquid. For example, the liquid electrolyte may further include a lithium salt. For example, the liquid electrolyte may be an ionic liquid, an organic solvent, a mixture of a lithium salt and an organic solvent, a mixture of an ionic liquid and an organic solvent, or a mixture of a lithium salt, an ionic liquid, and an organic solvent.
[0080] According to one embodiment, the organic solvent may be any organic solvent used in the art. The organic solvent may include, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0081] For example, the ionic liquid refers to a salt or a molten salt in a liquid state at room temperature that has a melting point below room temperature and is composed only of ions. The ionic liquid may comprise at least one selected from compounds comprising, for example, a) at least one cation selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof, and b) at least one anion selected from BF4-, PF6-, AsF6-, SbF6-, AlCl4-, HSO4-, ClO4-, CH3SO3-, CF3CO2-, Cl-, Br-, I-, BF4-, SO4-, CF3SO3-, (FSO2)2N-, (C2F5SO2)2N-, (C2F5SO2)(CF3SO2)N-, and (CF3SO2)2N-.
[0082] For example, the polymer solid electrolyte may be impregnated into an electrolyte solution within a lithium battery to form a gel polymer electrolyte. The gel polymer electrolyte may further include inorganic particles.
[0083] According to one embodiment, the polymer electrolyte may further include a solid electrolyte.
[0084] The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof.
[0085] Solid electrolytes are, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes are Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≤x<1, O≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12(M = Te, Nb, or Zr, x is an integer from 1 to 10) is one or more selected from. The solid electrolyte is manufactured by a sintering method, etc. For example, the oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0 <a<2) 중에서 선택된 가넷계(Garnet-type) 고체전해질이다.
[0086] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in a range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zn 1-x GeO4("LISICON", 0≤x<1), Li 3+y PO 4-x N x( "LIPON", 0 <x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4("ThioLISICON"), Li2O-Al2O3-TiO2-P2O 5(An inorganic solid electrolyte prepared by adding "LATP") etc. to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof can be used as a sulfide solid electrolyte. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S -P2S5-Z m S n (0 <m<10, 0<n<10, Z=Ge, Zn 또는 Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; 및 Li2S-SiS2-Li p MO q (0 <p<10, 0<q<10, M=P, Si, Ge, B, Al, Ga 또는 In)을 포함한다. 이와 관련하여, 황화물계 고체전해질 재료는 황화물계 고체전해질 물질의 원료 시작 물질(예를 들면, Li2S, P2S5, 등)을 용융 담금질법(melt quenching method), 기계적 밀링법 등에 의해 처리함으로써 제조될 수 있다. 또한, 소성(calcinations) 공정이 상기 처리 후에 수행될 수 있다. 황화물계 고체전해질은 비정질이거나, 결정질이거나, 이들이 혼합된 상태일 수 있다.
[0087] According to one embodiment, the thickness of the polymer electrolyte (120) may be 4 to 20 μm.
[0088] According to one embodiment, the polymer electrolyte is useful as a polymer electrolyte of a lithium battery. For example, the lithium battery may be a non-anode lithium metal battery.
[0089] For example, the lithium battery may include a lithium-air battery, a lithium-ion battery, a lithium polymer battery, a lithium sulfur battery, etc., all of which use lithium electrodes.
[0090] The polymer electrolyte (120) according to one embodiment can be used as a protective film of an electrode current collector (110) or as an electrolyte. The polymer electrolyte has excellent interfacial properties and a high lithium transfer constant, and thus can have excellent lithium ion transfer capability.
[0091] According to one embodiment, the electrode structure (10) may further include an interlayer disposed between the electrode collector (110) and the polymer electrolyte (120).
[0092] According to one embodiment, the interlayer may be directly disposed on, for example, one or both surfaces of the electrode current collector (110). Accordingly, no other layer may be disposed between the electrode current collector (110) and the interlayer. By directly disposing the interlayer (not shown) on one or both surfaces of the electrode current collector (110), the bonding force between the electrode current collector (110) and the polymer electrolyte (120) may be further enhanced.
[0093] The thickness of the intermediate layer (not shown) is, for example, 30% or less of the thickness of the negative electrode current collector (110). The thickness of the intermediate layer (not shown) is, for example, 0.01 to 30%, 0.1 to 30%, 0.5 to 30%, 1 to 25%, 1 to 20%, 1 to 15%, 1 to 10%, 1 to 5%, or 1 to 3% of the thickness of the negative electrode current collector (210). The thickness of the intermediate layer (not shown) is, for example, 10 nm to 5 ㎛, 50 nm to 5 ㎛, 200 nm to 4 ㎛, 500 nm to 3 ㎛, 500 nm to 2 ㎛, 500 nm to 1.5 ㎛, or 700 nm to 1.3 ㎛. By having the above intermediate layer (not shown) with a thickness in this range, the bonding force between the electrode current collector (110) and the polymer electrolyte (120) can be further improved, and an increase in interface resistance can be suppressed.
[0094] For example, the intermediate layer (not shown) may include a binder. By including the binder in the intermediate layer, the bonding strength between the electrode current collector (110) and the polymer electrolyte (120) may be further improved. The binder included in the intermediate layer (not shown) may be, for example, a conductive binder or a non-conductive binder.
[0095] The conductive binder may be, for example, an ion-conducting binder and / or an electron-conducting binder. A binder having both ion-conducting and electron-conducting properties may be classified as either an ion-conducting binder or an electron-conducting binder.
[0096] The ion-conducting binder is, for example, polystyrene sulfonate (PSS), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP, polyvinylidene fluoride-hexafluoropropylene), polyvinyl fluoride (PVF, polyvinylidene fluoride), polymethyl methacrylate (PMMA, poly(methylmethacrylate), polyethylene oxide (PEO, polyethylene oxide), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, and polyacetylene. The ion-conducting binder may include a polar functional group. Examples of the ion-conducting binder including a polar functional group include Nafion, Aquibion, etc. (Aquivion), Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), lithium 9,10-diphenylatlacene-2-sulfonate 9,10-diphenylanthracene-2-sulfonate, DPASLi+), etc.Electronically conductive binders include, for example, polyacetylene, polythiophene, polypyrrole, poly(p-phenylene), poly(phenylenevinylene), poly(phenylenesulfide), polyaniline, etc. The intermediate layer may be a conductive layer comprising, for example, a conductive polymer.
[0097] The binder included in the intermediate layer may be, for example, a fluorinated binder. The fluorinated binder included in the intermediate layer may be, for example, polyvinylidene fluoride (PVDF). The intermediate layer may be disposed on the negative electrode current collector (210) in a dry or wet manner, for example. The intermediate layer may be, for example, a binding layer including a binder.
[0098] The intermediate layer may additionally include, for example, a carbon-based conductive material. By including the carbon-based conductive material, the intermediate layer may be, for example, a conductive layer. The intermediate layer may be, for example, a conductive layer including a binder and a carbon-based conductive material.
[0099] The intermediate layer may be disposed on the electrode current collector (110) in a dry manner, for example, by deposition such as CVD or PVD. The intermediate layer may be disposed on the electrode current collector (110) in a wet manner, for example, by spin coating, dip coating, or the like. The intermediate layer may be disposed on the electrode current collector (110) by, for example, depositing a carbon-based conductive material on the electrode current collector (110) by deposition. The dry-coated intermediate layer may be made of a carbon-based conductive material and may not include a binder. Alternatively, the intermediate layer may be disposed on the electrode current collector (110) by, for example, coating a composition including a carbon-based conductive material, a binder, and a solvent on the surface of the negative electrode current collector and drying it. The intermediate layer may have a single-layer structure or a multi-layer structure including a plurality of layers.
[0100]
[0101] [Method for manufacturing electrode structure (10)]
[0102] A method for manufacturing an electrode structure (10) according to an embodiment will be described.
[0103] A method for manufacturing an electrode structure (10) according to one embodiment may include the steps of: preparing an electrode current collector (110); preparing a polymer electrolyte forming composition including a first polymer, a second polymer, a metal salt, and an initiator; applying the polymer electrolyte forming composition onto the electrode current collector (110); and forming an electrode structure (10) including a polymer electrolyte (120) from the electrode current collector (110) to which the polymer electrolyte forming composition is applied. For example, the electrode current collector (110) may include nickel (Ni) or chromium (Cr), the first polymer may include a polymer including a polar functional group, and the second polymer may include a polyurethane-based polymer.
[0104] For example, even if the electrode current collector (110) includes nickel (Ni) or chromium (Cr), and a polymer electrolyte forming composition including a metal salt is applied on the electrode current collector (110), a radical scavenger (e.g., Cu) from the electrode current collector (110) 2+ ) may not be formed. Accordingly, the polymerization reaction of the first polymer and the second polymer included in the composition for forming a polymer electrolyte is easily performed, so that the polymer electrolyte (120) is formed more easily, and the adhesive force between the polymer electrolyte (120) and the electrode current collector (110) is further improved, so that the durability of the electrode current collector (10) can be further improved. In addition, since the polymer electrolyte (120) includes a metal salt (122), lithium can be more uniformly deposited on the electrode current collector (110).
[0105] For example, the description of the electrode current collector (110), the first polymer, the second polymer, the metal salt, and the polymer electrolyte (120) refers to the description described above.
[0106] According to one embodiment, the composition for forming a polymer electrolyte includes a first polymer, a second polymer, a metal salt, and an initiator, and a polymer electrolyte can be formed from the composition for forming a polymer electrolyte. For example, the polymer electrolyte can be formed through a polymerization reaction of the first polymer and the second polymer included in the composition for forming a polymer electrolyte.
[0107] The polymerization reaction can be carried out by applying heat or irradiating light, such as UV light. Here, heat or light can be applied within a range that does not negatively affect the lithium metal electrode. For example, the polymerization reaction can be carried out by applying heat.
[0108] The above polymerization reaction may be a copolymerization reaction, a crosslinking reaction or a grafting reaction.
[0109] When heat is applied or light such as UV is irradiated to perform a polymerization reaction, the heat or light may be applied within a range that does not negatively affect the electrode current collector (110).
[0110] According to another embodiment, it is also possible to perform a polymerization reaction of the first polymer and the second polymer by irradiating light at room temperature (25°C). A photopolymerization initiator is used during the crosslinking reaction by irradiating light. The photopolymerization initiator may be any compound that can form radicals by light such as ultraviolet rays, without limitation on its composition. As the photopolymerization initiator, for example, one or more selected from the group consisting of 2-hydroxy2-methyl-1-phenyl-propan-1-one (HMPP), benzoin ether, dialkyl acetophenone, hydroxyl alkylketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone may be used. The above acylphosphine may be, for example, 2,4,6-trimethyl-benzoyl-trimethyl phosphine oxide.
[0111] According to another embodiment, the polymer electrolyte-forming composition may be heated to initiate a polymerization reaction between the first polymer and the second polymer. A thermal polymerization initiator is used during the crosslinking reaction using heat. Any photopolymerization initiator capable of forming radicals by heat may be used without limitation in its composition.
[0112] As the above thermal polymerization initiator, one or more selected from the group of initiators consisting of a persulfate initiator, an azo initiator, a peroxide initiator, and ascorbic acid can be used. Specifically, examples of persulfate-based initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8), and examples of azo-based initiators include 2, 2-azobis-(2-amidinopropane) dihydrochloride, 2, 2-azobis-(N, N-dimethylene)isobutyramidine dihydrochloride, 2-(carbamoylazo)isobutylonitril, 2, Examples of the peroxide initiator include 2-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), etc., and t-butyl peroxide, dicumyl peroxide, t-amyl peroxide, etc.
[0113] According to one embodiment, the step of forming a polymer electrolyte on the electrode current collector may include heating the polymer electrolyte forming composition applied on the electrode current collector at 60 to 180°C for 1 to 15 hours and vacuum drying. For example, the heating of the electrode current collector applied with the polymer electrolyte forming composition may be performed for 1 to 12 hours, 1 to 10 hours, 2 to 15 hours, 4 to 15 hours, or 4 to 12 hours. For example, the heating of the electrode current collector applied with the polymer electrolyte forming composition may be performed at 80 to 180°C, 100 to 180°C, 60 to 160°C, 60 to 140°C, or 80 to 140°C.
[0114] According to one embodiment, the polymer forming composition may further include the lithium salt described above.
[0115] According to one embodiment, the polymer-forming composition may further comprise the organic solvent described above. For example, when the polymer-forming composition further comprises an organic solvent, a gel polymer electrolyte comprising the organic solvent may be formed from the polymer-forming composition. For example, the polymer-forming composition may further comprise the liquid electrolyte described above.
[0116] For descriptions of the above lithium salt, the above organic solvent and the above liquid electrolyte, refer to the above-described description.
[0117]
[0118] [Lithium battery]
[0119] A lithium battery according to one embodiment may include the electrode structure described above. By including the electrode structure described above, the lithium battery can simultaneously provide improved capacity and excellent room temperature and high temperature lifespan characteristics.
[0120] Lithium batteries may be, but are not limited to, lithium primary batteries, lithium secondary batteries, lithium-sulfur batteries, lithium-air batteries, etc., and any lithium battery used in the relevant technical field may be used.
[0121] Lithium batteries are manufactured by, for example, the following exemplary methods, but are not necessarily limited to these methods and are adjusted according to required conditions.
[0122] Referring to FIGS. 2 and 3, a lithium battery according to an embodiment will be described in detail. FIG. 3 shows a state in which a lithium metal layer (125) is deposited as the lithium battery of FIG. 2 is charged.
[0123] A lithium battery (100) according to one embodiment may include the electrode structure (10) described above. For example, the lithium battery (100) may include the electrode structure (10) described above and a positive electrode disposed in the electrode structure (10).
[0124] According to one embodiment, the polymer electrolyte (120) included in the lithium battery (100) may have a solid, liquid or gel form.
[0125] A lithium battery (100) according to an embodiment may include, as shown in FIG. 2, an electrode structure (10) including a negative electrode current collector (110); and a polymer electrolyte (120) disposed on the negative electrode current collector (110); and a positive electrode (150) disposed on the polymer electrolyte (120). In this case, the negative electrode may include a negative electrode current collector (110) free of a negative electrode active material layer, and the positive electrode (250) may include a positive electrode current collector (140) and a positive electrode active material layer (130) disposed on the positive electrode current collector (140).
[0126] According to one embodiment, a lithium battery (100) may further include a lithium metal layer (125) formed between a negative electrode current collector (110) and a polymer electrolyte (120), as shown in FIG. 3. For example, the lithium metal layer (125) may include a lithium alloy generated by a reaction between lithium ions included in the polymer electrolyte (120) and metal cations included in a metal salt included in the polymer electrolyte (120) during a process of charging the lithium battery (100). In this case, the lithium alloy may function as a nucleation site for lithium ions to be deposited. For example, the lithium metal layer (125) may dissociate into lithium ions and metal cations during a discharge process, so that the thickness of the lithium metal layer (125) may be reduced. For example, when the lithium battery (100) is completely discharged, the lithium battery (100) may not include the lithium metal layer (125).
[0127] According to one embodiment, a lithium battery (100) including the above-described electrode structure (10) may further include a protective layer (not shown) disposed between the negative electrode and the polymer electrolyte.
[0128] Referring to FIG. 1, the protective layer (not shown) can be formed between the negative electrode collector (110) and the polymer electrolyte (120).
[0129] Referring to FIG. 2, the protective layer (not shown) may be formed between the negative electrode current collector (110) and the polymer electrolyte (120). For example, the protective layer (not shown) may be formed between the lithium metal layer (125) and the polymer electrolyte (120).
[0130]
[0131] [Cathode current collector]
[0132] According to one embodiment, the electrode current collector (110) included in the electrode structure (10) may be a negative current collector. For example, the electrode structure (10) may include an electrode current collector (110) which is a negative current collector and a polymer electrolyte (120) disposed on the electrode current collector (110).
[0133] According to one embodiment, the negative electrode current collector may be free of a negative electrode active material layer before charge and discharge. For example, the negative electrode current collector may be free of a lithium metal layer before charge and discharge. For example, in the case of a lithium battery in which the negative electrode current collector is free of a negative electrode active material layer or a lithium metal layer before charge and discharge, dendrite formation can be prevented, thereby improving life characteristics.
[0134] For a description of the negative electrode collector, refer to the description of the electrode collector (110) described above.
[0135]
[0136] [Polymer electrolyte (120)]
[0137] For example, the polymer electrolyte (120) refers to the description of the polymer electrolyte (120) included in the electrode structure (10) described above.
[0138] According to another embodiment, the polymer electrolyte (120) may further include a nonwoven fabric. The nonwoven fabric may serve to support at least one selected from lithium metal and lithium alloys precipitated during the charging process. For example, the nonwoven fabric may be omitted. For example, if the negative electrode current collector is of the mesh type, the nonwoven fabric may not be used.
[0139] The above nonwoven fabric may have a porosity of 10 to 90%, for example, 10 to 80%, for example, 10 to 50 vol%, for example, 25 to 50 vol%, and an average pore size of 0.1 to 10 µm, for example, 0.01 to 8 µm, for example, 0.1 to 1.0 µm. The average pore size represents the diameter when the pore shape is spherical, and represents the major axis length when the pore shape is non-spherical.
[0140] According to one embodiment, the nonwoven fabric may include one or more nonwoven fabrics selected from cellulose, polyester (e.g., polyethylene terephthalate (PET), polyetherimide, polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyamide, polyacetal, polycarbonate, polyimide, polyetherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, nylon, and polyparaphenylenebenzobisoxazole.
[0141]
[0142] [Cathode: Lithium metal layer]
[0143] Referring to FIG. 3, the lithium battery (100) may further include a lithium metal layer (125) disposed between the electrode current collector (110) and the polymer electrolyte (120). For example, the lithium metal layer (125) may include lithium metal or a lithium alloy. For example, the lithium metal layer (125) may be a lithium electrodeposition layer.
[0144] For example, the lithium metal layer (125) may be generated when lithium ions included in the polymer electrolyte (120) are electrodeposited on the electrode current collector (110) as the lithium battery (100) is charged. For example, the lithium metal layer (125) may be generated when lithium ions included in the polymer electrolyte (120) and metal ions of a metal salt included in the polymer electrolyte (120) form a lithium alloy and are electrodeposited on the electrode current collector (110) as the lithium battery (100) is charged.
[0145] For example, the lithium metal layer (125) may include a lithium alloy and a lithium metal. For example, the lithium alloy included in the lithium metal layer (125) may weaken the reactivity of the lithium metal, thereby effectively preventing a side reaction between the lithium metal layer (125) and the polymer electrolyte (120). In addition, the lithium alloy included in the lithium metal layer (125) may function as a nucleation site for lithium electrodeposition, thereby allowing lithium ions to be more uniformly electrodeposited. In addition, the lithium metal layer (125) has excellent electrical conductivity, so that the internal resistance of the lithium battery (100) including the lithium metal layer (125) may be reduced. Accordingly, the lithium battery (100) including the lithium metal layer (125) may have improved not only life characteristics but also charge and discharge efficiency.
[0146] According to one embodiment, the lithium metal layer (125) may include, for example, plated lithium or a lithium alloy. The lithium metal layer (125) may be a lithium electrodeposited layer. For example, the lithium alloy may be an alloy of lithium ions and metal ions included in the above-described metal salt, and the metal ions may include the above-described lithium-compatible metal. In this case, the lithium alloy may be an alloy of lithium and the lithium-compatible metal. For example, when the lithium-compatible metal is silver (Ag), the lithium alloy may include a Li-Ag alloy.
[0147] According to one embodiment, the lithium metal layer (125) may not include a carbon-based negative electrode active material. Accordingly, the lithium metal layer (125) may be formed of a metal-based negative electrode active material.
[0148] For example, the thickness of the lithium metal layer (125) may be, for example, 0.1 ㎛ to 100 ㎛, 0.1 ㎛ to 80 ㎛, 1 ㎛ to 80 ㎛, or 10 ㎛ to 80 ㎛, but is not necessarily limited to this range and may be adjusted according to the required shape, capacity, etc. of the lithium battery. If the thickness of the lithium metal layer (125) increases excessively, the structural stability of the lithium battery may deteriorate and side reactions may increase. If the thickness of the lithium metal layer (125) is excessively small, the energy density of the lithium metal battery may decrease.
[0149]
[0150] [anode]
[0151] As shown in FIGS. 2 and 3, a positive electrode active material layer (130) is disposed on a positive electrode current collector (140) to form a positive electrode (150). For example, a positive electrode active material layer (130) may be disposed on an electrode structure (10) including a polymer electrolyte (120), and a positive electrode current collector (140) may be disposed on the positive electrode active material layer (130). More specifically, a positive electrode active material layer (130) may be disposed on a polymer electrolyte (120) in an electrode structure (10), and a positive electrode current collector (140) may be disposed on the positive electrode active material layer (130).
[0152]
[0153] [Anode: Anode current collector]
[0154] Referring to FIGS. 2 and 3, the positive electrode (150) includes a positive electrode current collector (140). For example, the positive electrode (150) can be prepared by forming the positive electrode active material layer (130) on the positive electrode current collector (140).
[0155] For example, the positive electrode current collector (140) may include indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
[0156] According to one embodiment, the positive electrode collector (140) may include aluminum (Al).
[0157] According to one embodiment, the positive electrode current collector (140) may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. Since the base film includes a thermoplastic polymer, the base film may be liquefied when a short circuit occurs, thereby suppressing a rapid increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The metal layer can act as an electrochemical fuse and be cut off in case of overcurrent to prevent a short circuit. The limit current and the maximum current can be controlled by adjusting the thickness of the metal layer. The metal layer can be plated or deposited on the base film. When the thickness of the metal layer is reduced, the limit current and / or the maximum current of the positive electrode current collector (140) decrease, so that the stability of the lithium battery in case of a short circuit can be improved. A lead tab can be added on the metal layer for connection to the outside. The lead tab can be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, etc. During welding, the base film and / or the metal layer melt, so that the metal layer can be electrically connected to the lead tab. In order to make the welding of the metal layer and the lead tab more secure, a metal chip can be added between the metal layer and the lead tab.The metal piece may be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, etc. The metal piece may be, for example, aluminum foil, copper foil, SUS foil, etc. After the metal piece is placed on the metal layer, the lead tab may be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece may melt, so that the metal layer or the metal layer / metal piece laminate may be electrically connected to the lead tab. A metal chip and / or a lead tab may be added to a portion of the metal layer. The base film may have a thickness of, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. When the base film has a thickness in this range, the weight of the positive electrode current collector can be more effectively reduced. The melting point of the base film may be, for example, 100 to 300°C, 100 to 250°C or less, or 100 to 200°C. Since the base film has a melting point within this range, the base film can be easily combined with the lead tab during the welding process by melting. To improve the adhesion between the base film and the metal layer, a surface treatment such as corona treatment may be performed on the base film. The thickness of the metal layer may be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to 1 μm. Since the metal layer has a thickness within this range, the stability of the electrode assembly can be secured while maintaining conductivity. The thickness of the metal piece may be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness within this range, the connection between the metal layer and the lead tab can be performed more easily. By having this structure, the positive electrode current collector (140) can reduce the weight of the electrode and consequently improve the energy density.
[0158]
[0159] [Anode: Anode active material layer]
[0160] The above positive electrode active material layer (130) may include a positive electrode active material, a conductive material, and a binder.
[0161] For example, the cathode active material may be at least one of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof, and a specific example thereof is Li a A 1-b B 1 b D 1 2 (in the above formula, 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B 1 b O 2-c D 1 c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B 1 b O 4-c D 1 c (In the above formula, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B 1 c D 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Cob B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c D α (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 α (In the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 2 (in the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Lia CoG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (in the above formula, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Any compound represented by the chemical formula Fe2(PO4)3(0 ≤ f ≤ 2); LiFePO4 can be used:
[0162] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; B 1 is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, Ga, Si, W, Mo, Cu, Zn, Ti, boron (B), rare earth elements or a combination thereof; D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F 1 is F, S, P, Cl, Br or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I is Cr, V, Fe, Sc, Y or a combination thereof; J may be V, Cr, Mn, Co, Ni, Cu or a combination thereof.
[0163] For example, the positive electrode active material may include a lithium transition metal oxide containing nickel and another transition metal. In the lithium transition metal oxide containing nickel and another transition metal, the content of nickel may be 60 mol% or more, for example, 75 mol% or more, for example, 80 mol% or more, for example, 85 mol% or more, for example, 90 mol% or more, based on the total mole number of transition metals.
[0164] For example, the lithium transition metal oxide may be a compound represented by the following chemical formula 3:
[0165] <Chemical Formula 3>
[0166] Li a Ni x Co y M z O 2-b A b
[0167] In chemical formula 3, 1.0≤a≤1.2, 0≤b≤0.2, 0.6≤x<1, 0≤y≤0.3, 0 <z≤0.3, x+y+z=1, M은 망간(Mn), 바나듐(V), 마그네슘(Mg), 갈륨(Ga), 실리콘(Si), 텅스텐(W), 몰리브덴(Mo), 철(Fe), 크롬(Cr), 구리(Cu), 아연(Zn), 티타늄(Ti), 알루미늄(Al) 및 보론(B)으로 이루어진 군으로부터 선택된 하나 이상이고,
[0168] A is F, S, Cl, Br or a combination thereof.
[0169] For example, in chemical formula 3, 0.7≤x<1, 0 <y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.3, 0<z≤0.3; 0.8≤x<1, 0<y≤0.2, 0<z≤0.2; 0.83≤x<0.97, 0<y≤0.15, 0<z≤0.15; 또는 0.85≤x<0.95, 0<y≤0.1, 0<z≤0.1일 수 있다.
[0170] For example, the lithium transition metal oxide may be at least one of the compounds represented by the following chemical formulae 3-1 and 3-2:
[0171] <Chemical Formula 3-1>
[0172] LiNi x Co y Mn z O2
[0173] In Chemical Formula 3-1, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이고,
[0174] <Chemical Formula 3-2>
[0175] LiNi x Co y Al z O2
[0176] In Chemical Formula 3-2, 0.6≤x≤0.95, 0 <y≤0.2, 0<z≤0.1이다. 예를 들어, 0.7≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.8≤x≤0.95, 0<y≤0.3, 0<z≤0.3이다. 예를 들어, 0.82≤x≤0.95, 0<y≤0.15, 0<z≤0.15이다. 예를 들어, 0.85≤x≤0.95, 0<y≤0.1, 0<z≤0.1이다.
[0177] For example, lithium transition metal oxide is LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.88 Co 0.08 Mn 0.04 O2, LiNi 0.8 Co 0.15 Mn 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.88 Co 0.1 Mn 0.02 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.2 O2 or LiNi 0.88 Co 0.1 Al 0.02 It could be O2.
[0178] For example, the above-mentioned positive electrode active material may be used as one having a coating layer on the surface of the lithium transition metal oxide, or may be used by mixing the lithium transition metal oxide and a lithium transition metal oxide having a coating layer.
[0179] For example, the coating layer may include a coating element compound of an oxide, a hydroxide, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element.
[0180] For example, the compound forming the coating layer may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or mixtures thereof. The coating layer forming process may use any coating method as long as it can coat the lithium transition metal oxide with the coating elements by a method (e.g., spray coating, dipping, etc.) that does not adversely affect the properties of the positive electrode active material. Since this is well understood by those working in the relevant field, a detailed description thereof will be omitted.
[0181] Carbon black, graphite particles, etc. may be used as the above-mentioned conductive material, but are not limited thereto, and any conductive material that can be used in the relevant technical field may be used.
[0182] As the above binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene and mixtures thereof, or styrene butadiene rubber polymers may be used, but are not limited thereto, and any binder that can be used in the relevant technical field may be used.
[0183]
[0184] [Separator]
[0185] A lithium battery according to an embodiment may further include a separator (not shown).
[0186] Specific examples of the above separator include polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof, and mixed multilayer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and a polypropylene / polyethylene / polypropylene three-layer separator may be used.
[0187] According to one embodiment, the battery case including the lithium battery may be cylindrical, square, thin-film, etc. For example, the lithium battery may be a large-scale thin-film battery. The lithium battery may be a lithium ion battery.
[0188] According to one implementation example, the lithium battery (100) may include, for example, a lithium air battery, a lithium sulfur battery, etc.
[0189] According to one embodiment, the lithium battery (100) can be used in electric vehicles (EVs) due to its excellent lifespan and high-rate characteristics. For example, it can be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, it can be used in fields requiring large amounts of power storage. For example, it can be used in electric bicycles, power tools, etc.
[0190] When stacking multiple lithium batteries (100) according to an embodiment, a gel-type electrolyte may be placed between the positive electrode and the liquid-impermeable ion-conductive composite membrane. The gel-type electrolyte may include, for example, a VDF-HFP copolymer, a lithium salt, and a solvent.
[0191] Referring to FIG. 4, a lithium battery (1) according to one embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). The positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). A polymer electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing the lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0192] For example, a polymer electrolyte including a positive electrode (3), a negative electrode (2), and a separator (4) is wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). A liquid electrolyte is injected into the battery case (5) and sealed with a cap assembly (6), thereby completing a lithium battery (1). The battery case (5) is cylindrical, but is not necessarily limited to this shape, and may be, for example, square, thin-film, etc.
[0193] Referring to FIG. 5, a lithium battery (1) according to one embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). A separator (4) is disposed between the positive electrode (3) and the negative electrode (2), and the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding a current formed in the battery structure (7) to the outside may be included. The above-described polymer electrolyte is injected into the battery case (5) and sealed to complete the lithium battery (1).
[0194] For example, after a polymer electrolyte including a separator (4) is placed between a positive electrode (3) and a negative electrode (2), the positive electrode (3), the negative electrode (2), and the separator (4) are wound or folded to form a battery structure (7). The formed battery structure (7) is accommodated in a battery case (5). An electrode tab (8) that serves as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. A liquid electrolyte may be injected into the battery case (5) and sealed to complete the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin film shape, etc.
[0195] Referring to FIG. 6, a lithium battery (1) according to an embodiment includes a positive electrode (3), the above-described negative electrode (2), and a separator (4). The above-described polymer electrolyte including the separator (4) is disposed between the positive electrode (3) and the negative electrode (2), thereby forming a battery structure. The battery structure (7) is stacked in a bi-cell structure and then accommodated in a battery case (5). An electrode tab (8) serving as an electrical path for guiding the current formed in the battery structure (7) to the outside may be included. A liquid electrolyte is injected into the battery case (5) and sealed, thereby completing the lithium battery (1). The battery case (5) is not necessarily limited to a square shape, but may be, for example, a cylindrical shape, a thin-film shape, etc.
[0196] A pouch-type lithium battery corresponds to the lithium batteries of FIGS. 4 to 6, each of which uses a pouch as a battery case. The pouch-type lithium battery includes one or more battery structures. A polymer electrolyte is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are laminated in a bi-cell structure, then impregnated with a liquid electrolyte, and accommodated and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the drawings, a polymer electrolyte including the above-described positive electrode, negative electrode, and separator may be simply laminated and accommodated in a pouch in the form of an electrode assembly, or may be wound or folded into a jelly-roll-shaped electrode assembly and then accommodated in a pouch. Subsequently, a liquid electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0197] Lithium batteries are used in electric vehicles (EVs) due to their excellent cycle life and high-rate characteristics. For example, they are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). They are also used in applications requiring large amounts of power storage, such as electric bicycles and power tools.
[0198] Lithium batteries are stacked in multiple layers to form a battery module, and the multiple battery modules form a battery pack. Such a battery pack can be used in any device requiring high capacity and high output. For example, it can be used in laptops, smartphones, electric vehicles, etc. The battery module includes, for example, multiple batteries and a frame that holds them. The battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. The multiple battery packs are controlled by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0199] The following examples and comparative examples are provided for further details. However, the examples are provided for illustrative purposes only and are not intended to be limiting.
[0200]
[0201] Manufacturing Example 1: Manufacturing of an electrode structure
[0202] A nickel current collector was prepared. A polymer electrolyte forming composition was prepared by dissolving 0.625 g of poly(ethylene glycol) diacrylate (PEGDA), 1.125 g of polyurethane, 1.17 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), 0.75 g of silver nitrate (AgNO3), and 0.002 g of t-amyl peroxide as a thermal initiator in 9.0 g of dimethylformamide (DMF). The polymer electrolyte forming composition was cast onto the nickel current collector using a doctor blade. Thereafter, an electrode structure was manufactured by crosslinking and drying in a vacuum oven at 110°C for more than 6 hours.
[0203]
[0204] Manufacturing Examples 2 to 5 and Comparative Manufacturing Examples 1 to 2
[0205] A polymer electrolyte was prepared in the same manner as in Example 1, except that the type of electrode current collector, type and content of metal salt were changed as shown in Table 1 below.
[0206] Type of electrode current collectorType of metal saltContent of metal saltManufacturing example 1 Nickel metal AgNO3 0.75 gManufacturing example 2 Copper metal with nickel coating on the entire surface AgNO3 0.75 gManufacturing example 3 Chromium metal AgNO3 0.75 gManufacturing example 4 Copper metal with nickel coating on the entire surface Mg(NO3)2 0.75 gManufacturing example 5 Copper metal with nickel coating on the entire surface AgNO3 0.5 gComparative manufacturing example 1 Copper metal AgNO3 0.75 gComparative manufacturing example 2 Copper metal with nickel coating on the entire surface--
[0207] Evaluation Example 1: Telephone Rate Evaluation
[0208] Regarding the polymer electrolytes and compositions for forming polymer electrolytes manufactured according to Manufacturing Examples 1 to 5 and Comparative Manufacturing Examples 1 to 2 1 H-NMR was measured. NMR was measured with a 600 MHz spectrometer, and the method for preparing a sample for NMR measurement is as follows. 0.03 g of the composition for forming a polymer electrolyte and 0.0004 g of a reference substance (p-Xylene, para-xylene) are dissolved in 1 mL of an NMR solvent (DMSO-d6, dimethyl sulfoxide-d6). The prepared polymer electrolyte is placed in a circular hole with a diameter of 16 mm in 1 mL of an NMR solvent (DMSO-d6, dimethyl sulfoxide-d6), and 0.0004 g of a reference substance (p-Xylene, para-xylene) is added and dissolved.
[0209] Polymer electrolytes and compositions for forming polymer electrolytes prepared according to Manufacturing Examples 1 to 5 and Comparative Manufacturing Examples 1 to 2 1 Among the results of H-NMR measurement, the area of hydrogen corresponding to the acrylate group of PEGDA (A peak with chemical shift of 6.3 ppm, B peak with 6.2 ppm, and C peak with 5.9 ppm) was calculated compared to the area of the reference substance, p-Xylene, when it was 1000, and is shown in Table 2 below. In addition, the conversion rate was calculated according to the following Equation 1 and is shown in Table 2 below.
[0210] [Formula 1]
[0211] Conversion rate (%) = [1-1 / 3 ((A peak area of polymer electrolyte / A peak area of polymer electrolyte forming composition) + (B peak area of polymer electrolyte / B peak area of polymer electrolyte forming composition) + (C peak area of polymer electrolyte / C peak area of polymer electrolyte forming composition))] x 100
[0212] Classification A peak area B peak area C peak area Conversion rate (%) Composition for forming polymer electrolyte 143.6 132.0 148.4 - Manufacturing example 12.8 3.0 2.898 Manufacturing example 21.10 20.7 99.5 Manufacturing example 36.15 96.2 95.7 Manufacturing example 44.3 3.11 898.1 Manufacturing example 51.10 10.7 99.6 Comparative manufacturing example 162.2 63.4 64.15 5.2 Comparative manufacturing example 258.7 59.2 67.3 56.3
[0213] Referring to this, it was confirmed that the polymer electrolytes of Manufacturing Examples 1 to 5 had superior conversion rates compared to Comparative Manufacturing Example 1. From this, it was confirmed that most of the polymer electrolytes according to Manufacturing Examples 1 to 5 participated in the polymerization reaction without unreacted polymers.
[0214]
[0215] Example 1: Manufacturing of lithium battery (pouch cell)
[0216] LiNi 0.6 Co 0.2 Al 0.2 O2, a conductive agent (Super-P; Timcal Ltd.), a binder, and N-methylpyrrolidone were mixed to obtain a cathode composition. LiNi in the cathode composition 0.6 Co 0.2 Al 0.2 The mixing weight ratio of O2, the challenge agent, and the binder was 97.5:1.5:1.
[0217] The above positive electrode composition was coated on top of aluminum foil (thickness: about 15 μm) and dried in a vacuum at about 110°C to manufacture a positive electrode.
[0218] A lithium metal battery (pouch cell) was manufactured by stacking the positive electrode, polyolefin-based separator, liquid electrolyte, and polymer electrolyte of the electrode structure according to Manufacturing Example 1 so that they were adjacent to each other according to the above process.
[0219] Examples 2 to 5 and Comparative Examples 1 to 2: Manufacturing of lithium batteries (pouch cells)
[0220] A lithium battery was manufactured in the same manner as in Example 1, except that the type of polymer electrolyte used was changed as shown in Table 3 below.
[0221]
[0222] Evaluation Example 2: Charge / Discharge Characteristics
[0223] Lithium batteries (coin cells) manufactured according to Examples 1 to 5 and Comparative Examples 1 to 2 were charged at a constant current of 0.1 C at 45°C until the voltage reached 4.30 V (vs. Li), and then cut-off was achieved at a current of 0.05 C while maintaining 4.30 V in constant voltage mode. Subsequently, discharge was performed at a constant current of 0.1 C until the voltage reached 3.6 V (vs. Li) (formation stage, 1st cycle). This charge-discharge process was repeated two more times to complete the formation process.
[0224] The lithium battery that had undergone the above-described Mars step was charged at a constant current of 0.2 C in a voltage range of 3.6 to 4.3 V vs. lithium metal at 45°C, and then cut-off was achieved at a current rate of 0.05 C while maintaining 4.30 V in constant voltage mode. Subsequently, constant current discharge was performed at 0.5 C until a cut-off voltage of 3.6 V was reached. The above-described charge and discharge process was repeated a total of 200 times.
[0225] In all of the above charge / discharge cycles, a 5-minute pause was provided after each charge / discharge cycle. Here, the capacity retention rate at the 200th cycle is defined by Equation 2 below.
[0226] [Formula 2]
[0227] Capacity retention rate (%) = [200 th Discharge capacity in cycle / 1 st Discharge capacity in a cycle
[0228] ]x 100
[0229] 200 th The capacity retention rate and discharge capacity during the cycle were measured and are listed in Table 3 below.
[0230] Polymer electrolyte High temperature evaluation (45℃) Capacity (mAh) Capacity retention rate (%) Example 1 Manufacturing example 115.375 Example 2 Manufacturing example 216.977 Example 3 Manufacturing example 315.172 Example 4 Manufacturing example 414.365 Example 5 Manufacturing example 514.767 Comparative example 1 Comparative manufacturing example 111.355 Comparative example 2 Comparative manufacturing example 210.551
[0231]
[0232] Referring to Table 3, Examples 1 to 5, which each include an electrode structure according to Manufacturing Examples 1 to 5, had superior room temperature capacity characteristics and capacity retention characteristics compared to Comparative Examples 1 to 2, which each include an electrode structure according to Comparative Manufacturing Examples 1 to 2.
[0233] While the above has been described with reference to drawings and examples, these are merely exemplary, and those skilled in the art will appreciate that various modifications and equivalent implementations are possible. Accordingly, the scope of protection of the present invention should be defined by the appended claims.
[0234] [Explanation of symbols]
[0235] 100: Lithium battery
[0236] 110: Cathode collector 120: Polymer electrolyte
[0237] 130: Cathode active material layer 140: Cathode current collector
[0238] 150: Anode 125: Metal layer
Claims
1. Electrode collector; and A polymer electrolyte disposed on the electrode collector; The above electrode collector contains nickel (Ni), chromium (Cr) or zinc (Zn), The polymer electrolyte comprises a crosslinked structure including repeating units (A) derived from a first polymer and repeating units (B) derived from a second polymer, and a metal salt, The first polymer comprises a polymer containing a polar functional group, An electrode structure in which the second polymer comprises a polyurethane-based polymer.
2. In paragraph 1, An electrode structure in which the surface of the electrode collector contains nickel (Ni) or chromium (Cr) and does not contain copper (Cu) metal.
3. In paragraph 1, The above electrode collector comprises a base film and a metal layer disposed on one or both sides of the base film, The above base film comprises a metal or polymer, Among the above base films, the metal includes indium (In), copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li) or an alloy thereof. Among the above base films, the polymer includes polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI) or a combination thereof, The above metal layer contains nickel (Ni) or chromium (Cr), or The above electrode collector is an electrode structure made of nickel (Ni) or chromium (Cr).
4. In paragraph 1, An electrode structure wherein the metal salt comprises gold (Au), silver (Ag), platinum (Pt), zinc (Zn), silicon (Si), magnesium (Mg), or any combination thereof.
5. In paragraph 1, The above metal salt is AgNO 3, An electrode structure containing AuCl3, Mg(NO3)2, Zn(NO3)2, etc.
6. In paragraph 1, An electrode structure in which the content of the metal salt is 1 to 50 parts by weight based on 100 parts by weight of the cross-linked structure.
7. In paragraph 1, An electrode structure, wherein the polymer including a polar functional group included in the first polymer comprises polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene glycol diacrylate, polyethylene glycol methyl ether acrylate, polymethyl methacrylate, polyethyl methacrylate, polycaprolactone, polyethylene carbonate, polypropylene carbonate, or any combination thereof.
8. In paragraph 1, An electrode structure wherein the first polymer further comprises one or more terminal double bonds.
9. In paragraph 1, An electrode structure, wherein the first polymer comprises polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene glycol diacrylate, polyethylene glycol methyl ether acrylate, or any combination thereof.
10. In paragraph 1, An electrode structure wherein the second polymer comprises polyurethane, urethane acrylate, urethane methacrylate, perfluoropolyether urethane acrylate, perfluoropolyether urethane methacrylate, or any combination thereof.
11. In paragraph 1, The content of the repeating unit (A) derived from the first polymer is 50 to 90 wt% with respect to the total weight of the crosslinked structure, An electrode structure in which the content of the repeating unit (B) derived from the second polymer is 10 to 50 wt% with respect to the total weight of the crosslinked structure.
12. In paragraph 1, An electrode structure wherein the polymer electrolyte further comprises a lithium salt.
13. In paragraph 12, The above lithium salts are LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 An electrode structure comprising SO2)(x and y are each 1 to 20), LiCl, LiI or a mixture thereof.
14. In paragraph 1, The above polymer electrolyte is a polymer electrolyte further comprising an organic solvent or an ionic liquid.
15. In paragraph 14, The organic solvent comprises propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether or a mixture thereof, The above ionic liquid contains cations and anions, The above cation includes at least one selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof. The above anion is BF4 - , PF6 - , AsF6 - , SbF6 - , AlCl4 - , HSO4 - , ClO4 - , CH3SO3 - , CF3CO2 - , Cl - , Br - , I - , BF4 - , SO4 - , CF3SO3 - , (FSO2)2N - , (C2F5SO2)2N - , (C2F5SO2)(CF3SO2)N - , and (CF3SO2)2N - An electrode structure comprising at least one selected from among:
16. In paragraph 1, An electrode structure wherein the thickness of the polymer electrolyte is 4 to 20 μm.
17. Step of preparing the electrode collector; A step of preparing a composition for forming a polymer electrolyte comprising a first polymer, a second polymer, a metal salt, and an initiator; A step of applying the polymer electrolyte forming composition on the electrode current collector; and A step of applying a polymer electrolyte on an electrode current collector to which the composition for forming the polymer electrolyte is applied, The above electrode collector contains nickel (Ni) or chromium (Cr), The first polymer comprises a polymer containing a polar functional group, A method for manufacturing an electrode structure, wherein the second polymer comprises a polyurethane polymer.
18. In paragraph 17, A method for manufacturing an electrode structure, wherein the step of forming a polymer electrolyte on the electrode current collector comprises heating a polymer electrolyte forming composition applied on the electrode current collector at 60 to 180°C for 1 to 15 hours and vacuum drying to form a polymer electrolyte on the electrode current collector.
19. In paragraph 17, The above initiator includes a thermal initiator, A method for manufacturing an electrode structure, wherein the thermal initiator comprises at least one selected from the group of initiators consisting of a persulfate-based initiator, an azo-based initiator, a peroxide-based initiator, and ascorbic acid.
20. A lithium battery comprising an electrode structure according to claims 1 to 16.
Citation Information
Patent Citations
Method for manufacturing a secondary lithium ion battery using a polymer electrolyte
KR1020000045100A
Polymeric gel electrolyte and lithium batteryemploying the same
KR1020020083117A
Composite polymer electrolytes having differentmorphology for lithium rechargeable battery and methodfor preparing the same
KR1020040092188A
Composite polymer electrolytes including single-ionconductor for lithium rechargeable battery and methodfor preparing the same
KR1020040092189A
Process for preparing lithium polymer secondary batteries employing gel polymerelectrolyte
KR1020120006730A