Method for manufacturing ferroelectric materials through plasma-enhanced chemical vapor deposition-based ferroelectric crystal structure induction
By using controlled Ar radicals in plasma chemical vapor deposition to form orthorhombic phases in hafnium zirconium oxide thin films, the method addresses the challenge of low-temperature damage and enables the production of semiconductor devices with ferroelectric properties, such as negative capacitance transistors, with enhanced electrical performance and flexibility.
Patent Information
- Application Number
- PCT/KR2024/003898
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional plasma chemical vapor deposition methods damage thin film layers due to high energy plasma movement, preventing the formation of ferroelectric crystal structures at low temperatures and thus limiting the production of semiconductor devices with ferroelectric properties.
The method involves preparing a substrate with a thin film of ferroelectric material, such as hafnium zirconium oxide, and exposing it to controlled Ar radicals using plasma chemical vapor deposition to form an orthorhombic phase with minimal damage, allowing for the creation of ferroelectric crystal structures even at low temperatures.
This approach enables the formation of ferroelectric orthorhombic phases with preserved crystal structure and properties, facilitating the production of semiconductor devices like negative capacitance transistors with improved electrical characteristics and flexibility in device design.
Smart Images

Figure KR2024003898_03102024_PF_FP_ABST
Abstract
Description
A method for manufacturing ferroelectric materials by inducing ferroelectric crystal structures using plasma chemical vapor deposition.
[0001] The present invention relates to a method for inducing a ferroelectric crystal structure, and more particularly, to a method for inducing a ferroelectric material to exhibit ferroelectricity by changing the crystal structure of the material at a low temperature using a plasma chemical vapor deposition method.
[0002]
[0003] Ferroelectric materials are materials that exhibit spontaneous polarization even without an external electric field. A transistor utilizing these ferroelectric materials is the negative capacitance field-effect transistor (NCFET).
[0004] In the literature, Ferroelectricity Enhancement in Hf0.5Zr0.5O2 Based Tri-Layer Capacitors at Low-Temperature (350 °C) Annealing Process, reported in IEEE Electron Device Letters, vol. 42, no. 6, pp. 812-815, June 2021, a capacitor was fabricated by forming HZO having an orthorhombic phase, which has ferroelectricity, using rapid thermal annealing equipment (RTA) at a low temperature of 350 °C.
[0005] In addition, in the literature of A highly CMOS compatible hafnia-based ferroelectric diode reported in Nat Commun 11, 1391 (2020) as a prior art2, a diode having ferroelectric properties was fabricated by forming HZO having an orthorhombic phase, which is a ferroelectric phase, using rapid thermal annealing equipment (RTA) at a low temperature of 400°C.
[0006] However, in the case of prior art 1, a capacitor was made by forming an orthorhombic phase with ferroelectricity using RTA at a low temperature of 350°C, but a transistor using this was failed to be made.
[0007] In addition, in the case of prior art 2, a ferroelectric diode was implemented by forming an orthorhombic phase exhibiting ferroelectricity using RTA at a low temperature of 400°C, but, as in prior art 1, the production of a transistor using this failed.
[0008] Therefore, even if the prior art implemented a ferroelectric capacitor or diode by forming an orthorhombic phase that exhibits ferroelectricity at low temperatures, it had a limitation in that it could not be used to create a semiconductor device.
[0009] Meanwhile, plasma-enhanced chemical vapor deposition (PECVD) offers the advantage of low-temperature processing due to its synthesis via plasma. However, conventional PECVD processes suffer from the drawback that the plasma, which travels along an electric field and acquires significant energy, can damage the thin film layer. This prevents the formation of the ferroelectric crystal structure during the low-temperature process and damages the thin film. Consequently, it has limitations in that it cannot fully demonstrate the semiconductor properties.
[0010]
[0011] (Patent Document 1) KR 10-2022-0107226 A
[0012]
[0013] The technical problem to be achieved by the present invention is to form an orthorhombic phase, a crystal structure that exhibits ferroelectricity even at low temperatures, by contacting an HZO thin film with Ar radicals generated through plasma using a plasma chemical vapor deposition method, and to provide a semiconductor device manufactured using such a ferroelectric.
[0014] The technical problems to be solved by the present invention are not limited to the technical problems mentioned above, and other technical problems not mentioned can be clearly understood by a person having ordinary skill in the technical field to which the present invention belongs from the description below.
[0015]
[0016] In order to achieve the above technical task, one embodiment of the present invention provides a method for manufacturing a ferroelectric material, including the steps of: preparing a substrate; depositing a ferroelectric material thin film on the substrate through sputtering; moving Ar radicals to the ferroelectric material thin film using plasma; and forming a ferroelectric crystal structure by bringing the ferroelectric material thin film into contact with the Ar radicals.
[0017] In an embodiment of the present invention, the ferroelectric material may be characterized as hafnium zirconium oxide (HZO).
[0018] In an embodiment of the present invention, it may be characterized in that Ar radicals whose flow is controlled through plasma increase the reactivity of oxygen in the hafnium zirconium oxide thin film, thereby forming a ferroelectric orthorhombic phase.
[0019] In an embodiment of the present invention, the substrate may be characterized as being a Si substrate.
[0020] In an embodiment of the present invention, the step of moving Ar radicals to the HZO thin film using the plasma may be characterized by including a step of converting Ar into Ar radicals using a plasma generating device and a step of controlling the flow of the Ar radicals using the plasma to prevent collision with the ferroelectric material thin film.
[0021] In an embodiment of the present invention, the flow of the Ar radicals may be characterized in that the Ar radicals move by diffusion along the quartz tube.
[0022] In an embodiment of the present invention, the step of moving Ar radicals to the ferroelectric material thin film using the plasma may be characterized in that it is performed at a temperature of 300°C to 500°C.
[0023] In an embodiment of the present invention, the step of moving Ar radicals to the ferroelectric material thin film using the plasma is 5.0 E -2 5.0 E 0 It can be characterized as being performed under pressure.
[0024]
[0025] In order to achieve the above technical task, another embodiment of the present invention provides a ferroelectric manufactured according to the above manufacturing method.
[0026]
[0027] In order to achieve the above technical problem, another embodiment of the present invention provides a negative capacitance transistor characterized by including: a substrate; a ferroelectric material thin film positioned on the substrate and exhibiting a ferroelectric crystal structure according to the manufacturing method of claim 1; an oxide insulator layer positioned on the ferroelectric material thin film; a channel semiconductor layer positioned on the oxide insulator layer; and a source electrode and a drain electrode positioned on the oxide insulator layer and spaced apart from each other with the channel semiconductor layer interposed therebetween.
[0028] In an embodiment of the present invention, the ferroelectric material thin film may be characterized in that the HZO thin film is a hafnium zirconium oxide (HZO) thin film.
[0029] In an embodiment of the present invention, the HZO thin film may be characterized by exhibiting ferroelectricity through plasma chemical vapor deposition.
[0030] In an embodiment of the present invention, the oxide insulator may be characterized by being selected from the group including HfO2, ZrO2, or Al2O3.
[0031] In an embodiment of the present invention, the channel semiconductor may be characterized by being selected from the group including IGZO, MoS2, WS2, WSe2, or Te.
[0032] In an embodiment of the present invention, the source electrode and the drain electrode may be characterized in that they are selected from the group including Ti, Au, Mo, Ag, or Al.
[0033]
[0034] According to an embodiment of the present invention, by controlling the movement of Ar radicals using plasma rather than an electric field, strong collisions between Ar radicals and HZO thin films can be prevented, thereby minimizing damage to the HZO thin film. When Ar radicals come into contact with the surface of the HZO thin film, the HZO thin film is transformed into an orthorhombic phase exhibiting ferroelectricity. The HZO thin film with minimized damage can be fully utilized as a ferroelectric formed using plasma-enhanced chemical vapor deposition.
[0035] Applying ferroelectric HZO thin films as the ferroelectric layer of transistors allows for the observation of previously unattainable low-temperature electrical characteristics and the demonstration of transistor characteristics with NC (Negative Capacitance) effects. Furthermore, the low-temperature process enables flexible devices and top gate applications, and the fabrication of transistors with diverse performance and effects utilizing various electrode and channel materials.
[0036] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.
[0037]
[0038] Figure 1 is an image showing a typical plasma enhanced chemical vapor deposition (PECVD) process.
[0039] Figure 2 is an image showing the plasma enhanced chemical vapor deposition (PECVD) process in the present invention.
[0040] Figure 3 is a structural diagram of a NCFET (Negative Capacitance Field-Effect Transistor).
[0041] Figure 4 is a graph of (a) voltage-polarization and (b) voltage-current at 300°C based on plasma enhanced chemical vapor deposition (PECVD).
[0042] Figure 5 is a voltage-polarization graph at temperatures of 300°C and 400°C and at 700°C RTA annealing based on plasma-enhanced chemical vapor deposition (PECVD).
[0043] Figure 6 is a graph showing the implementation of an NCFET using a HZO thin film exhibiting an orthorhombic phase.
[0044] Figure 7 is a graph showing (a) implementation of NCFET, (b) and (c) SS values in the forward and reverse states.
[0045]
[0046] Hereinafter, the present invention will be described with reference to the attached drawings. However, the present invention can be implemented in various different forms and is therefore not limited to the embodiments described herein. In the drawings, irrelevant parts have been omitted for clarity of description, and similar parts have been designated with similar reference numerals throughout the specification.
[0047] Throughout the specification, when a part is said to be "connected (connected, contacted, or coupled)" to another part, this includes not only cases where it is "directly connected," but also cases where it is "indirectly connected" with another part in between. Furthermore, when a part is said to "include" a component, this does not exclude other components, but rather implies that it may include other components, unless otherwise specifically stated.
[0048] The terminology used herein is merely used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprises" or "has" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0049] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.
[0050]
[0051] A method for manufacturing a ferroelectric according to an embodiment of the present invention is described.
[0052] A method for manufacturing a ferroelectric film according to one embodiment of the present invention may include the steps of: preparing a substrate; depositing a ferroelectric material thin film on the substrate through sputtering; moving Ar radicals to the ferroelectric material thin film using plasma; and forming a ferroelectric crystal structure by contacting the ferroelectric material thin film with the Ar radicals.
[0053] First, a substrate is prepared. The substrate may be a Si substrate. The Si substrate is cleaned and the SiO2 formed on the surface is removed.
[0054] The following is a step of depositing a thin film of a ferroelectric material on the substrate by sputtering. The ferroelectric material may be hafnium zirconium oxide (HZO). The HZO thin film is deposited on a cleaned Si substrate by sputtering equipment.
[0055] The following is a step of moving Ar radicals to the ferroelectric material thin film using plasma. When moving Ar radicals to the HZO thin film using the plasma, the step may include a step of converting Ar into Ar radicals using a plasma generating device and a step of controlling the flow of the Ar radicals using plasma to prevent collision with the HZO thin film.
[0056] For this movement, a temperature of 300℃ to 500℃ and 5.0 E -2 5.0 E 0 It is preferable to perform it under pressure.
[0057]
[0058] Figure 1 is an image showing a general plasma enhanced chemical vapor deposition (PECVD) process, and Figure 2 is an image showing a plasma enhanced chemical vapor deposition (PECVD) process in the present invention.
[0059] Referring to Figures 1 and 2, the conventional PECVD process is structured so that the plasma and heat sources are located in the same location, and the gas flow rate through the plasma cannot be controlled, which inevitably leads to damage to the thin film in general cases. However, the current PECVD structure has the plasma and heat sources (heaters) separated, minimizing damage to the thin film.
[0060] Accordingly, a Si substrate on which a thin film layer has been deposited is placed in a quartz tube in the heater section of a PECVD device with a structure in which the plasma generator and heater are far apart. The interior of the quartz tube of the PECVD device is then placed under a high vacuum. The plasma generator is then used to convert Ar into Ar radicals, and the flow of the Ar radicals generated using the plasma is slowly controlled to prevent collisions with excessively high energy. Consequently, damage to the thin film can be minimized.
[0061] The flow of the above Ar radicals can be carried out by diffusion along the quartz tube. The Ar radicals are carried by diffusion along the quartz tube in the direction in which the pump draws in the gas.
[0062] The final step is the step where the ferroelectric material thin film comes into contact with the Ar radicals to form a ferroelectric crystal structure. In the case of the HZO thin film, the step where the ferroelectric orthorhombic phase is formed is where Ar radicals whose flow is controlled through plasma increase the reactivity of oxygen in the HZO thin film, thereby forming the ferroelectric orthorhombic phase.
[0063] The slowly moving Ar radicals, controlled by the plasma flow, can modify the crystal structure of the HZO thin film by making oxygen more reactive without damaging the surface of the HZO thin film. The low-temperature thermal energy provided by the heater and the energy of the Ar radicals serve to replace the thermal energy at high temperatures.
[0064] Typically, ferroelectric materials exhibit ferroelectricity only in the orthorhombic phase, which is formed at high temperatures. Therefore, forming the orthorhombic phase requires significant energy and heat. However, the high-temperature process imposes limitations on the substrate, electrodes, channel materials, and semiconductor structures created using the substrate. In PECVD, plasma can be used as a substitute for heat energy. While conventional PECVD uses an electric field to move ions, in the present invention, the ions are moved within the quartz by the pressure difference generated by the pump. These moved ions then contact the thin film layer of the material through diffusion, and the thin film layer receives sufficient heat energy from the heater, enabling the formation of the orthorhombic phase, which exhibits ferroelectricity even at low temperatures. Since the Ar ions move by diffusion, not by an electric field, the thin film layer is not significantly damaged, allowing it to maintain its crystal structure. The orthorhombic phase of the ferroelectric thus formed exhibits polarization that is not significantly different from that observed at high temperatures.
[0065]
[0066] Hereinafter, a ferroelectric according to another embodiment of the present invention will be described.
[0067] A ferroelectric according to one embodiment of the present invention can be manufactured according to the above manufacturing method.
[0068] The above ferroelectric material may include an HZO thin film that exhibits an orthorhombic phase of ferroelectricity in the case of an HZO thin film.
[0069]
[0070] Below, a negative capacitance transistor according to another embodiment of the present invention is described.
[0071] FIG. 3 is a structural diagram of a NCFET (Negative Capacitance Field-Effect Transistor). Referring to FIG. 3, a negative capacitance transistor according to an embodiment of the present invention may include a substrate (100), a ferroelectric material thin film (200) positioned on the substrate (100) and exhibiting a ferroelectric crystal structure according to the manufacturing method, an oxide insulator layer (300) positioned on the ferroelectric material thin film (200), a channel semiconductor layer (400) positioned on the oxide insulator layer (300), and a source electrode and a drain electrode (500) positioned on the oxide insulator layer (300) and spaced apart from each other with the channel semiconductor layer (400) interposed therebetween.
[0072] The above ferroelectric material thin film may be a hafnium zirconium oxide (HZO) thin film.
[0073] An HZO thin film is deposited on the substrate by sputtering, and formed into an orthorhombic phase with ferroelectricity by PECVD. The oxide insulator layer on the HZO thin film may be hafnium oxide (HfO2). The channel semiconductor layer positioned on the oxide insulator layer may be IGZO (Indium-Gallium-Zinc-Oxide).
[0074] After the above channel semiconductor layer is formed, the shape can be completed through a photolithography process and an etching process.
[0075] And, a transistor can be manufactured by depositing a source electrode and a drain electrode that are positioned on the oxide insulator layer and are spaced apart from each other with the channel semiconductor layer interposed therebetween through a lift-off process and an E-beam evaporator.
[0076] The above oxide insulator may be selected from the group including, but not limited to, HfO2, ZrO2 or Al2O3.
[0077] The above channel semiconductor may be selected from the group including, but not limited to, IGZO, MoS2, WS2, WSe2, or Te.
[0078] The above source electrode and drain electrode may be selected from the group including, but not limited to, Ti, Au, Mo, Ag or Al.
[0079]
[0080] According to embodiments of the present invention, a thin film with minimal damage can be formed into a ferroelectric film using PECVD and can be fully utilized, thereby exhibiting the characteristics of a transistor with the NC (Negative Capacitance) effect. Furthermore, the low-temperature process enables utilization as a flexible device and top gate, and the manufacture of transistors with diverse performance and effects utilizing various electrode and channel materials.
[0081]
[0082] Hereinafter, manufacturing examples and experimental examples of the present invention will be described in detail.
[0083]
[0084] <Manufacturing Example 1: Ferroelectric>
[0085]
[0086] The Si substrate is cleaned using ultrasonication for 10 minutes each in the order of acetone, IPA (isopropyl alcohol), and DI water. The SiO2 formed on the surface of the cleaned Si substrate is removed using buffered oxide etchant (BOE).
[0087] A thin film layer of HZO is deposited on a cleaned Si substrate using a sputtering device.
[0088] In a PECVD device with a structure where the plasma generator and heater are located far apart, a Si substrate on which a thin film layer has been deposited is placed in a quartz tube in the heater section. The inside of the quartz tube of the PECVD device is created into a high vacuum.
[0089] Ar is converted into Ar radicals using a plasma generator. The flow of Ar radicals generated using plasma is slowly controlled to prevent collisions with the HZO thin film at excessively high energy.
[0090] Slowly moving Ar radicals make oxygen more reactive without damaging the surface of the HZO thin film, thereby forming an orthorhombic crystal structure. At this time, the Ar radicals move by diffusion along the quartz tube in the direction in which the pump draws gas.
[0091]
[0092] <Manufacturing Example 2: Negative Capacitance Transistor>
[0093]
[0094] Through the process of the above Manufacturing Example 1, HZO deposited on a Si substrate is formed into an orthorhombic phase with ferroelectricity through PECVD. An oxide insulator layer and a channel semiconductor layer are each deposited and etched into the desired shape through a photolithography process and an etching process. The source electrode and drain electrode are deposited through a lift-off process and an E-beam evaporator to complete the transistor fabrication.
[0095]
[0096] <Experimental Example>
[0097]
[0098] Figure 4 is a graph of (a) voltage-polarization and (b) voltage-current at 300°C based on plasma enhanced chemical vapor deposition (PECVD).
[0099] Referring to Fig. 4, the PE curve was measured based on the orthorhombic phase of the ferroelectric material formed using PECVD, and the electrical characteristics were confirmed by fabricating a TFT based on this. The measurement results obtained an anticlockwise value indicating a NCFET and an SS < 60 mV / dec value. It was confirmed that the orthorhombic phase with ferroelectric characteristics can be formed at low temperatures. It can be confirmed that the polarization value has a non-zero constant value up and down when V is 0. This value is Pr, or Remanent Polarization, which is an inherent value of a ferroelectric, and having this value means that it is a ferroelectric. Therefore, it can be confirmed that the HZO material has ferroelectric characteristics by having an orthorhombic phase.
[0100]
[0101] Figure 5 is a voltage-polarization graph at temperatures of 300°C and 400°C and at 700°C RTA annealing based on plasma-enhanced chemical vapor deposition (PECVD).
[0102] Referring to Figure 5, by comparing the general RTA 700℃ condition with the Ar plasma and 300℃ and 400℃ conditions, it can be confirmed that even at a low temperature of 300℃, using Ar plasma can have a polarization value similar to that of using RTA.
[0103]
[0104] Figure 6 is a graph showing the implementation of an NCFET using a HZO thin film exhibiting an orthorhombic phase.
[0105] Referring to Figure 6, Forward and Reverse represent the direction of current according to voltage. Generally, Forward and Reverse appear in opposite directions, which is called Clockwise, which appears in general n-type semiconductors, and when the opposite, Anti-Clockwise, appears in n-type semiconductors, the Negative Capacitance (NC) effect appears. In p-type semiconductors, it appears in the opposite direction to the n-type semiconductor. Therefore, it can be confirmed that an NCFET exhibiting the NC effect has been implemented.
[0106]
[0107] Figure 7 is a graph showing (a) implementation of NCFET, (b) and (c) SS values in the forward and reverse states.
[0108] Referring to Fig. 7, the SS (subthreshold swing) can be calculated from the graph in Fig. 6, and it can be confirmed that the SS value is less than 60 mV / dec. This is because the minimum SS value at room temperature is limited to 60 mV / dec in general Si-based semiconductors due to the thermal limit of carriers in the Maxwell-Boltzmann distribution. Therefore, the fact that an SS value of less than 60 mV / dec is obtained confirms that the NC effect is exhibited beyond the theoretical value.
[0109]
[0110] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will readily appreciate that the present invention can be readily modified into other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.
[0111] The scope of the present invention is indicated by the claims described below, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.
[0112]
[0113] [Explanation of symbols]
[0114] 100: Substrate
[0115] 200: HZO thin film
[0116] 300: Oxide insulator layer
[0117] 400: Channel semiconductor layer
[0118] 500: Source electrode and drain electrode
Claims
1. Step for preparing the substrate; A step of depositing a thin film of ferroelectric material on the substrate by sputtering; A step of moving Ar radicals to the ferroelectric material thin film using plasma; and A method for manufacturing a ferroelectric material, comprising: a step of contacting the ferroelectric material thin film with the Ar radicals to form a ferroelectric crystal structure.
2. In paragraph 1, A method for manufacturing a ferroelectric material, characterized in that the ferroelectric material is hafnium zirconium oxide (HZO).
3. In paragraph 2, A method for manufacturing a ferroelectric film, characterized in that Ar radicals whose flow is controlled through plasma increase the reactivity of oxygen in the hafnium zirconium oxide thin film, thereby forming a ferroelectric orthorhombic phase.
4. In paragraph 1, A method for manufacturing a ferroelectric material, characterized in that the substrate is a Si substrate.
5. In paragraph 1, The step of moving Ar radicals to the ferroelectric material thin film using the above plasma is: A step of converting Ar into Ar radicals using a plasma generator; and A method for manufacturing a ferroelectric material, characterized by including a step of controlling the flow of Ar radicals using plasma to prevent collision with a thin film of ferroelectric material.
6. In paragraph 5, A method for manufacturing a ferroelectric material, characterized in that the flow of the Ar radicals moves by diffusion along a quartz tube.
7. In paragraph 1, A method for manufacturing a ferroelectric material, characterized in that the step of moving Ar radicals to the ferroelectric material thin film using the plasma is performed at a temperature of 300°C to 500°C.
8. In paragraph 1, The step of moving Ar radicals to the ferroelectric material thin film using the above plasma is 5.0 E -2 5.0 E 0 A method for manufacturing a ferroelectric material, characterized in that it is performed under pressure.
9. A ferroelectric manufactured according to the manufacturing method of paragraph 1.
10. Substrate; A thin film of a ferroelectric material positioned on the substrate and exhibiting a ferroelectric crystal structure according to the manufacturing method of claim 1; An oxide insulating layer positioned on the above ferroelectric material thin film; a channel semiconductor layer positioned on the oxide insulator layer; and A negative capacitance transistor characterized by comprising a source electrode and a drain electrode positioned on the oxide insulator layer and spaced apart from each other with a channel semiconductor layer interposed therebetween.
11. In paragraph 10, A negative capacitance transistor, characterized in that the above ferroelectric material thin film is a hafnium zirconium oxide (HZO) thin film.
12. In paragraph 10, A negative capacitance transistor characterized in that the above ferroelectric material thin film exhibits ferroelectricity by a plasma chemical vapor deposition method.
13. In paragraph 10, The above oxide insulator is, A negative capacitance transistor characterized by being selected from the group comprising HfO2, ZrO2 or Al2O3.
14. In paragraph 10, The above channel semiconductor is, A negative capacitance transistor characterized by being selected from the group comprising IGZO, MoS2, WS2, WSe2, or Te.
15. In paragraph 10, A negative capacitance transistor, characterized in that the source electrode and the drain electrode are selected from the group comprising Ti, Au, Mo, Ag or Al.
Citation Information
Patent Citations
A method for forming a thin complete high-permittivity dielectric layer
KR1020070067079A
Method of forming a dielectric layer in semiconductor memory device
KR1020090019139A
Semiconductor device
KR1020170060247A
Holographic waveguide with aberration compensation element and display apparatus including the same
KR1020220039524A
Connection structure embedded substrate
KR1020230003864A