Positive electrode active material, positive electrode slurry, positive electrode sheet, battery, and electric device

By doping non-Mn elements and particle gradation in lithium manganese phosphate, the problems of low gram capacity and short cycle life of lithium-ion battery cathode active materials are solved, and battery performance with high energy density and long cycle life is achieved.

WO2024212182A1PCT designated stage expired Publication Date: 2024-10-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/088145
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The cathode active materials of lithium-ion batteries have problems such as low gram capacity, short cycle life and high manufacturing cost in industrial production and application. In particular, lithium manganese phosphate materials are prone to form an SEI film during the charge and discharge process, resulting in a decrease in energy density and Cycle life is shortened.

Method used

By doping lithium manganese phosphate with non-Mn elements and doping elements that meet specific ionic radius and valence change voltage conditions, the cathode active material formed has the effect of improving gram capacity, structural stability and cycle performance, and is passed through the particle level The selection of compounding and doping elements improves electronic conductivity and rate performance.

Benefits of technology

It achieves an increase in the gram capacity of the cathode active material, optimizes structural stability, extends cycle life and reduces manufacturing costs, while improving the energy density and cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023088145-FTAPPB-I100001
    Figure PCTCN2023088145-FTAPPB-I100001
  • Figure PCTCN2023088145-FTAPPB-I100002
    Figure PCTCN2023088145-FTAPPB-I100002
  • Figure 00000030_0000
    Figure 00000030_0000
Patent Text Reader

Abstract

The present application discloses a positive electrode active material, a positive electrode slurry, a positive electrode sheet, a battery, and an electric device. The positive electrode active material comprises: a first positive electrode active material, the first positive electrode active material comprising lithium manganese phosphate; and a second positive electrode active material, the second positive electrode active material being different from the first positive electrode active material, wherein the lithium manganese phosphate has a doping element, and the doping element satisfies at least one of the following conditions: the ionic radius of the doping element and the ionic radius of the manganese element satisfy the condition that |a-b| / b is not greater than 10%, wherein a is the ionic radius of the doping element, and b is the ionic radius of the manganese element; the valence variation voltage of the doping element is U, wherein 2 V<U<5.5 V; the chemical activity of a chemical bond formed by the doping element and O is not lower than the chemical activity of a P-O bond; and the highest valence of the doping element is not greater than 6.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material, positive electrode slurry, positive electrode sheet, battery and electrical device Technical field

[0001] The present disclosure relates to the field of batteries, and specifically, to positive electrode active materials, positive electrode slurries, positive electrode sheets, batteries and electrical devices. Background technique

[0002] With the development of lithium-ion battery technology, lithium-ion batteries have been widely used in energy storage power systems such as hydraulic, thermal, wind and solar power stations due to their high energy density, long cycle life and environmental friendliness, and have been widely used in many fields such as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. As the positive electrode active material of lithium-ion batteries, each has its own advantages and disadvantages. With the deepening of understanding and research, how to utilize the respective advantages of positive electrode active materials to improve the performance and stability of lithium-ion batteries has also begun to attract attention. At present, there are still many problems to be solved in the industrial production and application of lithium-ion batteries.

[0003] Application content

[0004] In the first aspect of the present application, the present application proposes a positive electrode active material, including: a first positive electrode active material, the first positive electrode active material includes lithium manganese phosphate; a second positive electrode active material, the second positive electrode active material is different from the first positive electrode active material, wherein, the lithium manganese phosphate has a doping element, and the doping element satisfies at least one of the following conditions: the ionic radius of the doping element and the ionic radius of manganese element satisfy: |a - b| / b is not greater than 10%, where a is the ionic radius of the doping element and b is the ionic radius of manganese element; the valence change voltage of the doping element is U, 2V < U < 5.5V; the chemical activity of the chemical bond formed by the doping element and O is not less than the chemical activity of the P - O bond; the highest valence of the doping element is not greater than 6. Thus, the positive electrode active material obtained by mixing different particles has a high specific capacity and excellent cycle performance.

[0005] According to an embodiment of the present application, the specific capacity of the second positive electrode active material is not less than the specific capacity of the first positive electrode active material. Thus, the specific capacity of the positive electrode active material can be increased.

[0006] According to an embodiment of the present application, the specific capacity of the first positive electrode active material is 135 mAh / g - 150 mAh / g, and the specific capacity of the second positive electrode active material is 170 mAh / g - 230 mAh / g. Thus, the specific capacity of the positive electrode active material can be further increased.

[0007] According to an embodiment of the present application, the discharge voltage platform of the positive electrode active material is no greater than the discharge voltage platform of the second positive electrode active material, thereby improving the structural stability of the positive electrode active material during the cycle.

[0008] According to an embodiment of the present application, the discharge voltage platform of the first positive electrode active material is no greater than the discharge voltage platform of the second positive electrode active material, thereby further improving the structural stability of the positive electrode active material during cycling.

[0009] According to an embodiment of the present application, the discharge voltage platform of the first positive electrode active material is 3.70 V-3.80 V, and the discharge voltage platform of the second positive electrode active material is 3.80 V-3.90 V. Thus, the energy density of the battery can be improved.

[0010] According to an embodiment of the present application, the compaction density of the positive electrode active material is not less than the compaction density of the first positive electrode active material under a pressure of 3 T. Thus, the energy density of a battery having the positive electrode active material can be increased.

[0011] According to an embodiment of the present application, the compaction density of the first positive electrode active material is no greater than the compaction density of the second positive electrode active material at a pressure of 3 T. Thus, the energy density of a battery having the positive electrode active material can be further improved.

[0012] According to an embodiment of the present application, at a pressure of 3T, the compaction density of the first positive electrode active material is 1.8 g / cm 3 -2.5g / cm 3 Under 3T pressure, the compaction density of the second positive electrode active material is 3.0g / cm 3 -3.4g / cm 3 Thus, the energy density of the battery having the positive electrode active material can be further improved.

[0013] According to an embodiment of the present application, the electronic conductivity of the second positive electrode active material is not less than the electronic conductivity of the first positive electrode active material at a temperature of 25° C. This can improve the electronic conductivity of the positive electrode active material and reduce the internal energy consumption of the positive electrode active material during the charge and discharge process.

[0014] According to an embodiment of the present application, the first positive electrode active material is a secondary particle, the secondary particles of the first positive electrode active material have a Dv50 particle size of 2 μm to 9 μm, and the primary particles of the first positive electrode active material have a Dv50 particle size of 10 nm to 600 nm. Thus, a positive electrode active material with a higher compaction density can be obtained through particle grading.

[0015] According to an embodiment of the present application, the first positive electrode active material is a primary particle, and the Dv50 particle size of the primary particle of the first positive electrode active material is 500 nm-1200 nm. Thus, a positive electrode active material with a higher compaction density can be obtained through particle grading.

[0016] According to an embodiment of the present application, the second positive electrode active material is a secondary particle, the secondary particles of the second positive electrode active material have a Dv50 particle size of 7 μm to 11 μm, and the primary particles of the second positive electrode active material have a Dv50 particle size of 50 nm to 800 nm. Thus, a positive electrode active material with a higher compaction density can be obtained through particle grading.

[0017] According to an embodiment of the present application, the second positive electrode active material is a primary particle, and the Dv50 particle size of the primary particle of the second positive electrode active material is 3000nm-5000nm. Thus, a positive electrode active material with a higher compaction density can be obtained through particle grading.

[0018] According to an embodiment of the present application, the mass fraction of the first positive electrode active material in the positive electrode active material is 10 wt % to 90 wt %, thereby improving the structural stability of the positive electrode active material and reducing the manufacturing cost.

[0019] According to an embodiment of the present application, the mass fraction of the second positive electrode active material in the positive electrode active material is 10 wt % to 90 wt %, thereby increasing the gram capacity of the positive electrode active material.

[0020] According to an embodiment of the present application, the Dv90 particle size of the positive electrode active material is 0.9 μm-8 μm, and the Dv10 particle size of the positive electrode active material is 0.2 μm-3.0 μm. Thus, a positive electrode active material with a higher gram capacity can be obtained.

[0021] According to an embodiment of the present application, the Dv90 particle size of the positive electrode active material is 0.9 μm-18 μm, and the Dv10 particle size of the positive electrode active material is 0.2 μm-7.0 μm. Thus, a positive electrode active material with excellent structural stability, excellent cycle life, and low manufacturing cost can be obtained.

[0022] According to an embodiment of the present application, the Dv50 particle size of the positive electrode active material is 0.5 μm-10 μm, thereby obtaining a positive electrode active material with higher gram capacity, better structural stability, better cycle life and lower manufacturing cost.

[0023] According to an embodiment of the present application, the mass fraction of manganese in the positive electrode active material is 10 wt % to 21 wt %, thereby further reducing the manufacturing cost of the positive electrode active material.

[0024] According to an embodiment of the present application, the ratio of the mass fraction of manganese element to the mass fraction of cobalt element in the positive electrode active material is (10:5)-(21:0.4). Thereby, it helps to improve the structural stability and conductivity of the positive electrode active material.

[0025] According to an embodiment of the present application, the ratio of the mass fraction of manganese element to the mass fraction of nickel element in the positive electrode active material is (10:30)-(21:6). Thereby, it helps to improve the specific capacity of the positive electrode active material.

[0026] According to an embodiment of the present application, the ratio of the mass fraction of manganese element to the mass fraction of iron element in the positive electrode active material is (10:13)-(21:0.8). Thereby, it helps to improve the structural stability of the positive electrode active material and reduce the manufacturing cost.

[0027] According to an embodiment of the present application, the ratio of the mass fraction of manganese element to the mass fraction of iron element in the first positive electrode active material is (6:4)-(7:3). Thereby, it helps to improve the structural stability of the positive electrode active material and reduce the production and manufacturing cost.

[0028] According to an embodiment of the present application, the doping element includes one or both of a first doping element and a second doping element. The first doping element is doped at the manganese site, and the second doping element is doped at the phosphorus site. Among them, the first doping element satisfies at least one of the following conditions: the ionic radius of the first doping element and the ionic radius of the manganese element satisfy: |a - b| / b is not greater than 10%, where a is the ionic radius of the first doping element and b is the ionic radius of the manganese element; the valence change voltage of the first doping element is U, 2V < U < 5.5V. Among them, the second doping element satisfies at least one of the following conditions: the chemical activity of the chemical bond formed by the second doping element and O is not less than the chemical activity of the P - O bond; the highest valence of the second doping element is not greater than 6. Thereby, the conductivity and specific capacity of the first positive electrode active material can be improved by the doping element, and the disadvantages of its poor stability and cycle life can be improved or even overcome to a certain extent.

[0029] According to an embodiment of the present application, at least two of the first doping elements are contained. Thereby, the conductivity and specific capacity of the first positive electrode active material can be further improved.

[0030] According to an embodiment of the present application, the first doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge. This can further reduce the lattice change rate of the first positive electrode active material and the surface activity of the first positive electrode active material, thereby suppressing Mn dissolution and side reactions at the interface between the positive electrode active material and the electrolyte.

[0031] According to an embodiment of the present application, the second doping element includes one or more elements selected from B (boron), S, Si, and N. This can increase the change rate of the Mn-O bond, improve the migration barrier of small polarons in the first positive electrode active material, and enhance the electronic conductivity.

[0032] According to an embodiment of the present application, the second positive electrode active material includes at least one of optionally doped lithium cobalt oxide, optionally doped lithium manganese oxide, optionally doped nickel-cobalt ternary material, and optionally doped lithium iron phosphate. This can further increase the specific capacity of the positive electrode active material.

[0033] According to the embodiment of the present application, the lithium cobalt oxide satisfies the general formula Li 1+z Co 1-x-y Ma x Mb y O2, wherein 0≤x≤0.01, 0≤y≤0.01, and -0.05≤z≤0.08; the Ma comprises a doped constant-valence element, including at least one of Al, Ga, Hf, Mg, Sn, Zn, and Zr; and the Mb comprises a doped variable-valence element, including at least one of Ni, Mn, V, Mo, Nb, Cu, Fe, In, W, and Cr. This improves the discharge voltage platform, cycle life, and rate capability of the positive electrode active material.

[0034] According to the embodiment of the present application, the lithium manganate satisfies the general formula Li a Mn 2-b M b O 4-c X c , wherein 0.9≤a≤1.2, 0≤b≤0.2, and 0≤c≤0.2; M and X are doping elements, M includes at least one of Li, Cr, Co, Ni, Mg, Ca, Sr, Ba, Na, K, Al, Be, B, Ti, Zr, Cu, Zn, Ga, Sn, or V; and the doping element X includes at least one of F, Cl, Br, I, or S. Thus, the specific capacity and cycle life of the positive electrode active material can be improved.

[0035] According to the embodiment of the present application, the nickel-cobalt ternary material satisfies the general formula Li a Ni bCo c M1 d M2 e O f R g , where 0.75 ≤ a ≤ 1.2, 0 < b < 1, 0 < c < 1, 0 < d < 1, 0 ≤ e ≤ 0.2, 1 ≤ f ≤ 2.5, 0 ≤ g ≤ 1, and f + g ≤ 3; M1 is Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and R includes at least one of N, F, S, Cl. Thus, the specific capacity per gram and the cycle life of the positive electrode active material can be improved.

[0036] According to an embodiment of the present application, the lithium iron phosphate satisfies the general formula LiFe a M b PO4, where 0.2 ≤ a < 1 and 0 < b ≤ 0.8; M includes one of Ti, Mg, V, Mn, Cr, Zr, Nb, W. Thus, the cycle life of the positive electrode active material can be improved.

[0037] According to an embodiment of the present application, the energy density of the film layer formed when the positive electrode active material is disposed on the surface of the positive electrode current collector is not less than the energy density of the film layer formed when the first positive electrode active material is disposed on the surface of the positive electrode current collector. Thus, the battery containing the aforementioned positive electrode active material has a high energy density.

[0038] In a second aspect of the present application, the present application provides a positive electrode paste, comprising: the aforementioned positive electrode active material. Thus, the positive electrode paste has all the characteristics and advantages of the aforementioned positive electrode active material, which will not be elaborated herein.

[0039] In a third aspect of the present application, the present application provides a positive electrode plate, comprising: a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector, the positive electrode active material layer comprising the aforementioned positive electrode active material, and / or, the positive electrode active material layer is formed using the aforementioned positive electrode paste. Thus, the positive electrode plate has all the characteristics and advantages of the aforementioned positive electrode active material and the aforementioned positive electrode paste, which will not be elaborated herein.

[0040] According to an embodiment of the present application, the mass fraction of manganese in the positive electrode active material layer is 10 wt% - 21 wt%. Thus, the structural stability of the positive electrode active material can be improved and the manufacturing cost can be reduced.

[0041] According to an embodiment of the present application, the ratio of the mass fraction of manganese to the mass fraction of cobalt in the positive electrode active material layer is (10:5) - (21:0.4). Thus, it helps to reduce the film resistivity of the positive electrode plate.

[0042] According to an embodiment of the present application, the ratio of the mass fraction of manganese to the mass fraction of nickel in the positive electrode active material layer is (10:30)-(21:6), thereby helping to improve the energy density of the positive electrode sheet.

[0043] According to an embodiment of the present application, the ratio of the mass fraction of manganese to the mass fraction of iron in the positive electrode active material layer is (10:13)-(21:0.8), which helps to improve the cycle performance of the positive electrode sheet.

[0044] According to the embodiment of the present application, the area of ​​1×10 -4 cm 2 The positive electrode sheet is provided with a region located on a side of the positive electrode active material layer away from the positive electrode current collector, wherein the amount of the first positive electrode active material in the region is not less than the amount of the second positive electrode active material. Thus, the energy density and cycle life of the positive electrode sheet can be improved.

[0045] In a fourth aspect of the present application, a battery is provided, comprising: the aforementioned positive electrode active material and / or the aforementioned positive electrode sheet. Thus, the battery has all the features and advantages of the aforementioned positive electrode active material and the aforementioned positive electrode sheet, which will not be further elaborated here.

[0046] In a fifth aspect of the present application, an electrical device is provided, comprising: the aforementioned positive electrode active material, and / or the aforementioned positive electrode sheet, and / or the aforementioned battery. Thus, the electrical device possesses all the features and advantages of the aforementioned positive electrode active material, the aforementioned positive electrode sheet, and the aforementioned battery, and no further description is given here. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0048] FIG1 is a schematic diagram of a battery according to one embodiment of the present application;

[0049] FIG2 is an exploded view of a battery according to an embodiment of the present application shown in FIG1 ;

[0050] FIG3 is a schematic diagram of a battery module according to one embodiment of the present application;

[0051] FIG4 is a schematic diagram of a battery pack according to one embodiment of the present application;

[0052] FIG5 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG4 ;

[0053] FIG6 is a schematic diagram of an electric device using a battery as a power source according to an embodiment of the present application. DETAILED DESCRIPTION

[0054] Embodiments of the present application will be described in detail below. Examples of the embodiments are shown in the accompanying drawings, where the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below by referring to the accompanying drawings are exemplary and are only used to explain the present application and should not be construed as a limitation to the present application. Unless otherwise specified, all technical terms used in the present application have the same meaning as commonly understood by those skilled in the art to which the present application belongs. All patents and published publications related to the present application are incorporated into the present application by reference in their entirety. The term "comprising" or "including" is an open expression, that is, it includes the content specified in the present application, but does not exclude other aspects.

[0055] While lithium manganese phosphate has advantages such as low cost and excellent thermal runaway performance, it also has defects such as low specific capacity and fast initial cycle decay. For example, during the first charge-discharge process of the battery cell, the electrolyte will undergo a reduction decomposition reaction on the surface of the negative electrode and form a solid electrolyte interface film (SEI film). The formation of the SEI film will consume a large amount of active lithium, resulting in a decrease in the actual energy density of the battery compared to the theoretical calculated value. During the cycling process of the battery cell, phenomena such as cracking and pulverization of lithium manganese phosphate particles and thickening and repair of the SEI film will continuously consume active lithium, causing a significant decrease in the cycle life of the battery. By mixing a first positive electrode active material including lithium manganese phosphate with a second positive electrode active material different from the first positive electrode active material, the obtained positive electrode active material has the respective advantages of the first positive electrode active material and the second positive electrode active material, which can make the positive electrode active material have high structural stability, high specific capacity, and low manufacturing cost. A battery having the aforementioned positive electrode active material has both high energy density, excellent cycle life, and low manufacturing cost.

[0056] In a first aspect of the present application, the present application provides a positive electrode active material, comprising: a first positive electrode active material, the first positive electrode active material including lithium manganese phosphate; a second positive electrode active material, the second positive electrode active material being different from the first positive electrode active material, wherein the lithium manganese phosphate has a doping element, and the doping element satisfies at least one of the following conditions: the ionic radius of the doping element and the ionic radius of manganese element satisfy: |a - b| / b is not greater than 10%, where a is the ionic radius of the doping element and b is the ionic radius of manganese element; the valence change voltage of the doping element is U, 2V < U < 5.5V; the chemical activity of the chemical bond formed by the doping element and O is not less than the chemical activity of the P - O bond; the highest valence of the doping element is not greater than 6.

[0057] The present application can achieve at least one of the following effects by doping non-Mn elements in lithium manganese phosphate: 1) reducing the lattice change rate of the first positive electrode active material to reduce the lattice constant difference between the two phases at the grain boundary, reduce the interface stress, and enhance the Li + The invention discloses the following three aspects: 1) the transmission capacity at the interface, thereby improving the rate performance of the positive electrode active material; 2) promoting the utilization of the capacity of the first positive electrode active material and improving the battery capacity; 3) making the bond length change rate of the Mn-O bond faster, reducing the migration barrier of the small polaron of the first positive electrode active material, thereby improving the electronic conductivity; 4) reducing the activity of oxygen on the surface of the first positive electrode active material, thereby inhibiting the dissolution of Mn and reducing the interfacial side reaction between the positive electrode active material and the electrolyte; 5) reducing the concentration of antisite defects in the material, thereby improving the kinetic performance and specific capacity of the positive electrode active material; 6) changing the morphology of the first positive electrode active material, thereby improving the compaction density.

[0058] In the present application, by mixing the second positive electrode active material with the first positive electrode active material, the positive electrode active material has the advantages of the first positive electrode active material while also having the advantages of the second positive electrode active material. For example, when the second positive electrode active material and the first positive electrode active material are of different material types, the positive electrode active material can have a higher gram capacity and better structural stability; when the second positive electrode active material and the first positive electrode active material have different particle sizes, by grading the particle sizes of the second positive electrode active material and the first positive electrode active material, a positive electrode active material with lower manufacturing cost, a positive electrode active material layer with higher compaction density, and a battery with higher energy density can be obtained. By using the positive electrode active material obtained by mixing the two particles, the battery can simultaneously take into account higher energy density, better cycle life, and lower manufacturing cost.

[0059] According to some embodiments of the present application, the gram capacity of the second positive electrode active material may be no less than the gram capacity of the first positive electrode active material. By mixing the second positive electrode active material having a gram capacity greater than or equal to that of the first positive electrode active material with the second positive electrode active material, the positive electrode active material can have a higher gram capacity while having better structural stability and lower manufacturing cost.

[0060] According to some embodiments of the present application, the gram capacity of the first positive electrode active material may be 135 mAh / g-150 mAh / g.

[0061] In some embodiments, the gram capacity of the first positive active material can be 135 mAh / g, 136 mAh / g, 137 mAh / g, 138 mAh / g, 139 mAh / g, 140 mAh / g, 141 mAh / g, 142 mAh / g, 143 mAh / g, 144 mAh / g, 145 mAh / g, 146 mAh / g, 147 mAh / g, 148 mAh / g, 149 mAh / g, or 150 mAh / g.

[0062] According to some embodiments of the present application, the gram capacity of the second positive electrode active material may be 170 mAh / g-230 mAh / g.

[0063] In some embodiments, the second positive active material can have a passenger capacity of 170 mAh / g, 175 mAh / g, 180 mAh / g, 185 mAh / g, 190 mAh / g, 195 mAh / g, 200 mAh / g, 205 mAh / g, 210 mAh / g, 215 mAh / g, 220 mAh / g, 225 mAh / g, or 230 mAh / g.

[0064] As an example, the gram capacity can be tested by referring to the following method: the positive electrode active material to be tested is assembled into a button battery for testing. The button battery is charged to 4.3V at 0.1C, and then charged at a constant voltage at 4.3V to a current less than or equal to 0.05mA. After standing for 5 minutes, it is then discharged to 2.0V at 0.1C. The discharge capacity at this time is the gram capacity.

[0065] As an example, the assembly of button batteries can refer to the following method: (1) Preparation of positive electrode sheet: Add positive electrode active material, polyvinylidene fluoride (PVDF), and conductive carbon to a certain amount of N-methylpyrrolidone (NMP), and the mass ratio of positive electrode active material: binder: conductive agent is 90:5:5. Stir in a drying room to form a uniform positive electrode slurry, and control the viscosity to be 3000Pa·S-10000mPa·S. Apply the above positive electrode slurry on aluminum foil, and make positive electrode sheet after drying. Use a punching machine to prepare the positive electrode sheet into a 7mm radius round sheet for standby use; (2) Preparation of negative electrode sheet: The negative electrode current collector is selected to be a metal lithium sheet with a radius of 8mm and a thickness of 0.6mm; (3) Preparation of electrolyte: The electrolyte is 1mol / L A mixed solution of LiPF6 solution and 5wt.% fluoroethylene carbonate (FEC), wherein the solvent of the LiPF6 solution is ethylene carbonate (EC): diethyl carbonate (DEC): dimethyl carbonate (DMC) in a volume ratio of 1:1:1; (4) Button battery assembly: The assembly process needs to be performed in an inert atmosphere glove box. The battery shell is CR2032 model. The positive electrode shell is placed flat on a glass plate with the opening facing up. The gasket and the positive electrode sheet are placed in the positive electrode shell in sequence with insulating tweezers. The positive electrode sheet is located in the center of the positive electrode shell. A pipette is used to draw 10μl of electrolyte and drop it on the positive electrode. On the surface of the electrode, wet the positive electrode, clamp the separator (radius 9.5mm, thickness 14μm, PE material + double-sided coated ceramic) to cover the positive electrode, use a pipette to draw 10μl of electrolyte and drop it on the surface of the separator, clamp the lithium sheet and place it in the middle of the separator, clamp the gasket and place it in the center of the lithium sheet, clamp the spring and place it on the gasket, align them strictly, clamp the negative electrode shell, cover it with the opening facing down, use insulated tweezers to place the button battery with the negative side facing up on the button battery sealing machine mold, adjust the pressure to 800Pa and press for 5s to complete the button battery assembly, wipe the button battery shell clean with a paper towel, and it can be used for testing.

[0066] According to some embodiments of the present application, the charge and discharge platforms of a first positive electrode active material and a second positive electrode active material having different discharge voltage platforms can complement each other and produce a synergistic effect, thereby achieving an optimal match between the ion conductivity and the electronic conductivity of the positive electrode plate, and the lithium ion solid phase diffusion coefficient and resistance of the positive electrode plate are both within an optimal range, thereby significantly improving the rate performance of the battery. For example, the discharge voltage platform of the positive electrode active material can be no greater than the discharge voltage platform of the second positive electrode active material, thereby significantly improving the structural stability of the positive electrode active material during the cycle process.

[0067] According to some embodiments of the present application, when the discharge voltage platform of the first positive electrode active material is not greater than the discharge voltage platform of the second positive electrode active material, the discharge voltage platform of the positive electrode active material can be made less than or equal to the discharge voltage platform of the second positive electrode active material.

[0068] According to some embodiments of the present application, the discharge voltage platform of the first positive electrode active material may be 3.70V-3.80V.

[0069] In some embodiments, the discharge voltage plateau of the first cathode active material may be 3.70V, 3.71V, 3.72V, 3.73V, 3.74V, 3.75V, 3.76V, 3.77V, 3.78V, 3.79V, or 3.80V.

[0070] According to some embodiments of the present application, the discharge voltage platform of the second positive electrode active material may be 3.80V-3.90V.

[0071] In some embodiments, the discharge voltage plateau of the first cathode active material may be 3.80V, 3.81V, 3.82V, 3.83V, 3.84V, 3.85V, 3.86V, 3.87V, 3.88V, 3.89V, or 3.90V.

[0072] As an example, the discharge voltage platform can be tested by referring to the following method: the positive electrode active material to be tested is assembled into a button cell for gram capacity test, and the discharge voltage platform can be calculated using the formula: discharge voltage platform = discharge energy / discharge capacity.

[0073] According to some embodiments of the present application, the compaction density is closely related to the energy density, rate capability, internal resistance, and cycle life of the positive electrode sheet. In the present application, under a pressure of 3T, the compaction density of the positive electrode active material may be no less than the compaction density of the first positive electrode active material. By adding the second positive electrode active material, the gaps between the second positive electrode active material in the positive electrode active material layer can be filled with the first positive electrode active material, thereby increasing the compaction density of the positive electrode active material.

[0074] According to some embodiments of the present application, the compaction density of the first positive electrode active material and the compaction density of the second positive electrode active material are not particularly limited. For example, under a pressure of 3T, the compaction density of the first positive electrode active material may not be greater than the compaction density of the second positive electrode active material.

[0075] According to some embodiments of the present application, at a pressure of 3T, the compaction density of the first positive electrode active material may be 1.8 g / cm 3 -2.5g / cm 3 At a pressure of 3T, the compaction density of the second positive electrode active material can be 3.0 g / cm 3 -3.4g / cm 3When the compaction density of the first positive electrode active material and the compaction density of the second positive electrode active material are within the above range, the positive electrode active material particles are fully in contact with each other without blocking the ion movement channel. At the same time, it ensures that the electrons have good conductivity and rapid ion movement during high current discharge, reduces discharge polarization, and improves the discharge voltage platform.

[0076] In some embodiments, at a pressure of 3T, the compaction density of the first positive electrode active material may be 1.8 g / cm 3 , 1.9g / cm 3 , 2.0g / cm 3 , 2.1g / cm 3 , 2.2g / cm 3 , 2.3g / cm 3 , 2.4g / cm 3 or 2.5g / cm 3 .

[0077] In some embodiments, at a pressure of 3T, the compaction density of the second positive electrode active material may be 3.0 g / cm 3 , 3.1g / cm 3 、3.2g / cm 3 , 3.3g / cm 3 or 3.4g / cm 3 .

[0078] As an example, the compaction density can be tested by referring to the following method: take 5g of powder and place it in a special compaction mold (American CARVER mold, model 13mm), and then place the mold on the compaction density instrument. Apply a pressure of 3T, read the thickness of the powder under pressure on the device (the thickness after unloading), and calculate the compaction density by ρ=m / v. The area value used is the standard small picture area of ​​1540.25mm 2 .

[0079] According to some embodiments of the present application, the electronic conductivity of the second positive electrode active material is no less than that of the first positive electrode active material at a temperature of 25°C. The addition of the second positive electrode active material can effectively improve the overall electronic conductivity of the positive electrode active material, resulting in the positive electrode active material having superior electrical conductivity and lower internal resistance.

[0080] As an example, the electronic conductivity of the positive electrode active material can be tested by the following method: take a clean glass slide with a width of b, and use conductive silver glue to fix the first / second / third / fourth copper wires (circular cross-section, cross-sectional diameter of 0.1 mm) on the glass slide in sequence. The four wires are arranged parallel to each other (the wires are parallel to the width of the glass slide), the distance between the first wire and the second wire and the distance between the third wire and the fourth wire are equal to 10 mm, and the distance between the second and third wires is 50 mm. One end of the four wires is flush with the edge of the glass slide, and the other end extends outside the glass slide; the positive electrode active material and N-methylpyrrolidone are mixed into a slurry in a mass ratio of 75:25 and applied to the above-mentioned glass slide (complete coverage), and the coating thickness is controlled to be 0.1 mm. Then, the glass slide is placed in a vacuum oven at 100°C and dried for 2 hours and then taken out. An ammeter is used to test the current I between the first wire and the fourth wire and the voltage U between the second wire and the third wire. The conductivity = (I×50) / (U×0.1×b), and the unit is S / mm.

[0081] According to some embodiments of the present application, when the first positive electrode active material is a secondary particle, the Dv50 particle size of the secondary particle of the first positive electrode active material can be 2μm-9μm, and the Dv50 particle size of the primary particle of the first positive electrode active material can be 10nm-600nm. The size of the first positive electrode active material particles will affect the processing of the positive electrode active material and the compaction density performance of the positive electrode sheet. By selecting a first positive electrode active material with an average particle size of the primary particles within the above range, it is possible to effectively reduce the agglomeration of the first positive electrode active material particles caused by the average particle size of the primary particles of the first positive electrode active material being too small, making it difficult to disperse it in the positive electrode slurry and requiring more binder, resulting in poor brittleness of the electrode sheet; and reduce the occurrence of the situation where the gaps between the positive electrode active material particles are large, the internal resistance is increased, and the compaction density is reduced due to the average particle size of the primary particles of the first positive electrode active material particles being too large.

[0082] In some embodiments, when the first positive electrode active material is a secondary particle, the Dv50 particle size of the secondary particles of the first positive electrode active material may be 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm or 9μm, and the Dv50 particle size of the primary particles of the first positive electrode active material may be 10nm, 20nm, 50nm, 80nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 550nm or 600nm.

[0083] According to some embodiments of the present application, when the first positive electrode active material is a primary particle, the Dv50 particle size of the first positive electrode active material may be 500 nm-1200 nm.

[0084] In some embodiments, when the first positive active material is a primary particle, the Dv50 particle size of the first positive active material can be 500nm, 550nm, 600nm, 650nm, 700nm, 750nm, 800nm, 850nm, 900nm, 950nm, 1000nm, 1050nm, 1100nm, 1150nm or 1200nm.

[0085] According to some embodiments of the present application, when the second positive electrode active material is a secondary particle, the Dv50 particle size of the secondary particles of the second positive electrode active material can be 7μm-11μm, and the Dv50 particle size of the primary particles of the second positive electrode active material can be 50nm-800nm. By using a second positive electrode active material having a particle size slightly larger than that of the first positive electrode active material to form a positive electrode active material, the first positive electrode active material can fill the gaps between the second positive electrode active material in the positive electrode active material layer, thereby increasing the compaction density of the positive electrode active material and reducing the internal resistance of the positive electrode active material.

[0086] In some embodiments, when the second positive electrode active material is a secondary particle, the Dv50 particle size of the secondary particles of the second positive electrode active material may be 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm or 11 μm, and the Dv50 particle size of the primary particles of the first positive electrode active material may be 50 nm, 70 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm or 800 nm.

[0087] According to some embodiments of the present application, when the second positive electrode active material is a primary particle, the Dv50 particle size of the second positive electrode active material is 3000 nm-5000 nm.

[0088] In some embodiments, when the second cathode active material is a primary particle, the Dv50 particle size of the second cathode active material may be 3000 nm, 3200 nm, 3400 nm, 3600 nm, 3800 nm, 4000 nm, 4200 nm, 4400 nm, 4600 nm, 4800 nm, or 5000 nm.

[0089] According to some embodiments of the present application, the mass fraction of the first positive electrode active material in the positive electrode active material may be 10 wt %-90 wt %. When the mass fraction of the first positive electrode active material in the positive electrode active material is within the above range, the positive electrode active material has higher structural stability and lower manufacturing cost.

[0090] In some embodiments, the mass fraction of the first positive electrode active material in the positive electrode active material can be 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt% or 90wt%.

[0091] According to some embodiments of the present application, the mass fraction of the second positive electrode active material in the positive electrode active material may be 10 wt %-90 wt %. When the mass fraction of the second positive electrode active material in the positive electrode active material is within the above range, the positive electrode active material has a higher gram capacity.

[0092] In some embodiments, the mass fraction of the second positive electrode active material in the positive electrode active material can be 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt% or 90wt%.

[0093] In this application, the ratio of the first positive electrode active material to the second positive electrode active material in the positive electrode active material may affect the electrical properties of the positive electrode active material, such as specific capacity and structural stability. For example, when the content of a certain material in the positive electrode active material is high, the performance advantages of the material are more evident in the positive electrode active material.

[0094] According to some embodiments of the present application, according to different ratios of the first positive electrode active material and the second positive electrode active material, the particle size range of the positive electrode active material will fluctuate and adjust accordingly. For example, when the positive electrode active material contains a larger amount of the second positive electrode active material and a smaller amount of the first positive electrode active material, the Dv90 particle size of the positive electrode active material can be 0.9μm-8μm, and the Dv10 particle size of the positive electrode active material can be 0.2μm-3.0μm. When the difference in Dv50 particle size between the first positive electrode active material and the second positive electrode active material is not less than 2.2μm, there will be two peaks in the Dv10 particle size in the particle size distribution of the positive electrode active material, corresponding to the particle size of the first positive electrode active material and the particle size of the second positive electrode active material respectively; there will be a single peak in the Dv90 particle size of the positive electrode active material in the particle size distribution, corresponding to the particle size of the second positive electrode active material. When the difference in Dv50 particle size between the first positive electrode active material and the second positive electrode active material is less than 2.2 μm, there is only a single peak in the Dv10 particle size in the particle size distribution of the positive electrode active material, which corresponds to the particle size of the mixed particles after the first positive electrode active material and the second positive electrode active material are mixed, and there is a single peak in the Dv90 particle size of the positive electrode active material in the particle size distribution, which corresponds to the particle size of the second positive electrode active material.

[0095] According to some embodiments of the present application, when the positive electrode active material contains a smaller amount of the second positive electrode active material and a larger amount of the first positive electrode active material, the Dv90 particle size of the positive electrode active material may be 0.9 μm-18 μm, and the Dv10 particle size of the positive electrode active material may be 0.2 μm-7.0 μm. When the difference in Dv50 particle size between the first positive electrode active material and the second positive electrode active material is not less than 2.2 μm, the Dv10 particle size in the particle size distribution of the positive electrode active material will have two peaks, corresponding to the particle size of the first positive electrode active material and the particle size of the second positive electrode active material, respectively; and the Dv90 particle size of the positive electrode active material in the particle size distribution will have a single peak, corresponding to the particle size of the first positive electrode active material. When the difference in Dv50 particle size between the first positive electrode active material and the second positive electrode active material is less than 2.2 μm, there is only a single peak in the Dv10 particle size in the particle size distribution of the positive electrode active material, which corresponds to the particle size of the mixed particles after the first positive electrode active material and the second positive electrode active material are mixed, and there is a single peak in the Dv90 particle size of the positive electrode active material in the particle size distribution, which corresponds to the particle size of the first positive electrode active material.

[0096] According to some embodiments of the present application, when the positive electrode active material contains a second positive electrode active material and a first positive electrode active material in similar amounts, the Dv50 particle size of the positive electrode active material can be 0.5μm-10μm. When the difference in Dv50 particle size between the first positive electrode active material and the second positive electrode active material is not less than 2.2μm, there will be two peaks in the Dv50 particle size distribution of the positive electrode active material, corresponding to the particle size of the first positive electrode active material and the particle size of the second positive electrode active material, respectively, and the difference between the two peaks is not less than 2.2μm. When the difference in Dv50 particle size between the first positive electrode active material and the second positive electrode active material is less than 2.2μm, there will be a single peak in the Dv50 particle size distribution of the positive electrode active material, corresponding to the particle size of the mixed particles after the first positive electrode active material and the second positive electrode active material are mixed.

[0097] The aforementioned Dv90 particle size refers to the particle size corresponding to when the cumulative volume distribution percentage of the positive electrode active material reaches 90%. The aforementioned Dv50 particle size refers to the particle size corresponding to when the cumulative volume distribution percentage of the positive electrode active material reaches 50%. The aforementioned Dv10 particle size refers to the particle size corresponding to when the cumulative volume distribution percentage of the positive electrode active material reaches 10%. In the present application, the Dv90 particle size, Dv50 particle size, and Dv10 particle size of the positive electrode active material can all be measured using laser diffraction particle size analysis. As an example, the particle size of the positive electrode active material can be measured with reference to the standard GB / T 19077-2016 using a laser particle size analyzer (such as Malvern Master Size 3000).

[0098] According to some embodiments of the present application, the mass fraction of manganese in the positive electrode active material may be 10 wt% to 21 wt%. When the mass fraction of manganese in the positive electrode active material is within the aforementioned range, it can effectively avoid problems such as poor structural stability and decreased density of the positive electrode active material that may be caused by an excessive manganese content, thereby improving the battery's cycling, storage, and compaction density performance. It can also avoid problems such as a low discharge voltage plateau that may be caused by an excessively low manganese content, thereby improving the battery's energy density.

[0099] In some embodiments, the mass fraction of manganese in the positive electrode active material can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt% or 21wt%.

[0100] According to some embodiments of the present application, the ratio of the mass fraction of manganese to the mass fraction of cobalt in the positive electrode active material can be (10:5)-(21:0.4). When the ratio of the mass fraction of manganese to the mass fraction of cobalt in the positive electrode active material is within the aforementioned range, the positive electrode active material has both a higher discharge voltage platform and higher structural stability and higher electronic conductivity.

[0101] According to some embodiments of the present application, the ratio of the mass fraction of manganese to the mass fraction of nickel in the positive electrode active material can be (10:30) to (21:6). When the ratio of the mass fraction of manganese to the mass fraction of nickel in the positive electrode active material is within the aforementioned range, the positive electrode active material has both a high discharge voltage platform and structural stability, and a high specific capacity.

[0102] According to some embodiments of the present application, the ratio of the mass fraction of manganese to the mass fraction of iron in the positive electrode active material can be (10:13) to (21:0.8). When the ratio of the mass fraction of manganese to the mass fraction of iron in the positive electrode active material is within the aforementioned range, the positive electrode active material has a higher discharge voltage platform and structural stability, as well as lower manufacturing costs.

[0103] According to some embodiments of the present application, the ratio of the mass fraction of manganese to the mass fraction of iron in the first positive electrode active material is (6:4)-(7:3). When the ratio of the mass fraction of manganese to the mass fraction of iron in the first positive electrode active material is within the aforementioned range, the positive electrode active material has a higher discharge voltage platform and structural stability, as well as lower manufacturing costs.

[0104] As an example, the mass fraction of elements in the positive electrode active material can be tested and obtained by referring to the following method: take about 0.2g of the positive electrode active material in a 30ml digestion tank, retain one digestion tank without sample as a blank sample, move the digestion tank containing the positive electrode chemical material sample into the fume hood and add 12ml of reverse aqua regia. When adding reverse aqua regia, add it along the inner wall of the digestion tank so that the residual sample on the inner wall is washed into the bottom of the tank, then install the top cover, insulation sleeve, gasket, microwave digestion device, nut in sequence, tighten the nut with a wrench, then turn on the microwave digester, insert the optical fiber sensor in the microwave digester into the bottom of the previously assembled digestion tank containing the sample, balance the digestion tank in the microwave digester, and start digestion (digestion program 6min heating to 1 20 ℃ hold for 8min, heat to 160 ℃ for 5min, hold for 8min, heat to 180 ℃ for 5min, hold for 5min), cool to room temperature after completion and take out, place the digestion tank in a fume hood, slowly unscrew the nut to release the air, remove the previously installed parts in turn, transfer the solution in the digestion tank to a 100ml volumetric flask through a funnel (filter paper is required), then rinse the digestion tank with ultrapure water, and transfer the rinse liquid to the volumetric flask, using 10ml of ultrapure water for each rinse, shake the solution in the 100ml volumetric flask, use a pipette to take 1ml of the shaken solution and add it to another 100ml volumetric flask, then add ultrapure water to make up the volume (the total solution reaches 100ml), and finally use ICP-OES to test the sample solution. Among them, when preparing reverse aqua regia, 1000ml of ultrapure water can be poured into a 2500ml glass bottle, and then 750ml of concentrated nitric acid and 250ml of concentrated hydrochloric acid are added in sequence, stirred evenly and set aside, wherein the concentrated nitric acid is a concentrated nitric acid solution with a mass fraction of 68%, and the concentrated hydrochloric acid is a concentrated hydrochloric acid solution with a mass fraction of 68%, or hydrogen chloride gas and ultrapure water are added to ultrapure water with a mass ratio of 68% and 32% respectively, and the required concentrated hydrochloric acid can be obtained after complete dissolution.

[0105] In particular, the manganese content can be determined by the following method: dissolving the positive electrode active material in dilute hydrochloric acid (concentration 10-30%), using ICP to test the content of each element in the solution, and then measuring and converting the manganese content to obtain its weight percentage.

[0106] According to some embodiments of the present application, the doping elements include one or two of a first doping element and a second doping element, the first doping element is doped at the manganese position, and the second doping element is doped at the phosphorus position. By simultaneously doping at the Mn position and the P position of the first positive electrode active material, not only can the dissolution of manganese be effectively reduced, thereby reducing the manganese ions migrating to the negative electrode, reducing the electrolyte consumed due to the decomposition of the SEI film, and improving the cycle life of the battery, it can also promote the adjustment of the Mn-O bond, reduce the lithium ion migration barrier, promote lithium ion migration, and improve the rate performance of the battery.

[0107] According to some embodiments of the present application, when the first doping element is a manganese-site doping, the first doping element may satisfy at least one of the following conditions: the ionic radius of the first doping element and the ionic radius of the manganese element satisfy: |a - b| / b is not greater than 10%, where a is the ionic radius of the first doping element and b is the ionic radius of the manganese element; the variable valence voltage of the first doping element is U, and 2V < U < 5.5V. Further, the ionic radius of the first doping element and the ionic radius of the manganese element may satisfy: |a - b| / b is not greater than 5%. By selecting an appropriate Mn-site doping element, the lattice change rate of lithium manganese phosphate during the lithium deintercalation / insertion process can be improved, the structural stability of the positive electrode active material can be enhanced, the dissolution of manganese can be effectively reduced, and the oxygen activity on the particle surface can be decreased. Furthermore, the specific capacity of the positive electrode active material can be increased, and the interfacial side reaction between the material and the electrolyte during use can be reduced, thereby improving the cycling performance of the material, etc. More specifically, by selecting an element with an ionic radius similar to that of the Mn element as the Mn-site doping element, or by selecting an element with a variable valence range within the variable valence range of Mn for doping, the change amount of the bond length between the doping element and O and the bond length of the Mn - O bond can be controlled, which is beneficial to stabilizing the lattice structure of the doped positive electrode active material. In addition, a vacancy element that plays a role in supporting the lattice can be introduced at the Mn site. For example, the valence of this element is greater than or equal to the sum of the valences of Li and Mn, which is equivalent to introducing a vacant site that cannot combine with Li at the active and easily dissolved Mn site, thereby playing a role in supporting the lattice.

[0108] According to some embodiments of the present application, when the second doping element is a phosphorus-site dopant, the second doping element may satisfy at least one of the following conditions: the chemical activity of the chemical bond formed by the second doping element with O is no less than that of the P-O bond; and the maximum valence of the second doping element is no greater than 6. Selecting an appropriate P-site doping element can help modify the ease of variation of the Mn-O bond length, thereby improving electronic conductivity and lowering the lithium ion migration barrier, promoting lithium ion migration, and enhancing the rate performance of the secondary battery. Specifically, the tetrahedral structure of the P-O bond itself is relatively stable, making it difficult to vary the Mn-O bond length, resulting in a high lithium ion migration barrier for the material as a whole. An appropriate P-site doping element can improve the robustness of the P-O bond tetrahedron, thereby improving the rate performance of the material. Specifically, an element whose chemical activity with O is no less than that of the P-O bond can be selected for doping at the P-site to modify the ease of variation of the Mn-O bond length. In this application, unless otherwise specified, "the chemical activity of the chemical bond formed with O is no less than that of the P-O bond" can be determined using test methods for determining chemical bond activity known to those skilled in the art. For example, it can be determined by detecting the bond energy, or by referring to the electrochemical potential of the oxidation or reduction reagent used to break the chemical bond. Alternatively, an element with a valence not significantly higher than that of P, such as less than 6, can be selected for doping at the P position, thereby reducing the repulsive effect between Mn and P elements and improving the specific capacity and rate performance of the positive electrode active material.

[0109] According to some embodiments of the present application, when the first doping element is manganese doping, the first positive electrode active material may contain at least two first doping elements.

[0110] According to some embodiments of the present application, the first doping element may include one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge. By doping with two or more metals within the above range, doping at the manganese position is beneficial for enhancing the doping effect, further reducing the surface oxygen activity, and thus inhibiting the dissolution of manganese. In addition, the doping of multiple elements can increase the synergistic effect between the elements, for example, while increasing the battery capacity, reducing the lattice change rate of the material and enhancing the dynamic performance of the battery.

[0111] According to some embodiments of the present application, the second doping element may include one or more elements selected from B (boron), S, Si, and N. Doping with elements within the above range helps reduce the lattice change rate of lithium manganese phosphate in the first positive electrode active material during lithium insertion and extraction, improves the structural stability of the first positive electrode active material, effectively reduces the dissolution of manganese and reduces the oxygen activity on the particle surface; when the elements doped at the phosphorus position include the above elements, it also helps to change the difficulty of the Mn-O bond length change, thereby improving electronic conductivity and reducing the lithium ion migration barrier, promoting lithium ion migration, and improving the rate performance of the battery.

[0112] According to some embodiments of the present application, the type of the second positive electrode active material is not particularly limited, as long as it can achieve complementary advantages with the first positive electrode active material. For example, the second positive electrode active material can include at least one of optionally doped lithium cobalt oxide, optionally doped lithium manganese oxide, optionally doped nickel-cobalt ternary material, and optionally doped lithium iron phosphate. When the second positive electrode active material is within the above range, it can effectively increase the specific capacity of the positive electrode active material and also improve the cycle life of the battery.

[0113] According to some embodiments of the present application, lithium cobalt oxide satisfies the general formula Li 1+z Co 1-x-y Ma x Mb y O2, where 0≤x≤0.01, 0≤y≤0.01, and -0.05≤z≤0.08; Ma comprises a doped constant-valence element, Ma including at least one of Al, Ga, Hf, Mg, Sn, Zn, and Zr; Mb comprises a doped variable-valence element, Mb including at least one of Ni, Mn, V, Mo, Nb, Cu, Fe, In, W, and Cr. Lithium cobalt oxide has the advantages of simple synthesis, long cycle life, high operating voltage, and good rate performance. By mixing the first and second positive electrode active materials, a positive electrode active material combining the advantages of both materials can be obtained.

[0114] According to some embodiments of the present application, lithium manganate satisfies the general formula Li a Mn 2-b M b O 4-c X c, where 0.9 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0 ≤ c ≤ 0.2; M and X are doping elements, M includes at least one of Li, Cr, Co, Ni, Mg, Ca, Sr, Ba, Na, K, Al, Be, B, Ti, Zr, Cu, Zn, Ga, Sn, and V; the doping element X includes at least one of F, Cl, Br, I, and S. Lithium manganate has a low production cost and excellent structural stability. By mixing the first positive electrode active material with the second positive electrode active material, a positive electrode active material with the advantages of both materials can be obtained.

[0115] According to some embodiments of the present application, the nickel-cobalt ternary material satisfies the general formula Li a Ni b Co c M1 d M2 e O f R g , where 0.75 ≤ a ≤ 1.2, 0 < b < 1, 0 < c < 1, 0 < d < 1, 0 ≤ e ≤ 0.2, 1 ≤ f ≤ 2.5, 0 ≤ g ≤ 1, f + g ≤ 3; M1 is Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and R includes at least one of N, F, S, Cl. Thus, the specific capacity per gram and structural stability of the positive electrode active material can be improved. The nickel-cobalt ternary material combines the advantages of lithium nickelate and lithium cobaltate, and reduces the manufacturing cost and improves the structural stability by introducing manganese element and / or aluminum element. By mixing the first positive electrode active material with the second positive electrode active material, a positive electrode active material with the advantages of both materials can be obtained.

[0116] According to some embodiments of the present application, lithium iron phosphate satisfies the general formula LiFe a M b PO4, where 0.2 ≤ a < 1, 0 < b ≤ 0.8; M includes one of Ti, Mg, V, Mn, Cr, Zr, Nb, W. Lithium iron phosphate has the advantages of good structural stability, low manufacturing cost, environmental friendliness, and excellent cycle life. By mixing the first positive electrode active material with the second positive electrode active material, a positive electrode active material with the advantages of both materials can be obtained.

[0117] As an example, a spherical aberration electron microscope (ACSTEM) can be used to perform high-spatial-resolution characterization of the internal and surface structures of the positive electrode active material, and the chemical formula of the positive electrode active material can be obtained by combining three-dimensional reconstruction technology.

[0118] As an example, after confirming the mass fraction of each element using ICP, the mass of each element can be obtained by testing the sample mass using ICP, and then the molar amount can be confirmed by the molar mass of each element, and finally the chemical formula can be calculated.

[0119] According to some embodiments of the present application, the energy density of the film formed when the positive electrode active material is disposed on the surface of the positive electrode current collector is not less than the energy density of the film formed when the first positive electrode active material is disposed on the surface of the positive electrode current collector. As a result, the positive electrode active material has a higher energy density. The positive electrode active material layer prepared by mixing the first positive electrode active material and the second positive electrode active material has a better energy density.

[0120] In a second aspect of the present application, a positive electrode slurry is provided, comprising: the aforementioned positive electrode active material. Thus, the positive electrode slurry has all the characteristics and advantages of the aforementioned positive electrode active material, which will not be described in detail here.

[0121] In a third aspect, the present application provides a positive electrode sheet comprising: a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises the aforementioned positive electrode active material. Thus, the positive electrode sheet possesses all the features and advantages of the aforementioned positive electrode active material, which will not be further elaborated here.

[0122] According to some embodiments of the present application, the mass fraction of the manganese element in the positive electrode active material layer is not particularly limited. For example, the mass fraction of the manganese element in the positive electrode active material layer may be 10 wt %-21 wt %.

[0123] In some embodiments, the mass fraction of manganese element in the positive electrode active material layer can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt% or 21wt%.

[0124] According to some embodiments of the present application, the ratio of the mass fraction of manganese to the mass fraction of cobalt in the positive electrode active material layer is (10:5)-(21:0.4), thereby helping to improve the conductivity of the positive electrode sheet.

[0125] According to some embodiments of the present application, the ratio of the mass fraction of manganese to the mass fraction of nickel in the positive electrode active material layer is (10:30)-(21:6), thereby helping to improve the energy density of the positive electrode sheet.

[0126] According to some embodiments of the present application, the ratio of the mass fraction of manganese to the mass fraction of iron in the positive electrode active material layer is (10:13)-(21:0.8), which helps to improve the cycle performance of the positive electrode sheet.

[0127] According to some embodiments of the present application, in the present application, there is at least one surface with an area of ​​1×10 -4 cm 2 The first positive electrode active material has a smaller particle size than the second positive electrode active material. When the first positive electrode active material has a smaller particle size than the second positive electrode active material in the region, and the first positive electrode active material has a smaller particle size than the second positive electrode active material in the region, the first positive electrode active material particles can fill the gaps between the second positive electrode active material particles in the positive electrode active material layer, thereby increasing the compaction density of the positive electrode active material.

[0128] In the fourth aspect of the present application, the present application proposes a battery comprising: the aforementioned positive electrode sheet. As a result, the battery has all the features and advantages of the aforementioned positive electrode sheet, which will not be repeated here. Typically, a battery comprises a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the charge and discharge process of the battery, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0129] According to some embodiments of the present application, the positive electrode current collector has two opposite surfaces in its own thickness direction, and the positive electrode active material layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0130] According to some embodiments of the present application, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0131] According to some embodiments of the present application, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0132] According to some embodiments of the present application, the positive electrode active material layer may further optionally include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0133] According to some embodiments of the present application, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0134] According to some embodiments of the present application, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.

[0135] According to some embodiments of the present application, the negative electrode current collector has two opposite surfaces in its thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0136] According to some embodiments of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0137] According to some embodiments of the present application, the negative electrode active material may adopt the negative electrode active material for batteries known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate, etc. The silicon-based material may include at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material may include at least one of elemental tin, tin oxide compounds and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0138] According to some embodiments of the present application, the negative electrode active material layer may further include a binder. The binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0139] According to some embodiments of the present application, the negative electrode active material layer may further optionally include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0140] According to some embodiments of the present application, the negative electrode active material layer may optionally further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0141] According to some embodiments of the present application, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0142] According to some embodiments of the present application, an electrolyte serves to conduct ions between the positive and negative electrodes. The present application does not specifically limit the type of electrolyte, and the electrolyte may be selected based on needs. For example, the electrolyte may be liquid, gel, or solid.

[0143] According to some embodiments of the present application, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0144] According to some embodiments of the present application, the electrolyte salt may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0145] According to some embodiments of the present application, the solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0146] According to some embodiments of the present application, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0147] According to some embodiments of the present application, the battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0148] According to some embodiments of the present application, the material of the isolation membrane may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0149] According to some embodiments of the present application, the positive electrode sheet, the negative electrode sheet and the separator can be made into an electrode assembly through a winding process or a lamination process.

[0150] According to some embodiments of the present application, a secondary battery may include an outer package that can be used to encapsulate the electrode assembly and the electrolyte.

[0151] According to some embodiments of the present application, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery can also be a soft shell, such as a pouch-type soft shell. The material of the soft shell can be plastic, and examples of plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0152] According to some embodiments of the present application, the present application has no particular restrictions on the shape of the battery, which can be cylindrical, square or any other shape. For example, Figure 1 is a battery 5 with a square structure as an example. Specifically, with reference to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a accommodating cavity. The shell 51 has an opening connected to the accommodating cavity, and the cover plate 53 can be covered on the opening to close the accommodating cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the accommodating cavity. The electrolyte is impregnated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0153] According to some embodiments of the present application, batteries can be assembled into battery modules, and the number of batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module. Figure 3 is a battery module 4 as an example. Referring to Figure 3, in the battery module 4, a plurality of batteries 5 can be arranged in sequence along the length direction of the battery module 4. Of course, they can also be arranged in any other manner. The plurality of batteries 5 can further be fixed by fasteners. The battery module 4 can also include a housing having a accommodating space, and the plurality of batteries 5 are accommodated in the accommodating space.

[0154] According to some embodiments of the present application, the above-mentioned battery modules can also be assembled into a battery pack. The number of battery modules contained in the battery pack can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery pack. Figures 4 and 5 are a battery pack 1 as an example. Referring to Figures 4 and 5, the battery pack 1 may include a battery box and a plurality of battery modules 4 arranged in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can be covered on the lower box body 3 to form a closed space for accommodating the battery module 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0155] In the fifth aspect of the present application, the present application proposes an electrical device, comprising: the aforementioned positive electrode plate, and / or the aforementioned battery. As a result, the electrical device has all the features and advantages of the aforementioned battery, which will not be repeated here. Batteries, battery modules, or battery packs can be used as power sources for electrical devices, or as energy storage units for electrical devices. Electrical devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Electrical devices can select batteries, battery modules or battery packs according to their usage requirements.

[0156] According to some embodiments of the present application, FIG6 illustrates an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.

[0157] According to some embodiments of the present application, the power-consuming device may also be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and may use a battery as a power source.

[0158] The present invention will be described below by way of specific examples. It should be noted that the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. Where specific techniques or conditions are not specified in the examples, they are determined according to the techniques or conditions described in the literature in this area or according to the product specifications. Reagents or instruments not specified by manufacturer are all commercially available conventional products.

[0159] Example 1

[0160] Preparation of the first positive electrode active material:

[0161] (1) Preparation of Fe, Co, V and S co-doped manganese oxalate

[0162] 689.6 g of manganese carbonate, 455.27 g of ferrous carbonate, 4.65 g of cobalt sulfate, and 4.87 g of vanadium dichloride were added to a mixer and thoroughly mixed for 6 hours to obtain a mixture. The mixture was then transferred to a reactor, and 5 L of deionized water and 1260.6 g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours until the reaction terminated and no bubbles were generated, resulting in a manganese oxalate suspension co-doped with Fe, Co, and V. The suspension was then filtered, dried at 120°C, and sand-milled to obtain manganese oxalate particles with a particle size of 100 nm.

[0163] (2) Preparation of Li 0.997 Mn 0.60 Fe 0.393 V 0.004 Co 0.003 P 0.997 S 0.003 O4

[0164] 1793.1 g of manganese oxalate prepared in (1), 368.3 g of lithium carbonate, 1146.6 g of ammonium dihydrogen phosphate, and 4.9 g of dilute sulfuric acid were added to 20 L of deionized water, stirred thoroughly, and uniformly mixed at 80° C. for 10 h to obtain a slurry. The slurry was transferred to a spray drying apparatus for spray drying and granulation to obtain a powder. The powder was sintered in a roller kiln at 700° C. for 4 h in a protective atmosphere (90% nitrogen and 10% hydrogen) to obtain a first positive electrode active material.

[0165] Example 10:

[0166] Preparation of a first positive electrode active material;

[0167] (1) Preparation of Fe, Co, V and S co-doped manganese oxalate

[0168] 689.6 g of manganese carbonate, 455.27 g of ferrous carbonate, 4.65 g of cobalt sulfate, and 4.87 g of vanadium dichloride were added to a mixer and thoroughly mixed for 6 hours to obtain a mixture. The mixture was then transferred to a reactor, and 5 L of deionized water and 1260.6 g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours until the reaction terminated and no bubbles were generated, resulting in a manganese oxalate suspension co-doped with Fe, Co, and V. The suspension was then filtered, dried at 120°C, and sand-milled to obtain manganese oxalate particles with a particle size of 100 nm.

[0169] (2) Preparation of primary particles

[0170] 1793.1 g of manganese oxalate prepared in (1), 368.3 g of lithium carbonate, 1146.6 g of ammonium dihydrogen phosphate, and 4.9 g of dilute sulfuric acid were added to 20 L of deionized water, stirred thoroughly, and uniformly mixed at 80°C for 10 h to obtain a slurry. The slurry was transferred to a spray dryer for spray drying and granulation to obtain a powder. The powder was sintered in a roller kiln at 700°C for 3 h in a protective atmosphere (90% nitrogen and 10% hydrogen) to obtain primary particles.

[0171] (3) Preparation of Li 0.997 Mn 0.60 Fe 0.393 V 0.004 Co 0.003 P 0.997 S 0.003 O4

[0172] The primary particles are spray-dried to form a monodisperse primary particle powder after evaporation of the solvent. The powder is sintered in a roller kiln at 800° C. for 2 hours in a nitrogen protective atmosphere to obtain a first positive electrode active material.

[0173] The first positive electrode active material in Examples 2-9, Examples 19-27 and Comparative Example 1 is the same as the first positive electrode active material in Example 1, and the first positive electrode active material in Examples 11-18, Examples 28-36 and Comparative Example 2 is the same as the first positive electrode active material in Example 10.

[0174] The second positive electrode active material in Examples 1-36 and Comparative Examples 3-4 all adopts commercially available materials from Ningbo Rongbai New Energy Technology Co., Ltd. The second positive electrode active material in Example 1 is LiNi 0.55 Co 0.05 Mn 0.4 O2, the second positive electrode active material in Example 10 is LiNi 0.8 Co 0.1 Mn 0.1 O2.

[0175] The second positive electrode active material in Examples 2-9, Examples 28-36 and Comparative Example 3 is the same as the second positive electrode active material in Example 1, and the second positive electrode active material in Examples 10-18, Examples 19-27 and Comparative Example 4 is the same as the second positive electrode active material in Example 10.

[0176] The positive electrode active materials in Comparative Examples 1 and 2 include only the first positive electrode active material, and the positive electrode active materials in Comparative Examples 3 and 4 include only the second positive electrode active material.

[0177] The following tests were performed on the first positive electrode active material and the second positive electrode active material in Examples 1-36 and Comparative Examples 1-4:

[0178] 1. Determination of chemical formula: After confirming the mass fraction of each element by ICP, the mass of each element can be obtained by ICP testing the sample mass. The molar amount can then be confirmed by the molar mass of each element, and the chemical formula can be finally calculated.

[0179] 2. Gram capacity test: Assemble the positive electrode active material to be tested into a button cell for testing. Charge the button cell to 4.3V at 0.1C, then charge at a constant voltage at 4.3V until the current is less than or equal to 0.05mA, let it stand for 5 minutes, and then discharge it to 2.0V at 0.1C. The discharge capacity at this time is the gram capacity.

[0180] 3. Discharge voltage platform test: Assemble the positive electrode active material to be tested into a button cell for gram capacity test. The discharge voltage platform can be calculated using the formula: discharge voltage platform = discharge energy / discharge capacity.

[0181] 4. Compaction density test: Take 5g of powder and place it in a special compaction mold (American CARVER mold, model 13mm), then place the mold on the compaction density instrument. Apply 3T of pressure, read the thickness of the powder under pressure on the instrument (the thickness after pressure relief), and calculate the compaction density by ρ = m / v. The area value used is the standard small picture area of ​​1540.25mm 2 .

[0182] 5. Particle size test: refer to standard GB / T 19077-2016 and use a laser particle size analyzer (such as Malvern Master Size 3000) for measurement.

[0183] The test results show that:

[0184] The first positive electrode active material in Examples 1-9, Examples 19-27 and Comparative Example 1 is a material having a chemical formula satisfying Li 0.997 Mn 0.60 Fe 0.393 V0.004 Co 0.003 P 0.997 S 0.003 The primary particles of O4 have a Dv50 particle size of 670nm, a gram capacity of 142mAh / g, a discharge voltage platform of 3.73V, and a compaction density of 2.31g / cm 3 .

[0185] The first positive electrode active material in Examples 10-18, Examples 28-36 and Comparative Example 2 is a material having a chemical formula satisfying Li 0.997 Mn 0.60 Fe 0.393 V 0.004 Co 0.003 P 0.997 S 0.003 The secondary particles of O4 have a Dv50 particle size of 3.8 μm, the primary particles of the secondary particles have a Dv50 particle size of 230 nm, a gram capacity of 144 mAh / g, a discharge voltage platform of 3.73 V, and a compaction density of 1.87 g / cm 3 .

[0186] The second positive electrode active material in Examples 1-9, Examples 28-36 and Comparative Example 3 is a material having a chemical formula of LiNi 0.55 Co 0.05 Mn 0.4 The primary particles of O2 have a Dv50 particle size of 3000nm, a gram capacity of 170mAh / g, a discharge voltage platform of 3.88V, and a compaction density of 3.12g / cm 3 .

[0187] The second positive electrode active material in Examples 10-18, Examples 19-27 and Comparative Example 4 is a material having a chemical formula of LiNi 0.8 Co 0.1 Mn 0.1 The secondary particles of O2 have a Dv50 particle size of 9.1 μm, the primary particles of the secondary particles have a Dv50 particle size of 500 nm, a gram capacity of 200 mAh / g, a discharge voltage platform of 3.82 V, and a compaction density of 3.21 g / cm 3 .

[0188] The positive electrode active materials in Examples 1-36 and Comparative Examples 1-4 were used to prepare batteries, and the specific steps were as follows:

[0189] Positive electrode sheet preparation: Positive electrode active material, polyvinylidene fluoride (PVDF), and conductive carbon were added to a certain amount of N-methylpyrrolidone (NMP) at a mass ratio of 90:5:5 for positive electrode active material: binder: conductive agent. The mixture was stirred in a drying room to form a uniform positive electrode slurry with a viscosity controlled between 3000 Pa·s and 10000 mPa·s. The slurry was then coated onto aluminum foil and dried to form a positive electrode sheet. The mass fractions of the first and second positive electrode active materials in the positive electrode active material are shown in Table 1.

[0190] Preparation of negative electrode sheet: Graphite, sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), and conductive carbon are added to a certain amount of deionized water. The mass ratio of graphite: sodium carboxymethyl cellulose: styrene-butadiene rubber: conductive agent is 90:2:3:5. Stir to form a uniform negative electrode slurry. The viscosity is controlled to be 3000Pa·S-10000mPa·S. The above negative electrode slurry is coated on copper foil and dried to form a negative electrode sheet.

[0191] The prepared positive electrode sheet, negative electrode sheet and separator (polyethylene (PE) porous polymer film) are made into corresponding battery cells according to a Z-shaped stacking structure, and the battery cells are vacuum dried at 90°C for 12 hours, and then the positive and negative electrode tabs are ultrasonically welded. The positive electrode uses an aluminum tab and the negative electrode uses a nickel tab. The positive and negative electrode tabs are located on the same side of the battery cell. The battery cell after the tab welding is placed in an aluminum-plastic film of appropriate size for top-side sealing. The top-side sealing temperature is 145°C, and the electrolyte is injected (the electrolyte is a mixed solution of 1 mol / L LiPF6 solution and 5 wt.% fluoroethylene carbonate (FEC), wherein the solvent of the LiPF6 solution is ethylene carbonate (EC): diethyl carbonate (DEC): dimethyl carbonate (DMC) in a volume ratio of 1:1:1). The prepared soft-pack laminated battery is obtained by standing, forming, aging, exhausting, secondary sealing, and capacity testing.

[0192] The following performance tests were performed on the batteries prepared in Examples 1-36 and Comparative Examples 1-4. The test results are shown in Table 1:

[0193] 1. Compaction density test of positive electrode: At room temperature, first weigh 10mm of the current collector to be made. 2 The weight of the disc is m1. Measure the current collector with a thickness of d1. Then take a cold-pressed positive electrode sheet with a size of 10m (length) * 200mm (width) (the positive electrode active material layer is on both the front and back of the current collector). Starting from one end of the electrode sheet, take a 10mm diameter in the middle of the 1m, 3m, 5m, 7m and 9m length electrode sheets. 2The weight of the small discs is measured separately, which is recorded as m2, m3, m4, m5 and m6; the thickness of the small discs is measured separately, which is recorded as d2, d3, d4, d5 and d6. The compacted density = ((m2+m3+m4+m5+m6) / 5 / 10-m1 / 10) / ((d2+d3+d4+d5+d6) / 5-d1)*1000, where m is g / mm 2 , d is in mm.

[0194] 2. Cycle life test: The prepared soft-pack laminated battery is charged to 4.4V at 0.5C0 at 2.5-4.4V in a constant temperature environment of 25°C, then charged at a constant voltage at 4.4V to a current ≤ 0.05C0, allowed to stand for 5 minutes, and then discharged to 2.5V at 1C0. The capacity is recorded as Cn (n = 1, 2, 3...). The above operation is repeated. The capacity retention rate is calculated according to the ratio of Cn / C3. When Cn / C3×100%=80%, the corresponding number of cycles is extracted as the examination index of the cycle capacity.

[0195] 3. Thermal runaway temperature test: Place the soft-pack laminated battery in a high-temperature box and raise the temperature from 25°C to 100°C at a rate of 5°C / min and hold it for 1 hour. Then increase the temperature at a rate of 5°C / min, holding it for 30 minutes each time the temperature is increased by 5°C. Stop the test when the temperature reaches 200°C or the battery cell runs away, and record the ambient temperature when thermal runaway occurs.

[0196] Table 1

[0197] In Comparative Examples 1 and 2, the mass fraction of the first positive electrode active material is 100 wt %, and the mass fraction of the second positive electrode active material is 0 wt %. In Comparative Examples 3 and 4, the mass fraction of the second positive electrode active material is 100 wt %, and the mass fraction of the first positive electrode active material is 0 wt %.

[0198] The test results show that the compaction density of the positive electrode sheets in Examples 1-36 is higher than the compaction density of the positive electrode sheets in Comparative Examples 1 and 2, the cycle life of the batteries in Examples 1-36 is better than the cycle life of the batteries in Comparative Examples 1-4, and the thermal runaway temperature of the batteries in Examples 1-36 is higher than the thermal runaway temperature of the batteries in Comparative Examples 1-4.

[0199] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly specifying the quantity of the technical features indicated. "First feature" and "second feature" may include one or more of the features.

[0200] In this application, all numerical values ​​disclosed herein are approximate, regardless of whether the word "about" or "approximately" is used. The numerical value of each number may vary by less than 10% or by a reasonable difference considered by a person skilled in the art, such as 1%, 2%, 3%, 4% or 5%.

[0201] In the description of this application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for example, and may be any technical feature connected by "and / or" in this application.

[0202] In the description of this specification, reference to the terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.

[0203] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A positive electrode active material, wherein include: a first positive electrode active material, the first positive electrode active material comprising lithium manganese phosphate; a second positive electrode active material, the second positive electrode active material being different from the first positive electrode active material, Wherein, the lithium manganese phosphate has a doping element, and the doping element satisfies at least one of the following conditions: The ionic radius of the doping element and the ionic radius of the manganese element satisfy: |ab| / b is not greater than 10%, wherein a is the ionic radius of the doping element, and b is the ionic radius of the manganese element; The valence change voltage of the doping element is U,2V <U<5.5V; The chemical activity of the chemical bond formed by the doping element and O is not less than the chemical activity of the PO bond; The maximum valence of the doping element is no more than 6.

2. The positive electrode active material according to claim 1, wherein The gram capacity of the second positive electrode active material is not less than the gram capacity of the first positive electrode active material.

3. The positive electrode active material according to claim 1 or 2, wherein The gram capacity of the first positive electrode active material is 135 mAh / g-150 mAh / g, and the gram capacity of the second positive electrode active material is 170 mAh / g-230 mAh / g.

4. The positive electrode active material according to any one of claims 1 to 3, wherein The discharge voltage platform of the positive electrode active material is not greater than the discharge voltage platform of the second positive electrode active material.

5. The positive electrode active material according to any one of claims 1 to 4, wherein The discharge voltage platform of the first positive electrode active material is not greater than the discharge voltage platform of the second positive electrode active material.

6. The positive electrode active material according to any one of claims 1 to 5, wherein The discharge voltage platform of the first positive electrode active material is 3.70V-3.80V, and the discharge voltage platform of the second positive electrode active material is 3.80V-3.90V.

7. The positive electrode active material according to any one of claims 1 to 6, wherein Under a pressure of 3T, the compaction density of the positive electrode active material is not less than the compaction density of the first positive electrode active material.

8. The positive electrode active material according to any one of claims 1 to 7, wherein Under a pressure of 3T, the compaction density of the first positive electrode active material is not greater than the compaction density of the second positive electrode active material.

9. The positive electrode active material according to any one of claims 1 to 8, wherein At a pressure of 3T, the compaction density of the first positive electrode active material is 1.8 g / cm 3 -2.5g / cm 3 ; Under 3T pressure, the compaction density of the second positive electrode active material is 3.0g / cm 3 -3.4g / cm 3 .

10. The positive electrode active material according to any one of claims 1 to 9, wherein: At a temperature of 25° C., the electronic conductivity of the second positive electrode active material is not less than the electronic conductivity of the first positive electrode active material.

11. The positive electrode active material according to any one of claims 1 to 10, wherein: The first positive electrode active material is a secondary particle, the Dv50 particle size of the secondary particle of the first positive electrode active material is 2 μm-9 μm, and the Dv50 particle size of the primary particle of the first positive electrode active material is 10 nm-600 nm.

12. The positive electrode active material according to any one of claims 1 to 10, wherein: The first positive electrode active material is a primary particle, and the Dv50 particle size of the primary particle of the first positive electrode active material is 500nm-1200nm.

13. The positive electrode active material according to any one of claims 1 to 12, wherein: The second positive electrode active material is a secondary particle, the Dv50 particle size of the secondary particle of the second positive electrode active material is 7 μm-11 μm, and the Dv50 particle size of the primary particle of the second positive electrode active material is 50 nm-800 nm.

14. The positive electrode active material according to any one of claims 1 to 12, wherein: The second positive electrode active material is a primary particle, and the Dv50 particle size of the primary particle of the second positive electrode active material is 3000nm-5000nm.

15. The positive electrode active material according to any one of claims 1 to 14, wherein: The mass fraction of the first positive electrode active material in the positive electrode active material is 10 wt % to 90 wt %.

16. The positive electrode active material according to any one of claims 1 to 15, wherein: The mass fraction of the second positive electrode active material in the positive electrode active material is 10 wt % to 90 wt %.

17. The positive electrode active material according to any one of claims 1 to 16, wherein: The Dv90 particle size of the positive electrode active material is 0.9 μm-8 μm, and the Dv10 particle size of the positive electrode active material is 0.2 μm-3.0 μm.

18. The positive electrode active material according to any one of claims 1 to 16, wherein: The Dv90 particle size of the positive electrode active material is 0.9 μm-18 μm, and the Dv10 particle size of the positive electrode active material is 0.2 μm-7.0 μm.

19. The positive electrode active material according to any one of claims 1 to 16, wherein: The Dv50 particle size of the positive electrode active material is 0.5 μm-10 μm.

20. The positive electrode active material according to any one of claims 1 to 19, wherein: The mass fraction of manganese element in the positive electrode active material is 10wt%-21wt%.

21. The positive electrode active material according to any one of claims 1 to 20, wherein: The ratio of the mass fraction of the manganese element to the mass fraction of the cobalt element in the positive electrode active material is (10:5)-(21:0.4).

22. The positive electrode active material according to any one of claims 1 to 21, wherein: The ratio of the mass fraction of the manganese element to the mass fraction of the nickel element in the positive electrode active material is (10:30)-(21:6).

23. The positive electrode active material according to any one of claims 1 to 22, wherein: The ratio of the mass fraction of the manganese element to the mass fraction of the iron element in the positive electrode active material is (10:13)-(21:0.8).

24. The positive electrode active material according to any one of claims 1 to 23, wherein: The ratio of the mass fraction of the manganese element to the mass fraction of the iron element in the first positive electrode active material is (6:4)-(7:3).

25. The positive electrode active material according to any one of claims 1 to 24, wherein: The doping element includes one or both of a first doping element and a second doping element, the first doping element is manganese doping, and the second doping element is phosphorus doping, Wherein, the first doping element satisfies at least one of the following conditions: The ionic radius of the first doping element and the ionic radius of the manganese element satisfy: |ab| / b is not greater than 10%, wherein, a is the ionic radius of the first doping element, and b is the ionic radius of the manganese element; The valence change voltage of the first doping element is U,2V <U<5.5V, Wherein, the second doping element satisfies at least one of the following conditions: The chemical activity of the chemical bond formed by the second doping element and O is not less than the chemical activity of the PO bond; The maximum valence of the second doping element is no more than 6.

26. The positive electrode active material according to claim 25, wherein Contains at least two of the first doping elements.

27. The positive electrode active material according to claim 25 or 26, wherein The first doping element includes one or more elements of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge.

28. The positive electrode active material according to any one of claims 25 to 27, wherein: The second doping element includes one or more elements selected from the group consisting of B (boron), S, Si and N.

29. The positive electrode active material according to any one of claims 1 to 28, wherein The second positive electrode active material includes at least one of optionally doped lithium cobalt oxide, optionally doped lithium manganese oxide, optionally doped nickel-cobalt ternary material and optionally doped lithium iron phosphate.

30. The positive electrode active material according to claim 29, wherein The lithium cobalt oxide satisfies the general formula Li 1+z Co 1-x-y Ma x Mb y O2, Among them, 0≤x≤0.01, 0≤y≤0.01, -0.05≤z≤0.08; The Ma includes a doped constant-valence element, and the Ma includes at least one of Al, Ga, Hf, Mg, Sn, Zn, and Zr; the Mb includes a doped variable-valence element, and the Mb includes at least one of Ni, Mn, V, Mo, Nb, Cu, Fe, In, W, and Cr.

31. The positive electrode active material according to claim 29, wherein The lithium manganate satisfies the general formula Li a Mn 2-b M b O 4-c X c , Among them, 0.9≤a≤1.2, 0≤b≤0.2, 0≤c≤0.2; M and X are doping elements, M includes at least one of Li, Cr, Co, Ni, Mg, Ca, Sr, Ba, Na, K, Al, Be, B, Ti, Zr, Cu, Zn, Ga, Sn and V; the doping element X includes at least one of F, Cl, Br, I or S.

32. The positive electrode active material according to claim 29, wherein The nickel-cobalt ternary material satisfies the general formula Li a Ni b Co c M1 d M2 e O f R g , Among them, 0.75≤a≤1.2,0 <b<1,0<c<1,0<d<1,0≤e≤0.2,1≤f≤2.5,0≤g≤1,f+g≤3; M1 includes Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and R includes at least one of N, F, S, and Cl.

33. The positive electrode active material according to claim 29, wherein The lithium iron phosphate satisfies the general formula LiFe α M β PO4, Among them, 0.2≤a<1,0 <b≤0.8; M includes one of Ti, Mg, V, Mn, Cr, Zr, Nb, and W.

34. The positive electrode active material according to any one of claims 1 to 33, wherein: The energy density of the film layer formed when the positive electrode active material is disposed on the surface of the positive electrode current collector is not less than the energy density of the film layer formed when the first positive electrode active material is disposed on the surface of the positive electrode current collector.

35. A positive electrode slurry, wherein: include: The positive electrode active material according to any one of claims 1 to 34.

36. A positive electrode sheet, wherein: include: A positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector, wherein the positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 34, and / or the positive electrode active material layer is formed by the positive electrode slurry according to claim 35.

37. The positive electrode sheet according to claim 36, wherein: The mass fraction of manganese element in the positive electrode active material layer is 10wt%-21wt%.

38. The positive electrode sheet according to claim 36 or 37, wherein: The ratio of the mass fraction of the manganese element to the mass fraction of the cobalt element in the positive electrode active material layer is (10:5)-(21:0.4).

39. The positive electrode sheet according to any one of claims 36 to 38, wherein: The ratio of the mass fraction of the manganese element to the mass fraction of the nickel element in the positive electrode active material layer is (10:30)-(21:6).

40. The positive electrode sheet according to any one of claims 37 to 39, wherein: The ratio of the mass fraction of the manganese element to the mass fraction of the iron element in the positive electrode active material layer is (10:13)-(21:0.8).

41. The positive electrode sheet according to any one of claims 36 to 40, wherein: The area is 1×10 -4 cm 2 A region is formed, the region is located on a surface of the positive electrode active material layer on one side away from the positive electrode current collector, and the amount of the first positive electrode active material in the region is not less than the amount of the second positive electrode active material.

42. A battery, wherein: include: The positive electrode active material according to any one of claims 1 to 34, and / or the positive electrode sheet according to any one of claims 36 to 41.

43. An electrical device, wherein: include: The positive electrode active material according to any one of claims 1 to 34, and / or the positive electrode sheet according to any one of claims 36 to 41, and / or the battery according to claim 42.

Citation Information

Patent Citations

  • Blended cathode materials

    CN103828099A

  • Mixed sulphate containing lithium-manganese-metal phosphate

    CN104603050A

  • Lithium ferric manganese phosphate positive electrode material as well as preparation method and application thereof

    CN115207306A

  • Lithium ion battery

    US20110269021A1