Electrolyte solution for hybrid electrolytic capacitors and hybrid electrolytic capacitor

The use of an aromatic carboxylic acid with a specific pKa range and a conductive polymer in the electrolytic solution for hybrid capacitors addresses the challenges of high withstand voltage and low ESR, particularly in high-temperature environments, resulting in improved performance for these capacitors.

WO2024214445A1PCT designated stage expired Publication Date: 2024-10-17SANYO CHEM IND LTD

Patent Information

Application Number
PCT/JP2024/008705
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-03-07
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing hybrid electrolytic capacitors face challenges in achieving high withstand voltage and maintaining low equivalent series resistance (ESR) characteristics, especially in high-temperature environments, as previous solutions do not adequately address these requirements.

Method used

An electrolytic solution for hybrid electrolytic capacitors containing an aromatic carboxylic acid with a substituent having 2 or more carbon atoms, which has an acid dissociation constant (pKa) of 1.0 to 4.5, is used, along with a conductive polymer in the solid electrolyte layer, to enhance capacitance and suppress ESR increase at high temperatures.

Benefits of technology

The proposed solution provides hybrid electrolytic capacitors with high withstand voltage and large capacitance while maintaining low ESR even in high-temperature conditions, making them suitable for various electrical and electronic applications, including automotive and mobile devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention relates to an electrolyte solution for hybrid electrolytic capacitors that contains an aromatic carboxylic acid (A) having a substituent with two or more carbon atoms, wherein the acid dissociation constant (pKa) of the carboxylic acid (A) obtained by the measurement method indicated below is 1.0-4.5. Measurement method: a 0.1 mol / L methanolic potassium hydroxide solution is dripped at 25°C into a solution comprising 1 part by weight of the carboxylic acid (A) and 99 parts by weight of methanol, and a point at which the drip amount is the smallest among the inflection points of the obtained titration curve is defined as the neutralization point. The pH when the drip amount is half of the drip amount of the neutralization point is set as the acid dissociation constant (pKa) of the carboxylic acid (A).
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte for hybrid electrolytic capacitor and hybrid electrolytic capacitor

[0001] The present invention relates to an electrolyte for a hybrid electrolytic capacitor, and a hybrid electrolytic capacitor including a capacitor element impregnated with the electrolyte for a hybrid electrolytic capacitor.

[0002] Hybrid electrolytic capacitors are widely used in a variety of electrical and electronic products, and their applications are diverse, including charge storage, noise removal, and phase adjustment. In recent years, their use in automotive applications has increased, and there is a growing need for higher voltage resistance, leading to various attempts at improvement.

[0003] For example, Patent Document 1 discloses a technique for increasing the withstand voltage of a capacitor by using an aliphatic carboxylic acid or a composite compound of an inorganic acid and an organic acid as an anion in the electrolyte, and Patent Document 2 discloses a technique for improving the ESR (equivalent series resistance) of a capacitor for high-voltage applications by using an ammonium salt of an aliphatic carboxylic acid in the electrolyte.

[0004] However, although the electrolytic capacitors described in Patent Documents 1 and 2 can withstand a high voltage, the withstand voltage is not sufficient, and the ESR characteristics in a high-temperature environment are also insufficient.

[0005] JP 2015-165550 A JP 2017-38010 A

[0006] An object of the present invention is to provide an electrolyte solution for a hybrid electrolytic capacitor that has a high withstand voltage and that, when used in a hybrid electrolytic capacitor, has a large capacitance even in a high-temperature environment and can suppress an increase in ESR.

[0007] The present inventors conducted extensive research to solve the above-mentioned problems and arrived at the present invention. Specifically, the present invention relates to an electrolyte solution for hybrid electrolytic capacitors containing an aromatic carboxylic acid (A) having a substituent with two or more carbon atoms, wherein the carboxylic acid (A) has an acid dissociation constant (pKa) of 1.0 to 4.5 as determined by the following measurement method. Measurement method: At 25°C, a 0.1 mol / L methanolic potassium hydroxide solution is added dropwise to a solution consisting of 1 part by weight of the carboxylic acid (A) and 99 parts by weight of methanol. The point at which the smallest amount of addition is taken as the neutralization point among the inflection points on the resulting titration curve. The pH at which the amount of addition is half of the neutralization point is taken as the acid dissociation constant (pKa) of the carboxylic acid (A).

[0008] The present invention also relates to a hybrid electrolytic capacitor including a capacitor element having an anode foil, a dielectric layer formed on the surface of the anode foil, and a layer of a solid electrolyte (C) in contact with the dielectric layer, wherein the capacitor element is impregnated with the electrolytic solution for a hybrid electrolytic capacitor of the present invention, and the layer of the solid electrolyte (C) contains a conductive polymer.

[0009] The electrolytic solution for a hybrid electrolytic capacitor of the present invention has a high withstand voltage and is therefore suitable for use in hybrid electrolytic capacitors. The hybrid electrolytic capacitor of the present invention contains the electrolytic solution for a hybrid electrolytic capacitor of the present invention, and therefore has a large capacitance and a suppressed increase in ESR in a high-temperature environment.

[0010] The electrolyte for hybrid electrolytic capacitors of the present invention is an electrolyte for hybrid electrolytic capacitors containing an aromatic carboxylic acid (A) having a substituent with two or more carbon atoms, characterized in that the acid dissociation constant (pKa) of the carboxylic acid (A) is 1.0 to 4.5, as determined by the following measurement method. Measurement method: At 25°C, a 0.1 mol / L methanolic potassium hydroxide solution is added dropwise to a solution consisting of 1 part by weight of the carboxylic acid (A) and 99 parts by weight of methanol, and the point at which the smallest amount of dropping is added among the inflection points on the resulting titration curve is taken as the neutralization point. The pH at which the amount of dropping is half of the neutralization point is taken as the acid dissociation constant (pKa) of the carboxylic acid (A).

[0011] The aromatic carboxylic acid (A) having a substituent with 2 or more carbon atoms (also simply referred to as carboxylic acid (A) in this specification) is not particularly limited, and examples thereof include compounds having an aromatic ring, a carboxyl group, and a substituent with 2 or more carbon atoms. From the viewpoint of withstand voltage, the carboxylic acid (A) preferably has at least one bond selected from the group consisting of an ester bond, an amide bond, an imide bond, an ether bond, a urethane bond, and a urea bond, and more preferably has an ester bond.

[0012] The carboxylic acid (A) having an ester bond may be, for example, an aromatic carboxylic acid having an aromatic ester group. In this specification, the aromatic ester group refers to a group in which a carbon atom constituting an aromatic ring is directly bonded to a carbon atom of the ester group.

[0013] The aromatic carboxylic acid having an aromatic ester group may be an ester compound of an aromatic carboxylic acid (a1) and an alcohol (a2). Examples of the aromatic carboxylic acid (a1) include aromatic dicarboxylic acids, aromatic tricarboxylic acids, aromatic tetracarboxylic acids, aromatic pentacarboxylic acids, and aromatic hexacarboxylic acids.

[0014] Examples of aromatic dicarboxylic acids include phthalic acid (including phthalic anhydride), isophthalic acid, and terephthalic acid. Examples of aromatic tricarboxylic acids include trimellitic acid (including trimellitic anhydride), 1,2,3-benzenetricarboxylic acid (including anhydride), and 1,3,5-tricarboxylic acid. Examples of aromatic tetracarboxylic acids include aromatic tetracarboxylic acids such as pyromellitic acid (including pyromellitic anhydride). Examples of aromatic pentacarboxylic acids include benzenepentacarboxylic acid (including anhydride). Examples of aromatic hexacarboxylic acids include mellitic acid (including mellitic anhydride).

[0015] Among these aromatic carboxylic acids (a1), from the viewpoint of suppressing an increase in ESR in a high-temperature environment and solubility in a solvent described below, preferred are phthalic acid (including phthalic anhydride), terephthalic acid, trimellitic acid (including trimellitic anhydride), pyromellitic acid (including pyromellitic anhydride), and mellitic acid (including mellitic anhydride), more preferred are phthalic acid (including phthalic anhydride), trimellitic acid (including trimellitic anhydride), and pyromellitic acid (including pyromellitic anhydride), and even more preferred is phthalic acid (including phthalic anhydride). The aromatic carboxylic acids (a1) may be used alone or in combination of two or more.

[0016] Examples of the alcohol (a2) include monools, diols, triols, and tetrahydric or higher alcohols.

[0017] Examples of monools include ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, dodecanol, and tetradecanol. The monool is preferably a monool having 2 to 10 carbon atoms. More specifically, the monool is preferably at least one selected from the group consisting of ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, and decanol. The monool may also have a substituent. Substituted monools include those in which one or more hydrogen atoms of the above-mentioned monools have been substituted with a substituent. Examples of substituents include halogen atoms (such as fluorine atoms, chlorine atoms, and bromine atoms) and alkoxy groups having 1 to 4 carbon atoms.

[0018] Examples of diols include alkylene glycols having 2 to 10 carbon atoms and polyalkylene glycols having an oxyalkylene unit having 2 to 6 carbon atoms.

[0019] Examples of alkylene glycols having 2 to 10 carbon atoms include ethylene glycol, propylene glycol, 1,4-butanediol, 1,10-butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, and decanediol. Examples of polyalkylene glycols having an oxyalkylene unit having 2 to 6 carbon atoms include polyethylene glycol, polypropylene glycol, polybutylene glycol, and polytetramethylene glycol. The number of oxyalkylene units in the polyalkylene glycol is not particularly limited, but is, for example, 2 or more. The number average molecular weight of the polyalkylene glycol is not particularly limited, but from the viewpoints of withstand voltage and solubility, it is preferably 2,000 or less, and more preferably 1,000 or less.

[0020] Examples of triols include glycerin and trimethylolpropane.

[0021] Examples of the tetrahydric or higher alcohol include pentaerythritol, dipentaerythritol, diglycerin, triglycerin, sorbitol, and sucrose.

[0022] From the viewpoints of withstand voltage and solubility in a solvent described later, the alcohol (a2) is preferably a diol, more preferably at least one selected from the group consisting of ethylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, and polytetramethylene glycol, and even more preferably at least one selected from the group consisting of ethylene glycol, polyethylene glycol, and polypropylene glycol. One type of alcohol (a2) may be used alone, or two or more types may be used in combination.

[0023] The method and conditions for reacting the aromatic carboxylic acid (a1) with the alcohol (a2) are not particularly limited, and conventionally known methods and conditions can be used. After the condensation reaction of the aromatic carboxylic acid (a1) with the alcohol (a2), ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, toluene, or the like may be added to the resulting reaction solution in order to precipitate a solid.

[0024] A preferred embodiment of the aromatic carboxylic acid having an aromatic ester group is an aromatic carboxylic acid having one aromatic ester group (aromatic carboxylic acid monoester). A preferred embodiment of the aromatic carboxylic acid monoester is a carboxylic acid represented by the following general formula (1):

[0025]

[0026] In general formula (1), R 1represents a residue obtained by removing a hydroxy group from a monool having 2 to 10 carbon atoms, which may have a substituent; a residue obtained by removing one hydroxy group from an alkylene glycol having 2 to 10 carbon atoms; a residue obtained by removing one hydroxy group from a polyalkylene glycol having an oxyalkylene unit having 2 to 6 carbon atoms; or a residue obtained by removing one hydroxy group from glycerin. Examples of monools having 2 to 10 carbon atoms include ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, and decanol. The monools having 2 to 10 carbon atoms may have a substituent. Examples of substituted monools having 2 to 10 carbon atoms include those in which one or more hydrogen atoms of the above-mentioned monools having 2 to 10 carbon atoms have been substituted with a substituent. Examples of the substituent include halogen atoms (such as fluorine atoms, chlorine atoms, and bromine atoms) and alkoxy groups having 1 to 4 carbon atoms. Examples of alkylene glycols having 2 to 10 carbon atoms include ethylene glycol, propylene glycol, 1,4-butanediol, 1,10-butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, and decanediol. Examples of polyalkylene glycols having an oxyalkylene unit having 2 to 6 carbon atoms include polyethylene glycol, polypropylene glycol, polybutylene glycol, and polytetramethylene glycol. The number of oxyalkylene units in the polyalkylene glycol is not particularly limited, but is, for example, 2 or more. The number-average molecular weight of the polyalkylene glycol is not particularly limited, but from the viewpoints of withstand voltage and solubility, it is preferably 2000 or less, more preferably 1000 or less. n is not particularly limited as long as it is an integer of 1 to 5, but from the viewpoint of withstand voltage, it is preferably an integer of 1 to 3, more preferably 1 or 2.

[0027] Specific examples of aromatic carboxylic acids having an aromatic ester group include decanol monoester phthalate, ethylene glycol monoester phthalate, polyethylene glycol monoester phthalate, polypropylene glycol monoester phthalate, glycerin monoester phthalate, decanol monoester terephthalate, ethylene glycol monoester terephthalate, polyethylene glycol monoester terephthalate, polypropylene glycol monoester terephthalate, glycerin monoester terephthalate, decanol monoester trimellitate, ethylene glycol monoester trimellitate, polyethylene glycol monoester trimellitate, polypropylene glycol monoester trimellitate, glycerin monoester trimellitate, decanol monoester pyromellitate, ethylene glycol monoester pyromellitate, polyethylene glycol monoester pyromellitate, polypropylene glycol monoester pyromellitate, glycerin monoester pyromellitate, decanol monoester mellitate, ethylene glycol monoester mellitate, polyethylene glycol monoester mellitate, polypropylene glycol monoester mellitate, and glycerin monoester mellitate.

[0028] From the viewpoint of simultaneously suppressing an increase in ESR in a high-temperature environment and ensuring a high withstand voltage, the carboxylic acid (A) is preferably an aromatic carboxylic acid having an aromatic ester group, more preferably an aromatic carboxylic acid having one aromatic ester group (aromatic carboxylic acid monoester), and even more preferably a carboxylic acid represented by the general formula (1). One type of the carboxylic acid (A) may be used alone, or two or more types may be used in combination.

[0029] The acid dissociation constant (pKa) of the carboxylic acid (A) determined by the above measurement method is not particularly limited as long as it is 1.0 to 4.5, but is preferably 1.5 to 4.0, and more preferably 2.0 to 4.0. If the pKa of the carboxylic acid (A) is less than 1.0, dissolution of the oxide film on the anode of the hybrid electrolytic capacitor will proceed, making it impossible to repair the oxide film, and the initial spark voltage (withstand voltage) may decrease. On the other hand, if the pKa exceeds 4.5, the effect of suppressing oxidative degradation of the conductive polymer will be insufficient, and the capacitance and ESR may deteriorate in high-temperature environments.

[0030] The pKa of the carboxylic acid (A) is expressed by the following formula: pKa = -log 10 (([(A) anion][proton]) / [(A)]) [(A) anion]: concentration of the carboxylic acid (A) anion (mol / L) [proton]: concentration of proton (mol / L) [(A)]: concentration of carboxylic acid (A) (mol / L) Furthermore, from the relationship between pKa and hydrogen ion concentration pH, the pH and pKa of the solution will be equal when 0.5 mol equivalents of a strong base are added to an acid.

[0031] In this specification, the pKa of the carboxylic acid (A) can be measured, for example, using an automatic titrator under the following conditions. Apparatus (example): Automatic titrator COM-A19 (manufactured by HIRANUMA Corporation) Electrode (example): Glass electrode GE-101B (manufactured by HIRANUMA Corporation) Measurement temperature: 25°C. A 0.1 mol / L methanolic potassium hydroxide solution is added dropwise to a solution consisting of 1 part by weight of the carboxylic acid (A) and 99 parts by weight of methanol at 25°C, and the point at which the smallest amount of addition is obtained among the inflection points of the titration curve is taken as the neutralization point. The pH at which the amount of addition is half of the neutralization point is taken as the acid dissociation constant (pKa) of the carboxylic acid (A).

[0032] The pKa of the carboxylic acid (A) can be adjusted, for example, by selecting a substituent having two or more carbon atoms. For example, the pKa can be lowered by introducing an electron-withdrawing group as the substituent having two or more carbon atoms, and the pKa can be increased by introducing an electron-donating group.

[0033] The content of the carboxylic acid (A) in the electrolytic solution for a hybrid electrolytic capacitor of the present invention is not particularly limited, but from the viewpoint of suppressing an increase in withstand voltage and ESR in a high-temperature environment, it is preferably 0.05 to 40% by weight, more preferably 1 to 30% by weight, and even more preferably 1 to 20% by weight.

[0034] In the electrolytic solution for hybrid electrolytic capacitors of the present invention, the content of the carboxylic acid (A) is not particularly limited, but is preferably 50 to 100% by weight, more preferably 60 to 100% by weight, and even more preferably 70 to 100% by weight, based on the total weight of the acid components (the total weight of the carboxylic acid (A) and the acid component (A') other than the carboxylic acid (A) described below), from the viewpoint of suppressing an increase in withstand voltage and ESR in a high-temperature environment.

[0035] The electrolytic solution for hybrid electrolytic capacitors of the present invention preferably further contains an alcohol (B) from the viewpoint of suppressing an increase in ESR in a high-temperature environment. Examples of the alcohol (B) include ethylene glycol, propylene glycol, 1,4-butanediol, 1,10-butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, n-decanol, 1,10-decanediol, glycerin, and polyalkylene glycols having an oxyalkylene unit having 2 to 6 carbon atoms.

[0036] Examples of polyalkylene glycols having an oxyalkylene unit having 2 to 6 carbon atoms include polyethylene glycol, polypropylene glycol, polybutylene glycol, and polytetramethylene glycol. The number of oxyalkylene units in the polyalkylene glycol is not particularly limited, but is, for example, 2 or more. The number average molecular weight of the polyalkylene glycol is not particularly limited, but from the viewpoint of withstand voltage, it is preferably 2000 or less, more preferably 1000 or less.

[0037] From the viewpoint of withstand voltage, the alcohol (B) is preferably at least one selected from the group consisting of ethylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, and polytetramethylene glycol, and more preferably at least one selected from the group consisting of ethylene glycol, polyethylene glycol, and polypropylene glycol. The alcohol (B) may be used alone or in combination of two or more.

[0038] When the electrolytic solution for a hybrid electrolytic capacitor of the present invention contains the alcohol (B), the content of the alcohol (B) in the electrolytic solution for a hybrid electrolytic capacitor of the present invention is not particularly limited, but from the viewpoint of suppressing an increase in withstand voltage and ESR in a high-temperature environment, it is preferably 40 to 99 wt %, more preferably 60 to 90 wt %, and even more preferably 75 to 90 wt %.

[0039] When the electrolytic solution for a hybrid electrolytic capacitor of the present invention contains the alcohol (B), the weight ratio ((B) / (A)) of the alcohol (B) to the carboxylic acid (A) in the electrolytic solution for a hybrid electrolytic capacitor of the present invention is not particularly limited, but from the viewpoint of withstand voltage, it is preferably 1 to 500, more preferably 1 to 200, and even more preferably 2 to 20.

[0040] The electrolyte solution for hybrid electrolytic capacitors of the present invention may contain an acid component (A') other than the carboxylic acid (A). Examples of the acid component (A') other than the carboxylic acid (A) include an aliphatic carboxylic acid having an aliphatic ester group and other acid components. In this specification, the term "aliphatic ester group" refers to a group in which a carbon atom constituting a non-aromatic hydrocarbon group is directly bonded to a carbon atom of the ester group. The non-aromatic hydrocarbon group may be acyclic (straight-chain or branched-chain) or cyclic.

[0041] The aliphatic carboxylic acid having an aliphatic ester group can be an ester compound of an aliphatic carboxylic acid (a'1) and an alcohol (a2). The alcohol (a2) can be the same as the alcohol (a2) used for the aromatic carboxylic acid having an aromatic ester group described above. The aliphatic carboxylic acid (a'1) can include aliphatic dicarboxylic acids, aliphatic tricarboxylic acids, and aliphatic tetracarboxylic acids.

[0042] Examples of the aliphatic dicarboxylic acid include malonic acid, succinic acid (including succinic anhydride), malic acid, fumaric acid, adipic acid, and sebacic acid. Examples of the aliphatic tricarboxylic acid include citric acid, isocitric acid, and propane-1,2,3-tricarboxylic acid. Examples of the aliphatic tetracarboxylic acid include cyclobutanetetracarboxylic acid (including anhydride) and 1,2,3,4-butanetetracarboxylic acid (including anhydride).

[0043] The method and conditions for reacting the aliphatic carboxylic acid (a'1) with the alcohol (a2) are not particularly limited, and conventionally known methods and conditions can be used. After the condensation reaction of the aliphatic carboxylic acid (a'1) with the alcohol (a2), ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, toluene, or the like may be added to the resulting reaction solution in order to precipitate a solid.

[0044] Examples of the other acid components include aromatic carboxylic acids such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, 1,2-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, acetylsalicylic acid, trimellitic acid, and pyromellitic acid; aliphatic carboxylic acids such as adipic acid, sebacic acid, azelaic acid, 1,6-decanedicarboxylic acid, 2-furancarboxylic acid, 3-furancarboxylic acid, and 2,5-furandicarboxylic acid; and acids such as phosphoric acid (phosphoric acid, diphosphorous acid, and phosphate esters) and boric acid (boric acid, borate esters, and borodisalicylic acid). Furthermore, examples of the other acid components include ester compounds of monocarboxylic acids having a sulfo group with alcohol (a2). Examples of monocarboxylic acids having a sulfo group include m-sulfobenzoic acid and o-sulfobenzoic acid. As the alcohol (a2), the same alcohol (a2) as that used for the aromatic carboxylic acid having an aromatic ester group described above can be used.

[0045] From the viewpoint of suppressing an increase in ESR in a high-temperature environment, the acid component (A') other than the carboxylic acid (A) is preferably at least one selected from the group consisting of benzoic acid, phthalic acid, and 2,5-furandicarboxylic acid, and more preferably phthalic acid.

[0046] From the viewpoint of achieving a high withstand voltage, the acid component (A') other than the carboxylic acid (A) is preferably at least one selected from the group consisting of an aliphatic carboxylic acid having an aliphatic ester group, an aromatic carboxylic acid, and boric acid, more preferably an aromatic carboxylic acid and boric acid, and even more preferably boric acid. The acid component (A') other than the carboxylic acid (A) may be used alone or in combination of two or more.

[0047] When the electrolytic solution for hybrid electrolytic capacitors of the present invention contains an acid component (A') other than the carboxylic acid (A), the content of the acid component (A') other than the carboxylic acid (A) in the electrolytic solution for hybrid electrolytic capacitors of the present invention is not particularly limited, but from the viewpoint of suppressing an increase in ESR in a high-temperature environment, it is preferably 10 wt % or less, more preferably 5 wt % or less, and even more preferably 1 wt % or less.

[0048] In the electrolyte solution for hybrid electrolytic capacitors of the present invention, the carboxylic acid (A) and the acid component (A') may be present in the form of an acid, or may be ionized and present as an anion. Examples of counter cations for the anions include ammonium, primary ammonium, secondary ammonium, tertiary ammonium, and amidinium. Examples of ammonium, primary ammonium, secondary ammonium, and tertiary ammonium include ammonium derived from ammonia, primary amines, secondary amines, and tertiary amines, respectively. Examples of these amines include methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, N,N-diisopropylethylamine, tetramethylethylenediamine, hexamethylenediamine, spermidine, spermine, amantadine, aniline, phenethylamine, toluidine, pyrrolidine, piperidine, piperazine, morpholine, ethylmorpholine, imidazole, pyridine, pyridazine, pyrimidine, pyrazine, 4-dimethylaminopyridine, and trimethanolamine. Examples of amidinium include 1,2,3,4-tetramethylimidazolinium, 1,3-dimethylimidazolium, 1,3-diisopropylimidazolium, 1,3-dibutylimidazolium, 1-methyl-3-propylimidazolium, 1-ethyl-3-methylimidazolium, 1-ethyl-2,3-dimethylimidazolium, 1-butyl-3-methylimidazolium, and 1-benzyl-3-methylimidazolium. One type of counter cation for the anion may be used alone, or two or more types may be used in combination.

[0049] From the viewpoint of suppressing an increase in ESR, the counter cation of the anion is preferably at least one selected from the group consisting of ammonium, primary ammonium and tertiary ammonium, and more preferably tertiary ammonium.

[0050] When the electrolytic solution for a hybrid electrolytic capacitor of the present invention contains a counter cation for the anion in addition to the carboxylic acid (A), the content of the substance that generates the counter cation for the anion (ammonia, primary amine, secondary amine, and tertiary amine) is not particularly limited, but from the viewpoint of suppressing an increase in withstand voltage and ESR in a high-temperature environment, it is preferably 0.1 to 20% by weight, more preferably 1.0 to 10% by weight, and even more preferably 2.0 to 5.0% by weight.

[0051] The hybrid electrolytic capacitor electrolyte solution of the present invention may further contain a solvent other than the alcohol (B). Examples of the solvent include water, alcohol solvents other than the alcohol (B) (e.g., methyl alcohol, ethyl alcohol, propyl alcohol, butyl alcohol, and ethylene glycol monobutyl ether), amide solvents (e.g., N-methylformamide, N-ethylformamide, and N,N-dimethylformamide), lactone solvents (e.g., α-acetyl-γ-butyrolactone, β-butyrolactone, γ-butyrolactone, γ-valerolactone, and δ-valerolactone), nitrile solvents (e.g., acetonitrile, propionitrile, butyronitrile, acrylonitrile, methacrylonitrile, and benzonitrile), sulfoxide solvents (e.g., dimethyl sulfoxide, methyl ethyl sulfoxide, and diethyl sulfoxide), and sulfone solvents (e.g., sulfolane and ethyl methyl sulfone). From the viewpoint of suppressing an increase in ESR, the solvent is preferably a lactone solvent or a sulfone solvent, more preferably a sulfone solvent, and even more preferably sulfolane. The above solvents may be used alone or in combination of two or more.

[0052] When the electrolytic solution for a hybrid electrolytic capacitor of the present invention contains water as a solvent, the content of water in the electrolytic solution for a hybrid electrolytic capacitor of the present invention is not particularly limited, but from the viewpoint of withstand voltage, it is preferably 0.05 to 40 wt %, more preferably 0.5 to 3.0 wt %.

[0053] The pH of the electrolyte solution for a hybrid electrolytic capacitor of the present invention at 25°C is not particularly limited, but from the viewpoints of suppressing an increase in ESR and withstand voltage, it is preferably 4 to 6, more preferably 4 to 5.5, and even more preferably 4 to 5. In this specification, the pH of the electrolyte solution for a hybrid electrolytic capacitor of the present invention at 25°C is a value measured directly with a pH meter.

[0054] The hybrid electrolytic capacitor of the present invention is a hybrid electrolytic capacitor including a capacitor element having an anode foil, a dielectric layer formed on the surface of the anode foil, and a layer of solid electrolyte (C) in contact with the dielectric layer, wherein the capacitor element is impregnated with the electrolytic solution for hybrid electrolytic capacitors of the present invention, and the solid electrolyte (C) contains a conductive polymer. In one aspect, the hybrid electrolytic capacitor of the present invention may also include a pair of lead wires and an outer casing in addition to the capacitor element. One end of each of the pair of lead wires is connected to the capacitor element. The outer casing encapsulates the capacitor element such that the other end of the lead wire extends to the outside. The outer casing is composed of a cylindrical case, a drawn portion provided on the outer periphery of the case, and a sealing body having a through hole for inserting the lead wire. The case houses a capacitor element impregnated with the electrolytic solution for hybrid electrolytic capacitors of the present invention. The lead wires, one end of which is connected to the capacitor element, are each inserted into the through hole of the sealing body and compressed by the drawn portion to be sealed.

[0055] An anode foil having a dielectric layer on its surface is formed, for example, by roughening an aluminum foil by etching and then chemically treating the surface with an anodized film, which is a dielectric. A capacitor element includes an anode foil, a dielectric layer formed on the surface of the anode foil, and a layer of solid electrolyte (C) in contact with the dielectric layer. The layer of solid electrolyte (C) contains a conductive polymer. A capacitor element typically includes a cathode foil and a separator in addition to the anode foil and the layer of solid electrolyte (C). In one embodiment, the capacitor element has a structure in which a laminate is wound, in which an anode foil, a dielectric layer formed on the surface of the anode foil, a layer of solid electrolyte (C) containing a conductive polymer, a separator, and a cathode foil are stacked in this order. The separator may be impregnated with the solid electrolyte (C) containing a conductive polymer. The method for forming the layer of solid electrolyte (C) containing a conductive polymer is not particularly limited and can be any known method, such as a method of impregnating the solid electrolyte (C) with a conductive polymer solution and then drying it, or a method of electrolytically polymerizing the conductive polymer to form the solid electrolyte (C). In the hybrid electrolytic capacitor of the present invention, the electrolytic solution for hybrid electrolytic capacitors of the present invention is impregnated into the capacitor element. Specifically, the electrolytic solution for hybrid electrolytic capacitors of the present invention is impregnated into the gaps in the layer of solid electrolyte (C) formed in the capacitor element.

[0056] The shape and size of the hybrid electrolytic capacitor of the present invention are not particularly limited. The structure of the hybrid electrolytic capacitor of the present invention is also not particularly limited. Examples include a wound-type hybrid electrolytic capacitor, i.e., a hybrid electrolytic capacitor having a structure in which an anode foil (e.g., aluminum oxide foil) having a dielectric layer (e.g., aluminum oxide layer) on its surface and a cathode foil (e.g., aluminum foil) are wound with a separator interposed between them. The method for manufacturing the hybrid electrolytic capacitor of the present invention is not particularly limited, and conventionally known methods can be used. For example, a method can be used in which the electrolyte solution for the hybrid electrolytic capacitor of the present invention is impregnated into a separator (e.g., kraft paper or manila paper) as a driving electrolyte, and the separator is interposed between the anode foil and the cathode foil. The separator is then wound and placed in a cylindrical aluminum case with a bottom, and the opening of the aluminum case is sealed with a sealing rubber (e.g., butyl rubber or silicone rubber).

[0057] In the hybrid electrolytic capacitor of the present invention, the layer of the solid electrolyte (C) contains a conductive polymer. Examples of conductive polymers include (co)polymers containing thiophene, 3,4-ethylenedioxythiophene, alkylated ethylenedioxythiophene, alkoxylated ethylenedioxythiophene, pyrrole, aniline, or the like as constituent monomers. However, it is preferable to use a (co)polymer containing 3,4-ethylenedioxythiophene as a constituent monomer, and it is more preferable to use poly(3,4-ethylenedioxythiophene) doped with polystyrene sulfonic acid. The conductive polymer may be used alone or in combination of two or more types.

[0058] The hybrid electrolytic capacitor of the present invention includes a capacitor element impregnated with the hybrid electrolytic capacitor electrolyte solution of the present invention, and is therefore advantageous in that it not only reduces the initial ESR but also suppresses the increase in ESR at high temperatures. While the mechanism for suppressing the increase in ESR at high temperatures is not yet clear, it is speculated as follows. The performance degradation (e.g., a decrease in ESR retention rate) of conventional hybrid electrolytic capacitor electrolyte solutions is thought to be caused by oxidative degradation and dedoping of the conductive polymer constituting the solid electrolyte. The hybrid electrolytic capacitor electrolyte solution of the present invention contains an aromatic carboxylic acid (A) having a substituent with two or more carbon atoms. The acid dissociation constant (pKa) of the carboxylic acid (A) measured by the above-described measurement method is 1.0 to 4.5. Therefore, by maintaining the pH at 25°C in the range of 4 to 6, it is thought that oxidative degradation and dedoping of the conductive polymer contained in the solid electrolyte (C) layer are suppressed.

[0059] <Others> The present specification discloses the following: <1> An electrolyte solution for hybrid electrolytic capacitors containing an aromatic carboxylic acid (A) having a substituent with two or more carbon atoms, wherein the carboxylic acid (A) has an acid dissociation constant (pKa) of 1.0 to 4.5 as determined by the following measurement method. Measurement method: At 25°C, a 0.1 mol / L methanolic potassium hydroxide solution is added dropwise to a solution consisting of 1 part by weight of the carboxylic acid (A) and 99 parts by weight of methanol. The point at which the smallest amount of added solution is obtained among the inflection points on the resulting titration curve is defined as the neutralization point. The pH at which the amount of added solution is half of the neutralization point is defined as the acid dissociation constant (pKa) of the carboxylic acid (A). <2> The electrolyte solution for hybrid electrolytic capacitors according to <1>, wherein the carboxylic acid (A) has at least one bond selected from the group consisting of an ester bond, an amide bond, an imide bond, an ether bond, a urethane bond, and a urea bond. <3> The electrolyte solution for hybrid electrolytic capacitors according to <1> or <2>, wherein the carboxylic acid (A) has an ester bond. <4> The electrolyte solution for a hybrid electrolytic capacitor according to any one of <1> to <3>, wherein the content of the carboxylic acid (A) is 50 to 100% by weight based on the total weight of the acid components. <5> The electrolyte solution for a hybrid electrolytic capacitor according to any one of <1> to <4>, further comprising an alcohol (B), wherein the weight ratio of the alcohol (B) to the carboxylic acid (A) ((B) / (A)) is 1 to 200. <6> The electrolyte solution for a hybrid electrolytic capacitor according to any one of <1> to <5>, wherein the carboxylic acid (A) contains a carboxylic acid represented by general formula (1).

[0060]

[0061] [In general formula (1), R 1represents a residue obtained by removing a hydroxy group from a monool having 2 to 10 carbon atoms which may have a substituent, a residue obtained by removing one hydroxy group from an alkylene glycol having 2 to 10 carbon atoms, a residue obtained by removing one hydroxy group from a polyalkylene glycol having an oxyalkylene unit having 2 to 6 carbon atoms, or a residue obtained by removing one hydroxy group from glycerin. n represents an integer of 1 to 5.] <7> A hybrid electrolytic capacitor including a capacitor element having an anode foil, a dielectric layer formed on the surface of the anode foil, and a layer of solid electrolyte (C) in contact with the dielectric layer, wherein the capacitor element is impregnated with the electrolytic solution for a hybrid electrolytic capacitor according to any one of <1> to <6>, and the layer of solid electrolyte (C) contains a conductive polymer.

[0062] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0063] <Method for measuring the acid dissociation constant (pKa) of carboxylic acid (A)> 99 parts by weight of methanol was added to 1 part by weight of carboxylic acid (A) at 25°C, and the mixture was shaken until completely dissolved. A 0.1 mol / L methanolic potassium hydroxide solution was added dropwise to the resulting carboxylic acid (A) methanol solution, and the point at which the smallest amount of addition was found among the inflection points on the resulting titration curve was determined as the neutralization point. The pH was read from the resulting titration curve when the amount of addition was half the neutralization point, and this pH was determined as the acid dissociation constant (pKa) of the carboxylic acid (A). The pKa of the acid component (A') was also measured in the same manner as the pKa of the carboxylic acid (A). pKa = -log 10 (([(A) anion][proton]) / [(A)]) [(A) anion]: concentration of carboxylic acid (A) anion (mol / L) [proton]: concentration of proton (mol / L) [(A)]: concentration of carboxylic acid (A) (mol / L) <Measurement conditions> Apparatus: automatic titrator COM-A19 (manufactured by HIRANUMA Co., Ltd.) Electrode: glass electrode GE-101B (manufactured by HIRANUMA Co., Ltd.) Measurement temperature: 25°C

[0064] <Production Example 1> 21.0 parts by weight (1 mol equivalent) of phthalic anhydride was charged into a Kolben, and 79.0 parts by weight (9.0 mol equivalent) of ethylene glycol was added dropwise to carry out a condensation reaction (esterification reaction) to obtain a reaction solution. 50.0 parts by weight of ethyl acetate was added to the obtained reaction solution, and the mixture was cooled to -5°C to precipitate a solid. The precipitated solid was separated by filtration and then dried to obtain 29.8 parts by weight of ethylene glycol phthalate monoester (A1). The acid dissociation constant (pKa) of ethylene glycol phthalate monoester (A1) was measured by the above-mentioned measurement method and found to be 3.8.

[0065] <Production Example 2> 14.7 parts by weight (1 mol equivalent) of terephthalic acid and 85.3 parts by weight (15.5 mol equivalent) of ethylene glycol were charged into a Kolben, heated to 140°C, and maintained for 3 hours to carry out a condensation reaction (esterification reaction). Thereafter, unreacted ethylene glycol was removed under reduced pressure (0.5 kPa) at 120°C, yielding 20 parts by weight of a mixture (A2) of ethylene glycol terephthalate monoester and ethylene glycol terephthalate diester. The acid dissociation constant (pKa) of the mixture (A2) of ethylene glycol terephthalate monoester and ethylene glycol terephthalate diester was measured by the above-mentioned measurement method and found to be 4.1.

[0066] <Production Example 3> A reaction was carried out in the same manner as in Production Example 1, except that phthalic anhydride was changed to 22.2 parts by weight (1 mol equivalent) of trimellitic anhydride and the charged weight of ethylene glycol was changed to 77.8 parts by weight (11.8 mol equivalent) in Production Example 1, to obtain 28.8 parts by weight of trimellitic acid ethylene glycol monoester (A3). The acid dissociation constant (pKa) of trimellitic acid ethylene glycol monoester (A3) was measured by the above-mentioned measurement method and was found to be 3.4.

[0067] <Production Example 4> A reaction was carried out in the same manner as in Production Example 1, except that phthalic anhydride was replaced with 15.9 parts by weight (1 mol equivalent) of trimellitic anhydride and ethylene glycol was replaced with 84.1 parts by weight (5.6 mol equivalents) of PEG200 (polyethylene glycol, number average molecular weight 200, manufactured by Sanyo Chemical Industries, Ltd.), to obtain 28.8 parts by weight of trimellitic acid polyethylene glycol monoester (A4). The acid dissociation constant (pKa) of trimellitic acid polyethylene glycol monoester (A4) was measured by the above-mentioned measurement method and was found to be 3.6.

[0068] <Production Example 5> A reaction was carried out in the same manner as in Production Example 1, except that phthalic anhydride was changed to 26.1 parts by weight (1 mol equivalent) of pyromellitic anhydride and 73.9 parts by weight (11.6 mol equivalents) of ethylene glycol in Production Example 1, to obtain 32.4 parts by weight of pyromellitic acid ethylene glycol monoester (A5). The acid dissociation constant (pKa) of pyromellitic acid ethylene glycol monoester (A5) was measured by the above-mentioned measurement method and was found to be 2.6.

[0069] <Production Example 6> A reaction was carried out in the same manner as in Production Example 1, except that phthalic anhydride was replaced with 11.6 parts by weight (1 mol equivalent) of pyromellitic anhydride and ethylene glycol was replaced with 88.4 parts by weight (9.7 mol equivalent) of PEG200 (polyethylene glycol, number average molecular weight 200, manufactured by Sanyo Chemical Industries, Ltd.), to obtain 20.6 parts by weight of pyromellitic acid polyethylene glycol monoester (A6). The acid dissociation constant (pKa) of pyromellitic acid polyethylene glycol monoester (A6) was measured by the above-mentioned measurement method and found to be 2.9.

[0070] <Production Example 7> A reaction was carried out in the same manner as in Production Example 1, except that phthalic anhydride was changed to 24.5 parts by weight (1 mol equivalent) of mellitic anhydride and 75.5 parts by weight (14.3 mol equivalents) of ethylene glycol in Production Example 1, to obtain 29.8 parts by weight of mellitic acid ethylene glycol monoester (A7). The acid dissociation constant (pKa) of mellitic acid ethylene glycol monoester (A7) was measured by the above-mentioned measurement method and was found to be 1.7.

[0071] Production Example 8 A reaction was carried out in the same manner as in Production Example 1, except that the amount of phthalic anhydride was changed to 5.1 parts by weight (1 mol equivalent) and the ethylene glycol was changed to 94.9 parts by weight (7.0 mol equivalent) of Sannix PP-400 (polypropylene glycol, number average molecular weight 400, manufactured by Sanyo Chemical Industries, Ltd.), to obtain 18.7 parts by weight of phthalic acid polypropylene glycol monoester (A8). The acid dissociation constant (pKa) of the phthalic acid polypropylene glycol monoester (A8) was measured by the above-mentioned measurement method and was found to be 3.9.

[0072] <Production Example 9> A reaction was carried out in the same manner as in Production Example 1, except that the amount of phthalic anhydride was changed to 2.5 parts by weight (1 mol equivalent) and the ethylene glycol was changed to 97.5 parts by weight (5.8 mol equivalent) of PEG1000 (polyethylene glycol, number average molecular weight 1000, manufactured by Sanyo Chemical Industries, Ltd.), to obtain 19.2 parts by weight of phthalic acid polyethylene glycol monoester (A9). The acid dissociation constant (pKa) of the phthalic acid polyethylene glycol monoester (A9) was measured by the above-mentioned measurement method and was found to be 4.2.

[0073] Production Example 10 A reaction was carried out in the same manner as in Production Example 1, except that the amount of phthalic anhydride was changed to 13.2 parts by weight (1 mol equivalent) and the amount of n-decanol was changed to 86.8 parts by weight (6.2 mol equivalent) of n-decanol in place of ethylene glycol, to obtain 27.2 parts by weight of n-decanol phthalate monoester (A10). The acid dissociation constant (pKa) of n-decanol phthalate monoester (A10) was measured by the above-mentioned method and was found to be 3.9.

[0074] Production Example 11 A reaction was carried out in the same manner as in Production Example 1, except that the amount of phthalic anhydride was changed to 12.9 parts by weight (1 mol equivalent) and the amount of ethylene glycol was changed to 87.1 parts by weight (5.7 mol equivalent) of 1,10-decanediol phthalate monoester (A11), to obtain 28.1 parts by weight of 1,10-decanediol phthalate monoester (A11). The acid dissociation constant (pKa) of the 1,10-decanediol phthalate monoester (A11) was measured by the above-mentioned measurement method and was found to be 4.0.

[0075] Production Example 12 A reaction was carried out in the same manner as in Production Example 1, except that the amount of phthalic anhydride was changed to 13.1 parts by weight (1 mol equivalent) and the amount of ethylene glycol was changed to 86.9 parts by weight (10.6 mol equivalent) of glycerin, to obtain 21.3 parts by weight of glycerin phthalate monoester (A12). The acid dissociation constant (pKa) of the glycerin phthalate monoester (A12) was measured by the above-mentioned measurement method and was found to be 3.7.

[0076] Production Example 13 The same procedure as in Production Example 1 was carried out, except that phthalic anhydride was replaced with 18.4 parts by weight (1 mol equivalent) of succinic anhydride and the amount of ethylene glycol charged was changed to 81.6 parts by weight (7.2 mol equivalents), to obtain 29.8 parts by weight of succinic acid ethylene glycol monoester (A'1). The acid dissociation constant (pKa) of succinic acid ethylene glycol monoester (A'1) was measured by the above-mentioned measurement method and was found to be 6.5.

[0077] <Production Example 14> Production Example 1 was repeated except that phthalic anhydride was replaced with 20.7 parts by weight (1 mol equivalent) of m-sulfobenzoic acid and the amount of ethylene glycol charged was changed to 79.3 parts by weight (12.5 mol equivalents), to obtain 27.0 parts by weight of m-sulfobenzoic acid ethylene glycol monoester (A'2). The acid dissociation constant (pKa) of m-sulfobenzoic acid ethylene glycol monoester (A'2) was measured by the above-mentioned measurement method and was found to be 0.9. The compounds used in each Production Example and the acid dissociation constant (pKa) of the resulting carboxylic acid (A) are shown in Table 1.

[0078]

[0079] Examples 1 to 17 and Comparative Examples 1 to 6 Preparation of Electrolyte Solutions for Hybrid Electrolytic Capacitors Electrolyte solutions (Y-1) to (Y-17) for hybrid electrolytic capacitors of the present invention (Examples) and electrolytic solutions (Y'-1) to (Y'-6) for hybrid electrolytic capacitors of the comparative examples were prepared by mixing the components in the compositions (parts by weight) shown in Table 2, and removing the carbon dioxide by degassing under reduced pressure as necessary. Note that for the electrolytic solution (Y-2) for hybrid electrolytic capacitors of the present invention, the carbon dioxide generated by the reaction of 1,2,3,4-tetramethylimidazolinium / methyl carbonate with an acid was removed by degassing under reduced pressure, and therefore the parts by weight excluding the carbon dioxide are shown in Table 2.

[0080]

[0081] The electrolytic solutions for hybrid electrolytic capacitors obtained in Examples 1 to 17 and Comparative Examples 1 to 6 were evaluated for "spark voltage" before (initial) and after the high-temperature test by the following method. The results are shown in Table 3. <Evaluation method for spark voltage> 2 Anode foil (chemically processed aluminum foil, manufactured by Nippon Capacitor Industrial Co., Ltd., 115HD-658Vf) having a dielectric layer of 10 ... 2 A plain aluminum foil (or a plain aluminum foil) was placed opposite each other in the hybrid electrolytic capacitor electrolyte, and a load of 2 mA was applied using a constant-voltage / constant-current DC power supply (GP0650-05R, manufactured by Takasago Machinery Co., Ltd.) at 85°C, and the voltage was measured. Time was plotted on the horizontal axis and voltage on the vertical axis. The voltage rise curve over time was observed, and the voltage at the point when the first disturbance in the rise curve due to spark or scintillation occurred was defined as the spark voltage. A higher spark voltage indicates a higher withstand voltage. <Method for Evaluating Spark Voltage After High-Temperature Test> The hybrid electrolytic capacitor electrolytes obtained in Examples 1 to 17 and Comparative Examples 1 to 6 were sealed in a sealed container and then left in a thermostatic chamber set at 125°C for 500 hours. The spark voltage of each hybrid electrolytic capacitor electrolyte was then evaluated using the method described above. In Comparative Example 3, the spark voltage could not be measured because the voltage could not be increased during the spark voltage evaluation.

[0082]

[0083] <Preparation of Hybrid Electrolytic Capacitors> An anode foil (chemically processed aluminum foil: 115HD-658Vf, manufactured by Nippon Capacitor Industrial Co., Ltd.) with a dielectric layer on its surface and a cathode foil (unprocessed aluminum foil: 30CB, manufactured by Nippon Capacitor Industrial Co., Ltd.) were connected to electrode tabs and placed opposite each other via a kraft paper separator to obtain an element. To repair cut surfaces and defects, the element was subjected to chemical repair at a voltage of 500 V in an ammonium borate aqueous solution, resulting in a capacitor element (theoretical capacity: 10.0 μF). The capacitor element was then vacuum-impregnated (vacuum degree: 20 mmHg) for 1 minute with a PEDOT / PSS aqueous dispersion (containing a polymer with 3,4-ethylenedioxythiophene as a constituent monomer and polystyrene sulfonic acid) (Heraeus Clevios PH500) and dried at 150°C for 30 minutes to obtain a capacitor element with a layer of solid electrolyte (C) formed on the surface of the dielectric layer. Next, the capacitor elements having a layer of solid electrolyte (C) formed on the surface of the dielectric layer were vacuum-impregnated (vacuum degree: 20 mmHg) for 1 minute at 50°C with the electrolytic solution for hybrid electrolytic capacitors obtained in Examples 1 to 17 and Comparative Examples 1 to 6. Finally, the capacitor elements having a solid electrolyte layer and impregnated with the electrolytic solution for hybrid electrolytic capacitors were housed in a case and crimped, and a load was applied by a constant current method (2 mA) at 85°C using a constant voltage / constant current DC power supply (GP0650-05R, manufactured by Takasago Machinery Works, Ltd.), and aging was performed up to 35 V, yielding hybrid electrolytic capacitors.

[0084] The resulting hybrid electrolytic capacitors were evaluated for "ESR" and "capacitance" before (initial) and after the high-temperature test using the following methods. The capacitance retention rate and ESR retention rate after the high-temperature test were calculated using the following methods. The results are shown in Table 4. In Comparative Example 3, the capacitor exploded during aging, preventing the production of a hybrid electrolytic capacitor, and therefore neither the ESR nor the capacitance could be measured. <ESR Evaluation Method> The ESR value of the hybrid electrolytic capacitors at 100 kHz was measured using an LCR meter (HIOKI E.E. Corporation, LCR HiTester 3532-50). A lower ESR value indicates a capacitor with superior operational stability. <Capacitance Evaluation Method> The capacitance of the hybrid electrolytic capacitors at 120 Hz was measured using an LCR meter (HIOKI E.E. Corporation, LCR HiTester 3532-50). <Evaluation of ESR and Capacitance After High-Temperature Test> The hybrid electrolytic capacitors were left in a thermostatic chamber set to 125°C for 500 hours. Thereafter, the ESR and capacitance of each hybrid electrolytic capacitor were evaluated using the method described above. <Calculation Method of Capacitance Retention Rate and ESR Retention Rate> The capacitance retention rate and ESR retention rate were calculated using the following formulas: Capacitance retention rate (%) = (Capacitance after high-temperature test) × 100 / (Initial capacitance) ESR retention rate (%) = (ESR value after high-temperature test) × 100 / (Initial ESR value)

[0085]

[0086] The hybrid electrolytic capacitor electrolytes of Examples 1 to 17 exhibited high withstand voltages both initially and after high-temperature testing. Furthermore, hybrid electrolytic capacitors using the hybrid electrolytic capacitor electrolytes of Examples 1 to 17 exhibited favorable initial characteristics (capacitance and ESR) and maintained favorable capacitance and ESR even after high-temperature testing. On the other hand, Comparative Examples 1 and 2 used (A'1) that did not contain a carboxylic acid (A) and had a pKa of greater than 4.5, resulting in insufficient suppression of oxidative degradation of the conductive polymer, and the capacitance and ESR of the hybrid electrolytic capacitors after high-temperature testing were significantly worsened. Comparative Example 3 used (A'2) that did not contain a carboxylic acid (A) and had a pKa of less than 1.0, resulting in failure to repair the oxide film on the anode, failure to increase the voltage in the spark voltage evaluation, and failure to produce a hybrid electrolytic capacitor due to rupture during aging. Comparative Examples 4 and 5 did not contain a carboxylic acid (A) and used acetylsalicylic acid (pKa = 4.7) or azelaic acid (pKa = 6.7), which have pKa values ​​exceeding 4.5, and therefore the effect of suppressing oxidation degradation of the conductive polymer was insufficient, resulting in significant deterioration in capacitance and ESR after high-temperature testing. Comparative Example 6 did not contain a carboxylic acid (A) and used phthalic acid, and therefore the spark voltage (withstand voltage) was insufficient.

[0087] The hybrid electrolytic capacitor using the electrolyte solution for hybrid electrolytic capacitors of the present invention suppresses an increase in ESR in high-temperature environments, and therefore can be suitably used as a component for electric and electronic products that can handle large currents. The electrolyte solution for hybrid electrolytic capacitors of the present invention is suitable for mobile applications such as laptop computers, which are susceptible to the influence of outside air temperature and tend to become hot when in operation, and is particularly suitable as an electrolyte solution for hybrid electrolytic capacitors for in-vehicle applications.

Claims

1. An electrolyte for hybrid electrolytic capacitors containing an aromatic carboxylic acid (A) having a substituent with two or more carbon atoms, the acid dissociation constant (pKa) of the carboxylic acid (A) being 1.0 to 4.5 as determined by the following measurement method. Measurement method: A 0.1 mol / L methanolic potassium hydroxide solution is dropped into a solution consisting of 1 part by weight of the carboxylic acid (A) and 99 parts by weight of methanol at 25°C, and the point with the smallest amount of dropping among the inflection points of the obtained titration curve is taken as the neutralization point. The pH at which the amount of dropping is half of the neutralization point is taken as the acid dissociation constant (pKa) of the carboxylic acid (A).

2. The electrolyte for a hybrid electrolytic capacitor according to claim 1, wherein the carboxylic acid (A) has at least one bond selected from the group consisting of an ester bond, an amide bond, an imide bond, an ether bond, a urethane bond and a urea bond.

3. The electrolyte for a hybrid electrolytic capacitor according to claim 1, wherein the carboxylic acid (A) has an ester bond.

4. The electrolyte for a hybrid electrolytic capacitor according to claim 1, wherein the content of the carboxylic acid (A) is 50 to 100% by weight based on the total weight of the acid components.

5. The electrolyte for a hybrid electrolytic capacitor according to claim 1, further comprising an alcohol (B), and the weight ratio ((B) / (A)) of the alcohol (B) to the carboxylic acid (A) is 1 to 200.

6. The electrolyte for a hybrid electrolytic capacitor according to claim 1, wherein the carboxylic acid (A) contains a carboxylic acid represented by general formula (1). [In general formula (1), R 1 represents a residue obtained by removing a hydroxy group from a monol having 2 to 10 carbon atoms which may have a substituent, a residue obtained by removing one hydroxy group from an alkylene glycol having 2 to 10 carbon atoms, a residue obtained by removing one hydroxy group from a polyalkylene glycol having an oxyalkylene unit having 2 to 6 carbon atoms, or a residue obtained by removing one hydroxy group from glycerin. n represents an integer of 1 to 5.] 7. A hybrid electrolytic capacitor comprising a capacitor element having an anode foil, a dielectric layer formed on the surface of the anode foil, and a layer of a solid electrolyte (C) in contact with the dielectric layer, wherein the capacitor element is impregnated with the electrolytic solution for a hybrid electrolytic capacitor according to any one of claims 1 to 6, and the layer of the solid electrolyte (C) contains a conductive polymer.

Citation Information

Patent Citations

  • Solid electrolytic capacitor and method of manufacturing the same

    JP2015165550A

  • Solid electrolytic capacitor and method for manufacturing solid electrolytic capacitor

    JP2017038010A

  • Process for making pulp having resistivity against mould

    JP1977001103A

  • Electrolyte for electrolytic capacitor

    JP2007042788A

  • Electrolytic capacitor

    JP2019068005A

Cited By

  • Electrolytic capacitor and electrolytic solution used for same

    WO2026094938A1