Coating film evaluation method
The coating film evaluation method uses Fourier transform infrared spectroscopy and surface roughness measurements to differentiate between deterioration mechanisms in titanium dioxide-containing coatings, addressing the challenge of evaluating similarity in deterioration behavior and ensuring accurate weathering resistance predictions.
Patent Information
- Application Number
- PCT/JP2023/014839
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
Existing methods struggle to accurately evaluate the similarity in deterioration behavior of titanium dioxide-containing coating films exposed to different conditions, as the deterioration mechanisms overlap, making it difficult to quantify the progress of molecular chain scission due to photooxidation, photolysis, and hydrolysis versus resin decomposition caused by photocatalytic action of titanium dioxide, and the reproducibility of accelerated weathering tests is uncertain.
A coating film evaluation method involving Fourier transform infrared spectroscopy to measure light absorption by methylene groups and surface roughness, allowing for the comparison of deterioration behavior across different conditions, and determining the similarity in deterioration mechanisms by calculating specific indices and surface roughness parameters.
Enables accurate evaluation of the similarity in deterioration behavior and identifies conditions that reproduce outdoor environmental deterioration effectively, improving the accuracy of weathering resistance predictions and material lifespan predictions.
Smart Images

Figure JP2023014839_17102024_PF_FP_ABST
Abstract
Description
Coating evaluation method
[0001] The present invention relates to a coating film evaluation method.
[0002] Titanium dioxide-containing coatings can become worn or chalky when exposed to ultraviolet light or water. This can be broadly classified into two degradation mechanisms: One is molecular chain scission of the coating resin due to photooxidation, photodecomposition, or hydrolysis.
[0003] For example, in acrylic polyurethanes, which are also used in paints for steel structures, photo-oxidation occurs at the methylene group at the α-position of the urethane bond, as shown in the following chemical reaction formula, which leads to hydrolysis of the oxide produced by the cage effect and β-cleavage, leading to molecular chain scission (Non-Patent Document 1). As this molecular chain scission progresses, the low-molecular-weight resin is lost from the surface layer, causing overall wear of the paint film.
[0004]
[0005] Another degradation mechanism is specific to coatings containing titanium dioxide, namely, resin decomposition due to the photocatalytic action of titanium dioxide. Titanium dioxide has excellent UV-shielding and coloring properties, but when exposed to UV rays in an environment where water and oxygen coexist, it decomposes water to generate hydroxyl radicals, which then cause resin decomposition (Non-Patent Document 2).
[0006] For example, when a coating film 202 containing titanium dioxide particles 201 shown in FIG. 2(a) is exposed to ultraviolet light, the coating film 202 around the particles 201 is decomposed, and voids 203 are formed around the particles 201, as shown in FIG. 2(b).
[0007] The balance between these two degradation mechanisms changes depending on the conditions under which titanium dioxide-containing coatings are degraded. However, because the molecular structures and degradation products of both degradation mechanisms overlap, it is difficult to directly quantify the progress of each degradation mechanism through component analysis of degraded coatings.
[0008] G. Wypych et al., "Handbook of Material Weathering 5th, Polyurethanes", Chem Tec Publishing, pp 473-480, 2013.G. Wypych et al., "Handbook of Material Weathering 5th, Pigments", Chem Tec Publishing, pp 552-562, 2013.
[0009] As mentioned above, existing evaluation technologies (measurement methods) cannot assess whether the deterioration states (deterioration behavior) of titanium dioxide-containing coatings deteriorated under different conditions are similar. For example, if the amount of wear differs between coatings deteriorated outdoors at different locations for the same period, it is difficult to determine whether the differences in deterioration behavior are due to a simple difference in the rate of deterioration, or whether the difference in deterioration behavior is due to a difference in the balance between "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" and "resin decomposition due to the photocatalytic action of titanium dioxide."
[0010] Furthermore, when evaluating the weather resistance of titanium dioxide-containing coatings using accelerated weathering tests, it is also difficult to verify whether the accelerated weathering tests adequately reproduce the deterioration that occurs in actual outdoor environments. When using the results of accelerated weathering tests to predict the lifespan of coatings intended for use in outdoor environments, the accuracy of the lifespan prediction results is greatly affected by the reproducibility of outdoor deterioration in the accelerated weathering tests. However, the lack of a method to verify the "reproducibility of outdoor deterioration in accelerated weathering tests" is a major problem.
[0011] The present invention has been made to solve the above problems, and its object is to make it possible to evaluate the similarity in the deterioration behavior of titanium dioxide-containing coating films deteriorated under different conditions.
[0012] The coating film evaluation method according to the present invention includes a first step of conducting a test of a plurality of test coating films, each of which is a coating film containing titanium dioxide, for a period of t under a plurality of deterioration tests each of which is different from one another; and a first step of measuring the Fourier transform infrared spectroscopy of the surface of each of the plurality of test coating films to determine the peak λ where absorption due to methylene groups occurs. M cm-1 A is the absorbance of λM (t), and normalization peak λ S cm -1 A is the absorbance of λS (t) was quantified, and the peak λ where absorption due to methylene groups occurs was measured by Fourier transform infrared spectroscopy on the surface of each of the multiple test coating films before the test. M cm -1 A is the absorbance of λM (0), and normalization peak λ S cm -1 A is the absorbance of λS (0), a(t) = {|A λM (t) / A λS (t) |÷| A λM (0) / A λS (0)|×100}; a third step of selecting, for each of a plurality of deterioration tests, from among a plurality of test coating films, a coating film to be evaluated that satisfies 35≦a(t)≦45; a fourth step of measuring the surface roughness of the coating film to be evaluated to obtain a measurement value; and a fifth step of comparing the measurement values of the coating films to be evaluated for each of a plurality of deterioration tests to evaluate the similarity of the deterioration behavior.
[0013] As described above, according to the present invention, the surface roughness of a test coating film is measured when the results of Fourier transform infrared spectroscopy measurement of the surface fall within a set range, making it possible to evaluate the similarity in the deterioration behavior of titanium dioxide-containing coating films deteriorated under different conditions.
[0014] Fig. 1 is a flow chart for explaining a coating film evaluation method according to an embodiment of the present invention, and Fig. 2 is an explanatory diagram for explaining the mechanism of deterioration specific to coating films containing titanium dioxide.
[0015] A coating film evaluation method according to an embodiment of the present invention will be described below with reference to FIG.
[0016] First, in a first step S101, a plurality of test coating films containing titanium dioxide are tested for a period of time t for each of a plurality of deterioration tests each having different conditions.
[0017] Next, in the second step S102, Fourier transform infrared spectroscopy is performed on the surface of each of the multiple test coatings that have been tested. For example, by using "ATR FT-IR" measurement, Fourier transform infrared spectroscopy can be performed on the surface of the test coating. In this measurement, the peak λ where absorption occurs due to methylene groups is measured. M cm -1 A is the absorbance of λM (t), and normalization peak λ S cm -1 A is the absorbance of λS (t) is quantified. From the measurement results, "a(t) = {|A λM (t) / A λS (t) |÷| A λM (0) / A λS (0)|×100}...(1)" is calculated.
[0018] Here, A λM (0) is the peak λ where methylene groups absorb light as measured by Fourier transform infrared spectroscopy on the surface of each of the multiple test coatings before the test. M cm -1 The absorbance of λS (0) is the normalization peak λ in the Fourier transform infrared spectroscopy measurement of the surface of each of the multiple test coatings before the test, which has been measured in advance. S cm -1 is the absorbance.
[0019] Next, in the third step S103, a coating film to be evaluated that satisfies 35≦a(t)≦45 is selected from the plurality of test coating films for each of the plurality of deterioration tests.
[0020] Next, in the fourth step S104, the surface roughness of the coating film to be evaluated is measured to obtain a measured value. The surface roughness of the coating film to be evaluated can be measured, for example, using an atomic force microscope. Alternatively, the surface roughness of the coating film to be evaluated can be measured to obtain the five-point peak height Sp5 and the five-point valley depth Sv5, and the measured value can be calculated by dividing Sp5 by Sv5. The five-point peak height (five-point peak region height) Sp5 and the five-point valley depth (five-point valley region depth) Sv5 are specified in the international standard "ISO 25178 Surface Quality (Surface Roughness Measurement)," which defines a method for evaluating surface roughness. The five-point peak height Sp5 represents the average of the peak region heights from the highest peak to the fifth highest peak in the defined region.
[0021] Next, in a fifth step S105, the measurement values of the evaluation target coating are compared for each of the multiple deterioration tests to evaluate the similarity of the deterioration behavior. In the fifth step S105, the difference between the measurement value of the evaluation target coating in one deterioration test to be compared and the measurement value of the evaluation target coating in the other deterioration test is first calculated. In other words, the measurement value of the evaluation target coating in one deterioration test to be compared is subtracted from the measurement value of the evaluation target coating in the other deterioration test to calculate a difference.
[0022] If the difference (subtracted value) is 0.15 or more, the coating film evaluated in one deterioration test is evaluated as having less resin decomposition due to the photocatalytic action of titanium dioxide than the coating film evaluated in the other deterioration test.
[0023] If the difference is −0.15 or less, the coating film evaluated in one deterioration test is evaluated as having greater resin decomposition due to the photocatalytic action of titanium dioxide than the coating film evaluated in the other deterioration test.
[0024] If the calculated difference is greater than -0.15 and less than 0.15, the coating film to be evaluated in one deterioration test and the coating film to be evaluated in the other deterioration test are evaluated to have the same degree of resin decomposition due to the photocatalytic action of titanium dioxide.
[0025] According to the above-described embodiment, it is possible to evaluate the similarity of deterioration behaviors that cannot be determined by a single index evaluated by a general analysis method.
[0026] For example, when evaluating titanium dioxide-containing coatings exposed outdoors at different locations, differences in the amount of wear alone do not tell us whether the deterioration rate is simply different, or whether the difference in deterioration behavior is due to a difference in the balance between "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" and "resin decomposition due to the photocatalytic action of titanium dioxide."
[0027] However, according to the embodiment, it is possible to evaluate whether there is a difference in the balance between the above two deterioration mechanisms (deterioration tests), and it is possible to know whether the difference in the amount of wear at different points is due to a difference in the deterioration rate or a difference in the deterioration behavior.
[0028] If there is a difference in the balance between the two degradation mechanisms between exposure points, it will be possible to more appropriately evaluate the degradation behavior of the coating by referring to the test results at an exposure point that is closer to the actual usage environment.Also, if there is no significant difference in the balance between the two degradation mechanisms between exposure points, it will be possible to roughly calculate the ratio of the degradation rates between exposure points from the amount of wear and other indicators.
[0029] Furthermore, by preparing titanium dioxide-containing coating films subjected to multiple types of accelerated weathering tests and titanium dioxide-containing coating films deteriorated in outdoor environments and then comparatively evaluating them using the coating evaluation method according to the above-described embodiment, it becomes possible to determine accelerated weathering test conditions that exhibit deterioration behavior most similar to outdoor environmental deterioration and that are highly reproducible to actual environmental deterioration. If an accelerated weathering test that is highly reproducible to actual environmental deterioration can be used, the weathering resistance of titanium dioxide-containing coating films can be more accurately evaluated. As a result, for example, it becomes possible to accurately identify titanium dioxide-containing paints with excellent weathering resistance. Furthermore, it becomes possible to improve the accuracy of material life predictions using weathering test results.
[0030] Consider comparing the deterioration behavior of a titanium dioxide-containing coating film between a first deterioration test (e.g., outdoor exposure test) and a second deterioration test (e.g., accelerated weathering test), each of which is conducted under different conditions. In this case, it is unclear how many hours of exposure time in the second deterioration test (accelerated weathering test) should be used to compare a sample that has been subjected to x hours (e.g., 1 year) in the first deterioration test (outdoor exposure test) in order to appropriately evaluate the difference in deterioration behavior.
[0031] Generally, it is conceivable to compare samples with similar values of a(t) in formula (1) (samples in which methylene groups have been decomposed to the same extent). However, the inventors have demonstrated through experiments that when evaluating differences in the deterioration behavior of titanium dioxide-containing coatings, a(t) is not necessarily any value within the range of 0≦a(t)≦100, but rather that there is an appropriate range of 35≦a(t)≦45. This is because, in order to evaluate the degree of "resin decomposition due to the photocatalytic action of titanium dioxide," it is necessary to use a sample in which void formation due to "resin decomposition due to the photocatalytic action of titanium dioxide" has progressed to an appropriate degree.
[0032] In the early stages of deterioration, titanium dioxide-containing coating films do not form voids due to "resin decomposition due to the photocatalytic action of titanium dioxide," making it difficult to evaluate the progress of "resin decomposition due to the photocatalytic action of titanium dioxide" using surface roughness parameters. For this reason, in the above-described embodiment, a threshold value of a(t)≦45 is set as the degree of deterioration at which the progress of "resin decomposition due to the photocatalytic action of titanium dioxide" can be evaluated using surface roughness parameters. Furthermore, if deterioration progresses too far, it becomes difficult to distinguish between voids formed by "resin decomposition due to the photocatalytic action of titanium dioxide" and unevenness resulting from coating film wear due to "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis." Therefore, a threshold value of 35≦a(t) is set as the degree of deterioration at which the progress of "resin decomposition due to the photocatalytic action of titanium dioxide" can be evaluated using surface roughness parameters.
[0033] Taking these two points into consideration, the condition 35≦a(t)≦45 was experimentally determined by the inventors through analysis of deteriorated coating films as a condition for which the present invention is applicable, and is not something that can be easily deduced.
[0034] Furthermore, the evaluation of the degree of progress of "resin decomposition due to the photocatalytic action of titanium dioxide" by "Sp5(t) / Sv5(t)" using the values of "five-point peak height Sp5(t)" and "five-point valley depth Sv5(t)" is not easily inferred. In titanium dioxide-containing coatings, the entire surface of the coating sample is depleted due to "molecular chain scission caused by photooxidation, photodecomposition, and hydrolysis," and void formation due to "resin decomposition due to the photocatalytic action of titanium dioxide" simultaneously occur. Therefore, there are no surface roughness parameters that correspond to the degree of progress of these two types of deterioration.
[0035] However, through analysis of deteriorated coatings, the inventors discovered for the first time that the value of "Sp5(t) ÷ Sv5(t)", which is the ratio of the "five-point peak height Sp5(t)", which is largely influenced by the wear of the entire surface of the coating sample due to "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis", to the "five-point valley depth Sv5(t)", which is largely influenced by the formation of voids due to "resin decomposition due to the photocatalytic action of titanium dioxide", well reflects the balance between the two types of deterioration.
[0036] The following explanation will be given using the results of an actual experiment.
[0037] [Preparation of Test Pieces] The titanium dioxide-containing paint to be evaluated was applied to N random substrates, followed by drying to prepare test pieces. The titanium dioxide-containing acrylic polyurethane resin paint to be evaluated was applied to 16 plastic substrates, followed by drying to prepare test pieces.
[0038] [Initial Value Measurement] For a test piece in an undegraded state (test time t=0), ATR FT-IR measurement is performed on the surface of the test piece, and surface roughness measurement is also performed to obtain initial values.
[0039] [Preparation of Degradation Test Specimens] Different degradation tests X (X=A, B, C, ...) for which degradation behavior is to be compared are determined. One or more test specimens having the above-described configuration are provided for each degradation test.
[0040] The following four tests were carried out as different degradation tests for comparing degradation behavior.
[0041] Deterioration test A: Outdoor exposure test This was carried out on an exposure stand facing south at an angle of 45 degrees on the coast of Miyakojima.
[0042] Deterioration test B: Outdoor exposure test This was carried out on an exposure stand facing south at an angle of 45 degrees on the coast of Miyakojima.
[0043] Deterioration test C: Outdoor exposure test This was carried out in Choshi, using an exposure rack facing south at an angle of 45 degrees.
[0044] Degradation Test D: Accelerated Weathering Test Tests were conducted based on JIS K5600-7-7A using an accelerated weathering tester SX75 manufactured by Suga Test Instruments Co., Ltd. The light source was a xenon light source. The test cycle consisted of a repeated cycle of 18 minutes of step 1 (water spray + light irradiation) and 102 minutes of step 2 (light irradiation only). The conditions for step 1 were a light irradiation intensity of 60 W / m2 (at 300-400 nm) and a chamber temperature of 38°C. The conditions for step 2 were a light irradiation intensity of 60 W / m2 (at 300-400 nm), a chamber temperature of 38°C, a black panel temperature of 63°C, and a chamber humidity of 50%. Five test specimens were used for each degradation test, and for degradation tests A, B, and C, samples were collected after 6, 9, 12, 18, and 24 months. For degradation test D, the test specimens were collected after 500, 1000, 1500, 2000, and 2500 hours.
[0045] For each degradation test, the test specimens are collected at least once (after time t1 has elapsed since the start of the test, after time t2 has elapsed, etc.) and subjected to "ATR FT-IR measurement" and "surface roughness measurement." The test specimens used for the measurement can be reused for the degradation test. Alternatively, the test specimens used for the measurement can be left as they were. ATR FT-IR measurement of the test specimen surfaces was performed using a PerkinElmer Frontier FT-IR spectrometer, using the reflection ATR method with a one-reflection germanium ATR plate. Here, measurements were performed with N = 3 test specimens for each test.
[0046] In each IR spectrum acquired by ATR FT-IR measurement, the peak λ where absorption occurs due to the methylene group M cm -1 A is the absorbance of λM (t) and the normalization peak λ S cm -1 A is the absorbance of λS (t) is quantified, and "a(t) = {|A λM (t) / A λS(t) |÷| A λM (0) / A λS (0)|×100}...(1)
[0047] In each measured IR spectrum, the peak at 2932 cm where absorption occurs due to the methylene group -1 The absorbance of A2932 (t) and the normalization peak 1384 cm -1 The absorbance A1384(t) was quantified and a(t) was calculated. The average values of N=3 for each test piece are shown in Table 1 below.
[0048] Next, for samples where 35≦a(t)≦45, the surface roughness was measured using a roughness measurement method such as an atomic force microscope (AFM) or laser microscope. For samples where 35≦a(t)≦45, the surface shape was measured using an atomic force microscope (AFM) with a cantilever of 10 nm and a field of view of 10 μm. As comparative examples, measurements were also performed for a(t)<35 and 45<a(t). For data where 35≦a(t)≦45 was satisfied, the a(t) value in Table 1 is underlined.
[0049] Next, for the data obtained by the measurement, the measured values of "five-point peak height Sp5(t)" and "five-point valley depth Sv5(t)" are obtained, and b(X) = {Sp5(t) ÷ Sv5(t)} is calculated. The average values for N = 3, excluding the maximum and minimum values, of the measurements of each test piece (N = 5) are shown in Table 1 below.
[0050] [Comparing the similarity of deterioration behavior for each deterioration test] The similarity of the deterioration behavior of the coating film is evaluated by comparing the b(X) values for each deterioration test. The similarity of the b(X) values indicates a close balance between "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" and "resin decomposition due to the photocatalytic action of titanium dioxide," and indicates similar deterioration behavior.
[0051] More specifically, the reference degradation test is designated Y, the degradation test to be compared is designated Z, and the following judgment is made, where "Δb(Z) = {b(Z) - b(Y)}". First, if Δb(Z) ≧ 0.15, degradation test Z exhibits less "resin decomposition due to the photocatalytic action of titanium dioxide" compared to degradation test Y. Furthermore, if Δb(Z) ≦ -0.15, degradation test Z exhibits more "resin decomposition due to the photocatalytic action of titanium dioxide" compared to degradation test Y. Furthermore, if -0.15 < Δb(Z) < 0.15, degradation test Z and degradation test Y exhibit the same degree of "resin decomposition due to the photocatalytic action of titanium dioxide".
[0052] The b(X) values for each degradation test were 0.52 (12M) and 0.40 (18M) for Degradation Test A (exposed to the coast of Miyakojima), 1.0 (12M) and 0.92 (18M) for Degradation Test B (exposed to the inland of Miyakojima), 1.0 (18M) and 0.89 (24M) for Degradation Test C (exposed to Choshi), and 1.4 (2000h) and 1.5 (2500h) for Degradation Test D (accelerated weathering test).
[0053] Comparing these, the values of Deterioration Test B (exposed inland on Miyako Island) and Deterioration Test C (exposed in Choshi) are close, and it can be determined that Deterioration Test B and Deterioration Test C have a similar balance between "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" and "resin decomposition due to the photocatalytic action of titanium dioxide," and therefore have similar degradation behavior.
[0054] It is thought that the rate at which "resin decomposition due to the photocatalytic action of titanium dioxide" progresses varies greatly depending on the wetness of the sample surface, and because both the Miyakojima inland exposure tests and the Choshi exposure tests were carried out at locations several kilometers from the coast, the wetness of the sample surface was similar, and it is thought that the balance between "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" and "resin decomposition due to the photocatalytic action of titanium dioxide" was similar, and therefore the evaluation results using b(X) can be said to be valid.
[0055] Next, if the reference deterioration test is B and the comparison deterioration test is Z, where "Δb(Z) = {b(Z) - b(B)}," then for deterioration test A, Δb(A) ≦ -0.15, and therefore it can be determined that deterioration test A (Miyakojima coastal exposure test) exhibited more "resin decomposition due to the photocatalytic action of titanium dioxide" than deterioration test B (Miyakojima). Since the temperature, humidity, precipitation, and other conditions were the same in deterioration test A (Miyakojima coastal exposure) and deterioration test B (Miyakojima inland exposure), it is thought that "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" would proceed in roughly the same way. Therefore, deterioration test A (Miyakojima coastal exposure), which is closer to the coast and more likely to keep the sample surface wet due to deliquescence of salts adhering to the sample surface, is thought to have exhibited more "resin decomposition due to the photocatalytic action of titanium dioxide," and the determination results can be said to be reasonable.
[0056] For Degradation Test C, -0.15<Δb(C)<0.15, so it can be determined that Degradation Test B (Miyakojima inland exposure) and Degradation Test C (Choshi exposure) have a similar balance between "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" and "resin decomposition due to the photocatalytic action of titanium dioxide." Both the Miyakojima inland exposure and Choshi exposure tests were conducted at locations several kilometers from the coast, so the wetness of the sample surfaces was similar, and it is thought that the progress of "resin decomposition due to the photocatalytic action of titanium dioxide" relative to "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" would be about the same, so the determination results can be said to be reasonable.
[0057] For Degradation Test D, Δb(D) is 0.15 or greater, so it can be determined that there was less "resin decomposition due to the photocatalytic action of titanium dioxide" in Degradation Test D (accelerated weathering test) than in Degradation Test B (exposure to inland Miyakojima). Considering that the water spray time in the accelerated weathering test was only 18 minutes out of a 120-minute cycle, it is considered a reasonable determination result that there was less "resin decomposition due to the photocatalytic action of titanium dioxide," which requires water.
[0058]
[0059] In Table 1, *1 indicates a result of surface roughness measurement carried out as a comparative example, even though a(t) is out of range. *2 indicates a process that is not required in the coating film evaluation method according to the embodiment, but shows the value of Sv5 as a comparative example. *3 indicates a process that is not required in the coating film evaluation method according to the embodiment, but was obtained as verification data.
[0060] In the above-described embodiment, an acrylic polyurethane paint was used as a sample of a titanium dioxide-containing coating film, but this is not limiting. The coating film evaluation method according to the embodiment can be applied to any coating material whose main degradation mechanisms are "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis" and "resin decomposition due to the photocatalytic action of titanium dioxide," and which shares the common feature that methylene groups are decomposed in both degradation mechanisms. Furthermore, the coating film evaluation method according to the embodiment is also considered applicable to polyester polyurethane paints, polyether polyurethane paints, fluororesin paints, melamine paints, and the like.
[0061] Here, we will explain the comparative examples. The degradation behavior of Degradation Test B (exposure inland of Miyakojima) and Degradation Test C (exposure at Choshi) was similar, but Degradation Test A (exposure at the coast of Miyakojima) was judged to have more "resin decomposition due to the photocatalytic action of titanium dioxide" than those of Degradation Test B and C.
[0062] If these three tests were compared using only the FT-IR measurement results, or only the AFM measurement results, or only the scanning electron microscope (SEM) observation results, without using the coating film evaluation method according to the embodiment, it would be impossible to determine whether the differences between the three tests are simply differences in the rate of deterioration or whether there are differences in the deterioration behavior. Therefore, the coating film evaluation method according to the embodiment can be said to be a useful method that can be used to evaluate whether there are differences in deterioration behavior between outdoor exposure points.
[0063] Furthermore, when the coating film evaluation method according to the embodiment was applied to test specimens (test pieces) subjected to Degradation Test D (accelerated weathering test) and Degradation Test B (Miyakojima inland exposure), it was determined that Degradation Test D (accelerated weathering test) experienced less "resin decomposition due to the photocatalytic action of titanium dioxide" than Degradation Test B (Miyakojima inland exposure), as described above. Even in these cases, if the two tests were compared using only FT-IR measurement results, AFM measurement results, or SEM observation results without using the coating film evaluation method according to the embodiment, the difference in degradation behavior between Degradation Test D and Degradation Test B would not be apparent, leading to the erroneous interpretation that "Degradation Test D (accelerated weathering test) is simply slow, and extending the test time would result in degradation similar to Degradation Test B (Miyakojima inland exposure)." For these reasons, the coating film evaluation method according to the embodiment can be said to be a useful method for verifying whether accelerated weathering tests adequately simulate degradation in real environments.
[0064] Next, we will provide additional information on the basis of the numerical value of 35≦a(t)≦45. Table 1 also shows, as reference data, the results of evaluating the amount of voids by SEM observation. When evaluating the similarity of deterioration behavior using the coating film evaluation method according to the embodiment, it is important that the surface roughness parameter reflects the state of void formation due to "resin decomposition due to the photocatalytic action of titanium dioxide." Therefore, it is necessary to set an upper limit for a(t) so as to exclude the initial stage of deterioration, when voids have not yet formed due to "resin decomposition due to the photocatalytic action of titanium dioxide." In the coating film evaluation method according to the embodiment, voids were observed in SEM observation under all of the deterioration conditions A, B, and C, and a threshold of a(t)≦45 was set as the degree of deterioration at which the progress of "resin decomposition due to the photocatalytic action of titanium dioxide" is reflected in the surface roughness parameter.
[0065] If the upper limit were set higher and judgment were made based on a(t)≦56, this would be inappropriate because it would include test specimens such as those with a(t)=56 under deterioration condition B and a(t=54 under deterioration condition C, in which voids have not yet occurred due to "resin decomposition due to the photocatalytic action of titanium dioxide" and the progress of "resin decomposition due to the photocatalytic action of titanium dioxide" is not reflected in the surface roughness parameters.
[0066] Furthermore, in order to apply the coating film evaluation method according to the embodiment, it is also important that the deterioration has not progressed too far. If the deterioration has progressed too far, it becomes difficult to distinguish between voids formed by "resin decomposition due to the photocatalytic action of titanium dioxide" and unevenness resulting from coating film wear due to "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis," and the degree of progress of "resin decomposition due to the photocatalytic action of titanium dioxide" cannot be accurately evaluated using surface roughness parameters.
[0067] In order to apply the coating film evaluation method according to the embodiment, it is important that the magnitude relationship of the b(X) value and the amount of voids match, and as a condition for this, the coating film evaluation method according to the embodiment sets a threshold value of 35≦a(t).
[0068] From Table 1, when 35≦a(t), the magnitude relationship of the b(X) value and the amount of voids match; however, when a(t)=30 under degradation condition A, SEM observation showed that there were more voids than when a(t)=35, but the value of b(X) calculated using the surface roughness parameters was higher than when a(t)=35, and the magnitude relationship of the amount of voids did not match the magnitude relationship of the b(X) value.
[0069] As described above, the condition 35≦a(t)≦45 is a condition that the inventors experimentally determined by analyzing deteriorated coating films as a condition under which the coating film evaluation method according to the embodiment can be applied, and is not something that can be easily inferred.
[0070] Furthermore, the reason why 0.15 is used as the threshold for determining Δb(X) is that when AFM measurements are performed N=3, the standard deviation of b(X) = {Sp5(t) ÷ Sv5(t)} is approximately 0.1, and 0.15 is set as the threshold for determining that there is a significant deviation in the value.
[0071] In addition, the coating film evaluation method according to the embodiment uses b(X) = {Sp5(t) ÷ Sv5(t)} as an evaluation index for the surface roughness profile, instead of Sv5, which represents the valley depth, as follows:
[0072] Table 1 shows Sv5 as comparative data. In general, it is expected that an increase in the Sv5 value correlates with the progress of void formation due to "resin decomposition due to the photocatalytic action of titanium dioxide." When comparing samples with similar a(t) values, namely, degradation test C, in which voids due to "resin decomposition due to the photocatalytic action of titanium dioxide" are present, and degradation test D, in which voids due to "resin decomposition due to the photocatalytic action of titanium dioxide" are not observed, it is expected that degradation test C, in which voids are formed, will have a larger Sv5 value. However, the results in Table 1 show that the Sv5 values are similar in degradation test C and degradation test D. This indicates that an increase in Sv5 does not necessarily correspond to the presence or absence of void formation due to "resin decomposition due to the photocatalytic action of titanium dioxide."
[0073] As in Deterioration Test D, there are cases where the Sv5 value increases due to an increase in the roughness of the sample surface caused by "molecular chain scission due to photo-oxidation, photo-decomposition, and hydrolysis" even when the formation of voids due to "resin decomposition due to the photocatalytic action of titanium dioxide" does not progress, making it clear that an increase in Sv5 does not necessarily coincide with the presence or absence of void formation due to "resin decomposition due to the photocatalytic action of titanium dioxide."
[0074] The inventors have conducted extensive research into a surface roughness parameter that can evaluate the progress of void formation due to "resin decomposition caused by the photocatalytic action of titanium dioxide" without being affected by the increase in sample surface roughness caused by "molecular chain scission due to photooxidation, photodecomposition, and hydrolysis," and have shown for the first time that the above-mentioned b(X) = {Sp5(t) ÷ Sv5(t)} is appropriate. This is not a value that is commonly used as a surface roughness parameter, and cannot be easily deduced by analogy.
[0075] As described above, according to the present invention, the surface roughness of a test coating film whose surface Fourier transform infrared spectroscopy results fall within a set range is measured, making it possible to evaluate the similarity of the deterioration behavior of titanium dioxide-containing coating films deteriorated under different conditions.The present invention also makes it possible to verify the reproducibility of outdoor deterioration in an accelerated weathering test.
[0076] It should be noted that the present invention is not limited to the embodiments described above, and it is clear that many modifications and combinations can be made by a person having ordinary knowledge in the art within the technical concept of the present invention.
[0077] 201... Particles, 202... Coating film, 203... Voids.
Claims
1. A first step of carrying out a test of a plurality of test coating films, each of which is a coating film containing titanium dioxide, for a period of t for each of a plurality of deterioration tests each having different conditions; and a first step of carrying out a Fourier transform infrared spectroscopic measurement of the surface of each of the plurality of test coating films for which the test has been carried out, to measure the peak λ where the methylene group absorbs light. M cm -1 A is the absorbance of λM (t), and normalization peak λ S cm -1 A is the absorbance of λS (t) is quantified, and the peak λ where absorption due to methylene groups occurs is measured by Fourier transform infrared spectroscopy of the surface of each of the plurality of test target coating films before the test is performed. M cm -1 A is the absorbance of λM (0), and normalization peak λ S cm -1 A is the absorbance of λS (0), a(t) = {|A λM (t) / A λS (t) |÷|A λM (0) / A λS a(t)|×100}, a third step of selecting, for each of the plurality of deterioration tests, from among the plurality of test coating films, a coating film to be evaluated that satisfies 35≦a(t)≦45, a fourth step of measuring the surface roughness of the coating film to be evaluated to obtain a measurement value, and a fifth step of comparing the measurement values of the coating films to be evaluated for each of the plurality of deterioration tests to evaluate a similarity in deterioration behavior.
2. A coating film evaluation method according to claim 1, wherein the fourth step comprises measuring the surface roughness of the coating film to be evaluated, obtaining a five-point peak height Sp5 and a five-point valley depth Sv5, and calculating Sp5÷Sv5 as the measured value.
3. A coating film evaluation method as claimed in claim 2, wherein the fifth step comprises determining a difference between the measurement value of the coating film to be evaluated in one deterioration test used for comparison and the measurement value of the coating film to be evaluated in the other deterioration test, and if the determined difference is 0.15 or more, evaluating the coating film to be evaluated in one deterioration test as having less resin decomposition due to the photocatalytic action of titanium dioxide compared to the coating film to be evaluated in the other deterioration test, if the determined difference is -0.15 or less, evaluating the coating film to be evaluated in one deterioration test as having more resin decomposition due to the photocatalytic action of titanium dioxide compared to the coating film to be evaluated in the other deterioration test, and if the determined difference is greater than -0.15 and less than 0.15, evaluating the coating film to be evaluated in one deterioration test and the coating film to be evaluated in the other deterioration test as having the same degree of resin decomposition due to the photocatalytic action of titanium dioxide.
4. A coating film evaluation method according to any one of claims 1 to 3, wherein the fourth step measures the surface roughness of the coating film to be evaluated using an atomic force microscope.
Citation Information
Patent Citations
Accelerated weathering resistant testing method
JP2003322607A
Testing method
JP2004212380A
Deterioration factor exposure amount measuring method of synthetic resin material
JP2016027331A
Weather resistance testing method and device
WO2022003856A1
Testing apparatus
WO2022259350A1
Cited By
Resin material analysis method and resin material analysis device
WO2026110630A1
Resin material analysis method and resin material analysis device
WO2026110631A1