Styrene block copolymer based self-healing thermoplastic elastomers and the production method thereof
The reactive melt blending method for styrene block copolymer-based TPEs addresses the limitations of existing self-healing TPEs by eliminating catalysts and cross-linking, resulting in recyclable, reprocessable, and environmentally friendly self-healing materials with improved durability and cost-effectiveness.
Patent Information
- Application Number
- PCT/TR2023/051625
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2024-10-03
AI Technical Summary
Current self-healing thermoplastic elastomers (TPEs) require catalysts, leading to environmental and health hazards, high production costs, and are not recyclable or reprocessable due to cross-linking reactions, limiting their industrial applicability and durability.
Styrene block copolymer-based self-healing TPEs are produced using the reactive melt blending method without catalysts, forming dynamic chemical bonds that allow for recyclability and reprocessability, eliminating the need for separation and purification processes and maintaining material integrity through external stimulus-independent healing.
The method enables the production of self-healing TPEs that are environmentally friendly, cost-effective, and suitable for industrial processing, with enhanced durability and long-term performance by preventing cross-linking reactions, thus extending material service life.
Smart Images

Figure IMGF000015_0001 
Figure 00000020_0000 
Figure 00000021_0000
Abstract
Description
[0001] STYRENE BLOCK COPOLYMER BASED SELF-HEALING THERMOPLASTIC ELASTOMERS AND THE PRODUCTION METHOD THEREOF
[0002] Technical Field of the Invention
[0003] The invention is related to styrene block copolymer-based self-healing thermoplastic elastomers (TPE) and the production method thereof. The self-healing TPEs that are the subject of the invention can be processed with industrial shaping processes and are recyclable and reprocessable. The self-healing styrene block copolymer-based TPEs, which are the subject of the invention, can be manufactured without the need for the use of any catalysts and solvents by minimising the damage to the environment and health of living organisms and eliminating the need for extra separation and / or purification processes.
[0004] State of the Art
[0005] Thermoplastic elastomers (TPE) are soft and flexible plastics that can be processed in processing machines used in the plastic and rubber industry and do not require vulcanisation like rubbers. Thermoplastic elastomers are frequently preferred in applications requiring soft, flexible and long-term using of plastics due to their low density, wide hardness range, low permanent deformation properties, high resistance to ultraviolet (UV) rays and ozone, applicability / usability in a wide temperature range, being recyclable and colouring. In addition to their elasticity and weather resistance properties just like rubber materials, TPEs also exhibit temperature resistance, mechanical strength, recyclability and reprocessability properties like thermoplastic materials.
[0006] Apart from the properties such as mechanical strength, temperature resistance and easy processability, the self-healing properties of plastics, which are in the current state of the art and frequently used in the industry, have become one of the important issues in material science. Self-healing feature can provide long-term durability in the structure by eliminating destructive damages such as micro, meso or macro cracks and tearing and punctures that occur on the material during its service life with autonomous (without any external stimulus) or non-autonomous (with the help of an external stimulus) repairing mechanisms. In this way, the service life of the materials can be extended, and significant application advantages can be obtained both technically and economically.
[0007] In the state of the art, although self-healing TPE materials are produced, the reactive melt blending method has not been used in the production of these materials. In thermosetting systems, the self-healing mechanism is generally achieved by microparticles embedded into the material and containing reaction-initiating chemicals. When damage occurs, micro particles are broken in the failuring domain then the reactive component in the particles is dispersed, and healing occurs by a chemical reaction in the damaged area. This healing provides a one-time repairing for each failuring domain for the material. The self-healing feature of thermoplastics is achieved by re-fusing of material in molten form (hot welding), but this is not defined as self- healing since it does not provide a healing by maintaining the shape of plastic in solid form. In rubber and elastomers, the self-healing mechanism is based on constructing chemical interactions between reactive groups on the polymer molecule. Therefore, there are a limited number of rubber and elastomer raw materials which are suitable for self-healing processes. These raw materials are generally halogen-containing and / or halogenated rubbers, and the reactivation of the polymer requires special organic reactions such as Diels-Alder reaction, disulphide metathesis, click reactions. In the state of the art, a blend that provides dynamic interactions can be produced by introducing additives and chemicals containing functional groups into the formulation during the preparation of the elastomer mixture, without the need for special polymeric raw materials and organic syntheses.
[0008] In the state of the art, when producing self-healing TPE materials, a catalyst is needed for grafting of reactive groups to the polymer chain. Catalysts used for grafting reactive groups onto plastics are organic peroxides such as dicumyl peroxide (DCP), benzoyl peroxide, lauryl peroxide (LP). These catalysts decompose at the reaction temperature to form active oxygen radicals and lead to grafting another organic group onto the polymer molecule via free radical mechanism. Organic peroxides are explosive and harmful compounds. Catalysts used in the production of functional elastomers are organo-metallic esterification catalysts, strong acid or base catalysts, nano-sized heterogeneous catalysts with high surface area, specific bioagents, enzymes, and peroxides as chemical effects and UV, microwave, light, sound waves and other physical stimuli as physical effects. Additionally, the use of catalysts in any reaction means process costs due to both raw materials and separation / purification operations. Primarily considering the environmental and health of living organisms, and then the process cost, completely eliminating the use of catalysts in the production of self- healing TPE materials provides a significant technical advantage.
[0009] In the state of the art, extra separation and / or purification processes must be applied when producing self-healing TPE materials. The mentioned separation and purification processes may include one or more of the unit operations such as precipitation, filtration, dissolving, extraction, concentration, neutralisation, washing and drying. These processes are techniques that are especially applied in the production of self- healing TPEs in solution medium. On the other hand, in polymer functionalisation processes carried out by reactive melt blending, the organic compounds remaining unreacted and the catalysts used might be needed to seperate. Because it is known that each component in the product composition has significant effects on the physical properties and application areas of end products. The application of such secondary separation processes in industrial polymer processing operations means both technical difficulty and very high production costs.
[0010] In the state of the art, while producing self-healing TPE materials, cross-linking reactions occur during the reaction. Since the self-healing feature in thermoset and vulcanised systems is based on chemical reactions, strong covalent bonds must be formed between the molecules. Covalent bonds are provided by cross-linking reactions. Cross-linking prevents the material to be recyclable and reprocessable.
[0011] In the state of the art, while self-healing TPE materials are produced, due to reasons such as the facts that the reactive melt blending method cannot be used, catalysts are needed for reactive group grafting reactions onto the polymer chain, which threaten the environment and health of living organisms and cause extra costs, TPEs in the state of the art are not recyclable and reprocessable, TPEs in the state of the art are not suitable for elastomer shaping processes, and extra separation and / or purification processes are used when producing self-repairing TPE materials, it has become necessary to introduce self-repairing, recyclable and reprocessable thermoplastic elastomers (TPE) that are suitable for elastomer shaping processes and the production method of these elastomers, in which all these problems are eliminated.
[0012] Brief Description and Aims of the Invention
[0013] In the invention, styrene block copolymer-based self-healing thermoplastic elastomers (TPE) and the production method thereof are described. The self-healing TPEs that are the subject of the invention can be processed with industrial shaping processes and are recyclable and reprocessable. The production of self-healing styrene block copolymer-based TPEs, which are the subject of the invention, can be manufactured without the need of catalysts using by minimising the damage to the environment and health of living organisms and eliminating the need for extra separation and / or purification processes. In the production method that is the subject of the invention, the reactive blending method in melt state is used.
[0014] An aim of the invention is to provide a self-healing thermoplastic elastomer that is suitable for industrial polymer processing operations. In the plastics industry, rubbers and elastomers with different properties and compositions are first mixed, compounded and kneaded to components are distributed among each other, and then a shaping process such as extrusion, injection moulding, compression moulding, casting, coating, calendaring and granulating, which is suitable to form the final product shape. Forming processes are the operations in which the vulcanisation reactions also occur in rubbers, and only kneading and shaping are applied for TPEs. The production of TPE, which is the subject of the invention, is carried out only by kneading and shaping processes among these mentioned methods. A self-healing TPE that is suitable for shaping processes is achieved by using the reactive melt blending method in the production method of the TPE that is the subject of the invention.
[0015] Another aim of the invention is to produce self-healing TPE without a need of catalyst using. In the production method of the invention, by using the reactive blending method in the melt state, the functional group grafting reaction to the styrene-based block copolymer is carried out without the use of any catalyst (e.g. organo-metallic esterification catalysts, strong acid or base catalysts, nano-sized heterogeneous catalysts with high surface area, specific bioagents, enzymes, peroxides, external stimuli such as UV, microwave, light or sound waves, etc.).
[0016] With the invention, a TPE production method is provided in which the damage to the environment and human health is minimised. In the production method of the invention, by using the reactive blending method in the melt state, the functional group grafting reaction to the styrene-based block copolymer is carried out without the use of any catalyst (e.g. organo-metallic esterification catalysts, strong acid or base catalysts, nano-sized heterogeneous catalysts with high surface area, specific bioagents, enzymes, peroxides, external stimuli such as UV, microwave, light or sound waves, etc.), eliminating the chemical effects that pose a threat to the environment and health of living organisms.
[0017] Another aim of the invention is to provide a production method in which the cost of self- healing TPE production is minimised. In the production method of the invention, by using the reactive blending method in the melt state, the functional group grafting reaction to the styrene-based block copolymer is carried out without the use of any catalyst (e.g. organo-metallic esterification catalysts, strong acid or base catalysts, nano-sized heterogeneous catalysts with high surface area, specific bioagents, enzymes, peroxides, external stimuli such as UV, microwave, light or sound waves, etc.). Therefore, a lower-cost self-healing TPE production is achieved, compared to the state of the art, since the catalyst cost is eliminated in the production method of the invention.
[0018] Another aim of the invention is to produce a TPE that eliminates the extra separation and / or purification processes in the production of self-healing TPE. In the invention, the production of TPE, which eliminates the extra separation and / or purification processes in the production of self-healing TPE, is made by adding proper amount of reactive components equivalently according to the amount of functional groups.
[0019] In the invention, self-healing TPE materials are also ensured to be recyclable and reprocessable. Self-healing TPE materials, which are recyclable and reprocessable, are provided by the fact that cross-linking reactions do not occur in the production method of the invention. Since the functional compounds used in reactive melt blending in the invention do not contain more than two reactive groups that make covalent bonds in the same molecule, no cross-linking reaction occurs between polymer chains. However, the reactive additives and functional groups used in this invention are compounds that create dynamic bonding.
[0020] Description of Drawings
[0021] Figure 1. FTIR spectra of TPEs produced by reactive blending, (a) SEBS-PMAO blend, (b) functional SEBS-PMAO blend compounded with triazole, (c) functional SEBS-PMAO blend compounded with zinc nitrate tetrahydrate (Zn(NO3)2.4H2O).
[0022] Figure 2. Change in FTIR spectra of TPEs produced by reactive blending depending on blending time.
[0023] Figure 3. Change of the ratios of peak intensities at the wavenumbers of 1725 cm-1and 700 cm-1in FTIR spectra of TPEs produced by reactive blending, with mixing time.
[0024] Figure 4. Change in the intensity of imide bond formed by maleic anhydride / triazole equivalent; where A) MAh:Triazole of 1 :1 and B) MAh:Triazole of 2:1 .
[0025] Figure 5. Optical microscope (Nikon Eclipse E200) images of the damaged crossection of TPE obtained using 45 g poly(styrene-b-ethylene-r-butylene-b-styrene) (SEBS), 45 g paraffinic oil with a viscosity of 8.3 cSt at 40°C, 10 g poly(maleic anhydride-alt-1 -octadecene) (PMAO), 2.4 g 3-amino-1 ,2,4 triazole and 3.6 g Zn(NO3)2.4H2O, before damage and healed for 6 hours and 24 hours.
[0026] Figure 6. Tensile test results of TPEs produced by the method in which 20 g poly(styrene-b-ethylene-r-butylene-b-styrene) (SEBS), 20 g paraffinic oil with a viscosity of 8.3 cSt at 40°C as plasticizer, 60 g maleic anhydride grafted poly(styrene- b-ethylene-r-butylene-b-styrene) (SEBS-g-MA), 0.5 g 3-amino-1 ,2,4 triazole and 0.8 g Zn(NO3)2.4H2O are used.
[0027] Detailed Description of the Invention
[0028] The invention is related to styrene block copolymer-based self-healing thermoplastic elastomers (TPE) and the production method thereof. The self-healing TPEs that are the subject of the invention can be manufactured with industrial shaping processes and are recyclable and reprocessable. The production of self-repairing styrene block copolymer-based TPEs, which are the subject of the invention, is achieved without the need of catalyst using, minimising the damage to the environment and health of living organisms and eliminating the need for extra separation and / or purification processes. The self-healing TPE production that is the subject of the invention is implemented by functionalising styrene block copolymer-based TPEs that do not contain functional groups in four-stage by reactive blending method in the melt state and creating dynamic chemical bonds that are sensitive to external effects.
[0029] The production method of styrene block copolymer-based self-healing thermoplastic elastomers (TPE) that is the subject of the invention comprises the process steps of; i. Swelling the block copolymer by mixing styrene block copolymer and plasticizer and waiting, ii. Preparing an elastomer blend by loading the mixture of plasticizer and styrene block copolymer with maleic anhydride or maleic acid copolymer into the melt blending device, mixing and kneading, iii. Carrying out a reaction between maleic anhydride or maleic acid groups and the amine compound by adding a cyclic amine compound into the elastomer blend, mixing and kneading, and iv. Forming complex and / or chelate bonds between the functional groups of maleic anhydride or maleic acid and the amine compound and the metal by adding metal salt to the elastomer blend functionalised with maleic anhydride or maleic acid groups and amine compound, mixing and kneading.
[0030] In one embodiment of the invention, the production method of styrene block copolymer-based self-healing thermoplastic elastomers (TPE) that is the subject of the invention comprises the processing steps of; i. Swelling the block copolymer by mixing styrene block copolymer and plasticizer and waiting, ii. Preparing an elastomer blend by loading the mixture of plasticizer and styrene block copolymer with maleic anhydride or maleic acid copolymer into the melt blending device, mixing and kneading at 130-200°C and for 5-15 minutes, iii. Carrying out a reaction between maleic anhydride or maleic acid groups and the amine compound by adding a cyclic amine compound into the elastomer blend, mixing and kneading in the melt blending device for 5-15 minutes at 130-200°C, and iv. Forming complex and / or chelate bonds between the functional groups of maleic anhydride or maleic acid and the amine compound and the metal by adding metal salt to the elastomer blend functionalised with maleic anhydride or maleic acid groups and amine compound, mixing and kneading in the melt blending device for 5-15 minutes at 130-200°C.
[0031] The melt blending device used in the method of the invention can be single screw, twin screw, multi-screw (planetary type), tandem extruders, banbury, kneader, internal mixer or compaunder and the mixing speed is 50-200 rpm. These devices are used in mixture preparation and kneading steps.
[0032] Styrene block copolymers mentioned in the process steps (i) and (ii) in the method that is subject of the invention are;
[0033] • poly(styrene-b-butadiene-b-styrene) (SBS)
[0034] • poly(styrene-b-ethylene-r-butylene-b-styrene) (SEBS)
[0035] • poly(styrene-b-isoprene-b-styrene) (SIS)
[0036] • poly(styrene-b-ethylene-r-propylene) (SEP)
[0037] • poly(styrene-b-ethylene-r-propylene-b-styrene) (SEPS)
[0038] • poly(styrene-b-isobutylene-b-styrene) (SIBS)
[0039] • poly(styrene-b-ethylene-b-ethylene-r-propylene-b-styrene) (SEEPS) or
[0040] • poly(styrene-b-ethylene-b-ethylene-r-propylene-b-styrene) (SEEPS-OH) with hydroxyl end groups.
[0041] The styrene ratios of these styrene block copolymers can vary between 10-70% by weight, and they can possess different molecular weights.
[0042] The plasticizers mentioned in the process steps (i) and (ii) in the method that is the subject of the invention are;
[0043] • paraffinic oils or
[0044] • mineral oils. The mentioned plasticizers can be in liquid or solid form and possess different viscosity and density values.
[0045] Maleic anhydride and maleic acid copolymers mentioned in the process steps (ii), (iii) and (iv) of the method that is the subject of the invention are;
[0046] • maleic anhydride grafted poly(styrene-b-ethylene-r-butylene-b-styrene) (SEBS- g-MA)
[0047] • maleic anhydride grafted polyisoprene (PI-g-MA)
[0048] • poly[(isobutylene-sub-maleic acid, ammonium salt)-co-(isobutylene-sub-maleic anhydride)]
[0049] • poly(maleic anhydride-sub-1 -octadecene) (PMAO)
[0050] • poly(isobutylene-sub-maleic anhydride) (PIB-sub-MAh)
[0051] • poly(methyl vinyl ether-alt-maleic anhydride)
[0052] • poly(methyl vinyl ether-alt-maleic acid) or
[0053] • styrene-maleic anhydride copolymers (SMA).
[0054] The maleic anhydride and maleic acid ratios of said maleic anhydride and maleic acid copolymers are 0.2-70% by weight and they can possess different molecular weights. For the production of self-healing TPE, the formulation is created by calculating the amount of functional groups according to the maleic anhydride or acid ratio or the acid number of the copolymers.
[0055] The cyclic amine compounds mentioned in the process step (iii) of the method that is the subject of the invention are;
[0056] • 3-Amino-1 ,2,4-triazole
[0057] • 3-Amino-1 H-1 ,2,4-triazole
[0058] • 4-Amino-1 ,2,4-triazole
[0059] • 4-Amino-4H-1 ,2,4-triazole
[0060] • 3, 5-Diamino-1 ,2,4-triazole
[0061] • 3-Amino-1 ,2,4-triazine
[0062] • aminopyrazine
[0063] • 2-Aminopyrimidine
[0064] • 4-Aminopyrimidine • 2,3-Diaminopyridine or
[0065] • 2,6-Diaminopyridine.
[0066] The metal salts mentioned in process step (iv) of the method that is the subject of the invention are all inorganic or organic salts of Fe2+, (Fe3+), (Zn2+), (Co2+), (Ni2+) or (Cu2+) metals.
[0067] In one embodiment of the invention, the production method of styrene block copolymer-based self-healing thermoplastic elastomers (TPE) that is the subject of the invention comprises the process steps of; i. Swelling the block copolymer by mixing 45 g of poly(styrene-b-ethylene-r- butylene-b-styrene) (SEBS) and 45 g of paraffinic oil with a viscosity of 8.3 cSt at 40°C as a plasticizer and waiting for 2 hours, ii. Preparing an elastomer blend by loading the mixture of SEBS and paraffinic oil as plasticizer and 10 g of poly(maleic anhydride-alt-1 -octadecene) (PMAO) with an acid number of 310 mg KOH / g into the melt blending device, mixing and kneading at 165°C, at a mixing speed of 75 rpm for 10 minutes, iii. Creating reaction between PMAO and 3-amino-1 ,2,4 triazole by adding 2.4 g of 3-amino-1 ,2,4 triazole to the elastomer blend and mixing and kneading it in the melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm, and iv. Forming complex and / or chelate bonds between 3-amino-1 ,2,4 triazole and PMAO functional groups and metal by adding 3.6 g of zinc nitrate tetrahydrate (Zn(NO3)2.4H2O) as a metal salt to the elastomer blend functionalised with 3-amino-1 ,2,4 triazole and PMAO and mixing and kneading in a melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm.
[0068] In a different embodiment of the invention, the production method of styrene block copolymer-based self-healing thermoplastic elastomers (TPE) that is the subject of the invention comprises the process steps of; i. Swelling the block copolymer by mixing 41 g of poly(styrene-b-ethylene-r- butylene-b-styrene) (SEBS) and 41 g of paraffinic oil with a viscosity of 8.3 cSt at 40°C as a plasticizer and waiting for 2 hours, ii. Preparing an elastomer blend by loading the mixture of SEBS and paraffinic oil as plasticizer into the melt blending device together with 18 g of styrenemaleic anhydride copolymer (SMA) with a styrene / maleic anhydride ratio of 5.33 / 1.00 and mixing and kneading at 165°C at a mixing speed of 75 rpm for 10 minutes, iii. Creating reaction between SMA and 3-amino-1 ,2,4 triazole by adding 2.4 g of 3-amino-1 ,2,4 triazole to the elastomer blend and mixing and kneading it in the melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm, and iv. Forming complex and / or chelate bonds between 3-amino-1 ,2,4 triazole and SMA functional groups and metal by adding 3.6 g of zinc nitrate tetrahydrate (Zn(NO3)2.4H2O) as a metal salt to the elastomer blend functionalised with 3-amino-1 ,2,4 triazole and PMAO and mixing and kneading in a melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm.
[0069] In a different embodiment of the invention, the production method of styrene block copolymer-based self-repairing thermoplastic elastomers (TPE) that is the subject of the invention comprises the process steps of; i. Swelling the block copolymer by mixing 20 g of poly(styrene-b-ethylene-r- butylene-b-styrene) (SEBS) and 20 g of paraffinic oil with a viscosity of 8.3 cSt at 40°C as a plasticizer and waiting for 2 hours, ii. Forming an elastomer blend by loading the mixture of SEBS and plasticizer paraffinic oil into the melt blending device together with 60 g of maleic anhydride graft poly(styrene-b-ethylene-r-butylene-b-styrene) (SEBS-g-MA) with a maleic anhydride ratio of 1.0% by weight and an acid number of 10 mg CHgONa / g and mixing and kneading in a melt blending device at 165°C at a mixing speed of 75 rpm for 10 minutes, iii. Creating reaction between SEBS-g-MA and 3-amino-1 ,2,4 triazole by adding 0.5 g of 3-amino-1 ,2,4 triazole to the elastomer blend and mixing and kneading it in the melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm, and iv. Forming complex and / or chelate bonds between 3-amino-1 ,2,4 triazole and SEBS-g-MA functional groups and metal by adding 0.8 g of zinc nitrate tetrahydrate (Zn(NO3)2.4H2O) as a metal salt to the elastomer blend functionalised with 3-amino-1 ,2,4 triazole and SEBS-g-MA and mixing and kneading in a melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm.
[0070] In the method of the invention, test specimens were prepared by moulding the functional elastomer blends produced by the melt blending method in a hot pres at 160°C, under 5 tons for 5 minutes. The prepared test specimens were kept under room conditions for 24 hours and then cutting-joining operations were carried out. The parts with cut surfaces attached to each other were kept at a temperature between 60-120°C for 2-48 hours to form dynamic bonds that enable functional elastomers to heal themselves. The self-healing performances of functional elastomer blends were quantified by mechanical tests such as weight bearing and tensile test.
[0071] Figure 1 shows the FTIR spectra, (a) SEBS-PMAO blend, (b) functional SEBS-PMAO blend compounded with triazole, (c) functional SEBS-PMAO blend compounded with zinc nitrate tetrahydrate (NO3)2.4H2O), of TPEs produced by reactive blending.
[0072] Figure 2 shows the change in FTIR spectra of TPEs produced by reactive blending depending on the blending time. In the FTIR spectra given in Figure 2, a peak belonging to the characteristic C=O bonds of maleic anhydride groups is seen at 1780 cm-1in the SEBS-PMAO blend. It is seen that the intensity of 1780 cm-1peak decreases with the addition of the cyclic amine compound (3-amino 1 ,2,4-triazole) and the imide bond is formed by binding the cyclic amine compound to the maleic anhydride groups (1725 cm-1). It was determined that the intensity of imide peak did not change depending on the mixing time and the functionalisation reaction occurred within 10 minutes of mixing.
[0073] Figure 3 shows the change in the ratio of intensity of the 1725 cm-1peak, which indicates the formation of the imide bond, to the intensity of the characteristic peak of the -CH2 groups, which remains unchanged in the copolymer structure, over time, depending on the mixing time. It was determined that the intensity of the imide peak did not change depending on the mixing time and the functionalisation reaction occurred within 10 minutes of mixing.
[0074] Figure 4 shows the change in the intensity of the imide bond formed by the reaction between equivalent maleic anhydride and triazole. It was determined that the intensity of imide bond increased with the increasing amount of cyclic amine.
[0075] In Figure 5, cross-sectional images of the damaged area of TPE obtained using 45 g poly(styrene-b-ethylene-r-butylene-b-styrene) (SEBS), 45 g paraffinic oil with a viscosity of 8.3 cSt at 40°C, 10 g poly(maleic anhydride-sub-1 -octadecene) (PMAO), 2.4 g 3-amino-1 ,2,4 triazole and 3.6 g Zn(NO3)2.4H2O are represented before the damage, after 6-hour and after 24-hour healings. As seen in the microscope photos, the joining line disappears with time.
[0076] Figure 6 shows the tensile test results performed with a crosshead speed of 20 mm / minute for TPEs produced with the method in which 20 g poly(styrene-b-ethylene- r-butylene-b-styrene) (SEBS), 20 g paraffinic oil with a viscosity of 8.3 cSt at 40°C as plasticizer, 60 g maleic anhydride grafted poly(styrene-b-ethylene-r-butylene-b- styrene) (SEBS-g-MA), 0.5 g 3-amino-1 ,2,4 triazole and 0.8 g Zn(NO3)2.4H2O are used. It was determined that the elongation at break value of the undamaged functional elastomer prepared by said method was 700% and the tensile strength was 4 MPa. It was determined that the elongation at break and tensile strength values of the damaged specimen increased with the increase in temperature and time, and the elastic modulus values of all healed samples were the same or very close to the undamaged one.
[0077] The functionalisation of elastomer formed by reactions between amine and maleic anhydride and the complex formation by metal addition to this functional elastomer are shown. Depending on the given reaction, self-healing occurs through hydrogen interactions and metal-chelate bonding between functional groups. Reaction 1
[0078] 10
Claims
CLAIMS1. The production method of styrene block copolymer-based self-healing thermoplastic elastomers (TPE), comprising the process steps of; i. Swelling the block copolymer by mixing styrene block copolymer and plasticizer and waiting, ii. Preparing an elastomer blend by loading the styrene block copolymer and plasticizer mixture with maleic anhydride or maleic acid copolymer into the melt blending device, mixing and kneading, iii. Carrying out a reaction between maleic anhydride or maleic acid groups and the amine compound by adding a cyclic amine compound into the elastomer blend, mixing and kneading, and iv. Forming complex and / or chelate bonds between the functional groups of maleic anhydride or maleic acid and the amine compound and the metal by adding metal salt into the elastomer blend functionalised with maleic anhydride or maleic acid groups and amine compound, mixing and kneading.
2. A method according to claim 1 , comprising the process steps of: i. Swelling the block copolymer by mixing styrene block copolymer and plasticizer and waiting, ii. Preparing an elastomer blend by loading the styrene block copolymer and plasticizer mixture with maleic anhydride or maleic acid copolymer into the melt blending device, mixing and kneading at 130- 200°C and for 5-15 minutes, iii. Carrying out a reaction between maleic anhydride or maleic acid groups and the amine compound by adding a cyclic amine compound into the elastomer blend, mixing and kneading in the melt blending device for 5-15 minutes at 130-200°C, and iv. Forming complex and / or chelate bonds between the functional groups of maleic anhydride or maleic acid and the amine compound and the metal by adding metal salt into the elastomer blendfunctionalised with maleic anhydride or maleic acid groups and amine compound, mixing and kneading in the melt blending device for 5-15 minutes at 130-200°C.
3. A method according to Claims 1 or 2, wherein the styrene block copolymer mentioned in the process steps (i) and (ii) are;• poly(styrene-b-butadiene-b-styrene) (SBS)• poly(styrene-b-ethylene-r-butylene-b-styrene) (SEBS)• poly(styrene-b-isoprene-b-styrene) (SIS)• poly(styrene-b-ethylene-r-propylene) (SEP)• poly(styrene-b-ethylene-r-propylene-b-styrene) (SEPS)• poly(styrene-b-isobutylene-b-styrene) (SIBS)• poly(styrene-b-ethylene-b-ethylene-r-propylene-b-styrene) (SEEPS) or• poly(styrene-b-ethylene-b-ethylene-r-propylene-b-styrene) (SEEPS-OH) with hydroxyl end groups.
4. Method according to Claim 3, wherein said styrene block copolymer ratios are 10-70% by weight.
5. A method according to Claims 1 or 2, wherein the plasticiser mentioned in the process steps (i) and (ii) are;• paraffinic oils or• mineral oils.
6. A method according to Claims 1 or 2, wherein the maleic anhydride and / or maleic acid copolymers mentioned in the process steps (ii), (iii) and (iv) are;• maleic anhydride grafted poly(styrene-b-ethylene-r-butylene-b-styrene) (SEBS- g-MA)• maleic anhydride grafted polyisoprene (PI-g-MA)• poly[(isobutylene-sub-maleic acid, ammonium salt)-co-(isobutylene-sub-maleic anhydride)]• poly(maleic anhydride-sub-1 -octadecene) (PMAO)• poly(isobutylene-sub-maleic anhydride) (PIB-sub-MAh)• poly(methyl vinyl ether-alt-maleic anhydride)poly(methyl vinyl ether-alt-maleic acid) or styrene-maleic anhydride (SMA) copolymers.
7. A method according to Claim 6, wherein the maleic anhydride or maleic acid ratios of said maleic anhydride and maleic acid copolymers is 0.2-70% by weight.
8. A method according to Claims 1 or 2, wherein the cyclic amine compounds mentioned in the process step (iii) are;• 3-Amino-1 ,2,4-triazole• 3-Amino-1 H-1 ,2,4-triazole• 4-Amino-1 ,2,4-triazole• 4-Amino-4H-1 ,2,4-triazole• 3, 5-Diamino-1 ,2,4-triazole• 3-Amino-1 ,2,4-triazine• aminopyrazine• 2-Aminopyrimidine• 4-Aminopyrimidine• 2,3-Diaminopyridine or• 2,6-Diaminopyridine.
9. A method according to Claims 1 or 2, wherein the metal salts mentioned in process step (iv) are all inorganic or organic salts of Fe2+, (Fe3+), (Zn2+), (Co2+), (Ni2+) or (Cu2+) metals.10.A method according to Claim 9, wherein said inorganic salt is zinc nitrate tetrahydrate (Zn(NO3)2.4H2O).
11. A method according to Claims 1 or 2, comprising the process steps of: i. Swelling the block copolymer by mixing 45 g of poly(styrene-b- ethylene-r-butylene-b-styrene) (SEBS) and 45 g of paraffinic oil with a viscosity of 8.3 cSt at 40°C as a plasticizer and waiting for 2 hours,ii. Preparing an elastomer blend by loading the mixture of SEBS and paraffinic oil as plasticizer and 10 g of poly(maleic anhydride-alt-1 - octadecene) (PMAO) with an acid number of 310 mg KOH / g into the melt blending device, mixing and kneading at 165°C, at a mixing speed of 75 rpm and for 10 minutes, iii. Creating reaction between PMAO and 3-amino-1 ,2,4 triazole by adding 2.4 g of 3-amino-1 ,2,4 triazole into the elastomer blend and mixing and kneading in the melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm, and iv. Forming complex and / or chelate bonds between 3-amino-1 ,2,4 triazole and PMAO functional groups and metal by adding 3.6 g of zinc nitrate tetrahydrate (Zn(NO3)2.4H2O) as a metal salt to the elastomer blend functionalised with 3-amino-1 ,2,4 triazole and PMAO and mixing and kneading in a melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm.
12. A method according to Claims 1 or 2, comprising the process steps of: i. Swelling the block copolymer by mixing 41 g of poly(styrene-b- ethylene-r-butylene-b-styrene) (SEBS) and 41 g of paraffinic oil with a viscosity of 8.3 cSt at 40°C as a plasticizer and waiting for 2 hours, ii. Preparing an elastomer blend by loading the mixture of SEBS and paraffinic oil as plasticizer into the melt blending device together with 18 g of styrene-maleic anhydride copolymer (SMA) with a styrene / maleic anhydride ratio of 5.33 / 1 .00 and mixing and kneading at 165°C at a mixing speed of 75 rpm and for 10 minutes, iii. Creating reaction between SMA and 3-amino-1 ,2,4 triazole by adding 2.4 g of 3-amino-1 ,2,4 triazole to the elastomer blend and mixing and kneading it in the melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm, and iv. Forming complex and / or chelate bonds between 3-amino-1 ,2,4 triazole and PMAO functional groups and metal by adding 3.6 g of zinc nitrate tetrahydrate (Zn(NO3)2.4H2O) as a metal salt to the elastomer blend functionalised with 3-amino-1 ,2,4 triazole andPMAO and mixing and kneading in a melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm. A method according to Claims 1 or 2, comprising the process steps of: i. Swelling the block copolymer by mixing 20 g of poly(styrene-b- ethylene-r-butylene-b-styrene) (SEBS) and 20 g of paraffinic oil with a viscosity of 8.3 cSt at 40°C as a plasticizer and waiting for 2 hours, ii. Preparing an elastomer blend by loading the mixture of SEBS and plasticizer paraffinic oil into the melt blending device together with 60 g of maleic anhydride graft poly(styrene-b-ethylene-r-butylene- b-styrene) (SEBS-g-MA) with a maleic anhydride ratio of 1 .0% by weight and an acid number of 10 mg CHaONa / g and mixing and kneading in a melt blending device at 165°C at a mixing speed of 75 rpm and for 10 minutes, iii. Creating reaction between SEBS-g-MA and 3-amino-1 ,2,4 triazole by adding 0.5 g of 3-amino-1 ,2,4 triazole to the elastomer blend and mixing and kneading it in the melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm, and iv. Forming complex and / or chelate bonds between 3-amino-1 ,2,4 triazole and SEBS-g-MA functional groups and metal by adding 0.8 g of zinc nitrate tetrahydrate (Zn(NO3)2.4H2O) as a metal salt to the elastomer blend functionalised with 3-amino-1 ,2,4 triazole and SEBS-g-MA and mixing and kneading in a melt blending device for 10 minutes at 165°C at a mixing speed of 75 rpm. A self-healing thermoplastic elastomer based on styrene block copolymer produced by a method according to claim 1 or 2. A self-healing thermoplastic elastomer based on styrene block copolymer produced by a method according to any one of claims 1 1 to 13.
Citation Information
Patent Citations
Cable-sheath material with self-repair function, preparation method and cable sheath
CN108342048A
Self-healing thermoplastic elastomer material
CN110684364A
Thermoplastic elastomer composition and method for preparing same
EP3351595A1
Self-repairing cable