Method for producing a seal on a layer or coating of an electrochemical cell, and electrochemical cell comprising a seal

The use of shear-thinning and thixotropic sealants with controlled rheological properties and silica additives in stencil printing addresses air bubble and accuracy issues, enabling high-height electrochemical cell seals with improved design freedom and reduced cycle times.

WO2024213598A1PCT designated stage expired Publication Date: 2024-10-17ROBERT BOSCH GMBH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/059764
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-11
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Stencil printing for electrochemical cell seals faces challenges with air bubbles and dimensional inaccuracies due to thick stencil usage, leading to incomplete or defective prints, especially when achieving high layer heights required for complex designs.

Method used

Employing a sealant or adhesive with specific rheological properties such as shear-thinning behavior, thixotropy, and surface tension within defined ranges, along with the addition of silica, to optimize stencil printing processes, ensuring complete filling without air bubbles and maintaining dimensional accuracy.

Benefits of technology

The method allows for the production of seals with heights up to 1500 μm, enhancing design freedom and tolerance compensation while reducing cycle times and costs by minimizing air bubbles and ensuring high dimensional accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024059764_17102024_PF_FP_ABST
    Figure EP2024059764_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a seal on a layer or coating (1) of an electrochemical cell by means of stencil printing, wherein a sealant and / or adhesive (2) having a structurally viscous and / or thixotropic behaviour is used as the printing material. According to the invention, a sealant and / or adhesive (2) is used having a) a static viscosity at the shear rate of 100 s-1 of 5 to 20 Pa*s, preferably 10 to 15 Pa*s, more preferably 12.5 Pa*s, b) a thixotropy index (TI) of 50 to 250 Pa*s / s, preferably 120 to 180 Pa*s / s, more preferably 150 Pa*s / s, and c) a surface tension of 15 to 35 mN / m, preferably up to 30 mN / m, more preferably 25 mN / m. The invention also relates to an electrochemical cell comprising a seal produced according to the method.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Description

[0002] Title:

[0003] Method for producing a seal on a layer or sheet of an electrochemical cell, electrochemical cell with a seal

[0004] The invention relates to a method for producing a seal on a layer or ply of an electrochemical cell, in particular a fuel cell, electrolysis cell, or battery cell. The layer or ply can be, for example, a monopolar or bipolar plate, a separator plate, and / or a membrane-electrode assembly.

[0005] Furthermore, the invention relates to an electrochemical cell, in particular a fuel, electrolysis or battery cell, with a seal which has been produced by a method according to the invention.

[0006] State of the art

[0007] Electrochemical cells, such as fuel cells, electrolysis cells, or battery cells, have a multi-layered structure. This structure requires intermediate seals to separate the media supplied to a cell during operation. To form the seals, a sealant and / or adhesive is applied to a layer or ply of the cell. Dispensing or printing processes are particularly used for this purpose.

[0008] The mass production of electrochemical cells requires high processing speed, meaning short cycle times, as well as high process stability. Stencil printing, in particular, meets these requirements. The printing process for stencil printing is essentially divided into the following three sub-processes: 1. Application of the sealant and / or adhesive to the stencil, which has previously been placed on the layer or ply to be printed.

[0009] 2. Filling the stencil recess or recesses with the sealant and / or adhesive in a squeegee process,

[0010] 3. Release the sealant and / or adhesive from the stencil recess(es) by separating the stencil from the layer or ply.

[0011] The stencil thickness determines the layer height of the applied structure, with typical layer heights ranging from 300 pm to 500 pm. However, for seals in electrochemical cells, layer heights of up to 1500 pm are required to achieve tolerance compensation and allow for maximum freedom in the design of the applied structures. Depending on the specific sealing concept, the applied structures can be large and / or complex.

[0012] To achieve the layer heights required for electrochemical cell seals during stencil printing, thicker stencils must be used. However, this increases the risk of air bubbles being incorporated during the squeegee process for filling the stencil recess(es) with the applied sealant and / or adhesive, which subsequently lead to defects. This is because the volume of the stencil recess(es) to be filled with the sealant and / or adhesive increases with the stencil thickness.

[0013] This problem is explained below with reference to Figures 1a) and 1b). These show a stencil 3 lying on a layer or ply 1 with a recess 5, which is filled with a sealant and / or adhesive 2 using a squeegee 6. For this purpose, the squeegee 6 is pulled over the surface 4 of the stencil 3 facing away from the layer or ply 1. In the squeegee direction (see arrow) towards the end of the recess 5, not all of the air can be displaced from the recess 5, so that an air bubble 8 forms in the recess 5, which prevents the recess 5 from being completely filled with the sealant and / or adhesive 2. In this case, the printed image is incomplete or has defects. The risk of an enclosed air bubble 8 increases with the thickness d of the stencil 3. Another problem, which can also lead to the formation of bubbles, is described below with reference to Figures 2a) to 2e).It occurs when the sealant and / or adhesive 2 is released from the stencil 3 or when the stencil 3 is separated from the layer or ply 1 (Figure 2b)). This is because part of the sealant and / or adhesive 2 can then adhere to the underside of the stencil 3 and form threads 10 (Figure 2c)). This applies in particular if the stencil 3 has webs 9 for stabilization and / or for connecting several stencil parts. The threads 10, also called filaments, are pulled or stretched when the stencil 3 is lifted until they tear or detach from the stencil 3 (Figure 2d)). When the threads 10 subsequently collapse, air bubbles 8 can then form (Figure 2e).

[0014] Depending on the rheology of the sealant and / or adhesive, another undesirable effect may occur during release. This is illustrated as an example in Figure 3. Here, when the sealant and / or adhesive 2 is released, it does not adhere to the stencil 3, but rather flows (spreads or slumps). The result is that the printed structure is not dimensionally accurate and lacks clear contours.

[0015] The present invention is concerned with the object of minimizing the problems described above which occur during the production of a seal by means of stencil printing, so that a higher dimensional accuracy and a print image which is as free from errors as possible are achieved.

[0016] To achieve this objective, the method having the features of claim 1 is proposed. Advantageous developments of the invention are set forth in the subclaims. Furthermore, an electrochemical cell with a seal is specified.

[0017] Disclosure of the invention

[0018] A method is proposed for producing a seal on a layer or sheet of an electrochemical cell by means of stencil printing, wherein a sealant and / or adhesive with pseudoplastic and / or thixotropic behavior is used as the printing material. According to the invention, a sealant and / or adhesive with a) a steady-state viscosity at a shear rate of 100 s 1from 5 to 20 Pa*s, preferably from 10 to 15 Pa*s, further preferably from 12.5 Pa*s, b) a thixotropy index (TI) of 50 to 250 Pa*s / s, preferably from 120 to 180 Pa*s / s, further preferably from 150 Pa*s / s, and c) a surface tension of 15 to 35 mN / m, preferably 20 to 30 mN / m, further preferably from 25 N / m.

[0019] For a printing material with pseudoplastic behavior, the shear stress increases disproportionately with increasing shear rate. This means that the viscosity decreases with increasing shear rate. The shear rates introduced into the printing material by the squeegee movement, which usually exceed 100 s 1 therefore lead to a reduction in viscosity, which proves to be an advantage when filling the stencil recess(es) with the sealant and / or adhesive.

[0020] After the sealant and / or adhesive has been released, very low shear rates of less than 0.1 s 1 At the same time, a higher viscosity is required to prevent the sealant and / or adhesive from flowing. After the doctor blade process, the viscosity should therefore recover as quickly as possible. The rate of viscosity recovery, or the thixotropic behavior of the sealant and / or adhesive, plays a significant role in this.

[0021] The surface tension of the sealant and / or adhesive, in turn, influences the formation of threads and, if necessary, bubbles when separating the stencil.

[0022] The three rheological properties mentioned above, in combination, are therefore crucial for the stencil printing process and for achieving the required layer heights. By using a sealant and / or adhesive as a printing material whose values ​​for these three rheological properties lie within the specified ranges, the printability of the printing material can be improved, on the one hand, and the dimensional accuracy of the seal produced from the printing material can be increased, on the other hand. In addition, a further positive effect is achieved, which is evident in the fact that the printing material is less sensitive to increasing squeegee speed. Tests have shown that, for example, the squeegee speed can be increased from 40 mm / s to 160 mm / s without compromising the other advantages regarding the printability of the printing material and the dimensional accuracy of the printed structure.This means that cycle times can be reduced, which in turn reduces costs.

[0023] To determine the steady-state viscosity at a shear rate of 100 s 1 Reference is made to DIN EN ISO 3219-1 (edition 2021 -08) and DIN EN ISO 3219-2 (edition 2021 -08). According to the standards, the so-called rotational rheometer method can be used. In this method, the steady-state viscosity is determined at a shear rate of 100 s 1 measured under homogeneous shear flow. A plate-on-plate or a cone-on-plate measurement geometry can be used.

[0024] Thixotropy is defined in DIN 1342-3:2003-11. Furthermore, reference is made to the technical report DIN / TR 91143-2 "Rheological Test Methods" - Part 2: "Thixotropy - Determination of Time-Dependent Structural Change - Fundamentals and Interlaboratory Comparison"; text in German and English, edition 2022-07. To determine the thixotropy index (TI), which describes the thixotropic behavior of a material, the standards DIN EN ISO 3219-1 (edition 2021-08) and DIN EN ISO 3219-2 (edition 2021-08) can also be used, particularly with regard to the procedure and measuring instruments. This means that the rotational rheometer method can also be used here. The thixotropy index (TI) can then be calculated from the measured values ​​using the following formula:

[0025] A concrete test setup and procedure for determining the TI is described in more detail below using the attached Figure 4.

[0026] The following standards can be used to determine the surface tension: DIN EN 14370:2004, Edition 2004-11 - Surface-active agents - Determination of surface tension and / or

[0027] DIN EN ISO 19403-3:2020, edition 2020-04 - Paints and varnishes - Wettability - Part 3: Determination of surface tension of liquids by the hanging drop method (ISO 19403-3:2017).

[0028] Preferably, a UV- and / or thermally curing sealant and / or adhesive is used. Such sealants and / or adhesives have the advantage of curing very quickly when exposed to UV light and / or heat, which in turn has a beneficial effect on reduced cycle times.

[0029] Furthermore, it is preferred to use a sealant and / or adhesive based on epoxy, silicone, and / or acrylate, for example, based on epoxy-acrylate. Such sealants and / or adhesives inherently exhibit favorable rheological properties, particularly with regard to the required surface tension. The use of an appropriate sealant and / or adhesive therefore contributes to achieving the required surface tension.

[0030] In a further development of the invention, it is proposed that a sealant and / or adhesive be used that contains silica, in particular highly dispersed silica. Alternatively or additionally, silica, preferably highly dispersed silica, can be added to the sealant and / or adhesive used. The silica, in particular the highly dispersed silica, influences the pseudoplastic and / or thixotropic behavior of the sealant and / or adhesive, so that the steady-state viscosity at a shear rate of 100 s 1and the thixotropy index can be specifically controlled. The silica has no significant influence on the surface tension. The basis of the sealant and / or adhesive plays a primary role in the surface tension, with this preferably being an epoxy, silicone and / or acrylate basis. Specific additives, such as silicone-containing surface additives, can be added to specifically control the surface tension. The proposed process enables the production of seals with heights over 300 pm, preferably over 500 pm. With the height of the seal, the design freedom as well as the possibility of tolerance compensation across the seal increases. In the proposed process, the sealant and / or adhesive is therefore preferably applied to the layer or ply by means of stencil printing in a layer thickness of 300 to 1500 pm, preferably 500 to 1500 pm.

[0031] Furthermore, the following steps are preferably carried out to apply the sealant and / or adhesive to the layer or ply:

[0032] Placing a stencil on the layer or layer,

[0033] Applying the sealant and / or adhesive to the surface of the stencil facing away from the layer or ply,

[0034] Filling at least one recess of the stencil with the sealant and / or adhesive using a squeegee which is pulled over the surface of the stencil, whereby any air present in the recess is displaced by the sealant and / or adhesive.

[0035] The rheological properties of the sealant and / or adhesive used ensure that at least one recess in the stencil is completely filled with the sealant and / or adhesive. This means that no air bubbles remain, which could lead to defects after the sealant and / or adhesive is released. Furthermore, the sealant and / or adhesive is prevented from flowing. Due to the optimized rheological properties of the sealant and / or adhesive, the squeegee speed can also be increased, thus reducing cycle times.

[0036] Preferably, the sealant and / or adhesive is applied to a monopolar or bipolar plate, a separator plate, and / or a membrane-electrode assembly of the electrochemical cell. The seal made from the sealant and / or adhesive then serves to separate the media within the electrochemical cell and / or seal it off from the outside.

[0037] Furthermore, an electrochemical cell is proposed which comprises at least one layer or ply with a seal produced by a method according to the invention and having a height of 300 to 1500 pm, preferably 500 to 1500 pm. Since the seal is produced by the method according to the invention, it exhibits high dimensional accuracy despite its considerable height.

[0038] The layer or ply to which the sealant and / or adhesive is applied to create a seal can, in particular, be a monopolar or bipolar plate, a separator plate, and / or a membrane-electrode assembly of the electrochemical cell. In this case, the seal can be used to separate media within the electrochemical cell or to seal the electrochemical cell from the outside.

[0039] The invention and its advantages are explained in more detail below with reference to the accompanying drawings. These show:

[0040] Fig. 1 a) and b) each show a longitudinal section through a layer or layer of an electrochemical cell with a stencil applied during the doctor blade process,

[0041] Fig. 2 a) to e) each show a longitudinal section through a layer or ply of an electrochemical cell during printing by means of a stencil printing process,

[0042] Fig. 3 shows a longitudinal section through a layer or layer of an electrochemical cell during printing by means of a stencil printing process and

[0043] Fig. 4 is a diagram showing a measurement profile for determining the thixotropy index (TI).

[0044] Detailed description of the drawings

[0045] The problems frequently encountered in the production of a seal using stencil printing have already been described at the beginning with reference to Figures 1 a) and b), Figures 2a) to e), and Figure 3, so reference is made to this part of the description. Therefore, the invention and its advantages are explained in more detail below with reference to Figure 4.

[0046] The diagram in Figure 4 shows an example of a measurement profile for determining the thixotropy index (TI) of a sealant and / or adhesive sample exhibiting pseudoplastic or thixotropic behavior. The rotational rheometer method was used to determine the thixotropic behavior, using a plate-on-plate measurement geometry. The plate diameter was 25 mm, and the plate spacing was 0.4 mm.

[0047] To investigate the time-dependent development of the sample structure, two measurement sections Ai and A2 were combined in series. The first measurement section Ai was used to simulate the shear during the doctor blade process, with a high shear rate of 200 s 1 for at least 10 to 20 seconds. The goal was to destroy the sample's internal structure as much as possible. The second measurement section, A2, was intended to simulate the recovery phase and thus the structural recovery after the doctor blade process. For this purpose, a low shear rate of 0.1 s 1for at least 180 seconds. In the meantime, the viscosity rj of the sample was measured at a first time ti , which coincides with the end of the first measurement section Ai, so that the viscosity qi measured at time ti represents the viscosity of the sample after the high shear stress. A further measurement was carried out at time t2, 10 seconds after time ti, i.e. during the recovery phase. The viscosity rp measured at time t2, or the viscosity increase after 10 seconds of recovery phase (this period is designated as t?i in the diagram in Figure 4), is characteristic of the thixotropic behavior of the sample. From the measured values ​​qi and rp, it was then possible to use the equation the thixotropy index (TI) can be determined.

Claims

Claims 1 . Method for producing a seal on a layer or ply (1) of an electrochemical cell by means of stencil printing, wherein a sealant and / or adhesive (2) with a structurally viscous and / or thixotropic behavior is used as the printing material, characterized in that a sealant and / or adhesive (2) with a) a stationary viscosity at the shear rate 100 s 1 from 5 to 20 Pa*s, preferably from 10 to 15 Pa*s, further preferably from 12.5 Pa*s, b) a thixotropy index (TI) of from 50 to 250 Pa*s / s, preferably from 120 to 180 Pa*s / s, further preferably from 150 Pa*s / s, and c) a surface tension of from 15 to 35 mN / m, preferably from 20 to 30 mN / m, further preferably 25 mN / m, is used.

2. Method according to claim 1, characterized in that a UV and / or thermally curing sealant and / or adhesive (2) is used.

3. Method according to claim 1 or 2, characterized in that a sealant and / or adhesive (2) based on epoxy, silicone and / or acrylate, for example based on epoxy-acrylate, is used.

4. Method according to one of the preceding claims, characterized in that silica, preferably highly dispersed silica, is added to the sealant and / or adhesive (2).

5. Method according to one of the preceding claims, characterized in that the sealant and / or adhesive (2) is applied to the layer or ply (1) by means of stencil printing in a layer thickness of 300 to 1500 pm, preferably of 500 to 1500 pm.

6. Method according to one of the preceding claims, characterized in that the following steps are carried out to apply the sealant and / or adhesive (2) to the layer or ply (1): Placing a stencil (3) on the layer or ply (1), applying the sealant and / or adhesive (2) to the surface (4) of the stencil (3) facing away from the layer or ply (1), Filling at least one recess (5) of the stencil (3) with the sealant and / or adhesive (2) with the aid of a squeegee (6) which is drawn over the surface (4) of the stencil (3) for this purpose, wherein air (7) present in the recess (5) is displaced by the sealant and / or adhesive (2).

7. Method according to one of the preceding claims, characterized in that the sealing and / or adhesive (2) is applied by means of stencil printing to a mono- or bipolar plate, a separator plate and / or a membrane-electrode arrangement of the electrochemical cell.

8. Electrochemical cell, comprising at least one layer or ply (1) with a seal which has been produced by a method according to one of the preceding claims and has a height of 300 to 1500 pm, preferably of 500 to 1500 pm.

9. Electrochemical cell according to claim 8, characterized in that the layer or layer (1) is a mono- or bipolar plate, a separator plate and / or a membrane-electrode arrangement of the electrochemical cell.

Citation Information

Patent Citations

  • Method for manufacturing substrate-integrated gasket

    EP3306723A1

  • Screen printing method

    JP2004167709A

  • Sealing structure of fuel cell and process for molding rubber packing

    US20060099330A1