PMNT target material and preparation method therefor

Through a two-step synthesis method and appropriate processing, the problem of PMNT target density and uniformity is solved, the preparation of large-sized and high-quality targets is achieved, the yield of thin film products is improved and the cost is reduced.

WO2024212487A1PCT designated stage expired Publication Date: 2024-10-17BEIJING SINOMA SYNTHETIC CRYSTALS CO LTD +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/128466
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-11
Filing Date
2023-10-31
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing PMNT ceramic targets have poor density, high porosity, and uneven grain sizes, making it difficult to meet high-performance requirements. Moreover, the preparation of single-crystal targets is difficult and expensive. The multi-piece splicing method causes plasma during the coating process. Poor non-uniformity reduces sputtering effect.

Method used

A two-step synthesis method is used to prepare PMNT targets. First, the MNT precursor is mixed with PbO and treated at high temperature to obtain PMNT powder. Then, ball milling, granulation, sieving, cold isostatic pressing and hot pressing sintering are performed. MgO, Nb2O5, TiO2, To determine the particle size and purity of PbO powder, use polyvinyl alcohol as a binder and perform cold isostatic pressing and hot pressing to obtain PMNT targets with high density, uniformity and purity.

Benefits of technology

It achieves the preparation of large-sized and high-quality PMNT targets, improves the yield of thin film products, reduces costs, improves the microstructure uniformity and density of the targets, and meets high-performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023128466_17102024_PF_FP_ABST
    Figure CN2023128466_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a preparation method for a PMNT target material, comprising: obtaining an MNT precursor; mixing the MNT precursor with PbO, and treating same at a high temperature to obtain PMNT powder; carrying out ball milling, granulation, sieving, cold isostatic pressing, binder discharging, and hot-pressing sintering treatment on the PMNT powder to obtain a PMNT target material. By means of the provided preparation method, a PMNT target material having uniform microstructure, high density and high purity can be obtained, and particularly, a large-sized high-quality PMNT target material can be obtained, thereby improving the yield of PMNT thin film products and reducing costs.
Need to check novelty before this filing date? Find Prior Art

Description

A PMNT Target and Its Preparation Method

[0001] This application claims the priority of a Chinese patent application with the application number 202310381212.8, titled "A PMNT Target and Its Preparation Method", filed with the Chinese Patent Office on April 11, 2023. The entire content of this application is incorporated herein by reference in its entirety. Technical Field

[0002] This application relates to the technical field of piezoelectric materials, and particularly to a PMNT target and its preparation method. Background Art

[0003] Lead magnesium niobate-lead titanate (chemical formula: (1 - x)[Pb(Mg 1 / 3 Nb<> 2 / 3 )O3]-x(PbTiO3), where 0 < x < 1, abbreviated as PMNT) - related relaxor ferroelectric materials are widely used in microwave tunable devices, transducers, sensors, optical waveguides and other fields due to their excellent dielectric, piezoelectric, pyroelectric, electro - optical and nonlinear optical properties. Compared with bulk materials, the thinning technology of high - performance relaxor ferroelectric materials is the key to the development of integrated circuits. The thin film can be directly deposited on the integrated circuit, compatible with the signal reading circuit, without cutting, with high integration and low cost, which is of great significance for realizing the miniaturization of devices and systems. The preparation of thin films by magnetron sputtering coating process is one of the physical vapor deposition methods. It mainly uses high - energy particles generated by glow discharge to bombard the target material, so that the target material sputters out molecules or atoms and deposits on the substrate surface to form a thin film. Its advantages are low film - forming temperature, high film quality, high crystallinity and good compatibility with microelectronic processes, which is convenient for fabricating devices.

[0004] Currently, PMNT thin films are mainly obtained by sputtering PMNT ceramic targets. The PMNT ceramic targets in the prior art have poor density and high porosity; the grain sizes are different and unevenly distributed; there are impurities and defects at the grain boundaries, which cannot meet the current performance requirements for high - performance PMNT target materials. Another way to obtain a target is PMNT single crystal. The preparation of single - crystal targets is difficult and costly, and it is difficult to prepare large - size (over 4 inches) high - quality targets. If multiple target pieces are spliced together, during the coating process, the more the number of spliced pieces and gaps, the worse the plasma uniformity, which will lead to local abnormal discharges and other situations, greatly reducing the sputtering effect, and thus reducing the quality and yield of the coated products.

[0005] Summary of the Invention

[0006] The purpose of this application is to provide a PMNT target material and its preparation method, which can improve the target material's microstructural uniformity, density, and purity. In particular, it can produce large-scale, high-quality PMNT targets, thereby increasing the yield of PMNT thin film products and reducing costs. The specific technical solution is as follows:

[0007] The first aspect of the present application provides a method for preparing a PMNT target, comprising the following steps:

[0008] (1) MgO, Nb2O5, and TiO2 powders were weighed according to the chemical composition of the PMNT target, then mixed, dried, and high-temperature treated at 1180°C-1250°C for 120 min-240 min to obtain a MNT precursor;

[0009] (2) weighing an MNT precursor and PbO powder according to the chemical composition of the PMNT target, mixing the MNT precursor and PbO, drying, and high-temperature treating at 800° C. to 860° C. for 120 min to 240 min to obtain PMNT powder;

[0010] (3) ball-milling the PMNT powder, adding a binder, granulating, and sieving;

[0011] (4) cold isostatic pressing to obtain a PMNT blank, and heat-treating the PMNT blank at 500° C. to 700° C. for 1.5 to 4 hours to perform a binder removal treatment to obtain a PMNT green blank;

[0012] (5) hot pressing and sintering the PMNT green body to obtain a PMNT target;

[0013] The chemical composition of the PMNT target is (1-x)[Pb(Mg 1 / 3 Nb 2 / 3 )O3]-x(PbTiO3), where x is 0.1-0.4.

[0014] In one embodiment of the present application, the particle size of the MgO, Nb2O5, TiO2 and PbO powders is 100nm-200nm.

[0015] In one embodiment of the present application, the method further comprises pre-calcining the MgO before weighing.

[0016] In one embodiment of the present application, the binder is an aqueous solution of polyvinyl alcohol (PVA), the concentration of the binder is 5%-10%, and the amount of the binder added is 0.5%-2% based on the weight of the PMNT powder.

[0017] In one embodiment of the present application, the cold isostatic pressing pressure is 100 MPa-200 MPa, and the time is 10 min-40 min.

[0018] In one embodiment of the present application, the hot pressing sintering is performed at a pressure of 20 MPa-30 MPa, and the temperature is kept at 1180° C.-1250° C. for 200 min-300 min.

[0019] The second aspect of the present application provides a PMNT target prepared using the preparation method provided in the first aspect of the present application.

[0020] In one embodiment of the present application, the size of the PMNT target is 4.3 inches to 4.6 inches.

[0021] Beneficial effects of this application:

[0022] The present application provides a PMNT target material and a preparation method thereof. The chemical composition of the PMNT target material is (1-x)[Pb(Mg 1 / 3 Nb 2 / 3 )O3]-x(PbTiO3), where x is 0.1-0.4, is prepared by preparing a MNT precursor, which is then mixed with PbO and subjected to high-temperature treatment to obtain PMNT powder. The PMNT powder is then subjected to ball milling, granulation, screening, cold isostatic pressing, binder removal, and hot pressing sintering to obtain a PMNT target. The preparation method provided herein can produce PMNT targets with uniform microstructure, high density, and high purity, particularly large-scale, high-quality PMNT targets, thereby improving the yield of PMNT thin film products and reducing costs.

[0023] Of course, it is not necessary to achieve all the advantages described above at the same time when implementing any product or method of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings described herein are used to provide further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.

[0025] FIG1 is an X-ray diffraction spectrum of the PMNT target in Example 1;

[0026] FIG2 is an X-ray diffraction spectrum of the PMNT target in Comparative Example 1;

[0027] FIG3 is a scanning electron microscope image of the PMNT target in Example 1;

[0028] FIG4 is a scanning electron microscope image of the PMNT target in Comparative Example 1;

[0029] FIG5 is a picture of the PMNT target sample in Example 3. DETAILED DESCRIPTION

[0030] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and examples. It is apparent that the described examples are only a portion of the embodiments of this application, rather than all of them. All other embodiments obtained by those skilled in the art based on this application are within the scope of protection of this application.

[0031] The first aspect of the present application provides a method for preparing a PMNT target, comprising the following steps:

[0032] (1) MgO, Nb2O5, and TiO2 powders were weighed according to the chemical composition of the PMNT target, then mixed, dried, and high-temperature treated at 1180°C-1250°C for 120 min-240 min to obtain a MNT precursor;

[0033] (2) Weighing the MNT precursor and PbO powder according to the chemical composition of the PMNT target, mixing the MNT precursor and PbO, drying, and high-temperature treating at 800°C-860°C for 120min-240min to obtain PMNT powder;

[0034] (3) ball-milling the PMNT powder, adding a binder, granulating, and sieving;

[0035] (4) cold isostatic pressing to obtain a PMNT blank, and then heat-treating the PMNT blank at 500°C-700°C for 1.5 hours to 4 hours to obtain a PMNT blank;

[0036] (5) hot pressing and sintering the PMNT green body to obtain a PMNT target;

[0037] The chemical composition of PMNT target is (1-x)[Pb(Mg 1 / 3 Nb 2 / 3 )O3]-x(PbTiO3), where x is 0.1-0.4.

[0038] This application uses a two-step synthesis method to first prepare an MNT precursor, then mix it with PbO and perform high-temperature treatment to obtain a PMNT powder raw material with a single perovskite structure. The PMNT powder raw material is then ball-milled, granulated, screened, cold isostatically pressed, debinded, and hot-pressed and sintered. Finally, after machining, a PMNT target with uniform microstructure, high density, and high purity is obtained. The one-step method for synthesizing PMNT targets can easily lead to changes in the chemical composition of the PMNT target and produce microstructural inhomogeneities. However, this application uses a PbO-MNT precursor mixed with the target to react and obtain the PMNT target, resulting in a PMNT target with uniform microstructure, high density, and high purity.

[0039] Typically, the starting raw materials, MgO, Nb2O5, TiO2, and PbO, are high-purity reagents with a purity greater than 99.99%. When the purity of the starting raw materials, MgO, Nb2O5, TiO2, and PbO, falls within the above range, the impact of impurities on the purity of the PMNT target can be reduced, thereby improving the quality of the PMNT target.

[0040] In the present application, there is no particular limitation on the mixing method, as long as the purpose of the present application can be achieved, for example, wet mixing, such as ball milling; when the mixing method is ball milling, for example, the ball milling time can be 20h-26h, and the ball mill speed can be 90r / min-120r / min.

[0041] In the present application, there is no particular limitation on the drying method, as long as the purpose of the present application can be achieved, for example, the drying method is oven drying.

[0042] In the present application, there is no particular limitation on the ball milling method, as long as the purpose of the present application can be achieved. For example, the material of the ball mill is nylon, the grinding balls are alumina balls, and the ball milling medium is anhydrous ethanol; when ball milling and mixing, the mass ratio of large grinding balls, medium grinding balls and small grinding balls in the ball mill is 1:2:4, and the mass ratio of materials, grinding balls and ball milling media is 2:1.2:1.

[0043] In this application, PMNT powder undergoes particle grading after sieving. The method of particle grading is not particularly limited, as long as it achieves the objectives of this application. For example, the granulated particles can be sieved through 25-mesh, 60-mesh, and 100-mesh standard sieves, and the oversize particles can be mixed in a mass ratio of 4:3:1. Particle grading helps improve the density of the powder and enhance its fluidity.

[0044] In one embodiment of the present application, the particle size of the MgO, Nb2O5, TiO2 and PbO powders is 100nm-200nm. When the particle size of the MgO, Nb2O5, TiO2 and PbO powders is controlled within the above range, they have better sintering activity and are conducive to powder dispersion.

[0045] In one embodiment of the present application, the MgO is pre-calcined before weighing the MgO, Nb2O5, and TiO2 powders according to the chemical composition of the PMNT target. The present application does not specifically limit the pre-calcination method, as long as it achieves the objectives of the present application. For example, the pre-calcination method is drying. In the present application, pre-calcining the MgO can prevent moisture absorption by the MgO powder, which can lead to inaccurate stoichiometric ratios.

[0046] In one embodiment of the present application, the binder is an aqueous solution of polyvinyl alcohol (PVA) at a concentration of 5%-10%, and the amount added is 0.5%-2% based on the weight of the PMNT powder. When the binder is selected from the above substances and the concentration and amount of the binder are controlled within the above ranges, a good granulation effect is achieved, facilitating colloid discharge without causing pollution.

[0047] In one embodiment of the present application, the cold isostatic pressing pressure is 100 MPa-200 MPa, and the time is 10 min-40 min. When the cold isostatic pressing pressure and time are controlled within the above ranges, it is beneficial to reduce costs, obtain high-quality green bodies, and facilitate green body forming.

[0048] In one embodiment of the present application, the hot-pressing sintering pressure is 20 MPa-30 MPa, and the temperature is maintained at 1180°C-1250°C for 200-300 minutes. When the hot-pressing sintering pressure, temperature, and time are controlled within these ranges, it helps reduce costs, minimize equipment wear, and increase the density of the PMNT target.

[0049] In this application, after the PMNT green body is hot-pressed and sintered, it is further machined to level the outer edges and end faces and polish them smooth. This application does not particularly limit the machining method, as long as it can achieve the purpose of this application, such as a lathe.

[0050] The second aspect of the present application provides a PMNT target prepared using the preparation method provided in the first aspect of the present application.

[0051] In one embodiment of the present application, the size of the PMNT target is 4.3 inches to 4.6 inches.

[0052] Example

[0053] The following examples and comparative examples are provided to more specifically illustrate the embodiments of the present invention. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0054] Test methods and equipment:

[0055] X-ray diffraction spectrum test:

[0056] The prepared PMNT target was tested using an X-ray powder diffractometer (model: Bruker D8 Advance) (Cu Kα), wherein the scanning range 2θ was 10°-80°, the scanning rate was 6° / min, and the test temperature was 20±5°C.

[0057] Element mass percentage test:

[0058] At room temperature, the prepared PMNT target was tested using an inductively coupled plasma mass spectrometer (ICP) of MS Agilent 7700.

[0059] Scanning electron microscope (SEM) image test:

[0060] At room temperature, a scanning electron microscope (model SU1510) was used to test the prepared PMNT target and observe the cross-sectional micromorphology of the PMNT target.

[0061] Example 1

[0062] The chemical composition is 0.62[Pb(Mg 1 / 3 Nb 2 / 3 )O3]-0.38(PbTiO3) PMNT target preparation method, comprising the following steps:

[0063] First, MgO is pre-calcined, and the corresponding weights of TiO2, MgO, and Nb2O5 are weighed according to the composition of the desired product, and ball-milled on a ball mill at a speed of 100 r / min for 24 hours to obtain MNT slurry; the slurry is sieved once with a 20-mesh sieve and poured into a container, and then placed in an oven and dried at 100°C for 12 hours to obtain MNT raw material; the MNT raw material is placed in a corundum crucible, covered and sealed, and placed in a box-type electric furnace, heated to 800°C over 180 minutes, then heated to 1100°C over 120 minutes, then heated to 1250°C over 60 minutes, kept warm for 180 minutes, cooled to 700°C over 180 minutes, then cooled to 300°C over 120 minutes, and finally naturally cooled to room temperature to obtain an MNT precursor.

[0064] An excess of 1% PbO and a MNT precursor were weighed according to the weight of the desired product and ball-milled in a ball mill at a speed of 100 r / min for 24 hours. The mixture was then placed in an oven and dried at 100°C for 12 hours to obtain a mixed PMNT powder. The mixed PMNT powder was placed in a corundum crucible, sealed with a lid, and placed in a box-type electric furnace. The temperature was set to increase from room temperature to 600°C over 180 minutes, and then to 850°C over 360 minutes. After maintaining at 850°C for 180 minutes, the temperature was decreased to 300°C over another 180 minutes and naturally cooled in the furnace to obtain PMNT powder.

[0065] After adding an 8% polyvinyl alcohol (PVA) aqueous solution binder, granulation was performed. The binder addition amount was 1% based on the weight of PMNT powder. The granulated particles were sieved through standard sieves of 25 mesh, 60 mesh, and 100 mesh, and the sieve-surface materials were mixed in a mass ratio of 4:3:1.

[0066] The granulated raw material was cold isostatically pressed into a green billet at 180 MPa for 30 min, and then subjected to a debinding treatment in a box-type electric furnace at 650° C. for 2 h.

[0067] The green blank was placed in a hot pressing sintering furnace for hot pressing sintering, and a pressure of 25 MPa was applied. The temperature was raised from room temperature to 800°C over 180 minutes, and then to 1250°C over 360 minutes. After being kept at 1250°C for 240 minutes, the temperature was dropped to 600°C over 180 minutes. The blank was naturally cooled in the furnace to obtain a PMNT ceramic blank. Finally, the outer edge and end face of the blank were trimmed and smoothed on a machining lathe to make a PMNT target.

[0068] The X-ray diffraction spectrum of the obtained PMNT target is shown in Figure 1.

[0069] As can be seen from the figure, the crystal phase of the PMNT target prepared in this embodiment contains only the perovskite phase, indicating that the crystal phase of the PMNT target obtained by the preparation method of this application is single and does not contain impurity crystal phase, which is conducive to further obtaining high-quality PMNT target.

[0070] The scanning electron microscope image of the obtained PMNT target is shown in FIG3 .

[0071] As can be seen from the figure, the PMNT target material prepared in this embodiment has uniform grain size, no pores, and high density, which is conducive to improving the subsequent sputtering effect.

[0072] The size of the obtained PMNT target is 4.6 inches, indicating that this embodiment can obtain a large-sized PMNT target while meeting the performance requirements such as purity, density, and material uniformity, which is beneficial to improving the yield of PMNT thin film products and reducing costs.

[0073] Example 2

[0074] The chemical composition is 0.75[Pb(Mg 1 / 3 Nb 2 / 3 )O3]-0.25(PbTiO3) PMNT target preparation method, comprising the following steps:

[0075] First, MgO is pre-calcined, and the corresponding weights of TiO2, MgO, and Nb2O5 are weighed according to the composition of the desired product, and ball-milled on a ball mill at a speed of 100 r / min for 24 hours to obtain MNT slurry; the slurry is sieved once with a 20-mesh sieve and poured into a container, and then placed in an oven and dried at 100°C for 12 hours to obtain MNT raw material; the MNT raw material is placed in a corundum crucible, covered and sealed, and placed in a box-type electric furnace, heated to 800°C over 180 minutes, then heated to 1100°C over 120 minutes, then heated to 1220°C over 60 minutes, kept warm for 180 minutes, cooled to 700°C over 180 minutes, then cooled to 300°C over 120 minutes, and finally naturally cooled to room temperature to obtain an MNT precursor.

[0076] An excess of 1% PbO and an MNT precursor were weighed according to the weight of the desired product and ball-milled on a ball mill at a speed of 100 r / min for 24 hours. The mixture was then placed in an oven and dried at 100°C for 12 hours to obtain a mixed PMNT powder. The mixed PMNT powder was placed in a corundum crucible, sealed with a lid, and placed in a box-type electric furnace. The temperature was set to increase from room temperature to 650°C over 180 minutes, and then to 820°C over 360 minutes. After maintaining at 820°C for 180 minutes, the temperature was decreased to 300°C over another 180 minutes and naturally cooled in the furnace to obtain PMNT powder.

[0077] After adding an 8% polyvinyl alcohol (PVA) aqueous solution binder, granulation was performed. The binder addition amount was 1% based on the weight of PMNT powder. The granulated particles were sieved through standard sieves of 25 mesh, 60 mesh, and 100 mesh, and the sieve-surface materials were mixed in a mass ratio of 4:3:1.

[0078] The granulated raw materials were cold isostatically pressed into green billets at a pressure of 150 MPa for 30 min, and then subjected to debinding treatment in a box-type electric furnace at 650° C. for 2 h.

[0079] The green body was placed in a hot pressing sintering furnace for hot pressing sintering, and a pressure of 25 MPa was applied. The temperature was raised from room temperature to 800°C over 180 minutes, and then to 1250°C over 360 minutes. After being kept at 1250°C for 240 minutes, the temperature was dropped to 600°C over 180 minutes. The green body was naturally cooled in the furnace to obtain a PMNT ceramic body. Finally, the outer edge and end face of the green body were trimmed and smoothed on a machining lathe to make a PMNT target.

[0080] The size of the obtained PMNT target is 4.3 inches, which shows that this embodiment can obtain a large-sized PMNT target while meeting the performance requirements such as purity, density, and material uniformity, thereby facilitating the acquisition of high-quality PMNT films.

[0081] Example 3

[0082] The chemical composition is 0.82[Pb(Mg 1 / 3 Nb 2 / 3 )O3]-0.18(PbTiO3) PMNT target preparation method, comprising the following steps:

[0083] First, MgO is pre-calcined, and the corresponding weights of TiO2, MgO, and Nb2O5 are weighed according to the composition of the desired product, and ball-milled on a ball mill at a speed of 100 r / min for 24 hours to obtain MNT slurry; the slurry is sieved once with a 20-mesh sieve and poured into a container, and then placed in an oven and dried at 100°C for 12 hours to obtain MNT raw material; the MNT raw material is placed in a corundum crucible, covered and sealed, and placed in a box-type electric furnace, heated to 800°C over 180 minutes, then heated to 1100°C over 120 minutes, then heated to 1200°C over 60 minutes, kept warm for 180 minutes, cooled to 650°C over 180 minutes, then cooled to 300°C over 120 minutes, and finally naturally cooled to room temperature to obtain an MNT precursor.

[0084] An excess of 1% PbO and an MNT precursor were weighed according to the weight of the desired product and ball-milled in a ball mill at a speed of 100 r / min for 24 hours. The mixture was then placed in an oven and dried at 100°C for 12 hours to obtain a mixed PMNT powder. The mixed PMNT powder was placed in a corundum crucible, sealed with a lid, and placed in a box-type electric furnace. The temperature was set to increase from room temperature to 700°C over 180 minutes, then to 850°C over 360 minutes, maintained at 850°C for 180 minutes, and then decreased to 300°C over 180 minutes. The mixture was then naturally cooled in the furnace to obtain PMNT powder.

[0085] After adding an 8% polyvinyl alcohol (PVA) aqueous solution binder, granulation was performed. The binder addition amount was 1% based on the weight of PMNT powder. The granulated particles were sieved through standard sieves of 25 mesh, 60 mesh, and 100 mesh, and the sieve-surface materials were mixed in a mass ratio of 4:3:1.

[0086] The granulated raw materials were cold isostatically pressed into green billets at a pressure of 150 MPa for 25 min, and then subjected to debinding treatment in a box-type electric furnace at 680° C. for 2 h.

[0087] The green body was placed in a hot pressing sintering furnace for hot pressing sintering, and a pressure of 24 MPa was applied. The temperature was raised from room temperature to 800°C over 180 minutes, and then to 1210°C over 360 minutes. After being kept at 1210°C for 240 minutes, the temperature was dropped to 600°C over 180 minutes. The green body was naturally cooled in the furnace to obtain a PMNT ceramic body. Finally, the outer edge and end face of the green body were trimmed and smoothed on a machining lathe to make a PMNT target.

[0088] The size of the obtained PMNT target is 4.5 inches. The obtained PMNT target sample is shown in Figure 5, which shows that this embodiment can obtain a large-sized PMNT target while meeting the performance requirements such as purity, density, and material uniformity, thereby facilitating the acquisition of high-quality PMNT films.

[0089] Comparative Example 1

[0090] The chemical composition is 0.62[Pb(Mg 1 / 3 Nb 2 / 3 )O3]-0.38(PbTiO3) PMNT ceramic target preparation method, comprising the following steps:

[0091] According to the above chemical composition, the required TiO2, MgO, Nb2O5, and PbO were weighed in proportion and ball-milled at a speed of 100 r / min for 24 h. After ball milling, the mixture was dried to form a mixed powder.

[0092] The mixed powder was placed in a corundum crucible, sealed with a lid, and placed in a box-type electric furnace. The temperature in the furnace was set to rise from room temperature to 500°C over 180 minutes, then to 850°C over 210 minutes, maintained at 850°C for 180 minutes, then decreased to 550°C over 180 minutes, and then decreased to room temperature over another 180 minutes to obtain PMNT powder.

[0093] After adding an 8% aqueous solution of polyvinyl alcohol (PVA) binder, the binder was added in an amount of 1% based on the weight of the PMNT powder. The granulated particles were sieved through a 100-mesh standard sieve.

[0094] The granulated raw materials were dry pressed into green billets, and then subjected to debinding treatment in a box-type electric furnace at 650°C for 2 hours;

[0095] The green billet was placed in a tubular furnace for atmospheric sintering. The specific process was as follows: the temperature in the furnace was raised from room temperature to 750°C over 240 minutes, then to 1100°C over 210 minutes, maintained at 1100°C for 360 minutes, then lowered to 600°C over 180 minutes, and then to room temperature over another 180 minutes. The oxygen flow rate was 0.3L / min to 0.7L / min.

[0096] The X-ray diffraction spectrum of the obtained PMNT ceramic target is shown in Figure 2.

[0097] As can be seen from the figure, during the synthesis process using the existing technology, part of Nb2O5 reacts with PbO to form Pb2Nb2O7 pyrochlore phase, so that the prepared PMNT ceramic target contains a second phase, resulting in low material purity.

[0098] The scanning electron microscope image of the obtained PMNT ceramic target is shown in FIG4 .

[0099] As can be seen from the figure, the ceramic contains a large number of pores and impurities, which reduces the density. At the same time, the grain boundaries are obvious and the grain size is uneven, which will have an adverse effect on the subsequent sputtering effect.

[0100] The size of the obtained PMNT target is 4.1 inches, indicating that a large-sized PMNT target can be obtained in this comparative example, but the performance of the PMNT target is poor and cannot meet the existing requirements for PMNT target properties such as purity, density, and material uniformity, and high-quality PMNT thin film materials cannot be obtained.

[0101] Comparative Example 2

[0102] The chemical composition is 0.62[Pb(Mg 1 / 3 Nb 2 / 3 )O3]-0.38(PbTiO3) single crystal PMNT target material, comprising the following steps:

[0103] According to the composition of the desired product, weigh the corresponding weight of MgO, Nb2O5, PbO, and TiO2 and mix them by ball milling at a speed of 100 r / min for 24 h. After ball milling, dry the mixture to form a mixed powder.

[0104] The mixed powder was placed in a corundum crucible, covered and sealed, and placed in a box-type electric furnace. A heating program was set so that the temperature in the furnace increased from room temperature to 500°C over 180 minutes, then to 850°C over 210 minutes, maintained at 850°C for 180 minutes, then decreased to 550°C over 180 minutes, and then decreased to room temperature over another 180 minutes to obtain PMNT polycrystalline material.

[0105] PMNT crystals were grown using the crucible descent method. The furnace temperature was controlled between 1300°C and 1350°C at a descent rate of 0.3 mm / h to 0.6 mm / h. After growth was complete, the temperature was lowered to room temperature at a rate of 40°C to 60°C to obtain PMNT crystals.

[0106] The resulting single-crystal PMNT target material is 3 inches in size. Since single crystals cannot currently grow larger than 4 inches in diameter, producing large-scale single-crystal targets is extremely difficult, resulting in extremely low yields and making them unsuitable for producing large-scale PMNT films.

[0107] The mass percentages of the elements in the PMNT targets prepared in the examples and comparative examples of the present application are shown in Table 1.

[0108] Table 1

[0109] Referring to the Examples and Comparative Examples, it can be seen from Table 1 that the measured values ​​of the mass percentages of the elements in the PMNT target obtained by the preparation method of the present application are basically consistent with the target values, with a small relative error. This shows that the two-step sintering synthesis method of MNT and lead oxide adopted in the present application avoids the formation of the pyrochlore phase, so that the actual chemical composition of each component in the prepared PMNT target is highly consistent with the chemical composition of the original design, which is conducive to the growth of high-purity and high-quality PMNT targets, thereby improving the yield of thin film products.

[0110] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A method for preparing a PMNT target material, It is characterized in that The following steps are involved: (1) Weigh MgO and Nb according to the chemical composition of PMNT target 2 O 5 and TiO 2 The powder is then mixed, dried, and subjected to high temperature treatment at 1180°C-1250°C for 120min-240min to obtain an MNT precursor; (2) weighing an MNT precursor and a PbO powder according to the chemical composition of the PMNT target, mixing the MNT precursor and the PbO, drying, and subjecting the mixture to a high temperature treatment at 800° C. to 860° C. for 120 min to 240 min to obtain a PMNT powder; (3) ball-milling the PMNT powder, adding a binder, granulating, and sieving; (4) cold isostatic pressing to obtain a PMNT blank, and heat-retaining the PMNT blank at 500° C. to 700° C. for 1.5 h to 4 h to perform a binder removal treatment to obtain a PMNT green blank; (5) hot pressing and sintering the PMNT green billet to obtain a PMNT target; The chemical composition of the PMNT target is (1-x)[Pb(Mg 1 / 3 Nb 2 / 3 ) 3 ]-x(PbTiO 3 ), where x is 0.1-0.

4.

2. The preparation method according to claim 1, It is characterized in that The MgO, Nb 2 O 5 、TiO 2 The particle size of the PbO powder is 100nm-200nm.

3. The preparation method according to claim 1, It is characterized in that The method further comprises pre-calcining the MgO before weighing.

4. The preparation method according to claim 1, It is characterized in that The adhesive is a polyvinyl alcohol aqueous solution, the concentration of the adhesive is 5%-10%, and the amount of the adhesive added is 0.5%-2% based on the weight of the PMNT powder.

5. The preparation method according to claim 1, It is characterized in that The cold isostatic pressing process is performed under a pressure of 100 MPa to 200 MPa and lasts for 10 min to 40 min.

6. According to the preparation method of claim 1, It is characterized in that The hot pressing sintering pressure is 20MPa-30MPa, and the temperature is kept at 1180°C-1250°C for 200min-300min.

7. A PMNT target prepared by the preparation method according to any one of claims 1 to 6.

8. The PMNT target according to claim 7, having a size of 4.3 inches to 4.6 inches.

Citation Information

Patent Citations

  • Pyroelectric material and preparation method thereof

    CN103601489A

  • Method for improving Curie temperatures, piezoelectricity and thermal stability of PMN-PT

    CN107915486A

  • Lead magnesium niobate-lead titanate based piezoelectric ceramic material and preparation method thereof

    CN114621009A

  • PMNT target material and preparation method thereof

    CN116553928A

  • Multi layer ceramic capacitor

    JP1998189384A