A method of synthesizing quantum dots
The synthesis of quantum dots using copper and indium precursors with hexamethyldisilathiane addresses the limitations of conventional NIR systems by enhancing PLQE and emission range, achieving efficient near-infrared emission beyond 900 nm.
Patent Information
- Application Number
- PCT/SG2024/050189
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional near-infrared (NIR) quantum dots, such as lead-chalcogenide and indium arsenide, face regulatory concerns and toxicity issues, while CuInS2 dots have limited emission beyond 900 nm with low photoluminescence quantum efficiency (PLQE) at longer wavelengths.
A method of synthesizing quantum dots by heating copper and indium precursors with a C6-C14 thiol in the presence of a solvent, followed by adding hexamethyldisilathiane, which enhances reactivity and nucleation/growth pathways, resulting in copper indium dichalcogenide quantum dots with improved PLQE at higher wavelengths.
The method produces quantum dots with a peak emission wavelength of 900-1100 nm and increased PLQE, overcoming the limitations of conventional NIR systems by achieving higher efficiency and broader emission range with improved size distribution and emissive site density.
Smart Images

Figure SG2024050189_03102024_PF_FP_ABST
Abstract
Description
[0001] A METHOD OF SYNTHESIZING QUANTUM DOTS
[0002] References to Related Application
[0003] This application claims priority to Singapore application number 10202300890P filed with the Intellectual Property Office of Singapore on 31 March 2023, the contents of which are hereby incorporated by reference.
[0004] Technical Field
[0005] The present invention generally relates to a method of synthesizing quantum dots. The method further relates to quantum dots obtained by or obtainable by the method as described herein and a device comprising the quantum dots.
[0006] Background Art
[0007] Colloidal quantum dots (QDs) exhibiting size-tuneable photoluminescence (PL), high PL quantum efficiency (PLQE) and solution processability have been widely implemented in photovoltaic, lighting and display devices. In particular, nearinfrared (NIR) emitting QDs have attracted immense interest in the past decade due to emerging NIR lighting applications, such as depth-sensing, robotics, biomedical imaging, night vision, surveillance, and optical communications.
[0008] Conventional NIR systems are primarily based on lead-chalcogenide (PbX, X = S or Se) QDs. However, the inclusion of Pb, which is regulated by the Restriction of Hazardous Substances (RoHS) directive, raises concerns about the suitability of Pb- containing QDs for consumer electronic products.
[0009] Another convention NIR system comprises InAs QDs, which have a bulk bandgap of 0.4 eV and are also capable of NIR emissions. Although no regulations are in place to control the use of As, InAs QDs are generally considered toxic and hence undesirable.
[0010] Another convention NIR system comprises CuInS2 QDs, which are Pb- and As-free alternatives with markedly lower toxicity levels, lower synthesis costs and emission tuneable up to about 1000 nm. The conventional CuInS2 QDs have a PL of up to 868 nm. However, the conventional NIR-emitting CuInS2 QDs have so far been limited to an emission of less than 900 nm with PLQE dropping drastically to less than 30% at longer wavelengths.
[0011] Accordingly, there is a need for quantum dots and an NIR system that ameliorate one or more disadvantages mentioned above. Summary
[0012] In one aspect, there is provided a method of synthesizing quantum dots, comprising the steps of: a) heating a copper precursor, an indium precursor and a Co-Ci4 thiol in the presence of a solvent to form a solution; and b) adding hexamethyldisilathiane to the solution of the heating step a) to form the quantum dots.
[0013] Advantageously, the present method uses a combination of the C&-C14 thiol and hexamethyldisilathiane to provide sulfur element. The above combination provides an improved reactivity to the synthesis process compared with conventional methods where only one reagent is used to provide sulfur element. This results in a separation of nucleation and growth pathways of the quantum dots, thus contributing to a faster rate of reaction when forming the quantum dots, leading to a narrower size distribution of the quantum dots.
[0014] Further advantageously, the above combination generates a higher density of emissive Cu-deficiency sites in the quantum dots synthesized. This results in an increase in photoluminescence quantum efficiency of the quantum dots at higher wavelengths, such as more than 900 nm.
[0015] In another aspect, there are provided quantum dots comprising a copper indium dichalcogenide, wherein: a) the quantum dots comprise copper element and indium element at a molar ratio in the range of about 0.7: 1 to about 0.9: 1, b) the quantum dots have a mean size in the range of about 3 nm to about 4 nm, and c) the quantum dots have a peak emission wavelength in the range of about 900 nm to about 1100 nm.
[0016] In another aspect, there are provided quantum dots obtained by or obtainable by the method as described herein.
[0017] In another aspect, there is provided a device comprising the quantum dots as described herein.
[0018] Definitions
[0019] The following words and terms used herein shall have the meaning indicated:
[0020] The term “alkane” as used herein includes within its meaning straight chain or branched chain saturated hydrocarbons having from 16 to 20 carbon atoms, c.g., 16, 17, 18, 19 or 20 carbon atoms. For example, the term “alkane” includes, but is not limited to, 1-hcxadccanc, 1-hcptadccanc, 1-octadccanc, 1-nonadccanc, 1-icosanc, and constitutional isomers thereof.
[0021] The term “alkene” as used herein includes within its meaning straight chain or branched chain hydrocarbons having 1 C=C bond and from 16 to 20 carbon atoms, e.g., 16, 17, 18, 19 or 20 carbon atoms. For example, the term “alkene” includes, but is not limited to, 1-hcxadcccnc, 1-hcptadcccnc, 1-octadcccnc, 1-nonadcccnc, 1- cicoscnc, and constitutional isomers thereof.
[0022] The term “thiol” as used herein includes within its meaning hydrocarbons having one or more -SH substituents.
[0023] The word “substantially” does not exclude “completely” e.g. a composition which is “substantially free” from Y may be completely free from Y. Where necessary, the word “substantially” may be omitted from the definition of the invention.
[0024] Unless specified otherwise, the terms "comprising" and "comprise", and grammatical variants thereof, are intended to represent "open" or "inclusive" language such that they include recited elements but also permit inclusion of additional, unrecited elements.
[0025] The term "about" as used herein typically means + / - 5 % of the stated value, more typically + / - 4 % of the stated value, more typically + / - 3 % of the stated value, more typically, + / - 2 % of the stated value, even more typically + / - 1 % of the stated value, and even more typically + / - 0.5 % of the stated value.
[0026] Throughout this disclosure, certain embodiments may be disclosed in a range format. It should be understood that the description in range format is merely for convenience and brevity and should not be construed as an inflexible limitation on the scope of the disclosed ranges. Accordingly, the description of a range should be considered to have specifically disclosed all the possible sub-ranges as well as individual numerical values within that range. For example, description of a range such as from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6 etc., as well as individual numbers within that range, for example, 1, 2, 3, 4, 5, and 6. This applies regardless of the breadth of the range.
[0027] Certain embodiments may also be described broadly and generically herein. Each of the narrower species and subgeneric groupings falling within the generic disclosure also form part of the disclosure. This includes the generic description of the embodiments with a proviso or negative limitation removing any subject matter from the genus, regardless of whether or not the excised material is specifically recited herein. Detailed Disclosure of Embodiments
[0028] Exemplary, non-limiting embodiments of a method of synthesizing quantum dots will now be disclosed.
[0029] The method comprises the steps of: a) heating a copper precursor, an indium precursor and a C / ,-Ci4 thiol in the presence of a solvent to form a solution; b) adding hexamethyldisilathiane to the solution of the heating step a) to form the quantum dots.
[0030] The copper precursor may be selected from Cui, CuBr, CuCl, CuOAc, CuS or combinations thereof. The copper precursor may be Cui.
[0031] The indium precursor may be selected from InE, InBr?, InCh, In(OAc)a, indium (III) acetylacetonate or combinations thereof. The indium precursor may be Inf OAc)?,.
[0032] The C&-C14 thiol may be a CG thiol, a C7 thiol, a Cs thiol, a C9 thiol, a C10 thiol, a C11 thiol, a C12 thiol, a C13 thiol, or a C14 thiol. The CG-CU thiol may be 1 -hexanethiol, 1- heptanethiol, 1 -octanethiol, 1 -nonanethiol, 1 -decanethiol, 1-undecanethiol, 1- dodecanethiol, 1 -tridecanethiol, 1 -tetradecanethiol or a constitutional isomer thereof.
[0033] The solvent may be a C16-C20 alkane or a C16-C20 alkene. The solvent may be a Cis alkene. The solvent may be 1-hexadecane, 1-hexadecene, 1 -heptadecane, 1- heptadecene, 1-octadecane, 1-octadecene, 1-nonadecane, 1-nonadecene, 1-icosane, 1-eicosene or a constitutional isomer thereof.
[0034] The copper precursor and the indium precursor may have a molar ratio in the range of about 1:0.8 to about 1:1.2, about 1: 1 to about 1: 1.2 or about 1:0.8 to about 1:1. The copper precursor and the indium precursor may have a molar ratio of about 1:1.
[0035] The copper precursor and the C6-C14 thiol may have a molar ratio in the range of about 1:100 to about 1:500, about 1:300 to about 1:500 or about 1: 100 to about 1:300. The copper precursor and the CG-CH thiol may have a molar ratio of about 1 :200. The copper precursor and the C6-C14 thiol may have a molar ratio of about 1:400.
[0036] The copper precursor may have a concentration in the range of about 0.01 M to about 0.02 M, about 0.015 M to about 0.02 M or about 0.01 M to about 0.015 M, based on the total volume of the solution. The copper precursor may have a concentration of about 0.015 M based on the total volume of the solution.
[0037] The heating step a) may be undertaken at a temperature in the range of about 100 °C to about 200 °C, about 150 °C to about 200 °C or about 100 °C to about 150 °C.
[0038] The heating step a) may be undertaken in an inert atmosphere. The heating step a) may be undertaken in an argon or nitrogen atmosphere. The heating step a) may be undertaken for a duration in the range of about 10 minutes to about 20 minutes, about 15 minutes to about 20 minutes or about 10 minutes to about 15 minutes.
[0039] The method may further comprise a step al) of treating the copper precursor, the indium precursor, the Ce-Ci4 thiol and the solvent at a reduced pressure before the heating step a). The reduced pressure may be a pressure in the range of about 0 Pa to about 1000 Pa, about 0 Pa to about 100 Pa, about 0 Pa to about 10 Pa or about 0 Pa to about 1 Pa. Therefore, the reduced pressure may be regarded as a vacuum environment.
[0040] The treating step al) may be undertaken at a temperature in the range of about 50 °C to about 100 °C, about 75 °C to about 100 °C or about 50 °C to about 75 °C.
[0041] The treating step al) may be undertaken for a duration in the range of about 0.5 hours to about 2 hours, about 1 hour to about 2 hours or about 0.5 hours to about 1 hour.
[0042] The copper precursor used in the heating step a) and hcxamcthyldisilathianc used in the adding step b) may have a molar ratio in the range of about 1:2 to about 1:6, about 1:4 to about 1:6 or about 1:2 to about 1:4. The copper precursor used in the heating step a) and hexamethyldisilathiane used in the adding step b) may have a molar ratio of about 1:4.
[0043] The adding step b) may be undertaken at a temperature in the range of about 150 °C to about 250 °C, about 200 °C to about 250 °C or about 150 °C to about 200 °C. The adding step b) may be undertaken at a temperature of about 200 °C.
[0044] The adding step b) may be undertaken while the solution of the heating step a) is being heated. Therefore, the temperature of the adding step b) may be increasing during the adding step b). The adding step b) may be undertaken for a short duration such that the temperature of the entire adding step b) is about 200 °C.
[0045] The adding step b) may be undertaken for a duration in the range of about 0.5 seconds to 1 minute, about 5 seconds to about 1 minute, about 10 seconds to about 1 minute, about 0.5 seconds to about 10 seconds or about 0.5 seconds to about 5 seconds.
[0046] The adding step b) may be undertaken in an inert atmosphere. The adding step b) may be undertaken in an argon or nitrogen atmosphere. The adding step b) may be undertaken in an argon glovebox.
[0047] The method may further comprise a step bl) of heating the mixture of step b) after the adding step b).
[0048] The heating step bl) may be undertaken at a temperature in the range of about 200 °C to about 300 °C, about 250 °C to about 300 °C or about 200 °C to about 250 °C. The heating step bl ) may be undertaken at a temperature of about 250 °C. The heating step bl) may be undertaken for a duration in the range of about 10 minutes to about 50 minutes, about 30 minutes to about 50 minutes or about 10 minutes to about 30 minutes.
[0049] The heating step bl) may be undertaken in an inert atmosphere. The heating step bl) may be undertaken in an argon or nitrogen atmosphere. The heating step bl) may be undertaken in an argon glovebox.
[0050] The method may further comprise a step of c) reacting a zinc precursor with the quantum dots after the adding step b).
[0051] Therefore, the method may comprise the steps of: a) heating the copper precursor, the indium precursor and the Cs-Ci4 thiol in the presence of a solvent to form a solution; b) adding hexamethyldisilathiane to the solution of the heating step a) to form the quantum dots; and c) reacting a zinc precursor with the quantum dots of the adding step b).
[0052] During the reacting step c), the zinc precursor may form a shell -like structure that at least partially covers or encapsulates the quantum dots of the adding step b). Accordingly, the quantum dots of the adding step b) may be regarded as a core-like structure after the reacting step c) and the reacting step c) may provide a core-shell structure.
[0053] The zinc precursor may be a zinc salt of a fatty acid. The zinc precursor may be selected from Zn(oleate)2, Zn(stearate)2, Zn(laurate)2, Zn(myristate)2, Zn(palmitate)2 or combinations thereof.
[0054] The copper precursor used in the heating step a) and the zinc precursor used in the reacting step c) may have a molar ratio in the range of about 1 :5 to about 1 : 15, about 1 : 10 to about 1 : 15 or about 1 :5 to about 1 : 10. The copper precursor used in the heating step a) and the zinc precursor used in the reacting step c) may have a molar ratio of about 1: 10.
[0055] The reacting step c) may be undertaken for a duration in the range of about 10 minutes to about 30 minutes, about 20 minutes to about 30 minutes or about 10 minutes to about 20 minutes. The reacting step c) may be undertaken for a duration of about 20 minutes.
[0056] During the reacting step c), the zinc precursor may be added to the mixture of the adding step b) at a constant rate. Therefore, the zinc precursor may be dissolved in the solvent to form a zinc precursor solution, and the zinc precursor solution may be added using a syringe pump. The zinc precursor solution may be added at a rate in the range of about 0.3 mL / minute to about 0.7 mL / minute, about 0.5 mL / minute to about 0.7 mL / minutc or about 0.3 mL / minutc to about 0.5 mL / minutc. The zinc precursor solution may be added at a rate of about 0.5 mL / minutc.
[0057] The reacting step c) may be undertaken at a temperature in the range of about 150 °C to about 250 °C, about 200 °C to about 250 °C or about 150 °C to about 200 °C. The reacting step c) may be undertaken at a temperature of about 200 °C.
[0058] The reacting step c) may be undertaken in an inert atmosphere. The reacting step c) may be undertaken in an argon or nitrogen atmosphere. The reacting step c) may be undertaken in an argon glovebox.
[0059] The method may further comprise a step cl) of isolating the quantum dots after the reacting step c).
[0060] The isolating step cl) may comprise precipitating, centrifuging and / or washing the quantum dots.
[0061] Exemplary, non-limiting embodiments of quantum dots will now be disclosed.
[0062] The quantum dots may comprise a copper indium dichalcogenide. Therefore, the quantum dots may be regarded or used as a semiconductor.
[0063] The quantum dots may comprise copper element and indium element at a molar ratio in the range of about 0.7:1 to about 0.9: 1, about 0.8: 1 to about 0.9: 1 or about 0.7: 1 to about 0.8: 1.
[0064] The quantum dots may have a mean size in the range of about 3 nm to about 4 nm, about 3 nm to about 3.5 nm or about 3.5 nm to about 4 nm.
[0065] The mean size of the quantum dots may have a standard deviation in the range of about 0.5 nm to about 1 nm, about 0.7 nm to about 1 nm or about 0.5 nm to about 0.7 nm.
[0066] The copper indium di ch al cogen ide may be copper indium disulfide.
[0067] The quantum dots may further comprise a zinc chalcogenide shell that at least partially covers or encapsulates the copper indium dichalcogenide. Therefore, the copper indium dichalcogenide may be regarded as a core and the quantum dots may be regarded as having a core / shell structure.
[0068] Therefore, the quantum dots may have a copper indium dichalcogenide / zinc chalcogenide core / shell structure.
[0069] Tn the shell, the zinc chalcogenide may be ZnS, ZnSe, ZnSeS or a combination thereof. Tn one example, the quantum dots are CuTnS2 / ZnS quantum dots.
[0070] The quantum dots may have a peak emission wavelength in the range of about 800 nm to about 1 100 nm, about 900 nm to about 1 100 nm, about 1000 nm to about 1 100 nm, about 800 nm to about 1000 nm or about 800 nm to about 900 nm. The quantum dots may have a photolumincsccncc quantum efficiency of at least about 50%, at least about 55%, at least about 60% or at least about 65% at an emission wavelength of at least about 900 nm.
[0071] Exemplary, non-limiting embodiments of quantum dots will now be disclosed.
[0072] The quantum dots are obtained by or obtainable by the method as described herein. Based on the method as described herein, two types of quantum dots may be obtained. The first type of quantum dots may be obtained by or obtainable by the method after step (b) while the second type of quantum dots may be obtained by or obtainable by the method after step (c). Both types of quantum dots may have photoluminescence, electroluminescence and light emission properties.
[0073] The first and second types of quantum dots may comprise copper element and indium element at a molar ratio in the range of about 0.7 : 1 to about 0.9:1, about 0.8: 1 to about 0.9: 1 or about 0.7: 1 to about 0.8: 1. As the first and second types of quantum dots comprise less copper element compared to indium element, the first and second types of quantum dots comprise copper-related defects or deficiency sites. Advantageously, the first and second types of quantum dots have higher peak emission wavelengths and have a high photolumincsccncc quantum efficiency at higher wavelengths.
[0074] The first type of quantum dots may have a peak emission wavelength in the range of about 800 nm to about 1100 nm, about 900 nm to about 1100 nm, about 1000 nm to about 1100 nm, about 800 nm to about 1000 nm or about 800 nm to about 900 nm.
[0075] The second type of quantum dots may have a higher peak emission wavelength. Accordingly, the second type of quantum dots may have a peak emission wavelength in the range of about 900 nm to about 1100 nm, about 1000 nm to about 1100 nm or about 900 nm to about 1000 nm.
[0076] The first type of quantum dots may have a photoluminescence quantum efficiency of at least about 35%, at least about 40%, at least about 45%, at least about 50%, at least about 55%, at least about 60% or at least about 65% at an emission wavelength of at least about 900 nm.
[0077] The second type of quantum dots may have a higher photoluminescence quantum efficiency. Accordingly, the second type of quantum dots may have a photoluminescence quantum efficiency of at least about 50%, at least about 55%, at least about 60% or at least about 65% at an emission wavelength of at least about 900 nm.
[0078] The second type of quantum dots may have an emission profile with less than about 0.1%, about 0.3%, about 0.5%, about 1% or about 2% of a total emission being at wavelengths below 700 nm. Therefore, the second type of quantum dots may be visually transparent or substantially visually transparent. The second type of quantum dots may have a photolumincsccncc spectrum that has a full width at half-maximum (FWHM) in the range of about 200 nm to about 300 nm, about 250 nm to about 300 nm or about 200 nm to about 250 nm.
[0079] Advantageously, both types of quantum dots are thermally stable. The second type of quantum dots may have a photoluminescence intensity that is at least about 70%, about 75%, about 80% or about 83% maintained after heating at about 80 °C for about 90 minutes.
[0080] The first type of quantum dots may be copper indium dichalcogenide quantum dots such as CuInSi quantum dots. The second type of quantum dots may be copper indium dichalcogcnidc quantum dots further comprising a zinc chalcogenide shell, such as a ZnS shell, a ZnSc shell, a ZnScS shell or a combination thereof. Where the copper indium dichalcogcnidc is CuInS2 and the zinc chalcogenide shell is a ZnS shell, the second type of quantum dots may be regarded as CulnS2 / ZnS quantum dots. The second type of quantum dots may have a core-shell structure or configuration where the copper indium dichalcogenide forms the core and the zinc chalcogenide forms the shell, whereby the zinc chalcogenide shell at least partially covers or encapsulates the copper indium dichalcogenide core.
[0081] Where the quantum dots arc CulnS? quantum dots (with or without the shell), advantageously, the use of hcxamcthyldisilathianc in the method described herein may result in a faster rate of reaction compared with conventional methods where only one reagent is used to provide the sulfur element, leading to an increase in the density of emissive Cu-dcficicncy sites in the quantum dots, thus contributing to the increase in the photolumincsccncc quantum efficiency as compared to quantum dots formed from the conventional methods.
[0082] The first type of quantum dots and the second type of quantum dots may independently have a size in the range of about 0.5 nm to about 8 nm, about 1 nm to about 8 nm, about 2 nm to about 8 nm, about 0.5 nm to about 7, about 0.5 nm to about 6 nm, about 1 nm to about 6 nm or about 2 nm to about 6 nm.
[0083] The first type of quantum dots may have a mean size in the range of about 2 nm to about 3 nm, about 2 nm to about 2.5 nm or about 2.5 nm to about 3 nm.
[0084] The mean size of the first type of quantum dots may have a standard deviation in the range of about 0.5 nm to about 1 nm, about 0.7 nm to about 1 nm or about 0.5 nm to about 0.7 nm.
[0085] The second type of quantum dots may have a mean size in the range of about 3 nm to about 4 nm, about 3 nm to about 3.5 nm or about 3.5 nm to about 4 nm.
[0086] The mean size of the second type of quantum dots may have a standard deviation in the range of about 0.5 nm to about 1 nm, about 0.7 nm to about 1 nm or about 0.5 nm to about 0.7 nm. Both types of the quantum dots may be regarded as non-toxic due to the absence of hazardous elements.
[0087] Exemplary, non-limiting embodiments of a device will now be disclosed.
[0088] The device comprises the quantum dots as described herein. Therefore, the device may be a lighting device. The device may be a light emitting diode.
[0089] The quantum dots as described herein may be in the form of a layer or a film in the device. Both types of the quantum dots described above may be used in the lighting device, preferably the second type of quantum dots is used.
[0090] The device may further comprise an electron transport / inj ection layer. The electron transport / inj ection layer is not particularly limited and exemplarily, may comprise zinc oxide (ZnO). The electron transport / injection layer may exemplarily further comprise polyethyleneimine ethoxylated (PE1E).
[0091] The device may further comprise a hole-transport / injection layer. The hole- transport / injection layer is not particularly limited and exemplarily may comprise poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4’-(N-(p-butylphenyl))diphenylamine)] (TFB). The hole-transport / injection layer may exemplarily further comprise molybdenum trioxidc (MoOs).
[0092] The device may further comprise electrodes. Each electrode is not particularly limited and exemplarily may independently comprise indium tin oxide (ITO) or silver.
[0093] With reference to FIG. 4A, the device may comprise five layers, namely from top to bottom, the hole injection layer (402, such as MoOa) coupled to an anode (such as silver), the hole transport layer (404, such as TFB), the layer of the quantum dots as described herein (406), the electron transport layer (408, such as PEIE) and the electron injection layer (410, such as ZnO) coupled to a cathode (such as ITO).
[0094] Therefore, in an example, the device has a structure of ITO / ZnO / PEIE / quantum dots layer / TFB / MoOa / sil ver.
[0095] The device may show a red-shifted electroluminescence (EL) at about 900 nm to about 1000 nm, about 900 nm to about 950 nm or about 950 nm to about 1000 nm. The device may show a red-shifted EL at about 940 nm. This is because the quantum dots are in a solid state and have a film / layer form, where they are closely packed.
[0096] The device may have an EL spectra that remain stable with negligible spectral shifts within an increasing driving voltage applied thereto.
[0097] The device may have a turn on voltage (Von, when the device has a radiance of about 0.01 W sr1m-2) of about 1 V to about 1.5 V. The device may have a turn on voltage of about 1.2 V. The device may have a maximum external quantum efficiency (EQE) of at least about 7.5%, about 8%, about 8.1% or about 8.2%. Advantageously, the maximum EQE of the present device is at least about 1.3-fold, about 1.4-fold or about 1.5-fold compared to the maximum EQE of a device comprising conventional quantum dots. This is primarily due to the high photolumincsccncc quantum efficiency of the quantum dots as described herein.
[0098] The device may have an average EQE of at least about 7%, about 7.5%, about 7.7% or about 7.8%. The device may have a standard deviation of the EQE of at most about 0.5%, about 0.3% or about 0.2%. Advantageously, the device has a low standard deviation of the EQE and is highly reproducible.
[0099] The device may have a Tso lifetime of at least about 32 minutes, about 35 minutes, about 38 minutes or about 40 minutes at an initial brightness of about 0.14 Wsr-1nT2. Advantageously, this is significantly higher than the Tso lifetime of a device comprising conventional quantum dots, which may be about 30 minutes. This is because the quantum dots as described herein are thermally stable as described above.
[0100] Brief Description of Drawings
[0101] The accompanying drawings illustrate a disclosed embodiment and serves to explain the principles of the disclosed embodiment. It is to be understood, however, that the drawings are designed for purposes of illustration only, and not as a definition of the limits of the invention.
[0102] FIG. 1A
[0103] [FIG. 1 A] shows absorbance and photoluminescence (PL) spectral evolution of CuInS2-DDT / ZnS quantum dots (QDs) during its synthesis.
[0104] FIG. IB
[0105] [FIG. 1B] shows absorbance and PL spectral evolution of CuTnS2-HMDS / ZnS QDs during its synthesis.
[0106] FIG. 2A
[0107] [FIG. 2A] shows visible (left) and near-infrared (NIR, right) images of solutions of CulnS2-DDT / ZnS and CulnS2-HMDS / ZnS QDs under ambient lighting.
[0108] FIG. 2B
[0109] [FIG. 2BJ shows powder XRD patterns of CulnS2-DDT, CulnS2-DDT / ZnS, CulnS2- HMDS and CulnS2-HMDS / ZnS QDs. Reference plots show the XRD position and intensities corresponding to known structures of chalcopyrite CuInS2 and ZnS. The dotted lines correspond to the (112), (220) and (312) planes of chalcopyrite CuInS2 and (111), (220) and (311) planes of ZnS. The peak at 29 20“ for CuInS2-
[0110] DDT / ZnS and CuInSi-HMDS / ZnS marked with an asterisk represents the (006) plane of ZnIn2S4- FIG. 2C
[0111] [FIG. 2CJ is a transmission electron microscope (TEM) image of CulnSz-DDT QDs. The scale bar in FIG. 2C corresponds to a length of 80 nm.
[0112] FIG. 2D
[0113] [FIG. 2D] is a size distribution histogram of CuInS2-DDT QDs.
[0114] FIG. 2E
[0115] [FIG. 2E] is a transmission electron microscopy (TEM) image of CuInSz-HMDS QDs. The scale bar in FIG. 2E corresponds to a length of 80 nm.
[0116] FIG. 2F
[0117] [FIG. 2F] is a size distribution histogram of CuInSz-HMDS QDs.
[0118] FIG. 3
[0119] [FIG. 3] shows PL delay curves of solutions of CuInSz-DDT / ZnS and CuInSz- HMDS / ZnS QDs.
[0120] FIG. 4A
[0121] [FIG. 4A] is a schematic diagram of a light emitting diode (LED) device comprising the QDs as described herein.
[0122] FIG. 4B
[0123] [FIG. 4B] shows electroluminescence (EL) spectra of the CuInSi-HMDS / ZnS NIR LED. Inset shows a NIR image of the LED when operating.
[0124] FIG. 4C
[0125] [FIG. 4C] shows combined current density and radiance versus voltage plots of the CuInSz-HMDS / ZnS NIR LED.
[0126] FIG. 4D
[0127] [FIG. 4D] shows the external quantum efficiency (EQE) versus current density of the CuInS2-HMDS / ZnS NIR LED. Inset shows the histogram of efficiencies of 23 devices.
[0128] FIG. 5
[0129] [FIG. 5] shows PL spectra of CuInS2-DDT / ZnS and CuInS2-HMDS / ZnS with a ZnS shelling temperature of 250 °C.
[0130] FIG. 6A
[0131] [FIG. 6A] is a TEM image of CuInS2-DDT / ZnS at mid-point synthesis (18 minutes). FIG. 6B
[0132] [FIG. 6BJ is a size distribution histogram of CuInSz-DDT / ZnS at mid-point synthesis (18 minutes).
[0133] FIG. 6C
[0134] [FIG. 6C] is a TEM image of CuInSz-HMDS / ZnS at mid-point synthesis (9 minutes).
[0135] FIG. 6D
[0136] [FIG. 6D] is a size distribution histogram of CuInSz-HMDS / ZnS at mid-point synthesis (9 minutes).
[0137] FIG. 7 A
[0138] [FIG. 7A] is a TEM image of CuInS2-DDT / ZnS QDs.
[0139] FIG. 7B
[0140] [FIG. 7B] is a size distribution histogram of CuInSz-DDT / ZnS QDs.
[0141] FIG. 7C
[0142] [FIG. 7C] is a TEM image of CuInS2-HMDS / ZnS QDs.
[0143] FIG. 7D
[0144] [FIG. 7DJ is a size distribution histogram of CuInS2-HMDS / ZnS QDs.
[0145] FIG. 8
[0146] [FIG. 8J shows PL delay curves of CuInSz-DDT / ZnS and CuInS2-HMDS / ZnS QDs.
[0147] FIG. 9A
[0148] [FIG. 9AJ shows combined current density and radiance versus voltage plots of a CuInS2-DDT / ZnS QD LED.
[0149] FIG. 9B
[0150] [FIG. 9B] shows EQE versus current density of the CuInS2-DDT / ZnS QD LED.
[0151] FIG. 10
[0152] [FIG. 10] is a lifetime plot of CuInS2-DDT / ZnS and CuInS2-HMDS / ZnS QD LEDs measured under constant current with an initial radiance of 0.14 W sr1m ~2.
[0153] FIG. 11
[0154] [FIG. 11] shows the thermal stability of both CuInS2-DDT / ZnS and CuInS2- HMDS / ZnS QDs at 80 °C for 90 minutes. Examples
[0155] Non-limiting examples of the invention will be further described in greater detail by reference to specific Examples, which should not be construed as in any way limiting the scope of the invention.
[0156] Example 1 - Preparation of Quantum Dots
[0157] To form CidnSi quantum dots (QD), a mixture of cationic precursors was heated up together with long chain thiols such as 1 -dodecanethiol (DDT), which served as the anionic sulfur precursor as well as the stabilizing surface ligand. A supplementary sulfur source, hexamethyldisilathiane (HMDS) was also used. HMDS has a higher precursor reactivity compared to DDT. Due to the use of HMDS and DDT, this gave rise to better size homogeneity and an improvement in photoluminescence quantum efficiency (PLQE) of the QDs. The QDs synthesized with and without HMDS will be referred to as CuInSi-HMDS and C11I11S2-DDT respectively.
[0158] Preparation of Zn(oleate)2 precursor
[0159] In a 50 mL round-bottom flask (RBF), zinc acetate (3 mmol, 565.5 mg, 99.99%, purchased from Sigma-Aldrich, Singapore) and oleic acid (2.5 mL, 90%, purchased from Sigma- Aldrich, Singapore) were mixed with ODE (90%, purchased from Sigma-Aldrich, Singapore, degassed under vacuum and dried with activated molecular sieves before use) to a total volume of 25 mL. Vacuum was applied to the RBF and the mixture was heated to 80 °C for 30 minutes. After filling the RBF with argon, the solution was heated to 160 °C and stirred for 1 hour in argon to form a clear solution. The solution was subsequently cooled to 80 °C and was vacuumed for 30 minutes before backfilling the RBF with argon.
[0160] Synthesis of CuInS2-DDT / ZnS quantum dots (QDs)
[0161] In a 50 mL RBF, copper (I) iodide (0.1 mmol, 19.05 mg, 98% purchased from Sigma- Aldrich, Singapore), indium acetate (0.1 mmol, 29.20 mg, 99.99%, purchased from Sigma-Aldrich, Singapore) and 5 mL DDT (98%, purchased from Sigma-Aldrich, Singapore) were added to 2.5 mL of ODE. The mixture was vacuumed for 1 hour at 60 °C. Afterwards, the RBF was refilled with argon, and heated to 135 °C for approximately 15 minutes. When all the solids have dissolved, the temperature was raised to 250 °C and maintained for approximately 36 minutes. This longer reaction time of 36 minutes was necessary to propagate the growth of CuInSz-DDT QDs to achieve the same optical absorption and emission wavelengths as the CuInSi- HMDS / ZnS QDs. The RBF was then cooled to 200 °C, and 10 mL of Zn(oleate)2 was injected at a rate of 0.5 mL / minute.
[0162] Synthesis of CuInS2-HMDS / ZnS QDs
[0163] In a 50 mL RBF, copper (I) iodide (0.1 mmol, 19.05 mg), indium acetate (0.1 mmol, 29.20 mg) and 5 mL DDT were added to 2.5 mL of ODE. The mixture was vacuumed for 1 hour at 60 °C. Afterwards, the RBF was refilled with argon, and heated to 135 °C for approximately 15 minutes. In an argon-filled glovebox, 60 uL HMDS (synthesis grade, purchased from Sigma-Aldrich, Singapore) was diluted in 1 mL of ODE and used as HMDS precursor. When all the solids have dissolved, the temperature was raised to 250 °C and the HMDS precursor was quickly injected when the RBF reached 200 °C. The temperature of the reaction mixture was maintained at 250 °C for approximately 18 minutes. The RBF was then cooled to 200 °C, and 10 mL of Zn(olcatc)2 was injected at a rate of 0.5 mL / minutc.
[0164] Work up and purification
[0165] Ethanol (purchased from VWR Chemicals, Singapore) was added to both CuInSz- DDT / ZnS and CuInS2-HMDS / ZnS to precipitate the QDs followed by centrifugation at 10000 rpm for 5 minutes. The clear supernatant was carefully removed using a dropper and the precipitate obtained was dispersed in 10 mL of HPLC hexane (purchased from Fisher Chemical, Singapore). The purified QDs were stored in the refrigerator for further use.
[0166] Example 2 - Characterization of Quantum Dots
[0167] Photoluminescence quantum efficiency (PLQE)
[0168] The photoluminescence (PL) spectra and PLQE were obtained by photo-exciting the samples in an integrating sphere, using a Spectra-Physics 405 nm (100 mW, CW) diode laser, and measuring the photoluminescence using a calibrated Ocean Optics Flame-T and Flame-NIR spectrometer.
[0169] UV-visible (UV-Vis) absorption spectroscopy
[0170] UV-Vis absorbance spectra were obtained using the PerkinElmer Lambda 750 UV / Vis / NIR Spectrometer.
[0171] Transmission electron microscopy (TEM)
[0172] TEM samples were prepared by diluting the purified QD solutions in toluene and then drop-casted on a carbon-coated copper grid (300 mesh) and left to dry overnight. TEM images were recorded using JEOL 2200FS field emission electron microscope operated at 200 kV.
[0173] X-ray diffraction (XRD)
[0174] Powder X-ray diffractograms were obtained using Bruker D8 ADVANCE with X- ray source of wavelength 1.542 A (Cu Ka line). The purified QD solutions were washed for additional 5 times using ethanol and re-dispersed in hexane before dropcasting onto a standard single-crystal Si zero diffraction support plate and left to dry overnight. Inductively coupled plasma-optical emission spectroscopy (ICP-OES)
[0175] The elemental composition of the QDs was measured using Perkin Elmer Avio 500 ICP-OES. To prepare the sample for ICP-OES measurement, the purified QDs were left in a vacuum oven overnight until a dry solid was obtained. 5 mg of the solid QDs was digested with HNO3 / HCI (1:3, HNO3 was purchased from Honeywell, Singapore and HC1 was purchased from VWR Chemicals, Singapore) on hotplate for 2 hours and topped up to 10 mL with H2O. The solution was filtered before analysis.
[0176] Time-resolved photoluminescence (TRPL)
[0177] TRPL decays were acquired using the Horiba Fluoromax Plus Spectrofluorometer. Samples were excited using Horiba DD- 405L light source with a peak wavelength at 401 nm, a typical pulse width of 45 ps, and a repetition rate of 100 MHz.
[0178] The PL decay curves were fitted using the biexponential equation: where / is the normalized PL intensity, Ai and A 2 are the amplitudes of the respective exponential terms, Ti and T2are the fluorescent lifetimes, and I is time.
[0179] The contribution of each exponential term can be determined by taking the ratio:
[0180] The reaction progress of both syntheses was monitored by drawing aliquots and diluting it in hexane. FIGS. 1A and IB summarize the evolution in the PL and absorbance spectral features of the QDs at different stages of the synthesis. The introduction of HMDS is accompanied with a distinct change in the color of the solution from yellow to deep red within a span of a few seconds, indicating the rapid nucleation of CuInS2 QDs. The resulting solution shows a broadband absorption throughout the entire visible region at 200 °C which was not observed in the absence of HMDS. The CuInS2-HMDS QDs were also immediately emissive at 710 nm, and quickly redshifts to 870 nm within 18 minutes of reaction time at 250 °C.
[0181] The growth of CuInS2-HMDS QDs is approximately two times faster than the case without HMDS, which took double the time to attain the same wavelength. It was rationalized that the faster rate of reaction could be due to the greater ease of decomposition of HMDS due to the weaker Si-S bonds compared to the C-S bonds in HMDS and DDT, respectively. Nonetheless, it was still essential to incorporate DDT in the synthesis of CuInS2-HMDS as the omission of DDT gave no detectable photoluminescence due to the preferential formation of binary Cu2S, which appeared as black solids in the reaction mixture. This was consistent with past literatures whereby DDT balances the reactivity of Cu+and In3+.
[0182] Lastly, the CulnS? QDs were shelled with ZnS and this resulted in a slight redshift in the PL to 920 nm, suggesting the formation of an atop ZnS shell. The outermost ZnS shell played a pivotal role as the passivating layer, resulting in an observable increase in the PLQE from 40% to 65% and 20% to 40% in the case with and without HMDS, respectively. The use of zinc carboxylates, as in the present synthesis, resulted in extensive etching of the luminescent CuInSz core through cationic exchange, inducing a spectral blucshift. ft was shown that through the combination of a continuous injection methodology as well as the use of a lower reaction temperature of 200 °C, it was possible to promote the growth of ZnS shell with minimal cationic exchange. Specifically, ZnS shell grown at a higher temperature of 250 °C resulted in a blucshift back to 825 nm (sec FIG. 5). Nevertheless, it was noted that intcrfacial cationic exchange at the QDs’ surface cannot be completely eradicated, as seen from the emergence of a new absorbance feature at wavelength ^'500 nm (^2.5 eV) which was significantly lower in energy compared to the bulk bandgap of ZnS (3.5 eV). This has been previously associated with the formation of rhombohcdral ZnlrrS-i, which has a lower bandgap of 2.5 eV.
[0183] With a final photolumincsccncc wavelength of 920 nm and strong absorbance across the entire visible spectral region, the CuInSVZnS QDs solution appeared black in color as shown in FIG. 2A. Notably, the spectral emission of the QDs was completely contained within the NIR spectral region, with less than 0.5% of the emission profile falling in the region below 700 nm. This makes the QDs highly suitable for applications that require covert and non-visiblc illumination such as facial recognition, depth sensing, eye-tracking, security and anti-countcrfciting technologies.
[0184] The introduction of HMDS had negligible effect on the crystal structure of the synthesized QDs which can be seen from the powder X-ray diffraction (XRD) patterns of CuInS2-DDT and CulnSe-HMDS in FIG. 2B, where both QDs adopted the tetragonal chalcopyrite structure with the high intensity peaks corresponding exactly at the (112), (220), and (312) planes. Shelling with ZnS resulted in negligible changes to these peaks possibly due to comparatively thinner shell layer and similar diffraction angles to CuInS2- Instead, a low angle peak at 10 20° emerged, which can likewise be associated with the Zn-In-S alloy, ZnIn2S4, identified earlier.
[0185] TEM images in FIGS. 2C and 2E revealed that both CuInS2 QDs were tetrahedral, which was consistent with the tetragonal chalcopyrite structure derived from XRD studies. More importantly, it was noted that CuInS2-DDT QDs have a broad distribution with sizes (apex to base) ranging from 0.9 to 6.8 nm (sec FIG. 2D) and a mean size of 2.8 nm. The difference in size homogeneity was even more apparent in the earlier stages of the synthesis, whereby the size of CuInS2-DDT QDs ranged all the way from 0.5 nm to 9.8 nm (sec FIGS. 6A and 6B). On the other hand, CuInS2- HMDS QDs had a narrower size distribution which persisted throughout the synthesis (see FIGS. 6C and 6D), with its size increasing from 2.3 nm to 2.8 nm by the end of 18 minutes (see FIG. 2F). In both eases, a majority of the QDs were between 1.5 and 2.5 nm, with the larger particles (>4 nm) in CuInS2-DDT occurring randomly throughout the ensemble. The better size homogeneity of CuInSz-HMDS QDs was likely the result of the accelerated rate of reaction in the presence of HMDS. The higher reactivity of HMDS allowed for rapid nucleation of CuInS2 QDs, followed by a slow growth that is fed by the less reactive DDT. The rapid nucleation and slower growth led to better size uniformity, as observed in CuInSz-HMDS QDs. The improved size uniformity of CuInSz-HMDS was similarly observed after ZnS shelling as shown in FIGS. 7A to 7D.
[0186] Surprisingly, the full width at half -maximum (FWHM) of the PL spectra of CuInS2- HMDS / ZnS QDs (217 nm) did not improve, which suggested that the inhomogeneous broadening from the distribution of nanocrystal sizes did not contribute significantly to the spectral linewidth. Hence, to gain a better understanding of the emission mechanism as well as the make-up of the QDs, elemental analysis was conducted by ICP-OES which revealed a Cu / In ratio of 0.86 and 1.02 for CuInS2-HMDS and CuInS2-DDT QDs, respectively. A smaller Cu content was similarly observed in CuInS2-HMDS / ZnS (Cu / In = 0.79) when compared to CuInS2-DDT / ZnS (Cu / In = 0.86) QDs. While the exact emission mechanism of CuInS2 QDs is still under debate, it has been generally accepted that the emission centers originate from intragap Cu- related defects. Based on these studies and the present examples, it was postulated that the present faster-reacting HMDS has generated an increase in the density of emissive Cu-dcficicncy sites in the QDs, and thus contributed to the increase in PLQE. This was also in line with numerous current literatures where Cu-dcficicnt CuInS2 QDs were shown to be more emissive than the stoichiometric ones. The Cu- deficiency emission theory was also consistent with the observed broad linewidth that was minimally affected by the QD size distribution.
[0187] TRPL studies on the CuInS2 QDs revealed that the PL decays arc biexponential (see FIG. 3), which fits the equation 1(f) = Aiexp(~t / z\) + A2exp(-t / r2). The PL relaxation consisted of fast (ri 10 ns) and slow (z2^300 ns) components, and its respective contribution (Ai and A2) are summarized in Table 1.
[0188] Table 1. Summary of the biexponential decay fit parameters for decay curves.
[0189] The fast decay likely corresponded to the depopulation of excited states by non- radiative trap-assisted recombination, which were often associated with surface defects. The longer time constant, on the other hand, can be attributed to radiative recombination from Cu-deficiency sites. More importantly, it was noted that CuInS2- HMDS QDs exhibited superior radiative recombination with a higher Az of 77.4% as compared to CuInS2-DDT QDs (66.0%). Core-shelling with ZnS further suppressed the fast decay channel in both CuInS2-DDT / ZnS and CuInS2-HMDS / ZnS QDs (see FIG. 8 and Table 2 below). This was coupled with a significant increase in fluorescence lifetime, which was consistent with the increase in PLQE observed earlier.
[0190] Table 2. Summary of the biexponential decay fit parameters for decay curves.
[0191] Example 3 - Preparation of Light Emitting Diodes
[0192] To demonstrate the electroluminescent (EL) properties of the CuInS2-HMDS / ZnS QDs, a highly efficient near-infrared (NIR) light emitting diode (LED) was prepared using a solution-processed device structure of indium tin oxide (ITO)Zzinc oxide (ZnO) / polyethyleneimine ethoxylated (PEIE)ZQDsZpoly[(9,9-dioctylfluorenyl-2,7- diyl)-cn-(4,4’-(ZV-(p-butylphenyl))diphenylamine)] (TFB) / molybdenum trioxide (MoOO / silver (Ag).
[0193] For LED application, 1 mL of QDs were further washed with 2 mL of ethanol for an additional 5 times. Prior to the second and fourth round of purification, 1 mL of HPLC hexane was added to solubilize the QDs before the addition of ethanol. The final precipitate was re-dispersed in HPLC hexane to give a concentration of 25 mgZmL.
[0194] Synthesis of ZnO nanoparticles
[0195] Zinc acid dihydrate (2.96 g, 99%, purchased from Sigma-Aldrich, Singapore) was dissolved in 120 mL of methanol (purchased from VWR Chemicals, Singapore) at 63 °C. A solution of potassium hydroxide (KOH, purchased from GCE laboratory chemicals, Switzerland) dissolved in 60 mL methanol was then added swiftly. The reaction mixture was stirred for 2.5 hours, and the precipitated product was collected by decanting the solvent. The precipitate was purified for a total of three times by adding methanol and decanting. The final product was collected by centrifuge at 10000 rpm for 5 minutes, followed by dispersion in n-butanol to give a concentration of 30 mg / mL.
[0196] LED fabrication
[0197] Pre-patterned ITO-glass substrates (8 Q n1) were cleaned in detergent solution (Mama Lemon purchased from Lion corporation, Singapore), deionized water (filtered using a 35 inch x 7 inch DI column), acetone (purchased from VWR Chemicals, Singapore) and isopropanol (purchased from VWR Chemicals, Singapore) for 30 minutes respectively, and then dried with an argon gun.
[0198] The substrates were treated in a UV-ozone cleaner for 30 minutes before spin-coating subsequent layers. ZnO nanoparticles were deposited by spin-coating at 1500 rpm for 1 minute. This process was repeated twice, followed by annealing at 140 °C for 10 minutes. Afterwards, a thin layer of PEIE (80% ethoxylated solution, purchased from Sigma-Aldrich, Singapore) as a 0.4 wcight% solution in 2-mcthoxycthanol (99.8%, purchased from Sigma- Aldrich, Singapore) was spin-coated at 5000 rpm for 1 minute. The layers were annealed at 110 °C for 20 minutes.
[0199] When the substrates cooled down to room temperature, 60 pL of QDs with a concentration of 25 mg / mL in HPLC hexane was dropped and spin-coated at 2000 rpm for 1 minute. The substrates were then transferred into an argon-fillcd glovebox for the deposition of subsequent layers. A TFB (purchased from American Dye Source, Canada) hole-transport layer was spin-coated from a chlorobenzene solution (anhydrous, 99.8%, purchased from Sigma-Aldrich, Singapore) with a concentration of 20 mg / mL. Finally, 10 nm MoOs (99.97%, purchased from Sigma-Aldrich, Singapore) and 80 nm Ag (purchased from Kurt J. Lcskcr, Pennsylvania, United States of America) were sequentially evaporated through a shadow mask at a pressure below 10"6Torr (or 10"5Pa). The area of the device was defined by the overlap between the ITO and Ag electrode, which was 4 mm2.
[0200] Example 4 - Characterization of Light Emitting Diodes
[0201] The current density vs. voltage characteristics were measured using a Keithley 2450 source-measure unit. The voltage was swept from 0 V to 7 V at 0.05 V steps and a delay time of 1 second. Simultaneously, the photon flux was measured using a 3.1 mm2Thorlabs InGaAs photodiode with NIST traceable calibration at a distance of 100 mm. The EL spectra were recorded using a combination of two calibrated Ocean Optics Flame-T and Flame-NIR spectrometers to cover the entire visible and NIR- SWIR spectral range. External quantum efficiency (EQE) was calculated by taking a Lambertian emission profile. The device lifetime was measured using the same setup, but under a constant current condition at an initial brightness of 0.14 W sr1m-2. The device prepared showed a slightly redshifted EL at 940 nm due to the closepacking of the QDs in solid state films. The EL spectra remained stable with negligible spectral shifts as the driving voltage was increased (see FIG. 4B). The characteristics of the best performing device arc summarized in FIGS. 4C and 4D. In particular, a radiance of 13.3 W sr1m2(see FIG. 4C) and a maximum EQE of 8.2% were recorded (see FIG. 4D). This was a 1.4-fold improvement from the device employing CuInSj-DDT / ZnS QDs (see FIGS. 9A and 9B). The better device performance can be largely attributed to the higher PLQE of CuInSi-HMDS / ZnS QDs. In addition, a high average EQE of 7.8% was observed across 23 devices. The variation in device performance was minimal with a small standard deviation of 0.3%, which suggested good reproducibility of the present devices.
[0202] The LED was then subjected to operational stability testing, which gave a modest Tso lifetime of --'40 minutes at an initial brightness of 0.14 W sr-1m-2(see FIG. 10). A shorter Tso of 30 minutes was recorded for devices employing CuInS2-DDT / ZnS QDs. The modest device lifespan was likely due to the degradation of CuInS2 / ZnS QDs from Joule heating during device operation.
[0203] To better understand the thermal stability of the QDs, the QDs were subjected to 90 minutes of heat treatment at 80 °C and the PL intensities of both QDs were recorded at a fixed time interval. Both CuInS2-HMDS / ZnS and CuInS2-DDT / ZnS QDs showed an initial drop in PL intensity to --'79% its original value within the first 10 minutes, and eventually stabilized at 83% and 74%, respectively (see FIG. 11). The better thermal stability of CuInS2-HMDS / ZnS QDs was consistent with the longer device lifetime observed. While the degradation mechanism of the QDs in a device setup likely comprised of a combination of various factors, the thermal stability of the QDs has to be improved in order to enhance the operational lifetime of the LEDs.
[0204] Industrial Applicability
[0205] The quantum dots of the disclosure may be used in a variety of applications that require covert and non-visible illumination such as photovoltaic devices, lighting devices, display devices and other devices that require facial recognition, depthsensing, eye-tracking, security, robotics, biomedical imaging, night vision, surveillance, optical communications and anti-counterfeiting technologies.
[0206] It will be apparent that various other modifications and adaptations of the invention will be apparent to the person skilled in the art after reading the foregoing disclosure without departing from the spirit and scope of the invention and it is intended that all such modifications and adaptations come within the scope of the appended claims.
Claims
Claims1. A method of synthesizing quantum dots, comprising the steps of: a) heating a copper precursor, an indium precursor and a Ce-Cu thiol in the presence of a solvent to form a solution; and b) adding hexamethyldisilathiane to the solution of the heating step a) to form the quantum dots.
2. The method of claim 1, further comprising a step of c) reacting a zinc precursor with the quantum dots after the adding step b).
3. The method of claim 1 or 2, wherein the copper precursor is selected from Cui, CuBr, CuCl, CuOAc, CuS or combinations thereof.
4. The method of any one of claims 1 to 3, wherein the indium precursor is selected from Inis, InBrs, InCIs, In(OAc)s, indium (III) acetylacetonate or combinations thereof.
5. The method of any one of claims 1 to 4, wherein the Ce-Ci thiol is a C12 thiol.
6. The method of any one of claims 1 to 5, wherein the solvent is a C16-C20 alkane or a C16-C20 alkene.
7. The method of any one of claims 1 to 6, wherein the copper precursor and the indium precursor have a molar ratio in the range of about 1:0.8 to about 1:1.2.
8. The method of any one of claims 1 to 7, wherein the copper precursor and the Ce- Cu thiol have a molar ratio in the range of about 1:100 to about 1:500.
9. The method of any one of claims 1 to 8, wherein the heating step a) is undertaken at a temperature in the range of about 100 °C to about 200 °C.
10. The method of any one of claims 1 to 9, wherein the copper precursor used in the heating step a) and hexamethyldisilathiane used in the adding step b) have a molar ratio in the range of about 1:2 to about 1:6.
11. The method of any one of claims 1 to 10, wherein the adding step b) is undertaken at a temperature in the range of about 150 °C to about 250 °C.
12. The method of any one of claims 2 to 11, wherein the zinc precursor is selected from Zn(oleate)2, Zn(stearatc)2, Zn(laurate)2, Zn(myristate)2, Zn(palmitate)2 or combinations thereof.
13. The method of any one of claims 2 to 12, wherein the copper precursor used in the heating step a) and the zinc precursor used in the reacting step c) have a molar ratio in the range of about 1 :5 to about 1 :15.
14. The method of any one of claims 2 to 13, wherein the reacting step c) is undertaken for a duration in the range of about 10 minutes to about 30 minutes.
15. The method of any one of claims 2 to 14, wherein the reacting step c) is undertaken at a temperature in the range of about 150 °C to about 250 °C.
16. Quantum dots comprising a copper indium dichalcogenide, wherein: a) the quantum dots comprise copper element and indium element at a molar ratio in the range of about 0.7:1 to about 0.9:1, b) the quantum dots have a mean size in the range of about 3 nm to about 4 nm, and c) the quantum dots have a peak emission wavelength in the range of about 900 nm to about 1100 nm.
17. The quantum dots of claim 16, further comprising a zinc chalcogenide shell that at least partially covers or encapsulates the copper indium dichalcogenide.
18. The quantum dots of claim 16 or 17, wherein the quantum dots have a photoluminescence quantum efficiency of at least about 50% at an emission wavelength of at least about 900 nm.
19. Quantum dots obtained by or obtainable by the method of any one of claims 1 to 15.
20. The quantum dots of claim 19, wherein the quantum dots comprise copper clement and indium element at a molar ratio in the range of about 0.7 : 1 to about 0.9: 1.
21. The quantum dots of claim 19 or 20, wherein the quantum dots have a peak emission wavelength in the range of about 900 nm to about 1100 nm.
22. The quantum dots of any one of claims 19 to 21, wherein the quantum dots have a photoluminescence quantum efficiency of at least about 50% at an emission wavelength of at least about 900 nm.
23. A device comprising the quantum dots of any one of claims 16 to 22.
Citation Information
Patent Citations
Synthesis method of near-infrared core-shell structure quantum dot CuInS2 / ZnS
CN115340863A
Method for producing compound semiconductor particle
JP2012066982A
Method of forming CIS / zns core / shell quantum dots by solvothermal method
KR1020130004739A
Method for fabricating of Cu-In-S based quantum dots emitting visible to near-Infrared
KR102224913B1
Cited By
Preparation method of water-soluble copper-iron-sulfur colloidal quantum dots with near-infrared absorption characteristic
CN119875615A