Metal negative electrode protective film, secondary battery and electric device
By using A-based protective films in metal lithium batteries, the problem of active lithium consumption and dendrite growth in the negative electrode protective film is solved, the energy density and cycle performance of the battery are improved, and the service life of the battery is extended.
Patent Information
- Application Number
- PCT/CN2024/086761
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-17
AI Technical Summary
In existing metal lithium batteries, the formation and regeneration of the negative electrode protective film consumes active lithium, resulting in reduced battery energy density, short service life, and problems of dendrite growth and electrolyte reactive active material consumption.
An A-based protective film is used, which contains fluoride of the A element. The A element is sodium, potassium, rubidium, cesium, magnesium and calcium. The B element is lithium, sodium, potassium, magnesium and calcium. By forming a stable solid on the surface of the metal negative electrode The electrolyte interface inhibits dendrite growth and active material consumption and improves the electrochemical performance of the battery.
It achieves stable formation and regeneration of the negative electrode protective film, reduces the consumption of active materials, improves the energy density and cycle performance of the battery, inhibits the formation of dendrites, and extends the service life of the battery.
Smart Images

Figure CN2024086761_17102024_PF_FP_ABST
Abstract
Description
Metal negative electrode protective film, secondary battery and electrical device Technical Field
[0001] The present disclosure relates to the field of secondary batteries, and in particular to a metal negative electrode protective film, a secondary battery, and an electrical device. Background Art
[0002] Secondary batteries are important materials for electrical energy transfer and are widely used in new energy vehicles, portable electronics, energy storage, and other fields. In recent years, the application of batteries in electric vehicles has further increased our demand for high-energy-density and low-cost batteries, which has forced researchers to develop new high-energy-density battery systems.
[0003] Anode materials are one of the key factors limiting the energy density of secondary batteries. Metal anodes, due to their extremely high specific capacity and low electrode potential, can significantly improve the energy density of secondary batteries. However, most metal anodes suffer from issues such as dendrite growth, rapid active material consumption, and high reactivity with electrolytes, limiting their application. For example, in lithium secondary batteries, graphite anodes are a key factor limiting the energy density of existing lithium-ion batteries. As a high-energy-density anode material, lithium metal can significantly improve the energy density of lithium batteries. Lithium metal is extremely reactive, undergoing chemical and electrochemical reactions with most electrolytes, leading to rapid consumption of both the lithium metal and the electrolyte, reducing the battery's coulombic efficiency. Lithium atoms have a directional growth tendency during deposition, causing lithium metal to deposit in a dendritic manner. This results in significant volume deformation of the lithium metal during cycling, making it difficult to form a stable solid-electrolyte interphase (SEI) on the lithium metal surface. Furthermore, there is the risk of lithium dendrites piercing the separator, causing the battery to short-circuit. Currently, the direct use of lithium metal as anode in commercial applications still faces several technical challenges.
[0004] The uneven deposition / stripping of lithium ions causes lithium dendrites to easily peel off from the main body of metallic lithium and generate dead lithium, causing battery short circuit, which is very likely to cause battery explosion and pose a safety hazard. The SEI formed by metallic lithium during the cycle is helpful in blocking the mutual consumption between metallic lithium and electrolyte. However, conventional electrolytes either cannot generate a stable SEI on the metallic lithium electrode, thus failing to provide long-term, high-efficiency protection for metallic lithium batteries, or they cause the passage of solvent molecules and other ions other than lithium ions in the electrolyte, causing them to react with the metallic lithium negative electrode to generate by-products, consuming the active substances in the battery, or the generated SEI has weak conductivity for lithium ions, increasing the impedance of the battery and reducing the rate performance of the battery. Therefore, constructing a negative electrode protective film (SEI) with high stability, strong lithium conductivity and strong ability to inhibit side reactions is a key factor in improving the electrochemical performance of metallic lithium batteries.
[0005] In traditional lithium metal batteries, the formation and / or regeneration of the negative electrode protective film (SEI) on the surface of lithium metal consumes lithium ions, which leads to the following problems: (1) the content of active lithium in the battery is reduced, and the battery capacity is reduced; (2) the lithium ions consumed by the formation and / or regeneration of the traditional lithium metal negative electrode protective film come from the electrolyte and / or the positive electrode. Since the lithium content in the electrolyte and the positive electrode is very limited, the regeneration of SEI will quickly consume the active lithium in the battery, thereby reducing the battery life. The research papers "Electroless Formation of a Fluorinated Li / Na Hybrid Interphase for Robust Lithium Anodes" and "Improving metallic lithium anode with NaPF6 additive in LiPF6-carbonate electrolyte" reported that the sodium-containing negative electrode protective film (SEI) can improve the electrochemical performance of the negative electrode, but the sodium element in the SEI comes from the electrolyte or the positive electrode, making it difficult to maintain the long-term stability of the SEI structure, limiting the long-term cycle performance of the battery.
[0006] Therefore, there is an urgent need in this field to develop a new type of metal negative electrode protective film that can overcome the above-mentioned technical defects.
[0007] Summary of the Invention
[0008] In order to solve the problems existing in the prior art, including: 1. The side reaction between the metal negative electrode and the electrolyte continues to occur, and the formation and regeneration of the metal negative electrode SEI consumes a large amount of active material; 2. The electrolyte cannot form a stable SEI on the metal negative electrode, thereby failing to provide long-term, high-efficiency protection for the negative electrode; 3. The SEI of the metal negative electrode has a weak conductivity to the active material elements, which increases the impedance of the battery, reduces the battery's rate performance, and the negative electrode is prone to dendrite growth. On the one hand, the present disclosure provides an A-based protective film for the metal negative electrode of a secondary battery, wherein the A-based protective film conducts the B element as the active material in the secondary battery electrolyte;
[0009] The metal negative electrode includes a negative electrode base layer, the negative electrode base layer includes at least one inactive layer containing element A, and the element A is at least one of sodium, potassium, rubidium, cesium, magnesium and calcium.
[0010] The element B is different from the element A and is at least one of lithium, sodium, potassium, magnesium and calcium, and the redox reaction potential of the element B is lower than that of the element A.
[0011] Wherein, the A-based protective film contains fluoride of element A and is located on at least part of the surface of the negative electrode base layer of the metal negative electrode. The formation and regeneration of the A-based protective film consumes the inactive material of the negative electrode base layer, thereby reducing the consumption of the active material element B, which is one of the core innovations of the present invention. In the present invention, the active material undergoes a reversible valence change in the battery charging and discharging process, and a reversible electrochemical reaction occurs. The inactive layer is a functional auxiliary layer for achieving uniform deposition of the active material. This functional auxiliary layer is a key material for forming the negative electrode protective film (SEI) and for dynamically repairing the negative electrode protective film. The B element ions are reduced in the form of B element metal during charging and oxidized to B element ions during discharging, so the active material is B element metal. Specifically, the A element is not embedded in the positive electrode material or the positive electrode material preferentially embeds the B element, so the A element ions cannot be reversibly embedded in and out of the positive electrode material, that is, the A element ions cannot reversibly gain or lose electrons during the charging and discharging process of the battery, that is, they cannot reversibly participate in the charging and discharging of the battery.
[0012] In some embodiments of the present disclosure, the A-based protective film includes a solid electrolyte interface (SEI) film constructed on the surface of the negative electrode base layer, an SEI film formed in situ by the electrolyte and the negative electrode base layer, or a combination thereof.
[0013] In some embodiments of the present disclosure, the A-based protective film further comprises a fluoride of the B element.
[0014] In some embodiments of the present disclosure, the electrolyte contains fluorine-containing anions. Preferably, the fluorine-containing anions contained in the electrolyte are selected from at least one of bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate and difluorophosphate.
[0015] In some embodiments of the present disclosure, the in-situ formation of the SEI film includes formation through a self-limiting reaction between the negative electrode base layer and the electrolyte under battery charge-discharge or non-charge-discharge conditions.
[0016] In another aspect, the present disclosure provides a method for preparing the A-based protective film, the method comprising:
[0017] (1) Under the protection of an inert gas, melting the A element metal and an optional auxiliary metal, and cooling to obtain a negative electrode base layer including at least one inactive layer containing the A element;
[0018] (2) compounding the negative electrode base layer onto the current collector surface to obtain a metal negative electrode; and
[0019] (3) Under the protection of an inert gas, the metal negative electrode is brought into contact with an electrolyte to form an A-based protective film on at least a portion of the surface of the negative electrode base layer.
[0020] In some embodiments of the present disclosure, the electrolyte comprises fluoride.
[0021] In some embodiments of the present disclosure, the inert gas includes at least one of nitrogen, argon, and neon.
[0022] In some embodiments of the present disclosure, the concentration of the electrolyte is between 0.5 mol / L and 7 mol / L.
[0023] In another aspect, the present disclosure provides a secondary battery comprising a positive electrode sheet, an electrolyte, a metal negative electrode sheet, and the A-based protective film, wherein the metal negative electrode comprises a negative electrode base layer, the negative electrode base layer comprises at least one inactive layer containing element A, and the element A is at least one of sodium, potassium, rubidium, cesium, magnesium, and calcium.
[0024] The electrolyte includes B element as an active material;
[0025] The element B is different from the element A and is at least one of lithium, sodium, potassium, magnesium and calcium, and the redox reaction potential of the element B is lower than that of the element A.
[0026] The A-based protective film contains fluoride of element A and is located on at least a portion of the surface of the negative electrode base layer of the metal negative electrode.
[0027] In some embodiments of the present disclosure, the metal negative electrode further includes a negative electrode enhancement film located on at least a portion of the surface of the A-based protective film.
[0028] In some embodiments of the present disclosure, the A element and the B element are combined in any of the following ways: a combination of magnesium element and sodium element, a combination of magnesium element and lithium element, a combination of magnesium element and potassium element, a combination of magnesium element and calcium element, a combination of sodium element and potassium element, a combination of sodium element and lithium element, a combination of sodium element and calcium element, a combination of calcium element and potassium element, a combination of calcium element and lithium element, or a combination of potassium element and lithium element.
[0029] In some embodiments of the present disclosure, the solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound, and a ketal compound.
[0030] On the other hand, the present disclosure provides an electrical device including the secondary battery.
[0031] The surface of the metal negative electrode of the secondary battery in the present invention can form a stable A-based protective film (such as a sodium-based protective film), which is generated by a self-limiting reaction between the negative electrode base layer and the electrolyte. The composition is mainly inorganic fluoride, the structure is stable, and it is difficult to dissolve in the electrolyte. The formation and regeneration of the A-based protective film consumes the inactive substances in the negative electrode base layer, thereby reducing the consumption of active substances. It has a strong ion (for example, lithium ion) conductivity, promotes ions to obtain electrons and reduce on the surface of the negative electrode base layer, and inhibits the generation of dendrites. At the same time, the conductivity of the solvent molecules in the electrolyte is weak, avoiding adverse side reactions at the negative electrode, thereby inhibiting the decomposition of the electrolyte and the loss of active substances, maintaining the stability of the metal negative electrode structure, and improving the electrochemical performance of the battery.
[0032] The negative electrode base layer of the present invention is selected from the simple substances of sodium, potassium, rubidium, cesium, magnesium and calcium, or alloys of sodium, potassium, rubidium, cesium, magnesium and calcium as an inactive layer. When the B element metal is deposited on the surface of the negative electrode base layer in the form of dendrites, the B element metal and the A element metal in the negative electrode base layer form a primary battery in a local area. The A and B elements have different redox reaction potentials. Driven by the redox potential difference, the B atoms in the B element dendrites dissolve in the form of B element ions, pass through the A-based protective film and re-obtain electrons on the negative electrode surface to be reduced and deposited. After the B element ions that pass through the A-based protective film are deposited again on the negative electrode surface, they can quickly diffuse and dissolve with the negative electrode base layer, thereby eliminating the B element dendrites.
[0033] In the present invention, element B acts as an active material, reversibly gaining and losing electrons and undergoing reversible valence changes during the battery's charge and discharge processes. The negative electrode substrate layer containing the inactive substance element A is a functional auxiliary material that achieves uniform deposition of element B metal and eliminates dendrite growth. This functional auxiliary material is a key material for forming the negative electrode protective film (i.e., SEI) and for dynamically repairing the negative electrode protective film, and is also one of the core points of the present invention.
[0034] These and other features and advantages will become apparent from reading the following detailed description and referring to the associated drawings.It is to be understood that both the foregoing general description and the following detailed description are illustrative only and are not restrictive of the aspects claimed. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] FIG1 is a schematic diagram of the structure of a metal negative electrode sheet with an A-based protective film in a specific embodiment of the present application.
[0036] FIG2 is a SEM image of the negative electrode base layer after the battery cycle is completed in Example 7 of the present application.
[0037] FIG3 is a SEM image of the negative electrode base layer in Comparative Example 6 of the present application after the battery cycle is completed. DETAILED DESCRIPTION
[0038] The present application is described in detail below with reference to the accompanying drawings, and the features of the present application will be further revealed in the following specific description.
[0039] " Scope " disclosed herein is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a scope with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for a particular parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0040] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution. In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0041] In this application, unless otherwise specified, the terms "include" and "comprising" used herein may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0042] In the description herein, unless otherwise indicated, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0043] It should be understood that, in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, features defined as "first", "second", etc. may explicitly or implicitly include one or more of such features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0044] It should be noted that, in the description of the present invention, unless otherwise expressly specified or limited, the terms "disposed," "connected," and "connected" should be understood in a broad sense. For example, they may refer to fixed connections, detachable connections, or integral connections; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; and internal connections between two components. Those skilled in the art will understand the specific meanings of the above terms in the present invention based on specific circumstances.
[0045] In order to solve the problems of dendrite formation and active material consumption in the metal negative electrode of the prior art during the charge and discharge cycle, while maintaining the high energy density of the battery, the present disclosure provides an A-based protective film for the metal negative electrode of a secondary battery. The A-based protective film is constructed on a metal negative electrode plate containing a metal element of sodium, potassium, rubidium, cesium, magnesium, or calcium, or an alloy of sodium, potassium, rubidium, cesium, magnesium, or calcium as the negative electrode base layer, thereby inhibiting the reaction between the electrolyte and the negative electrode, reducing the loss of active metal and electrolyte, promoting the migration and diffusion of ions, and inhibiting the formation of dendrites, thereby improving the electrochemical performance of the battery. In the secondary battery, the A metal or A alloy inactive layer serves as the negative electrode base layer of the negative electrode plate. When the redox reaction potential of the B element is lower than that of the A element, the A metal or A alloy negative electrode base layer can eliminate the B metal dendrites deposited on its surface. Furthermore, the negative electrode base layer containing element A can serve as the source of element A in the negative electrode protective film. As an inactive layer, the negative electrode base layer consumes inactive material to provide element A for the formation and regeneration of the A-based protective film, thereby reducing the consumption of active element B and protecting element B. As mentioned above, active material elements have a direct impact on battery capacity, reversibly gaining and losing electrons during the battery's charge and discharge process, participating in charge transfer. Inactive material elements have no direct impact on battery capacity and cannot reversibly participate in charge transfer during the battery's charge and discharge process.
[0046] In the present disclosure, metal dendrites are eliminated through the principle of the primary battery, providing the possibility of eliminating the formation of metal dendrites from the principle level. The present disclosure adopts an inactive layer containing element A metal or element A alloy as the negative electrode base layer, and adopts element B as the active material. When element B ions are deposited on the surface of the inactive layer containing A in the form of dendrites, the metal dendrites of element B and the inactive layer containing A form a primary battery in the local area. The redox potential of element B is lower than that of element A. Driven by the redox potential difference between element A and element B, metal dendrites of element B are dissolved in the form of element B ions and obtain electrons on the surface of the inactive layer containing A and are reduced and deposited. The metal of element A and the metal of element B fuse with each other, and the metal of element B deposited on the surface of the metal of element A can diffuse rapidly with the metal of element A, thereby avoiding the formation of metal dendrites of element B. The present disclosure is different from the mechanism of the prior art in which two or more cations act as carriers to suppress the formation of metal dendrites. The element A ions in the present disclosure do not act as carriers and reversibly participate in the charge transfer during the battery charging and discharging process, but eliminate metal dendrites of element B through the mechanism of the primary battery and the formation of BA alloy. The present invention uses cations of a single metal as carriers, which is beneficial to reducing the manufacturing, use and management costs of the battery.
[0047] In order to inhibit the reaction between the electrolyte and the negative electrode, reduce the loss of active materials and electrolytes, and promote the migration and diffusion of ions, the A-based protective film for the metal negative electrode of the secondary battery of the present invention can conduct the B element as the active material in the secondary battery electrolyte. Preferably, the A-based protective film can hinder the passage of solvent molecules, thereby preventing them from contacting the negative electrode base layer in the metal negative electrode; wherein, the metal negative electrode includes a negative electrode base layer, the negative electrode base layer includes at least one inactive layer containing element A, and the A element is at least one of sodium, potassium, rubidium, cesium, magnesium and calcium, the B element is different from the A element, and is at least one of lithium, sodium, potassium, magnesium and calcium, and the redox reaction potential of the B element is lower than that of the A element, wherein the A-based protective film contains a fluoride of the A element and is located on at least a portion of the surface of the negative electrode base layer of the metal negative electrode.
[0048] In a specific embodiment, the A element and the B element are combined in any of the following ways: a combination of magnesium element and sodium element, a combination of magnesium element and lithium element, a combination of magnesium element and potassium element, a combination of magnesium element and calcium element, a combination of sodium element and potassium element, a combination of sodium element and lithium element, a combination of sodium element and calcium element, a combination of calcium element and potassium element, a combination of calcium element and lithium element, or a combination of potassium element and lithium element.
[0049] In a specific embodiment, the A-based protective film may include at least one layer, wherein the A-based protective film includes a solid electrolyte interface (SEI) film (artificially) constructed on the surface of the negative electrode base layer, an SEI film formed in situ by the electrolyte and the negative electrode base layer, or a combination thereof, for example, a single-layer or multi-layer SEI film formed by a mixed combination of artificial construction and in situ reaction.
[0050] In a specific embodiment, in the case of an A-based protective film formed by the in-situ reaction between the sodium negative electrode base layer and the electrolyte, the main component of the A-based protective film is an inorganic salt containing cations of the element A. The A-based protective film with the inorganic salt as the main component has high structural stability and is poorly soluble in the electrolyte, which is beneficial for improving the long-term cycle stability of the battery and inhibiting the formation of metal dendrites.
[0051] In a specific embodiment, the electrolyte contains fluorine-containing anions. Preferably, the fluorine-containing anions contained in the electrolyte are selected from at least one of bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate and difluorophosphate. In a preferred embodiment, the electrolyte contains hexafluorophosphate of element B cations. In a preferred embodiment, the anion that undergoes a self-limiting reaction with the negative electrode base layer is hexafluorophosphate. The reaction of the fluorine-containing anions with the negative electrode base layer can form an A-based protective film with higher ionic conductivity, improve the stability of the A-based protective film, and limit adverse side reactions between the electrolyte and the negative electrode base layer.
[0052] In a specific embodiment, the in-situ formation of the SEI film includes formation through a self-limiting reaction between the negative electrode substrate layer and the electrolyte under battery charge-discharge or non-charge-discharge conditions.
[0053] As shown in Figure 1, the negative electrode plate 1 includes a current collector 11, at least one layer of inactive material containing element A metal or element A alloy formed on the surface of the current collector 11 as a negative electrode base layer 12, an A-based negative electrode protection film 13 formed on at least part of the surface of the negative electrode base layer 12, and a negative electrode reinforcement film 14 formed on at least part of the surface of the A-based negative electrode protection film 13.
[0054] In one embodiment of the present disclosure, a method for preparing the A-based protective film includes:
[0055] (1) Under the protection of an inert gas, melting element A metal, or element A and optional other alloy materials, and cooling to obtain a negative electrode base layer including at least one inactive layer containing element A; In a specific embodiment, under the protection of an inert gas, heating a metal element of sodium, potassium, magnesium, or calcium, or a mixture of a metal element of sodium, potassium, magnesium, or calcium and a certain proportion of other alloy materials, completely melting and fully and evenly stirring, and cooling to obtain a negative electrode base layer composed of a metal element of sodium, potassium, magnesium, or calcium or an alloy of sodium, potassium, magnesium, and calcium;
[0056] (2) compounding the negative electrode base layer onto the surface of the current collector to obtain a metal negative electrode; in a specific embodiment, the negative electrode base layer is heated under the protection of an inert gas, and a conductive carrier (current collector) is brought into contact with the negative electrode base layer to obtain a metal negative electrode loaded with the negative electrode base layer and the conductive carrier; and
[0057] (3) Under the protection of an inert gas, the metal negative electrode is brought into contact with an electrolyte, and an A-based protective film is formed on at least a portion of the surface of the negative electrode base layer. In a specific embodiment, under the protection of an inert gas, the metal negative electrode that has not been cooled is inserted into the electrolyte for quenching to obtain a metal negative electrode having an A-based protective film.
[0058] In a specific embodiment, the electrolyte contains fluoride, and the time for the negative electrode base layer to react with the electrolyte to form the A-based protective film is 0.1-20 hours, 0.5-15 hours, 1-10 hours, 3-8 hours, or any numerical range consisting of the end values of the above ranges. When the reaction time for forming the A-based protective film is within the above range, the A-based protective film has a high ionic conductivity, can effectively block adverse side reactions between the negative electrode base layer and the electrolyte, inhibit dendrite formation, improve battery production efficiency, and reduce battery manufacturing costs.
[0059] In some embodiments of the present disclosure, the inert gas includes at least one of nitrogen, argon, and neon.
[0060] In some embodiments of the present disclosure, the concentration of the electrolyte is between 0.5 mol / L and 7 mol / L, between 1 mol / L and 6 mol / L, between 3 mol / L and 5 mol / L, or any numerical range consisting of the end values of the above ranges. When the concentration of the electrolyte is within the above range, the electrolyte has high ionic conductivity, strong operability, and good wettability, and can efficiently form an A-based protective film with high ionic conductivity and stable structure on the surface of the negative electrode base layer, thereby inhibiting the formation of dendrites.
[0061] In the present disclosure, a secondary battery includes a positive electrode plate, an electrolyte, a metal negative electrode plate and the A-based protective film, wherein the metal negative electrode includes a negative electrode base layer, the negative electrode base layer includes at least one inactive layer containing element A, and the element A is at least one of sodium, potassium, rubidium, cesium, magnesium and calcium, the electrolyte includes element B as an active material, which is at least one of lithium, sodium, potassium, magnesium and calcium, the element B is a different element from A, and the redox reaction potential of element B is lower than that of element A, wherein the A-based protective film contains fluoride of element A and is located on at least a portion of the surface of the negative electrode base layer of the metal negative electrode.
[0062] In some embodiments of the present disclosure, the metal negative electrode further includes a negative electrode enhancement film located on at least a portion of the surface of the A-based protective film.
[0063] In some embodiments of the present disclosure, the A element and the B element are combined in any of the following ways: a combination of magnesium element and sodium element, a combination of magnesium element and lithium element, a combination of magnesium element and potassium element, a combination of magnesium element and calcium element, a combination of sodium element and potassium element, a combination of sodium element and lithium element, a combination of sodium element and calcium element, a combination of calcium element and potassium element, a combination of calcium element and lithium element, or a combination of potassium element and lithium element.
[0064] In some embodiments of the present disclosure, the solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound, and a ketal compound.
[0065] In another preferred embodiment, the positive electrode active material does not undergo a reversible electrochemical reaction with element A ions or preferentially undergoes a reversible electrochemical reaction with element B ions; preferably, the positive electrode active material is a polyanion salt type, a metal oxide type, or a compound type.
[0066] In some embodiments of the present disclosure, the B element is lithium, the A element is sodium, and the positive electrode plate includes at least one of lithium cobaltate, lithium manganeseate, lithium nickelate, lithium iron phosphate, lithium nickel cobalt manganeseate, lithium nickel cobalt aluminum oxide, lithium manganese iron phosphate and lithium manganese phosphate.
[0067] In the present disclosure, the electrolyte comprises a solvent and a fluorine-containing salt. The electrolyte comprises at least one anion selected from fluorine-containing anions, preferably at least one selected from bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate, and difluorophosphate.
[0068] In the present disclosure, the solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound and a ketal compound. In a preferred embodiment, the solvent is an ether solvent. More preferably, the solvent is ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, polyethylene glycol dimethyl ether, ethylene glycol methyl ether ethyl ether, ethylene glycol diethyl ether, diethylene glycol methyl ether ethyl ether, diethylene glycol diethyl ether, triethylene glycol methyl ether ethyl ether, triethylene glycol diethyl ether, tetraethylene glycol methyl ether ethyl ether, tetraethylene glycol diethyl ether, ethylene glycol methyl ether propyl ether, ethylene glycol ethyl ether propyl ether, ethylene glycol dipropyl ether, diethylene glycol methyl ether propyl ether, diethylene glycol ethyl ether propyl ether, diethylene glycol dipropyl ether, triethylene glycol methyl ether propyl ether, triethylene glycol ethyl ether At least one of propyl ether, triethylene glycol dipropyl ether, tetraethylene glycol methyl ether propyl ether, tetraethylene glycol ethyl ether propyl ether, tetraethylene glycol dipropyl ether, ethylene glycol methyl ether butyl ether, ethylene glycol ethyl ether butyl ether, ethylene glycol propyl ether butyl ether, ethylene glycol dibutyl ether, diethylene glycol methyl ether butyl ether, diethylene glycol ethyl ether butyl ether, diethylene glycol propyl ether butyl ether, diethylene glycol dibutyl ether, triethylene glycol methyl ether butyl ether, triethylene glycol ethyl ether butyl ether, triethylene glycol propyl ether butyl ether, triethylene glycol dibutyl ether, tetraethylene glycol methyl ether butyl ether, tetraethylene glycol ethyl ether butyl ether, tetraethylene glycol propyl ether butyl ether, and tetraethylene glycol dibutyl ether. When the electrolyte solvent is selected from the above range, the reaction activity of the solvent with the negative electrode base layer is low, the structures of the negative electrode base layer and the A-based protective film are stable, the ionic conductivity of the electrolyte and the A-based protective film is high, dendrite formation is suppressed, the battery charge and discharge coulomb efficiency is high, and the service life is long.
[0069] In the present disclosure, the concentration of the fluorine-containing salt in the electrolyte is 0.5mol / L-7mol / L, 1mol / L-5mol / L, 2mol / L-4mol / L or any numerical range consisting of the end values of the above ranges. In some embodiments of the present application, the electrolyte further includes additives, and the additives include, but are not limited to: 1,3-dioxolane, 1,4-dioxane, trioxymethylene, lithium nitrate, lithium fluorosulfonate, sulfur dioxide, fluoroethylene carbonate, 12-crown ether-4, 15-crown ether-5 and 18-crown ether-6. In some embodiments, the mass content of the additive in the electrolyte is 0.1% to 20%, 1% to 15% or 5% to 10%.
[0070] secondary batteries
[0071] The secondary battery of this application includes a positive electrode (pole), a negative electrode (pole), a separator (optional), and an electrolyte (liquid or solid electrolyte). During the battery's charge and discharge process, active ions are intercalated and released back and forth between the positive and negative electrodes. The electrolyte acts as a conductor of ions between the positive and negative electrodes.
[0072] [Positive electrode]
[0073] In the secondary battery of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode film layer (or positive electrode active material layer) provided on at least one surface of the positive electrode current collector and including a positive electrode active material. For example, the positive electrode current collector has two surfaces opposite to each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is provided on any one or both of the two opposite surfaces of the positive electrode current collector. In the secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. For example, the metal foil may be an aluminum foil, and the composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene PP, polyethylene terephthalate PET, polybutylene terephthalate PBT, polystyrene PS, polyethylene PE and its copolymers, etc.).
[0074] In the secondary battery of the present application, the positive electrode active material containing the metal element B can be a positive electrode active material for secondary batteries known in the art. For example, the positive electrode active material may include one or more of the following: a layered oxide containing element B ions, a polyanion material, or a Prussian blue-based material. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for secondary batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more.
[0075] In some embodiments, the positive electrode film layer may also optionally include a binder. Non-limiting examples of binders that can be used for the positive electrode film layer may include one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. In an embodiment of the present application, the first positive active material layer and / or the second positive active material layer each independently contain a binder selected from polyvinylidene fluoride, polyacrylic acid, polytetrafluoroethylene, polyimide and combinations thereof.
[0076] In some embodiments, the positive electrode film layer may further optionally include a conductive agent. Examples of conductive agents for the positive electrode film layer may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In an embodiment of the present application, the first positive electrode active material layer and / or the second positive electrode active material layer each independently contain a conductive agent selected from graphite, carbon black, acetylene black, graphene, carbon nanotubes, and combinations thereof.
[0077] In one embodiment of the present application, the positive electrode can be prepared in the following manner: the above-mentioned components for preparing the positive electrode, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a uniform positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0078] [Negative electrode]
[0079] In the secondary battery of the present application, the negative electrode plate does not exclude other additional functional layers in addition to the negative electrode base layer. For example, in certain embodiments, the negative electrode plate of the present application may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode base layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode plate of the present application may further include a covering protective layer covering the surface of the second negative electrode film layer.
[0080] In the secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, the metal foil may be a copper foil, silver foil, iron foil, or a foil composed of alloys of the above metals. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material base layer (such as a base layer made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene PE, and copolymers thereof).
[0081] [Electrolytes]
[0082] The electrolyte conducts ions between the positive and negative electrodes. The electrolyte can be selected from at least one of a solid electrolyte, a semi-solid electrolyte, and a liquid electrolyte. In one embodiment of the present application, the electrolyte may optionally contain additives. For example, the additives may include one or more of the following: negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, additives that improve battery low-temperature performance, etc.
[0083] [Isolation film]
[0084] In one embodiment of the present application, the secondary battery further comprises a separator, which separates the anode side of the secondary battery from the cathode side, and provides selective permeation or blocking for substances of different types, sizes and charges in the system. For example, the separator can insulate electrons, physically isolate the positive electrode and the negative electrode of the secondary battery, prevent internal short circuits and form an electric field in a certain direction, and at the same time allow ions in the battery to pass through the separator and move between the positive and negative electrodes. In one embodiment of the present application, the material used to prepare the separator may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different. In an embodiment of the present application, the separator is selected from polyolefin separators, polyester separators, polyimide separators, polyamide separators and cellulose separators.
[0085] In one embodiment of the present application, the positive electrode sheet, negative electrode sheet and separator can be made into an electrode assembly / bare cell through a winding process or a lamination process.
[0086] In one embodiment of the present application, the secondary battery may include an outer packaging that can be used to encapsulate the above-mentioned electrode assembly and electrolyte. In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. In other embodiments, the outer packaging of the secondary battery can be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.
[0087] The shape of the secondary battery of the present application may be cylindrical, square or any other shape. The outer packaging may include a shell and a cover plate, and the shell may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell has an opening connected to the receiving cavity, and the cover plate can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly through a winding process or a lamination process, and the electrode assembly is encapsulated in the receiving cavity, and the electrolyte is impregnated in the electrode assembly. The number of electrode assemblies contained in the secondary battery may be one or more.
[0088] In one embodiment of the present application, several secondary batteries may be assembled together to form a battery module. The battery module includes two or more secondary batteries, and the specific number depends on the application of the battery module and the parameters of a single battery module.
[0089] In a battery module, multiple secondary batteries may be arranged sequentially along the length of the battery module. Of course, they may also be arranged in any other manner. Furthermore, the multiple secondary batteries may be secured using fasteners. Optionally, the battery module may further include a housing having a storage space, wherein the multiple secondary batteries are housed in the storage space.
[0090] In one embodiment of the present application, two or more of the aforementioned battery modules can be assembled into a battery pack. The number of battery modules contained in the battery pack depends on the application of the battery pack and the parameters of the individual battery modules. The battery pack can include a battery box and multiple battery modules disposed within the battery box. The battery box includes an upper box body and a lower box body. The upper box body can cover the lower box body and fit well therewith to form an enclosed space for accommodating the battery modules. The two or more battery modules can be arranged in the battery box in any desired manner.
[0091] In one embodiment of the present application, an exemplary battery pack may include a battery case and a plurality of battery modules disposed within the battery case. The battery case includes an upper case and a lower case, with the upper case covering the lower case and forming an enclosed space for accommodating the battery modules. The plurality of battery modules may be arranged in any manner within the battery case.
[0092] Electrical devices
[0093] In one embodiment of the present application, an electrical device of the present application includes at least one of the secondary battery, battery module, or battery pack of the present application, and the secondary battery, battery module, or battery pack can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device includes, but is not limited to, mobile digital devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc.
[0094] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0095] In the following, the influence of the secondary battery manufactured according to the embodiment of the present application on the performance of the electrochemical device is characterized based on specific examples. However, it should be pointed out that the scope of protection of the present application is defined by the claims and is not limited to the above specific embodiments.
[0096] Example
[0097] Unless otherwise specified, all raw materials used in the present invention were of analytical grade and all water used was deionized water.
[0098] 1. Preparation of positive electrode sheet
[0099] 10 wt% of polyvinylidene fluoride was dissolved in N-methylpyrrolidone as a binder, and 80 wt% of a polyanion salt-type positive electrode active material containing B element (see Table 1-4 for details) and 10 wt% of conductive carbon black were added to prepare a uniformly dispersed positive electrode slurry. The positive electrode slurry was evenly coated on the surface of the aluminum foil current collector and transferred to a vacuum oven for thorough drying. The obtained positive electrode sheet was rolled and punched to obtain the target positive electrode disc.
[0100] 2. Preparation of negative electrode sheet
[0101] In an Ar atmosphere, element A metal (see Table 1-4 for details), or element A metal and other alloy component powders are placed in a stainless steel crucible and heated until completely melted and fully stirred. After cooling, an inactive layer material containing element A is obtained.
[0102] The inactive layer material containing element A is compounded on the surface of the copper foil by cold pressing or hot pressing to obtain a negative electrode base layer with a layered structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by atomization spraying or sputtering to obtain a negative electrode base layer with a granular structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by extrusion to obtain a negative electrode base layer with a strip structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by atomization spraying or sputtering to obtain a negative electrode base layer with a three-dimensional structure.
[0103] The negative electrode reinforcement film material is compounded on the surface of the negative electrode base layer by cold pressing or hot pressing to obtain the negative electrode plate.
[0104] 3. Preparation of Isolation Membrane
[0105] A polypropylene porous polymer film is used as the separator.
[0106] 4. Preparation of Electrolyte
[0107] Under an Ar atmosphere, a fully dried fluorine-containing salt (see Table 1-4 for details) or a non-fluorine-containing salt (lithium nitrate) is dissolved in an organic solvent of ethylene glycol dipropyl ether, and the mixture is stirred thoroughly to prepare an electrolyte.
[0108] 5. Preparation of Button Cells
[0109] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation layer, and the electrolyte is added to assemble the button battery.
[0110] According to the above preparation method, button batteries of Examples 1 to 20 and Comparative Examples 1 to 11 were prepared.
[0111] According to the test results of Examples 1 to 4 and Comparative Examples 1 to 5 in Table 1, when element A is sodium and element B is lithium (Example 1, Na-Li); element A is magnesium and element B is lithium (Example 2, Mg-Li); element A is calcium and element B is lithium (Example 3, Ca-Li); or element A is sodium and element B is calcium (Example 4, Na-Ca) (all satisfying that the redox potential of element B is lower than that of element A), the negative electrode base layer containing element A can effectively inhibit the formation of metal dendrites of element B, and the ion conductivity of the A-based protective film is strong, which can effectively inhibit the occurrence of adverse side reactions in the battery. The secondary battery has good cycle performance (expressed in the number of cycles, <500 is "poor", 500-530 is "medium", and >530 is "excellent") and first cycle coulombic efficiency (expressed in first cycle efficiency). According to the test results of Comparative Example 1 (Li-Na), when the redox reaction potential of element B is higher than that of element A, the structure of the negative electrode base layer containing element A is unstable, and the formation of metal dendrites of element B cannot be effectively suppressed, and the cycle life and first cycle coulombic efficiency of the secondary battery are reduced. According to the test results of Comparative Example 2 (Cu-Li) and Comparative Example 3 (Mg-Zn), when element A is not one of sodium, potassium, rubidium, cesium, magnesium, and calcium, and / or element B is not one of lithium, sodium, potassium, magnesium, and calcium, the negative electrode base layer containing element A cannot suppress the generation of metal dendrites of element B, and the A-based protective film cannot suppress the formation of metal dendrites of element B and the occurrence of adverse side reactions, and the cycle life and first cycle coulombic efficiency of the secondary battery are reduced. According to the test results of Comparative Example 4 (Li-Li) and Comparative Example 5 (Na-Na), when element A and element B are the same element, the A-based protective film cannot effectively suppress the generation of dendrites, which also leads to a decrease in the cycle life and first cycle coulombic efficiency of the secondary battery.
[0112] Table 1
[0113] According to the test results of Examples 5 to 12 and Comparative Examples 6 to 7 in Table 2, when the electrolyte contains fluorine-containing anions, the main component of the A-based protective film includes metal fluoride, which has high ion conductivity and structural stability, can effectively inhibit the formation of B element metal dendrites, inhibit the occurrence of adverse side reactions in the battery, and improve the coulombic efficiency and cycle performance of the battery. According to the test results of Comparative Examples 6 to 7, when the electrolyte does not contain fluorine-containing anions, the ion conductivity of the negative electrode protective film is weak, it is difficult to inhibit the adverse side reactions between the negative electrode base layer and the electrolyte and the formation of B element metal dendrites, and the coulombic efficiency and cycle performance of the battery are poor.
[0114] Figure 2 is a SEM image of the negative electrode base layer after the battery cycle is completed in Example 7 of the present application. As shown in Figure 2, when the electrolyte contains fluoride-containing anions, there are almost no dendrites in the negative electrode base layer.
[0115] Figure 3 is a SEM image of the negative electrode base layer after the battery cycle is completed in Comparative Example 6 of the present application. As shown in Figure 3, when the electrolyte does not contain fluoride-containing anions, a large number of dendrites exist in the negative electrode base layer.
[0116] Table 2
[0117] According to the test results of Examples 13 to 16 and Comparative Examples 8 to 9 in Table 3, when the film-forming reaction time of the A-based protective film is between 0.1 hours and 20 hours, the A-based protective film has a higher ion conductivity, can effectively block the adverse side reactions between the negative electrode base layer and the electrolyte, the battery has a higher coulombic efficiency and cycle stability, and the battery production efficiency is high. According to the test results of Comparative Example 8, when the film-forming time of the A-based protective film is too short, the film-forming effect of the A-based protective film is not ideal, it is difficult to effectively block the adverse side reactions between the negative electrode base layer and the electrolyte, the negative electrode is prone to form B element metal dendrites, and the coulombic efficiency and cycle stability of the battery are poor. According to the test results of Comparative Example 9, when the film-forming reaction time of the A-based protective film is too long, although the electrochemical performance of the battery is not significantly affected, the production efficiency of the battery is low, resulting in high production costs of the battery.
[0118] Table 3
[0119] According to the test results of Examples 17 to 20 and Comparative Examples 10 to 11 in Table 4, when the concentration of the electrolyte is in the range of 0.5 mol / L to 7 mol / L, the electrolyte has good A-based protective film forming performance, the electrolyte has high ionic conductivity and wettability, the polarization during the battery cycle is small, the formation of B element metal dendrites can be effectively suppressed, the adverse side reactions are suppressed, and the battery has high coulombic efficiency and cycle performance. According to the test results of Comparative Example 10, when the electrolyte concentration is too small, the film-forming performance of the electrolyte is weak, the A-based protective film is difficult to effectively suppress the adverse side reactions between the negative electrode base layer and the electrolyte, the negative electrode forms B element metal dendrites, the active material and the electrolyte are consumed quickly, and the coulombic efficiency and cycle performance of the battery are poor. According to the test results of Comparative Example 11, when the concentration of the electrolyte is too large, the viscosity of the electrolyte is high, the ionic conductivity is low, the polarization during the battery cycle is large, the negative electrode is prone to dendrite formation, and the coulombic efficiency and cycle performance of the battery are poor.
[0120] Table 4
[0121] Test Method
[0122] 1. Cyclic performance test
[0123] At 25°C, the secondary batteries prepared in the Examples and Comparative Examples were subjected to full charge and discharge cycle testing at a 0.5C rate. The number of cycles at which the battery capacity reached 80% or less of its initial capacity was recorded (recorded as the nth cycle). A higher n indicates better cycling performance. A cycle greater than 530 cycles indicates excellent cycling performance, a cycle between 500 and 530 cycles indicates fair cycling performance, and a cycle less than 500 cycles indicates poor cycling performance.
Claims
1. An A-based protective film for a metal negative electrode of a secondary battery, wherein the A-based protective film conducts the B element as an active material in the electrolyte of the secondary battery; in, The metal negative electrode includes a negative electrode base layer, the negative electrode base layer includes at least one inactive layer containing an element A, and the element A is at least one of sodium, potassium, rubidium, cesium, magnesium and calcium, The B element is different from the A element and is at least one of lithium, sodium, potassium, magnesium and calcium, and the redox reaction potential of the B element is lower than that of the A element. Wherein, the A-based protective film contains fluoride of element A and is located on at least a portion of the surface of the negative electrode base layer of the metal negative electrode.
2. The A-based protective film according to claim 1, characterized in that: The A-based protective film includes a solid electrolyte interface (SEI) film artificially constructed on the surface of the negative electrode substrate layer, or an SEI film formed in situ by the electrolyte and the negative electrode substrate layer, or a combination thereof; preferably, the in situ formed SEI film is formed by a self-limiting reaction occurring between the negative electrode substrate layer and the electrolyte.
3. The A-based protective film according to claim 1, characterized in that: The A-based protective film further contains a fluoride of the B element.
4. The A-based protective film according to claim 2, characterized in that: The electrolyte contains fluorine-containing anions. Preferably, the fluorine-containing anions contained in the electrolyte are at least one selected from bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate and difluorophosphate.
5. The A-based protective film according to claim 2, characterized in that: The solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound and a ketal compound.
6. The A-based protective film according to claim 2, characterized in that: The concentration of the electrolyte is between 0.5 mol / L and 7 mol / L.
7. A secondary battery comprising a positive electrode sheet, an electrolyte, a metal negative electrode sheet and the A-based protective film according to any one of claims 1 to 6.
8. The secondary battery according to claim 7, characterized in that: Also included is a negative electrode enhancement film located on at least a portion of the surface of the A-based protective film.
9. The secondary battery according to claim 7, characterized in that: The element A is combined with the element B in any of the following ways: a combination of magnesium and sodium, a combination of magnesium and lithium, a combination of magnesium and potassium, a combination of magnesium and calcium, a combination of sodium and potassium, a combination of sodium and lithium, a combination of sodium and calcium, a combination of calcium and potassium, a combination of calcium and lithium, or a combination of potassium and lithium.
10. An electrical device comprising the secondary battery according to any one of claims 7 to 9.
Citation Information
Patent Citations
An alkali metal-based composite negative electrode and application thereof
CN109037627A
Lithium metal battery, negative electrode, electrolyte and preparation of negative electrode
CN110880618A
Negative electrode current collector as well as preparation method and application thereof
CN112103512A
Silicon-carbon composite material and preparation method thereof, negative electrode and battery
CN112750993A
Negative electrode material and preparation method and application thereof
CN114050263A
Cited By
Secondary battery, method for preparing negative electrode sheet, battery module, battery pack, and electric device
WO2026174998A1