Catalyst particles, membrane electrode assembly, and fuel cell

Catalyst particles with Pt and Sn on a carbon carrier, in contact with an ionic liquid, address the durability and performance issues of conventional Pt-supported carbon catalysts by enhancing catalytic activity and reducing electronic resistance, leading to improved fuel cell IV characteristics.

WO2024214559A1PCT designated stage expired Publication Date: 2024-10-17TOPPAN HOLDINGS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012905
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-03-28
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional Pt-supported carbon catalysts in fuel cells face issues with durability due to Pt particle aggregation and elution into the electrolyte layer, leading to decreased performance, and heat treatment of Pt-SnO2 catalysts results in lower IV characteristics and increased electronic resistance.

Method used

Catalyst particles with a conductive carbon carrier and metal particles containing Pt and Sn, where at least a portion of the Sn is an oxide, are in contact with an ionic liquid, and the Pt:Sn atomic ratio is between 3:1 to 10:1, with a G/D ratio of 1.2 to 2.2, and an imidazolium salt ionic liquid, such as 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, is used to improve catalytic activity and durability.

Benefits of technology

The solution enhances the IV characteristics of fuel cells by suppressing Pt oxidation, maintaining catalytic activity, and reducing electronic resistance, resulting in improved durability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012905_17102024_PF_FP_ABST
    Figure JP2024012905_17102024_PF_FP_ABST
Patent Text Reader

Abstract

These catalyst particles each comprise a conductive carrier and metal particles that are supported by the conductive carrier. The metal particles contain Pt and Sn, some or all of Sn in the metal particles is in the form of oxide, and at least a part of the surface of each metal particle is in contact with an ionic liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst particles, membrane electrode assemblies, and fuel cells

[0001] The present invention relates to catalyst particles, a membrane electrode assembly including the catalyst particles, and a fuel cell including the membrane electrode assembly.

[0002] A known solid polymer fuel cell is one that includes an electrolyte layer formed from an ion exchange resin, a fuel-side electrode (anode) to which fuel is supplied, and an oxygen-side electrode (cathode) to which oxygen is supplied.

[0003] In such a fuel cell, fuel is supplied to the anode and air is supplied to the cathode, which generates an electromotive force and generates electricity.

[0004] For example, a Pt-supported carbon catalyst, in which Pt particles are supported on carbon, has been proposed as a cathode catalyst, but this Pt-supported carbon catalyst has a problem with durability. Specifically, the Pt particles supported on the carbon aggregate or dissolve into the electrolyte layer, which can lead to a decrease in fuel cell performance.

[0005] Patent Document 1 reports catalyst particles having carbon particles carrying Pt, with Sn oxide disposed on the Pt particles. It describes that the specific surface area of ​​the platinum particles is increased and the tin oxide on the Pt surface suppresses the aggregation of the Pt particles, resulting in both high activity and good durability.

[0006] In addition, in Non-Patent Document 1, carbon particles carrying a PtSn alloy are heat-treated to separate the Pt phase and SnO 2 By phase separation, Pt-SnO 2 SnO particles are produced. 2 They reported that electrons are donated from the Pt phase to the Pt phase, improving the activity of Pt and suppressing oxidation.

[0007] WO2014 / 136798 publication

[0008] Phase Segregated Pt-SnO2 / C Nanohybrids for Highly Efficient Oxygen Reduction Electrocatalysis, J. Guan, et al., small, 2020, 16, 2005048.

[0009] However, Pt—SnO 2 In the evaluation of power generation by a membrane electrode assembly including catalyst particles, SnO 2 is hydrophilic, making the catalyst layer more susceptible to flooding; 2 The heat treatment for forming the phase reduces the crystallinity of the carbon and increases the electronic resistance, resulting in a problem of lower IV characteristics than in a membrane electrode assembly containing Pt catalyst particles.

[0010] The present inventors have 2 We found that by contacting particles with an ionic liquid, flooding can be suppressed and IV characteristics can be improved.

[0011] In view of the above, an object of the present invention is to provide catalyst particles, a membrane electrode assembly, and a fuel cell that are excellent in IV characteristics of the membrane electrode assembly.

[0012] [1] A catalyst particle comprising a conductive support and metal particles supported on the conductive support, the metal particles containing Pt and Sn, with some or all of the Sn in the metal particles being an oxide, and at least a portion of the surface of the metal particles being in contact with an ionic liquid. [2] The catalyst particle according to [1], wherein the conductive support is formed from carbon, and the peak intensity ratio of the G band to the D band (G / D ratio) measured by Raman spectroscopy is 1.2 or more and 2.2 or less at a laser wavelength of 532 nm. [3] The catalyst particle according to [1] or [2], wherein the atomic ratio of Pt to Sn in the metal particles is in the range of 3:1 to 10:1. [4] The catalyst particle according to any one of [1] to [3], wherein the ionic liquid is an imidazolium salt. [5] The catalyst particle according to [4], wherein the ionic liquid is 1-alkyl-3-methylimidazolium bis(tolylomethanesulfonyl)imide. [6] The catalyst particles according to [4], wherein the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. [7] A membrane electrode assembly comprising a polymer electrolyte membrane and a cathode electrode catalyst layer, wherein the cathode electrode catalyst layer comprises the catalyst particles according to any one of [1] to [6]. [8] The membrane electrode assembly according to [7], wherein the cathode electrode catalyst layer further comprises a conductive auxiliary. [9] The membrane electrode assembly according to [8], wherein the conductive auxiliary is vapor-grown carbon fiber.

[10] A fuel cell comprising the membrane electrode assembly according to [7], [8], or [9].

[0013] According to one aspect of the present invention, it is possible to provide catalyst particles, a membrane electrode assembly for a fuel cell, and a fuel cell, which have excellent IV characteristics.

[0014] 1 is an explanatory diagram schematically illustrating the entire catalyst particle according to an embodiment of the present invention;

[0023] FIG. 2 is an explanatory diagram schematically illustrating the vicinity of the surface of the conductive support of FIG.

[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. <Overall Configuration of Catalyst Particle> Fig. 1 is an explanatory diagram that schematically shows the entire catalyst particle according to an embodiment of the present invention.

[0016] 1, a catalyst particle 1 according to this embodiment includes a conductive support 2, a plurality of metal particles 3 supported on the conductive support 2, and an ionic liquid 4. Each of the above components will be described in detail below.

[0017] (Conductive Support) The conductive support 2 is not particularly limited to a specific material as long as it is particles of a conductive material. The conductive support 2 is preferably carbon particles. In particular, it is preferable that the conductive support is carbon particles having a peak intensity ratio (G / D ratio) of G band to D band by Raman spectroscopy of 1.2 or more and 2.2 or less. Furthermore, the conductive support 2 is preferably carbon particles having the above-mentioned peak intensity ratio (G / D ratio) of 1.6 or more. In this embodiment, the wavelength of the laser light used in Raman spectroscopy is 532 nm. In this embodiment, the G band by Raman spectroscopy is a wavelength of 1580 cm -1 The D band in Raman spectroscopy refers to the Raman peak located around 1360 cm -1 This refers to a Raman peak located near the peak intensity ratio (G / D ratio). If the peak intensity ratio (G / D ratio) is less than 1.2, the electronic resistance is high and the degree of improvement in the IV characteristics may be small. If the peak intensity ratio (G / D ratio) is more than 2.2, the crystallinity of the carbon particles is high and it may be difficult to support metal particles.

[0018] (Metal Particles 3) The metal particles 3 used in the catalyst particles 1 contain Pt and Sn, and at least a part or all of the Sn is an oxide. The Sn oxide is SnO x The oxidation state of Sn is not particularly specified because it varies depending on the catalyst synthesis conditions, MEA production conditions, and power generation conditions, but it can be expressed as fully oxidized SnO 2 This is desirable because it is chemically stable.

[0019] The ratio (atomic ratio) of metal elements in the metal particles 3 may be Pt:Sn = 3:1 to 10:1. If the amount of Sn is greater than Pt:Sn = 3:1, Sn and its oxides themselves are not active, so the number of active Pt sites decreases and the overall catalytic activity decreases. If the amount of Sn is less than Pt:Sn = 10:1, the effect of Sn oxides on improving the activity of Pt cannot be obtained.

[0020] The metal particles 3 may have a PtSn alloy phase and a Sn oxide phase, but preferably have a Pt phase 3a and a Sn oxide phase 3b, as shown in Fig. 2. It is preferable that the metal particles 3 have a Pt phase 3a and a Sn oxide phase 3b, and that the Sn oxide phase 3b is dispersed within the Pt phase 3a.

[0021] It is preferable that at least a part of the Sn oxide phase 3 b is exposed on the surface of the metal particle 3 .

[0022] By heat treating PtSn alloy particles in an oxidizing atmosphere such as an oxygen-containing atmosphere, metal particles containing Pt and Sn having an Sn oxide phase can be obtained. In particular, when heat treatment is performed under conditions in which sufficient oxygen is present, Pt phase 3a and SnO x phase (e.g., SnO 2 The metal particles 3 separated into the metal particles (phase) 3b can be easily obtained.

[0023] PtSn alloy is heat treated to form Pt phase and SnO x By phase separation, SnO x The phase can be selectively provided on the Pt particles, and SnO x This can promote electron donation from the catalyst to Pt, thereby increasing the catalytic activity of Pt.

[0024] (Ionic Liquid) The ionic liquid is in contact with the surfaces of the metal particles 3. By having the surfaces of the Pt phase of the metal particles 3 in contact with the ionic liquid, the generation of oxides derived from water is suppressed and flooding in the membrane electrode assembly is suppressed. The ionic liquid may further be in contact with the surface and the interior of the conductive support 2.

[0025] Although there is no particular limitation on the ionic liquid 5, it is preferably an imidazolium salt. An imidazolium salt is a salt of a cation having an imidazole ring structure and a counter anion. Examples of the cation are as follows: R and R' are independently -CH 3 , -C 2 H 5 , -C 3 H 7 , -C 4 H 9 , -C6 H 13 , -CH 2 -CH=CH 2 is.

[0026] An example of a counter anion is Cl. - ,Br - , I - , BF 4 - , P.F. 6 - , FSI ((FSO 2 ) 2 N - ), TFSI((CF 3 SO 2 ) 2 N - ) is more preferable. Among these, ionic liquid 5 preferably contains 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The alkyl moiety may be methyl, ethyl, propyl, butyl, pentyl, heptyl, hexyl, octyl, nonyl, or decyl. Butyl is particularly preferable as the alkyl moiety. In other words, ionic liquid 5 is more preferably 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.

[0027] (Composition of catalyst particles) The proportion of metal particles supported in catalyst particles 1 may be 30 parts by mass or more and 60 parts by mass or less, relative to 100 parts by mass of the total of the conductive support and the metal particles. 50 parts by mass is particularly preferred. If the proportion is less than 30 parts by mass, the catalyst layer thickness of the membrane electrode assembly increases, and the IV characteristics may not improve easily. If the proportion is more than 60 parts by mass, it may become difficult to disperse and support the metal particles on the conductive support, and the metal particles may aggregate and become larger, resulting in a decrease in mass activity.

[0028] The amount of ionic liquid 5 in the catalyst particle 1 (impregnated amount of ionic liquid 5) may correspond to a volume of 15 vol% or more and 80 vol% or less of the pore volume of the conductive support 2 and the metal particles 3. More specifically, the content of ionic liquid 5 in the catalyst particle 1 is preferably within a range of 30 vol% or more and 60 vol% or less of the pore volume of the conductive support 2 and the metal particles 3 of the catalyst particle 1, and more preferably within a range of 45 vol% or more and 55 vol% or less. The pore volume in the conductive support 2 and the metal particles 3 of the catalyst particle 1 can be determined, for example, by low-temperature nitrogen adsorption. In this embodiment, the total volume of pores from 2 nm to 100 nm is used as the pore volume. If the impregnated amount of ionic liquid 5 is less than 15 vol% of the pore volume of the catalyst particle, the ionic liquid 5 may not be sufficiently effective in terms of oxygen reduction activity. Furthermore, if the amount of ionic liquid 5 impregnated is more than 80 vol% of the pore volume of the catalyst particle, the ionic liquid 5 cannot be stably retained in the catalyst particle 1, and some of the ionic liquid 5 may flow out during the manufacturing process or liquid preparation process of the catalyst particle 1, or during power generation in a fuel cell incorporating an electrode using the catalyst particle 1. Furthermore, if the amount of ionic liquid 5 impregnated is large, oxygen may be less likely to permeate from the ionic liquid layer to the surface of the metal particle, increasing resistance and possibly deteriorating IV performance.

[0029] [Method for Producing Catalyst Particles] The above catalyst particles can be produced as follows.

[0030] A conductive support carrying PtSn alloy particles is prepared. Any known synthesis method may be used. Next, the conductive support carrying PtSn alloy particles is heat-treated in an oxygen atmosphere, such as air, to obtain catalyst particles having a Pt phase or a PtSn phase and an Sn oxide phase. Increasing the heat treatment temperature promotes phase separation between the metal layer of the PtSn alloy particles and the Sn oxide phase, but this tends to decrease the G / D ratio of the conductive support. Therefore, it is preferable to appropriately adjust the heat treatment temperature and time.

[0031] Next, the conductive support carrying the catalyst particles is impregnated with an ionic liquid. Specifically, the conductive support carrying the catalyst particles is impregnated with an ionic liquid solution, and then the solvent is removed. An example of the solvent is acetonitrile. This allows the ionic liquid to adhere to the surfaces of the metal particles.

[0032] <Membrane Electrode Assembly for Fuel Cells> The membrane electrode assembly for fuel cells according to this embodiment includes a polymer electrolyte membrane and a catalyst layer (electrode catalyst layer) containing the above-described catalyst particles 1. The membrane electrode assembly for fuel cells according to this embodiment includes, for example, a polymer electrolyte membrane and a pair of catalyst layers that contain the catalyst particles 1 and sandwich the polymer electrolyte membrane from above and below. The catalyst layer on the anode side may not include the above-described catalyst particles 1, and only the catalyst layer on the cathode side may include the above-described catalyst particles 1.

[0033] The polymer electrolyte membrane is made of a polymer material having proton conductivity, and for example, a fluorine-based electrolyte membrane or a hydrocarbon-based polymer electrolyte membrane can be used. Examples of fluorine-based polymer electrolyte membranes that can be used include Nafion (registered trademark) manufactured by DuPont, Flemion (registered trademark) manufactured by Asahi Glass Co., Ltd., Aciplex (registered trademark) manufactured by Asahi Kasei Corporation, and Gore Select (registered trademark) manufactured by Gore. Examples of hydrocarbon-based polymer electrolyte membranes that can be used include electrolyte membranes made of sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, and sulfonated polyphenylene. The thickness of the polymer electrolyte membrane can be, for example, 0.05 to 0.25 mm.

[0034] The catalyst layer may further contain a conductive additive in addition to the catalyst particles. Examples of the conductive additive include vapor-grown carbon fiber (VGCF), thin-layer graphene, and carbon nanotubes (CNT), and VGCF is particularly preferred.

[0035] The content of the linear material such as VGCF in the catalyst layer is preferably in the range of 0.1 parts by mass to 45 parts by mass, more preferably in the range of 1 part by mass to 30 parts by mass, and even more preferably in the range of 10 parts by mass to 20 parts by mass, relative to 100 parts by mass of the entire catalyst layer. If the content of the fibrous material in the catalyst layer is within the above range, the catalyst layer can be endowed with even better electronic conductivity and can also contribute to maintaining the structure of the catalyst layer.

[0036] The catalyst layer may further contain an ionomer (polymer electrolyte). The ionomer in the catalyst layer may be the same type as or different from the ionomer in the polymer electrolyte membrane. The amount of ionomer used in the catalyst layer according to this embodiment may be such that the ratio of the ionomer mass to the mass of catalyst particle 1 (ionomer mass / (total mass of conductive support, metal particles, and ionic liquid)) is 0.2 or more and 0.4 or less. If this ratio is lower than 0.2, proton conduction may be insufficient, resistance may increase, and IV performance may be reduced. If the ratio is higher than 0.4, the number of pores in the catalyst layer may be reduced, resulting in insufficient water discharge and oxygen diffusion, and IV performance may be reduced.

[0037] <Fuel Cell> The fuel cell according to this embodiment includes the above-described membrane electrode assembly. The fuel cell according to this embodiment includes, for example, a pair of gas diffusion layers, each of which is arranged to face a corresponding catalyst layer of the above-described membrane electrode assembly. The gas diffusion layers and the catalyst layers form a cathode (positive electrode) and an anode (negative electrode).

[0038] (Effects of this embodiment) The catalyst particle 1 according to this embodiment has the following effects: (1) In the catalyst particle 1 and membrane electrode assembly according to this embodiment, the metal particles contain Pt and Sn, some or all of the Sn in the metal particles is an oxide, and at least a portion of the surface of the metal particles is in contact with the ionic liquid.

[0039] In this configuration, the presence of the Sn oxide phase in the metal particles suppresses oxidation of Pt, improving durability. xThe hydrophilicity of the metal particle surfaces due to the phase is suppressed, and flooding within the catalyst layer of the membrane electrode assembly can be suppressed.

[0040] (2) The electrode catalyst layer according to one example of this embodiment contains the above-described catalyst particles 1 and a conductive additive. With this configuration, the conductive additive can compensate for the decrease in electronic conductivity that accompanies the decrease in crystallinity of carbon due to heat treatment during catalyst particle synthesis.

[0041] EXAMPLES The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0042] <Synthesis of Pt particle-supported carbon (catalyst A)> Pt particle-supported carbon was synthesized according to a known method, and had a Pt loading of Pt / C=50 / 50 (wt / wt). The carbon support used had a G band / D band ratio of 1.6 or more as determined by Raman spectroscopy.

[0043] <Synthesis of PtSn alloy particle-supported carbon (catalyst B)> PtSn alloy particle-supported carbon was synthesized according to a known method, and had a PtSn loading of PtSn / C = 50 / 50 (wt / wt), and the carbon support had a G band / D band ratio of 1.6 or more as determined by Raman spectroscopy. The atomic ratio of the PtSn alloy particles was 3:1. In addition, part of the Sn in the PtSn alloy particles was partially oxidized in the working environment to form SnO. x It had become.

[0044] SnO in Pt phase 2 Synthesis of carbon (catalyst C) carrying metal particles with dispersed PtSn alloy particles> The synthesized carbon carrying PtSn alloy particles (catalyst B) is heat-treated in the atmosphere (at 200°C to 400°C for 1 hour) to dissolve SnO in the Pt phase. 2 Carbon supported with dispersed metal particles was synthesized.

[0045] Synthesis of ionic liquid-impregnated catalyst particles (catalyst D) The synthesized PtSn alloy particle-supported carbon (catalyst B) was added to acetonitrile and ultrasonically dispersed for 30 minutes, after which an ionic liquid was added in an amount of 50% of the pore volume of the PtSn alloy particle-supported carbon. After stirring overnight with a stirrer, the acetonitrile was removed with an evaporator to obtain ionic liquid-impregnated catalyst particles (catalyst D).

[0046] <Synthesis of ionic liquid-impregnated catalyst particles (Catalyst E)> SnO 2 The carbon carrying the dispersed metal particles (catalyst C) was added to acetonitrile and subjected to ultrasonic dispersion for 30 minutes, after which an ionic liquid was added in an amount of 50% of the pore volume of the carbon carrying the metal particles. After stirring overnight with a stirrer, the acetonitrile was removed with an evaporator to obtain ionic liquid-impregnated catalyst particles (catalyst E).

[0047] Example 1 Ionic liquid-impregnated catalyst particles (catalyst E) were synthesized by contacting heat-treated catalyst C with an ionic liquid according to the procedure in <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>. 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio of the carbon was evaluated by Raman spectroscopy and found to be 1.1. A catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2 The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0048] Example 2 Catalyst E was produced in the same manner as in Example 1, except that the type of carbon support used as the starting material was different. Specifically, ionic liquid-impregnated catalyst particles (catalyst E) were synthesized by contacting Catalyst C, which had been heat-treated, with an ionic liquid according to <Synthesis of Ionic Liquid-Impregnated Catalyst Particles (Catalyst E)>. 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio was evaluated to be 1.2 by Raman spectroscopy. A catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2 The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0049] Example 3 Catalyst E was produced in the same manner as in Example 1, except that the type of supported carbon used as the starting material was different. Specifically, ionic liquid-impregnated catalyst particles were synthesized by contacting Catalyst C, which had been heat-treated, with an ionic liquid according to <Synthesis of Ionic Liquid-Impregnated Catalyst Particles (Catalyst E)>. 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio was evaluated to be 1.7 by Raman spectroscopy. A catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (Catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0050] Example 4: Following the procedure described in <Synthesis of Ionic Liquid-Impregnated Catalyst Particles (Catalyst D)>, ionic liquid was brought into contact with PtSn alloy particle-supported carbon (Catalyst B) that had not been heat-treated, to synthesize ionic liquid-impregnated catalyst particles (Catalyst D). The ionic liquid used was 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The PtSn alloy particles had a Pt:Sn atomic ratio of 3:1. The G / D ratio was evaluated by Raman spectroscopy and was found to be 2.0. A catalyst ink was prepared by adding the ionic liquid-impregnated catalyst particles (Catalyst D) and an ionomer to a mixed solution containing water, IPA, and ethanol, without adding VGCF. An electrolyte membrane containing 0.2 mg / cm of platinum was coated. 2 The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0051] Example 5 Catalyst E was produced in the same manner as in Example 4, except that the type of carbon support used as the starting material was different. Specifically, ionic liquid-impregnated catalyst particles (Catalyst D) were synthesized by contacting an ionic liquid with PtSn alloy particle-supported carbon (Catalyst B) that had not been heat-treated, according to the procedure described in <Synthesis of Ionic Liquid-Impregnated Catalyst Particles (Catalyst D)>. The ionic liquid used was 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The PtSn alloy particles used had a Pt:Sn atomic ratio of 3:1. The G / D ratio was evaluated by Raman spectroscopy and was found to be 2.2. A catalyst ink was prepared by adding the ionic liquid-impregnated catalyst particles (Catalyst D) and an ionomer to a mixed solution containing water, IPA, and ethanol, without adding VGCF. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2 The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0052] Example 6 Catalyst E was produced in the same manner as in Example 2, except that the atomic ratio of the starting PtSn alloy particles was different. Specifically, ionic liquid-impregnated catalyst particles (catalyst E) were synthesized by contacting Catalyst C, which had been heat-treated, with an ionic liquid according to <Synthesis of Ionic Liquid-Impregnated Catalyst Particles (Catalyst E)>. 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 2:1. The G / D ratio was evaluated by Raman spectroscopy and found to be 1.2. A catalyst ink was prepared by adding the ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0053] Example 7 Catalyst E was produced in the same manner as in Example 2, except that the atomic ratio of the starting PtSn alloy particles was different. Specifically, ionic liquid-impregnated catalyst particles (Catalyst E) were synthesized by contacting Catalyst C, which had been heat-treated, with an ionic liquid according to <Synthesis of Ionic Liquid-Impregnated Catalyst Particles (Catalyst E)>. The ionic liquid used was 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The atomic ratio of Pt to Sn in the metal particles was 10:1. The G / D ratio was evaluated by Raman spectroscopy and found to be 1.2. A catalyst ink was prepared by adding ionic liquid-impregnated catalyst particles (Catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2 The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0054] Example 8 Catalyst E was produced in the same manner as in Example 2, except that the atomic ratio of the starting PtSn alloy particles was different. Specifically, ionic liquid-impregnated catalyst particles (catalyst E) were synthesized by contacting Catalyst C, which had been heat-treated, with an ionic liquid according to the procedure described in <Synthesis of Ionic Liquid-Impregnated Catalyst Particles (Catalyst E)>. The ionic liquid used was 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The atomic ratio of Pt to Sn in the metal particles was 11:1. The G / D ratio was evaluated as 1.2 by Raman spectroscopy. A catalyst ink was prepared by adding the ionic liquid-impregnated catalyst particles (catalyst E), ionomer, and VGCF to a mixed solution containing water, IPA, and ethanol. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2 The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0055] Example 9 Ionic liquid-impregnated catalyst particles (catalyst E) were produced in the same manner as in Example 2. Specifically, ionic liquid-impregnated catalyst particles (catalyst E) were synthesized by contacting Catalyst C, which had been heat-treated, with an ionic liquid according to the procedure described in <Synthesis of ionic liquid-impregnated catalyst particles (catalyst E)>. 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide was used as the ionic liquid. The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio was evaluated by Raman spectroscopy and was found to be 1.2. A catalyst ink was prepared by adding the ionic liquid-impregnated catalyst particles (catalyst E) and an ionomer to a mixed solution containing water, IPA, and ethanol, without adding VGCF. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0056] Comparative Example 1: Pt-supported carbon (catalyst A) was synthesized according to the procedure in <Synthesis of Pt-supported carbon (catalyst A)>. The G / D ratio was evaluated by Raman spectroscopic analysis and found to be 1.7. A catalyst ink was prepared by adding Pt-supported carbon (catalyst A) and an ionomer to a mixed solution containing water, IPA, and ethanol, without adding VGCF. An electrolyte membrane was prepared with a platinum content of 0.2 mg / cm. 2 The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0057] (Comparative Example 2) <SnO in Pt phase> 2 Heat treatment was performed according to the procedure described in "Synthesis of Carbon Supported with Metal Particles Dispersed in a Phase (Catalyst C)" to synthesize catalyst particles (Catalyst C). The atomic ratio of Pt to Sn in the metal particles was 3:1. The G / D ratio was evaluated by Raman spectroscopic analysis and found to be 1.2. A catalyst ink was prepared by adding the catalyst particles (Catalyst C) and an ionomer to a mixed solution containing water, IPA, and ethanol without adding VGCF. An electrolyte membrane containing 0.2 mg / cm of platinum was coated. 2The catalyst ink was then applied to the electrolyte membrane on the opposite side of the cathode catalyst layer so that the platinum amount was 0.05 mg / cm. ... 2 The catalyst ink was applied so that the thickness of the anode electrode became 100 μm and then dried to prepare an anode-side catalyst layer, thereby preparing a membrane electrode assembly.

[0058] <Membrane Electrode Assembly Evaluation> The prepared membrane electrode assembly, gasket, and GDL (Gas Diffusion Layer) were each incorporated into a JARI standard cell, and the IV characteristics were evaluated under the power generation conditions described in "Common Fundamental Technology for Cell Evaluation and Analysis" in the "Promotion of Practical Use of Polymer Electrolyte Fuel Cells" technical development project by NEDO. A durability test was conducted using a load response of 6,000 cycles, as described in "Common Fundamental Technology for Cell Evaluation and Analysis" in the "Promotion of Practical Use of Polymer Electrolyte Fuel Cells" technical development project by the New Energy and Industrial Technology Development Organization (NEDO). After the durability test, the IV characteristics were evaluated again.

[0059]

[0060] The columns "Voltage before endurance" and "Voltage after endurance" in Table 1 show voltages of 1.5 A / cm in IV measurements before and after the durability test for Examples 1 to 9 and Comparative Example 2. 2 The values ​​shown are comparisons of the voltage at this time with the voltage in Comparative Example 1. Examples in which the voltage was improved by 50 mV or more compared to Comparative Example 1 are marked with a double circle, examples in which the voltage was improved by the same amount to 50 mV or less are marked with a circle, and examples in which the voltage was lower than in Comparative Example 1 are marked with an x.

[0061] Compared to Comparative Example 2, Examples 1 to 9 show that impregnating catalyst particles with an ionic liquid improves the voltage before and after endurance testing. Furthermore, they show that the pre-endurance voltage is further improved when the G / D ratio of the carbon used as the conductive support is in the range of 1.2 to 2.2. Furthermore, Examples 2 and 9 show that the pre-endurance voltage is improved when VGCF is added as a conductive auxiliary. Examples 2, 6, 7, and 8 show that the pre-endurance voltage is further improved when the Pt:Sn element ratio is in the range of 3:1 to 10:1.

[0062] The fuel cell electrode material according to the present invention is used as an electrode for power sources for various portable electronic devices, automobiles, and household electrical appliances.

[0063] 1... catalyst particles, 2... conductive support (carbon), 3... metal particles, 4... ionic liquid

Claims

1. A catalyst particle comprising a conductive support and metal particles supported on the conductive support, the metal particles containing Pt and Sn, some or all of the Sn in the metal particles being an oxide, and at least a portion of the surface of the metal particles being in contact with an ionic liquid.

2. The catalyst particles according to claim 1, wherein the conductive support is made of carbon, and the peak intensity ratio (G / D ratio) of G band to D band by Raman spectroscopy is 1.2 or more and 2.2 or less at a laser wavelength of 532 nm.

3. The catalyst particles according to claim 1 or 2, wherein the atomic ratio of Pt to Sn in the metal particles is in the range of 3:1 to 10:

1.

4. The catalyst particles according to claim 1 or 2, wherein the ionic liquid is an imidazolium salt.

5. The catalyst particles according to claim 4, wherein the ionic liquid is 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.

6. The catalyst particles according to claim 4, wherein the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.

7. A membrane electrode assembly comprising a polymer electrolyte membrane and a cathode side electrode catalyst layer, the cathode side electrode catalyst layer comprising the catalyst particles according to claim 1 or 2.

8. The membrane electrode assembly according to claim 7, wherein the cathode side electrode catalyst layer further contains a conductive auxiliary.

9. The membrane electrode assembly of claim 8, wherein said conductive aid is vapor grown carbon fiber.

10. A fuel cell comprising the membrane electrode assembly of claim 7.

Citation Information

Patent Citations

  • Catalyst for solid polymer fuel cell cathodes and method for producing catalyst for solid polymer fuel cell cathodes

    WO2014136798A1

  • Catalyst layer for fuel cell, catalyst layer for fuel cell provided with substrate using the same, gas diffusion electrode for fuel cell, laminate of catalyst layer for fuel cell and electrolyte membrane, membrane electrode assembly for fuel cell, fuel cell and method for producing the same

    JP2012216313A

  • Coated fuel cell catalyst materials

    JP2022128440A

  • Substrate processing apparatus