Positive electrode material, and positive electrode and lithium secondary battery comprising same
A cathode material with a bi-modal particle size distribution and specific compositions addresses the issues of energy bulk density and particle breakage in lithium secondary batteries, improving stability and performance by minimizing fine powder generation and enhancing electrochemical characteristics.
Patent Information
- Application Number
- PCT/KR2024/004740
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-17
AI Technical Summary
Lithium secondary batteries face challenges with energy bulk density and particle breakage during rolling, leading to reduced lifespan and electrochemical performance due to the instability of nickel-rich lithium composite transition metal oxides, which results in poor thermal stability and increased fine powder generation.
A cathode material with a bi-modal particle size distribution, comprising a first active material in the form of single particles and a second active material in the form of secondary particles, with specific particle size ratios and compositions, is developed to minimize particle breakage and enhance energy density and electrochemical performance.
The cathode material improves energy bulk density, reduces fine powder generation, and enhances the lifespan and electrochemical performance of lithium secondary batteries by maintaining particle stability during rolling and charging processes.
Smart Images

Figure KR2024004740_17102024_PF_FP_ABST
Abstract
Description
Cathode material, cathode containing same, and lithium secondary battery
[0001] Cross-citation with related applications
[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2023-0047003, filed April 10, 2023, the entire contents of which are incorporated herein by reference.
[0003] Technology field
[0004] The present invention relates to a cathode material for a lithium secondary battery, a cathode including the same, and a lithium secondary battery.
[0005]
[0006] As technological development and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which boast high energy density and voltage, long cycle life, and low self-discharge rates, are commercialized and widely used.
[0007] Lithium-composite transition metal oxides are used as cathode active materials in lithium secondary batteries. Among these, lithium-cobalt-composite metal oxides such as LiCoO2, which exhibit high operating voltage and excellent capacity characteristics, are primarily used. However, LiCoO2 suffers from poor thermal properties due to crystal structure instability following delithiation. Furthermore, its high cost limits its mass use as a power source in fields such as electric vehicles.
[0008] As a material to replace the above LiCoO2, lithium manganese composite metal oxides (such as LiMnO2 or LiMn2O4), lithium iron phosphate compounds (such as LiFePO4), or lithium nickel composite metal oxides (such as LiNiO2) have been developed. Among these, research and development on lithium nickel composite metal oxides, which have a high reversible capacity of about 200 mAh / g and make it easy to implement large-capacity batteries, is being actively studied. However, LiNiO2 has inferior thermal stability compared to LiCoO2, and there was a problem that the positive electrode active material itself decomposed when an internal short circuit occurred due to external pressure in a charged state, causing the battery to rupture and catch fire. Accordingly, as a method to improve the low thermal stability of LiNiO2 while maintaining the excellent reversible capacity, lithium transition metal oxides in which some of the Ni was replaced with Co, Mn, or Al were developed.
[0009] In the case of lithium ion batteries using such lithium composite transition metal oxides, particularly lithium composite transition metal oxides containing a high nickel (Ni-rich) content, as cathode active materials, the capacity of the battery, whether it has high output, and whether gas is generated at high temperatures are affected not only by chemical properties such as the composition of the cathode active material, the content of impurities, and the content of lithium byproducts present on the surface, but also by physical properties such as the size, surface area, density, and shape of the cathode active material particles.
[0010] In general, in order to maximize the volumetric energy density of a battery, a method has been used in which a large-particle-diameter cathode active material is mixed with a small-particle-diameter cathode active material, thereby improving the energy volumetric density of the battery by having the small-particle-diameter cathode active material fill the gaps between the large-particle-diameter cathode active material particles. In addition, a method of rolling the cathode active material layer using a roll press has been used to manufacture a cathode active material layer with a more dense structure. At this time, due to the difference in particle strength between the large-particle-diameter cathode active material and the small-particle-diameter cathode active material, excessive cracks occur in the particles with relatively weak particle strength during rolling, which not only causes the particles to lose their original shape, but also causes the contact area with the electrolyte to become excessively large, resulting in a problem in that the life characteristics deteriorate when applied to a battery.
[0011] Therefore, there is a need to develop a cathode material that can improve energy volume density while suppressing particle breakage during rolling for cathode manufacturing and improving life characteristics.
[0012] [Prior Art Literature]
[0013] [Patent Document]
[0014] (Patent Document 1) Korean Patent Publication No. 2021-0117212
[0015]
[0016] The object of the present invention is to provide a cathode material having improved energy volume density while reducing particle breakage during rolling for cathode manufacturing.
[0017] Another object of the present invention is to provide a cathode comprising the cathode material and exhibiting excellent electrochemical performance by alleviating breakage of the cathode active material particles contained therein.
[0018] Another object of the present invention is to provide a lithium secondary battery including the positive electrode.
[0019]
[0020] To solve the above problem, the present invention provides a cathode material, a cathode for a lithium secondary battery including the cathode material, and a lithium secondary battery.
[0021]
[0022] (1) The present invention comprises a first positive electrode active material in the form of a single particle; and a second positive electrode active material in the form of a particle, the average particle diameter (D) being greater than that of the first positive electrode active material. 50 ) contains a large second positive electrode active material; and has a positive electrode material of 6,500 kgf / cm 2 When pressure is applied, a cathode material is provided in which the volume of particles having a particle diameter of 1 ㎛ or less is 10% or less of the total volume of particles present in the cathode material.
[0023] (2) The present invention provides a cathode material having a bi-modal particle size distribution in the above (1).
[0024] (3) The present invention, in the above (1) or (2), has an average particle diameter (D) of the first positive electrode active material. 50 ) is the average particle diameter (D) of the second positive electrode active material. 50 ) provides a cathode material with a content of 50% or less.
[0025] (4) The present invention provides a cathode material in any one of the above (1) to (3), wherein the single particle form is single crystal.
[0026] (5) The present invention provides a cathode material in which the weight ratio of the first cathode active material and the second cathode active material is 1:0.1 to 10 in any one of the above (1) to (4).
[0027] (6) In any one of (1) to (5), the first positive electrode active material has an average particle diameter (D 50 ) provides a cathode material having a diameter of 1 ㎛ or more and 10 ㎛ or less.
[0028] (7) In any one of (1) to (6), the second positive electrode active material has an average particle diameter (D 50 ) provides a cathode material having a diameter of 6 ㎛ or more and 25 ㎛ or less.
[0029] (8) The present invention provides a cathode material in any one of (1) to (7) above, wherein the first cathode active material has a composition represented by the following chemical formula 1.
[0030] [Chemical Formula 1]
[0031] Li 1+a1 Ni x1 Co y1 M 1 z1 M 2 w1 O2
[0032] In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, and M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, and -0.1≤a1≤0.3, 0.6≤x1<1.0, 0 <y1<0.4, 0<z1<0.4, 0≤w1≤0.1이다.
[0033] (9) The present invention provides a cathode material in any one of the above (1) to (8), wherein the second cathode active material has a composition represented by the following chemical formula 2.
[0034] [Chemical Formula 2]
[0035] Li 1+a2 Ni x2 Co y2 M 3 z2 M 4 w2 O2
[0036] In the above chemical formula 2, M 3is at least one selected from the group consisting of Mn and Al, and M 4 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, and -0.1≤a2≤0.3, 0.6≤x2<1.0, 0 <y2<0.4, 0<z2<0.4, 0≤w2≤0.1이다.
[0037] (10) The present invention provides a positive electrode including a positive electrode active material layer including any one of the positive electrode materials of (1) to (9).
[0038] (11) The present invention provides a lithium secondary battery including a positive electrode according to (10).
[0039]
[0040] The cathode material according to the present invention comprises a first cathode active material in the form of a single particle; and a second particle in the form of a secondary particle, the average particle diameter (D) being greater than that of the first cathode active material. 50 ) contains a large second positive electrode active material; and has a positive electrode material of 6,500 kgf / cm 2 When pressure is applied, the volume of particles having a particle diameter of 1 ㎛ or less relative to the total volume of particles present in the positive electrode material is satisfied to be 10% or less, so that the phenomenon of particle breakage of the positive electrode material during rolling for the manufacture of the positive electrode is reduced. Accordingly, when the positive electrode material according to the present invention is used, the occurrence of side reactions with the electrolyte caused by particle breakage of the positive electrode material can be minimized, and excellent capacity characteristics and life characteristics can be implemented.
[0041]
[0042] Figure 1 is an SEM photograph of the first positive electrode active material manufactured in Manufacturing Example 2.
[0043] Figure 2 is an SEM photograph of the second positive electrode active material manufactured in Manufacturing Example 1.
[0044] Figure 3 is an SEM photograph of a small-diameter secondary particle positive electrode active material manufactured in Comparative Manufacturing Example 1.
[0045] Figure 4 is an SEM photograph of a small-diameter single-particle positive electrode active material manufactured in Comparative Manufacturing Example 2.
[0046] Figure 5 shows the 6,500 kgf / cm of the cathode material manufactured in Example 1. 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0047] Figure 6 shows the 6,500 kgf / cm of the cathode material manufactured in Example 2. 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0048] Figure 7 shows the cathode material manufactured in Comparative Example 1 at 6,500 kgf / cm 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0049] Figure 8 shows the positive electrode material manufactured in Comparative Example 2 at 6,500 kgf / cm 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0050] Figure 9 shows the positive electrode material manufactured in Comparative Example 3 at 6,500 kgf / cm 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0051] Figure 10 is an EBSD-IPF map for the first positive electrode active material manufactured in Manufacturing Example 2.
[0052] Figure 11 shows data related to battery characteristic evaluation (capacity retention rate) of a lithium secondary battery including a cathode material manufactured in Example 1 and Comparative Example 1.
[0053] Figure 12 shows data related to battery characteristic evaluation (volume change rate) of a lithium secondary battery including a cathode material manufactured in Example 1 and Comparative Example 1.
[0054]
[0055] Hereinafter, the present invention will be described in more detail.
[0056]
[0057] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.
[0058] In this specification, it should be understood that terms such as “include,” “have,” or “have” are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0059] In the present invention, the term 'primary particle' means the smallest particle unit recognized when observing a positive electrode active material using a scanning electron microscope (SEM), and 'secondary particle' means a secondary structure formed by the aggregation of multiple primary particles.
[0060] In the present invention, the term "secondary particle form" refers to a spherical form formed by the agglomeration of tens to hundreds of primary particles manufactured by conventional methods, and means a form composed of more than 50 primary particles. Specifically, the secondary particle form in the present invention is a form in which more than 50 primary particles are agglomerated, and may also be a form in which hundreds or thousands of particles are agglomerated.
[0061] In the present invention, the term 'single particle form' is a concept that is contrasted with the spherical secondary particle form formed by agglomeration of tens to hundreds of primary particles manufactured by a conventional method, and means a form formed of 50 or fewer primary particles. Specifically, in the present invention, the single particle form may be a single particle formed of one primary particle, or may be a secondary particle form in which two or more, and 5 or fewer, 10 or fewer, 15 or fewer, 20 or fewer, 25 or fewer, 30 or fewer, 35 or fewer, 40 or fewer, 45 or fewer, or 50 or fewer primary particles are agglomerated.
[0062] In the present invention, the term 'single crystal' may be used instead of the term 'single crystal', and means a positive electrode active material or a lithium composite transition metal oxide containing 1 to 50 crystal grains. Typically, a single crystal particle refers to a particle in which the entire sample is composed of only one crystal grain or grain region. In the present invention, the single crystal positive electrode active material or single crystal positive electrode active material may be a single crystal particle composed of 1 to 50 single crystal grains, specifically, 1 crystal grain in the present invention, or an aggregate of 2 or more, and 5 or less, 10 or less, 15 or less, 20 or less, 25 or less, 30 or less, 35 or less, 40 or less, 45 or less, or 50 or less single crystal grains, and may exhibit characteristics similar to a single single crystal grain by containing a small number of single crystal grains. The above 'grain' or 'grain region' refers to a region in which atoms within a sample are continuously and periodically arranged in one direction. The above grain can be analyzed using an electron backscatter diffraction (ESBD) analyzer.
[0063] In the present invention, the term 'average particle diameter (D 50)' means the particle size at the 50% point of the volume cumulative distribution according to particle size. The above average particle size is calculated by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., S3500 from Microtrac), and measuring the difference in diffraction pattern according to particle size when the particles pass through the laser beam to calculate the particle size distribution, and calculating the particle diameter at the point where it becomes 50% of the volume cumulative distribution according to particle size in the measuring device, thereby obtaining D 50 can be measured.
[0064] In the present invention, the term 'fine powder' refers to a particle having a particle diameter of 1㎛ or less when a particle size distribution is calculated by dispersing a pressurized target powder in a dispersion medium, introducing the powder into a commercially available laser diffraction particle size measuring device (e.g., Microtrac's S3500), and measuring the difference in diffraction pattern according to particle size when the particles pass through a laser beam.
[0065]
[0066] cathode material
[0067] Hereinafter, the cathode material according to the present invention will be described.
[0068]
[0069] The cathode material of the present invention comprises a first cathode active material in the form of a single particle; and a second particle form, and has an average particle diameter (D) greater than that of the first cathode active material. 50 ) contains a large second positive electrode active material; and has a positive electrode material of 6,500 kgf / cm 2 When pressure is applied, the volume of particles having a particle diameter of 1 ㎛ or less is 10% or less of the total volume of particles present in the positive electrode material.
[0070]
[0071] High-Ni content cathode active materials in the form of secondary particles have the advantage of excellent energy density, but they have the problem of inevitably causing crystal structure instability due to structural distortion and fine particle generation caused by internal cracks during repeated charge / discharge processes. The higher the degree of single particle size of the cathode active material, the less likely it is that the particles will break or collapse during rolling, and the lower the rate of fine particle generation during rolling. However, the problem of low energy density occurs.
[0072] Accordingly, the inventors of the present invention have developed a first positive electrode active material in the form of a single particle; and a second positive electrode active material in the form of a secondary particle, having an average particle diameter (D) greater than that of the first positive electrode active material. 50 ) contains a large second positive electrode active material; and has a positive electrode material of 6,500 kgf / cm 2 When pressure is applied, if the volume of particles having a particle diameter of 1 ㎛ or less relative to the total volume of particles present in the positive electrode material is 10% or less, it is possible to suppress particle collapse during rolling, thereby reducing the generation of fine particles and improving the rolling properties of the electrode, and thus completing the present invention.
[0073]
[0074] The cathode material according to the present invention includes a first cathode active material in the form of a single particle. That is, the first cathode active material is in the form of a single particle or a single particle formed by agglomeration of 2 or more and 50 or less primary particles. Specifically, the first cathode active material may be in the form of a single particle formed by agglomeration of 2 or more, 5 or less, and 10 or less primary particles. The single particle form is distinguished from a secondary particle formed by agglomeration of more than 50 primary particles. When the first cathode active material is in the form of a single particle, the stability is excellent, and even when a cathode material including the first cathode active material is rolled, the cathode material does not break or crack, thereby reducing side reactions between the cathode material and the electrolyte. As a result, the durability against volume changes during charge and discharge of the battery is improved, and the life characteristics can be improved. When the above first positive electrode active material is in the form of secondary particles, there is a problem that the positive electrode material including the positive electrode active material is broken or cracked, resulting in poor life characteristics due to a side reaction between the positive electrode material and the electrolyte.
[0075] According to one embodiment of the present invention, the single particle form may be single-crystalline. Specifically, the single particle form may be a single particle composed of one primary particle. In this case, the single particle form may be a primary particle composed of one single crystal particle, or a primary particle composed of two or more, and five or less, or ten or less single crystal particles. In addition, the single particle form may be a secondary particle form in which two or more, and five or less, or ten or less primary particles are aggregated. In this case, the single particle form may be a form in which primary particles composed of one single crystal particle are aggregated, or a form in which primary particles composed of two or more, and five or less, or ten or less single crystal particles are aggregated. When the single particle form is single-crystalline, the grain boundary is reduced, so that side reactions between the cathode material and the electrolyte can be reduced.
[0076]
[0077] The cathode material according to the present invention includes a second cathode active material in the form of secondary particles. That is, the second cathode active material is in the form of secondary particles in which more than 50 primary particles are aggregated. The form of the secondary particles is distinguished from a single particle or a single particle form in which 2 or more and 50 or fewer primary particles are aggregated. When the second cathode active material has the form of secondary particles, the energy density can be improved by reducing the voids within the cathode material. As a result, the capacity characteristics of the battery can be improved. When the second cathode active material is in the form of single particles, the energy density of the cathode material including it is lowered, which causes problems in which the capacity characteristics are inferior.
[0078]
[0079] The above second positive electrode active material has a larger average particle diameter (D) than the above first positive electrode active material. 50 ) is large. The higher the degree of single particle size of the cathode material, the less the breakage or collapse of particles during rolling, and the lower the rate of fine particle generation during rolling, so that when manufacturing a cathode using it, it can exhibit excellent electrochemical performance. It is in the form of a single particle, and the average particle diameter (D 50 ) is a smaller first cathode active material and secondary particle form, and has an average particle diameter (D 50 ) By including a larger second cathode active material, the degree of single particle size of the cathode material can be increased while maintaining the energy density. As a result, the battery characteristics of the battery including the cathode material can be improved.
[0080]
[0081] The cathode material according to the present invention has a pressure of 6,500 kgf / cm 2 When a pressure of 6,500 kgf / cm is applied to the cathode material, the volume of particles having a diameter of 1 ㎛ or less is 10% or less of the total volume of particles present in the cathode material. Specifically, when a pressure of 6,500 kgf / cm is applied to the cathode material 2When pressure is applied, the volume of particles having a particle diameter of 1 ㎛ or less relative to the total volume of particles present in the positive electrode material may be 10% or less, 9% or less, 8% or less, 7% or less, 6% or less, or 5% or less, and may be 0.01% or more.
[0082] The volume of particles with a diameter of 1 ㎛ or less relative to the total volume of particles present in the above cathode material, i.e., the fine particle generation rate, is 6,500 kgf / cm after filling 3 g of the cathode material into a circular mold with a diameter of 1.3 cm using a 9 ton press. 2 After applying pressure, the particle distribution of the positive electrode material is measured, and the ratio of fine particles having a particle size of 1 ㎛ or less is obtained from this, and this value is defined as the fine particle generation rate. Since the first positive electrode active material and the second positive electrode active material contained in the positive electrode material before pressurization do not contain fine particles having a particle size of 1 ㎛ or less or are contained in a very small amount, the content of fine particles having a particle size of 1 ㎛ or less contained in the positive electrode material after pressurization can be measured, and this can be defined as the fine particle generation rate.
[0083]
[0084] According to one embodiment of the present invention, the cathode material of the present invention comprises a first cathode active material and a second cathode active material having different average particle diameters, and may have a bimodal particle size distribution. When the cathode material has a bimodal particle size distribution, the single particle size of the cathode material can be increased while maintaining energy density. As a result, the battery characteristics of a battery including the cathode material can be improved.
[0085]
[0086] According to one embodiment of the present invention, the first positive electrode active material has a relatively average particle diameter (D 50 ) are small particles, and the second positive electrode active material has a relatively average particle diameter (D 50 ) is a large particle, and specifically, the average particle diameter (D) of the first positive electrode active material 50 ) is the average particle diameter (D) of the second positive electrode active material.50 ) with an average particle size (D) of less than 50% 50 ) and specifically may be 50% or less, 10% to 50%, 10% to 45%, 10% to 42%, 12% to 50%, 12% to 45%, 12% to 42%, 15% to 50%, 15% to 45%, or 15% to 42%, and more specifically may be 20% to 40%. The average particle diameter (D of the second positive electrode active material 50 ) based on the average particle diameter (D) of the first positive electrode active material 50 ) When the above range is satisfied, particle breakage of the cathode material including them can be effectively reduced.
[0087]
[0088] According to one embodiment of the present invention, the weight ratio of the first positive electrode active material and the second positive electrode active material may be 1:0.1 to 10. Specifically, the weight ratio of the first positive electrode active material and the second positive electrode active material may be 1:1 to 8 or 1:1 to 5, more specifically 1:1 to 4. When the first positive electrode active material and the second positive electrode active material are included in the above weight ratio, particle breakage of the positive electrode material including them can be effectively reduced, and the positive electrode material can exhibit excellent electrochemical performance while obtaining an effect of improving the rolling density.
[0089]
[0090] According to one embodiment of the present invention, the first positive electrode active material exhibits a particle strength that is at least twice as strong as the particle strength of the second positive electrode active material, specifically, it may exhibit a particle strength of 2 to 10 times, or 2 to 8 times, and more specifically, 2.2 to 6 times. When the first positive electrode active material exhibits a particle strength within the above range based on the particle strength of the second positive electrode active material, particle breakage of a positive electrode material including them can be effectively reduced.
[0091]
[0092] According to one embodiment of the present invention, the cathode material includes a first cathode active material and a second cathode active material, and the first cathode active material and the second cathode active material satisfy a ratio of particle sizes within the above range and a weight ratio, so that particle breakage of the cathode material including them together can be effectively reduced, thereby exhibiting excellent life characteristics.
[0093]
[0094] According to one embodiment of the present invention, the first positive electrode active material has an average particle diameter (D 50 ) may be 1 ㎛ or more and 10 ㎛ or less. Specifically, it may be 1 ㎛ or more, 2 ㎛ or more, 3 ㎛ or more, or 4 ㎛ or more, and may be 5 ㎛ or less, 6 ㎛ or less, 7 ㎛ or less, 8 ㎛ or less, 9 ㎛ or less, or 10 ㎛ or less. The average particle diameter (D of the first positive electrode active material 50 ) is within the above range, the stability is excellent, and even when the positive electrode material including it is rolled, the positive electrode material does not break or crack, so that side reactions between the positive electrode material and the electrolyte can be reduced. As a result, the durability against volume change during charge and discharge of the battery is improved, and the life characteristics can be improved.
[0095] According to one embodiment of the present invention, the second positive electrode active material has an average particle diameter (D 50 ) may be 6 ㎛ or more and 25 ㎛ or less. Specifically, it may be 6 ㎛ or more, 7 ㎛ or more, 8 ㎛ or more, 9 ㎛ or more, or 10 ㎛ or more, and may be 11 ㎛ or less, 12 ㎛ or less, 13 ㎛ or less, 14 ㎛ or less, 15 ㎛ or less, 16 ㎛ or less, 17 ㎛ or less, 18 ㎛ or less, 19 ㎛ or less, 20 ㎛ or less, 21 ㎛ or less, 22 ㎛ or less, 23 ㎛ or less, 24 ㎛ or less, or 25 ㎛ or less. The average particle diameter (D of the second positive electrode active material 50 ) is within the above range, there is an effect of improving energy density.
[0096]
[0097] The average particle diameter (D) of the first positive electrode active material and the second positive electrode active material 50 ) satisfies the above range, the particle breakage of the positive electrode material including them is mitigated, and also, as the second positive electrode active material particles are filled between the first positive electrode active material particles, the tap density of the positive electrode material including them can be improved. The higher the tap density, the higher the packing density of the electrode, so that when manufacturing an electrode using this, a slurry including the positive electrode material having the above tap density can be thinly applied to the surface of the positive electrode current collector, so that the thickness of the electrode after coating is improved to be thin, and during the rolling process, the particle breakage of the first positive electrode active material in the form of single particles is reduced, and also, since the pressure required to reach the electrode thickness for matching the rolling density is less, the cracking of the positive electrode material due to rolling can be improved. In addition, since the voids between the particles are reduced, the volumetric energy density is improved, so that the capacity characteristics can be further improved.
[0098]
[0099] Meanwhile, since the particle strength of the positive electrode active material varies depending on the composition and properties of the precursor for the positive electrode active material (transition metal hydroxide, transition metal oxyhydroxide, etc.) as a raw material and the firing conditions, a positive electrode active material having a desired particle strength can be manufactured by appropriately controlling the firing conditions (temperature and time) depending on the composition and / or properties (surface area, density, shape, etc.) of the precursor for the positive electrode active material.
[0100]
[0101] The first positive electrode active material and the second positive electrode active material may each independently include a lithium composite transition metal oxide in which the molar ratio of nickel among the transition metals is 60% or more. Since the high nickel-containing lithium transition metal oxide has a large capacity per unit volume, when applied to a battery, it can realize excellent capacity characteristics.
[0102]
[0103] According to one embodiment of the present invention, the first positive electrode active material may have a composition represented by the following chemical formula 1.
[0104] [Chemical Formula 1]
[0105] Li 1+a1 Ni x1 Co y1 M 1 z1 M 2 w1 O2
[0106] In the above chemical formula 1,
[0107] M 1 is at least one selected from the group consisting of Mn and Al,
[0108] M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,
[0109] -0.1≤a1≤0.3, 0.6≤x1<1.0, 0 <y1<0.4, 0<z1<0.4, 0≤w1≤0.1이다.
[0110] The above a1 represents the molar ratio of lithium in the lithium composite transition metal oxide, and may be -0.1≤a1≤0.3, specifically 0≤a1≤0.25, and more specifically 0≤a1≤0.10.
[0111] The above x1 represents the molar ratio of nickel among the total transition metals in the lithium composite transition metal oxide, and may be 0.6≤x1<1.0, specifically 0.6≤x1≤0.99 or 0.7≤x1≤0.99, and more specifically 0.8≤x1≤0.95. When the nickel content satisfies the above range, excellent capacity characteristics can be realized.
[0112] The above y1 represents the molar ratio of cobalt among the total transition metals in the lithium composite transition metal oxide, and is 0. <y1<0.4, 구체적으로 0<y1≤0.35, 더욱 구체적으로 0.01≤y1≤0.3일 수 있다.
[0113] The above z1 is an element M among all transition metals in the lithium composite transition metal oxide. 1 It represents the molar ratio of 0 <z1≤0.4, 구체적으로 0<z1<0.35, 더욱 구체적으로 0.01≤z1≤0.30일 수 있다.
[0114] The above w1 is M among all transition metals 2 It represents the molar ratio of , and may be 0≤w1≤0.1, specifically 0≤w1≤0.08, and more specifically 0≤w1≤0.05.
[0115] The above x1, y1, z1, w1 may be x1+y1+z1+w1=1.
[0116]
[0117] According to one embodiment of the present invention, the second positive electrode active material may have a composition represented by the following chemical formula 2.
[0118] [Chemical Formula 2]
[0119] Li 1+a2 Ni x2 Co y2 M 3 z2 M 4 w2 O2
[0120] In the above chemical formula 2,
[0121] M 3is at least one selected from the group consisting of Mn and Al,
[0122] M 4 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf,
[0123] -0.1≤a2≤0.3, 0.6≤x2<1.0, 0 <y2<0.4, 0<z2<0.4, 0≤w2≤0.1이다.
[0124] The above a2 represents the molar ratio of lithium in the lithium composite transition metal oxide, and may be -0.1≤a2≤0.3, specifically 0≤a2≤0.25, and more specifically 0≤a2≤0.10.
[0125] The above x2 represents the molar ratio of nickel among the total transition metals in the lithium composite transition metal oxide, and may be 0.6≤x2<1.0, specifically 0.6≤x2≤0.99 or 0.7≤x2≤0.99, and more specifically 0.8≤x2≤0.95. When the nickel content satisfies the above range, excellent capacity characteristics can be realized.
[0126] The above y2 represents the molar ratio of cobalt among the total transition metals in the lithium composite transition metal oxide, 0 <y2<0.4, 구체적으로 0<y2≤0.35, 더욱 구체적으로 0.01≤y2≤0.3일 수 있다.
[0127] The above z2 is an element M among all transition metals in the lithium complex transition metal oxide. 3 It represents the molar ratio of 0 <z2≤0.40, 구체적으로 0<z2<0.35, 더욱 구체적으로 0.01≤z2≤0.30일 수 있다.
[0128] The above w2 is M among all transition metals 4 It represents the molar ratio of , and may be 0≤w2≤0.1, specifically 0≤w2≤0.08, and more specifically 0≤w2≤0.05.
[0129] The above x2, y2, z2, w2 may be x2+y2+z2+w2=1.
[0130]
[0131] The first positive electrode active material and the second positive electrode active material may have the same or different compositions. For example, the first positive electrode active material may be a lithium composite transition metal oxide having a nickel molar ratio of 88 mol% or more among transition metals, and the second positive electrode active material may be a lithium composite transition metal oxide having a nickel molar ratio of 86 mol% among transition metals.
[0132]
[0133] Meanwhile, the first positive electrode active material and the second positive electrode active material may further include, if necessary, a coating layer including one or more elements (hereinafter referred to as “coating elements”) selected from the group consisting of Co, Al, B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La, and Hf on the surface of the lithium transition metal oxide. When the coating layer as described above is included, contact between the lithium transition metal oxide and the electrolyte is blocked, so that gas generation and transition metal elution due to side reactions with the electrolyte can be effectively suppressed.
[0134]
[0135] The above coating layer can be formed by mixing a lithium transition metal oxide and a raw material containing the coating element, and then heat-treating the mixture at a temperature of 200°C to 800°C.
[0136]
[0137] anode
[0138] In addition, the present invention provides a positive electrode for a lithium secondary battery, including a positive electrode active material layer including the positive electrode material. Specifically, the positive electrode includes a positive electrode current collector, and a positive electrode active material layer positioned on at least one surface of the positive electrode current collector, the positive electrode active material layer including the positive electrode material.
[0139]
[0140] According to one embodiment of the present invention, the positive electrode active material layer may have a porosity of 10% to 30% by volume, specifically 15% to 30% by volume, and more specifically 18% to 27% by volume.
[0141]
[0142] According to one embodiment of the present invention, when the positive electrode active material layer has the porosity, the positive electrode may include particles having a particle size of less than 1 μm at 50% or less based on the total particle volume of the positive electrode active material layer when measuring PSD (Particle Size Distribution).
[0143]
[0144] The positive electrode may specifically include particles having a diameter of less than 1 μm in an amount of 0.01% to 50%, 0.05% to 30%, 0.1% to 28%, 0.05% to 27.5%, 0.1% to 27.5%, 0.05% to 15%, or 0.1% to 15% based on the total volume of positive electrode active material particles.
[0145] The above positive electrode can contain only a small amount of fine powder having a particle size of less than 1 ㎛ within the above range, even when the positive electrode active material layer is rolled to have a porosity within the above range during the manufacture of the positive electrode due to the alleviation of particle breakage of the positive electrode material.
[0146] The volume of the particles having a diameter of less than 1 ㎛ may be measured by rolling the positive electrode active material layer including the positive electrode material to form a positive electrode active material layer, specifically, to form a positive electrode active material layer, and then heat-treating the positive electrode active material layer in an air atmosphere at a temperature of 500°C for 2 hours, to form a positive electrode active material layer of 10 to 30 vol%, specifically, to form a positive electrode active material layer of 18 to 24 vol%.
[0147] The volume of the particles having a diameter of less than 1 ㎛ above may be a ratio of the volume when the total volume of the positive electrode active material particles included in the positive electrode active material layer is set to 100%, and specifically, after measuring the PSD using 'MICROTRAC S3500' of MICROTRAC, 'CILAS920, France' of CILAS, and 'Mastersizer2000, USA' of MALVERN, the area of the particles having a diameter of less than 1 ㎛ in the PSD graph may be obtained by dividing the area by the total area.
[0148]
[0149] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0150]
[0151] The above-described positive electrode active material layer may include a conductive material and a binder together with the positive electrode material according to the present invention described above.
[0152]
[0153] The above cathode material may be included in an amount of 80 to 99 wt%, more specifically 85 to 98 wt%, based on the total weight of the cathode active material layer. When included in the above content range, excellent capacity characteristics may be exhibited.
[0154]
[0155] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used. The conductive material may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0156]
[0157] The above binder serves to improve the adhesion between positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the positive electrode active material layer.
[0158]
[0159] The above-described positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the positive electrode material according to the present invention is used. Specifically, the positive electrode material and optionally, a binder, a conductive agent, and additives, if necessary, are dissolved or dispersed in a solvent to form a positive electrode active material layer. The composition is applied to a positive electrode current collector, followed by drying and rolling. At this time, the types and contents of the positive electrode material, binder, and conductive agent are as described above.
[0160]
[0161] The solvent may be a solvent generally used in the relevant technical field, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.
[0162]
[0163] Additionally, in another method, the positive electrode may be manufactured by casting the composition for forming the positive electrode active material layer on a separate support, and then laminating the resulting film on a positive electrode current collector by peeling it off from the support.
[0164]
[0165] lithium secondary battery
[0166] In addition, the present invention can manufacture an electrochemical device including the positive electrode. The electrochemical device may be a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.
[0167]
[0168] The lithium secondary battery specifically includes a positive electrode, a negative electrode positioned opposite the positive electrode, and a separator and electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is the same as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.
[0169]
[0170] The above lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, negative electrode, and separator, and a sealing member that seals the battery container.
[0171]
[0172] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0173]
[0174] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0175]
[0176] The above negative electrode active material layer optionally includes a binder and a conductive material together with the negative electrode active material.
[0177]
[0178] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO β(0<β<2), SnO2, vanadium oxide, lithium vanadium oxide, and other metal oxides capable of doping and dedoping lithium; or composites containing the above metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.
[0179]
[0180] The above negative electrode active material may be included in an amount of 80 to 99 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material layer.
[0181]
[0182] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0183]
[0184] The conductive agent is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10 parts by weight or less, preferably 5 parts by weight or less, based on 100 parts by weight of the total weight of the negative electrode active material layer. The conductive agent is not particularly limited as long as it has conductivity and does not cause a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0185]
[0186] For example, the negative electrode active material layer can be manufactured by applying and drying a negative electrode composite prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector, or by casting the negative electrode composite on a separate support and then laminating the resulting film on a negative electrode current collector by peeling it off from the support.
[0187]
[0188] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. can also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength can be used, and can optionally be used in a single-layer or multi-layer structure.
[0189]
[0190] In addition, examples of the electrolyte used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0191]
[0192] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0193] As the organic solvent, any solvent that can serve as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without particular limitation. Specifically, the organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); Alcohol solvents such as ethyl alcohol, isopropyl alcohol, etc.; nitriles such as R-CN (R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes, etc. can be used. Among these, carbonate solvents are preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.
[0194]
[0195] The above lithium salt can be used without any special limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the above lithium salt is LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2 can be used. It is recommended that the concentration of the lithium salt be within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0196]
[0197] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the total weight of the electrolyte.
[0198]
[0199] As described above, a lithium secondary battery including a cathode material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and lifespan characteristics, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0200]
[0201] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0202]
[0203] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0204] There is no particular limitation on the external shape of the lithium secondary battery of the present invention, but it may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.
[0205] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but can also be preferably used as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.
[0206]
[0207] Hereinafter, the present invention will be described in detail with reference to examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention should not be construed as being limited to the examples described below. The examples of the present invention are provided to more fully explain the present invention to those of ordinary skill in the art.
[0208]
[0209] Manufacturing example
[0210] Manufacturing Example 1 - Manufacturing of the second positive electrode active material
[0211] NiSO4, CoSO4, and MnSO4 were dissolved in water so that the molar ratio of nickel:cobalt:manganese was 88:5:7 to prepare a 2 M transition metal-containing solution.
[0212] A container containing the above transition metal-containing solution, a container containing a 25 wt% NaOH solution, and a container containing a 15 wt% NH4OH aqueous solution were each connected to a 200 L batch reactor set at 55°C.
[0213] Next, deionized water was added to the batch reactor, and nitrogen gas was purged to remove dissolved oxygen in the water, creating a non-oxidizing atmosphere within the reactor. Afterwards, NaOH was added, and stirring was performed at a stirring speed of 250 rpm, maintaining the pH within the reactor at 11.7.
[0214] Afterwards, the transition metal-containing solution was injected into the reactor at a rate of 250 mL / hr, NH4OH aqueous solution was injected at a rate of 40 mL / hr, and NaOH aqueous solution was injected at a rate so that the pH of the reaction solution could be maintained at 11.7. After 6 hours of reaction, stirring was stopped and the supernatant was removed to concentrate. This process was repeated 4 to 5 times to obtain the average particle diameter (D 50 ) were grown until the particles reached approximately 10 μm.
[0215] The particles thus manufactured were filtered through a filter press and then dried at 130°C for 24 hours to obtain Ni. 0.885 Co 0.035 Mn 0.080 A precursor for a second positive electrode active material having a composition of (OH)2 was obtained.
[0216] Next, LiOH·H2O was added to the precursor for the second cathode active material so as to be 1.06 equivalents, Al(OH)3 was added, and the mixture was calcined at 640°C for 5 hours in an oxygen atmosphere, and then re-calcined at 775°C for 5 hours, so that the molar ratio of nickel:cobalt:manganese:aluminum was 86:5:7:2, and the average particle diameter (D 50 ) was prepared as a second positive electrode active material in the form of secondary particles having a size of approximately 10 μm.
[0217]
[0218] Manufacturing Example 2 - Manufacturing of the first positive electrode active material
[0219] Positive electrode active material precursor [Composition: Ni 0.885 Co 0.035 Mn 0.08 (OH)2, average particle size (D) 50 ) 4 ㎛] and anhydrous LiOH as a lithium raw material were mixed in a molar ratio of 1:1, and the first firing was performed at 850°C for 6 hours in an oxygen atmosphere to manufacture a plastic product. After pulverizing the plastic product, anhydrous LiOH was additionally mixed in a molar ratio of 1:0.03, and the second firing was performed at 800°C for 10 hours in an oxygen atmosphere to obtain an average particle size (D 50 ) A first positive electrode active material in the form of single particles of 4 μm was manufactured.
[0220]
[0221] Comparative Manufacturing Example 1 - Manufacturing of Small-Diameter Secondary Particle Positive Electrode Active Material
[0222] In the above manufacturing example 1, the concentration process was repeated 2 to 3 times to obtain the average particle size (D 50 ) was grown until the particles reached approximately 4 μm. A precursor for a secondary particle positive electrode active material was prepared in the same manner as in Manufacturing Example 1.
[0223] Next, the average particle diameter (D) was determined in the same manner as in Manufacturing Example 1, except that the precursor for the secondary particle positive electrode active material was used. 50 ) A secondary particle cathode active material with a particle size of 4 ㎛ was manufactured.
[0224]
[0225] Comparative Manufacturing Example 2 - Manufacturing of Small-Particle Single-Particle Positive Electrode Active Material
[0226] Positive electrode active material precursor [Composition: Ni 0.885 Co 0.035 Mn 0.08 (OH)2, average particle size (D) 50 ) 4 ㎛] and anhydrous LiOH as a lithium raw material were mixed in a molar ratio of 1:1.03, and first calcined at 850℃ for 16 hours in an oxygen atmosphere to obtain an average particle size (D 50 ) A small-diameter single-particle cathode active material with a particle size of 4 ㎛ was manufactured.
[0227]
[0228] Examples and Comparative Examples
[0229] Example 1
[0230] A cathode material was manufactured by mixing the first cathode active material manufactured in Manufacturing Example 2 and the second cathode active material manufactured in Manufacturing Example 1 at a weight ratio of 1:4.
[0231]
[0232] Example 2
[0233] A cathode material was manufactured by mixing the first cathode active material manufactured in Manufacturing Example 2 and the second cathode active material manufactured in Manufacturing Example 1 at a weight ratio of 1:1.
[0234]
[0235] Comparative Example 1
[0236] A cathode material was manufactured by mixing the small-diameter secondary particle cathode active material manufactured in Comparative Manufacturing Example 1 and the second cathode active material manufactured in Manufacturing Example 1 at a weight ratio of 1:4.
[0237]
[0238] Comparative Example 2
[0239] A cathode material was manufactured by mixing the small-diameter secondary particle cathode active material manufactured in Comparative Manufacturing Example 1 and the second cathode active material manufactured in Manufacturing Example 1 at a weight ratio of 1:1.
[0240]
[0241] Comparative Example 3
[0242] A cathode material was manufactured by mixing the small-particle single-particle cathode active material manufactured in Comparative Manufacturing Example 2 and the second cathode active material manufactured in Manufacturing Example 1 at a weight ratio of 1:4.
[0243]
[0244] Experimental Example 1
[0245] For each of the positive electrode active materials manufactured in Manufacturing Example 2, Comparative Manufacturing Example 1, and Comparative Manufacturing Example 2, SEM photographs were obtained using a scanning electron microscope (SEM) (FEI, Quanta), and these are shown in FIGS. 1 to 4.
[0246]
[0247] Figure 1 is an SEM photograph of the first positive electrode active material manufactured in Manufacturing Example 2.
[0248] Figure 2 is an SEM photograph of the second positive electrode active material manufactured in Manufacturing Example 1.
[0249] Figure 3 is an SEM photograph of a small-diameter secondary particle positive electrode active material manufactured in Comparative Manufacturing Example 1.
[0250] Figure 4 is an SEM photograph of a small-diameter single-particle positive electrode active material manufactured in Comparative Manufacturing Example 2.
[0251]
[0252] Through Figure 1, it was confirmed that the first positive electrode active material was in the form of a single particle.
[0253] Specifically, it was confirmed that the first cathode active material is in the form of secondary particles in which 1 to 10 primary particles, more specifically 1 to 5 primary particles, are aggregated.
[0254] Through Figure 2, it was confirmed that the second positive electrode active material was in the form of secondary particles in which more than 50 primary particles were aggregated.
[0255]
[0256] Experimental Example 2
[0257] Using PSA (MICROTRAC S3500 from MICROTRAC), the particle size distribution of each cathode material manufactured in the above examples and comparative examples was measured before and after pressurization.
[0258] Specifically, the particle size distribution before pressurization was measured by uniformly mixing 50 mg of each of the cathode materials manufactured in the above examples and comparative examples with 40 ml of distilled water and 500 μL of a dispersant and injecting them into a PSA.
[0259] After pressurization, the particle size distribution was determined by placing 3 g of each of the cathode materials manufactured in the above examples and comparative examples into a circular mold with a diameter of 1.3 cm, and pressing the cathode materials into the mold with a 9-ton press at 6,500 kgf / cm 2 After pressurizing with a pressure of , the pressurized cathode material was crushed into powder, and then, using PSA (MICROTRAC S3500 from MICROTRAC), 50 mg of each of the crushed cathode materials was uniformly mixed with 40 ml of distilled water and 500 μL of dispersant, and injected into the PSA for measurement.
[0260] 6,500 kgf / cm for the cathode materials manufactured in each example and comparative example 2 The particle size distribution curves measured by PSA before and after applying pressure are shown in Figures 5 to 9 below, and using the particle size distribution curves measured by PSA, the volume of particles with a particle diameter of 1 ㎛ or less (fine particle generation rate (%)) relative to the total volume of particles present in the cathode material after applying pressure was measured, and the results are shown in Table 1 below.
[0261]
[0262] Figure 5 shows the 6,500 kgf / cm of the cathode material manufactured in Example 1. 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0263] Figure 6 shows the 6,500 kgf / cm of the cathode material manufactured in Example 2. 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0264] Figure 7 shows the cathode material manufactured in Comparative Example 1 at 6,500 kgf / cm 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0265] Figure 8 shows the positive electrode material manufactured in Comparative Example 2 at 6,500 kgf / cm 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0266] Figure 9 shows the positive electrode material manufactured in Comparative Example 3 at 6,500 kgf / cm 2 This is a particle size distribution curve measured by PSA before and after applying pressure.
[0267]
[0268] Through FIG. 5 and FIG. 7, it was confirmed that the positive electrode materials of Example 1 and Comparative Example 1 contained two types of positive electrode active materials at the same mixing ratio, and each of the two types of positive electrode active materials had the same particle size, but the change in particle size after pressurization of Example 1 was significantly less than that of Comparative Example 1.
[0269] Through FIG. 6 and FIG. 8, it was confirmed that the positive electrode materials of Example 2 and Comparative Example 2 also contained two types of positive electrode active materials at the same mixing ratio, and each of the two types of positive electrode active materials had the same particle size, but the change in particle size after pressurization of Example 2 was significantly less than that of Comparative Example 2.
[0270] Through FIG. 5 and FIG. 9, it was confirmed that the cathode materials of Example 1 and Comparative Example 3 differ only in the manufacturing method of the first cathode active material, specifically the sintering step, but that Example 1 has a significantly smaller change in particle size after pressurization than Comparative Example 3.
[0271]
[0272] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Differentiation rate (%) 4.6 3.7 16.9 25.2 16.33
[0273]
[0274] Through the above Table 1, the cathode materials manufactured in Examples 1 and 2 had a fine particle generation rate, i.e., 6,500 kgf / cm in the cathode material. 2 When pressure was applied, it was confirmed that the volume of particles with a particle diameter of 1 ㎛ or less was 10% or less of the total volume of particles present in the positive electrode material.
[0275] In comparison, it was confirmed that the cathode materials manufactured in Comparative Examples 1 to 3 had a fine particle generation rate of more than 10%.
[0276]
[0277] Experimental Example 3
[0278] Using an ion milling system (JBOL, IB19520CCP) (acceleration voltage: 6 kV), the first positive electrode active material manufactured in Manufacturing Example 2 was subjected to Ar ion milling for 2 hours to prepare a cross-sectional sample.
[0279] The cross-sectional samples of the first cathode active material were measured and analyzed using a field emission scanning electron microscope (SEM, JEOL JSM-7900F with Oxford symmetry EBSD detector) (acceleration voltage: 20 kV). EBSD IPF maps were created using AztecCrystal from OXFORD Instruments as the image processing-EBSD quantification analysis software.
[0280]
[0281] Figure 10 is an EBSD-IPF map for the first positive electrode active material manufactured in Manufacturing Example 2.
[0282]
[0283] Through Fig. 10, it was confirmed that the first positive electrode active material of Manufacturing Example 2 was single-crystalline. Specifically, it was confirmed that the first positive electrode active material was composed of one primary particle composed of one or more and ten or less, more specifically one or more and five or less single-crystalline particles, or that the primary particles were in an aggregated form.
[0284]
[0285] Experimental Example 4
[0286] - Coin-type half-cell manufacturing
[0287] A positive electrode slurry was prepared by mixing 97.5 wt% of the positive electrode materials manufactured in Example 1 and Comparative Example 1, 1.0 wt% of carbon black as a conductive material, and 1.5 wt% of polyvinylidene fluoride (PVDF) as a binder (specifically, 1.4 wt% of KF9709 and 0.1 wt% of BM740H) in an N-methylpyrrolidone (NMP) solvent. The prepared positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and then rolled to a porosity of 24% to prepare a positive electrode.
[0288] An electrode assembly was manufactured using a lithium metal electrode as the negative electrode and a porous polyethylene separator interposed between the positive and negative electrodes. This was placed inside a battery case, and an electrolyte solution containing 1.0 M LiPF6 dissolved in an organic solvent containing ethylene carbonate (EC): ethyl methyl carbonate (EMC): diethyl carbonate (DEC) in a volume ratio of 3:3:4 was injected to manufacture a coin-type half-cell.
[0289]
[0290] -Battery characteristic evaluation
[0291] After charging (0.1C, cut-off current: 0.05C) to 4.25 V at 25 ℃ using the CC-CV method, the battery was discharged (0.1C) to 3.0 V using the CC method, and the charge / discharge capacity (mAh / g) at this time was measured. The measured charge / discharge capacity (mAh / g) and the percentage of discharge capacity to charge capacity (efficiency (%)) were calculated, and the results are shown in Table 2 below.
[0292]
[0293] Classification @25℃, 0.1C / 0.1C Charge capacity (mAh / g) Discharge capacity (mAh / g) Efficiency (%) Example 1229.2209.491.4 Comparative example 1230.7207.790
[0294] Through Table 2, it was confirmed that the secondary battery using the cathode material according to the present invention has excellent discharge capacity and efficiency at room temperature.
[0295]
[0296] Experimental Example 5
[0297] -Manufacturing pouch-type monocell batteries
[0298] A positive electrode slurry was prepared by mixing 97.5 wt% of the positive electrode materials manufactured in Example 1 and Comparative Example 1, 1.0 wt% of carbon black as a conductive material, and 1.5 wt% of polyvinylidene fluoride (PVDF) as a binder (specifically, 1.4 wt% of KF9709 and 0.1 wt% of BM740H) in an N-methylpyrrolidone (NMP) solvent. The prepared positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and then rolled to a porosity of 24% to prepare a positive electrode.
[0299] A negative electrode slurry was prepared by mixing a negative electrode active material consisting of natural graphite and artificial graphite in a weight ratio of 5:5, a Super C conductive agent, an additive (Daicel, DAICEL2200), and a binder (ZEON, BML302) in water in a weight ratio of 95.6:1.0:2.3:1.1. The negative electrode slurry was applied to one surface of a copper current collector, dried at 130°C, and rolled to prepare a negative electrode.
[0300] An electrode assembly was manufactured by interposing a porous polyethylene separator between the positive and negative electrodes. This was placed inside a battery case, and an electrolyte solution containing 1.0 M LiPF6 dissolved in an organic solvent of ethylene carbonate (EC): ethyl methyl carbonate (EMC): diethyl carbonate (DEC) in a volume ratio of 3:3:4 was injected to manufacture a pouch-type monocell.
[0301] - Battery Characteristics Evaluation 1
[0302] Using the pouch-type monocell manufactured as described above, a cycle of charging (0.33C) to 4.25 V in a CC-CV manner at 45°C and discharging (0.33C) to 3.0 V in a CC manner was considered as one cycle, and a total of 400 cycles of charging and discharging were repeated, and the discharge capacities in the first cycle, the 100th cycle, and the 400th cycle were measured, and the percentage of the discharge capacity in the 100th cycle to the discharge capacity in the first cycle (capacity retention rate) 100 (%)) and the percentage of discharge capacity of the 400th cycle to the discharge capacity of the first cycle (capacity retention rate) 400 (%)) are shown in Table 3 and Figure 11 below.
[0303]
[0304] Figure 11 shows data related to battery characteristic evaluation (capacity retention rate) of a lithium secondary battery including a cathode material manufactured in Example 1 and Comparative Example 1.
[0305]
[0306] Capacity retention rate 100 (%) Capacity retention rate 400 (%)Example 194.7187.93Comparative Example 194.2187.37
[0307] Through Table 3, it was confirmed that the secondary battery using the cathode material according to the present invention has excellent life characteristics.
[0308]
[0309] -Battery Characteristics Evaluation 2
[0310] Using the pouch-type monocell manufactured as described above, the cathodes were separated after charging (0.33C) to 4.25 V at 25°C using the CC-CV method. The separated cathodes were placed in a cell pouch, additional electrolyte was added, and the pouch was sealed to prepare a sample. The sample was stored at 60°C for 12 weeks, and the degree of volume change was measured, and the percentage of the volume of the 12-week sample relative to the volume of the 0-week sample (volume change rate (%)) is shown in Table 4 and Fig. 12 below.
[0311]
[0312] Figure 12 shows data related to battery characteristic evaluation (volume change rate) of a lithium secondary battery including a cathode material manufactured in Example 1 and Comparative Example 1.
[0313]
[0314] Volume change rate (%) Example 132.1 Comparative example 142.7
[0315] Through Table 4, it was confirmed that the secondary battery using the cathode material according to the present invention has an excellent effect in reducing gas generation.
Claims
1. A first positive electrode active material in the form of a single particle; and It is in the form of secondary particles and has an average particle diameter (D) greater than that of the first positive electrode active material. 50 ) contains a large second positive electrode active material; 6,500 kgf / cm for cathode material 2 A cathode material in which the volume of particles having a particle diameter of 1 ㎛ or less is 10% or less of the total volume of particles present in the cathode material when pressure is applied.
2. In paragraph 1, A cathode material having a bimodal particle size distribution.
3. In paragraph 1, The average particle diameter (D) of the first positive electrode active material 50 ) is the average particle diameter (D) of the second positive electrode active material. 50 ) Cathode material with a content of 50% or less.
4. In paragraph 1, The above single particle form is a cathode material having a single crystal structure.
5. In paragraph 1, A cathode material in which the first cathode active material and the second cathode active material have a weight ratio of 1:0.1 to 10.
6. In paragraph 1, The above first positive electrode active material has an average particle diameter (D 50 ) is a cathode material having a diameter of 1 ㎛ or more and 10 ㎛ or less.
7. In paragraph 1, The above second positive electrode active material has an average particle diameter (D 50 ) A cathode material having a diameter of 6 ㎛ or more and 25 ㎛ or less.
8. In paragraph 1, The above first positive electrode active material is a positive electrode material having a composition represented by the following chemical formula 1: [Chemical Formula 1] Li 1+a1 Ni x1 Co y1 M 1 z1 M 2 w1 O2 In the above chemical formula 1, M 1 is at least one selected from the group consisting of Mn and Al, M 2 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, -0.1≤a1≤0.3, 0.6≤x1<1.0, 0 <y1<0.4, 0<z1<0.4, 0≤w1≤0.1이다.
9. In paragraph 1, The above second positive electrode active material is a positive electrode material having a composition represented by the following chemical formula 2: [Chemical Formula 2] Li 1+a2 Ni x2 Co y2 M 3 z2 M 4 w2 O2 In the above chemical formula 2, M 3 is at least one selected from the group consisting of Mn and Al, M 4 is at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, S, Sr, Ta, La and Hf, -0.1≤a2≤0.3, 0.6≤x2<1.0, 0 <y2<0.4, 0<z2<0.4, 0≤w2≤0.1이다.
10. A positive electrode comprising a positive electrode active material layer including the positive electrode material of any one of claims 1 to 9.
11. A lithium secondary battery comprising the positive electrode of Article 10.
Citation Information
Patent Citations
Machine learning-based perimeter intrusion detection system using radar
KR102377226B1
Lithium ion secondary battery
JP2013065468A
Lithium containing composite oxide powder and process for production of the same
KR1020090032138A
Positive-electrode active material for lithium rechargeable battery
KR1020160049519A
Positive electrode active material for lithium secondary battery, preparing method of the same, positive electrode and lithium secondary battery including the same
KR102325727B1