Carbon-silicon / carbon composite and method for producing same
The carbon-silicon/carbon composite addresses the mechanical instability of silicon-based anode active materials by forming a silicon/carbon composite matrix within a porous carbon support, converting Si-Si bonds to Si-C bonds, which enhances mechanical stability and electrical conductivity, resulting in improved battery performance.
Patent Information
- Application Number
- PCT/KR2023/022024
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-29
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-17
AI Technical Summary
Silicon-based anode active materials for secondary batteries face mechanical instability due to volume expansion during charging and discharging, leading to structural damage and poor cycle characteristics, as conventional carbon supports with micropores fail to adequately accommodate the expansion of silicon crystals formed through chemical vapor deposition.
A carbon-silicon/carbon composite is created by forming a silicon/carbon composite matrix within the pores and on the surface of a porous carbon support with controlled pore properties, where the silicon/carbon composite matrix includes silicon and carbon in a specific weight ratio, and is heat-treated to convert Si-Si bonds into Si-C bonds, enhancing mechanical stability and electrical conductivity.
The carbon-silicon/carbon composite effectively alleviates stress from volume expansion, improves capacity retention, and enhances the electrical conductivity of the negative electrode active material, leading to better performance in secondary batteries.
Smart Images

Figure KR2023022024_17102024_PF_FP_ABST
Abstract
Description
Carbon-silicon / carbon composite and method for producing the same
[0001] The present invention relates to a carbon-silicon / carbon composite, and more particularly, to a carbon-silicon / carbon composite and a method for producing the same.
[0002] With the recent development of the information and communication industry, demand for electronic devices has been rapidly increasing, and with the revitalization of the electric vehicle market, demand for batteries used in these electronic devices and electric vehicles has also increased significantly.
[0003] Secondary batteries, including lithium secondary batteries and all-solid-state batteries containing liquid electrolytes, are the most widely used for these applications due to their high energy density and minimal self-discharge when not in use. Secondary batteries generally consist of a positive electrode, a negative electrode, and an electrolyte (liquid or solid). Carbon-based materials such as graphite are widely used as the negative electrode active material.
[0004] Recently, attempts have been made to use silicon-based anode active materials to improve the capacity of secondary batteries. Silicon, with its theoretically very high energy density, is attracting attention as a next-generation battery anode material to replace graphite. However, it reacts with lithium during charge and discharge, increasing its volume by up to 300%. This causes the silicon anode material to fracture during charge and discharge, resulting in significantly poor mechanical stability.
[0005] To solve these problems, a composite obtained by forming a silicon layer on a porous carbon support with excellent electrical conductivity has been proposed. However, since conventional carbon supports mainly have micropores, there is a problem that deposition does not reach the deep pores well when chemical vapor deposition (CVD) or the like is performed in a subsequent process, and the silicon crystals formed on the carbon support are large, so the phenomenon of fracture due to volume expansion cannot be sufficiently resolved.
[0006] An object of the present invention is to provide a carbon-silicon / carbon composite in which a silicon / carbon composite matrix is formed in the pores and / or surface of a porous carbon support having controlled pore characteristics.
[0007] Another object of the present invention is to provide a method for producing the above carbon-silicon / carbon composite.
[0008] Another object of the present invention is to provide a negative electrode active material comprising the above carbon-silicon / carbon composite.
[0009] The present invention provides a carbon-silicon / carbon composite comprising a porous carbon support and a silicon / carbon composite matrix disposed on the surface and within the pores of the porous carbon support.
[0010] According to one embodiment of the present invention, the porous carbon support may have a volume ratio of mesopores having a pore size of 2 to 50 nm of 10 to 80% based on the total pore volume.
[0011] In addition, the porous carbon support may have a BET specific surface area of 300 to 3,000 m2 / g, a tap density of 0.05 to 0.5 g / ㎖, and an average particle diameter of 1 to 20 ㎛.
[0012] The above silicon / carbon composite matrix may contain silicon and carbon in a weight ratio of 1:2 to 1:0.1.
[0013] Additionally, the silicon / carbon composite matrix may be 10 to 90 wt% of the total weight of the carbon-silicon / carbon composite.
[0014] Additionally, it may further include a carbon layer formed on the silicon / carbon composite matrix.
[0015]
[0016] In addition, the present invention provides a method for producing a carbon-silicon / carbon composite, comprising (1) a step of forming silicon on the surface and inside the pores of a porous carbon support to obtain a carbon-silicon composite, and (2) a step of heat-treating the carbon-silicon composite.
[0017] According to one embodiment of the present invention, the heat treatment step can be performed by heat treating the carbon-silicon composite at a temperature of 800 to 1,000°C to convert some of the Si-Si bonds of the silicon into Si-C bonds.
[0018] In addition, the heat treatment step can be performed by forming a carbon layer on the carbon-silicon composite at a temperature of 800 to 1,000°C while converting some of the Si-Si bonds of the silicon into Si-C bonds.
[0019]
[0020] In addition, the present invention provides a negative electrode active material comprising the above-described carbon-silicon / carbon composite and a carbon-based negative electrode material.
[0021]
[0022] In addition, the present invention provides an all-solid-state battery including a solid electrolyte interphase (SEI) film including the carbon-silicon / carbon composite described above.
[0023] A carbon-silicon / carbon composite according to an embodiment of the present invention forms a silicon / carbon composite matrix in the pores and / or surface of a porous carbon support having a high proportion of mesopores among the total pores, thereby exhibiting excellent electrical conductivity, alleviating stress due to volume expansion of silicon, and exhibiting excellent capacity retention when the carbon-silicon / carbon composite is used as an anode active material.
[0024] In addition, the manufacturing method according to the embodiment of the present invention can easily manufacture a carbon-silicon / carbon composite having the above characteristics.
[0025] Figure 1 shows the results of X-ray diffraction analysis of composite particles of the reference example, examples 1 to 2, and comparative example 1.
[0026] Figure 2 shows the results of X-ray diffraction analysis according to heat treatment temperature to confirm the conversion of Si-Si bonds in carbon-silicon composites into Si-C bonds.
[0027] Figures 3 and 4 show the electrochemical analysis results of batteries manufactured using the composites of the reference example, examples 1 to 2, and comparative example 1.
[0028] The present invention is not limited to the contents disclosed below, and may be modified in various forms as long as the gist of the invention is not changed.
[0029] As used herein, the term “comprising” means that other components may be included unless otherwise stated.
[0030] All numbers and expressions indicating the amounts of components, reaction conditions, etc. described in this specification are to be understood as being modified in all cases by the term “about” unless otherwise stated.
[0031] The present invention will be described in more detail below.
[0032] carbon-silicon / carbon composites
[0033] According to one embodiment of the present invention, a carbon-silicon / carbon composite is provided, comprising a porous carbon support and a silicon / carbon composite matrix disposed on the surface and within the pores of the porous carbon support.
[0034] Hereinafter, each component of a carbon-silicon / carbon composite according to one embodiment of the present invention is described.
[0035] porous carbon support
[0036] A carbon-silicon / carbon composite according to an embodiment of the present invention comprises a porous carbon support.
[0037] The porous carbon support may have a volume ratio of mesopores having a pore size of 2 to 50 nm based on the total pore volume of 10 to 80%, preferably 30 to 60%, and more preferably 40 to 50%. If the volume ratio of the mesopores of the porous carbon support is less than 10%, the number of micropores may be too large, so that a relatively large amount of silicon source may be deposited on the outside, and if the volume ratio of the mesopores of the porous carbon support exceeds 80%, the hardness of the particles is insufficient, so that when an electrode is manufactured using the same, there is a concern that the structure of the electrode may collapse.
[0038] In addition, the porous carbon support may have an average particle size of 1 to 20 μm. Preferably, the porous carbon support may have an average particle size of 3 to 20 μm, more preferably, an average particle size of 3 to 10 μm. When the average particle size of the porous carbon support is less than 1 μm, the silicon source cannot sufficiently penetrate into the pores and is deposited only on the outside of the particles, and when the average particle size of the porous carbon support exceeds 20 μm, it is difficult for the silicon source to sufficiently deposit into the pores.
[0039] In addition, the porous carbon support may have a BET specific surface area of 300 to 3,000 m2 / g. Preferably, the porous carbon support may have a BET specific surface area of 300 to 1,500 m2 / g, more preferably 500 to 1,500 m2 / g. When the BET specific surface area of the porous carbon support is less than 300 m2 / g, there may be too many macropores and thus a lack of effective pores, and when the BET specific surface area of the porous carbon support exceeds 3,000 m2 / g, there may be too many micropores and thus a large amount of silicon source may be deposited on the outside of the particles.
[0040] In addition, the porous carbon support may have a tap density of 0.05 to 0.5 g / ml. Preferably, the porous carbon support may have a tap density of 0.05 to 0.3 g / ml, more preferably, a tap density of 0.1 to 0.3 g / ml. When the tap density of the porous carbon support is less than 0.05 g / ml, process control may be difficult during deposition of the silicon source, which may result in a decrease in yield, and when the tap density of the porous carbon support exceeds 0.5 g / ml, uniform coating may be difficult during deposition of the silicon source.
[0041] Since the carbon-silicon / carbon composite according to an embodiment of the present invention includes a porous carbon support having the above characteristics, when such a carbon-silicon / carbon composite is used as a negative electrode active material, it has excellent electrical conductivity and can relieve stress due to volume expansion of silicon.
[0042] silicon / carbon composite matrix
[0043] A carbon-silicon / carbon composite according to an embodiment of the present invention comprises a silicon / carbon composite matrix disposed on the surface and inside the pores of a porous carbon support.
[0044] In the present invention, the silicon / carbon composite matrix may mean a continuous phase in which a silicon portion formed by a Si-Si bond and a silicon carbide portion formed by a Si-C bond are mixed.
[0045] In a specific example of the present invention, as described below, silicon is formed on a porous carbon support to obtain a carbon-silicon composite, and then heat-treated at a temperature of 800 to 1,000°C to convert some of the Si-Si bonds of the silicon into Si-C bonds, thereby obtaining a silicon / carbon composite matrix.
[0046] In another specific embodiment of the present invention, as described below, a silicon / carbon composite matrix can be obtained by forming silicon on a porous carbon support to obtain a carbon-silicon composite, and then converting some of the Si-Si bonds of the silicon into Si-C bonds while forming a carbon layer on the carbon-silicon composite at a temperature of 800 to 1,000°C.
[0047] In a specific embodiment of the present invention, the silicon / carbon composite matrix may include crystalline silicon particles. At this time, the size of the silicon crystals may be on the nanoscale. Specifically, the average size of the silicon crystals in the silicon / carbon composite matrix may be 10 nm or less. Preferably, the average size of the silicon crystals in the silicon / carbon composite matrix may be 8 nm or less, 5 nm or less, 3 nm or less, or 1 nm or less.
[0048] When the average size of silicon crystals in the silicon / carbon composite matrix satisfies the above range, the size of the stress due to volume expansion of silicon is reduced, so the life characteristics of the negative electrode active material can be improved.
[0049] Meanwhile, the silicon / carbon composite matrix may contain silicon and carbon in a weight ratio of 1:2 to 1:0.1, and preferably, silicon and carbon in a weight ratio of 1:1.9 to 1:0.15. If the weight ratio of silicon and carbon is less than 1:2 (silicon less than 1, carbon more than 2), the problem caused by volume expansion of silicon during charge and discharge may not be solved, which may cause structural damage to the negative electrode material and deteriorate cycle characteristics, and if the weight ratio exceeds 1:0.1 (silicon more than 1, carbon less than 0.1), the electric capacity may be reduced.
[0050] Meanwhile, the silicon / carbon composite matrix may be 10 to 90 wt% of the total weight of the carbon-silicon / carbon composite, and preferably 15 to 85 wt%. If the silicon / carbon composite matrix is less than 10 wt% of the total weight of the carbon-silicon / carbon composite, the electric capacity may be reduced, and if it exceeds 90 wt%, the problem caused by volume expansion of silicon during charge and discharge may not be resolved, which may cause structural damage to the negative electrode material and deteriorate cycle characteristics.
[0051] carbon layer
[0052] According to another embodiment of the present invention, the carbon-silicon / carbon composite may further include a carbon layer formed on the silicon / carbon composite matrix.
[0053] When the above carbon-silicon / carbon composite further includes a carbon layer, it can secure better electrical conductivity and its specific surface area can be appropriately controlled, so that when this composite is used as an anode active material of a secondary battery, the capacity retention rate of the secondary battery can be further improved.
[0054] The electrical conductivity of a negative electrode active material is a critical factor in facilitating electron transfer during electrochemical reactions. If the carbon content of the carbon-silicon / carbon composite used as the negative electrode active material is insufficient, the electrical conductivity of the negative electrode active material may be insufficient. Therefore, by further incorporating a carbon layer onto the silicon / carbon composite matrix, the charge / discharge capacity, initial charge efficiency, and capacity retention of the secondary battery can be improved, while providing superior electrical conductivity, suppressing electrolyte side reactions, and further enhancing the performance of the secondary battery.
[0055] At this time, the thickness of the carbon layer may be 1 nm to 1 ㎛, preferably 3 to 150 nm, and more preferably 5 to 100 nm. When the thickness of the carbon layer is within this range, the effect of improving conductivity can be obtained while suppressing the decrease in capacity of the secondary battery.
[0056] The carbon layer may include one or more selected from graphene, carbon nanotubes, carbon nanofibers, and graphite. Specifically, the carbon layer may include graphene and may additionally include graphite, but is not particularly limited thereto.
[0057]
[0058] Method for manufacturing carbon-silicon / carbon composites
[0059] A carbon-silicon / carbon composite according to one embodiment of the present invention is manufactured by a manufacturing method including the step of (1) forming silicon on the surface and inside the pores of a porous carbon support to obtain a carbon-silicon composite, and (2) heat-treating the carbon-silicon composite.
[0060] Hereinafter, each step of a method for manufacturing a carbon-silicon / carbon composite according to one embodiment of the present invention is described.
[0061] Step (1)
[0062] In the above step (1), silicon is formed on the surface and inside the pores of the porous carbon support to manufacture a carbon-silicon composite.
[0063] In a specific embodiment of the present invention, the step of forming silicon on the surface and within the pores of the porous carbon support can be performed using a device (e.g., a rotary kiln) and a method (e.g., chemical vapor deposition (CVD)) known in the art to which the present invention pertains. Specifically, silicon can be formed on the surface and within the pores of the porous carbon support by supplying a silicon source to the porous carbon support and performing CVD.
[0064] In a specific embodiment of the present invention, the silicon source may include at least one selected from silane (SiH4), dichlorosilane (SiH2Cl2), silicon tetrafluoride (SiF4), silicon tetrachloride (SiCl4), methylsilane (CH3SiH3), and disilane (Si2H6), but is not particularly limited thereto.
[0065] CVD of a silicon source can be performed at a temperature of 300 to 700°C. For example, CVD of a silicon source can be performed at a temperature of 400 to 600°C, 400 to 500°C, or 400 to 450°C, but is not particularly limited to this range. In addition, CVD can be performed at atmospheric pressure, and may be performed under a low vacuum of about 10 Torr if necessary. In addition, the deposition can be performed under a silane (SiH4) gas atmosphere of, for example, 50 sccm or more and 500 sccm or less.
[0066] Step (2)
[0067] In the above step (2), a step of heat treating the carbon-silicon composite is performed.
[0068] According to one embodiment of the present invention, the heat treatment step can be performed by heat treating the carbon-silicon composite at a temperature of 800 to 1,000°C to convert some of the Si-Si bonds of the silicon into Si-C bonds.
[0069] At this time, the heat treatment step can be performed at a temperature of 800 to 1,000°C, preferably 800 to 950°C, more preferably 850 to 950°C, and even more preferably 900 to 950°C. When the carbon-silicon composite is heat treated at this temperature, some of the Si-Si bonds in the silicon layer can be converted to Si-C bonds to form a silicon / carbon composite matrix.
[0070] The above heat treatment time can be appropriately adjusted depending on the heat treatment temperature, the pressure during the heat treatment, and the desired carbon-silicon content ratio. For example, the above reaction time may range from 10 to 120 minutes, specifically from 30 to 90 minutes, or more specifically from 30 to 50 minutes, but is not specifically limited to this range.
[0071] In a specific embodiment of the present invention, the heat treatment of the carbon-silicon composite may be performed in an inert gas atmosphere. In a preferred embodiment of the present invention, the heat treatment of the carbon-silicon composite may be performed in a nitrogen or argon atmosphere, but is not particularly limited thereto.
[0072] A carbon-silicon / carbon composite having a silicon / carbon composite matrix can be manufactured by heat treatment of the carbon-silicon composite.
[0073] In addition, according to another embodiment of the present invention, the heat treatment step can be performed by forming a carbon layer on a carbon-silicon composite at a temperature of 800 to 1,000°C while converting some of the Si-Si bonds of the silicon into Si-C bonds.
[0074] The step of forming a carbon layer on the particle surface of the carbon-silicon composite may be performed using a device and method known in the technical field to which the present invention pertains, such as a chemical pyrolysis deposition method, but is not particularly limited thereto.
[0075] At this time, the step of forming the carbon layer can be performed by heat-treating the carbon-silicon composite at a temperature of 800 to 1,000°C in the presence of a gaseous carbon source. Preferably, the heat treatment of the carbon-silicon composite in the presence of a gaseous carbon source can be performed at a temperature of 800 to 950°C, more preferably at a temperature of 850 to 950°C. When the carbon-silicon composite is heat-treated at this temperature in the presence of a gaseous carbon source, some of the Si-Si bonds of the silicon layer can be converted to Si-C bonds to form a silicon / carbon composite matrix.
[0076] In a preferred embodiment of the present invention, the carbon source may include at least one selected from the group consisting of methane, ethane, propane, butane, methanol, ethanol, propanol, propanediol, butanediol, ethylene, propylene, butylene, butadiene, cyclopentene, acetylene, benzene, toluene, xylene, ethylbenzene, naphthalene, anthracene, and dibutylhydroxytoluene, but is not particularly limited thereto.
[0077] When forming a carbon layer on the particle surface of a carbon-silicon composite, it can be performed in the presence of at least one inert gas selected from the group consisting of hydrogen, nitrogen, helium, and argon in addition to the above carbon source.
[0078] The reaction time (heat treatment time) for forming a carbon layer can be appropriately adjusted depending on the heat treatment temperature, the pressure during the heat treatment, the composition of the gas mixture, and the desired carbon coating amount. For example, the above-mentioned reaction time may range from 10 to 120 minutes, specifically from 20 to 90 minutes, or even more specifically from 30 to 60 minutes, but is not specifically limited to this range.
[0079] In a specific example of the present invention, when forming a carbon layer on the particle surface of a carbon-silicon composite, the process can be performed by mixing a solution in which a carbon source is dispersed in a solvent as needed with the carbon-silicon composite, and then drying and heat-treating the mixture at a temperature of 800 to 1,000°C.
[0080] In a preferred embodiment of the present invention, the carbon source may be selected from the group consisting of pitch, hydrocarbon-based material, and petroleum-based material. More specifically, the pitch may be petroleum-based pitch, coal-based pitch, or a mixture thereof, the hydrocarbon-based material may be furfuryl alcohol or a phenolic resin, and the petroleum-based material may be pyrolysis fuel oil (PFO), naphtha cracking bottom oil (NCB), ethylene cracker bottom oil (EBO), vacuum residue (VR), de-asphalted oil (DAO), atmospheric residue (AR), fluid catalytic cracking decant oil (FCC-DO), residue fluid catalytic cracking decant oil (RFCC-DO), or heavy aromatic oil. The solvent may be tetrahydrofuran (THF) or an alcohol.
[0081] By performing heat treatment while forming the above carbon layer, a carbon-silicon / carbon composite including a carbon layer on a silicon / carbon composite matrix can be manufactured.
[0082] Preliminary stage
[0083] Meanwhile, according to one embodiment of the present invention, the method for manufacturing the carbon-silicon / carbon composite may further include, before step (1), (a) a step of synthesizing pitch by thermal decomposition and polycondensation of a petroleum-based raw material, (b) a step of solidifying and pulverizing the pitch to obtain pitch in the form of pellets or powder, (c) a step of stabilizing the pitch, (d) a step of carbonizing the stabilized pitch to obtain a carbonized body, and (e) a step of activating the carbonized body to obtain a porous carbon support.
[0084] In step (a), pitch can be synthesized by thermal decomposition and polycondensation of petroleum-based raw materials.
[0085] In a specific embodiment of the present invention, the petroleum-based raw material may include at least one selected from the group consisting of pyrolysis fuel oil (PFO), naphtha cracking residue (NCB), ethylene cracker bottom oil (EBO), vacuum residue (VR), de-asphalted oil (DAO), atmospheric residue (AR), fluid catalytic cracking (RFCC-DO) oil, residue fluid catalytic cracking decant oil (RFCC-DO), and heavy aromatic oil. In a preferred specific embodiment of the present invention, the petroleum-based raw material may include pyrolysis fuel oil.
[0086] In a specific embodiment of the present invention, the petroleum-based raw material may contain an aromatic compound in an amount of 10 to 90 wt%. Preferably, the petroleum-based raw material may contain an aromatic compound in an amount of 20 to 80 wt%, more preferably 30 to 70 wt%. When the content of the aromatic compound in the petroleum-based raw material satisfies the above range, even if the solid pitch pellets described below are stabilized, carbonized, and activated without separately pulverizing, a porous carbon support having controlled pore characteristics can be obtained.
[0087] In a specific embodiment of the present invention, the aromatic compound may be a compound having 1 to 4 aromatic rings. Specifically, the aromatic compound may include at least one selected from the group consisting of substituted or unsubstituted benzene, naphthalene, phenanthrene, indene, biphenyl, anthracene, tetralin, and fluorene. In this case, even if the solid pitch pellets described below are stabilized, carbonized, and activated without separately pulverizing, a porous carbon support having controlled pore characteristics can be obtained.
[0088] In a specific embodiment of the present invention, the thermal decomposition and polycondensation of the petroleum-based raw material can be carried out at a temperature of 350 to 500°C. In a preferred specific embodiment of the present invention, the thermal decomposition and polycondensation of the petroleum-based raw material can be carried out at a temperature of 400 to 500°C. In a more preferred specific embodiment of the present invention, the thermal decomposition and polycondensation of the petroleum-based raw material can be carried out at a temperature of 430 to 470°C. When the temperature of the thermal decomposition and polycondensation of the petroleum-based raw material is 350 to 500°C, a pitch containing a large amount of relatively low molecular weight components can be produced, and in the activation process of step (e) described below, components having relatively small molecular weights are vaporized first, thereby sufficiently forming mesopores in the carbon support. If the thermal decomposition and polycondensation temperature of petroleum-based raw materials is less than 350°C, it is difficult to manufacture pitch that is solid at room temperature, and if this temperature exceeds 500°C, the pitch contains a lot of relatively high molecular weight components, making it difficult to manufacture a carbon support having mesopores.
[0089] In a specific embodiment of the present invention, the thermal decomposition and polycondensation of the petroleum raw material may be performed under an atmosphere of an oxidizing gas, an inert gas, or a mixture thereof. In a preferred specific embodiment of the present invention, the oxidizing gas may be oxygen, ozone, or a combination thereof, the inert gas may be nitrogen, helium, neon, argon, or a combination thereof, and the mixture thereof may be air, but is not particularly limited thereto.
[0090] When an oxidizing gas is used during the thermal decomposition and polycondensation of petroleum-based raw materials, a pitch with a high softening point can be produced, but it is difficult to perform the thermal decomposition and polycondensation at high temperatures. When an inert gas is used during the thermal decomposition and polycondensation of petroleum-based raw materials, thermal decomposition and polycondensation can be performed at high temperatures, but it is difficult to produce a pitch with a relatively high softening point. When a mixed gas of an oxidizing gas and an inert gas is used during the thermal decomposition and polycondensation of petroleum-based raw materials, thermal decomposition and polycondensation can be performed at relatively high temperatures, thereby producing a pitch with a relatively high softening point.
[0091] In a specific embodiment of the present invention, the gas may be supplied at a flow rate of 10 to 800 ml / min during the thermal decomposition and polycondensation of a petroleum-based raw material. In a preferred specific embodiment of the present invention, the gas may be supplied at a flow rate of 100 to 500 ml / min during the thermal decomposition and polycondensation of a petroleum-based raw material. When the flow rate of the gas is less than 10 ml / min, the yield of the pitch increases, but the low molecular weight component increases too much, which is disadvantageous for subsequent processes (e.g., stabilization). When the flow rate of the gas exceeds 800 ml / min, the yield of the pitch may decrease.
[0092] In a specific embodiment of the present invention, the thermal decomposition and polycondensation of the petroleum-based raw material can be carried out for 1 to 10 hours. In a preferred embodiment of the present invention, the thermal decomposition and polycondensation of the petroleum-based raw material can be carried out for 2 to 8 hours. In a more preferred embodiment of the present invention, the thermal decomposition and polycondensation of the petroleum-based raw material can be carried out for 2 to 7 hours. If the thermal decomposition and polycondensation time of the petroleum-based raw material is less than 1 hour, it is difficult to produce a pitch having a high softening point, and if the thermal decomposition and polycondensation time of the petroleum-based raw material exceeds 10 hours, an excessive amount of quinoline-insoluble components may be produced.
[0093] In a specific embodiment of the present invention, the thermal decomposition and polycondensation of the petroleum-based raw material may be performed under stirring. The stirring conditions for the petroleum-based raw material are not particularly limited, but, for example, a stirrer rotating at 10 to 500 rpm may be used.
[0094] In a specific embodiment of the present invention, the pitch synthesized in step (a) may have a softening point of 200 to 350°C. In a preferred embodiment of the present invention, the pitch may have a softening point of 200 to 330°C. In a more preferred embodiment of the present invention, the pitch may have a softening point of 200 to 300°C. Since the pitch manufactured according to the present invention has a high softening point, when used as a precursor for manufacturing a carbon support, the stabilization process is easy, and a high yield can be obtained after carbonization and activation.
[0095] In a specific embodiment of the present invention, the yield of the pitch synthesized in step (a) may be 10 to 50 wt%. In a preferred embodiment of the present invention, the yield of the pitch may be 10 to 40 wt%. In a more preferred embodiment of the present invention, the yield of the pitch may be 20 to 30 wt%.
[0096] In a specific embodiment of the present invention, a step of pretreating the petroleum-based raw material may be performed prior to step (a). By removing low-boiling-point components contained in the petroleum-based raw material through the pretreating step, a pitch having a higher softening point can be produced.
[0097] In a specific embodiment of the present invention, the pretreatment step may be performed at a temperature equal to or lower than the thermal decomposition and polycondensation temperature of the petroleum-based raw material in step (a), but is not particularly limited to this condition. Specifically, the pretreatment step may be performed at 250 to 450°C, preferably 250 to 400°C, and more preferably 300 to 400°C.
[0098] In a specific embodiment of the present invention, the pretreatment step may be performed for a time equal to or shorter than the thermal decomposition and polycondensation time of the petroleum-based raw material in step (a), but is not particularly limited to this condition. Specifically, the pretreatment step may be performed for 1 to 8 hours, preferably 1 to 6 hours, and more preferably 1 to 5 hours.
[0099] Additionally, in step (b), the pitch can be solidified and pulverized to obtain a pitch in the form of pellets or powder.
[0100] The liquid pitch obtained in step (a) is solidified, for example, by extrusion and cooling, and pelletized into a desired size to obtain solid pitch pellets. The process of extruding, cooling, and pelletizing the liquid pitch to obtain solid pitch pellets can be performed using commercially available equipment. For example, this process can be performed using a double-belt cooler & flaker from IPCO, but is not particularly limited to this equipment.
[0101] The pitch pellets obtained in step (b) have an average particle size of 1 to 30 mm, preferably 5 to 25 mm. When the average particle size of the pitch pellets is within this range, a porous carbon support can be manufactured through stabilization, carbonization, and activation described below without separately pulverizing the pitch pellets.
[0102] However, if necessary, the pitch pellets obtained in step (b) may be further crushed or pulverized and classified. The pitch pellets can be further finely divided through crushing or pulverization, and the particle size distribution of the pitch pellets can be made uniform through classification. Here, classification may be performed by dry classification, wet classification, or classification using a sieve. By crushing or pulverizing and classification, powdered pitch having an average particle size of 50 to 500 μm can be obtained.
[0103] And, in step (c), a step of stabilizing the pitch can be performed.
[0104] First, the pitch obtained in step (b) is subjected to primary oxidation to stabilize the carbon structure of the pitch.
[0105] In a specific embodiment of the present invention, the stabilization of the pitch may be performed in an oxidizing gas atmosphere. In a preferred embodiment of the present invention, the stabilization of the pitch may be performed in an air atmosphere, but is not particularly limited thereto.
[0106] In a specific embodiment of the present invention, the pitch stabilization may be performed at a temperature of 100 to 500°C, preferably 150 to 300°C. When the pitch stabilization is performed at this temperature, the carbon structure within the pitch changes from thermoplastic to thermosetting, and the structure can be stably maintained during the subsequent carbonization process. At this time, the heating rate may be 2 to 10°C / min. If the heating rate is too slow, productivity may be poor, and if the heating rate is excessively fast, uniform stabilization treatment may be difficult.
[0107] In a specific embodiment of the present invention, the stabilization of the pitch can be performed at a pressure of 0.1 to 10 bar, preferably 0.5 to 5 bar. When the stabilization of the pitch is performed at this pressure, the structure of the pitch, including the carbon within the pitch, can be sufficiently stabilized.
[0108] In a specific embodiment of the present invention, the stabilization of the pitch can be performed under conditions of a flow rate of an oxidizing gas, preferably air, of 0.1 to 500 ml / min, preferably 1 to 300 ml / min. When the stabilization of the pitch is performed under these oxidizing gas flow rates, the structure of the carbon within the pitch can be sufficiently stabilized.
[0109] In a specific embodiment of the present invention, the pitch stabilization may be performed for 1 to 10 hours, preferably 2 to 8 hours. If the pitch stabilization is performed for this period of time, the structure of the pitch, including the carbon within the pitch, can be sufficiently stabilized.
[0110] And, in step (d), the stabilized pitch is carbonized to obtain a carbonized body. Through carbonization of the pitch, other functional groups contained in the pitch are removed, and a carbonized body composed of substantially pure carbon can be obtained.
[0111] In a specific embodiment of the present invention, the carbonization of the pitch may be performed under an inert gas atmosphere. In a preferred embodiment of the present invention, the carbonization of the pitch may be performed under a nitrogen or argon atmosphere, but is not particularly limited thereto.
[0112] In a specific embodiment of the present invention, carbonization of the pitch may be performed at a temperature of more than 700°C and less than or equal to 1,000°C, preferably 800 to 900°C. If the temperature during carbonization of the pitch is lower than this range, carbonization may not be sufficiently achieved, and if the temperature during carbonization of the pitch is higher than this range, the carbonization yield may decrease.
[0113] In a specific embodiment of the present invention, the carbonization of the pitch can be performed under conditions of a flow rate of an inert gas, preferably nitrogen, of 0.1 to 30 ml / min, preferably 0.1 to 10 ml / min. When the carbonization of the pitch is performed under these inert gas flow rates, the pitch can be sufficiently carbonized.
[0114] In a specific embodiment of the present invention, the carbonization of the pitch may be performed for 0.5 to 5 hours, preferably 1 to 3 hours. If the carbonization of the pitch is performed for this period of time, the pitch can be sufficiently carbonized.
[0115] And, in step (e), the carbonized body (carbonized pitch) is activated to obtain a porous carbon support. By activating the carbonized body, pores are formed in the pitch pellets, thereby obtaining a porous carbon support.
[0116] In a specific embodiment of the present invention, the activation of the carbonized body may be performed in an oxidizing gas atmosphere. In a preferred embodiment of the present invention, the activation of the carbonized body may be performed in a steam atmosphere, but is not particularly limited thereto.
[0117] In a specific embodiment of the present invention, the activation of the carbonized body can be performed at a temperature of more than 700°C and less than or equal to 1,000°C, preferably 800 to 900°C. When the activation of the carbonized body is performed at this temperature, a porous carbon support in which micropores and mesopores are sufficiently formed can be obtained.
[0118] In a specific embodiment of the present invention, activation of the carbonized body can be performed at a pressure of 0.1 to 10 bar, preferably 0.1 to 5 bar. When activation of the carbonized body is performed at this pressure, a porous carbon support in which micropores and mesopores are sufficiently formed can be obtained.
[0119] In a specific embodiment of the present invention, the activation of the carbonized body can be performed under conditions of a flow rate of an oxidizing gas, preferably water vapor, of 0.1 to 100 ml / min, preferably 0.1 to 50 ml / min. When the activation of the carbonized body is performed under these oxidizing gas flow rates, a porous carbon support in which micropores and mesopores are sufficiently formed can be obtained.
[0120] In a specific embodiment of the present invention, the activation of the carbonized body may be performed for 0.5 to 5 hours, preferably 1 to 3 hours. When the activation of the carbonized body is performed for this period of time, a porous carbon support in which micropores and mesopores are sufficiently formed can be obtained.
[0121] In a specific embodiment of the present invention, the stabilization, carbonization, and activation of steps (c) to (e) above can each be performed in a microwave-assisted heating furnace. In a preferred embodiment of the present invention, the stabilization, carbonization, and activation of steps (c) to (e) above can all be performed in a microwave-assisted heating furnace. A microwave-assisted heating furnace is preferred because it can increase the temperature of the pitch itself without increasing the external temperature of the pitch, but is not particularly limited thereto.
[0122] In a specific embodiment of the present invention, the above steps (c) to (e) can be performed continuously in a single device. In a preferred embodiment of the present invention, the above steps (c) to (e) can be performed continuously in a single rotary kiln, but the device is not particularly limited thereto. By performing the above steps (c) to (e) continuously in a single device, process optimization can be achieved.
[0123] In a specific embodiment of the present invention, the porous carbon support obtained in step (e) may be further pulverized or ground and classified. The porous carbon support can be further finely divided through pulverization or grounding, and the particle size distribution of the porous carbon support can be made uniform through classification. Here, the classification may be dry classification, wet classification, classification using a sieve, etc. By the pulverization or grounding and classification treatment, a porous carbon support powder having an average particle size of 1 to 20 μm, a BET specific surface area of 300 to 3,000 m2 / g, and a tap density of 0.05 to 0.5 g / ml can be obtained. In addition, the porous carbon support powder may have a volume ratio of mesopores having a pore size of 2 to 50 nm based on the total pore volume of 10 to 80%.
[0124] Meanwhile, in the case where the porous carbon support is obtained by stabilizing, carbonizing and activating the pitch without further pulverizing in the above step (b), the carbon support may be pulverized (or further classified) to have an average particle size of 1 to 20 μm, but is not limited thereto.
[0125]
[0126] In a method for manufacturing a carbon-silicon / carbon composite according to an embodiment of the present invention, the obtained carbon-silicon / carbon composite may be pulverized or ground and classified. Through pulverization or grounding, the porous carbon support can be further finely divided, and through classification, the particle size distribution of the composite can be uniform. Here, classification may be performed by dry classification, wet classification, or classification using a sieve.
[0127] Negative active material
[0128] According to another embodiment of the present invention, a negative active material comprising a carbon-silicon / carbon composite is provided.
[0129] The negative active material according to an embodiment of the present invention may include a carbon-silicon / carbon composite.
[0130] Additionally, the negative electrode active material according to an embodiment of the present invention may further include a carbon-based negative electrode material, specifically a graphite-based negative electrode material, in addition to the carbon-silicon / carbon composite. For example, the negative electrode active material may be obtained by mixing the carbon-silicon / carbon composite according to an embodiment of the present invention with a carbon-based negative electrode material, such as a graphite-based negative electrode material.
[0131] Here, the carbon-based negative electrode material may include, but is not particularly limited to, at least one selected from the group consisting of natural graphite, artificial graphite, soft carbon, hard carbon, mesocarbon, carbon fiber, carbon nanotube, pyrolytic carbon, coke, organic polymer compound sintered body, and carbon black.
[0132] The content of the carbon-based negative electrode material in the negative electrode active material according to an embodiment of the present invention may be 2 to 80 wt%, preferably 5 to 70 wt%, and more preferably 30 to 70 wt%, based on the total weight of the negative electrode active material.
[0133] The negative active material according to an embodiment of the present invention can be effectively used in manufacturing a secondary battery, specifically, a negative electrode of a secondary battery and a negative electrode of an all-solid-state battery.
[0134] All-solid-state batteries
[0135] According to another embodiment of the present invention, an all-solid-state battery is provided comprising a solid electrolyte interphase (SEI) film including the carbon-silicon / carbon composite.
[0136] The above-described all-solid-state battery may be an all-solid-state battery including a positive electrode, a negative electrode, and a solid electrolyte between the positive electrode and the negative electrode, and the negative electrode may include a negative electrode active material layer, and may include a solid electrolyte interphase (SEI) film including the carbon-silicon / carbon composite described above on at least a portion of the negative electrode active material particles of the negative electrode active material layer.
[0137] Meanwhile, the above-described negative electrode active material particles may be carbon-based negative electrode materials, and in this case, since the content may be the same as that described in the content of the above-described negative electrode active material, the related description will be omitted.
[0138] In addition, in addition to the negative active material particles and SEI film of the above-described all-solid-state battery, the negative electrode configuration, positive electrode configuration, and solid electrolyte configuration can be applied to known all-solid-state battery configurations, and thus the present invention does not specifically limit them.
[0139]
[0140] Example
[0141] The present invention is described in more detail by the following examples. The following examples are merely illustrative of the present invention and are not intended to limit the scope of the present invention.
[0142] Examples 1-2 and Comparative Example 1
[0143] 300 g of petroleum residue oil (YNCC, HTC PFO (pyrolysis fuel oil)) was placed in a reactor equipped with a stirrer, and pyrolysis and polycondensation were performed at 450°C for 3 hours while supplying nitrogen at a flow rate of 100 ml / min. During this time, the stirrer was rotated at a speed of 200 rpm to mix the reactants. The polymerized pitch was solidified and pelletized to obtain solid pitch pellets with an average particle size of 1–30 mm.
[0144] The solid pitch pellets obtained above were pulverized to produce pitch particles with an average particle size of 200 μm, and then placed in a rotary kiln with three zones to sequentially perform stabilization, carbonization, and activation. The conditions for stabilization, carbonization, and activation are as shown in Table 1 below.
[0145] The specific surface area of the carbon support was measured using a Belsorp mini II according to ASTM D4820-93. The tap density of the carbon support was measured using a tap density analyzer (Electrolab, ETD-1020x) according to ASTM B527. The average particle size of the carbon support was measured using a particle size analyzer (Horiba, Laser Particle Analyzer, LA-960V2) according to ASTM E112. The results are shown in Table 1.
[0146] Step Condition Standard Example Stabilization temperature (℃) 300 hours (hr) 3 Atmospheric air Carbonization temperature (℃) 900 hours (hr) 1 Atmospheric nitrogen Activation temperature (℃) 900 hours (hr) 3 Water vapor flow rate (㎖ / min) 200 Support properties Average particle size (㎛) 200 Specific surface area (㎡ / g) 705 Tap density (g / ㎖) 0.54
[0147] The porous carbon support of the reference example was pulverized with a pulverizer (NETZSCH, air jet mill) to obtain a fine powder of the porous carbon support with an average particle size of 7 ㎛. Next, 15 g of the fine powder of this porous carbon support was placed in a rotary kiln, and silane (SiH4) gas was injected to form a silicon layer on the porous carbon support. The silicon layer formation conditions and the physical properties of the carbon support after the silicon layer formation are shown in Table 2 below.
[0148] Step Conditions Criteria Example Silicon layer formation conditions Batch (g) 15 Pressure Normal pressure Temperature (℃) 475 Time (hr) 120 Carbon-silicon composite properties after silicon layer formation Average particle size (㎛) 8.9 Specific surface area (㎡ / g) 10.4 Tap density (g / ㎖) 0.6
[0149] The carbon-silicon composite obtained above was placed in a rotary kiln and heat-treated at 900°C for 30 minutes in an argon atmosphere (Example 1). In addition, the same carbon-silicon composite was placed in a rotary kiln and heat-treated at 900°C (Example 2) and 700°C (Comparative Example 1) for 30 minutes in the presence of ethylene to form a carbon layer.
[0150] Exam example
[0151] (1) X-ray diffraction analysis
[0152] X-ray diffraction analysis was performed on the particles of the above standard examples, examples 1 to 2, and comparative example 1 under the conditions below, and the results are shown in Fig. 1.
[0153] - Equipment: D-MAX 2200 (RIGAKU)
[0154] - Angle: 20~70°
[0155] - Sampling W.: 0.01
[0156] - X-Ray 40kV / 30mA
[0157] - DivSlit: 1 / 2 deg.
[0158] - DivH.L.Slit: 10 mm
[0159] - SctSlit: 1 / 2 deg.
[0160] - RecSlit: 0.15 mm
[0161] As can be seen from Fig. 1, no Si-C bond was formed in the carbon-silicon composite of the reference example and the carbon-silicon-carbon composite of comparative example 1. On the other hand, it was confirmed that a Si-C bond was formed in the carbon-silicon / carbon composite of example 1 and the carbon-silicon / carbon-carbon composite of example 2.
[0162] In addition, as confirmed from Fig. 2, the reason why the SiC peak of Comparative Example 1 in which the heat treatment temperature is 700°C is not observed was identified through the observation of the SiC peak at a temperature of 850°C or higher in Fig. 1, and it was identified that the SiC peak was observed in Fig. 1 for Examples 1 and 2 in which the heat treatment temperature is 900°C.
[0163] (2) Electrochemical evaluation
[0164] Half coin cells were manufactured using each of the composites of the reference example, Example 2, and Comparative Example 1, and then electrochemical evaluation was performed. The conditions for manufacturing the half coin cells are shown in Table 3, and the evaluation results are shown in Tables 4 and 5 and FIGS. 3 and 4. In Table 3, AM, CM, and BM represent the active material (silane-deposited porous carbon support), conductor (Super P carbon black), and binder (styrene-butadiene rubber / carboxymethyl cellulose 5:5), respectively, and EC, EMC, DMC, FEC, VC, and PS represent ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, fluoroethylene carbonate, vinylene carbonate, and propane sultone, respectively.
[0165] Composition (AM:CM:BM) 8:1:1 Areal capacity (mAh / cm2) 1 Electrolyte 1.3 M LiPF 6 EC / EMC / DMC 3:5:2, FEC 10%, LiBF 4 0.2%, 0.5% VC, 1% PS Cut-off voltage (V) Formation: 0.005-1.5, Cycle test: 0.005-1.2 C-rate (C) Formation: 0.1-0.1, 0.01 C cut-off (CV) at 0.005 V
[0166] Sample charge capacity (mAh / g)Discharge capacity (mAh / g)ICE (%)Standard Example 1,9421,77991.6Example 21,1971,05588.1Comparative Example 12,4752,27692.0
[0167] Sample discharge capacity (mAh / g) ICE (%) Cycle retention rate Standard Example 1,77991.674.7 (20 cycles) Exemplary Example 21,05588.196.3 (50 cycles) Comparative Example 12,27692.076.5 (50 cycles)
[0168] As confirmed from Tables 4 to 5 and Figures 3 to 4 above, in the case of the half coin cell manufactured from the composite of the example, the capacity decreased due to a decrease in the content of silicon, but the cycle retention was significantly superior to that of the reference example and the comparative example.
Claims
1. Porous carbon support; and A carbon-silicon / carbon composite comprising a silicon / carbon composite matrix disposed on the surface and inside the pores of the porous carbon support.
2. In paragraph 1, The above porous carbon support is a carbon-silicon / carbon composite having a volume ratio of mesopores with a pore size of 2 to 50 nm of 10 to 80% based on the total pore volume.
3. In paragraph 1, The above porous carbon support is a carbon-silicon / carbon composite having a BET specific surface area of 300 to 3,000 m2 / g, a tap density of 0.05 to 0.5 g / ㎖, and an average particle diameter of 1 to 20 ㎛.
4. In paragraph 1, The above silicon / carbon composite matrix is a carbon-silicon / carbon composite containing silicon and carbon in a weight ratio of 1:2 to 1:0.
1.
5. In paragraph 1, A carbon-silicon / carbon composite wherein the silicon / carbon composite matrix is 10 to 90 wt% of the total weight of the carbon-silicon / carbon composite.
6. In paragraph 1, A carbon-silicon / carbon composite further comprising a carbon layer formed on the silicon / carbon composite matrix. 7.(1) A step of forming silicon on the surface and inside the pores of a porous carbon support to obtain a carbon-silicon composite; and (2) A method for manufacturing a carbon-silicon / carbon composite, comprising a step of heat-treating the carbon-silicon composite.
8. In paragraph 7, A method for manufacturing a carbon-silicon / carbon composite, wherein the heat treatment step is performed by heat treating the carbon-silicon composite at a temperature of 800 to 1,000°C to convert some of the Si-Si bonds of the silicon into Si-C bonds.
9. In paragraph 7, A method for manufacturing a carbon-silicon / carbon composite, wherein the heat treatment step is performed by forming a carbon layer on the carbon-silicon composite at a temperature of 800 to 1,000°C while converting some of the Si-Si bonds of the silicon into Si-C bonds.
10. Carbon-silicon / carbon composite according to any one of claims 1 to 6; and A negative electrode active material comprising a carbon-based negative electrode material.
11. An all-solid-state battery comprising a SEI (Solid Electrolyte Interphase) film comprising a carbon-silicon / carbon composite according to any one of claims 1 to 6.
Citation Information
Patent Citations
Synthesis of SiC powder with carbon deposition on the silicon powder
KR1020120011178A
Multi-shell structures and fabrication methods for battery active materials with expansion properties
KR1020150036109A
Negative electrode material of lithium battery and method for manufacturing the same
KR1020170080530A
System and Method for Predicting SOC of Batteries based on Natural Language Processing Neural Network
KR1020240077505A
KR20190122805A