Preparation method for aerogel-modified concrete
By introducing foam under normal pressure after vacuum stirring, combined with the mixing of hydrophilic modified aerogel and hydrophobic aerogel, the problem of difficulty in mixing airgel and foam concrete is solved, and efficient insulation and strength improvement are achieved.
Patent Information
- Application Number
- PCT/CN2023/088649
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-24
AI Technical Summary
It is difficult to achieve effective mixing of airgel and foam concrete with existing technology, resulting in insufficient thermal insulation and strength properties.
The airgel and concrete raw materials are mixed under vacuum stirring conditions, and then foam is introduced under normal pressure conditions, and the mixture of hydrophilic modified airgel and hydrophobic airgel is used to improve the mixing uniformity and performance.
It significantly improves the thermal insulation effect and strength of concrete, avoids the reduction of foaming agent effect caused by vacuum mixing, and maintains the mechanical strength of concrete.
Smart Images

Figure CN2023088649_24102024_PF_FP_ABST
Abstract
Description
A method for preparing aerogel-modified concrete Technical Field
[0001] The invention belongs to the technical field of building thermal insulation and relates to a method for preparing aerogel-modified concrete. Background Art
[0002] As demand for green, energy-saving, and environmentally friendly buildings continues to increase, the performance of building insulation materials largely determines the level of energy consumption. Foam concrete is a widely used building insulation material, and optimizing its thermal insulation performance meets the current demand for green and sustainable development.
[0003] Aerogel is a lightweight, solid material with a three-dimensional network structure and nanoscale pores. It boasts a large surface area, high porosity, low density, and extremely low thermal conductivity, enhancing the performance of traditional insulation materials.
[0004] Some existing technologies attempt to improve the thermal insulation properties of foamed concrete by adding aerogel. However, aerogel powder is extremely light and floats above the foamed concrete slurry during mixing, making it difficult to mix. There is an urgent need to develop a method for effectively adding aerogel to achieve a modified foamed concrete with excellent thermal insulation and strength properties.
[0005] To solve the problem of aerogel powder and foam concrete being difficult to mix, the main methods currently used include increasing the stirring time and changing the mixing ratio. However, most of the existing methods can only improve the mixing of aerogel powder particles in the foam concrete slurry, and cannot effectively achieve uniform mixing.
[0006] Summary of the Invention
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0008] A method for preparing aerogel-modified concrete comprises: mixing aerogel with raw materials and auxiliary materials of concrete under vacuum stirring conditions, then introducing foam under normal pressure conditions and mixing again to obtain the aerogel-modified concrete.
[0009] According to an embodiment of the present invention, the conditions for vacuum stirring specifically include: stirring at an absolute pressure of less than 5 KPa; vacuum stirring time of no more than 15 minutes; and stirring temperature of 8°C to 30°C.
[0010] According to an embodiment of the present invention, the aerogel is added into the raw materials of the modified concrete.
[0011] According to an embodiment of the present invention, the method of introducing foam includes directly adding a foaming agent, or mixing a foaming agent with water to prepare the foam.
[0012] According to an embodiment of the present invention, the raw material of the aerogel-modified concrete is selected from cement, which includes silicate cement, aluminate cement, sulphoaluminate cement and magnesium oxychloride cement.
[0013] According to an embodiment of the present invention, in the aerogel-modified concrete, the mass ratio of aerogel to cement is (0-30):100 and the content of the aerogel is not zero.
[0014] According to an embodiment of the present invention, in the aerogel-modified concrete, the particle size of the aerogel is 1 nm-50 nm.
[0015] According to an embodiment of the present invention, the aerogel is selected from hydrophilically modified aerogels and / or hydrophobic aerogels.
[0016] According to a preferred embodiment of the present invention, the aerogel includes hydrophilic modified aerogel and hydrophobic aerogel, wherein the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 100:(0-200) and the content of the hydrophobic aerogel is not zero.
[0017] Preferably, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 100:(100-200).
[0018] According to an embodiment of the present invention, the hydrophilically modified aerogel is a hydrophilically modified aerogel particle.
[0019] According to an embodiment of the present invention, the contact angle between the hydrophilic modified aerogel and water is less than 90°.
[0020] According to an embodiment of the present invention, the contact angle of the hydrophobic aerogel with water is greater than 90°.
[0021] According to an embodiment of the present invention, the auxiliary material includes water and at least one of the following substances: vitrified microspheres, a water reducing agent, a foaming agent and fly ash.
[0022] According to an embodiment of the present invention, the addition amount of the auxiliary material is 0.1 to 50 parts by mass per 100 parts by mass of cement.
[0023] According to an embodiment of the present invention, the amount of water is 20 to 100 parts by mass per 100 parts by mass of cement.
[0024] According to an embodiment of the present invention, the water reducing agent is in an amount of 0.01-20 parts by mass per 100 parts by mass of cement.
[0025] According to an embodiment of the present invention, the water reducer is selected from calcium lignin sulfonate, sodium lignin sulfonate, magnesium lignin sulfonate, sulfonated melamine formaldehyde resin, aromatic amino sulfonate polymer, aliphatic hydroxy sulfonate polymer, HSB aliphatic high-efficiency water reducer, casein, polycarboxylic acid high-performance water reducer, polyoxyethylene dioleate, tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxyethylene sorbitol lanolin oleic acid derivative, polyoxyethylene sorbitol lanolin derivative, polyoxypropylene stearate, polyoxyethylene (5EO) lanolin ether, anhydrous sorbitan laurate, polyoxyethylene fatty acid, polyoxyethylene oxypropylene oleate, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, gur gum, fatty acid polyethylene glycol ester.
[0026] According to an embodiment of the present invention, the fly ash is in an amount of 0.5-20 parts by mass per 100 parts by mass of cement.
[0027] According to an embodiment of the present invention, the auxiliary material may also be selected from one or more of silica fume, ground slag powder, and phosphorus slag powder.
[0028] According to an embodiment of the present invention, preferably, the fly ash is selected from fly ash of not less than Grade II in the national standard GB / T 1596-2017 "Fly ash used in cement and concrete".
[0029] According to an embodiment of the present invention, the amount of the vitrified microspheres is 5 to 40 parts by mass per 100 parts by mass of cement.
[0030] According to an embodiment of the present invention, the reinforcing fibers are selected from inorganic fibers and organic fibers. Preferably, the reinforcing fibers are short fibers, specifically fibers with a length of 3 mm to 60 mm.
[0031] According to an embodiment of the present invention, the reinforcing fiber is present in an amount of 0.5 to 5 parts by mass per 100 parts by mass of cement.
[0032] According to an embodiment of the present invention, before the vacuum stirring, the cement, auxiliary materials and aerogel are premixed to obtain a uniform premix. Preferably, the temperature during premixing is controlled at 8°C to 30°C.
[0033] According to an embodiment of the present invention, the mass ratio of the foaming agent to the cement is 0.1 to 10:100. Beneficial effects
[0034] 1. This invention proposes a method for preparing aerogel-modified concrete. This method first performs vacuum mixing, then adds a foaming agent and stirs under normal pressure. This method effectively overcomes the problem of reduced foaming agent effectiveness caused by the introduction of vacuum mixing in the prior art. This method achieves excellent mixing while fully utilizing the foaming agent's function, producing a concrete with significantly improved thermal insulation and strength.
[0035] 2. The present invention further introduces hydrophilic modified aerogel, which is easier to mix with concrete slurry. In addition, compared with untreated hydrophobic aerogel, the hydrophilic modified aerogel has better thermal insulation performance.
[0036] 3. In order to solve the problem that adding hydrophilic modified aerogel to concrete will lead to a decrease in concrete strength, the present invention also proposes a solution of mixing hydrophilic modified aerogel with hydrophobic aerogel. Under the premise of maintaining thermal insulation performance, the strength is maintained without decreasing. That is, the mixed aerogel has better thermal insulation performance and the strength of the concrete does not decrease much. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] FIG1 is a schematic diagram of a preparation process of aerogel-modified concrete according to the present invention.
[0038] FIG2 is a schematic diagram of another preparation process of aerogel-modified concrete according to the present invention.
[0039] FIG3 is a line graph showing the compressive strength changes of the aerogel-modified concrete of the present invention at different aerogel addition ratios.
[0040] FIG4 is a line graph showing the change in thermal conductivity of the aerogel-modified concrete of the present invention at different aerogel addition ratios. DETAILED DESCRIPTION
[0041] As described above, the present invention provides a method for preparing aerogel-modified concrete, which comprises: mixing aerogel with raw materials and auxiliary materials of concrete under vacuum stirring conditions, then introducing foam under normal pressure conditions, and mixing again to obtain the aerogel-modified concrete.
[0042] The inventors discovered that while vacuum mixing can reduce the problem of aerogel splashing, it also reduces the effectiveness of the foaming agent. Therefore, the present invention first performs vacuum mixing, then introduces foam and stirs under normal pressure. This achieves better mixing while fully utilizing the foaming agent, resulting in a concrete with significantly improved thermal insulation and strength.
[0043] According to an embodiment of the present invention, the conditions for vacuum stirring specifically include: stirring at an absolute pressure of less than 5 KPa; a stirring time of no more than 15 minutes; and a stirring temperature of 8° C. to 30° C.
[0044] According to an embodiment of the present invention, the aerogel is added to the raw materials of the concrete. Preferably, the aerogel can be added in multiple additions to shorten the vacuum mixing time. The number of additions can be selected based on the actual situation, for example, 2-10 additions.
[0045] According to an embodiment of the present invention, the raw material of the aerogel-modified concrete is selected from cement, including Portland cement, aluminate cement, sulphoaluminate cement, and magnesium oxychloride cement. Preferably, the cement is Portland cement of grade 42.5 or above.
[0046] According to an embodiment of the present invention, in the aerogel-modified concrete, the mass ratio of aerogel to cement is (0-50):100 and the content of the aerogel is not 0, for example, 5:100, 10:100, 15:100, 20:100, 25:100, 30:100, 35:100, 40:100, 45:100, 50:100.
[0047] According to an embodiment of the present invention, in the aerogel-modified concrete, the particle size of the aerogel is 1 nm-50 nm, preferably 20 nm-50 nm, for example, 1 nm, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm.
[0048] According to an embodiment of the present invention, the aerogel is selected from hydrophilically modified aerogels and / or hydrophobic aerogels.
[0049] The study found that when hydrophilic modified aerogel is added, it is easier to mix with concrete slurry. In addition, compared with untreated hydrophobic aerogel, the hydrophilic modified aerogel has better thermal insulation performance.
[0050] According to a preferred embodiment of the present invention, the aerogel includes hydrophilic modified aerogel and hydrophobic aerogel, wherein the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 100:(0-200) and the content of the hydrophobic aerogel is not zero.
[0051] The study found that if only hydrophilic modified aerogel is added to concrete, the problem of reduced concrete strength will occur. However, if hydrophobic aerogel is introduced at the same time as hydrophilic modified aerogel, the strength can be maintained without reducing while maintaining thermal insulation performance. That is, the mixed aerogel has better thermal insulation performance and the strength of the concrete does not decrease much. Moreover, after adding hydrophobic powder as an additive, the dispersibility of the concrete slurry can also be improved.
[0052] Preferably, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 100:(150-200), for example, 100:150, 100:160, 100:170, 100:180, 100:190, or 100:200. Studies have found that when the mass ratio of the hydrophobic aerogel to the hydrophilic modified aerogel is within the above range, the thermal insulation performance of the aerogel-modified concrete can be ensured while maintaining the mechanical strength of the aerogel-modified concrete.
[0053] According to an embodiment of the present invention, the hydrophilically modified aerogel is a hydrophilically modified aerogel particle.
[0054] According to an embodiment of the present invention, the contact angle between the hydrophilic modified aerogel and water is less than 90°. Preferably, the surface of the hydrophilic modified aerogel contains hydrophilic groups, which are selected from groups known in the art, such as hydroxyl groups (-OH).
[0055] According to an embodiment of the present invention, the contact angle of the hydrophobic aerogel with water is greater than 90°. Preferably, the surface of the hydrophobic aerogel contains hydrophobic groups, which are selected from groups known in the art, such as alkoxy groups (-OR, R represents an alkyl group).
[0056] According to an embodiment of the present invention, the auxiliary materials include water and at least one of the following substances: glass beads, a water reducing agent, reinforcing fibers, a foaming agent, and fly ash. Exemplarily, the auxiliary materials include water, glass beads, a water reducing agent, reinforcing fibers, a foaming agent, and fly ash.
[0057] According to an embodiment of the present invention, the addition amount of the auxiliary material is 0.1 to 50 parts by mass per 100 parts by mass of cement.
[0058] According to an embodiment of the present invention, per 100 parts by mass of cement, the amount of water is 20 to 100 parts by mass, for example, 20 parts by mass, 30 parts by mass, 40 parts by mass, 50 parts by mass, 60 parts by mass, 70 parts by mass, 80 parts by mass, 90 parts by mass, or 100 parts by mass.
[0059] According to the embodiment of the present invention, the water reducer can improve the fluidity of the product during molding and processing; it does not affect the performance of the product, and is non-toxic and reasonably priced.
[0060] According to an embodiment of the present invention, the water reducer is 0.01-20 parts by mass per 100 parts by mass of cement, for example, 0.1 parts by mass, 1 part by mass, 5 parts by mass, 10 parts by mass, 15 parts by mass, or 20 parts by mass.
[0061] According to an embodiment of the present invention, the water reducer is selected from calcium lignin sulfonate, sodium lignin sulfonate, magnesium lignin sulfonate, sulfonated melamine formaldehyde resin, aromatic amino sulfonate polymer, aliphatic hydroxy sulfonate polymer, HSB aliphatic high-efficiency water reducer, casein, polycarboxylic acid high-performance water reducer, polyoxyethylene dioleate, tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxyethylene sorbitol lanolin oleic acid derivative, polyoxyethylene sorbitol lanolin derivative, polyoxypropylene stearate, polyoxyethylene (5EO) lanolin ether, anhydrous sorbitan laurate, polyoxyethylene fatty acid, polyoxyethylene oxypropylene oleate, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, gur gum, fatty acid polyethylene glycol ester.
[0062] According to an embodiment of the present invention, the amount of the vitrified microspheres is 5 to 40 parts by weight, for example, 10 parts by weight, 20 parts by weight, 30 parts by weight, or 40 parts by weight, per 100 parts by weight of cement.
[0063] According to an embodiment of the present invention, the glass microspheres can be selected from materials known in the art and are not specifically limited in the present invention.
[0064] According to an embodiment of the present invention, the reinforcing fibers are selected from inorganic fibers and organic fibers, such as polyester fibers, glass fibers, basalt fibers, etc. Preferably, the reinforcing fibers are short fibers, specifically fibers with a length of 3 mm to 60 mm, such as 10 mm, 20 mm, 30 mm, 40 mm, or 50 mm.
[0065] According to an embodiment of the present invention, the reinforcing fiber is present in an amount of 0.5-5 parts by mass, for example, 0.6 parts by mass, 0.7 parts by mass, 0.8 parts by mass, or 0.9 parts by mass, per 100 parts by mass of cement. In the present invention, the reinforcing fiber is used as a skeleton filling material to increase the strength of the aerogel-modified concrete.
[0066] According to an embodiment of the present invention, before the vacuum mixing, the raw materials, auxiliary materials and aerogel of the concrete can be premixed to obtain a uniform premix. Preferably, the temperature during premixing is controlled at 8°C to 30°C.
[0067] According to an embodiment of the present invention, the mass ratio of the foaming agent to the cement is 0.1 to 10:100, for example, 0.1:100 or 5:100.
[0068] According to an embodiment of the present invention, the foaming agent can be selected from foaming agents known in the art, for example, selected from rosin resin foaming agents, synthetic surfactant foaming agents, plant protein foaming agents, animal protein foaming agents, hydrogen peroxide foaming agents, ammonium bicarbonate foaming agents, azodicarbonamide foaming agents, aluminum powder foaming agents, alkylbenzene sulfonate foaming agents, and fatty alcohol sulfonate foaming agents.
[0069] Specifically, the foaming agent can be selected from at least one of sodium lauryl sulfate, sodium rosinate, triterpenoid saponin, sodium α-olefin sulfonate, and hydrolyzed waste animal hair.
[0070] According to an embodiment of the present invention, the fly ash is in an amount of 0.5-20 parts by mass per 100 parts by mass of cement.
[0071] According to an embodiment of the present invention, the fly ash is selected from one or more of fly ash, silica fume, ground slag powder, and phosphorus slag powder. Preferably, the fly ash should be fly ash of no less than grade II.
[0072] According to an embodiment of the present invention, the vacuum stirring and stirring are respectively carried out in a high-speed stirring device. Specifically, the high-speed stirring device can be a high-speed magnetic stirrer, a free-fall stirrer or a forced stirrer.
[0073] According to an embodiment of the present invention, after the foaming agent is added and mixed evenly, hardening and curing can be further performed. Preferably, the curing can be performed using methods known in the art.
[0074] Exemplarily, the curing includes: concrete covering and moisturizing curing. Furthermore, the moisturizing curing refers to curing at 20±2°C and relative humidity of 90% or more for more than 7 days.
[0075] The present invention also provides aerogel-modified concrete obtained by the above preparation method.
[0076] According to an embodiment of the present invention, the thermal conductivity of the aerogel-modified concrete is not higher than 0.40w / (mk), for example, 0.3w / (mk), 0.2w / (mk), 0.1w / (mk), 0.07w / (mk), or 0.05w / (mk).
[0077] According to an embodiment of the present invention, the compressive strength of the aerogel-modified concrete is 1 to 10 MPa, for example, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, or 9 MPa.
[0078] The technical solutions of the present invention will be described in further detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are encompassed within the scope of protection that the present invention is intended to protect.
[0079] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0080] The reagents used in the following examples are as follows:
[0081] Cement: Commercially available Portland cement can be used, with grade 42.5 and above Portland cement being preferred.
[0082] Vitrified microbeads: particle size is 100μm~300μm.
[0083] Hydrophobic aerogel: Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000.
[0084] Water reducer: polyoxyethylene oleate, Polyshun Chemical.
[0085] Foaming agent: Sodium dodecylbenzenesulfonate, Shandong Tenghang New Material Technology Co., Ltd.
[0086] Preparation Example 1
[0087] Preparation of hydrophilic modified aerogel:
[0088] Hydrophilic modification method 1: Take the above-mentioned hydrophobic aerogel (Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000), heat it at 200-350° C. for 1-10 minutes to obtain a hydrophilic modified aerogel.
[0089] Preparation Example 2
[0090] Preparation of hydrophilic modified aerogel:
[0091] Hydrophilic Modification Method 2: Take the hydrophobic aerogel (Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000), impregnate it with ethanol, and then dry it to obtain a hydrophilic modified aerogel. This can be done naturally or by heating. The heating and drying conditions are: high temperature (90-110°C) for 1-10 minutes.
[0092] The performance of the hydrophilic modified aerogel prepared in Preparation Example 2 is basically equivalent to that in Preparation Example 1. Both hydrophilic modification methods can achieve the hydrophilic modification effect.
[0093] Example 1
[0094] The preparation method of aerogel modified concrete is as follows:
[0095] A. Preparation of a hybrid aerogel: mixing a hydrophilic modified aerogel and a hydrophobic modified aerogel in proportion to obtain an aerogel; wherein the hybrid aerogel comprises the hydrophilic modified aerogel of Preparation Example 1 and a commercially available hydrophobic aerogel, and the mass ratio of the two is 1:1;
[0096] B. The aerogel obtained in step A is pre-mixed with cement, water, auxiliary materials and aerogel, and then stirred in a mixer to obtain concrete slurry. The specific preparation method is as follows (the following parts are all by mass):
[0097] 1) Pretreatment of concrete powder: sieve commercial concrete powder through a 100-150 mesh sieve to obtain concrete powder with a particle size of 100-120 mesh;
[0098] 2) Mixing dry powder raw materials: 100 parts of the concrete powder obtained in step 1) are mixed uniformly with 5 parts of mixed aerogel (including 2.5 parts of hydrophilic modified aerogel) and auxiliary materials at 2-8° C. to obtain a dry powder mixture, wherein the auxiliary materials include: 5 parts of a water reducer;
[0099] 3) Vacuum stirring: add 20-30 parts of water to the dry powder mixture in step 2), with the water temperature at 8-10°C, and evacuate to an absolute pressure of less than 5 kPa. Maintain vacuum and stir for 2 minutes to obtain slurry A;
[0100] 4) preparing foam: mixing 3 parts of a foaming agent, sodium lauryl sulfate, with 10 parts of water to form foam;
[0101] 5) Stirring at normal pressure: Add the foam prepared in step 4) to the slurry A obtained in step 3), and stir at normal pressure again (i.e., the stirring environment is at normal pressure) for 3 minutes to obtain slurry B;
[0102] C: pouring slurry B into a mold or applying it to the surface of the target substrate, and performing hardening and curing, specifically including: covering and moisturizing curing: the curing environment temperature is 20±2°C, the relative humidity is above 90%, and curing is performed for more than 7 days to obtain the aerogel-modified concrete.
[0103] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 9.66 MPa and a thermal conductivity of 0.208 W / (m·K), which are recorded in Table 1.
[0104] Example 1-1
[0105] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 1, except that in step 2), the mixed aerogel is 5 parts, of which the hydrophilic modified aerogel is added in an amount of 1.67 parts, that is, the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 1:2.
[0106] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 9.80 MPa and a thermal conductivity of 0.221 W / (m·K), which are recorded in Table 1.
[0107] Example 2
[0108] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 1, except that in step 2), the mixed aerogel is 10 parts, of which 5 parts are hydrophilic modified aerogel, and the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 1:1.
[0109] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 8.61 MPa and a thermal conductivity of 0.138 W / (m·K), which are recorded in Table 1.
[0110] Example 2-1
[0111] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 2, except that in step 2), the mixed aerogel is 10 parts, of which the hydrophilic modified aerogel is added in an amount of 3.33 parts, and the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 1:2.
[0112] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 8.83 MPa and a thermal conductivity of 0.152 W / (m·K), which are recorded in Table 1.
[0113] Example 3
[0114] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 1, except that in step 2), the mixed aerogel is 20 parts, of which the hydrophilic modified aerogel is added in an amount of 10 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.
[0115] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 5.12 MPa and a thermal conductivity of 0.100 W / (m·K), which are recorded in Table 1.
[0116] Example 3-1
[0117] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 3, except that in step 2), the mixed aerogel is 20 parts, of which the hydrophilic modified aerogel is added in an amount of 6.67 parts, and the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 1:2.
[0118] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 5.38 MPa and a thermal conductivity of 0.110 W / (m·K), which are recorded in Table 1.
[0119] Example 4
[0120] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 1, except that in step 2), the mixed aerogel is 15 parts, of which the hydrophilic modified aerogel is added in an amount of 7.5 parts, and the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 1:1.
[0121] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 6.52 MPa and a thermal conductivity of 0.114 W / (m·K), which are recorded in Table 1.
[0122] Example 4-1
[0123] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 4, except that in step 2), the mixed aerogel is 15 parts, of which the hydrophilic modified aerogel is added in an amount of 5 parts, and the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 1:2.
[0124] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 6.75 MPa and a thermal conductivity of 0.125 W / (m·K), which are recorded in Table 1.
[0125] Example 5
[0126] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 1, except that in step 2), the mixed aerogel is 25 parts, of which the hydrophilic modified aerogel is added in an amount of 12.5 parts, and the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 1:1.
[0127] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 4.20 MPa and a thermal conductivity of 0.094 W / (m·K), which are recorded in Table 1.
[0128] Example 5-1
[0129] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 5, except that in step 2), the mixed aerogel is 25 parts, of which the hydrophilic modified aerogel is added in an amount of 8.3 parts, and the mass ratio of hydrophilic modified aerogel to hydrophobic aerogel is 1:2.
[0130] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 4.42 MPa and a thermal conductivity of 0.101 W / (m·K), which are recorded in Table 1.
[0131] Example 6
[0132] The preparation method of the aerogel-modified concrete of this embodiment is basically the same as that of Example 1, except that only the hydrophilic modified aerogel of Preparation Example 1 is used in step A;
[0133] In step B, step 2) uses the hydrophilic modified aerogel of Preparation Example 1.
[0134] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 9.41 MPa and a thermal conductivity of 0.176 W / (m·K), which are recorded in Table 1.
[0135] Example 7
[0136] The preparation method of aerogel-modified concrete in this embodiment is basically the same as that in Example 1, except that only commercially available hydrophobic aerogel is used in step A;
[0137] In step B, step 2) uses commercially available hydrophobic aerogel.
[0138] The test shows that the aerogel-modified concrete of this embodiment has a compressive strength of 10.01 MPa and a thermal conductivity of 0.236 W / (m·K), which are recorded in Table 1.
[0139] Comparative Example 1
[0140] This comparative example is basically the same as Example 2, except that:
[0141] In step 3), the foam prepared in step 4) was also added, and no vacuum operation was performed. The mixture was directly stirred at normal pressure for 5 minutes to directly obtain slurry B.
[0142] The test shows that the compressive strength of the aerogel-modified concrete in this comparative example is 7.83 MPa and the thermal conductivity is 0.184 W / (m·K), which are recorded in Table 1.
[0143] Comparative Example 2
[0144] This comparative example is basically the same as Example 2-1, except that:
[0145] In step 3), the foam prepared in step 4) was also added, and no vacuum operation was performed. The mixture was directly stirred at normal pressure for 5 minutes to directly obtain slurry B.
[0146] The test shows that the compressive strength of the aerogel-modified concrete in this comparative example is 8.03 MPa and the thermal conductivity is 0.203 W / (m·K), which are recorded in Table 1.
[0147] Comparative Example 3
[0148] This comparative example is basically the same as Example 2, except that only hydrophilic modified aerogel is used in step 2), and the addition amount thereof is 10 parts.
[0149] In step 3), the foam prepared in step 4) was also added, and no vacuum operation was performed. The mixture was directly stirred at normal pressure for 5 minutes to directly obtain slurry B.
[0150] The test shows that the compressive strength of the aerogel-modified concrete in this comparative example is 7.61 MPa and the thermal conductivity is 0.158 W / (m·K), which are recorded in Table 1.
[0151] Comparative Example 4
[0152] This comparative example is basically the same as Example 2, except that only hydrophobic aerogel is used in step 2), and the amount of hydrophobic aerogel added is 10 parts.
[0153] In step 3), the foam prepared in step 4) was also added, and no vacuum operation was performed. The mixture was directly stirred at normal pressure for 5 minutes to directly obtain slurry B.
[0154] The test shows that the compressive strength of the aerogel-modified concrete in this comparative example is 8.16 MPa and the thermal conductivity is 0.211 W / (m·K), which are recorded in Table 1.
[0155] Table 1
[0156] The above describes exemplary embodiments of the present invention. However, the scope of protection of this application is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc. made by those skilled in the art within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing aerogel-modified concrete, It is characterized in that The preparation method comprises: mixing aerogel with raw materials and auxiliary materials of concrete under vacuum stirring conditions, and then introducing foam under normal pressure conditions and mixing them evenly to obtain the aerogel modified concrete.
2. The preparation method according to claim 1, It is characterized in that The vacuum stirring conditions specifically include: stirring under an absolute pressure of less than 5 KPa; stirring time is no more than 15 min; stirring temperature is 8° C. to 30° C.
3. The preparation method according to claim 2, It is characterized in that The raw material of the concrete is selected from cement; In the aerogel-modified concrete, the mass ratio of aerogel to concrete is (0-30):100 and the content of the aerogel is not 0; In the aerogel-modified concrete, the particle size of the aerogel is 1nm-50nm; The aerogel is selected from hydrophilically modified aerogels and / or hydrophobic aerogels.
4. The preparation method according to claim 3, It is characterized in that The aerogel includes hydrophilic modified aerogel and hydrophobic aerogel, wherein the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 100:(0-200) and the content of the hydrophobic aerogel is not zero.
5. The preparation method according to claim 4, It is characterized in that The hydrophilic modified aerogel is a hydrophilic modified aerogel particle; The contact angle between the hydrophilic modified aerogel and water is less than 90°; The contact angle between the hydrophobic aerogel and water is greater than 90°.
6. The preparation method according to claim 5, It is characterized in that The preparation method of the hydrophilic modified aerogel is to heat the hydrophobic aerogel at 200 to 350° C. for 1 to 10 minutes.
7. The preparation method according to claim 6, It is characterized in that The auxiliary materials include water and at least one of the following substances: vitrified microspheres, water reducing agent, fly ash, and reinforcing fiber; And / or, the amount of the auxiliary material added is 0.1 to 200 parts by mass per 100 parts by mass of cement.
8. The preparation method according to claim 7, It is characterized in that For every 100 parts by mass of cement, the amount of water is 100 to 120 parts by mass; And / or, the water reducing agent is 0.01-5 parts by mass per 100 parts by mass of cement; And / or, the vitrified microspheres are 5-40 parts by mass per 100 parts by mass of cement; And / or, the fly ash is 0.5-20 parts by mass per 100 parts by mass of cement; And / or, based on every 100 parts by mass of cement, the reinforcing fiber is 0.5-5 parts by mass.
9. The preparation method according to claim 8, It is characterized in that The thermal conductivity of the aerogel modified concrete is not higher than 0.30w / (mk).
10. The preparation method according to claim 9, It is characterized in that The reinforcing fibers are selected from inorganic fibers and organic fibers.
11. The preparation method according to claim 10, It is characterized in that Before the vacuum mixing, the raw materials, auxiliary materials and aerogel of the concrete are premixed to obtain a uniform premix.
12. The preparation method according to claim 11, It is characterized in that The mass ratio of the foaming agent to the cement is 0.1-10:100.
Citation Information
Patent Citations
Super-thermal-insulation aerogel foamed concrete and preparation method thereof
CN107265962A
Super-thermal-insulation aerogel foamed concrete and preparation method thereof
CN107265963A
Aerogel foam concrete and preparation method and application thereof
CN110803938A
Foam concrete and preparation method thereof
CN113603423A
Carbon sequestration thermal insulation concrete and preparation method thereof
CN115304398A