Pre-embedding agent, pre-embedded lithium positive electrode, pre-embedded sodium positive electrode, secondary battery comprising same, method for pre-embedding lithium, and method for pre-embedding sodium

By using a pre-intercalator with an organic sulfinate structure for lithium/sodium ion supplementation, the problem of insufficient energy density and side reaction loss of lithium/sodium batteries is solved, high energy density and stability are achieved, and by-product residues are avoided. Reduces production costs and is suitable for mass production.

WO2024212829A1PCT designated stage expired Publication Date: 2024-10-17ZHEJIANG YONGTAI TECH CO LTD

Patent Information

Application Number
PCT/CN2024/084855
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-03-29
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing lithium/sodium battery technology faces problems of insufficient energy density and lithium ion loss caused by side reactions. Existing pre-lithium doping technology has problems with by-product residue, poor safety and high cost. It lacks a stable and effective sodium pre-doping method.

Method used

The pre-intercalation agent with organic sulfinate structure is used for pre-intercalation of lithium/sodium. The supplement of lithium/sodium ions is achieved through electrode doping method, coating method or electrolyte dissolution method. The by-product is gas or can be dissolved in electrolyte to avoid residues, reduce costs and improve safety.

Benefits of technology

It achieves high specific energy density and volumetric energy density of lithium/sodium-ion batteries, with good stability, unaffected battery cycle performance, simple process, suitable for mass production, extending battery life and realizing the regeneration of used batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024084855_17102024_PF_FP_ABST
    Figure CN2024084855_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a pre-embedding agent using organic sulfinate as a framework for pre-embedding lithium or sodium, a pre-embedded lithium positive electrode, a pre-embedded sodium positive electrode, a secondary battery, and a method for pre-embedding lithium or sodium using the pre-embedding agent. The pre-embedding agent of the present invention has a high specific capacity, excellent stability, is free of residues, has excellent compatibility with a battery system, and can be well applied to lithium- or sodium-ion secondary batteries. A pre-embedding process of the method for pre-embedding lithium or sodium of the present invention is safe and convenient, the process is simple, the costs are low, and large-scale production can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Pre-embedding agent, pre-embedding lithium positive electrode, pre-embedding sodium positive electrode, secondary battery containing the same, and pre-embedding lithium and pre-embedding sodium methods Technical Field

[0001] The present invention relates to a pre-embedding agent, a pre-embedding lithium positive electrode containing a pre-embedding lithium material, a secondary battery containing the pre-embedding lithium positive electrode, and a pre-embedding lithium method. In addition, the present invention also relates to a pre-embedding sodium positive electrode containing a pre-embedding sodium material, a secondary battery containing the pre-embedding sodium positive electrode, and a pre-embedding sodium method. Background Art

[0002] Faced with growing energy demands and severe environmental challenges, the development of efficient and reliable energy storage technologies is urgent. Lithium / sodium battery technology is considered one of the most promising energy storage technologies. Due to its high energy density and low cost, it has been widely used in electric vehicles and portable electric devices. However, with the further development of human society, the requirements for energy storage technologies in various new applications have further increased, and current lithium / sodium battery technology faces the problem of insufficient energy density. Therefore, for lithium / sodium batteries, it is necessary to research the use of high-capacity anode materials; for example, new lithium batteries such as silicon (4200mAh g-1) and phosphorus (2596mAh g-1) are needed. However, these anode materials are accompanied by irreversible side reactions during the charge and discharge process, resulting in lithium ion loss and battery capacity degradation. For example, silicon-based materials (SiOx) undergo irreversible electrochemical reactions to form LiySiOx, which cannot be reused. At the same time, the formation of a protective interfacial layer (SEI) on the silicon anode surface also consumes some lithium ions. During the subsequent charging process, the lithium ions that can migrate back to the positive electrode are reduced, resulting in a loss of battery capacity and inability to fully utilize the positive electrode material. These side reactions cause the battery's first-cycle coulombic efficiency (ICE) and cycle efficiency (CE) to be far below 100%. Taking the SiO negative electrode as an example, its full-battery ICE is only 50%-60%, which means that the battery loses more than 40% of its capacity in the first cycle, greatly limiting the further development of these materials. Therefore, it is necessary to solve this problem through the method of pre-embedding lithium, that is, before assembling the battery, a certain amount of lithium is stored in the battery in advance to compensate for the lithium loss in the first cycle of the battery. For sodium batteries, the above problems also exist, but to date, there is no pre-embedding sodium agent and method in the industry that can stably, effectively and well replenish sodium.

[0003] Currently, the more mature pre-lithiation technologies mainly include two approaches: direct introduction of lithium sources through the negative electrode and addition through the positive electrode. While direct introduction of lithium sources through the negative electrode offers high pre-lithiation efficiency and eliminates the introduction of ineffective components, it also has high process requirements, high costs, and poor safety, making it unsuitable for large-scale production. While pre-lithiation through positive electrode addition offers the advantages of high safety and simple process requirements, it leaves residual byproducts in the battery after lithium addition, reducing the battery's energy density and easily forming pores in the positive electrode, which reduces the battery's cyclability. Therefore, there is an urgent need for a positive electrode lithium supplementation technology that eliminates residual byproducts and improves battery energy density.

[0004] Patent Document 1 discloses a method for pre-lithiation of lithium-sulfur battery electrodes. By pre-lithiating the sulfur positive electrode, the introduction of a lithium source into the negative electrode can be avoided. Due to the low conductivity of the sulfur positive electrode, heat release during contact with the lithium source is slow, which helps reduce safety risks and improves safety performance. Using lithium foil to lithiate the positive electrode avoids the introduction of other substances, which helps maintain energy density and is suitable for battery systems lacking a complete lithium source. However, Patent Document 1 requires the use of lithium metal, which is unstable in air and inconvenient to operate. Furthermore, the short-circuit lithium replenishment method, due to its violent reaction and difficult-to-control reaction time, can lead to instability at the positive electrode interface, affecting battery cycle performance.

[0005] Patent Document 2 discloses a double-layer composite diaphragm battery and a lithium replenishment method thereof, which can effectively avoid uncontrollable reaction speed during lithium replenishment, achieve the purpose of uniform lithium replenishment, and significantly improve the battery's first cycle charge and discharge efficiency and energy density. However, in the above-mentioned Patent Document 2, a three-electrode system containing lithium metal is used to replenish lithium for the battery. This method also requires the use of lithium metal materials and requires the landfilling of lithium metal electrodes between the double diaphragms. It has air instability and inconvenient operation, and the introduction of additional components will reduce the energy density of the battery system.

[0006] Patent document 3 discloses a method of using a sodium supplement additive Na2C x O y N z Mixing it with the cathode material in a certain proportion (5% to 20%) to form a mixed cathode material can replenish sodium in sodium-ion batteries. However, this method requires the materials to be sintered at high temperatures, which is costly. Moreover, after the sodium is replenished, the remaining components are buried in the battery, reducing the overall energy density of the battery.

[0007] Other existing technologies use sodium-supplementing additives such as Na5FeO4 or Na2C2O4 mixed with cathode materials in a specific ratio to create a mixed cathode material to replenish sodium in sodium-ion batteries. Similarly, these methods require the materials to undergo high-voltage decomposition, which reduces battery interface stability and affects the battery's long-term cycle life. Furthermore, the remaining components after sodium supplementation are buried in the battery, reducing the overall energy density.

[0008] Existing technology

[0009] Patent Document 1: CN116470165A

[0010] Patent Document 2: CN107845829A

[0011] Patent Document 3: CN110165218A

[0012] Summary of the Invention

[0013] Technical problem to be solved by the invention

[0014] The object of the present invention is to provide a pre-embedding agent, a pre-embedding lithium / sodium positive electrode, a lithium / sodium ion battery containing the same, and a pre-embedding lithium / sodium method, which has good stability, a safe and convenient pre-embedding lithium / sodium process, and a high energy density and capacity retention rate.

[0015] Technical means to solve the problem

[0016] The present invention provides an organic pre-intercalation agent that leaves little or no residue after pre-intercalation treatment. The pre-intercalation lithium / sodium positive electrode of the present invention is obtained by treating it with the organic pre-intercalation agent of the present invention. The pre-intercalation lithium / sodium method of the present invention is a method of pre-intercalating a positive electrode with lithium / sodium using the organic pre-intercalation agent of the present invention.

[0017] Effects of the Invention

[0018] The side groups of the organic pre-embedding agent of the present invention are adjustable, thereby enabling material structure design by selecting different side groups, and its synthesis process is simple and low-cost. In addition, the pre-embedding lithium / sodium pre-embedding via the organic pre-embedding agent has a high specific capacity and a moderate lithium / sodium desorption potential, which is compatible with the battery system. The pre-embedding agent of the present invention has good stability, a safe and convenient lithium / sodium pre-embedding process, few residual components in the battery system, no impact on battery cycle performance, a simple production process, low cost, and can be produced on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] FIG1 is a CV test curve and a charge-discharge test curve of a sodium trifluoromethanesulfinate button cell in Example 1 of the present invention.

[0020] FIG2 is a CV test curve and a charge-discharge test curve of a lithium trifluoromethanesulfinate button cell in Example 1 of the present invention.

[0021] FIG3 is an in-situ Raman test of the pre-lithiation method of lithium trifluoromethanesulfinate electrolyte in Example 1 of the present invention, and a Raman comparison of lithium trifluoromethanesulfinate powder, pure electrolyte, and lithium trifluoromethanesulfinate dissolved in pure electrolyte after charging.

[0022] FIG4 is a Raman comparison of a fresh sample of lithium trifluoromethanesulfinate and a sample stored in dry air in Example 1 of the present invention.

[0023] FIG5 is a charge-discharge curve test of pre-embedding agents with different side group substitutions in Examples 2, 3, 4, and 5 of the present invention.

[0024] FIG6 is a charge-discharge curve test of organic sodium sulfinates with different substituents according to the present invention.

[0025] FIG7 is a diagram showing the charge and discharge efficiency in Example 8 of the present invention.

[0026] FIG8 is a graph showing the charge and discharge efficiency in Example 9 of the present invention.

[0027] FIG9 is a comparison diagram of the lithium supplementation effect in Example 10 of the present invention.

[0028] FIG10 is a comparison diagram of the sodium supplementation effect of the electrolyte in Example 11 of the present invention.

[0029] FIG11 is a comparison diagram of the effect of sodium supplementation by coating the positive electrode surface in Example 12 of the present invention.

[0030] FIG12 is a comparison diagram of the effects of sodium supplementation by doping the positive electrode in Example 13 of the present invention.

[0031] FIG13 is a comparison diagram of the effects before and after pre-embedding sodium in Example 14 of the present invention.

[0032] FIG14 is a diagram showing the efficiency of multiple electrolyte lithium replenishment in Example 15 of the present invention. DETAILED DESCRIPTION

[0033] The present invention is described in detail below, but the present invention is not limited thereto and any changes can be made without departing from the scope of the present invention.

[0034] [Pre-embedding agent]

[0035] The pre-embedding agent of the present invention has an organic sulfinate structure as shown below:

[0036] In the above formula (1), R is selected from an alkyl group having 1 to 10 carbon atoms and a halogenated alkyl group; an aryl group having a benzene ring, a thiophene ring, a furan ring, or a pyridine ring and a halogenated aryl group; a chain ether group and a cyclic ether group having 1 to 10 carbon atoms; and a chain ester group and a cyclic ester group having 1 to 10 carbon atoms. X represents Na or Li.

[0037] Preferably, R is an alkyl group selected from -Me, -Et; a haloalkyl group selected from -CF3, -C2F5, -C4F9; an aryl group selected from -Ph, -CH3C6H4, -C5NH4, -C4H3S, -C4H3O; and a haloaryl group selected from -FC6H4, -ClC6H4.

[0038] In the present invention, when X is Na, sodium can be replenished for sodium ion secondary batteries, and when it is Li, lithium can be replenished for lithium ion secondary batteries. The capacities of the secondary batteries after pre-embedding treatment can reach 311 mAh / g and 262 mAh / g, respectively, and have a moderate lithium / sodium desorption potential of 3.2V-4.1V.

[0039] The following reaction occurs during the pre-intercalation of lithium / sodium in the pre-intercalation agent of the present invention:

[0040] As shown above, organic sulfinates maintain a balance of positive and negative ions. When the negative ions lose electrons and oxidize and decompose, the positive ions are released, replenishing lithium and sodium. This process is solely dependent on the oxidation potential of the negative ions, which is less than 4.3V relative to lithium metal and less than 4V relative to sodium metal, both within the normal operating voltage range of lithium-sodium batteries. Therefore, X can be either lithium or sodium. Other organic structures, such as organic sulfonates, organic carboxylates, organic pentafluorophosphates, organic trifluoroborates, and organic phenolates, cannot achieve the effects of the present invention because their negative ion oxidation potentials relative to lithium and sodium metal are outside the normal operating voltage range of lithium-sodium batteries.

[0041] Further, by selecting R, the side group of the above-mentioned organic pre-embedding agent can be adjusted, thereby, different parameters such as voltage, solubility and product can be adjusted to meet the use of different battery systems. For example, as shown in the above reaction formula, when R is methyl or ethyl, the gram capacity of the pre-embedding agent is the highest, the product is a full gas, the decomposition voltage is low, but the solubility is poor, and it is therefore suitable for use by scraping on the positive electrode surface, or for use by doping inside the positive electrode. When R is a fluoroalkyl group, the pre-embedding agent has a high solubility in the electrolyte, and is therefore suitable for use in the electrolyte. Among them, from the perspective of the gram capacity, voltage and solubility of the pre-embedding agent, trifluoromethyl is more preferred.

[0042] Because the organic sulfinate structure only occupies the mass and volume of active lithium or sodium ions in the battery, the pre-embedding agent of the present invention has high specific energy and volumetric energy density. When R is -Me, -Et, -CF3, or -C2F5, in addition to generating active lithium or sodium ions, the remaining products are gases that can be completely discharged from the battery system. When R is other groups, in addition to generating active lithium or sodium ions, the remaining products dissolve in the electrolyte as cosolvents, without increasing the overall volume of the battery, thus having a high volumetric energy density.

[0043] In the present invention, when pre-intercalating lithium or sodium using a pre-intercalating agent having the aforementioned organic sulfinate structure, the byproduct gas is completely discharged, resulting in minimal residual residue in the electrode and no reduction in the overall energy density of the battery. Consequently, when pre-intercalating lithium or sodium using an electrolyte, there is no residual residue and a large replenishment capacity, resulting in low cost, simple preparation, and easy storage.

[0044] The pre-embedding agent having the organic sulfinate structure in the present invention can be directly a commercial product. The lithium salt can also be obtained by a production method comprising the following steps.

[0045] Step (1): weighing the commercially available organic sulfinic acid sodium salt, placing it in a solvent, and recrystallizing it to obtain a pre-embedded sodium material;

[0046] Step (2): weighing the pre-embedded sodium material in step (1), placing it in an organic solvent, adding an appropriate amount of acid, stirring to react, extracting and drying, and evaporating the solvent;

[0047] Step (3): placing the product obtained in step (2) in deionized water, adding an appropriate amount of lithium salt, stirring to react, and evaporating the solvent;

[0048] Step (4): recrystallize the solid obtained in step (3) using ethyl acetate and dichloromethane; dry the obtained solid powder to obtain an organic sulfinate lithium salt as a pre-lithium embedding material.

[0049] Preferably, the solvent used in the above step (1) is at least one selected from water, ethyl acetate and ethanol.

[0050] The organic solvent used in the above step (2) is selected from at least one of acetonitrile, tetrahydrofuran, diethyl ether and ethanol. These solvents are preferred because of their good water solubility.

[0051] The acid used in the above step (2) is selected from non-oxidizing acids such as hydrochloric acid, sulfuric acid, and acetic acid.

[0052] The lithium salt used in the above step (3) is selected from water-soluble lithium salts such as lithium hydroxide, lithium carbonate, and lithium acetate.

[0053] Preferably, in the above step (2), after the acid is added, the stirring reaction time is 1-10 hours; after the lithium salt is added in step (3), the stirring reaction time is 5-10 hours; the drying process in the above steps can preferably be vacuum drying, at which time the temperature is 50-100° C. and the time is 10-24 hours.

[0054] [Pre-intercalation of lithium / sodium]

[0055] As the pre-intercalation lithium / sodium method of the present invention, specifically, the pre-intercalation agent of the present invention can be directly added to the electrolyte to carry out the electrochemical reaction of charging oxidation decomposition, or it can be implemented by electrode doping method or coating on the electrode surface.

[0056] As an electrode doping method, the following methods can be cited. The above-mentioned pre-embedding agent of the present invention is mixed with a positive electrode material, a conductive agent, a binder and a solvent as needed, and is evenly ground using a grinder such as an agate bead mill. Afterwards, a film is coated on the electrode current collector using a coating machine to form a thin film, and vacuum dried in a vacuum oven to obtain an electrode sheet containing the above-mentioned pre-embedding agent having the above-mentioned organic sulfinate structure of the present invention. The electrode sheet is assembled into a pre-packaged battery, and power is applied to perform the above-mentioned electrochemical reaction to perform the pre-embedding lithium / sodium process. Since the pre-embedding agent of the present invention can only produce gaseous by-products when performing the electrochemical reaction, it is possible to achieve full gas discharge of the by-products, thereby avoiding the introduction of additional components.

[0057] In addition to the above method, another advantage of the pre-embedding agent of the present invention is that it can be dissolved in conventional commercial battery electrolytes, which are then added to the battery to achieve pre-embedding of lithium / sodium in lithium / sodium batteries. In this method, specifically, the pre-embedding agent is dissolved in the battery electrolyte at a mass fraction of 0.1%-30%, preferably 0.1%-6%, and then the electrolyte is added to the battery to achieve pre-embedding of lithium / sodium in the battery. Preferred battery electrolytes are carbonate electrolytes or ether electrolytes.

[0058] When lithium and sodium are replenished through the electrolyte, the pre-intercalation agent exists in the electrolyte system as a free ion. During charging, a potential difference exists between the positive and negative electrodes of the battery. Under this potential difference, negative ions are concentrated and adsorbed on the surface of the positive electrode for electrochemical oxidation, while positive X ions are embedded in the negative electrode to replenish lithium and sodium.

[0059] As the pre-embedding agent of the present invention, and the method for pre-embedding lithium / sodium using the pre-embedding agent, it has the characteristics of being applicable to the above-mentioned electrode doping method and coating method, and can also directly dissolve the pre-embedding agent in the battery electrolyte, thereby having good compatibility with batteries and being effectively applicable to lithium batteries and sodium batteries. In addition, when it is directly dissolved in the electrolyte, it does not need to be used through positive electrode doping, and can be directly added and used through electrolyte preparation, which can more effectively avoid the introduction of additional components and will not lead to a decrease in battery energy density; further, for used batteries, especially waste lithium batteries, the battery can be pre-embedded with lithium / sodium multiple times by adding the electrolyte multiple times, thereby realizing the in-situ regeneration of waste lithium batteries without unpacking. The process of pre-embedding lithium / sodium by adding the electrolyte will not change the structure of the battery components, such as causing multiple holes in the positive electrode, and can more stably obtain pre-embedded lithium / sodium electrodes. In addition, the method of adding the electrolyte to the battery is highly integrated with the battery production process, does not require additional costs, and has a low cost of use.

[0060] [Lithium-ion secondary battery electrode]

[0061] As the positive electrode / negative electrode of the lithium ion secondary battery, for example, a positive electrode sheet / negative electrode sheet having a structure in which an active material layer containing a positive electrode active material / negative electrode active material and a binder is formed on a current collector can be used.

[0062] The positive electrode current collector and the negative electrode current collector of the present invention may be made of any material that can be used as a current collector for lithium ion batteries. For example, copper can be used as the negative electrode current collector, and aluminum can be used as the positive electrode current collector.

[0063] The positive electrode active material of the present invention can use any material that can be used as a positive electrode active material for lithium ion batteries, for example, organic sulfur positive electrodes such as sulfided polyacrylonitrile (SPAN), lithium iron phosphate, lithium cobalt oxide, lithium manganate, titanium disulfide, vanadium pentoxide, Prussian blue (Fe4[Fe(CN)6]3), NCM811 and other ternary materials.

[0064] The positive electrode may contain a binder. As the binder, any substance commonly used as a positive electrode binder for lithium ion batteries in the art, such as polyvinylidene fluoride (PVDF), polyacrylic acid-based binders, and polyurethane-based binders, can be used.

[0065] The negative electrode active material of the present invention can use any material that can be used as a negative electrode active material for a lithium ion battery, for example, lithium metal, graphite, silicon carbon, Si or a composite of these, such as a composite of Si and graphite, a composite of Si and lithium metal, a composite of graphite and lithium metal, etc.; silicon oxides such as silicon monoxide (SiO), etc.

[0066] The active material layer may further contain a conductive agent. Examples of the conductive agent include conductive carbon Super P, carbon nanotubes (CNTs), natural graphite, artificial graphite, cokes, carbon black, pyrolytic carbons, carbon fibers, calcined organic polymer compounds, and any other substance that can be used as a conductive agent for lithium-ion batteries in the art.

[0067] For the pre-embedded lithium positive electrode of the present invention, the pre-embedded lithium treatment can be implemented by dissolving the pre-embedded agent represented by formula (1) of the present invention in an electrolyte through an electrode doping method, a coating method, and an electrochemical reaction. The pre-embedded lithium / sodium electrode of the prior art requires the use of lithium metal materials. Such lithium metal materials are unstable in air and inconvenient to operate, and have violent reactions and difficult to control reaction time, which can lead to instability of the positive electrode interface and affect the battery cycle performance. The pre-embedded lithium material of the present invention having the above-mentioned organic sulfinate structure is stable to water and oxygen, easy to operate, and has a mild reaction process, which effectively avoids the above-mentioned problems.

[0068] Calculated based on a 1Ah battery, the initial efficiency of traditional LFP-graphite, ternary-graphite and lithium cobalt oxide-graphite battery systems is above 95%. To achieve 100% efficiency, the amount of lithium replenished needs to be between 0.1% and 5%. Special battery systems have lithium-free positive electrodes - graphite and lithium-free positive electrodes - copper. The battery system does not contain lithium ions, and the initial efficiency is around 50% after 100% lithium replenishment. To achieve 100% efficiency, the amount of lithium replenished needs to be between 100% and 200%.

[0069] As described above, since the product of the pre-intercalation treatment of the present invention is a gas or soluble in the electrolyte, the residual amount in the electrode is minimal and can be determined by the pre-intercalation agent content in the electrode before and after the pre-intercalation treatment. Assuming the pre-intercalation range for a 1Ah battery capacity is 0.1%-200%, the pre-intercalation agent content in the pre-intercalation lithium positive electrode before the pre-intercalation treatment is calculated using the following formula. The calculation for sodium batteries is the same as for lithium batteries.

[0070] Specifically, based on a 1Ah battery capacity, the amount of pre-embedded lithium relative to the 1Ah battery capacity is c 1*X% (Ah), and the capacity of the lithium supplement is (F is the Faraday constant; M is the molecular weight of the lithium supplement; N is the number of lithium ions in the lithium supplement, which is 1 in the formula (1) of the present invention), then the amount of the lithium supplement substance is Therefore, when F is taken as 96500, and calculated according to the above-mentioned conventional industrial pre-intercalation range of 0.1%-200%, that is, the pre-intercalation amount c relative to the 1Ah battery capacity is 1mAh-2000mAh, the minimum amount of pre-intercalation agent content in the pre-intercalation lithium positive electrode before pre-intercalation lithium treatment is 1*3.6*1000 / 96500=0.0374mmol, and the maximum amount is 2000*3.6*1000 / 96500=74.8mmol. The residual pre-intercalation agent in the treated electrode can be determined by measuring the residual amount of anions in the electrolyte and subtracting the above-mentioned amount before pre-intercalation treatment, but is not limited to this method. Since the pre-intercalation agent of the present invention can be completely free of residue, the pre-intercalation agent content in the pre-intercalation lithium positive electrode after pre-intercalation lithium treatment is theoretically essentially zero, and in actual industry, it can be less than 0.005mmol.

[0071] The pre-embedding agent having the above-mentioned organic sulfinate structure of the present invention can achieve multiple lithium replenishment of the battery by multiple additions of electrolyte to the used battery, thereby extending the life of the lithium-ion battery. Preferred combinations include the combination of a graphite negative electrode and a lithium iron phosphate positive electrode, a graphite negative electrode and a ternary positive electrode, a graphite negative electrode and a lithium cobalt oxide positive electrode, a graphite negative electrode and a lithium manganate positive electrode, a silicon-carbon negative electrode and a lithium iron phosphate positive electrode, a silicon-carbon negative electrode and a ternary positive electrode, a silicon-carbon negative electrode and a lithium cobalt oxide positive electrode, a silicon-carbon negative electrode and a lithium manganate positive electrode, a silicon negative electrode and a lithium iron phosphate positive electrode, a silicon negative electrode and a ternary positive electrode, a silicon negative electrode and a lithium cobalt oxide positive electrode, and a silicon negative electrode and a lithium manganate positive electrode. After multiple cycles, the battery system capacity decreases. By using the method of pre-embedding lithium with an electrolyte of the present invention, the life of the lithium-ion battery can be increased by 15-30 times. By using the pre-embedding agent having the above-mentioned organic sulfinate structure of the present invention to replenish lithium in the battery system via the electrolyte, waste lithium batteries can be regenerated in situ without unpacking. Compared with the existing technology, the operation convenience, environmental protection and cost are greatly improved.

[0072] In addition, the pre-embedding agent with the above-mentioned organic sulfinate structure of the present invention has sufficiently high specific energy and volume energy density, so it can be applied to low first-effect electrode materials such as silicon monoxide (SiO), silicon carbon, silicon, and black phosphorus. Although these low-first-effect electrode materials have high specific energy, stable cycle life and low cost, they cannot be used in practice because the first-cycle coulomb efficiency is lower than the 92% required for lithium batteries. However, by applying the pre-embedding agent with the above-mentioned organic sulfinate structure of the present invention, a high-energy density battery was successfully realized. In addition, the SiO material itself is stable to water, oxygen, etc., and its stability and energy density are greatly improved and the cost is greatly reduced compared with the existing commercial graphite negative electrode. As positive electrode materials that are paired with low first-effect electrode materials such as silicon monoxide (SiO), preferably included are NCM811, a combination of a silicon-carbon negative electrode and a ternary positive electrode, a combination of a silicon-carbon negative electrode and a lithium iron phosphate positive electrode, a combination of a silicon-carbon negative electrode and a lithium cobalt oxide positive electrode, a combination of a silicon-carbon negative electrode and a lithium manganate positive electrode, a combination of a silicon negative electrode and a ternary positive electrode, a combination of a silicon negative electrode and a lithium iron phosphate positive electrode, a combination of a silicon negative electrode and a lithium cobalt oxide positive electrode, a combination of a silicon negative electrode and a lithium manganate positive electrode, a combination of a black phosphorus negative electrode and a ternary positive electrode, a combination of a black phosphorus negative electrode and a lithium iron phosphate positive electrode, a combination of a black phosphorus negative electrode and a lithium cobalt oxide positive electrode, a combination of a black phosphorus negative electrode and a lithium manganate positive electrode, a combination of a silicon monoxide negative electrode and a ternary positive electrode, a combination of a silicon monoxide negative electrode and a lithium iron phosphate positive electrode, a combination of a silicon monoxide negative electrode and a lithium cobalt oxide positive electrode, and a combination of a silicon monoxide negative electrode and a lithium manganate positive electrode.

[0073] Furthermore, the pre-embedding agent of the present invention having the above-mentioned organic sulfinate structure is particularly suitable for battery systems in which both the positive and negative electrodes do not contain lithium due to its sufficiently high specific energy and volume energy density. As such electrode combinations, there can be listed a combination of lithium-free negative electrode material graphite and lithium-free positive electrode material sulfurized polyacrylonitrile (SPAN), a combination of lithium-free negative electrode material graphite and titanium disulfide positive electrode, a combination of lithium-free negative electrode material graphite and vanadium pentoxide positive electrode, a combination of silicon-carbon negative electrode and sulfurized polyacrylonitrile positive electrode, a combination of silicon-carbon negative electrode and titanium disulfide positive electrode, a combination of silicon-carbon negative electrode and vanadium pentoxide positive electrode, a combination of silicon negative electrode and sulfurized polyacrylonitrile positive electrode, a combination of silicon negative electrode and titanium disulfide positive electrode, and a combination of silicon negative electrode and vanadium pentoxide positive electrode. By applying the above-mentioned pre-embedding agent of the present invention, the energy density reaches 360Wh kg -1 , which is higher than the current lithium-ion batteries (such as lithium iron phosphate, lithium cobalt oxide and ternary material systems of 200-300Wh kg -1 ), and after 350 cycles of charge and discharge, its capacity retention rate is still above 80%.

[0074] The aforementioned lithium-free cathode material SPAN and graphite itself are stable to water, oxygen, and other factors. Compared to existing commercial lithium-containing cathode materials (such as lithium iron phosphate, lithium cobalt oxide, and ternary materials), its stability and processing convenience are significantly improved. The lithium-free cathode material SPAN is an organic polymer material, and its preparation process does not require the use of transition metals. Compared to existing commercial lithium-containing cathode materials (such as lithium iron phosphate, lithium cobalt oxide, and ternary materials), it is highly recyclable, has low production and recycling costs, and is more environmentally friendly. The synthesis process of pre-embedded lithium materials does not require high temperature and high pressure conditions, resulting in high stability and low production and storage costs.

[0075] [Sodium ion secondary battery electrode]

[0076] The sodium ion secondary battery electrode of the present invention can be obtained by the same method as the above-mentioned lithium ion secondary battery electrode, and the electrode material can use the materials that can be used for sodium ion secondary electrode in the above-mentioned lithium ion secondary battery electrode. For example, the electrode combination is classified according to the sodium positive electrode material, and polyanion sodium electrode system (XO4) can be listed. n- or (X m O 3m+1 ) n- (X=B, S, P, Si, As, Mo, W), layered oxide sodium battery system Na x MO2 (x = 0 ~ 1, M = Fe, Mn, Ni, Co, Cr) and its combination, Prussian blue sodium electrode system {Na x M1[M2(CN)6] 1-y ·□ y nH2O (0≤x≤2, 0≤y<1), M1 and M2 are transition metal ions with different coordinations (M1 coordinated with nitrogen and M2 coordinated with carbon), such as Mn, Fe, Co, Ni, Cu, Zn, Cr, etc.; □ is a vacancy [M2(CN)6], such as a sodium battery system. Conductive carbons include Super P and acetylene black. Binders include PVDF, PTFE, and carbon nanotubes.

[0077] From the perspective of better air stability, lower synthesis cost and process difficulty of sodium battery cathode materials, and greater suitability for large-scale preparation, P2-type layered oxides (Na 2 / 3 M x N y O2, x+y=1, M, N=Fe, Mn, Ni, Co, Cr), and the negative electrode material preferably used in combination with the positive electrode material is hard carbon. In addition, sodium-poor P2-type layered oxide (Na 0.67 Mn 0.67 Ni 0.33 The material itself is stable to water, oxygen, etc., and its stability is greatly improved and its cost is greatly reduced compared with existing commercial sodium-rich positive electrode materials.

[0078] Examples of hard carbon include resin carbon, organic polymer pyrolytic carbon, and carbon black, which are commonly used materials in the art. Examples of hard carbon negative electrode precursor materials include biomass, resin-based materials, and asphalt.

[0079] [Electrolyte]

[0080] As a lithium ion electrolyte, an electrolyte obtained by dissolving the pre-intercalation agent having the above-mentioned organic lithium sulfinate structure of the present invention in an organic solvent is used. In addition, it is also necessary to use an electrolyte obtained by dissolving other lithium salts in an organic solvent. As lithium salts, for example, LiClO4, LiPF6, LiAsF6, LiSbF6, LiBF4, LiSO3F, LiCF3SO3, LiN(SO2CF3)2, LiTFSI, LiN(SO2C2F5)2, LiN(SO2CF3)(COCF3), Li(C4F9SO3), LiC(SO2CF3)3, LiBOB, lower aliphatic carboxylic acid lithium salts, LiAlCl4, etc. can be mentioned. These can be used alone or as a mixture of two or more.

[0081] As the organic solvent, for example, carbonates such as propylene carbonate, ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), 4-trifluoromethyl-1,3-dioxolane-2-one, and 1,2-bis(methoxycarbonyloxy)ethane; ethers such as 1,3-dioxolane (DOL), 1,2-dimethoxyethane, 1,3-dimethoxypropane, pentafluoropropyl methyl ether, 2,2,3,3-tetrafluoropropyldifluoromethyl ether, tetrahydrofuran, and 2-methyltetrahydrofuran; esters such as methyl formate, methyl acetate, and γ-butyrolactone; nitriles such as acetonitrile and butyronitrile; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; carbamates such as 3-methyl-2-oxazolidinone; and sulfur-containing compounds such as cyclopentane, dimethyl sulfoxide, and 1,3-propane sultone.

[0082] As the sodium ion electrolyte, for example, an electrolyte prepared by dissolving the pre-intercalating agent having the organic sodium sulfinate structure of the present invention in an organic solvent can be used. Examples of the electrolyte include the carbonate electrolyte, sulfone electrolyte, ether electrolyte, and nitrile electrolyte.

[0083] The electrolyte is selected according to the battery system. The preferred electrolyte in the present invention is a carbonate electrolyte or an ether electrolyte. The following combinations can be listed, based on the molar ratio (mol / L) of the lithium salt to the solvent volume in the electrolyte: 1.0M NaClO4 (EC:DEC=1:1), 1.0M LiClO4 (EC:EMC=3:7), 1.0M LiPF6 (EC:EMC=3:7) + 1% LiClO4, 0.5M LiBOB + 0.5M LiTFSI (EC:EMC=3:7), 1.0M LiPF6 (DOL:DME=1:1) + 1% LiClO4, etc.

[0084] [Pre-installed batteries and secondary batteries]

[0085] The preassembled battery of the present invention is obtained by pre-packaging the pre-embedded lithium / sodium electrode of the present invention, charging the pre-assembled battery to form the pre-embedded lithium / sodium electrode, and then repackaging the pre-embedded lithium / sodium electrode to obtain the secondary battery of the present invention.

[0086] The present invention is not limited to the above-described embodiments, and various modifications can be made within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0087] Example

[0088] Although the present invention is described in detail based on the embodiments, the present invention is not limited thereto.

[0089] Example 1

[0090] 200 mmol of commercially available sodium trifluoromethanesulfinate was added to 500 ml of ethyl acetate and recrystallized. The resulting solid powder was then dried in a vacuum oven at 60-70°C for 10 hours to obtain the final pre-embedded sodium material, sodium trifluoromethanesulfinate. This pre-embedded sodium material is stable in dry air and can still be used normally after drying after absorbing moisture, demonstrating excellent chemical stability.

[0091] 100 mmol of sodium trifluoromethanesulfinate was added to 50 ml of acetonitrile and stirred evenly. 10 ml of concentrated hydrochloric acid was slowly added dropwise to form a white precipitate. After the addition was complete, the mixture was stirred at room temperature for 2 hours. After the reaction was complete, the precipitate was filtered to remove the precipitate, washed three times with ethyl acetate, and the filtrate was collected, dried over anhydrous sodium sulfate, and the solvent was removed to obtain trifluoromethanesulfinic acid.

[0092] The obtained trifluoromethylsulfinic acid was dissolved in 80ml of water, stirred evenly, and 90mmol of lithium hydroxide was added at 0°C. The temperature was slowly raised to room temperature and the reaction was carried out for 1 hour. After the reaction was completed, all the solvents were removed to obtain a white solid. An appropriate amount of ethyl acetate was added to the system to dissolve the solid. Dichloromethane was then added dropwise to the system until no more precipitation occurred, and a white solid was obtained by filtration. The same method was used for recrystallization three times, and the obtained solid powder was placed in a vacuum oven and vacuum-dried at 60-70°C for 10 hours to obtain the final pre-embedded lithium material, lithium trifluoromethylsulfinic acid. The pre-embedded lithium material is stable in dry air and can still be used normally after drying after absorbing moisture. It has good chemical stability.

[0093] Battery preparation and testing:

[0094] 50 mg of sodium trifluoromethanesulfinate was added to 1 g of sodium battery electrolyte (1.0 mol NaClO₄ EC:DEC = 1:1) and stirred to dissolve, yielding a sodium battery electrolyte with pre-intercalated sodium functionality. Carbon paper was used as the positive electrode. In a glove box, the positive electrode shell, carbon paper, separator, sodium sheet negative electrode, gasket, spring, and negative electrode shell were placed in sequence. The electrolyte was added, and the battery was secured using a battery press to assemble a button cell. As shown in Figure 1a, the assembled button cell was tested using an electrochemical workstation for CV curves with a scan range of 2.5-4.0 V and a scan rate of 0.1 mV / s. The CV curves demonstrate the irreversible sodium removal capacity of sodium trifluoromethanesulfinate. As shown in Figure 1b, the sodium trifluoromethanesulfinate removal capacity was tested using the button cell test channel, using constant current charge and discharge at a current of 0.06 mA and a cutoff voltage of 2.5-4.0 V. From the charge and discharge curves, it can be seen that sodium trifluoromethanesulfinate has a capacity close to 170mAh / g, and the decomposition potential is between 3.6-3.7V, which has a suitable sodium removal potential and meets the basic requirements of pre-embedded sodium materials.

[0095] Figure 1a shows the CV curve of the sodium trifluoromethanesulfinate button cell in this example. It can be seen that sodium trifluoromethanesulfinate begins to decompose upon charging at 3.7V, releasing sodium ions. Figure 1b shows the charge and discharge test of the sodium trifluoromethanesulfinate button cell in this example. It can be seen that sodium trifluoromethanesulfinate begins to decompose upon charging at 3.6V, with a capacity of nearly 170 mAh / g.

[0096] 10mg of lithium trifluoromethylsulfinate was added to 1g of lithium battery electrolyte (1.0mol LiClO4 EC:EMC=3:7) and stirred to dissolve, yielding a lithium battery electrolyte with pre-lithium insertion. Carbon paper was used as the positive electrode. In a glove box, the positive electrode shell, carbon paper, separator, lithium sheet negative electrode, gasket, spring, and negative electrode shell were placed in sequence. The electrolyte was added, and the battery was fixed using a battery press to assemble a button cell. As shown in Figure 2a, the assembled button cell was tested for CV curves using an electrochemical workstation with a scan range of 2.75-4.4V and a scan rate of 0.1mV / s. The CV curves demonstrate the irreversible delithiation capacity of lithium trifluoromethylsulfinate. As shown in Figure 2b, the delithiation capacity of lithium trifluoromethylsulfinate was tested using the button cell test channel, using constant current charge and discharge at a current of 0.06mA and a cutoff voltage of 2.75-4.3V. From the charge and discharge curves, it can be seen that lithium trifluoromethanesulfinate has a capacity close to 190mAh / g, and the decomposition potential is between 3.8-3.9V, which has a suitable delithiation potential and meets the basic requirements of pre-lithium insertion materials.

[0097] Figure 2a shows the CV curve of a lithium trifluoromethanesulfinate button cell in this embodiment. It can be seen that lithium trifluoromethanesulfinate begins to decompose upon charging at 3.8V, releasing lithium ions. Figure 2b shows the charge and discharge test of a lithium trifluoromethanesulfinate button cell in this embodiment. It can be seen that lithium trifluoromethanesulfinate begins to decompose upon charging at 3.8V, with a capacity of nearly 190 mAh / g.

[0098] Figure 3a shows the in-situ Raman measurement of the pre-lithiation method of the lithium trifluoromethanesulfinate electrolyte in this embodiment. It can be seen that the Raman characteristic peak of lithium trifluoromethanesulfinate gradually disappears during the charging process, indicating that the lithium trifluoromethanesulfinate in the electrolyte gradually decomposes and releases lithium ions. Figure 3b shows the Raman comparison of lithium trifluoromethanesulfinate powder, pure electrolyte, and lithium trifluoromethanesulfinate dissolved in pure electrolyte after charging in this embodiment. It can be seen that the Raman characteristic peak of lithium trifluoromethanesulfinate disappears after charging. At this time, the characteristic peak of the electrolyte is basically consistent with the Raman characteristic peak of the pure electrolyte, indicating that lithium trifluoromethanesulfinate completely disappears in the electrolyte after charging, and the charging pre-lithiation process has little effect on the electrolyte system.

[0099] FIG4 is a Raman comparison of a freshly prepared sample of lithium trifluoromethanesulfinate and a sample stored in dry air in this embodiment. It can be seen that the Raman characteristic peaks of the freshly prepared sample and the sample stored in air are basically consistent, indicating that the pre-embedded lithium material has good chemical stability.

[0100] Example 2

[0101] 200 mmol of commercially available sodium methanesulfinate was added to water and recrystallized. The resulting solid powder was then dried in a vacuum oven at 60-70°C for 10 hours to obtain the final pre-embedded sodium material, sodium methanesulfinate. This pre-embedded sodium material is stable in dry air and can still be used normally after drying after absorbing moisture, demonstrating excellent chemical stability.

[0102] 100 mmol of sodium methanesulfinate was added to 50 ml of acetonitrile and stirred. 10 ml of concentrated hydrochloric acid was slowly added dropwise to form a white precipitate. After the addition was complete, the mixture was stirred at room temperature for 2 hours. After the reaction was complete, the precipitate was filtered to remove the precipitate, washed three times with ethyl acetate, and the filtrate was collected, dried over anhydrous sodium sulfate, and the solvent was removed to obtain methanesulfinic acid.

[0103] The obtained methylsulfinic acid was dissolved in 80ml of water, stirred evenly, and 90mmol of lithium hydroxide was added at 0°C. The temperature was slowly raised to room temperature and the reaction was carried out for 1 hour. After the reaction was completed, all solvents were removed to obtain a white solid, which was washed three times with ethanol. The obtained solid powder was placed in a vacuum oven and vacuum-dried at 60-70°C for 10 hours to obtain the final pre-embedded lithium material, lithium methylsulfinic acid. The pre-embedded lithium material is stable in dry air and can still be used normally after drying after absorbing moisture. It has good chemical stability.

[0104] Battery preparation and testing:

[0105] 100mg of sodium methanesulfinate, 80mg of Super P, 400mg of PVDF solution (5% dissolved in NMP) and an appropriate amount of NMP were added to a ball mill and milled evenly using agate beads. A 200-micron thick film was scraped onto aluminum foil using a coating machine and vacuum dried in a vacuum oven at 60-70°C for 10 hours to obtain a sodium methanesulfinate electrode sheet, which was then cut into Φ12 discs. In a glove box, the positive electrode shell, sodium methanesulfinate electrode sheet, diaphragm, sodium sheet negative electrode, gasket, spring and negative electrode shell were placed in sequence, fixed using a battery press, and button cells were assembled. As shown in Figure 5a, the sodium methanesulfinate release capacity was tested using a button cell test channel, using constant current charge and discharge, a current of 0.06mA, and a cut-off voltage of 2.5-4.0V. From the charge and discharge curves, it can be seen that sodium methanesulfinate has a capacity of nearly 262 mAh / g, and the decomposition potential is between 3.2-3.3 V. It has a suitable sodium removal potential and meets the basic requirements of pre-embedded sodium materials.

[0106] Figure 5a shows the charge-discharge test of a sodium methanesulfinate button cell in this example. It can be seen that sodium methanesulfinate begins to decompose upon charge at 3.2V, with a capacity of approximately 262 mAh / g. This indicates that the pre-intercalation sodium material has a suitable sodium removal potential, meeting the basic requirements for pre-intercalation sodium materials.

[0107] 100mg of lithium methanesulfinate, 80mg of Super P, 400mg of PVDF solution (5% dissolved in NMP) and an appropriate amount of NMP were added to a ball mill and milled evenly using agate beads. A 200-micron thick film was scraped onto aluminum foil using a coating machine and vacuum-dried at 60-70°C in a vacuum oven for 10 hours to obtain a lithium methanesulfinate electrode sheet, which was then cut into Φ12 discs. In a glove box, the positive electrode shell, lithium methanesulfinate electrode sheet, diaphragm, lithium sheet negative electrode, gasket, shrapnel and negative electrode shell were placed in sequence, fixed using a battery press, and button cells were assembled. As shown in Figure 5b, the lithium methanesulfinate separation capacity was tested using a button cell test channel, using constant current charge and discharge, a current of 0.06mA, and a cut-off voltage of 2.75-4.3V. From the charge and discharge curves, it can be seen that lithium methanesulfinate has a capacity close to 310 mAh / g, and its decomposition potential is between 3.7-3.8 V. It has a suitable delithiation potential and meets the basic requirements of pre-lithium insertion materials.

[0108] Figure 5 shows the charge and discharge test of a lithium methanesulfinate button cell in this example. It can be seen that lithium methanesulfinate begins to decompose upon charge at 3.7V, with a capacity of approximately 311 mAh / g. This indicates that the pre-lithiation material has a suitable delithiation potential, meeting the basic requirements for pre-lithiation materials.

[0109] Example 3

[0110] 200 mmol of commercially available sodium ethylsulfinate was added to water and recrystallized. The resulting solid powder was then dried in a vacuum oven at 60-70°C for 10 hours to obtain the final pre-embedded sodium material, sodium ethylsulfinate. This pre-embedded sodium material is stable in dry air and can still be used normally after drying after absorbing moisture, demonstrating excellent chemical stability.

[0111] 100 mmol of sodium ethylsulfinate was added to 50 ml of acetonitrile and stirred. 10 ml of concentrated hydrochloric acid was slowly added dropwise to form a white precipitate. After the addition was complete, the mixture was stirred at room temperature for 2 hours. After the reaction was complete, the precipitate was removed by filtration and washed three times with ethyl acetate. The filtrate was collected, dried over anhydrous sodium sulfate, and the solvent was removed to obtain ethylsulfinic acid.

[0112] The obtained ethylsulfinic acid was dissolved in 80 ml of water and stirred evenly. 90 mmol of lithium hydroxide was added at 0 ° C and the temperature was slowly raised to room temperature for 1 hour. After the reaction was completed, all solvents were removed to obtain a white solid, which was washed three times with ethanol. The obtained solid powder was placed in a vacuum oven and vacuum-dried at 60-70 ° C for 10 hours to obtain the final pre-embedded lithium material lithium ethylsulfinate. The pre-embedded lithium material is stable in dry air and can still be used normally after drying after moisture absorption, and has good chemical stability.

[0113] Battery preparation and testing:

[0114] 100 mg of sodium ethylsulfinate, 80 mg of Super P, 400 mg of PVDF solution (5% dissolved in NMP) and an appropriate amount of NMP were added to a ball mill and milled evenly using agate beads. A 200 μm thick film was applied on aluminum foil using a coating machine and vacuum dried in a vacuum oven at 60-70°C for 10 hours to obtain a sodium ethylsulfinate electrode sheet, which was then cut into Φ12 discs. In a glove box, the positive electrode shell, sodium ethylsulfinate electrode sheet, diaphragm, sodium sheet negative electrode, gasket, spring and negative electrode shell were placed in sequence, fixed using a battery press, and button cells were assembled. As shown in Figure 5a, the sodium ethylsulfinate release capacity was tested using a button cell test channel, using constant current charge and discharge, a current of 0.06 mA, and a cut-off voltage of 2.5-4.0 V. From the charge and discharge curves, it can be seen that sodium ethylsulfinate has a capacity of nearly 230 mAh / g, and the decomposition potential is between 3.1-3.2 V, which has a suitable sodium removal potential and meets the basic requirements of pre-embedded sodium materials.

[0115] Figure 5a shows the charge-discharge test of a sodium ethylsulfinate button cell in this example. It can be seen that sodium ethylsulfinate begins to decompose upon charge at 3.1V, with a capacity of nearly 230 mAh / g. This indicates that the pre-intercalation sodium material has a suitable sodium removal potential, meeting the basic requirements for pre-intercalation sodium materials.

[0116] 100 mg of lithium ethylsulfinate, 80 mg of Super P, 400 mg of PVDF solution (5% dissolved in NMP) and an appropriate amount of NMP were added to a ball mill and milled evenly using agate beads. A 200-micron-thick film was applied on aluminum foil using a coating machine and vacuum-dried in a vacuum oven at 60-70°C for 10 hours to obtain a lithium ethylsulfinate electrode sheet, which was then cut into Φ12 discs. In a glove box, the positive electrode shell, lithium ethylsulfinate electrode sheet, diaphragm, lithium sheet negative electrode, gasket, spring and negative electrode shell were placed in sequence, fixed using a battery press, and button cells were assembled. As shown in Figure 5b, the lithium ethylsulfinate release capacity was tested using a button cell test channel, using constant current charge and discharge, a current of 0.06 mA, and a cut-off voltage of 2.75-4.3 V. From the charge and discharge curves, it can be seen that lithium ethylsulfinate has a capacity of nearly 265 mAh / g, and the decomposition potential is between 3.8-3.9 V. It has a suitable delithiation potential and meets the basic requirements of pre-lithium insertion materials.

[0117] Figure 5b shows the charge and discharge test of a lithium ethylsulfinate button cell in this example. It can be seen that the lithium ethylsulfinate begins to decompose upon charge at 3.8V and has a capacity of nearly 265 mAh / g. This indicates that the pre-lithiation material has a suitable delithiation potential, meeting the basic requirements for pre-lithiation materials.

[0118] Example 4

[0119] 200 mmol of commercially available sodium phenylsulfinate was added to water and recrystallized. The resulting solid powder was then dried in a vacuum oven at 60-70°C for 10 hours to obtain the final pre-embedded sodium material, sodium phenylsulfinate. This pre-embedded sodium material is stable in dry air and can still be used normally after drying after absorbing moisture, demonstrating excellent chemical stability.

[0120] 100 mmol of sodium phenylsulfinate was added to 50 ml of acetonitrile and stirred. 10 ml of concentrated hydrochloric acid was slowly added dropwise to form a white precipitate. After the addition was complete, the mixture was stirred at room temperature for 2 hours. After the reaction was complete, the precipitate was filtered to remove the precipitate, washed three times with ethyl acetate, and the filtrate was collected, dried over anhydrous sodium sulfate, and the solvent was removed to obtain phenylsulfinic acid.

[0121] The obtained phenylsulfinic acid was dissolved in 80 ml of water and stirred evenly. 90 mmol of lithium hydroxide was added at 0 ° C and the temperature was slowly raised to room temperature for 1 hour. After the reaction was completed, all solvents were removed to obtain a white solid, which was washed three times with ethanol. The obtained solid powder was placed in a vacuum oven and vacuum-dried at 60-70 ° C for 10 hours to obtain the final pre-embedded lithium material, lithium phenylsulfinate. The pre-embedded lithium material is stable in dry air and can still be used normally after drying after moisture absorption, and has good chemical stability.

[0122] Battery preparation and testing:

[0123] 100mg of sodium phenylsulfinate, 80mg of Super P, 400mg of PVDF solution (5% dissolved in NMP) and an appropriate amount of NMP were added to a ball mill and milled evenly using agate beads. A 200-micron-thick film was applied on aluminum foil using a coating machine and vacuum-dried in a vacuum oven at 60-70°C for 10 hours to obtain a sodium phenylsulfinate electrode sheet. The electrode sheet was cut into Φ12 discs. In a glove box, the positive electrode shell, sodium phenylsulfinate electrode sheet, diaphragm, sodium sheet negative electrode, gasket, spring and negative electrode shell were placed in sequence, fixed using a battery press, and button cells were assembled. As shown in Figure 5a, the sodium phenylsulfinate release capacity was tested using a button cell test channel, using constant current charge and discharge, a current of 0.06mA, and a cut-off voltage of 2.5-4.0V. From the charge and discharge curves, it can be seen that sodium phenylsulfinate has a capacity close to 163mAh / g, and the decomposition potential is between 3.3-3.4V, which has a suitable sodium removal potential and meets the basic requirements of pre-embedded sodium materials.

[0124] Figure 5a shows the charge-discharge test of a sodium phenylsulfinate button cell in this example. It can be seen that sodium phenylsulfinate begins to decompose at 3.3V and has a capacity of nearly 163 mAh / g. This indicates that the pre-intercalation sodium material has a suitable sodium removal potential, meeting the basic requirements for pre-intercalation sodium materials.

[0125] 100mg of lithium phenylsulfinate, 80mg of Super P, 400mg of PVDF solution (5% dissolved in NMP) and an appropriate amount of NMP were added to a ball mill and milled evenly using agate beads. A 200-micron-thick film was applied on aluminum foil using a film coater and vacuum-dried in a vacuum oven at 60-70°C for 10 hours to obtain a lithium phenylsulfinate electrode sheet. The electrode sheet was cut into Φ12 discs. In a glove box, the positive electrode shell, lithium phenylsulfinate electrode sheet, diaphragm, lithium sheet negative electrode, gasket, spring and negative electrode shell were placed in sequence, fixed using a battery press, and button cells were assembled. As shown in Figure 5b, the lithium phenylsulfinate release capacity was tested using a button cell test channel, using constant current charge and discharge, a current of 0.06mA, and a cut-off voltage of 2.75-4.3V. From the charge and discharge curves, it can be seen that lithium phenylsulfinate has a capacity of nearly 180 mAh / g, and the decomposition potential is between 3.9-4.0 V, which has a suitable delithiation potential and meets the basic requirements of pre-lithium insertion materials.

[0126] Figure 5b shows the charge-discharge test of a lithium phenylsulfinate button cell in this example. It can be seen that the lithium phenylsulfinate begins to decompose upon charge at 3.9V and has a capacity of nearly 181 mAh / g. This indicates that the pre-lithiation material has a suitable delithiation potential, meeting the basic requirements for pre-lithiation materials.

[0127] Example 5

[0128] 200 mmol of commercially available sodium p-tolylsulfinate was added to water and recrystallized. The resulting solid powder was then dried in a vacuum oven at 60-70°C for 10 hours to obtain the final pre-embedded sodium material, sodium p-tolylsulfinate. This pre-embedded sodium material is stable in dry air and can still be used normally after drying after absorbing moisture, demonstrating excellent chemical stability.

[0129] 100 mmol of sodium p-tolylsulfinate was added to 50 ml of acetonitrile and stirred. 10 ml of concentrated hydrochloric acid was slowly added dropwise to form a white precipitate. After the addition was complete, the mixture was stirred at room temperature for 2 hours. After the reaction was complete, the precipitate was filtered to remove the precipitate, washed three times with ethyl acetate, and the filtrate was collected, dried over anhydrous sodium sulfate, and the solvent was removed to obtain p-tolylsulfinic acid.

[0130] The obtained p-toluenesulfinic acid was dissolved in 80 ml of water and stirred evenly. 90 mmol of lithium hydroxide was added at 0 ° C and the temperature was slowly raised to room temperature for 1 hour. After the reaction was completed, all solvents were removed to obtain a white solid, which was washed three times with ethanol. The obtained solid powder was placed in a vacuum oven and vacuum-dried at 60-70 ° C for 10 hours to obtain the final pre-embedded lithium material p-toluenesulfinic acid lithium. The pre-embedded lithium material is stable in dry air and can still be used normally after drying after moisture absorption, and has good chemical stability.

[0131] Battery preparation and testing:

[0132] 100 mg of sodium p-tolylsulfinate, 80 mg of Super P, 400 mg of PVDF solution (5% dissolved in NMP) and an appropriate amount of NMP were added to a ball mill and milled evenly using agate beads. A 200 μm thick film was applied on aluminum foil using a film coater and vacuum dried in a vacuum oven at 60-70°C for 10 hours to obtain a sodium p-tolylsulfinate electrode sheet. The electrode sheet was cut into Φ12 discs. In a glove box, the positive electrode shell, sodium p-tolylsulfinate electrode sheet, diaphragm, sodium sheet negative electrode, gasket, spring and negative electrode shell were placed in sequence, fixed using a battery press, and button cells were assembled. As shown in Figure 5a, the sodium p-tolylsulfinate release capacity was tested using a button cell test channel, using constant current charge and discharge, a current of 0.06 mA, and a cut-off voltage of 2.5-4.0 V. From the charge and discharge curves, it can be seen that sodium p-tolylsulfinate has a capacity close to 150 mAh / g, and the decomposition potential is between 3.3-3.4 V, which has a suitable sodium removal potential and meets the basic requirements of pre-embedded sodium materials.

[0133] Figure 5a shows the charge-discharge test of a sodium p-tolylsulfinate button cell in this example. It can be seen that sodium p-tolylsulfinate begins to decompose at 3.3V and has a capacity of nearly 150 mAh / g. This indicates that the pre-intercalation sodium material has a suitable sodium removal potential, meeting the basic requirements for pre-intercalation sodium materials.

[0134] 100 mg of lithium p-toluenesulfinate, 80 mg of Super P, 400 mg of PVDF solution (5% dissolved in NMP) and an appropriate amount of NMP were added to a ball mill and milled evenly using agate beads. A 200-micron thick film was applied on aluminum foil using a coating machine and vacuum-dried in a vacuum oven at 60-70°C for 10 hours to obtain a lithium p-toluenesulfinate electrode sheet. The electrode sheet was cut into Φ12 discs. In a glove box, the positive electrode shell, lithium p-toluenesulfinate electrode sheet, diaphragm, lithium sheet negative electrode, gasket, spring and negative electrode shell were placed in sequence, fixed using a battery press, and button cells were assembled. As shown in Figure 5b, the lithium p-toluenesulfinate release capacity was tested using a button cell test channel, using constant current charge and discharge, a current of 0.06 mA, and a cut-off voltage of 2.75-4.3V. From the charge and discharge curves, it can be seen that lithium p-toluenesulfinate has a capacity close to 165 mAh / g, and the decomposition potential is between 3.9-4.0 V, which has a suitable delithiation potential and meets the basic requirements of pre-lithium embedding materials.

[0135] Figure 5b shows the charge-discharge test of a lithium p-toluenesulfinate button cell in this example. It can be seen that lithium p-toluenesulfinate begins to decompose upon charging at 3.9V, with a capacity of nearly 165 mAh / g. This indicates that the pre-lithiation material has a suitable delithiation potential, meeting the basic requirements for pre-lithiation materials.

[0136] Example 6

[0137] The pre-lithium intercalation materials, sodium p-chlorophenylsulfinate and lithium p-chlorophenylsulfinate, were prepared in the same manner as in Example 2, except that commercially available sodium p-chlorophenylsulfinate was used instead of sodium methanesulfinate. The pre-lithium intercalation materials were stable in dry air and could still be used normally after drying after absorbing moisture, demonstrating excellent chemical stability.

[0138] Battery preparation and testing:

[0139] Batteries were prepared and tested in the same manner as in Example 2. The desorption capacity of sodium p-chlorophenylsulfinate was tested using a button cell test channel. Constant current charging and discharging was used at a current of 0.06 mA and a cutoff voltage of 2.5-4.0 V. The sodium p-chlorophenylsulfinate was measured to have a capacity of approximately 135 mAh / g, and a decomposition potential between 3.3 and 3.4 V, indicating a suitable desodiumization potential, meeting the basic requirements for pre-sodium embedding materials. Similarly, the desorption capacity of lithium p-chlorophenylsulfinate was tested using a button cell test channel. Constant current charging and discharging was used at a current of 0.06 mA and a cutoff voltage of 2.75-4.3 V. The lithium p-chlorophenylsulfinate was measured to have a capacity of approximately 147 mAh / g, and a decomposition potential between 3.9 and 4.0 V, indicating a suitable delithiation potential, meeting the basic requirements for pre-lithium embedding materials.

[0140] Example 7

[0141] Pre-lithium intercalation materials, sodium tetrahydropyran-4-sulfinate and lithium tetrahydropyran-4-sulfinate, were prepared in the same manner as in Example 2, except that commercially available sodium tetrahydropyran-4-sulfinate was used instead of sodium methylsulfinate. The pre-lithium intercalation materials were stable in dry air and could still be used normally after drying after absorbing moisture, demonstrating excellent chemical stability.

[0142] Battery preparation and testing:

[0143] The battery was prepared and tested in the same manner as in Example 2. The sodium tetrahydropyran-4-sulfinate desorption capacity was tested using a button cell test channel. When constant current charging and discharging was used, the current was 0.06 mA, and the cut-off voltage was 2.5-4.0 V. The measured sodium tetrahydropyran-4-sulfinate had a capacity of approximately 157 mAh / g, and the decomposition potential was between 3.3-3.4 V, which had a suitable desodiumation potential and met the basic requirements for pre-sodium embedding materials. Similarly, the lithium tetrahydropyran-4-sulfinate desorption capacity was tested using a button cell test channel. When constant current charging and discharging was used, the current was 0.06 mA, and the cut-off voltage was 2.75-4.3 V. The measured lithium tetrahydropyran-4-sulfinate had a capacity of approximately 173 mAh / g, and the decomposition potential was between 3.9-4.0 V, which had a suitable delithiation potential and met the basic requirements for pre-lithium embedding materials.

[0144] Example 8

[0145] A lithium-free positive electrode material, sulfide polyacrylonitrile SPAN, is combined with graphite, and 2wt% lithium trifluoromethanesulfinate is dissolved in the electrolyte to construct a lithium-free soft-pack battery of approximately 28.6Ah.

[0146] The graphite used was commercially available graphite material (Sigma-Aldrich); the sulfided polyacrylonitrile used was a self-sintered material, and the elemental analysis results showed that the sulfur content was 39.5%, the carbon content was 40.58%, the nitrogen content was 15.05%, and the hydrogen content was 0.59%.

[0147] Conductive carbon, polyacrylonitrile sulfide, and PVDF in a 90:5:5 ratio were mixed with an appropriate amount of NMP, then evenly coated on aluminum foil, dried, and sheared to produce the positive electrode. Graphite, PVDF, and NMP in a 92:4:4 ratio were mixed with an appropriate amount of NMP, then evenly coated on copper foil, dried, and sheared to produce the negative electrode. This multilayer stack was used to construct a lithium-free soft-pack battery with an estimated 28.6Ah capacity, and the battery system was replenished with lithium through charging.

[0148] As shown in Figure 7, its energy density reaches 360Wh kg -1 Its first-cycle coulombic efficiency reaches 99.7%, and its capacity retention rate is still above 80% after 350 cycles of charge and discharge.

[0149] Example 9

[0150] Adopting positive electrode material NCM811 (LiNi 0.8 Mn 0.1 Co 0.1 O2) combined with SiO system, 2wt% lithium trifluoromethanesulfinate was dissolved in the electrolyte to construct a soft-pack lithium battery of about 14Ah.

[0151] SiO, conductive carbon (Super P), polyacrylic acid (PAA), and carbon nanotubes (CNTs) were mixed in a ratio of 80:10:4:6, and an appropriate amount of NMP was added and stirred evenly. The resulting negative electrode was coated on copper foil, dried, and sheared to produce the positive electrode. NCM 811, Super P, and PVDF were mixed in a ratio of 92:4:4, and an appropriate amount of NMP was added and stirred evenly. The resulting positive electrode was coated on aluminum foil, dried, and sheared to produce the negative electrode. A 14Ah dry cell battery was assembled with a negative to positive electrode capacity ratio of 1.01, and the battery system was replenished with lithium through charging.

[0152] As shown in Figure 8, its energy density reaches 352Wh kg -1 Its first-cycle coulombic efficiency reaches 99.7%, and after 800 cycles of charge and discharge, its capacity retention rate is still above 87.6%.

[0153] Example 10

[0154] Adopting positive electrode material NCM811 (LiNi 0.8 Mn 0.1 Co 0.1 O2) combined with SiO system, 2wt% lithium trifluoromethanesulfinate was dissolved in the electrolyte to construct a soft-pack lithium battery of about 3.0Ah.

[0155] The test conditions are as follows: electrode material loading 4.0mAh cm-2, negative electrode to positive electrode surface capacity ratio of 1.05, charge and discharge test at 0.5C rate. As shown in Figure 9, when no lithium replenishing material is added, the first efficiency of the soft pack battery is 57%. When the commercial lithium replenisher LNC is added, its first efficiency is increased to 62% at its maximum addition amount of 4% by mass. As shown in Figure 9, by replenishing lithium through the electrolyte in the present invention, its first efficiency can be increased to 100%, and compared with the battery system without adding lithium replenishing material and adding the commercial lithium replenisher LNC, while effectively improving the first efficiency of the battery, its cycle stability is not affected. After 800 stable cycles, its capacity retention rate is above 90%. It shows that the present invention has good practicality for lithium-poor battery systems.

[0156] Example 11

[0157] Sodium trifluoromethanesulfinate was dissolved in an electrolyte at 5 wt% to produce a sodium electrolyte with pre-intercalation of sodium. A sodium dry cell was assembled, the sodium electrolyte was injected, and the battery system was charged to replenish sodium. As shown in Figure 10, in a sodium-to-copper battery system, the addition of sodium trifluoromethanesulfinate to the electrolyte significantly improved both the charge and discharge capacities.

[0158] Example 12

[0159] A sodium-replenishing slurry is prepared by mixing 90 wt% sodium methanesulfinate with a certain proportion of conductive carbon and a binder. This slurry is then applied to the positive electrode sheet with a uniform thickness by knife coating. The slurry is then dried, assembled into a sodium-based dry cell, and then charged with sodium electrolyte. As shown in Figure 11, in a sodium-based copper battery system, the charge and discharge capacities of the positive electrode significantly improved after the sodium methanesulfinate coating was applied.

[0160] Example 13

[0161] Sodium methanesulfinate is mixed at a 5wt% ratio with a specific proportion of sodium cathode material, conductive carbon, and a binder to create a sodium cathode slurry. This slurry is then evenly coated onto the current collector to a desired thickness, dried, and assembled into a sodium dry cell. A sodium electrolyte is then injected and charged to replenish the sodium content of the battery system. As shown in Figure 12, in a sodium-to-copper battery system, adding a specific proportion of sodium methanesulfinate to the cathode significantly improves both the charge and discharge capacities.

[0162] Example 14

[0163] Using sodium-poor P2-type layered oxide (Na 0.67 Mn 0.67 Ni 0.33 O2) and hard carbon system, 5wt% sodium trifluoromethanesulfinate was dissolved in the electrolyte to construct a soft-pack sodium battery of about 1Ah.

[0164] Will Na 0.67 Mn 0.67 Ni 0.33 O2, conductive carbon (Super P), and PVDF were mixed in an 80:10:10 ratio with an appropriate amount of NMP, and then coated on aluminum foil to form the positive electrode. The mixture was then dried and cut to produce the positive electrode sheet. Hard carbon, Super P, and PVDF were mixed in a 92:4:4 ratio with an appropriate amount of NMP, and then coated on copper foil to form the negative electrode. The mixture was dried, cut, and assembled into a dry cell. A 1Ah dry cell was assembled with a negative to positive electrode capacity ratio of 1.1. Sodium replenishment was achieved through charging.

[0165] As shown in Figure 13, without sodium supplementation, the full battery has an initial capacity of only 77 mAh / g. By supplementing the electrolyte with sodium, an initial capacity of 96 mAh / g was achieved, which reaches the level of industrial sodium-rich cathode full batteries.

[0166] Example 15

[0167] A soft-pack lithium battery of approximately 1Ah is constructed using a graphite negative electrode and a lithium iron phosphate positive electrode system.

[0168] Conductive carbon, lithium iron phosphate, and PVDF in a 90:5:5 ratio were mixed with an appropriate amount of NMP, then evenly coated on aluminum foil, dried, and sheared to produce the positive electrode. Graphite, PVDF, and NMP in a 92:4:4 ratio were mixed with an appropriate amount of NMP, then evenly coated on copper foil, dried, and sheared to produce the negative electrode. These multiple layers were stacked to construct a 1Ah soft-pack battery. After 1800 cycles of 1C charge and discharge, the capacity decayed to 85%, resulting in the waste battery.

[0169] Without damaging the overall structure of the used battery, the electrolyte in the battery is drained out. 2 wt% lithium trifluoromethanesulfinate is dissolved in the electrolyte, and the electrolyte containing the lithium replenisher is injected into the used battery, and the battery system is replenished with lithium through charging.

[0170] As shown in Figure 14, after about 1800 cycles, the battery system capacity dropped to 85%. By using the method of replenishing lithium through the electrolyte described in the present invention, its capacity can be increased again to 99.6%. And after about 1800 cycles, the battery system capacity dropped again to 85%. By using the method of replenishing lithium through the electrolyte described in the present invention, its capacity can be increased again to 98.8%. And through the third cycle and electrolyte replenishment, the battery capacity can be restored to 98.1% again; after 7717 cycles, the battery capacity retention rate reached 97.4%. According to trend predictions, 30,000-60,000 battery cycles can be achieved.

[0171] First-cycle coulombic efficiency test method: Under constant current charge and discharge test conditions, the ratio of the first-cycle discharge capacity to the first-cycle charge capacity is the first-cycle coulombic efficiency.

[0172] Method for determining the capacity retention rate after n cycles of charge and discharge: Under constant current charge and discharge test conditions, the ratio of the discharge capacity of the nth cycle to the discharge capacity of the first cycle is the capacity retention rate after n cycles of charge and discharge.

[0173] Energy density test method: The product of the total capacity of the battery and the discharge voltage platform value is the battery capacity, the ratio of the battery capacity to the battery mass is the battery weight energy density, and the ratio of the battery capacity to the battery mass is the battery volume energy density.

[0174] The residual pre-embedding agent content in the electrodes of the above examples was measured and calculated to be less than 0.005 mmol.

[0175] Industrial applicability

[0176] According to the present invention, a pre-embedding agent, a pre-embedding lithium / sodium positive electrode, a lithium / sodium ion battery containing the same, and a pre-embedding lithium / sodium method can be provided, which have good stability, a safe and convenient pre-embedding lithium / sodium process, and a high energy density and capacity retention rate.

Claims

1. A pre-intercalation agent for pre-intercalating lithium or sodium, It is characterized in that The organic sulfinate represented by the following formula (1) is used as the skeleton. In the above formula (1), R is selected from an alkyl group having 1 to 10 carbon atoms and a halogenated alkyl group; an aryl group having a benzene ring, a thiophene ring, a furan ring, or a pyridine ring and a halogenated aryl group; a chain ether group and a cyclic ether group having 1 to 10 carbon atoms; a chain ester group and a cyclic ester group having 1 to 10 carbon atoms; and X represents Na or Li.

2. The pre-embedding agent according to claim 1, It is characterized in that In the formula (1), R is an alkyl group selected from -Me, -Et; -CF 3 , -C 2 F 5 , -C 4 F 9 haloalkyl; -Ph, -CH 3 C 6 H 4 , -C 5 NH 4 , -C 4 H 3 S, -C 4 H 3 O's aryl group; -FC 6 H 4 、-ClC 6 H 4 A halogenated aryl group.

3. A pre-embedded lithium positive electrode having a structure in which an active material layer containing a positive electrode active material, a conductive agent and a binder is formed on a current collector, It is characterized in that Pre-insertion lithium treatment is performed using the pre-insertion agent according to claim 1 or 2, wherein X in the formula (1) represents Li; Based on a 1Ah battery capacity, the content of the pre-embedded agent in the pre-embedded lithium positive electrode before the pre-embedded lithium treatment is n mol, and the content of the pre-embedded agent in the pre-embedded lithium positive electrode after the pre-embedded lithium treatment is less than 0.005 mmol, In the above formula, F is the Faraday constant, and c is the amount of pre-embedded lithium relative to the 1Ah battery capacity, measured in Ah.

4. The pre-embedded lithium positive electrode according to claim 3, It is characterized in that The positive electrode active material is selected from lithium iron phosphate, sulfide polyacrylonitrile (SPAN), ternary materials, lithium cobalt oxide, lithium manganese oxide, titanium disulfide, vanadium pentoxide, and Prussian blue.

5. A pre-installed lithium-ion secondary battery, It is characterized in that A lithium pre-embedded positive electrode as claimed in claim 3 or 4, and a negative electrode.

6. The preassembled lithium ion secondary battery according to claim 5, It is characterized in that The negative electrode is selected from graphite, lithium metal, silicon carbon, silicon, a composite of silicon and graphite, a composite of silicon and lithium metal, a composite of graphite and lithium metal, silicon monoxide, and black phosphorus.

7. A lithium ion secondary battery, It is characterized in that The preassembled lithium ion secondary battery according to claim 5 or 6 is obtained by subjecting the pre-lithium insertion treatment to the pre-assembled lithium ion secondary battery.

8. A pre-embedded sodium positive electrode having a structure in which an active material layer containing a positive electrode active material, a conductive agent and a binder is formed on a current collector, It is characterized in that The pre-embedding agent according to claim 1 or 2 is used for pre-embedding sodium treatment, wherein X in formula (1) represents Na; Based on the battery capacity of 1Ah, the content of the pre-embedding agent in the pre-embedding sodium positive electrode before the pre-embedding sodium treatment is n mol, and the content of the pre-embedding agent in the pre-embedding sodium positive electrode after the pre-embedding sodium treatment is less than 0.005 mmol, In the above formula, F is the Faraday constant, and c is the amount of pre-embedded sodium relative to the 1Ah battery capacity, measured in Ah.

9. The pre-embedded sodium positive electrode according to claim 8, It is characterized in that The positive electrode active material is selected from Na 0.67 Mn 0.67 Ni 0.33 O 2 P2-type layered oxide, Prussian blue, NaNi 0.33 Fe 0.33 Mn 0.33 O 2 Represents O3 type layered oxide, sodium vanadium phosphate.

10. A pre-installed sodium ion secondary battery, It is characterized in that A pre-embedded sodium positive electrode as claimed in claim 8 or 9.

11. The preassembled sodium ion secondary battery according to claim 10, It is characterized in that The negative electrode is selected from soft carbon and hard carbon.

12. A sodium ion secondary battery, It is characterized in that The pre-installed sodium ion secondary battery according to claim 10 or 11 is obtained by subjecting the pre-installed sodium ion secondary battery to the pre-sodium insertion treatment.

13. A method for pre-intercalating lithium or sodium, It is characterized in that The pre-intercalation agent according to claim 1 or 2 is used to carry out lithium or sodium pre-intercalation treatment.

14. The method for pre-inserting lithium or sodium according to claim 13, It is characterized in that The pre-intercalation agent is dissolved in an electrolyte to perform the pre-intercalation of lithium or sodium.

15. The method for pre-inserting lithium or sodium according to claim 14, It is characterized in that For the used battery electrode, the pre-intercalation agent is dissolved in the electrolyte, and the pre-intercalation lithium or sodium treatment is performed by adding the electrolyte.

16. The method for pre-inserting lithium or sodium according to claim 14 or 15, It is characterized in that The pre-embedding agent is dissolved in an electrolyte at a mass fraction of 0.1%-30% to perform the pre-embedding lithium or sodium treatment.

17. The method for pre-inserting lithium or sodium according to claim 13, It is characterized in that The pre-intercalation agent is doped into the positive electrode to perform the pre-intercalation of lithium or sodium.

18. The method for pre-inserting lithium or sodium according to claim 13, It is characterized in that The pre-intercalation agent is coated on the positive electrode to perform the pre-intercalation of lithium or sodium.

19. The method for pre-inserting lithium or sodium according to any one of claims 13-15, 17, and 18, It is characterized in that The electrolyte used in the lithium or sodium pre-intercalation treatment is a carbonate electrolyte or an ether electrolyte.

20. The method for pre-inserting lithium or sodium according to claim 19, It is characterized in that The carbonate electrolyte is selected from 1.0 mol NaClO 4 、1.0mol LiClO 4 、1.0mol LiPF 6 +1%LiClO 4 , 0.5mol LiBOB+0.5mol LiTFSI; the ether electrolyte is 1.0mol LiPF 6 +1%LiClO 4 .

21. A method for producing a pre-embedding agent for pre-embedding lithium, It is characterized in that The following steps are involved: Step (1): weighing an organic sulfinic acid sodium salt having an organic sulfinic acid salt structure of formula (1) according to claim 1 or 2, wherein X represents Na, placing the salt in a solvent, and recrystallizing the salt to obtain a pre-embedded sodium material; Step (2): weigh the pre-embedded sodium material in the above step (1), place it in an organic solvent, dropwise add an appropriate amount of acid, stir to react, extract and dry, and evaporate the solvent; Step (3): placing the product obtained in step (2) in deionized water, adding an appropriate amount of lithium salt, stirring to react, and evaporating the solvent; Step (4): recrystallize the solid obtained in step (3) using ethyl acetate and dichloromethane; dry the obtained solid powder to obtain an organic sulfinate lithium salt having an organic sulfinate structure of formula (1) according to claim 1 or 2, wherein X represents Li.

Citation Information

Patent Citations

  • Double-layer composite diaphragm cell and lithium supplement method thereof

    CN107845829A

  • Application of positive electrode sodium supplement agent in sodium ion battery

    CN110165218A

  • Lithium-sulfur battery electrode pre-lithiation method and lithium-sulfur battery

    CN116470165A

  • Method for pre-embedding lithium into positive electrode of lithium ion battery

    CN113097453A

  • Sodium ion battery

    CN114447333A

Cited By

  • Method for pre-embedding lithium / sodium into battery

    CN116487713A

  • A method for pre-lithiation / sodiation of a battery

    CN116487713B

  • Activation method of sodium-based silicate material as positive electrode of lithium-source-free lithium ion battery and application of sodium-based silicate material in lithium ion battery

    CN119601606A

  • Room-temperature sulfur-based sodium-ion battery based on hard carbon negative electrode and sulfurized polyacrylonitrile positive electrode and preparation of room-temperature sulfur-based sodium-ion battery

    CN120878942A

  • Sulfonate organic positive alkali metal ion supplement for secondary battery