Electrode binder for secondary battery including secondary-battery electrodes including carbon nanotubes, and uses thereof
The use of a binder with carboxyl group-containing non-crosslinked polymers and carbon nanotubes addresses the issue of volume changes in silicon-based secondary battery electrodes, enhancing durability and capacity retention by maintaining conductive paths and improving cycle characteristics.
Patent Information
- Application Number
- PCT/JP2024/014034
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-04-05
- Publication Date
- 2024-10-17
AI Technical Summary
Secondary battery electrodes with silicon-based active materials face challenges due to large volume changes during charging and discharging, leading to capacity deterioration and reduced durability, as the conductive paths between active materials are disrupted, resulting in poor capacity retention rates.
A binder for secondary battery electrodes containing carboxyl group-containing non-crosslinked polymers or their salts, combined with carbon nanotubes, is used to enhance binding properties and maintain conductive paths, allowing for higher cycle counts and improved charge/discharge capacity retention.
The binder composition effectively suppresses expansion and contraction of silicon-based active materials, maintaining conductive paths and improving the durability and cycle characteristics of secondary batteries, enabling longer battery life and higher capacity retention.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Electrode binder for secondary battery having secondary battery electrode containing carbon nanotubes and use thereof
[0001] The present invention relates to a binder for electrodes of a secondary battery having a secondary battery electrode containing carbon nanotubes, and to the use of the binder.
[0002] Various secondary batteries, such as nickel-metal hydride secondary batteries, lithium-ion secondary batteries, and electric double layer capacitors, have been put to practical use. Electrodes used in these secondary batteries are prepared by applying a composition for forming an electrode mixture layer containing an active material and a binder to a current collector, followed by drying. For example, in lithium-ion secondary batteries, an aqueous binder containing styrene butadiene rubber (SBR) latex and carboxymethyl cellulose (CMC) is used as the binder for the negative electrode mixture layer composition. Furthermore, binders containing aqueous solutions or dispersions of acrylic acid-based polymers are known as binders with excellent dispersibility and binding properties. Meanwhile, a solution of polyvinylidene fluoride (PVDF) in N-methyl-2-pyrrolidone (NMP) is widely used as the binder for the positive electrode mixture layer.
[0003] In recent years, as the applications of various secondary batteries have expanded, there has been a growing demand for improved energy density, reliability, and durability. For example, in order to increase the electrical capacity of lithium-ion secondary batteries, specifications using silicon-based active materials as negative electrode active materials have become more common. However, silicon-based active materials are known to undergo large volume changes during charge and discharge, and repeated use can lead to peeling or detachment of the electrode mixture layer, resulting in a decrease in battery capacity and deterioration of cycle characteristics (durability). In order to prevent such problems, it is generally effective to increase the binding properties of the binder, and studies on improving the binding properties of binders have been conducted with the aim of improving durability.
[0004] Binders using the above-mentioned acrylic acid-based polymers have been proposed as binders that have good binding properties and are effective in improving durability, and it is known that adding a conductive additive to a slurry for producing a negative electrode improves electrical contact between active materials and improves battery performance.
[0005] For example, Patent Documents 1 and 2 disclose that an electrode obtained from an electrode mixture layer composition containing a silicon-containing active material, a conductive additive, and a binder containing a monomer unit derived from acrylic acid and a monomer unit with a specific structure has excellent charge / discharge capacity. They specifically describe that the use of ketjen black or acetylene black as the conductive additive results in a high capacity retention rate after 10 or 30 charge / discharge cycles.
[0006] International Publication No. 2015 / 163302 Japanese Patent Application Laid-Open No. 2018-029069
[0007] The binders disclosed in Patent Documents 1 and 2 are both capable of imparting good binding properties, and as described above, can achieve a high capacity retention rate if the number of charge / discharge cycles is as small as about 10 to 30. However, with repeated charge / discharge cycles, the structure of the negative electrode deteriorates significantly due to expansion and contraction of the silicon-based active material, making it impossible to maintain a conductive path between the active materials, resulting in a problem of capacity deterioration.
[0008] The present invention has been made in view of the above circumstances, and aims to provide a binder for secondary battery electrodes that can suppress expansion and contraction due to charge and discharge and exhibit a high capacity retention rate over longer periods of use than conventional binders, even when using a silicon-based active material that is known to undergo large expansion and contraction due to charge and discharge. It is also an object of the present invention to provide a composition for secondary battery electrode mixture layers that contains the binder, and a secondary battery electrode and secondary battery obtained using the composition.
[0009] As a result of intensive research to solve the above-mentioned problems, the present inventors have found that by using a binder containing a carboxyl group-containing non-crosslinked polymer or a salt thereof as an electrode binder for a secondary battery having a secondary battery electrode containing carbon nanotubes (hereinafter also referred to as "CNTs") as a conductive additive, and by setting the degree of neutralization of the polymer to a specific value or more, it is possible to suppress expansion and contraction due to charge and discharge, and to exhibit an excellent charge and discharge capacity retention rate, even when the secondary battery is used at a higher number of cycles than conventionally, and have completed the present invention.
[0010] The present invention is as follows. [1] An electrode binder for a secondary battery having a secondary battery electrode containing carbon nanotubes, the electrode binder containing a carboxyl group-containing non-crosslinked polymer or a salt thereof, the degree of neutralization of the polymer being 50 mol% or more. [2] The electrode binder according to [1], wherein the carboxyl group-containing non-crosslinked polymer contains structural units derived from ethylenically unsaturated carboxylic acid monomers in an amount of 50 mass% or more and 100 mass% or less based on the total structural units of the carboxyl group-containing non-crosslinked polymer. [3] A composition for a secondary battery electrode mixture layer, comprising the electrode binder according to [1] or [2], carbon nanotubes, an active material, and water. [4] The composition for a secondary battery electrode mixture layer according to [3], wherein the content of the silicon active material is 5.0 mass% or more based on the total amount of the active material. [5] The composition for a secondary battery electrode mix layer according to [3] or [4], wherein the content of the electrode binder is 1.0 part by mass or more and 2.5 parts by mass or less, relative to 100 parts by mass of the total amount of the active material. [6] The composition for a secondary battery electrode mix layer according to any one of [3] to [5], wherein the content of the carbon nanotubes is 0.1 part by mass or more, relative to 100 parts by mass of the total amount of the active material. [7] The composition for a secondary battery electrode mix layer according to any one of [3] to [6], wherein the carbon nanotubes have a single-layer structure. [8] A secondary electrode comprising, on a surface of a current collector, a mix layer formed from the composition for a secondary battery electrode mix layer according to any one of [3] to [7]. [9] A secondary battery comprising the secondary electrode according to [8].
[0011] The electrode binder of the present invention makes it possible to obtain a secondary battery that exhibits an excellent charge / discharge capacity retention rate while suppressing expansion and contraction due to charge / discharge cycles during use for a longer period than conventional batteries.
[0012] The binder for secondary battery electrodes of the present invention (hereinafter also referred to as "the binder") contains a carboxyl group-containing non-crosslinked polymer (hereinafter also referred to as "the non-crosslinked polymer") or a salt thereof (hereinafter also referred to as "the non-crosslinked polymer salt"), and can be mixed with carbon nanotubes (hereinafter also referred to as "CNTs"), an active material, and water to form a composition for secondary battery electrode mixture layers (hereinafter also referred to as "the composition"). The composition is preferably in the form of an electrode slurry that can be applied to a current collector, in order to achieve the effects of the present invention. However, it may also be prepared in the form of a wet powder so that it can be pressed onto the current collector surface. The secondary battery electrode of the present invention is obtained by forming a mixture layer from the composition on the surface of a current collector such as copper foil or aluminum foil. Here, the binder is preferably used in a composition for secondary battery electrode mixture layers that contains a silicon-based active material as described below as the active material, in that the effects of the present invention are particularly significant.
[0013] The carbon nanotubes, the present non-crosslinked polymer and its manufacturing method, the composition for a secondary battery electrode mixture layer obtained using the present binder, the secondary battery electrode, and the secondary battery are each described in detail below. In this specification, "(meth)acrylic" means acrylic and / or methacrylic, and "(meth)acrylate" means acrylate and / or methacrylate. Furthermore, "(meth)acryloyl group" means acryloyl group and / or methacryloyl group. In the numerical ranges described in this specification in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages, and the upper or lower limit value of that numerical range may be replaced with a value shown in the examples.
[0014] 1. Carbon Nanotubes The carbon nanotubes (CNTs) used in the present composition have high conductivity and chemical stability and are used as a conductive additive to ensure electrical contact between active materials in the electrode mixture layer. CNTs have a cylindrical shape formed by rolling planar graphite. The type of CNT is not particularly limited, and single-walled CNTs (hereinafter also referred to as "single-walled CNTs") or multi-walled CNTs (hereinafter also referred to as "multi-walled CNTs") can be used. These can be used alone or in combination of two or more types. Single-walled CNTs are preferred as CNTs, as they provide particularly significant benefits. Single-walled CNTs have a structure in which one layer of graphite is rolled, while multi-walled CNTs have a structure in which two or more layers of graphite are rolled. The sidewalls of the CNTs do not have to have a graphite structure; CNTs with sidewalls having an amorphous structure are also considered CNTs in this specification.
[0015] The shape of the CNTs is not limited. Examples of such shapes include needle-like, cylindrical tubular, fishbone-like (fishbone or cup stacked), trump-like (platelet), and coil-like. Of these, needle-like or cylindrical tubular shapes are preferred. The CNTs may have a single shape or a combination of two or more shapes.
[0016] Examples of the form of CNT include graphite whiskers, filamentous carbon, graphite fibers, ultrafine carbon tubes, carbon tubes, carbon fibrils, carbon microtubes, and carbon nanofibers. CNT may have any one of these forms or a combination of two or more of these forms.
[0017] The average outer diameter of the CNTs is preferably 1 nm or more, more preferably 5 nm or less, and even more preferably 3 nm or less. The average outer diameter of the CNTs can be calculated by first observing and photographing the CNTs using a transmission electron microscope, randomly selecting 300 CNTs from the photograph, and measuring the outer diameter of each.
[0018] The average fiber length of the CNTs is preferably 0.5 μm or more, more preferably 0.8 μm or more, more preferably 1.0 μm or more, and even more preferably 5.0 μm or more. It is also preferably 20 μm or less, and more preferably 10 μm or less. The average fiber length of the CNTs can be calculated by first observing and photographing the CNTs using a scanning electron microscope, randomly selecting 300 CNTs from the photograph, and measuring the fiber length of each.
[0019] The aspect ratio is the value obtained by dividing the fiber length of CNT by the outer diameter. A typical aspect ratio can be calculated using the average fiber length and the average outer diameter. The higher the aspect ratio of a conductive additive, the higher the conductivity that can be obtained when an electrode is formed. The aspect ratio of CNT is preferably 30 or more, more preferably 50 or more, and even more preferably 80 or more. In addition, it is preferably 10,000 or less, more preferably 3,000 or less, and even more preferably 1,000 or less.
[0020] The specific surface area of CNT is 100m 2 / g or more, and 2 / g or more is more preferable, and 200m 2 / g or more is more preferable. 2 / g or less, and 2 / g or less is more preferable. The specific surface area of the CNTs can be calculated by the BET method using nitrogen adsorption measurements. When the average outer diameter, average fiber length, aspect ratio, and specific surface area of the CNTs are within the above ranges, they are likely to form well-developed conductive paths in the electrode.
[0021] The carbon purity of CNT is expressed as the content (mass%) of carbon atoms in the CNT. The carbon purity is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 98 mass% or more, relative to 100 mass% of CNT. By keeping the carbon purity within the above range, problems such as short circuits caused by the formation of dendrites due to impurities such as metal catalysts can be prevented.
[0022] The CNT may be surface-treated CNT, or a CNT derivative to which a functional group such as a carboxyl group has been added. Alternatively, CNT containing an organic compound, a metal atom, or a substance such as fullerene may also be used.
[0023] CNTs can be produced by, but are not limited to, laser ablation, arc discharge, thermal CVD, plasma CVD, and combustion. For example, CNTs can be produced by catalytically reacting a carbon source with a catalyst at 500 to 1000°C in an atmosphere with an oxygen concentration of 1% by volume or less. The carbon source may be at least one of a hydrocarbon and an alcohol.
[0024] 2. The Non-Crosslinked Polymer The non-crosslinked polymer can have a structural unit derived from an ethylenically unsaturated carboxylic acid monomer (hereinafter also referred to as "component (a)"), and can be introduced into the polymer by polymerizing a monomer component containing component (a).
[0025] <Structural Units Derived from Ethylenically Unsaturated Carboxylic Acid Monomers> The carboxyl group-containing non-crosslinked polymer (the present non-crosslinked polymer) contained in the present binder may have a structural unit derived from an ethylenically unsaturated carboxylic acid monomer (hereinafter also referred to as "component (a)"). When the present non-crosslinked polymer has such a structural unit and thus a carboxyl group, the adhesion to the current collector is improved, and the lithium ion desolvation effect and ionic conductivity are excellent, resulting in an electrode with low resistance and excellent high-rate characteristics. Furthermore, since the polymer chain adopts an extended conformation in water, it is believed that the dispersion stability of the active material, etc. in the present composition can be improved. The above-mentioned component (a) can be introduced into the polymer, for example, by polymerizing a monomer containing an ethylenically unsaturated carboxylic acid monomer. Alternatively, it can be obtained by (co)polymerizing a (meth)acrylic acid ester monomer and then hydrolyzing it. Alternatively, (meth)acrylamide, (meth)acrylonitrile, etc. may be polymerized and then treated with a strong alkali, or a method in which a polymer having a hydroxyl group is reacted with an acid anhydride may be used.
[0026] Examples of ethylenically unsaturated carboxylic acid monomers include (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, and fumaric acid; (meth)acrylamidoalkylcarboxylic acids such as (meth)acrylamidohexanoic acid and (meth)acrylamidododecanoic acid; and carboxyl group-containing ethylenically unsaturated monomers such as monohydroxyethyl succinate (meth)acrylate, ω-carboxy-caprolactone mono(meth)acrylate, and β-carboxyethyl (meth)acrylate, or their (partially) alkali-neutralized products. One of these may be used alone, or two or more may be used in combination. Among these, compounds having an acryloyl group as a polymerizable functional group are preferred, with acrylic acid being particularly preferred, because they have a high polymerization rate, resulting in a polymer with a long primary chain length and good binder binding strength. When acrylic acid is used as the ethylenically unsaturated carboxylic acid monomer, a polymer with a high carboxyl group content can be obtained.
[0027] The content of component (a) in the non-crosslinked polymer can be 50% by mass or more and 100% by mass or less, based on the total structural units of the non-crosslinked polymer. By including component (a) in this range, excellent adhesion to the current collector can be easily ensured. A lower limit of 50% by mass or more is preferable because the dispersion stability of the composition is improved and a higher binding strength can be obtained. It may be 60% by mass or more, 70% by mass or more, or even 80% by mass or more. The upper limit is, for example, 99.9% by mass or less, for example, 99.5% by mass or less, for example, 99% by mass or less, for example, 98% by mass or less, for example, 95% by mass or less, for example, 90% by mass or less, or for example, 80% by mass or less.
[0028] <Other Structural Units> In addition to component (a), the present non-crosslinked polymer may contain a structural unit (hereinafter also referred to as "component (b)") derived from another ethylenically unsaturated monomer copolymerizable therewith. Examples of component (b) include structural units derived from hydroxyl group-containing ethylenically unsaturated monomers (monomers represented by the following formula (1) and formula (2)), ethylenically unsaturated monomer compounds having anionic groups other than carboxyl groups such as sulfonic acid groups and phosphoric acid groups, or nonionic ethylenically unsaturated monomers. These structural units can be introduced by copolymerizing a monomer containing a hydroxyl group-containing ethylenically unsaturated monomer, an ethylenically unsaturated monomer compound having anionic groups other than carboxyl groups such as sulfonic acid groups and phosphoric acid groups, or a nonionic ethylenically unsaturated monomer. CH 2 = C(R 1 ) COOR 2 (1) [wherein, R 1 represents a hydrogen atom or a methyl group, R 2 represents a monovalent organic group having 1 to 8 carbon atoms and a hydroxyl group, (R 3 O) m H or R 4 O[CO(CH 2 ) 5 O] n H. Note that R 3 represents an alkylene group having 2 to 4 carbon atoms, R 4represents an alkylene group having 1 to 8 carbon atoms, m represents an integer of 2 to 15, and n represents an integer of 1 to 15.] CH 2 = C(R 5 ) CONR 6 R 7 (2) [wherein, R 5 represents a hydrogen atom or a methyl group, R 6 represents a hydroxyl group or a hydroxyalkyl group having 1 to 8 carbon atoms, R 7 represents a hydrogen atom or a monovalent organic group.
[0029] The proportion of the (b) component can be 0% by mass or more and 50% by mass or less relative to the total structural units of the non-crosslinked polymer. The proportion of the (b) component may be 0.1% by mass or more and 40% by mass or less, 0.5% by mass or more and 30% by mass or less, 1.0% by mass or more and 20% by mass or less, 2% by mass or more and 12.5% by mass or less, or 3% by mass or more and 10% by mass or less. Furthermore, when the (b) component is contained in an amount of 0.1% by mass or more relative to the total structural units of the non-crosslinked polymer, the affinity for the electrolyte solution is improved, and therefore, the effect of improving lithium ion conductivity can also be expected.
[0030] Among the above-mentioned components, the (b) component is preferably a hydroxyl group-containing ethylenically unsaturated monomer, because it provides excellent binding properties for a binder containing the present non-crosslinked polymer salt. Furthermore, a structural unit derived from a nonionic ethylenically unsaturated monomer is preferred, because it provides an electrode with good flex resistance. Examples of nonionic ethylenically unsaturated monomers include (meth)acrylamide and its derivatives, nitrile group-containing ethylenically unsaturated monomers, and alicyclic structure-containing ethylenically unsaturated monomers.
[0031] The monomer represented by the above formula (1) is a (meth)acrylate compound having a hydroxyl group. 2 When R is a monovalent organic group having 1 to 8 carbon atoms and a hydroxyl group, the number of the hydroxyl groups may be one or more. The monovalent organic group is not particularly limited, but examples thereof include alkyl groups which may have a linear, branched, or cyclic structure, as well as aryl groups and alkoxyalkyl groups. 2(R 3 O) m H or R 4 O[CO(CH 2 ) 5 O] n If H, then R 3 or R 4 The alkylene group represented by may be linear or branched.
[0032] Examples of the monomer represented by the formula (1) include hydroxyalkyl (meth)acrylates having a hydroxyalkyl group having 1 to 8 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, and hydroxyoctyl (meth)acrylate; polyalkylene glycol mono(meth)acrylates, such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polybutylene glycol mono(meth)acrylate, and polyethylene glycol-polypropylene glycol mono(meth)acrylate; dihydroxyalkyl (meth)acrylates, such as glycerin mono(meth)acrylate; caprolactone-modified hydroxymethacrylates (manufactured by Daicel Corporation, trade names "PLACCEL FM1," "PLACCEL FM5," etc.), caprolactone-modified hydroxyacrylates (manufactured by Daicel Corporation, trade names "PLACCEL FA1," "PLACCEL FA10L," etc.). The monomer represented by the formula (1) may be used singly or in combination of two or more.
[0033] The monomer represented by the formula (2) is a (meth)acrylamide derivative having a hydroxyl group or a hydroxyalkyl group having 1 to 8 carbon atoms. 7 represents a hydrogen atom or a monovalent organic group. The monovalent organic group is not particularly limited, but examples thereof include alkyl groups which may have a linear, branched, or cyclic structure, as well as aryl groups and alkoxyalkyl groups, and is preferably an organic group having 1 to 8 carbon atoms. In addition, R 7may be a hydroxyl group or a hydroxyalkyl group having 1 to 8 carbon atoms.
[0034] Examples of the monomer represented by formula (2) include hydroxy(meth)acrylamide; (meth)acrylamide derivatives having a hydroxyalkyl group having 1 to 8 carbon atoms, such as N-hydroxyethyl(meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, N-hydroxybutyl(meth)acrylamide, N-hydroxyhexyl(meth)acrylamide, and N-hydroxyoctyl(meth)acrylamide, N-methylhydroxyethyl(meth)acrylamide, and N-ethylhydroxyethyl(meth)acrylamide; and N,N-dihydroxyalkyl(meth)acrylamides, such as N,N-dihydroxyethyl(meth)acrylamide and N,N-dihydroxyethyl(meth)acrylamide. The monomer represented by formula (2) may be used singly or in combination of two or more.
[0035] Examples of the (meth)acrylamide derivative include N-alkyl(meth)acrylamide compounds such as N-isopropyl(meth)acrylamide and N-t-butyl(meth)acrylamide; N-alkoxyalkyl(meth)acrylamide compounds such as N-n-butoxymethyl(meth)acrylamide and N-isobutoxymethyl(meth)acrylamide; and N,N-dialkyl(meth)acrylamide compounds such as N,N-dimethyl(meth)acrylamide and N,N-diethyl(meth)acrylamide. These may be used alone or in combination of two or more.
[0036] Examples of the nitrile group-containing ethylenically unsaturated monomer include (meth)acrylonitrile; (meth)acrylic acid cyanoalkyl ester compounds such as cyanomethyl (meth)acrylate and cyanoethyl (meth)acrylate; cyano group-containing unsaturated aromatic compounds such as 4-cyanostyrene and 4-cyano-α-methylstyrene; vinylidene cyanide; and the like. One of these may be used alone, or two or more may be used in combination. Of the above, acrylonitrile is preferred because of its high nitrile group content.
[0037] Examples of the alicyclic structure-containing ethylenically unsaturated monomer include (meth)acrylic acid cycloalkyl esters which may have an aliphatic substituent, such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, cyclodecyl (meth)acrylate, and cyclododecyl (meth)acrylate; isobornyl (meth)acrylate, adamantyl (meth)acrylate, cyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and cycloalkyl polyalcohol mono(meth)acrylates such as cyclohexanedimethanol mono(meth)acrylate and cyclodecanedimethanol mono(meth)acrylate; and the like. These may be used alone or in combination of two or more.
[0038] In view of the excellent binding properties of the binder, the present non-crosslinked polymer preferably contains structural units derived from the monomer represented by the above formula (1), the monomer represented by the above formula (2), (meth)acrylamide and its derivatives, nitrile group-containing ethylenically unsaturated monomers, alicyclic structure-containing ethylenically unsaturated monomers, etc. Among these, as component (b), structural units derived from the monomer represented by the above formula (1) and the monomer represented by the above formula (2) are more preferred in view of the excellent effect of improving the binding properties of the present binder. Among the monomers represented by the above formula (1), hydroxyalkyl (meth)acrylates having a hydroxyalkyl group having 1 to 8 carbon atoms are more preferred, and 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are even more preferred. Furthermore, among the monomers represented by the above formula (2), (meth)acrylamide derivatives having a hydroxyalkyl group having 1 to 8 carbon atoms are more preferred, and N-hydroxyethyl(meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, and N-hydroxybutyl(meth)acrylamide are even more preferred.
[0039] Furthermore, when a structural unit derived from a hydrophobic ethylenically unsaturated monomer having a solubility in water of 1 g / 100 ml or less is introduced as component (b), it can exhibit strong interaction with the electrode material and exhibit good binding properties to the active material. This allows for a firm and well-integrated electrode mixture layer to be obtained, and therefore, as the "hydrophobic ethylenically unsaturated monomer having a solubility in water of 1 g / 100 ml or less," an alicyclic structure-containing ethylenically unsaturated monomer is particularly preferred.
[0040] Other nonionic ethylenically unsaturated monomers that may be used include, for example, (meth)acrylic acid esters. Examples of (meth)acrylic acid esters include (meth)acrylic acid alkyl ester compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; aromatic (meth)acrylic acid ester compounds such as phenyl (meth)acrylate, phenylmethyl (meth)acrylate, phenylethyl (meth)acrylate, and phenoxyethyl (meth)acrylate; and (meth)acrylic acid alkoxyalkyl ester compounds such as 2-methoxyethyl (meth)acrylate and 2-ethoxyethyl (meth)acrylate. These may be used alone or in combination of two or more.
[0041] From the viewpoints of binding strength with the active material and cycle characteristics, aromatic (meth)acrylic acid ester compounds are preferably used. From the viewpoints of further improving lithium ion conductivity and high-rate characteristics, compounds having an ether bond, such as (meth)acrylic acid alkoxyalkyl esters such as 2-methoxyethyl (meth)acrylate and 2-ethoxyethyl (meth)acrylate, are preferred, with 2-methoxyethyl (meth)acrylate being more preferred.
[0042] Among nonionic ethylenically unsaturated monomers, compounds having an acryloyl group are preferred because they have a fast polymerization rate, resulting in a polymer with a long primary chain length, and provide good binder binding strength.Furthermore, as the nonionic ethylenically unsaturated monomer, compounds whose homopolymer has a glass transition temperature (Tg) of 0°C or less are preferred because the resulting electrode has good flex resistance.
[0043] The non-crosslinked polymer salt is in the form of a salt in which some or all of the carboxyl groups contained in the polymer are neutralized. The type of salt is not particularly limited, but examples include alkali metal salts such as lithium salts, sodium salts, and potassium salts; alkaline earth metal salts such as magnesium salts, calcium salts, and barium salts; other metal salts such as aluminum salts; ammonium salts, and organic amine salts. Among these, alkali metal salts and alkaline earth metal salts are preferred, and alkali metal salts are more preferred, as they are less likely to adversely affect battery characteristics.
[0044] Regarding the Characteristics of the Non-Crosslinked Polymer Salt: The non-crosslinked polymer is used in the form of a salt, in which acid groups such as carboxyl groups derived from ethylenically unsaturated carboxylic acid monomers are neutralized so that the degree of neutralization in the composition is 50 mol% or higher. By achieving a degree of neutralization of 50 mol% or higher and increasing the glass transition temperature of the carboxyl group-containing non-crosslinked polymer, fusion and aggregation of the polymer due to heating when applying an electrode mixture layer composition containing the polymer to the current collector surface and drying it can be suppressed. This is thought to maintain a uniform structure in the electrode and further enhance the effect of conductive path formation by the addition of CNTs. The degree of neutralization is more preferably 60 mol% or higher, even more preferably 70 mol% or higher, even more preferably 75 mol% or higher, even more preferably 80 mol% or higher, and particularly preferably 85 mol% or higher, in order to achieve a superior charge / discharge capacity retention rate over longer periods of use than conventional methods. The upper limit of the degree of neutralization is 100 mol%, and may be 98 mol% or 95 mol%. In this specification, the degree of neutralization can be calculated from the amounts of a monomer having an acid group such as a carboxyl group and a neutralizing agent used for neutralization. The degree of neutralization can be confirmed by measuring the powder of the crosslinked polymer salt after drying it at 80°C under reduced pressure for 3 hours, and then measuring the intensity ratio of the peak derived from the C=O group of the carboxylic acid to the peak derived from the C=O group of the carboxylate salt.
[0045] The weight average molecular weight (Mw) of the present non-crosslinked polymer is not particularly limited, but is preferably 5,000 or more, more preferably 10,000 or more, in order to exhibit superior charge / discharge capacity retention over longer periods of use than conventional polymers. Mw may be 100,000 or more, 500,000 or more, or even 1,000,000 or more. The upper limit of Mw is also not particularly limited, but from the viewpoint of handling during production, it may be, for example, 10,000,000 or less, or 5,000,000 or less. In this specification, Mw can be measured by the GPC method described in the Examples.
[0046] <Method for Producing the Present Non-Crosslinked Polymer> The present non-crosslinked polymer can be produced by known polymerization methods (solution polymerization, precipitation polymerization, suspension polymerization, emulsion polymerization, etc.), which may be appropriately selected based on the molecular weight, composition, etc. The polymerization initiator may be, but is not limited to, known polymerization initiators such as azo compounds, organic peroxides, and inorganic peroxides. The conditions for use can be adjusted to generate an appropriate amount of radicals using known methods such as thermal initiation, redox initiation using a reducing agent, and UV initiation. Furthermore, known chain transfer agents may be used as needed for the purpose of adjusting the molecular weight, etc. Here, the present non-crosslinked polymer may contain 50% by mass or more and 100% by mass or less of an ethylenically unsaturated carboxylic acid monomer. The type of ethylenically unsaturated carboxylic acid monomer is as described above.
[0047] 3. Composition for Secondary Battery Electrode Mixture Layer The composition for secondary battery electrode mixture layer of the present invention contains the binder, carbon nanotubes (CNTs), an active material, and water. The amount of the binder used in the composition is preferably 0.5 parts by mass or more and 7.0 parts by mass or less, relative to 100 parts by mass of the total amount of active material. The amount used is, for example, 0.8 parts by mass or more and 3.0 parts by mass or less, such as 1.0 parts by mass or more and 2.5 parts by mass or less, or for example, 1.2 parts by mass or more and 1.5 parts by mass or less. When the amount of binder used is 0.5 parts by mass or more, sufficient binding strength can be obtained. Furthermore, dispersion stability of the active material and the like can be ensured, and a uniform mixture layer can be formed. When the amount of binder used is 1.5 parts by mass or less, the composition does not become highly viscous, ensuring coatability to the current collector. As a result, a mixture layer with a uniform and smooth surface can be formed.
[0048] The amount of CNT used in this composition is, for example, 0.01 parts by mass or more and 0.5 parts by mass or less, relative to 100 parts by mass of the total amount of active material. The content is, for example, 0.05 parts by mass or more and 0.3 parts by mass or less, and also, for example, 0.1 parts by mass or more and 0.2 parts by mass or less. When the CNT content is 0.01 parts by mass or more, a sufficient conductive path can be formed. When the CNT content is 0.2 parts by mass or less, the composition does not become highly viscous, ensuring coatability onto the current collector. Furthermore, aggregation of the CNTs does not occur, and as a result, an electrode with a uniform and smooth surface can be formed.
[0049] Among the above active materials, lithium salts of transition metal oxides can be used as the positive electrode active material. For example, layered rock salt type and spinel type lithium-containing metal oxides can be used. Specific compounds of the layered rock salt type positive electrode active material include lithium cobalt oxide, lithium nickel oxide, and ternary NCMs {Li(Ni x , Co y , Mn z ), x+y+z=1} and NCA{Li(Ni 1-a-b Co a Al b)}, etc. Examples of spinel-type positive electrode active materials include lithium manganate, etc. In addition to oxides, phosphates, silicates, sulfur, etc. are also used, and examples of phosphates include olivine-type lithium iron phosphate, etc. As the positive electrode active material, one of the above may be used alone, or two or more may be combined and used as a mixture or composite.
[0050] When a positive electrode active material containing a layered rock salt-type lithium-containing metal oxide is dispersed in water, the lithium ions on the active material surface are exchanged with hydrogen ions in the water, resulting in an alkaline dispersion. This may result in corrosion of aluminum foil (Al), a common positive electrode current collector material. In such cases, it is preferable to neutralize the alkali eluted from the active material by using the unneutralized or partially neutralized non-crosslinked polymer as a binder. Furthermore, it is preferable to use the unneutralized or partially neutralized non-crosslinked polymer in an amount such that the amount of unneutralized carboxyl groups in the non-crosslinked polymer is equivalent to or greater than the amount of alkali eluted from the active material.
[0051] Because all positive electrode active materials have low electrical conductivity, a conductive additive other than carbon nanotubes may be added. Examples of such conductive additives include carbon-based materials such as carbon black, carbon fiber, graphite powder, and carbon fiber. Of these, carbon black and carbon fiber are preferred because they are more likely to provide excellent conductivity. Furthermore, ketjen black and acetylene black are preferred as carbon black. The conductive additives may be used alone or in combination with two or more of the above. The amount of conductive additive other than carbon nanotubes used may be, for example, 0.2 to 20 parts by mass, or, for example, 0.2 to 10 parts by mass, per 100 parts by mass of the total active material, from the viewpoint of achieving both electrical conductivity and energy density. Furthermore, the positive electrode active material may be surface-coated with a conductive carbon-based material.
[0052] On the other hand, examples of negative electrode active materials include carbon-based materials, lithium metal, lithium alloys, and metal oxides, and one or more of these can be used in combination. Among these, active materials made of carbon-based materials such as natural graphite, artificial graphite, hard carbon, and soft carbon (hereinafter also referred to as "carbon-based active materials") are preferred, with graphite such as natural graphite and artificial graphite, and hard carbon being more preferred. In the case of graphite, spherical graphite is preferably used from the standpoint of battery performance, and its particle size preferably ranges from 1 to 20 μm, for example, and from 5 to 15 μm. In addition, to increase the energy density, metals or metal oxides capable of absorbing lithium, such as silicon and tin, can also be used as negative electrode active materials. Among these, silicon has a higher capacity than graphite, and active materials made of silicon-based materials such as silicon, silicon alloys, and silicon oxides such as silicon monoxide (SiO) (hereinafter also referred to as "silicon-based active materials") can be used. The amount of silicon-based active material used is 5.0 mass% or more, for example, 10.0 mass% or more, or for example, 20.0 mass% or more, relative to the total amount of active material, in order to improve the electrical capacity of the secondary battery.
[0053] Since the carbon-based active material itself has good electrical conductivity, it is not necessary to add a conductive additive other than carbon nanotubes. When a conductive additive is added for the purpose of further reducing resistance, etc., from the viewpoint of energy density, the amount used is, for example, 10 parts by mass or less, or, for example, 5 parts by mass or less, relative to 100 parts by mass of the total amount of the active material.
[0054] When the composition is in a slurry state, the amount of active material used is, for example, in the range of 10 to 75 mass %, or, for example, in the range of 30 to 65 mass %, based on the total amount of the composition. If the amount of active material used is 10 mass % or more, migration of binders and the like is suppressed, and this is also advantageous in terms of the cost of drying the medium. On the other hand, if the amount is 75 mass % or less, the fluidity and coatability of the composition can be ensured, and a uniform mixture layer can be formed.
[0055] The present composition uses water as a medium. Furthermore, for the purpose of adjusting the properties and drying properties of the present composition, the composition may be mixed with lower alcohols such as methanol and ethanol, carbonates such as ethylene carbonate, ketones such as acetone, or water-soluble organic solvents such as tetrahydrofuran and N-methyl-2-pyrrolidone. The proportion of water in the mixed medium is, for example, 50% by mass or more, or, for example, 70% by mass or more.
[0056] When the present composition is made into a coatable slurry state, the content of the water-containing medium in the entire present composition can be, for example, in the range of 25 to 60 mass %, and can also be, for example, 35 to 60 mass %, from the viewpoints of the coatability of the slurry, the energy cost required for drying, and productivity.
[0057] The present composition may further contain other binder components, such as styrene butadiene rubber (SBR)-based latex, carboxymethyl cellulose (CMC), acrylic latex, and polyvinylidene fluoride-based latex. When other binder components are used in combination, the amount thereof may be, for example, 0.1 to 5 parts by mass or less, or, for example, 0.1 to 2 parts by mass or less, or, for example, 0.1 to 1 part by mass or less, relative to 100 parts by mass of the total amount of active material. If the amount of other binder components used exceeds 5 parts by mass, resistance increases, and high-rate characteristics may become insufficient. Among the above, SBR-based latex and CMC are preferred in terms of their excellent balance of binding strength and flex resistance, and a combination of SBR-based latex and CMC is more preferred.
[0058] The SBR latex refers to an aqueous dispersion of a copolymer having structural units derived from an aromatic vinyl monomer such as styrene and structural units derived from an aliphatic conjugated diene monomer such as 1,3-butadiene. Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, vinyltoluene, and divinylbenzene, and one or more of these can be used. The structural units derived from the aromatic vinyl monomer in the copolymer can be, for example, in the range of 20 to 70% by mass, or, for example, in the range of 30 to 60% by mass, primarily from the viewpoint of binding properties. Examples of the aliphatic conjugated diene monomer include, for example, 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, and 2-chloro-1,3-butadiene, and one or more of these can be used. The structural units derived from the aliphatic conjugated diene monomer in the copolymer can be, for example, in the range of 30 to 70% by mass, or, for example, in the range of 40 to 60% by mass, in order to improve the binding properties of the binder and the flexibility of the resulting electrode. In addition to the above-mentioned monomers, the styrene / butadiene latex may also contain other monomers as copolymerization monomers, such as nitrile group-containing monomers such as (meth)acrylonitrile, carboxyl group-containing monomers such as (meth)acrylic acid, itaconic acid, and maleic acid, and ester group-containing monomers such as methyl (meth)acrylate, in order to further improve performance such as binding properties. The structural units derived from the other monomers in the copolymer can be, for example, in the range of 0 to 30% by mass, or, for example, in the range of 0 to 20% by mass.
[0059] The CMC refers to a nonionic cellulose-based semisynthetic polymer compound substituted with a carboxymethyl group and its salt. Examples of the nonionic cellulose-based semisynthetic polymer compound include alkyl celluloses such as methyl cellulose, methyl ethyl cellulose, ethyl cellulose, and microcrystalline cellulose; hydroxyethyl cellulose, hydroxybutyl methyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose stearoxy ether, carboxymethyl hydroxyethyl cellulose, alkyl hydroxyethyl cellulose, and nonoxynyl hydroxyethyl cellulose.
[0060] The composition for a secondary battery electrode mixture layer of the present invention contains the above-mentioned binder, CNT, active material, and water as essential components, and is obtained by mixing the components using known means. The method for mixing the components is not particularly limited, and known methods can be used. However, a preferred method is to dry-blend powder components such as the active material, conductive additive, and binder, then mix them with a dispersion medium such as water and disperse and knead them. When obtaining the composition in a slurry state, it is preferable to finish the slurry without poor dispersion or aggregation. Known mixers such as planetary mixers, thin film gyratory mixers, and planetary / revolving mixers can be used as mixing means. However, a thin film gyratory mixer is preferred because it can achieve a good dispersion state in a short time. Furthermore, when using a thin film gyratory mixer, it is preferable to perform pre-dispersion beforehand using a stirrer such as a disperser. The pH of the slurry is not particularly limited as long as the effects of the present invention are achieved, but it is preferably less than 12.5. For example, when CMC is added, it is more preferable that it be less than 11.5, and even more preferable that it be less than 10.5, in order to reduce the risk of hydrolysis. The viscosity of the slurry is not particularly limited as long as it exhibits the effects of the present invention, but the viscosity may be, for example, in the range of 100 to 30,000 mPa s, or, for example, 500 to 20,000 mPa s, or, for example, 1,000 to 10,000 mPa s, as Brookfield viscosity (25°C) at 20 rpm. If the viscosity of the slurry is within the above range, good coatability can be ensured.
[0061] 4. Secondary Battery Electrode The secondary battery electrode of the present invention comprises a mixture layer formed from the composition for a secondary battery electrode mixture layer of the present invention on the surface of a current collector made of copper, aluminum, or the like. The mixture layer is formed by applying the composition to the surface of the current collector and then drying to remove the medium, such as water. The method for applying the composition is not particularly limited, and known methods such as doctor blade coating, dipping, roll coating, comma coating, curtain coating, gravure coating, and extrusion can be used. Furthermore, the drying can be performed by known methods such as hot air blowing, reduced pressure, (far) infrared radiation, and microwave irradiation. Typically, the mixture layer obtained after drying is subjected to a compression treatment using a mold press, roll press, or the like. Compression brings the active material and binder into close contact, improving the strength of the mixture layer and its adhesion to the current collector. Compression can adjust the thickness of the mixture layer to, for example, approximately 30 to 80% of the thickness before compression, and the thickness of the mixture layer after compression is typically approximately 4 to 200 μm.
[0062] 5. Secondary Battery A secondary battery can be produced by providing the secondary battery electrode of the present invention with a separator and an electrolyte. The electrolyte may be liquid or gel-like. The separator is disposed between the positive and negative electrodes of the battery and serves to prevent short circuits due to contact between the electrodes and to retain the electrolyte to ensure ionic conductivity. The separator is preferably a film-like insulating microporous membrane that has good ion permeability and mechanical strength. Specific materials that can be used include polyolefins such as polyethylene and polypropylene, and polytetrafluoroethylene.
[0063] The electrolyte may be a known, commonly used one depending on the type of active material. Specific examples of the solvent for lithium ion secondary batteries include cyclic carbonates with high dielectric constants and high electrolyte dissolving ability, such as propylene carbonate and ethylene carbonate, and chain carbonates with low viscosity, such as ethyl methyl carbonate, dimethyl carbonate, and diethyl carbonate. These may be used alone or as a mixed solvent. The electrolyte may be prepared by dissolving LiPF in these solvents. 6 , LiSbF6 , LiBF 4 , LiClO 4 , LiAlO 4 In nickel-metal hydride secondary batteries, an aqueous solution of potassium hydroxide can be used as the electrolyte. A secondary battery is obtained by spirally or stacking positive and negative electrode plates separated by a separator and housing them in a case or the like.
[0064] The binder for secondary battery electrodes disclosed in this specification provides excellent toughness of the binder coating film after immersion in an electrolyte, and the electrode mixture layer for secondary batteries obtained using an electrode slurry containing the binder exhibits electrolyte resistance. Furthermore, secondary batteries equipped with electrodes obtained using the binder can ensure good integrity and exhibit good durability (cycle characteristics) even after repeated charge and discharge, making them suitable for use in automotive secondary batteries, etc.
[0065] The present invention will be specifically described below based on examples. However, the present invention is not limited to these examples. In the following, "parts" and "%" mean parts by mass and % by mass unless otherwise specified.
[0066] <<Production of the Present Non-Crosslinked Polymer Salt>> <Molecular Weight Measurement of Carboxyl Group-Containing Non-Crosslinked Polymer> 0.1 g of an aqueous solution containing a carboxyl group-containing non-crosslinked polymer (0.01 g as polymer solids) was collected and diluted with 40 g of 0.1 M sodium nitrate aqueous solution to obtain a measurement sample. The measurement sample was subjected to measurement by gel permeation chromatography (GPC) under the conditions described below to obtain the weight average molecular weight (Mw) calculated as sodium polyacrylate. (GPC Measurement Conditions) Column: 2 TSKgel GMPW columns manufactured by Tosoh Corporation Solvent: 0.1 M sodium nitrate aqueous solution Temperature: 40°C Detector: RI Flow rate: 0.5 mL / min
[0067] (Production Example 1: Production of Carboxyl Group-Containing Non-Crosslinked Polymer Salt R-1) Lithium hydroxide monohydrate in an amount equivalent to 90 mol % of the carboxylic acid and pure water were added to a 20 mass % aqueous solution of polyacrylic acid (manufactured by Toagosei Co., Ltd., product name "Jurymer (registered trademark) AC-10H") to obtain a 12 mass % aqueous solution R-1 of a carboxyl group-containing non-crosslinked polymer salt (lithium polyacrylate).
[0068] (Production Example 2: Production of carboxyl group-containing non-crosslinked polymer salt R-2) The same operation as in Production Example 1 was carried out, except that the carboxyl group-containing non-crosslinked polymer and the degree of neutralization were as shown in Table 1, to obtain a 12 mass % aqueous solution of carboxyl group-containing non-crosslinked polymer salt (lithium polyacrylate) R2.
[0069] (Production Examples 3 to 5 and Comparative Production Example 1: Production of Carboxyl Group-Containing Non-Crosslinked Polymer Salts R-2 to R-5 and R-7) The same procedure as in Production Example 1 was carried out except that the degree of neutralization was set as shown in Table 1, to obtain 12 mass % aqueous solutions of carboxyl group-containing non-crosslinked polymer salts (lithium polyacrylate) R-3 to R-5 and R-7.
[0070] (Production Example 6: Production of Carboxyl Group-Containing Non-Crosslinked Polymer Salt R-6) For polymerization, a reactor equipped with a stirring blade, a thermometer, a reflux condenser, and a nitrogen inlet tube was used. 132.1 parts of ion-exchanged water, 51.9 parts of acrylic acid (hereinafter referred to as "AA"), and 48.1 parts of 2-hydroxyethyl acrylate (hereinafter referred to as "HEA") were charged into the reactor. After the atmosphere inside the reactor was thoroughly replaced with nitrogen, the reactor was heated to raise the internal temperature to 80°C. After confirming that the internal temperature had stabilized at 80°C, 1.5 parts of ammonium peroxodisulfate was added as a polymerization initiator. Heat generation within the reaction was observed, and this point was designated as the polymerization initiation point. The polymerization reaction was continued while maintaining the internal temperature at 80°C by adjusting the external temperature (water bath temperature). Cooling of the reaction solution was started 5 hours after the polymerization initiation point. After the internal temperature had dropped to 25°C, lithium hydroxide monohydrate (hereinafter referred to as "LiOH.H") was added. 2 To the mixture was added 27.2 parts of a powder of carboxyl group-containing non-crosslinked polymer salt R-6 (hereinafter referred to as "R-6"). After the addition, stirring was continued for 12 hours at room temperature to obtain a 12% by mass aqueous solution of carboxyl group-containing non-crosslinked polymer salt R-6 (Li salt, degree of neutralization 90 mol%). The weight average molecular weight of R-6 was 150,000.
[0071]
[0072] Details of the compounds used in Table 1 are shown below. AC-10H: 20% by mass aqueous solution of polyacrylic acid (weight average molecular weight 800,000) (manufactured by Toagosei Co., Ltd., product name "Jurymer (registered trademark) AC-10H") AC-10L: 40% by mass aqueous solution of polyacrylic acid (weight average molecular weight 60,000) (manufactured by Toagosei Co., Ltd., product name "Jurymer (registered trademark) AC-10L") AA: acrylic acid HEA: 2-hydroxyethyl acrylate LiOH.H 2 O: Lithium hydroxide monohydrate NaOH: Sodium hydroxide
[0073] Example 1 (Preparation of electrode mixture layer composition (electrode slurry)) Artificial graphite (manufactured by Showa Denko K.K., trade name "SCMG-CF") and SiO (manufactured by Osaka Titanium Technologies Co., Ltd., 5 μm) were used as the active material. A mixture of cross-linked polymer R-1, styrene / butadiene latex (SBR), and sodium carboxymethyl cellulose (CMC) was used as the binder. Single-walled CNT (manufactured by OCSiAl, trade name "TuballBATT H") was used as the conductive additive. 2 Artificial graphite: SiO: non-crosslinked polymer salt R-1: SBR: CMC: single-walled CNT = 77.6:19.4:1.0:2.0:1.0:0.1 (solids content) was added to a planetary mixer (Hibismix 2P-03 manufactured by Primix Corporation) with water as a dilution solvent so that the solids concentration of the electrode mixture layer composition was 53 mass%, and the mixture was mixed for 1 hour and 30 minutes to prepare a slurry-state electrode mixture layer composition (electrode slurry).
[0074] (Preparation of negative electrode plate) Next, the electrode slurry was applied onto a 16.5 μm thick current collector (copper foil) using a variable applicator, and dried in a forced-air dryer at 80° C. for 15 minutes to form a mixture layer. After that, the thickness of the mixture layer was 50±5 μm and the mixture density was 1.60±0.10 g / cm. 3 After rolling to a thickness of 1 / 4", the mixture was punched out into a 3 cm square to obtain a negative electrode plate for battery evaluation.
[0075] (Preparation of Positive Electrode Plate) In N-methylpyrrolidone (NMP) solvent, LiNi was used as a positive electrode active material. 0.5 Co 0.2 Mn 0.3 O 2 A mixture of 100 parts of ethylenediamine fluoride (NCM) and 2 parts of acetylene black was added to the mixture, and 4 parts of polyvinylidene fluoride (PVDF) was added as a positive electrode binder to prepare a positive electrode mixture layer composition. The positive electrode mixture layer composition was applied to an aluminum current collector (thickness: 20 μm) and dried to form a mixture layer. Thereafter, the thickness of the mixture layer was 125 μm, and the mixture density was 3.0 g / cm. 3 After rolling to a thickness of 1 / 4", the mixture was punched out into a 3 cm square to obtain a positive electrode plate for battery evaluation.
[0076] (Preparation of Electrolyte Solution) Vinylene carbonate (VC) was added to a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio of EC:DMC=3:7) so that the concentration of VC was 1 mass % and fluoroethylene carbonate (FEC) was 2 mass %, and LiPF 6 was dissolved in a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0077] (Preparation of Secondary Battery) The battery was constructed by attaching lead terminals to the positive and negative electrodes, and placing the electrodes facing each other via a separator (made of polyethylene: film thickness 16 μm, porosity 47%), placing the electrode assembly in an aluminum laminate battery exterior, injecting the electrolyte, and sealing it to prepare a test battery. The design capacity of this prototype battery was 50 mAh. The design capacity of the battery was based on a charge cut-off voltage of 4.2 V.
[0078] <Evaluation of cycle characteristics> The lithium ion secondary battery of the laminated cell prepared above was charged and discharged at a charge / discharge rate of 0.1 C under conditions of CC discharge of 2.5 to 4.2 V in an environment of 45° C., and the initial capacity C 0 Furthermore, charging and discharging were repeated in an environment of 45°C at a charge / discharge rate of 0.5C under conditions of CC discharge of 2.5 to 4.2V, and the capacity C 100 and the capacity C after 300 cycles 300The cycle characteristics (ΔC) were calculated using the following formula: Charge / discharge capacity retention rate ΔC after 100 cycles 100 =C 100 / C 0 × 100 (%) Charge / discharge capacity retention rate ΔC after 300 cycles 300 =C 100 / C 0 × 100 (%) ΔC calculated by the above formula 100 The cycle characteristic was evaluated as "A" based on the following criteria. 300 The cycle characteristic was evaluated as "A" based on the following criteria. A higher ΔC value indicates better cycle characteristics. 100 (Criteria for determining the cycle characteristics ΔC) A: Charge / discharge capacity retention rate is 90% or more B: Charge / discharge capacity retention rate is 80% or more and less than 90% C: Charge / discharge capacity retention rate is 70% or more and less than 80% D: Charge / discharge capacity retention rate is less than 70% 300 Judgment criteria) A: Charge / discharge capacity retention rate is 80% or more B: Charge / discharge capacity retention rate is 70% or more and less than 80% C: Charge / discharge capacity retention rate is 60% or more and less than 70% D: Charge / discharge capacity retention rate is less than 60%
[0079] <Evaluation of Electrode Expansion Rate> The laminated cell lithium-ion secondary battery that had undergone the 300-cycle test described above was disassembled to recover the negative electrodes. Each recovered negative electrode was washed with DMC (dimethyl carbonate) solvent and allowed to air-dry at room temperature for one day, after which its thickness was measured. The measured thickness was then substituted into the following formula to calculate the negative electrode expansion rate: [Electrode Expansion Rate (%)] = 100 × {(Thickness of discharged negative electrode of battery) - (Thickness of copper foil)} / {(Thickness of negative electrode before assembly) - (Thickness of copper foil)} The electrode expansion rate calculated using the above formula was 168%, and this expansion rate was evaluated as "A" based on the following criteria. Note that a lower electrode expansion rate indicates a better electrode expansion suppression effect and better battery performance. (Criteria for determining electrode expansion rate) A: The electrode expansion rate is less than 180%. B: The electrode expansion rate is 180% or more and less than 200%. C: The electrode expansion rate is 200% or more and less than 250%. D: The electrode expansion rate is 250% or more.
[0080] Examples 2 to 15 and Comparative Examples 1 and 2 Electrode slurries were prepared in the same manner as in Example 1, except that the compositions were used as shown in Table 2. The cycle characteristics and electrode expansion coefficient of the negative electrode plates obtained using each electrode slurry were evaluated, and the results are shown in Table 2.
[0081]
[0082] Details of the compounds used in Table 2 are shown below: SBR: styrene butadiene rubber CMC: sodium carboxymethyl cellulose AB: acetylene black
[0083] <Evaluation Results> As is evident from the results of Examples 1 to 15, secondary batteries equipped with electrodes obtained using the secondary battery electrode mixture layer composition (electrode slurry) of the present invention not only exhibited excellent capacity retention at 100 cycles, but also demonstrated high capacity retention even after 300 charge / discharge cycles. Furthermore, the effect of suppressing expansion of the negative electrode after testing was also observed. This is thought to be because the higher the molecular weight of the non-crosslinked polymer, the stronger the bonding between the active materials, allowing the electrode structure to be maintained even over long-term use. Among these, when comparing the amount of carbon nanotubes used, the case where 0.1 parts by mass per 100 parts by mass of the total amount of active material (Example 1) showed superior capacity retention and expansion suppression effects at 300 cycles compared to the case where 0.05 parts by mass of single-walled CNTs (Example 2). This is thought to be due to the effect that, in response to the increase in distance between the active materials due to expansion of the negative electrode caused by repeated charge / discharge, the use of a larger amount of carbon nanotubes with a high aspect ratio structure increases the number of conductive paths formed, thereby reducing capacity degradation.
[0084] When focusing on the molecular weight of the carboxyl group-containing non-crosslinked polymer, a comparison between Examples 1 and 3 showed that the battery characteristics were superior when a higher molecular weight carboxyl group-containing non-crosslinked polymer was used (Example 1).
[0085] Focusing on the degree of neutralization of the carboxyl group-containing non-crosslinked polymer, the battery performance was found to be superior when the degree of neutralization of the polymer was 80 mol % (Example 4) compared to when the degree of neutralization of the polymer was 60 mol % (Example 5). This is thought to be because the higher the degree of neutralization of the carboxyl group-containing non-crosslinked polymer, the higher the glass transition temperature of the polymer, which suppresses fusion of the polymer during the heat drying step in the electrode production process, making it possible to obtain a uniform electrode.
[0086] In contrast, when the degree of neutralization of the carboxyl group-containing non-crosslinked polymer was 45 mol% (Comparative Example 1), the capacity retention rate at 100 cycles was slightly lower, and furthermore, the capacity retention rate at 300 cycles, which involved repeated charge and discharge, was significantly lower. This is thought to be because the fusion of the carboxyl group-containing non-crosslinked polymer deteriorated the structural uniformity in the mixture layer at the time of electrode fabrication, and local stress concentration occurred due to the suppression of expansion of the active material during charge and discharge, leading to destruction of the electrode structure.
[0087] When the neutralization salt was changed to a Na salt (Example 6), the battery performance was equivalent to that when the neutralization salt was changed to a Li salt (Example 1). This is thought to be because, in a 45°C environment, the battery exhibits equivalent binding properties and rigidity regardless of the type of neutralization salt of the non-crosslinked polymer.
[0088] Focusing on the content of structural units derived from ethylenically unsaturated carboxylic acid monomers, the battery characteristics were found to be superior when the content was 100% by mass (Example 1) compared to when the content was 52% by mass (Example 7). This is thought to be because the higher the content of carboxyl groups in the non-crosslinked polymer, the better the binding with the active material, and therefore destruction of the electrode structure can be suppressed even during long-term battery use.
[0089] When comparing the amounts of carboxyl group-containing non-crosslinked polymer salt used, the case where 1.0 part by mass of the carboxyl group-containing non-crosslinked polymer salt was used per 100 parts by mass of the total active material (Example 1) showed better capacity retention and expansion suppression effects at 300 cycles than the cases where 0.5 parts by mass of the carboxyl group-containing non-crosslinked polymer salt was used (Example 8), 1.5 parts by mass (Examples 9 and 10), and 3.0 parts by mass (Examples 11 and 12). This is because the smaller the amount of carboxyl group-containing non-crosslinked polymer salt used, the fewer bonds there are in the electrode, making it more likely that the distance between the active materials will increase due to high cycle counts of charge and discharge. Furthermore, the greater the amount of carboxyl group-containing non-crosslinked polymer salt used, the greater the number of bonds, but the brittleness of the polymer affects the electrode properties, making it more susceptible to stress caused by expansion and contraction of the active material, leading to deterioration.
[0090] Regarding the amount of silicon-based active material used, when it was increased to 29.1 parts by mass (Example 13) compared to Example 1, and when it was decreased to 9.7 parts by mass (Example 14) and 4.9 parts by mass (Example 15) compared to Example 1, good capacity retention and expansion suppression effects were also observed. This is thought to be because the combined use of this non-crosslinked polymer salt and single-walled CNTs enables repeated charge and discharge to be performed while suppressing structural destruction and conductive path disconnection in the mixture layer, regardless of the amount of silicon-based active material used.
[0091] In contrast, when a carboxyl group-containing non-crosslinked polymer salt was not used (Comparative Example 2), a good cycle retention rate was observed at 100 cycles, but the capacity deteriorated significantly after 300 cycles of repeated charge / discharge. This is thought to be because, at 100 cycles, the conductive paths between the active materials were maintained due to the good conductivity of the single-walled CNT, and the capacity was maintained, but when the non-crosslinked polymer salt was not used, the binding strength was significantly inferior, and therefore, the distance between the active materials increased with the number of repeated charge / discharge cycles, and the conductive paths through the single-walled CNT were also severed, leading to capacity deterioration.
[0092] A secondary battery equipped with an electrode obtained using the binder for secondary battery electrodes disclosed in this specification can ensure good integrity, and exhibits good durability (cycle characteristics) even after repeated charge and discharge while suppressing expansion and contraction due to charge and discharge over a longer period of use than conventional batteries, and is therefore expected to contribute to increasing the capacity of automotive secondary batteries, etc. The binder for secondary battery electrodes of the present invention can be particularly suitably used for electrodes of non-aqueous electrolyte secondary batteries, and is particularly useful for non-aqueous electrolyte lithium-ion secondary batteries with high energy density.
Claims
1. An electrode binder for a secondary battery having a secondary battery electrode containing carbon nanotubes, the electrode binder containing a carboxyl group-containing non-crosslinked polymer or a salt thereof, the degree of neutralization of the polymer being 50 mol % or more.
2. The electrode binder according to claim 1, wherein the carboxyl group-containing non-crosslinked polymer contains 50% by mass or more and 100% by mass or less of structural units derived from ethylenically unsaturated carboxylic acid monomers relative to the total structural units thereof.
3. A composition for a secondary battery electrode mixture layer, comprising the electrode binder according to claim 1 or 2, carbon nanotubes, an active material and water.
4. A composition for a secondary battery electrode mixture layer as described in claim 3, wherein the content of the silicon active material is 5.0 mass% or more based on the total amount of the active material.
5. A composition for a secondary battery electrode mixture layer as described in claim 3, wherein the content of the electrode binder is 1.0 part by mass or more and 2.5 parts by mass or less per 100 parts by mass of the total amount of the active material.
6. The composition for a secondary battery electrode mixture layer according to claim 3, wherein the content of the carbon nanotubes is 0.1 parts by mass or more per 100 parts by mass of the total amount of the active material.
7. The secondary battery electrode mixture layer composition according to claim 3, wherein the carbon nanotubes include a single-wall structure.
8. A secondary electrode comprising a current collector and a mixture layer formed from the composition for a secondary battery electrode mixture layer according to claim 3 on the surface of the current collector.
9. A secondary battery comprising the secondary electrode according to claim 8.
Citation Information
Patent Citations
Positive electrode for lithium ion secondary battery, and method for manufacturing the same
JP2014238944A
Negative electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2016066529A
Positive electrode for secondary batteries, method for producing same, slurry composition, and secondary battery
WO2013099990A1
Binder for nonaqueous electrolyte secondary cell electrode, method for producing binder, and use thereof
WO2017073589A1
Negative electrode for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
WO2022004540A1