Propylene-based polymer composition, film, and multilayer film
The propylene-based polymer composition, optimized through specific copolymer content and multistage polymerization, addresses the rigidity-sealability imbalance in conventional films, delivering enhanced rigidity and low-temperature sealing performance.
Patent Information
- Application Number
- PCT/JP2024/013566
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-04-02
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional propylene polymer compositions, particularly unstretched polypropylene films, excel in rigidity but fall short in low-temperature sealing properties, necessitating a balance between mechanical and sealing performance.
A propylene-based polymer composition with specific intrinsic viscosity ranges, copolymer content, and molecular weight distribution, combined with a multistage polymerization process and catalyst system, to produce films with enhanced rigidity and low-temperature sealability.
The resulting films achieve a well-balanced combination of rigidity and low-temperature sealability, outperforming conventional compositions in both physical properties and sealing efficiency.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Propylene-based polymer composition, film and multilayer film
[0001] The present invention relates to a propylene-based polymer composition, a film, and a multilayer film.
[0002] In recent years, there has been a demand for thinner packaging materials in order to reduce environmental impact. Thinner packaging materials result in a decrease in their rigidity, and thus packaging materials with high rigidity and other properties are in demand. Propylene-based polymer compositions are widely used as materials for various molded articles, and the properties required vary depending on the molding method and application. For example, films made from propylene-based polymer compositions are widely used as packaging films for food and miscellaneous goods, taking advantage of their excellent mechanical properties, such as rigidity, and optical properties, such as gloss. Polypropylene films are known to have an excellent balance between rigidity and heat resistance. Patent Document 1 also discloses an unstretched polypropylene film with particularly excellent rigidity, which uses a specific propylene-based polymer.
[0003] International Publication No. 2021 / 025142
[0004] Although the unstretched polypropylene film described in Patent Document 1 has excellent rigidity as described above, it has been found that there is room for improvement in low-temperature sealability when used as a sealant film. An object of the present invention is to provide a propylene-based polymer composition capable of forming a film having a well-balanced excellent rigidity and low-temperature sealability compared to conventionally known propylene-based polymer compositions, a film having the above-mentioned physical properties in a well-balanced excellent manner, and a multilayer film having the above-mentioned film.
[0005] As a result of extensive investigations, the present inventors have found that the propylene polymer composition described below can solve the above problems, and have thus completed the present invention.
[0006] The present invention relates to, for example, the following items [1] to [7]: [1] A propylene-based polymer composition comprising: a propylene-α-olefin copolymer (A) having an intrinsic viscosity [η] of from 10 dl / g to 15 dl / g as measured in a tetralin solvent at 135°C and containing from 5.0 mol% to 10 mol% of structural units derived from an α-olefin (excluding propylene); and a propylene-based polymer (B) having an intrinsic viscosity [η] of from 0.5 dl / g to 5 dl / g as measured in a tetralin solvent at 135°C, wherein the mass fraction of the propylene-α-olefin copolymer (A) is from 0.1 % to 8 % by mass and the mass fraction of the propylene-α-olefin copolymer (B) is from 92 % to 99.9 % by mass relative to 100 % by mass of the total of the propylene-α-olefin copolymer (A) and the propylene-based polymer (B).
[0007] [2] The propylene polymer composition according to [1] above, which has a melting point of 110° C. or more and 150° C. or less. [3] The propylene polymer composition according to [2] above, which has a content of structural units derived from α-olefins (excluding propylene) of 1 mol % or more and 10 mol % or less, where the total amount of structural units of the polymer in the composition is 100 mol %. [4] The propylene polymer composition according to [3] above, which has a melt flow rate (MFR) of 1 g / 10 min or more and 10 g / 10 min or less, measured at 230° C. under a load of 2.16 kg.
[0008] [5] The propylene polymer (B) comprises a propylene-α-olefin copolymer (B-1) having an intrinsic viscosity [η] measured in tetralin at 135°C of 0.5 dl / g or more and 2 dl / g or less, a content of structural units derived from α-olefins (excluding propylene) of 0.1 mol% or more and 10 mol% or less, and a molecular weight distribution (Mw / Mn (Mn is number average molecular weight, Mw is weight average molecular weight)) of 10 or more and 100 or less, and a propylene polymer (B-2) having an intrinsic viscosity [η] measured in tetralin at 135°C of 0.5 dl / g or more and 5 dl / g or less, a content of structural units derived from α-olefins (excluding propylene) of 1 mol% or more and 9 mol% or less, and a molecular weight distribution (Mw / Mn (Mn is number average molecular weight, Mw is weight average molecular weight)) of 2 or more and less than 10, The propylene-based polymer composition according to [4], wherein, based on 100% by mass of the total of the propylene-α-olefin copolymer (A) and the propylene-α-olefin copolymer (B-1), the mass fraction of the propylene-α-olefin copolymer (A) is 5% by mass or more and 50% by mass or less, and the mass fraction of the propylene-α-olefin copolymer (B-1) is 50% by mass or more and 95% by mass or less; and based on 100% by mass of the total of the propylene-α-olefin copolymer (A), the propylene-α-olefin polymer (B-1), and the propylene-based polymer (B-2), the total mass fraction of the propylene-α-olefin copolymer (A) and the propylene-α-olefin polymer (B-1) is 1% by mass or more and 30% by mass or less, and the mass fraction of the propylene-based polymer (B-2) is 70% by mass or more and 99% by mass or less.
[0009] [6] A film comprising the propylene-based polymer composition according to any one of [1] to [5]. [7] A multilayer film having a layer comprising the propylene-based polymer composition according to any one of [1] to [5].
[0010] From the propylene polymer composition of the present invention, a film having a good balance of rigidity and low-temperature sealability, and a multilayer film having the film can be suitably produced.
[0011] FIG. 2 is a diagram showing the balance of physical properties in Examples of the present invention and some Comparative Examples when the comonomer content of the propylene polymer (B-2) is 8.5 mol %.
[0012] Hereinafter, embodiments of the present invention will be described. The propylene polymer composition of the present invention contains a propylene-α-olefin copolymer (A) and a propylene polymer (B) described below. Unless otherwise specified, the propylene-α-olefin copolymer (A) and the propylene polymer (B) described below may each contain one type of polymer or two or more types of polymers.
[0013] <Propylene / α-olefin copolymer (A)> The propylene / α-olefin copolymer (A) has an intrinsic viscosity [η] measured in a tetralin solvent at 135°C in the range of 10 dl / g or more and 15 dl / g or less, preferably 10 dl / g or more and 13 dl / g or less, and more preferably 10.5 dl / g or more and 11.5 dl / g or less.
[0014] Hereinafter, the intrinsic viscosity [η] measured in tetralin solvent at 135° C. will also be simply referred to as “intrinsic viscosity [η].”
[0015] When the intrinsic viscosity [η] is equal to or higher than the lower limit, the rigidity of the film obtained from the propylene polymer composition is good.When the intrinsic viscosity [η] is equal to or lower than the upper limit, the low-temperature sealability of the film obtained from the propylene polymer composition is good.
[0016] The propylene-α-olefin copolymer (A) is a copolymer of propylene and an α-olefin (excluding propylene). Examples of the α-olefin include α-olefins having 2 to 12 carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 4-methyl-1-pentene, and 3-methyl-1-pentene. Among these α-olefins, ethylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene are preferred. One or more α-olefins can be used. The propylene-α-olefin copolymer (A) may be a random copolymer or a block copolymer. However, a random copolymer is more preferred because a film obtained from the propylene polymer composition has excellent transparency and a good balance between low-temperature sealability and rigidity.
[0017] The content of structural units derived from α-olefins (excluding propylene) in the propylene-α-olefin copolymer (A) is 5.0 mol% or more and 10 mol% or less, preferably 5.5 mol% or more and 9 mol% or less, more preferably 6.0 mol% or more and 8 mol% or less, and even more preferably more than 6.0 mol% and 8 mol% or less, when the total content of structural units derived from propylene and structural units derived from α-olefins (excluding propylene) is taken as 100 mol%. 13 It can be measured by C-NMR.
[0018] When the content of the structural units derived from the α-olefin is equal to or greater than the lower limit, the low-temperature sealability of the film obtained from the propylene-based polymer composition is good.When the content of the structural units derived from the α-olefin is equal to or less than the upper limit, the rigidity of the film obtained from the propylene-based polymer composition is good.
[0019] The melting point of the propylene-α-olefin copolymer (A) measured by DSC is preferably 145° C. or lower, since a film obtained from the propylene polymer composition has excellent transparency and a good balance between low-temperature sealability and rigidity. The melting point is more preferably 115° C. or higher.
[0020] <<Method for Producing Propylene-α-olefin Copolymer (A)>> In producing the propylene-α-olefin copolymer (A), polymerization of propylene and α-olefin can be carried out by a known method such as slurry polymerization, bulk polymerization, etc. It is also preferable to use a catalyst for producing polypropylene, which will be described later.
[0021] The propylene / α-olefin copolymer (A) is preferably produced by bulk polymerization of raw material monomers in the absence of hydrogen at a polymerization temperature of preferably 20 to 80°C, more preferably 40 to 70°C, and at a polymerization pressure of generally normal pressure to 9.8 MPa, preferably 0.2 to 4.9 MPa.
[0022] The propylene / α-olefin copolymer (A) can be produced by the above-mentioned method. For example, the propylene / α-olefin copolymer (A) and the propylene / α-olefin copolymer (B-1) described later can also be produced in one polymerization system or two or more polymerization systems.
[0023] In the above-mentioned method, a propylene-based polymer containing a relatively high molecular weight propylene / α-olefin copolymer (A) and a relatively low molecular weight propylene / α-olefin copolymer (B-1) can be obtained by two or more multi-stage polymerizations.
[0024] Hereinafter, the propylene / α-olefin copolymer containing the propylene / α-olefin copolymer (A) and the propylene / α-olefin copolymer (B-1) will also be referred to as the propylene / α-olefin copolymer (C).
[0025] As a method for producing the propylene / α-olefin copolymer (C), for example, a method of polymerizing propylene and an α-olefin in combination in the presence of a catalyst for producing polypropylene, which will be described later, in a multi-stage polymerization of two or more stages is preferred.
[0026] Specifically, this method involves polymerizing propylene in the substantial absence of hydrogen in the first polymerization stage to produce a propylene / α-olefin copolymer (A) having a relatively high molecular weight, and then producing a propylene / α-olefin copolymer (B-1) having a relatively low molecular weight in the second or subsequent polymerization stages. The method for adjusting the intrinsic viscosity [η] of the propylene / α-olefin copolymer produced in the second or subsequent stages is not particularly limited, but a method using hydrogen as a molecular weight modifier is preferred.
[0027] The production order (polymerization order) of the propylene-α-olefin copolymer (A) and the propylene-α-olefin copolymer (B-1) is preferably such that a relatively high molecular weight propylene-α-olefin copolymer (A) is produced in the substantial absence of hydrogen in the first stage, and then a relatively low molecular weight propylene-α-olefin copolymer (B-1) is produced in the second stage or later, for example, in the presence of hydrogen. While the production order can be reversed, in order to produce a relatively low molecular weight propylene-α-olefin copolymer (B-1) in the first stage and then a relatively high molecular weight propylene-α-olefin copolymer (A) in the second stage or later, it is necessary to remove as much of the molecular weight modifier, such as hydrogen, contained in the reaction product of the first stage before the start of polymerization in the second stage or later, which makes the polymerization apparatus complex and makes it difficult to increase the intrinsic viscosity [η] in the second stage or later.
[0028] The polymerization in each stage of the multistage polymerization can be carried out continuously or batchwise, but batchwise is preferred. When the propylene / α-olefin copolymer (C) is produced by a continuous multistage polymerization method, the residence time distribution can cause compositional unevenness among polymer particles, which can increase fisheyes (FE). However, by polymerizing by batchwise, a propylene / α-olefin copolymer (C) with low FE can be obtained. Therefore, by adopting the batchwise method, a film with low FE can be obtained, even though a high molecular weight propylene / α-olefin copolymer (A) is used.
[0029] <Catalyst for Polypropylene Production> A catalyst for polypropylene production (hereinafter also simply referred to as "catalyst") that can be used in the production of the propylene-α-olefin copolymer (A) can be formed from, for example, a solid catalyst component containing magnesium, titanium, and a halogen as essential components, an organometallic compound catalyst component such as an organoaluminum compound, and an electron-donor compound catalyst component such as an organosilicon compound. Representative catalyst components that can be used include the following:
[0030] (Solid Catalyst Component) The support constituting the solid catalyst component is preferably a support obtained from metallic magnesium, an alcohol, and a halogen and / or a halogen-containing compound.
[0031] The metallic magnesium may be in the form of granules, ribbons, powder, etc. Preferably, the metallic magnesium is not coated with magnesium oxide or the like on its surface.
[0032] As the alcohol, it is preferable to use a lower alcohol having 1 to 6 carbon atoms, and in particular, the use of ethanol can produce a support that significantly improves the expression of catalytic performance. The amount of alcohol used is preferably 2 to 100 moles, more preferably 5 to 50 moles, per mole of metallic magnesium. One or more types of alcohol can be used.
[0033] The halogen is preferably chlorine, bromine, or iodine, with iodine being preferred. Furthermore, the halogen-containing compound is preferably MgCl2 or MgI2. The amount of halogen or halogen-containing compound used is usually 0.0001 gram atom or more, preferably 0.0005 gram atom or more, and more preferably 0.001 gram atom or more, per gram atom of metallic magnesium. One or more types of halogen and halogen-containing compound can be used.
[0034] A method for obtaining a support by reacting metallic magnesium with an alcohol and a halogen and / or halogen-containing compound includes, for example, reacting metallic magnesium with an alcohol and a halogen and / or halogen-containing compound under reflux (e.g., about 79°C) until no further generation of hydrogen gas is observed (usually 20 to 30 hours). The reaction is preferably carried out in an inert gas atmosphere such as nitrogen gas or argon gas.
[0035] When the obtained support is used for synthesizing a solid catalyst component, it may be dried or may be filtered and washed with an inert solvent such as heptane. The obtained support is nearly granular and has a sharp particle size distribution. Furthermore, even when examining each particle, the variation in particle size is very small. In this case, it is preferable that the sphericity (S) expressed by the following formula (I) is less than 1.60, particularly less than 1.40, and the particle size distribution index (P) expressed by the following formula (II) is less than 5.0, particularly less than 4.0.
[0036] S = (E1 / E2) 2 In formula (I), E1 represents the contour length of the projection of the particle, and E2 represents the perimeter of a circle equal to the projected area of the particle.
[0037] P = D90 / D10 (II) In formula (II), D90 refers to the particle diameter corresponding to a mass cumulative fraction of 90%. That is, it indicates that the sum of the masses of particles smaller than the particle diameter represented by D90 is 90% of the total mass of all particles. D10 refers to the particle diameter corresponding to a mass cumulative fraction of 10%.
[0038] The solid catalyst component is usually obtained by contacting the support with at least a titanium compound. The contact with the titanium compound may be carried out in multiple batches. Examples of the titanium compound include titanium compounds represented by general formula (III):
[0039] TiX 1 n (OR 1 ) 4-n ...(III) In formula (III), X 1 is a halogen atom, particularly preferably a chlorine atom, and R 1is a hydrocarbon group having 1 to 10 carbon atoms, preferably a linear or branched alkyl group, and R 1 When a plurality of groups are present, they may be the same or different; n is an integer of 0 to 4.
[0040] Specific examples of titanium compounds include Ti(O-i-C3H7)4, Ti(O-C4H9)4, TiCl(O-C2H5)3, TiCl(O-i-C3H7)3, TiCl(O-C4H9)3, TiCl2(O-C4H9)2, TiCl2(O-i-C3H7)2, and TiCl4, with TiCl4 being preferred. One or more types of titanium compounds can be used.
[0041] The solid catalyst component is usually obtained by further contacting the support with an electron donor compound. An example of the electron donor compound is di-n-butyl phthalate. One or more electron donor compounds can be used.
[0042] When the titanium compound and the electron donor compound are brought into contact with the support, a halogen-containing silicon compound such as silicon tetrachloride can be also brought into contact with the support. One or more halogen-containing silicon compounds can be used.
[0043] The solid catalyst component can be prepared by known methods. For example, an inert hydrocarbon such as pentane, hexane, heptane, or octane is used as a solvent. The carrier, electron donor compound, and halogen-containing silicon compound are added to the solvent, and the titanium compound is then added while stirring. Typically, 0.01 to 10 moles, preferably 0.05 to 5 moles, of the electron donor compound are added per mole of carrier, calculated as magnesium atoms. Also, 1 to 50 moles, preferably 2 to 20 moles, of the titanium compound are added per mole of carrier, calculated as magnesium atoms. The catalytic reaction is carried out at 0 to 200°C for 5 minutes to 10 hours, preferably at 30 to 150°C for 30 minutes to 5 hours. After the reaction is complete, the resulting solid catalyst component is preferably washed with an inert hydrocarbon such as n-hexane or n-heptane.
[0044] The solid catalyst component may also be a component obtained by contacting a liquid magnesium compound with a liquid titanium compound in the presence of an electron donor compound. The contact with the liquid titanium compound may be carried out in multiple batches.
[0045] Liquid magnesium compounds can be obtained, for example, by contacting a known magnesium compound with an alcohol, preferably in the presence of a liquid hydrocarbon medium, to form a liquid. Examples of magnesium compounds include magnesium halides such as magnesium chloride and magnesium bromide. Examples of alcohols include aliphatic alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, and 2-ethylhexyl alcohol. Examples of liquid hydrocarbon media include hydrocarbon compounds such as heptane, octane, and decane. The amount of alcohol used in preparing the liquid magnesium compound is usually 1.0 to 25 moles, preferably 1.5 to 10 moles, per mole of the magnesium compound. One or more liquid magnesium compounds can be used.
[0046] Examples of the liquid titanium compound include the titanium compound represented by the general formula (III) described above. The amount of the liquid titanium compound used per mole of magnesium atom (Mg) contained in the liquid magnesium compound is usually 0.1 to 1,000 moles, preferably 1 to 200 moles. One or more liquid titanium compounds can be used.
[0047] Examples of electron donor compounds include dicarboxylic acid ester compounds such as phthalic acid esters, acid anhydrides such as phthalic anhydride, organosilicon compounds such as dicyclopentyldimethoxysilane, dicyclohexyldimethoxysilane, and cyclohexylmethyldimethoxysilane, polyethers, acid halides, acid amides, nitriles, and organic acid esters. The amount of electron donor compound used per mole of magnesium atom (Mg) contained in the liquid magnesium compound is typically 0.01 to 5 moles, preferably 0.1 to 1 mole. One or more electron donor compounds can be used. The temperature during contact is typically −70 to 200°C, preferably 10 to 150°C.
[0048] (Organometallic Compound Catalyst Component) Among the catalyst components, the organometallic compound catalyst component is preferably an organoaluminum compound. Examples of the organoaluminum compound include compounds represented by general formula (IV).
[0049] AlR 2 n X 2 3-n ...(IV) In formula (IV), R 2 is an alkyl group, a cycloalkyl group or an aryl group having 1 to 10 carbon atoms, and X 2 is a halogen atom or an alkoxy group, preferably a chlorine atom or a bromine atom; and n is an integer of 1 to 3.
[0050] Specific examples of the organoaluminum compound include trialkylaluminum compounds such as trimethylaluminum, triethylaluminum, and triisobutylaluminum, diethylaluminum monochloride, diisobutylaluminum monochloride, diethylaluminum monoethoxide, and ethylaluminum sesquichloride.
[0051] The organoaluminum compounds can be used singly or in combination. The amount of the organometallic compound catalyst component used is usually 0.01 to 20 moles, preferably 0.05 to 10 moles, per mole of titanium atom in the solid catalyst component.
[0052] (Electron-Donor Compound Catalyst Component) Among the catalyst components, the electron-donor compound component to be supplied to the polymerization system is preferably an organosilicon compound. Examples of the organosilicon compound include dicyclopentyldimethoxysilane, cyclohexylmethyldimethoxysilane, diethylaminotriethoxysilane, diisopropyldimethoxysilane, and cyclohexylisobutyldimethoxysilane.
[0053] The amount of the electron donor compound used is usually 0.01 to 20 moles, preferably 0.1 to 5 moles, per mole of titanium atom in the solid catalyst component.
[0054] (Pretreatment) The solid catalyst component is preferably subjected to pretreatment such as prepolymerization before use in polymerization. For example, an inert hydrocarbon such as pentane, hexane, heptane, or octane is used as a solvent, and the solid catalyst component, organometallic compound catalyst component, and, if necessary, an electron donor compound component are added to the solvent, and propylene is supplied with stirring to cause the reaction. Propylene is preferably supplied under a propylene partial pressure higher than atmospheric pressure, and the pretreatment is carried out at 0 to 100°C for 0.1 to 24 hours. After completion of the reaction, the pretreated product is preferably washed with an inert hydrocarbon such as n-hexane or n-heptane.
[0055] <Propylene Polymer (B)> The intrinsic viscosity [η] of the propylene polymer (B) is in the range of 0.5 dl / g or more and 5 dl / g or less, preferably 0.5 dl / g or more and 3 dl / g or less, more preferably 0.5 dl / g or more and 2 dl / g or less.
[0056] When the intrinsic viscosity [η] is equal to or higher than the lower limit, the low-temperature sealability of the film obtained from the propylene-based polymer composition is good.When the intrinsic viscosity [η] is equal to or lower than the upper limit, the fluidity of the propylene-based polymer composition is high, and the moldability is good.
[0057] The propylene polymer (B) is a copolymer of propylene and an α-olefin (excluding propylene). Examples of the α-olefin include α-olefins having 2 to 12 carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 4-methyl-1-pentene, and 3-methyl-1-pentene. Among these α-olefins, ethylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene are preferred. One or more α-olefins can be used. The α-olefin (excluding propylene) content of the propylene polymer (B) is preferably 1 mol % to 10 mol %, more preferably 5 mol % to 10 mol %. When the α-olefin (excluding propylene) content is within this range, the low-temperature sealability of a film obtained from the propylene polymer composition is excellent.
[0058] <<Method for Producing Propylene Polymer (B)>> The method for producing the propylene polymer (B) is not particularly limited, and the propylene polymer (B) can be produced, for example, by copolymerizing propylene and an α-olefin using a Ziegler-Natta catalyst or a metallocene catalyst, and a commercially available propylene polymer can be used as the propylene polymer (B). The propylene polymer (B) preferably contains a propylene-α-olefin copolymer (B-1) and a propylene polymer (B-2).
[0059] <Propylene / α-olefin copolymer (B-1)> The intrinsic viscosity [η] of the propylene / α-olefin copolymer (B-1) is in the range of 0.5 dl / g or more and 2 dl / g or less, preferably 0.5 dl / g or more and 1.5 dl / g or less, and more preferably 0.7 dl / g or more and 1.2 dl / g or less.
[0060] When the intrinsic viscosity [η] is equal to or higher than the lower limit, the low-temperature sealability of the film obtained from the propylene-based polymer composition is good.When the intrinsic viscosity [η] is equal to or lower than the upper limit, the fluidity of the propylene-based polymer composition is high, and the moldability is good.
[0061] The propylene-α-olefin copolymer (B-1) is a copolymer of propylene and an α-olefin (excluding propylene). Examples of the α-olefin include α-olefins having 2 to 12 carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 4-methyl-1-pentene, and 3-methyl-1-pentene. Preferred α-olefins are ethylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene. One or more α-olefins can be used.
[0062] The content of structural units derived from α-olefins (excluding propylene) in the propylene-α-olefin copolymer (B-1) is 0.1 mol % to 10 mol %, preferably 4 mol % to 10 mol %, and more preferably 5 mol % to 8 mol %, assuming that the sum of the content of structural units derived from propylene and the content of structural units derived from α-olefins is 100 mol %. 13 It can be measured by C-NMR.
[0063] When the content of the structural units derived from the α-olefin is equal to or greater than the lower limit, the low-temperature sealability of the film obtained from the propylene-based polymer composition is good.When the content of the structural units derived from the α-olefin is equal to or less than the upper limit, the rigidity of the film obtained from the propylene-based polymer composition is good.
[0064] The molecular weight distribution (Mw / Mn) of the propylene / α-olefin copolymer (B-1), measured by the method employed in the examples described below, is 10 or more and 100 or less, preferably 10 or more and 50 or less, and more preferably 10 or more and 20 or less, where Mn is the number average molecular weight and Mw is the weight average molecular weight.
[0065] When the Mw / Mn is equal to or greater than the lower limit, the dispersibility with the propylene-α-olefin copolymer (A) is good, and a film with low FE can be produced. When the Mw / Mn is equal to or less than the upper limit, the oligomer component in the propylene polymer composition is low, and smoke generation during molding and stickiness of the film can be suppressed.
[0066] <<Method for Producing Propylene / α-olefin Copolymer (B-1)>> The propylene / α-olefin copolymer (B-1) can be produced by the method described in the section on the method for producing the propylene / α-olefin copolymer (A) above.
[0067] The propylene / α-olefin copolymer (B-1) is preferably produced by polymerizing raw material monomers in the presence of hydrogen as a molecular weight modifier under conditions of a polymerization temperature of preferably 20 to 80°C, more preferably 40 to 70°C, and a polymerization pressure of generally normal pressure to 9.8 MPa, preferably 0.2 to 4.9 MPa.
[0068] <Propylene Polymer (B-2)> The intrinsic viscosity [η] of the propylene polymer (B-2) is in the range of 0.5 dl / g or more and 5 dl / g or less, preferably 0.5 dl / g or more and 3 dl / g or less, more preferably 1 dl / g or more and 2 dl / g or less.
[0069] When the intrinsic viscosity [η] is equal to or higher than the lower limit, the melt tension of the propylene-based polymer composition is high, resulting in good film formability, whereas when the intrinsic viscosity [η] is equal to or lower than the upper limit, the fluidity of the propylene-based polymer composition is high, resulting in good formability.
[0070] The propylene polymer (B-2) is a copolymer of propylene and an α-olefin (excluding propylene). Examples of the α-olefin include α-olefins having 2 to 12 carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 4-methyl-1-pentene, and 3-methyl-1-pentene. Preferred α-olefins are ethylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene. One or more α-olefins can be used.
[0071] The content of structural units derived from α-olefins (excluding propylene) in the propylene polymer (B-2) is 1 mol % or more and 9 mol % or less, preferably 3 mol % or more and 9 mol % or less, and more preferably 5 mol % or more and 9 mol % or less, when the sum of the content of structural units derived from propylene and the content of structural units derived from α-olefins is taken as 100 mol %. 13 It can be measured by C-NMR.
[0072] When the content of the structural units derived from the α-olefin is equal to or greater than the lower limit, the low-temperature sealability of the film obtained from the propylene-based polymer composition is good.When the content of the structural units derived from the α-olefin is equal to or less than the upper limit, the rigidity of the film obtained from the propylene-based polymer composition is good.
[0073] The Mw / Mn of the propylene polymer (B-2) is 2 or more and less than 10, preferably 3 or more and less than 10, and more preferably 4 or more and less than 10.
[0074] When the Mw / Mn ratio is equal to or greater than the lower limit, the flowability is improved and the resin pressure during molding can be suppressed.When the Mw / Mn ratio is equal to or less than the upper limit, the content of oligomer components in the propylene polymer composition is reduced, and smoke generation during molding and stickiness of the film can be suppressed.
[0075] <<Method for Producing Propylene-Based Polymer (B-2)>> The method for producing the propylene-based polymer (B-2) is not particularly limited. For example, the propylene-based polymer (B-2) can be produced by copolymerizing propylene and an α-olefin using a Ziegler-Natta catalyst or a metallocene catalyst. Alternatively, a commercially available polypropylene-based polymer can be used.
[0076] <Propylene / α-olefin copolymer (C)> The propylene / α-olefin copolymer (C) contains the propylene / α-olefin copolymer (A) and the propylene / α-olefin copolymer (B-1).
[0077] When the total mass fraction of the propylene-α-olefin copolymer (A) and the propylene-α-olefin copolymer (B-1) is taken as 100 mass%, the mass fraction of the propylene-α-olefin copolymer (A) is 5 mass% or more and 50 mass% or less, and the mass fraction of the propylene polymer (B-1) is 50 mass% or more and 95 mass% or less. Here, the mass fraction of the propylene-α-olefin copolymer (A) is preferably 10 mass% or more and 40 mass% or less, more preferably 15 mass% or more and 35 mass% or less, and the mass fraction of the propylene polymer (B-1) is preferably 60 mass% or more and 90 mass% or less, more preferably 65 mass% or more and 85 mass% or less. When the mass fractions of the propylene-α-olefin copolymer (A) and the propylene-α-olefin copolymer (B-1) are within the above ranges, the dispersibility of the propylene-α-olefin copolymer (C) and the propylene-based polymer (B-2) becomes good, and the film obtained from the propylene-based polymer composition has excellent, well-balanced rigidity and low-temperature sealability.
[0078] <<Method for Producing Propylene / α-olefin Copolymer (C)>> The propylene / α-olefin copolymer (C) can be produced by the method described in the production conditions section for the propylene / α-olefin copolymer (A).
[0079] The propylene polymer composition of the present invention may contain additives such as weather stabilizers, heat stabilizers, antistatic agents, antislip agents, antiblocking agents, antifogging agents, nucleating agents, decomposing agents, pigments, dyes, nucleating agents, plasticizers, hydrochloric acid absorbers, antioxidants, crosslinking agents, crosslinking accelerators, reinforcing agents, fillers, softeners, processing aids, activators, moisture absorbents, adhesives, flame retardants, and mold release agents, within the scope of the object of the present invention. One or more additives may be used.
[0080] <Propylene-Based Polymer Composition> The propylene-based polymer composition according to the present invention contains the propylene / α-olefin copolymer (A) and the propylene-based polymer (B).
[0081] When the total mass fraction of the propylene-α-olefin copolymer (A) and the propylene polymer (B) is taken as 100% by mass, the mass fraction of the propylene-α-olefin copolymer (A) is 0.1% by mass or more and 8% by mass or less, and the mass fraction of the propylene polymer (B) is 92% by mass or more and 99.9% by mass or less. Here, the mass fraction of the propylene-α-olefin copolymer (A) is preferably 0.5% by mass or more and 7% by mass or less, more preferably 0.5% by mass or more and 6% by mass or less, and the mass fraction of the propylene polymer (B) is preferably 93% by mass or more and 99.5% by mass or less, more preferably 94% by mass or more and 99.5% by mass or less. When the mass fractions of the propylene-α-olefin copolymer (A) and the propylene polymer (B) are within the above ranges, a film obtained from the propylene polymer composition has excellent, well-balanced rigidity and low-temperature sealability.
[0082] The melting point of the propylene polymer composition, measured under the conditions employed in the examples described below, is 110°C or higher and 150°C or lower, preferably 115°C or higher and 150°C or lower, and more preferably 120°C or higher and 150°C or lower.
[0083] When the melting point is equal to or higher than the lower limit, the rigidity of the film obtained from the propylene polymer composition is good, and when the melting point is equal to or lower than the upper limit, the low-temperature sealability of the film obtained from the propylene polymer composition is good.
[0084] The content of structural units derived from α-olefins (excluding propylene) in the propylene polymer composition is 1 mol % or more and 10 mol % or less, preferably 3 mol % or more and 9 mol % or less, and more preferably 5 mol % or more and 8 mol % or less, when the total of the structural units of the polymer in the composition is 100 mol %. 13 It can be measured by C-NMR.
[0085] When the content of the structural units derived from the α-olefin is equal to or greater than the lower limit, the low-temperature sealability of the film obtained from the propylene-based polymer composition is good.When the content of the structural units derived from the α-olefin is equal to or less than the upper limit, the rigidity of the film obtained from the propylene-based polymer composition is good.
[0086] The melt flow rate (MFR) of the propylene polymer composition measured at 230°C under a load of 2.16 kg is 1 g / 10 min or more and 10 g / 10 min or less, preferably 2 g / 10 min or more and 9 g / 10 min or less, more preferably 4 g / 10 min or more and 7 g / 10 min or less.
[0087] When the MFR of the propylene-based polymer composition is equal to or higher than the lower limit, the propylene-based polymer composition has high fluidity and good moldability, whereas when the MFR of the propylene-based polymer composition is equal to or lower than the upper limit, the propylene-based polymer composition has high melt tension and good film moldability.
[0088] The propylene polymer composition according to the present invention may contain a propylene-α-olefin copolymer (C) containing the propylene-α-olefin copolymer (A) and the propylene-α-olefin copolymer (B-1), and the propylene polymer (B-2).
[0089] The intrinsic viscosities [η] of the propylene-α-olefin copolymer (B-1) and the propylene polymer (B-2) contained in the propylene polymer composition preferably satisfy the relationship (the intrinsic viscosity [η] of the copolymer (B-1))≦(the intrinsic viscosity [η] of the polymer (B-2)), and the difference between the two intrinsic viscosities [η] is preferably 3 dl / g or less. When the intrinsic viscosities [η] of the copolymer (B-1) and the polymer (B-2) contained in the propylene polymer composition satisfy the above relationship, surface roughness (poor appearance) is less likely to occur during film formation. A film made of a composition containing the propylene-α-olefin copolymer (A) and the propylene-based polymer (B) or a film made of a composition containing the propylene-α-olefin copolymer (A), the propylene-α-olefin copolymer (B-1), and the propylene-based polymer (B-2) may be surface-treated from the viewpoint of improving printability, adhesiveness, or adhesion to an adhesive. Specifically, the film may be subjected to a surface treatment (also referred to as a "surface activation treatment") such as corona treatment, flame treatment, plasma treatment, primer coating treatment, or ozone treatment. The composition of the present invention requires only a small amount of energy output for the surface treatment, and the surface treatment can be carried out efficiently in a short time.
[0090] When the total mass fraction of the propylene-α-olefin copolymer (C) and the propylene polymer (B-2) is taken as 100% by mass, the mass fraction of the propylene-α-olefin copolymer (C) is 1% by mass or more and 30% by mass or less, and the mass fraction of the propylene polymer (B-2) is 70% by mass or more and 99% by mass or less. Here, the mass fraction of the propylene polymer (C) is preferably 1% by mass or more and 25% by mass or less, more preferably 1% by mass or more and 20% by mass or less, and the mass fraction of the propylene polymer (B-2) is preferably 75% by mass or more and 99% by mass or less, more preferably 80% by mass or more and 99% by mass or less. When the mass fractions of the propylene-α-olefin copolymer (C) and the propylene polymer (B-2) are within the above ranges, a film obtained from the propylene polymer composition has excellent, well-balanced rigidity and low-temperature sealability.
[0091] <<Method for Producing Propylene-Based Polymer Composition>> The propylene-based polymer composition of the present invention can be produced by blending the above-mentioned components. The components may be blended sequentially in any order, or may be mixed simultaneously. Alternatively, a multi-stage mixing method may be employed in which some components are mixed and then other components are mixed.
[0092] For example, a propylene-based polymer composition can be produced by mixing a propylene-α-olefin copolymer (C) containing a relatively high molecular weight propylene-α-olefin copolymer (A) and a relatively low molecular weight propylene-α-olefin copolymer (B-1) obtained by two or more multistage polymerizations with a propylene-based polymer (B-2), and additives may be added as necessary.
[0093] Examples of the method for blending the components include a method in which the components are mixed or melt-kneaded simultaneously or sequentially using a mixing device such as a Banbury mixer, a single-screw extruder, a twin-screw extruder, a high-speed twin-screw extruder, etc. The polymer temperature during melt-kneading is usually 180 to 280°C, preferably 180 to 260°C.
[0094] The propylene-based polymer composition may contain structural units derived from at least one type of biomass-derived propylene or α-olefin. The same type of monomers constituting the polymer may be composed solely of biomass-derived monomers, solely of fossil fuel-derived monomers, or both of biomass-derived monomers and fossil fuel-derived monomers. The biomass-derived monomer is a monomer derived from any renewable natural raw material, such as a plant-derived or animal-derived material, including fungi, yeast, algae, and bacteria, and its residues, and contains carbon. 14 C isotope 1×10 -12 The biomass-derived propylene and α-olefin are contained in a proportion of about 100 (pMC) as measured in accordance with ASTM D6866. Biomass-derived propylene and α-olefins can be obtained, for example, by conventionally known methods. It is preferable that the propylene-based polymer composition contains structural units derived from biomass-derived monomers from the viewpoint of reducing environmental load (mainly greenhouse gas emissions). If the polymer production conditions, such as the polymerization catalyst and polymerization temperature in the polymerization process, are the same, even if the raw material monomer contains a biomass-derived monomer, 14 C isotope 1×10 -12 ~1 x 10 -14 Other than the proportion of propylene and α-olefin copolymers, the molecular structure is the same as that of propylene-α-olefin copolymers made from fossil fuel-derived monomers, and therefore the performance is said to be the same.
[0095] The propylene polymer composition may contain structural units derived from at least one chemically recycled propylene or α-olefin. The same type of monomer constituting the polymer may consist solely of chemically recycled monomers, or may consist solely of fossil fuel-derived monomers, or may contain chemically recycled monomers together with fossil fuel-derived monomers and / or biomass-derived monomers. Chemically recycled propylene and α-olefins can be obtained, for example, by conventionally known methods. It is preferable for the propylene polymer composition to contain structural units derived from chemically recycled monomers from the viewpoint of reducing environmental impact (mainly waste reduction). Even if the raw material monomer contains a chemically recycled monomer, the chemically recycled monomer is a monomer obtained by depolymerizing or pyrolyzing a polymer such as waste plastic back into a monomer unit such as propylene, or a monomer produced using such a monomer as a raw material. Therefore, if the polymer production conditions, such as the polymerization catalyst, polymerization process, and polymerization temperature, are equivalent, the molecular structure of the propylene-α-olefin copolymer will be equivalent to that of a fossil fuel-derived monomer. Therefore, the performance is also expected to be unchanged.
[0096] Various molded articles can be obtained by molding the polypropylene polymer composition of the present invention according to known molding techniques, such as film molding, sheet molding, calendar molding, pressure molding, vacuum molding, pipe molding, profile extrusion molding, blow molding, laminate molding, injection molding, injection stretch blow molding, compression molding, and injection compression molding.
[0097] <Film, Multilayer Film> The film of the present invention is formed from the propylene-based polymer composition of the present invention.
[0098] The thickness of the film of the present invention is usually less than 200 μm, preferably 10 to 150 μm, more preferably 15 to 100 μm. The film of the present invention has excellent rigidity, so that it can be easily made thinner.
[0099] Examples of methods for producing the film include extrusion molding methods such as the T-die method and inflation method, compression molding, calendar molding, and casting.
[0100] Film formation can be performed, for example, as follows: The components constituting the propylene polymer composition may be directly charged into a hopper or the like of a film forming machine, or the components may be premixed using a ribbon blender, a Banbury mixer, a Henschel mixer, a super mixer, or the like, or may be melt-kneaded using a kneader such as a single-screw or twin-screw extruder or a roll to obtain a propylene polymer composition, which may then be formed into a film.
[0101] A specific example of film production will be explained using the T-die method. The above components are charged into an extruder and melt-kneaded usually at a temperature of 180 to 280°C, preferably 200 to 270°C, and then extruded into a film form from the die lip of a T-die. The molten film is cooled and taken up by a take-up machine such as nip rolls to obtain a film.
[0102] Examples of methods for cooling the molten film include cooling using rolls and air, such as the air knife method or air chamber method; narrow pressure cooling, such as the polishing roll method, swing roll method or belt casting method; and contact cooling with a refrigerant, such as water cooling.
[0103] The obtained film can be subjected to a film treatment method commonly used in film molding, such as corona discharge treatment or liquid coating treatment.
[0104] The multilayer film of the present invention comprises the film of the present invention.
[0105] The multilayer film may be a multilayer film having two or more layers of the film of the present invention, or may be a multilayer film having one or more layers of the film of the present invention and one or more other layers. By using a multilayer structure, various functions can be further imparted to the film. Methods used in this case include coextrusion and extrusion coating.
[0106] Examples of the other layer include a barrier layer for gases such as water vapor and oxygen, a sound absorbing layer, a light shielding layer, an adhesive layer, a pressure-sensitive adhesive layer, a colored layer, a conductive layer, and a recycled resin-containing layer.Specific examples of materials for forming the other layer include an olefin polymer composition other than the propylene polymer composition, a gas barrier resin composition, and an adhesive resin composition.
[0107] The film and multilayer film of the present invention can be used as a packaging film in a wide range of packaging fields, such as packaging various foods such as fresh foods such as vegetables and fish, dried foods such as snacks and noodles, and water-based foods such as soups and pickles; packaging medical products such as medical products in various forms such as tablets, powders, and liquids, and medical peripheral materials; and packaging various electrical devices such as cassette tapes and electrical components.
[0108] The present invention will be described in more detail below based on examples, but is not limited to these examples. The various properties of the polymers, polymer compositions, and films obtained in each example were measured and evaluated as follows.
[0109] (1) Mass Fraction In the Production Examples, the mass fractions of the propylene polymer obtained in the first stage (corresponding to the propylene-α-olefin copolymer (A)) and the propylene polymer obtained in the second stage (corresponding to the propylene-α-olefin copolymer (B-1)) were determined from the amount of reaction heat generated during polymerization that was removed.
[0110] (2) Intrinsic Viscosity [η] The intrinsic viscosity [η] (dl / g) was measured at 135°C in a tetralin solvent. The intrinsic viscosity [η]2 of the propylene polymer obtained in the second stage (corresponding to the propylene-α-olefin copolymer (B-1)) was calculated using the following formula: [η]2 = ([η] total ×100-[η]1×W1) / W2 [η] total : intrinsic viscosity of the entire propylene polymer [η]1: intrinsic viscosity of the propylene polymer obtained in the first stage W1: mass fraction (%) of the propylene polymer obtained in the first stage W2: mass fraction (%) of the propylene polymer obtained in the second stage
[0111] (3) Comonomer content: o-Dichlorobenzene / benzene-d6 (4 / 1 v / v) was used as the measurement solvent, and the measurement was performed under the following conditions (AVANCE III manufactured by Bruker Biospin): measurement temperature 120°C, pulse repetition time 5.5 seconds, pulse width 5.00 μsec. 1 H-NMR spectra were measured and the comonomer content was calculated. The comonomer content of the propylene-α-olefin copolymer (B-1) was calculated using the following formula: Comonomer content of propylene-α-olefin copolymer (B-1) × mass fraction of propylene-α-olefin copolymer (B-1) = Comonomer content of propylene-α-olefin copolymer (C) × mass fraction of propylene-α-olefin copolymer (C) − Comonomer content of propylene-α-olefin copolymer (A) × mass fraction of propylene-α-olefin copolymer (A). The comonomer content, intrinsic viscosity [η], and Mw / Mn of the propylene-α-olefin copolymer (A) were calculated from the measured values of the propylene-α-olefin copolymer (A) polymerized under the same conditions as in the first stage.
[0112] (4) Melt Flow Rate (MFR) The melt flow rate (MFR) (g / 10 min) was measured in accordance with JIS-K7210 at a measurement temperature of 230° C. and a load of 2.16 kgf (21.2 N).
[0113] (5) Mw / Mn The average molecular weight (number average molecular weight Mn, weight average molecular weight Mw) was obtained by gel permeation chromatography (GPC) using the following equipment and conditions, and the molecular weight distribution (Mw / Mn) was calculated. Mw / Mn of the propylene-α-olefin copolymer (B-1) was calculated by creating a GPC chart of the propylene-α-olefin copolymer (B-1) using the difference between the GPC chart of the propylene-α-olefin copolymer (C) and the GPC chart of the propylene-α-olefin copolymer (A).
[0114] GPC measurement device: Gel permeation chromatograph HLC-8321 GPC / HT type (manufactured by Tosoh Corporation) Analysis device: Data processing software Empower 3 (manufactured by Waters Corporation) Measurement conditions: Column: TSKgel GMH6-HT x 2 + TSKgel GMH6-HTL x 2 (both 7.5 mm ID x 30 cm, manufactured by Tosoh Corporation) Column temperature: 140°C Mobile phase: o-dichlorobenzene (containing 0.025% BHT) Detector: Differential refractometer Flow rate: 1.0 mL / min Sample concentration: 0.05% (w / v) Injection volume: 0.4 mL Sampling time interval: 1 s Column calibration: Monodisperse polystyrene (manufactured by Tosoh Corporation) Molecular weight conversion: PP conversion / general-purpose calibration method
[0115] (6) Melting Point The crystalline melting point was determined by measuring in accordance with JIS-K7121 using a differential scanning calorimeter (DSC, manufactured by PerkinElmer (Diamond DSC)) under the following measurement conditions. The apex of the endothermic peak in the fourth step when the measurement was performed under the following measurement conditions was defined as the crystalline melting point (Tm). When there are multiple endothermic peaks, the apex of the endothermic peak with the greatest peak height is defined as the crystalline melting point (Tm).
[0116] (Measurement conditions) Measurement environment: Nitrogen gas atmosphere Sample amount: 5 mg Sample shape: Press film (formed at 230°C, thickness 400 μm) Sample pan: Aluminum sample pan with flat bottom First step: Heat from 30°C to 230°C at 50°C / min and hold for 10 minutes. Second step: Cool to 30°C at 10°C / min. Third step: Hold at 30°C for 1 minute. Fourth step: Heat to 230°C at 10°C / min.
[0117] (7) Film Elastic Modulus The tensile modulus (MPa) was measured according to the method of JIS K7161. The measurement was carried out at 23°C in the extrusion direction (MD) of molding and in the direction perpendicular to the MD (TD). The higher the tensile modulus, the higher the rigidity.
[0118] (8) Sealing initiation temperature Using a Toyo Seiki heat seal tester, a 100 mm wide, 150 mm long test piece was cut from the film produced in the examples, folded in half lengthwise, and heat-sealed at a predetermined heater temperature under conditions of a pressure of 0.2 MPa and a sealing time of 1.0 second. The sealed test piece was then cut into a 15 mm wide test piece, and the peel strength (N / 15 mm) was measured using an Orientec Tensilon RT1225 at a test speed of 300 mm / min. The heater temperature was changed in 1°C increments, and the minimum heater temperature (hereinafter referred to as the "sealing initiation temperature") required to achieve a peel strength of 2.94 N / 15 mm or more was determined.
[0119] (9) Haze: Measured in accordance with ASTM D1003 (JIS K7136:2000).
[0120] [Production Example 1] (1) Preparation of magnesium compound A reaction vessel equipped with a stirrer (internal volume: 500 L) was thoroughly purged with nitrogen gas, and 97.2 kg of ethanol, 640 g of iodine, and 6.4 kg of metallic magnesium were charged. The mixture was stirred under reflux conditions and reacted until no more hydrogen gas was generated from the system, yielding a solid reaction product. The reaction liquid containing this solid reaction product was dried under reduced pressure to obtain the target magnesium compound (support for a solid catalyst).
[0121] (2) Preparation of a solid titanium catalyst component 30 kg of the above-mentioned magnesium compound (unground), 150 L of purified heptane (n-heptane), 4.5 L of silicon tetrachloride, and 5.4 L of di-n-butyl phthalate were added to a reaction vessel (internal volume: 500 L) equipped with a stirrer and thoroughly purged with nitrogen gas. The system was kept at 90°C, and 144 L of titanium tetrachloride was added with stirring. The reaction was carried out at 110°C for 2 hours, after which the solid component was separated and washed with purified heptane at 80°C. Further, 228 L of titanium tetrachloride was added, and the reaction was carried out at 110°C for 2 hours. The solid component was then thoroughly washed with purified heptane to obtain a solid titanium catalyst component.
[0122] (3) Preparation of Prepolymerization Catalyst: 0.956 mL of triethylaluminum, 0.322 mL of dicyclopentyldimethoxysilane, and 1.677 g of the solid titanium catalyst component obtained in (2) above were placed in a 200 mL flask containing 130 mL of heptane. The internal temperature was maintained at 15-20°C, and 5.04 g of propylene was added. The reaction was carried out with stirring for 60 minutes. The reaction was then carried out with stirring for 10 minutes to allow the remaining propylene to react. After polymerization, the solid component was allowed to settle, and the supernatant was removed and washed twice with heptane. The resulting prepolymerization catalyst was resuspended in purified heptane to a total heptane weight of 140 mL. As a result, a prepolymerization catalyst slurry was obtained in which 3.0 g of propylene was polymerized per 1 g of the solid titanium catalyst component.
[0123] (4) Main Polymerization: 1.5 kg of propylene and 13 g of ethylene were charged into a 5-liter SUS autoclave that had been thoroughly purged with nitrogen. The temperature was then raised to 50°C with thorough stirring, and 0.07 mL of triethylaluminum, 0.02 mL of dicyclopentyldimethoxysilane, and 8.0 mg of the prepolymerization catalyst slurry obtained in (3) above as a solid titanium catalyst component were added. Polymerization was carried out at 70°C for 21 minutes with thorough stirring. The system was then depressurized, and the polymer was recovered (completion of first-stage polymerization). The propylene polymer (A) polymerized under the same conditions as in the first stage had an intrinsic viscosity [η] of 11.4 dl / g and a comonomer content of 7.2 mol%.
[0124] The system was thoroughly purged with nitrogen. After completion of the nitrogen purge, 1.5 kg of propylene, 45 NL of hydrogen, and 10 g of ethylene were charged in this order, and the temperature was raised to 50°C with thorough stirring, and polymerization was carried out for 120 minutes. Thereafter, the system was depressurized, and the polymer was recovered (completion of second-stage polymerization). The obtained polymer was dried under reduced pressure at 80°C for 6 hours, yielding 164.4 g of a powdery random propylene polymer.
[0125] The proportion of the propylene polymer (A) produced in the first-stage polymerization, the proportion of the propylene polymer (B-1) produced in the second-stage polymerization, the intrinsic viscosity [η], the comonomer content, and the Mw / Mn were all calculated from the mass balance to be 29% by mass and 71% by mass, respectively, of the propylene polymer.
[0126] To this propylene-based polymer, 2000 ppm of Irganox 1010 (manufactured by BASF), 2000 ppm of Irgaphos 168 (manufactured by BASF), and 1000 ppm of Sandstab P-EPQ (manufactured by Clariant Japan) were added as antioxidants, and 1000 ppm of calcium stearate as a neutralizer, and the mixture was melt-kneaded in a twin-screw extruder to obtain a pellet-shaped propylene-based polymer. The propylene-based polymer finally obtained in this manner had an MFR of 0.74 g / 10 min and a comonomer content of 7.4 mol%.
[0127] [Production Example 2] Polymerization was carried out in the same manner as in Production Example 1, except that the amount of catalyst in the first stage was 21 mg, the amount of ethylene was 4.0 g, the amount of triethylaluminum was 0.18 mL, and the amount of dicyclopentyldimethoxysilane was 0.06 mL, and the amount of ethylene in the second stage was 2.0 g, and the amount of hydrogen was 35 NL. As a result, 317.7 g of a random propylene polymer was obtained.
[0128] Production Example 3 According to the production method described in Example 1 of JP 2019-137848 A, a propylene polymer including a propylene polymer having an intrinsic viscosity [η] of 11 dl / g and a component amount of 25% by mass and a propylene polymer having an intrinsic viscosity [η] of 0.99 dl / g and a component amount of 75% by mass was produced.
[0129] The physical properties of the propylene polymers obtained in Production Examples 1 to 3 are shown in Table 1.
[0130]
[0131] [Production Example 4] (1) Preparation of magnesium compound A reaction vessel equipped with a stirrer (internal volume: 500 L) was thoroughly purged with nitrogen gas, and 97.2 kg of ethanol, 640 g of iodine, and 6.4 kg of metallic magnesium were charged. The mixture was stirred under reflux conditions and reacted until no more hydrogen gas was generated from the system, yielding a solid reaction product. The reaction liquid containing this solid reaction product was dried under reduced pressure to obtain the target magnesium compound (support for a solid catalyst).
[0132] (2) Preparation of Solid Catalyst Component 30 kg of the magnesium compound (unground), 150 L of purified heptane (n-heptane), 4.5 L of silicon tetrachloride, and 5.4 L of di-n-butyl phthalate were added to a reactor (internal volume: 500 L) equipped with a stirrer and thoroughly purged with nitrogen gas. The system was kept at 90°C, and 144 L of titanium tetrachloride was added with stirring. The reaction was carried out at 110°C for 2 hours, after which the solid component was separated and washed with purified heptane at 80°C. Further, 228 L of titanium tetrachloride was added, and the reaction was carried out at 110°C for 2 hours. The solid component was then thoroughly washed with purified heptane to obtain a solid catalyst component.
[0133] (3) Pretreatment: 230 L of purified heptane was placed in a 500 L reactor equipped with a stirrer, and 25 kg of the solid catalyst component, triethylaluminum at a ratio of 1.0 mol / mol relative to the titanium atoms in the solid catalyst component, and dicyclopentyldimethoxysilane at a ratio of 1.8 mol / mol relative to the titanium atoms in the solid catalyst component were supplied. Then, propylene was supplied at a propylene partial pressure of 0.3 kgf / cm. 2 The mixture was introduced until the temperature reached G, and the reaction was carried out for 4 hours at 25° C. After the reaction was completed, the solid catalyst component was washed several times with purified heptane, and carbon dioxide was further supplied and stirred for 24 hours.
[0134] (4) Polymerization The treated solid catalyst component was supplied to a 200-liter polymerization apparatus equipped with a stirrer at a rate of 3 mmol / hr in terms of titanium atoms in the component, triethylaluminum at 4 mmol / kg-PP, and dicyclopentyldimethoxysilane at 1 mmol / kg-PP, respectively, and the polymerization temperature was 80°C and the polymerization pressure (total pressure) was 28 kgf / cm. 2Propylene, ethylene, 1-butene, and hydrogen were reacted in the reactor G. At this time, the feed rates of ethylene, 1-butene, and hydrogen were adjusted so as to achieve the desired ethylene and 1-butene contents and MFR. The composition analysis values (gas chromatography analysis) of the gas part in the polymerization reactor showed an ethylene concentration of 3.5 mol%, a 1-butene concentration of 4.9 mol%, and a hydrogen concentration of 2.5 mol%.
[0135] To the propylene-ethylene-1-butene copolymer thus obtained, 2000 ppm of Irganox 1010 (manufactured by BASF), 2000 ppm of Irgaphos 168 (manufactured by BASF), and 1000 ppm of Sandstab P-EPQ (manufactured by Clariant Japan) were added as antioxidants, and 1000 ppm of calcium stearate was added as a neutralizing agent. The mixture was melt-kneaded in a twin-screw extruder to obtain a pellet-shaped propylene-ethylene-1-butene random copolymer.
[0136] [Production Example 5: F-704NP] Prime Polypro F-704NP, a product of Prime Polymer Co., Ltd., was used. For convenience, this is referred to as Production Example 5.
[0137] The physical properties of the polymer obtained above are shown in Table 2.
[0138]
[0139] Example 1 A 25 μm thick film made of a propylene polymer composition was produced under the following conditions using 5% by mass of the propylene-α-olefin copolymer obtained in Production Example 1 and 95% by mass of the propylene-ethylene-1-butene random copolymer obtained in Production Example 4. T-die film-forming machine: manufactured by Plastics Technology Research Institute Co., Ltd. Model: GT-25-A Screw diameter: 25 mm, L / D=24 Screw rotation speed: 100 rpm Cylinder temperature settings: C1=200° C., C2=220° C. Head temperature setting: 240° C. T-die temperature settings: D1 to D3=250° C. T-die width: 230 mm, lip opening=2 mm Film winding speed: 11 m / s Roll temperature: 40° C.
[0140] The physical properties of the film are shown in Table 3. Example 2, Comparative Examples 1 to 8 Films were produced in the same manner as in Example 1, except that the blending compositions were changed as shown in Table 3.
[0141] The results obtained above are shown in Table 3.
[0142]
[0143] (10) Wet tension after surface treatment <Corona treatment> Using a corona treater (HFSS-101) manufactured by Kasuga Electric Co., Ltd., high frequency waves were generated under conditions of 200 V and 5 A, and then a film sample piece was placed on the sample stage, and the speed was set so that the high frequency waves were applied to the film surface for about 5 seconds, and the film sample piece was passed through. <Wet tension> The test was carried out in accordance with JIS K6768:1999 using a wet tension test mixture manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0144]
Claims
1. A propylene-α-olefin copolymer (A) having an intrinsic viscosity [η] of 10 dl / g or more and 15 dl / g or less as measured in a tetralin solvent at 135°C and containing 5.0 mol% or more and 10 mol% or less of structural units derived from an α-olefin (excluding propylene); and a propylene-based polymer (B) having an intrinsic viscosity [η] of 0.5 dl / g or more and 5 dl / g or less as measured in a tetralin solvent at 135°C, wherein the mass fraction of the propylene-α-olefin copolymer (A) is 0.1 mass% or more and 8 mass% or less, and the mass fraction of the propylene-based polymer (B) is 92 mass% or more and 99.9 mass% or less, relative to 100 mass% of the total of the propylene-α-olefin copolymer (A) and the propylene-based polymer (B).
2. The propylene polymer composition according to claim 1, having a melting point of 110°C or higher and 150°C or lower.
3. The propylene-based polymer composition according to claim 2, wherein the content of structural units derived from α-olefins (excluding propylene) is 1 mol % or more and 10 mol % or less, when the total of the structural units of the polymer in the composition is 100 mol %.
4. The propylene polymer composition according to claim 3, which has a melt flow rate (MFR) measured at 230° C. under a load of 2.16 kg of 1 g / 10 min or more and 10 g / 10 min or less.
5. The propylene-based polymer (B) includes a propylene-α-olefin copolymer (B-1) having an intrinsic viscosity [η] of 0.5 dl / g or more and 2 dl / g or less, a content of structural units derived from α-olefins (excluding propylene) of 0.1 mol% or more and 10 mol% or less, and a molecular weight distribution (Mw / Mn (Mn is number average molecular weight, Mw is weight average molecular weight)) of 10 or more and 100 or less, and a propylene-based polymer (B-2) having an intrinsic viscosity [η] of 0.5 dl / g or more and 5 dl / g or less, a content of structural units derived from α-olefins (excluding propylene) of 1 mol% or more and 9 mol% or less, and a molecular weight distribution (Mw / Mn (Mn is number average molecular weight, Mw is weight average molecular weight)) of 2 or more and less than 10, 5. The propylene-based polymer composition according to claim 4, wherein, based on a total 100% by mass of the propylene-α-olefin copolymer (A) and the propylene-α-olefin copolymer (B-1), a mass fraction of the propylene-α-olefin copolymer (A) is 5% by mass or more and 50% by mass or less, and a mass fraction of the propylene-α-olefin copolymer (B-1) is 50% by mass or more and 95% by mass or less; and, based on a total 100% by mass of the propylene-α-olefin copolymer (A), the propylene-α-olefin polymer (B-1), and the propylene-based polymer (B-2), a mass fraction of the propylene-α-olefin copolymer (A) and the propylene-α-olefin polymer (B-1) is 1% by mass or more and 30% by mass or less, and a mass fraction of the propylene-based polymer (B-2) is 70% by mass or more and 99% by mass or less.
6. A film comprising the propylene polymer composition according to any one of claims 1 to 5.
7. A multi-layer film having a layer made of the propylene polymer composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Polypropylene resin composition
JP1985058459A
Polyolefin-based resin composition
JP1997208761A
Propylene polymer, polypropylene-based resin composition containing the same polymer and injection-molded article obtained from the same composition
JP2005146160A
Polypropylene resin foam for covering
JP2006045268A
Production process of olefin (CO)polymer composition and production process of pre-activated catalyst used for the same
JP2008037908A
Cited By
Propylene polymer composition, film, and multilayer film
JPWO2024210117A1