Method for full-chain integrated recycling of lithium and graphite in spent batteries
By roasting and water leaching lithium combined with the flotation process, the problem of low recovery rate of lithium and graphite is solved, efficient recovery is achieved, the process is simplified, energy consumption is reduced, and resource waste is avoided.
Patent Information
- Application Number
- PCT/CN2023/088906
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
In the existing battery recycling process, the recovery rate of lithium and graphite is low, resulting in a waste of resources, and the pyrometallurgical process consumes high energy and fails to effectively recover lithium and graphite in used batteries.
By roasting the battery black powder of used batteries and leaching lithium with water, combined with the flotation process, using graphite collectors, flocculants and foaming agents for flotation, the efficient recovery of lithium and graphite is achieved, using closed-circuit selection and The sweeping process increases recovery rates.
A high recovery rate of lithium and graphite is achieved, resource waste is avoided, the process is simplified, energy consumption is reduced, and recovery efficiency is improved.
Smart Images

Figure CN2023088906_24102024_PF_FP_ABST
Abstract
Description
A full-chain integrated method for recycling lithium and graphite from waste batteries Technical Field
[0001] The present disclosure relates to the technical field of battery recycling, and in particular to a method for recycling lithium and graphite from waste batteries through a full-chain integrated approach. Background Art
[0002] With the rapid development of the new energy industry, the price of battery-grade lithium carbonate has risen from nearly 50,000 yuan / ton at the beginning of 2021 to 300,000 yuan / ton in March 2023. During this period, the price once exceeded 550,000 yuan / ton.
[0003] Currently, the recycling processes for used ternary lithium batteries are primarily divided into disassembly and hydrometallurgy, and pyrometallurgy. Hydrometallurgy involves leaching battery black powder with organic or inorganic acids and reducing agents. However, the lithium recovery rate is generally below 80%, and the graphite used in this process is treated as hazardous waste, resulting in significant resource waste. Pyrometallurgy, on the other hand, suffers from high energy consumption and the inability to recover lithium and graphite.
[0004] By recycling valuable metals and graphite from used batteries, returning them to the battery, achieving full component recovery and building a "full-chain integrated industrial park," costs can be reduced, efficiency can be increased, and resource waste can be avoided. However, currently, there is no method that can effectively and simultaneously recover both lithium and graphite from used batteries.
[0005] In view of this, the present disclosure is proposed.
[0006] Summary of the Invention
[0007] The purpose of the present disclosure is to provide a full-chain integrated method for recycling lithium and graphite from waste batteries. The method is simple and easy to implement, and can effectively recycle lithium and graphite in waste batteries. The recovery rates of lithium and graphite are both high, avoiding waste of resources.
[0008] In order to achieve the above-mentioned purpose of the present disclosure, the following technical solutions can be adopted:
[0009] The present disclosure provides a method for recycling lithium and graphite from waste batteries in an integrated and comprehensive manner, comprising the following steps:
[0010] The battery black powder obtained from the waste batteries is roasted and water-leached to extract lithium, and the leached residue is floated;
[0011] The flotation process includes: performing a roughing process on the water-soaked residue using a flotation agent to obtain a roughing foam material and a roughing liquid material; performing at least one fine separation on the roughing foam material to finally obtain a carbonaceous concentrate;
[0012] Flotation agents include graphite collectors, regulators and foaming agents; regulators include flocculants.
[0013] In some embodiments of the present disclosure, the graphite collector includes at least one of kerosene and diesel;
[0014] and / or, the flocculant comprises at least one of starch, sodium carboxymethyl cellulose and dextrin;
[0015] And / or, the foaming agent includes at least one of methyl isobutyl carbinol, pine oil and sec-octanol.
[0016] In some embodiments of the present disclosure, the amount of graphite collector is 50 g / t-500 g / t; and / or the amount of flocculant is 500 g / t-2000 g / t; and / or the amount of foaming agent is 50 g / t-400 g / t.
[0017] In some embodiments of the present disclosure, the regulator further includes at least one of a pH adjuster and a stabilizer.
[0018] In some embodiments of the present disclosure, the pH adjuster includes at least one of calcium oxide, calcium carbonate, calcium hydroxide, sodium carbonate, and sodium hydroxide;
[0019] And / or, the stabilizer includes at least one of aluminum sulfate, aluminum nitrate, aluminum chloride, polyaluminum chloride, ferric sulfate, ferric nitrate, ferrous sulfate, ferric chloride, ferrous chloride, magnesium nitrate, magnesium chloride and magnesium sulfate.
[0020] In some embodiments of the present disclosure, the amount of the pH adjuster is 200 g / t-4000 g / t, and / or the amount of the stabilizer is 200 g / t-2000 g / t.
[0021] In some embodiments of the present disclosure, the number of times of selection is n, where n≥2 and is an integer; during the first n-1 selection processes, the n-1th selected foam material and the n-1th selected middlings are obtained after each selection; the n-1th selected foam material is used as the raw material to be selected for the nth selection.
[0022] In some embodiments of the present disclosure, when n=2, the first concentrated middlings obtained from the first concentration are returned to the roughing process as the raw material to be selected.
[0023] In some embodiments of the present disclosure, when n=2, the second beneficiated middlings obtained in the second beneficiation are returned to the first beneficiation process as a raw material to be selected.
[0024] In some embodiments of the present disclosure, when n≥3, the n-1th concentrated middlings obtained from the n-1th concentration are returned to the n-2th concentration process as a raw material to be selected.
[0025] In some embodiments of the present disclosure, the n-th concentrated middlings obtained from the n-th concentration are returned to the (n-1)-th concentration process as raw materials to be selected.
[0026] In some embodiments of the present disclosure, when the selected middlings are returned to the second selection process as raw materials to be selected, the foam material from the first selection is combined with the middlings from the third selection for grinding and scrubbing before the second selection.
[0027] In some embodiments of the present disclosure, the scrubbing time is 2 min to 15 min.
[0028] In some embodiments of the present disclosure, the concentrator used in each concentrating step independently includes a graphite collector and a foaming agent.
[0029] In some embodiments of the present disclosure, the graphite collector used in each beneficiation process includes at least one of kerosene and diesel;
[0030] And / or, the foaming agent used in each beneficiation process includes at least one of methyl isobutyl carbinol, pine oil and secondary octanol.
[0031] In some embodiments of the present disclosure, the amount of graphite collector used in each beneficiation process is 0-150 g / t; and / or the amount of foaming agent used in each beneficiation process is 0-150 g / t.
[0032] In some embodiments of the present disclosure, flotation further comprises: subjecting the roughing slurry to at least one scavenging step to ultimately obtain carbonaceous tailings.
[0033] In some embodiments of the present disclosure, the number of sweeps is m, where m≥2 and is an integer; during the first m-1 sweeps, the m-1th sweep residual slurry and the m-1th sweep foam middlings are obtained after each sweep; the m-1th sweep residual slurry is used as the raw material to be selected for the mth sweep.
[0034] In some embodiments of the present disclosure, when m=2, the first scavenged foam middlings obtained in the first scavenging are returned to the roughing process as the raw material to be selected.
[0035] In some embodiments of the present disclosure, when m=2, the second scavenging foam middlings obtained in the second scavenging are returned to the first scavenging process as a raw material to be selected.
[0036] In some embodiments of the present disclosure, when m≥3, the m-1th scavenging foam middlings obtained in the m-1th scavenging are returned to the m-2th scavenging process as a raw material to be selected.
[0037] In some embodiments of the present disclosure, the m-th scavenging foam middlings obtained in the m-th scavenging are returned to the m-1-th scavenging process as a raw material to be selected.
[0038] In some embodiments of the present disclosure, the scavenging agent used in each scavenging independently includes a graphite collector and a foaming agent.
[0039] In some embodiments of the present disclosure, the graphite collector used in each sweeping process includes at least one of kerosene and diesel;
[0040] And / or, the foaming agent used in each sweeping process includes at least one of methyl isobutyl carbinol, pine oil and sec-octanol.
[0041] In some embodiments of the present disclosure, the amount of graphite collector used in each scavenging process is 0-150 g / t; and / or the amount of foaming agent used in each scavenging process is 0-150 g / t.
[0042] In some embodiments of the present disclosure, the number of rough selections is 1, the number of fine selections is 4, and the number of sweep selections is 2.
[0043] In some embodiments of the present disclosure, the main sources of battery black powder include positive electrode materials containing lithium and negative electrode materials containing graphite.
[0044] In some embodiments of the present disclosure, the source of battery black powder further includes at least one of a current collector and battery impurities.
[0045] In some embodiments of the present disclosure, the current collector includes copper foil or aluminum foil.
[0046] In some embodiments of the present disclosure, in terms of mass percentage, the battery black powder has a fixed carbon content of 30%-55%, a Li content of 3%-7%, a Ni content of 10%-35%, a Co content of 2%-5%, a Mn content of 2%-5%, a Cu content of 0.055-1%, an Al content of 0.05%-1%, and a Fe content of 0.05%-1%.
[0047] In some embodiments of the present disclosure, the preparation of battery black powder includes: discharging, crushing, cracking and screening waste batteries.
[0048] In some embodiments of the present disclosure, firing includes at least one of the following features:
[0049] Feature 1: Calcination temperature is 400℃-800℃;
[0050] Feature 2: Calcination time is 30min-180min;
[0051] Feature 3: Calcination is carried out in an oxygen-free environment.
[0052] In some embodiments of the present disclosure, the oxygen-free environment is provided by nitrogen or an inert gas.
[0053] In some embodiments of the present disclosure, water leaching of lithium includes a water leaching process, and the water leaching includes at least one of the following characteristics:
[0054] Feature 1: The solid-liquid ratio of water immersion is 1:3-1:10;
[0055] Feature 2: The water immersion temperature is 25℃-90℃;
[0056] Feature 3: The immersion time is 30min-120min;
[0057] Feature 4: Water immersion is carried out under stirring conditions.
[0058] In some embodiments of the present disclosure, the stirring speed during the water immersion process is 500 rpm-2000 rpm.
[0059] In some embodiments of the present disclosure, water leaching of lithium further includes a lithium extraction process, and the lithium extraction method includes evaporating the water leaching liquid obtained in the water leaching process.
[0060] In some embodiments of the present disclosure, evaporation is performed by water bath evaporation.
[0061] In some embodiments of the present disclosure, the temperature of the water bath evaporation is 80°C-100°C.
[0062] In some embodiments of the present disclosure, the process further includes dispersing the water-soaked residue before flotation.
[0063] In some embodiments of the present disclosure, the dispersion is in the form of ultrasonic dispersion.
[0064] In some embodiments of the present disclosure, ultrasonic dispersion includes at least one of the following features:
[0065] Feature 1: Ultrasonic dispersion is carried out by mixing the water-soaked residue with water at a liquid-to-solid ratio of 1:3-1:10;
[0066] Feature 2: Ultrasonic stirring intensity is 300rpm-1000rpm;
[0067] Feature 3: Ultrasonic dispersion time is 5min-20min.
[0068] In some embodiments of the present disclosure, after flotation, the flotation tailings product is further subjected to post-processing;
[0069] Post-processing includes acid leaching, impurity removal and extraction.
[0070] The present invention achieves a high lithium leaching rate by calcining and water-leaching battery black powder obtained from waste batteries to extract lithium. The resulting water-leached residue is subjected to a specific flotation process. The frother used in this flotation process increases the amount of foam, facilitating flotation. The flocculant used acts on the water-leached residue to cause flocculation, and the graphite collector then effectively captures the graphite.
[0071] This method is simple and easy to implement, and can effectively recycle lithium and graphite in waste batteries. The recovery rates of lithium and graphite are both high, avoiding waste of resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0073] FIG1 is an overall flow chart of the full-chain integrated method for recycling lithium and graphite from waste batteries provided by the present disclosure;
[0074] FIG2 is a flow chart of the flotation process in the full-chain integrated method for recovering lithium and graphite from waste batteries provided by the present disclosure. DETAILED DESCRIPTION
[0075] To make the purpose, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions in the embodiments of the present disclosure are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer were followed. Reagents or instruments used where the manufacturer is not specified are conventional products that can be purchased commercially.
[0076] The following is a detailed description of the full-chain integrated method for recycling lithium and graphite from waste batteries provided by the present invention.
[0077] Please refer to Figure 1 and Figure 2 together. The present disclosure proposes a full-chain integrated method for recovering lithium and graphite from waste batteries, including the following steps: roasting and water-leaching the battery black powder obtained from the waste batteries to extract lithium, and flotating the leached residue.
[0078] For reference, the main sources of battery black powder may include positive electrode materials containing lithium and negative electrode materials containing graphite.
[0079] Illustratively, the lithium-containing cathode material may include at least one of a binary cathode material, a ternary cathode material, a quaternary cathode material, and a higher-order cathode material.
[0080] In some embodiments, the metal elements contained in the binary positive electrode material may be, for example but not limited to, nickel and cobalt; the elements contained in the ternary positive electrode material may be, for example but not limited to, nickel, cobalt, and manganese; and the elements contained in the quaternary positive electrode material may be, for example but not limited to, nickel, cobalt, manganese, and aluminum.
[0081] Furthermore, the source of the battery black powder may also include at least one of the current collector and battery impurities.
[0082] The current collector may include, for example, copper foil or aluminum foil, etc. Battery impurities may include, for example, iron filings, etc.
[0083] For reference, in terms of mass percentage, the fixed carbon content in the battery black powder can be 30%-55% (such as 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52% or 55%, etc.), the Li content can be 3%-7% (such as 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5% or 7%, etc.), the Ni content can be 10%-35% (such as 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32% or 35%, etc.), and the Co content can be 2%-5% (such as 2%, 2.5 %, 3%, 3.5%, 4%, 4.5% or 5%, etc.), the Mn content may be 2%-5% (such as 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc.), the Cu content may be 0.055-1% (such as 0.055%, 0.01%, 0.02%, 0.05%, 0.1%, 0.2%, 0.5%, 0.8% or 1%, etc.), the Al content may be 0.05%-1% (such as 0.05%, 0.08%, 0.1%, 0.2%, 0.5%, 0.8% or 1%, etc.), and the Fe content may be 0.05%-1% (such as 0.05%, 0.08%, 0.1%, 0.2%, 0.5%, 0.8% or 1%, etc.).
[0084] It should be noted that, depending on the usage of the waste batteries, the chemical composition and content of the battery black powder obtained therefrom are not limited to the above ranges and can be determined according to the circumstances.
[0085] In some optional embodiments, the preparation of battery black powder may include: discharging, crushing, cracking and screening the waste batteries.
[0086] The above-mentioned discharge, fragmentation and cracking can all be carried out in conventional ways, which will not be described in detail here.
[0087] For reference, during the calcination process, the calcination temperature can be 400℃-800℃, such as 400℃, 450℃, 500℃, 550℃, 600℃, 650℃, 700℃, 750℃ or 800℃, etc., or any other value within the range of 400℃-800℃.
[0088] The calcination time may be 30 min-180 min, such as 30 min, 50 min, 80 min, 100 min, 120 min, 150 min or 180 min, or any other value within the range of 30 min-180 min.
[0089] In some specific optional embodiments, the calcination temperature may be 500° C., and the calcination time may be 180 min.
[0090] In some preferred embodiments, the calcination is performed in an oxygen-free environment, which can be provided by nitrogen or an inert gas (such as argon or helium).
[0091] It should be noted that the present invention does not use any additives during the calcination process. Instead, the battery black powder is calcined directly in an oxygen-free environment, eliminating the introduction of other impurity ions and facilitating subsequent impurity removal. Furthermore, the calcination process removes binders (such as PVDF) from the positive electrode active material, significantly improving the surface floatability difference between the positive and negative electrode active materials, facilitating flotation separation of the positive and negative electrode materials.
[0092] For reference, water leaching of lithium includes a water leaching process, and the solid-liquid ratio of the water leaching process can be 1:3-1:10, such as 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, or any other value within the range of 1:3-1:10.
[0093] The water immersion temperature may be 25° C.-90° C., such as 25° C., 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., or 90° C., or any other value within the range of 25° C.-90° C. In some further optional embodiments, the water immersion temperature is 25° C.-90° C.
[0094] The immersion time may be 30 min-120 min, such as 30 min, 50 min, 80 min, 100 min or 120 min, or any other value within the range of 30 min-120 min.
[0095] In some preferred embodiments, water immersion is performed under stirring conditions to improve the water immersion effect, which is beneficial to increasing the lithium leaching rate.
[0096] Illustratively, the stirring speed during the water immersion process may be 500 rpm-2000 rpm, such as 500 rpm, 800 rpm, 1000 rpm, 1200 rpm, 1500 rpm, 1800 rpm or 2000 rpm.
[0097] It should be noted that the above-mentioned water immersion process may be performed only once, or may be repeated multiple times as needed.
[0098] In some specific optional embodiments, the water immersion solid-liquid ratio may be 1:5, the water immersion temperature may be 80° C., the water immersion time may be 60 min, the stirring speed may be 1500 rpm, and the water immersion times may be 2 times.
[0099] As mentioned above, the water immersion process adopts higher stirring intensity and higher temperature, which is beneficial to improving the lithium leaching rate on the one hand, and on the other hand, the surface of the positive and negative active materials is more completely exposed under high-intensity stirring, which is beneficial to further increase the surface differences of the positive and negative electrode materials.
[0100] Furthermore, water leaching of lithium also includes a lithium extraction process, and the lithium extraction method includes evaporating the water leaching liquid obtained in the water leaching process, which can also be understood as evaporation of lithium.
[0101] For example, the evaporation can be performed by water bath evaporation.
[0102] The temperature of the water bath evaporation can be 80°C-100°C, such as 80°C, 85°C, 90°C, 95°C or 100°C, etc. until the water is completely evaporated.
[0103] In some specific optional embodiments, the temperature of the water bath evaporation is 90°C.
[0104] As mentioned above, water leaching can directly produce high-purity lithium-containing materials with a recovery rate exceeding 80%. The remaining lithium enters the subsequent acid leaching process through flotation, and the final lithium recovery rate of the entire process is ≥93%.
[0105] In the present disclosure, the water-leached residue may be dispersed before flotation.
[0106] For reference, the dispersion form may be ultrasonic dispersion.
[0107] In some embodiments, ultrasonic dispersion can be performed by mixing the water-soaked residue with water at a liquid-to-solid ratio of 1:3-1:10 (such as 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, etc.).
[0108] The ultrasonic stirring intensity may be 300 rpm-1000 rpm, such as 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm or 1000 rpm, or any other value within the range of 300 rpm-1000 rpm.
[0109] The ultrasonic dispersion time can be 5 min-20 min, such as 5 min, 8 min, 10 min, 12 min, 15 min, 18 min or 20 min, etc., or any other value within the range of 5 min-20 min.
[0110] In some specific optional embodiments, the solid-liquid ratio corresponding to ultrasonic dispersion can be 1:5, the stirring intensity can be 500 rpm, and the dispersion time can be 10 min.
[0111] By dispersing the water-soaked residue before flotation, it is more conducive to the subsequent flotation separation of graphite.
[0112] In the present disclosure, flotation may be performed in a flotation machine.
[0113] For reference, flotation includes: using a flotation agent to perform a roughing of the water-leached residue to obtain a roughing foam material and a roughing liquid material; and performing at least one fine separation of the roughing foam material to finally obtain a carbonaceous concentrate.
[0114] The flotation agents used in the roughing process may include graphite collectors, conditioning agents and frothers; conditioning agents include flocculants.
[0115] The graphite collector may, by way of example but not limitation, include at least one of kerosene and diesel. The flocculant may, by way of example but not limitation, include at least one of starch (preferably soluble starch, such as corn starch), sodium carboxymethyl cellulose, and dextrin. The foaming agent may, by way of example but not limitation, include at least one of methyl isobutyl carbinol (MIBC), pine oil, and octanol.
[0116] In some embodiments, the amount of the graphite collector used in the roughing process can be 50 g / t-500 g / t, such as 50 g / t, 80 g / t, 100 g / t, 150 g / t, 200 g / t, 250 g / t, 300 g / t, 350 g / t, 400 g / t, 450 g / t or 500 g / t, or any other value within the range of 50 g / t-500 g / t.
[0117] If the amount of graphite collector is less than 50g / t, it is not conducive to the quality of graphite products and the recovery rate is low; if it is higher than 500g / t, it is not conducive to the fixed carbon content of graphite products.
[0118] During the roughing process, the dosage of the flocculant can be 500g / t-2000g / t, such as 500g / t, 800g / t, 1000g / t, 1200g / t, 1500g / t, 1800g / t or 2000g / t, or any other value within the range of 500g / t-2000g / t.
[0119] If the dosage of flocculant is lower than 500g / t, it is not conducive to the quality of graphite products; if it is higher than 2000g / t, it is not conducive to the low graphite recovery rate.
[0120] During the roughing process, the amount of the foaming agent can be 50g / t-400g / t, such as 50g / t, 100g / t, 150g / t, 200g / t, 250g / t, 300g / t, 350g / t or 400g / t, or any other value within the range of 50g / t-400g / t.
[0121] If the amount of foaming agent is less than 50g / t, it is not conducive to the recovery rate of graphite products; if it is higher than 400g / t, it is not conducive to the quality of graphite products.
[0122] Furthermore, the regulator used in the roughing process may also include at least one of a pH regulator and a stabilizer.
[0123] The pH adjuster may illustratively but not limitatively include at least one of calcium oxide, calcium carbonate, calcium hydroxide, sodium carbonate and sodium hydroxide.
[0124] The stabilizer may illustratively but not limitatively include at least one of aluminum sulfate, aluminum nitrate, aluminum chloride, polyaluminum chloride, ferric sulfate, ferric nitrate, ferrous sulfate, ferric chloride, ferrous chloride, magnesium nitrate, magnesium chloride, and magnesium sulfate.
[0125] In some embodiments, the amount of the pH adjuster used in the roughing process can be 200 g / t-4000 g / t, such as 200 g / t, 500 g / t, 800 g / t, 1000 g / t, 1500 g / t, 2000 g / t, 2500 g / t, 3000 g / t, 3500 g / t or 4000 g / t, or any other value within the range of 200 g / t-4000 g / t.
[0126] If the amount of pH regulator is less than 200g / t, it is not conducive to the quality of graphite products; if it is higher than 4000g / t, it is not conducive to the quality of graphite products.
[0127] During the roughing process, the amount of the stabilizer can be 200 g / t-2000 g / t, such as 200 g / t, 500 g / t, 800 g / t, 1000 g / t, 1200 g / t, 1500 g / t, 1800 g / t or 2000 g / t, or any other value within the range of 200 g / t-2000 g / t.
[0128] If the amount of stabilizer is less than 200g / t, it is not conducive to the recovery rate of graphite products; if it is higher than 2000g / t, it is not conducive to the quality of graphite products.
[0129] In some specific optional embodiments, the graphite collector used in the roughing process is kerosene, the flocculant is starch, the foaming agent is MIBC, the pH adjuster is calcium oxide, and the stabilizer is aluminum sulfate; wherein the amount of kerosene is 212 g / t, the amount of starch is 1500 g / t, the amount of MIBC is 174 g / t, the amount of calcium oxide is 2000 g / t, and the amount of aluminum sulfate is 1000 g / t.
[0130] Continuing from the above, the principles of the roughing process include: the frother increases the foam volume, facilitating flotation; the flocculant acts on the water-leached residue (e.g., cobalt-manganese products), causing flocculation, which is then effectively captured by the graphite collector. The pH adjuster complements the flocculant to enhance the flocculation effect; the stabilizer increases the foam half-life, so increasing the amount of foam stabilizer can reduce the amount of frother.
[0131] Furthermore, the foam material obtained by rough selection is finely selected.
[0132] The preset number of selections is n times, where n≥2 and is an integer. For example, n can be 1, or 2, 3, 4 or more.
[0133] During the first n-1 rounds of selection, the n-1th round of selected foam material and the n-1th round of selected middlings are obtained after each selection; the n-1th round of selected foam material is used as the raw material to be selected for the nth round of selection (i.e., the next round of selection).
[0134] When n=2, the first-stage concentrated middlings obtained in the first concentration can be returned to the roughing process as a raw material to be selected. Furthermore, the second-stage concentrated middlings obtained in the second concentration can be returned to the first concentration process as a raw material to be selected.
[0135] When n≥3, the n-1th selected middlings obtained in the n-1th selection can be returned to the n-2th selection process as a raw material to be selected. Furthermore, the nth selected middlings obtained in the nth selection can also be returned to the n-1th selection process as a raw material to be selected.
[0136] By adopting a closed-circuit concentration method, that is, the middlings obtained from the concentration are not discharged, the recovery rate can be improved.
[0137] In some embodiments, when there is a selected middling ore returned to the second selection process as a raw material to be selected, before the second selection is carried out, the foam material of the first selection is combined with the middling ore of the third selection (i.e., the third selected middling ore obtained by the third selection) for grinding and scrubbing.
[0138] The scrubbing time can be illustratively 2 min-15 min, such as 2 min, 5 min, 8 min, 10 min, 12 min or 15 min, etc. In some specific optional embodiments, the scrubbing time can be 5 min.
[0139] Grinding and scrubbing can be carried out in equipment such as vertical mills or ball mills.
[0140] Grinding and scrubbing can create a fresh surface for graphite, which is beneficial to increasing the fixed carbon content of graphite products.
[0141] In the present disclosure, the concentrator used in each concentrating step may independently include a graphite collector and a foaming agent.
[0142] The graphite collector used in each beneficiation process may exemplarily but not limited to include at least one of kerosene and diesel. The foaming agent used in each beneficiation process may exemplarily but not limited to include at least one of methyl isobutyl carbinol, pine oil and sec-octanol.
[0143] In some embodiments, the amount of graphite collector used in each beneficiation process may be 0-150 g / t, such as 0 g / t, 5 g / t, 10 g / t, 20 g / t, 50 g / t, 80 g / t, 100 g / t, 120 g / t or 150 g / t, or any other value within the range of 0-150 g / t.
[0144] The amount of the foaming agent used in each beneficiation process can be 0-150 g / t, such as 0 g / t, 5 g / t, 10 g / t, 20 g / t, 50 g / t, 80 g / t, 100 g / t, 120 g / t or 150 g / t, or any other value within the range of 0-150 g / t.
[0145] In some specific optional embodiments, the graphite collector used in each beneficiation process may be kerosene, and the foaming agent may be MIBC. For example, in a four-pass beneficiation process, the amount of kerosene used in the first beneficiation process may be 53 g / t, and the amount of MIBC used may be 58 g / t; the amount of kerosene used in the second beneficiation process may be 53 g / t, and the amount of MIBC used may be 58 g / t; the amount of kerosene used in the third beneficiation process may be 53 g / t, and the amount of MIBC used may be 29 g / t; and the amount of kerosene used in the fourth beneficiation process may be 26.5 g / t, and the amount of MIBC used may be 0 g / t.
[0146] Furthermore, the flotation may also include: subjecting the roughing slurry to at least one scavenging process to finally obtain carbonaceous tailings.
[0147] The preset number of scanning times is m times, where m≥2 and is an integer. For example, m can be 1, or 2, 3, 4 or more.
[0148] During the first m-1 sweeping processes, the m-1th sweeping residual slurry and the m-1th sweeping foam middlings are obtained after each sweeping process; the m-1th sweeping residual slurry is used as the raw material to be selected for the mth sweeping process (i.e., the next sweeping process).
[0149] When m=2, the first scavenged foam middlings obtained in the first scavenging can be returned to the roughing process as a raw material to be selected. Furthermore, the second scavenged foam middlings obtained in the second scavenging can be returned to the first scavenging process as a raw material to be selected.
[0150] When m≥3, the m-1th scavenging foam middlings obtained in the m-1th scavenging can be returned to the m-2th scavenging process as a raw material to be selected. Furthermore, the mth scavenging foam middlings obtained in the mth scavenging can also be returned to the m-1th scavenging process as a raw material to be selected.
[0151] In the present disclosure, the scavenging agent used in each scavenging process may independently include a graphite collector and a foaming agent.
[0152] The graphite collector used in each scavenging process may exemplarily but not limited to include at least one of kerosene and diesel. The foaming agent used in each scavenging process may exemplarily but not limited to include at least one of methyl isobutyl carbinol, pine oil and sec-octanol.
[0153] In some embodiments, the amount of graphite collector used in each sweeping process may be 0-150 g / t, such as 0 g / t, 5 g / t, 10 g / t, 20 g / t, 50 g / t, 80 g / t, 100 g / t, 120 g / t or 150 g / t, or any other value within the range of 0-150 g / t.
[0154] The amount of foaming agent used in each sweeping process can be 0-150 g / t, such as 0 g / t, 5 g / t, 10 g / t, 20 g / t, 50 g / t, 80 g / t, 100 g / t, 120 g / t or 150 g / t, or any other value within the range of 0-150 g / t.
[0155] If the amount of graphite collector used in each scavenging process is higher than 150g / t, it is not conducive to the quality of graphite products; if the amount of foaming agent used in each scavenging process is higher than 150g / t, it is not conducive to the quality of graphite products.
[0156] In some specific optional embodiments, the graphite collector used in each scavenging process may be kerosene, and the foaming agent may be MIBC. For example, if the scavenging process is performed twice, the amount of kerosene used in the first scavenging process may be 106 g / t, and the amount of MIBC used may be 58 g / t; the amount of kerosene used in the second scavenging process may be 53 g / t, and the amount of MIBC used may be 58 g / t.
[0157] In some specific optional embodiments of the present disclosure, the number of roughing selections is 1, the number of fine selections is 4, and the number of scavenging selections is 2, that is, the corresponding flotation process is a "one roughing, four fine selections, and two scavenging" process.
[0158] Continuing from the above, the flotation process disclosed herein utilizes a flocculation flotation process. By adding reagents to the water-leached residue (e.g., cobalt-manganese products), it causes flocculation and suppresses its floatability, further enhancing the flotation separation efficiency of graphite. The addition of stabilizers during flotation stabilizes the flotation foam, increasing its half-life and reducing the amount of graphite collector and frother used.
[0159] Furthermore, after flotation, the flotation tailings product may be subjected to post-processing, such as acid leaching, impurity removal, and extraction.
[0160] It should be noted that the specific processing procedures and conditions involved in the above post-processing can refer to the corresponding conventional operations and will not be elaborated on here.
[0161] The features and performance of the present disclosure are further described in detail below with reference to the embodiments.
[0162] Example 1
[0163] Referring to FIG. 1 and FIG. 2 , this embodiment provides a method for recycling lithium and graphite from waste batteries in an integrated manner, including the following steps:
[0164] S1: Discharge, crush, crack and screen the waste ternary lithium batteries to obtain battery black powder (i.e. feed ore).
[0165] The sources of the battery black powder include nickel cobalt lithium manganese oxide ternary positive electrode material, graphite negative electrode material, current collector copper foil and aluminum foil, and battery impurities (iron filings).
[0166] In terms of mass percentage, the battery black powder has a fixed carbon content of 44.10%, a Li content of 4.04%, a Ni content of 26.80%, a Co content of 3.39%, a Mn content of 2.56%, a Cu content of 0.11%, an Al content of 0.10%, and a Fe content of 0.10%.
[0167] S2: calcining the battery black powder in an oxygen-free environment.
[0168] The oxygen-free environment was provided by nitrogen, the calcination temperature was 550°C, and the calcination time was 180 min.
[0169] S3: The calcined material is placed in a container for water immersion process. The water immersion conditions are: solid-liquid ratio of 1:5, water temperature of 80°C, stirring speed of 1500 rpm, water immersion time of 60 minutes, and water immersion times of 2 times.
[0170] S4 Lithium Evaporation: The water solution is evaporated in a water bath to concentrate the lithium carbonate, and the water bath is heated until the water is completely evaporated.
[0171] S5: Ultrasonic dispersion: Filter the material obtained in S4, put the filtered water-soaked residue into a container, add pure water to a liquid-solid ratio of 1:10, stir at 500 rpm, and ultrasonically disperse for 10 min.
[0172] S6: Flotation operation: The ultrasonically dispersed material is added to the flotation machine, and the flotation adopts a "one coarse, four fine, and two sweep" closed-circuit process.
[0173] The roughing foam material obtained by the roughing is subjected to the first cleaning to obtain the first cleaning foam material and the first cleaning middlings (recorded as middlings 3). The middlings 3 are returned to the roughing process as the raw material to be selected.
[0174] The first cleaned foam material is subjected to the second cleaned process to obtain the second cleaned foam material and the second cleaned middlings (recorded as middlings 4). The middlings 4 are returned to the first cleaned process as the raw material to be cleaned.
[0175] The second round of concentrated foam material was subjected to the third round of concentration to obtain the third round of concentrated foam material and the third round of concentrated middlings (recorded as middlings 5). Middlings 5 were returned to the second round of concentration as the raw material to be selected and ground and scrubbed in the vertical mill for 5 minutes with the new round of first round of concentrated foam material.
[0176] The foamed material from the third cleaning process is subjected to the fourth cleaning process to obtain concentrate and the fourth cleaning middlings (recorded as middlings 6). The middlings 6 are returned to the third cleaning process as the raw material to be cleaned.
[0177] The roughing liquid obtained from the roughing is subjected to the first scavenging to obtain the first scavenging foam middlings (referred to as middlings 2) and the first scavenging residual slurry. The middlings 2 are returned to the roughing process as the raw material to be selected.
[0178] The remaining slurry from the first scavenging process is subjected to the second scavenging process to obtain tailings and the second scavenging foam middlings (recorded as middlings 1). The middlings 1 are returned to the first scavenging process as the raw material to be selected.
[0179] The flotation agents used in the roughing process include a pH regulator (calcium oxide, 2000 g / t), a stabilizer (aluminum sulfate, 1000 g / t), a flocculant (corn starch, 1500 g / t), a graphite collector (kerosene, 212 g / t), and a frother (MIBC, 174 g / t).
[0180] The concentrators used in each concentrating process include a graphite collector (kerosene) and an optional frother (MIBC). The first concentrating process uses 53g / t kerosene and 58g / t MIBC; the second concentrating process uses 53g / t kerosene and 58g / t MIBC; the third concentrating process uses 53g / t kerosene and 29g / t MIBC; and the fourth concentrating process uses 26.5g / t kerosene and 0g / t MIBC.
[0181] The scavenging agents used in each scavenging process included a graphite collector (kerosene) and a foaming agent (MIBC). The first scavenging process used 106g / t of kerosene and 58g / t of MIBC, while the second scavenging process used 53g / t of kerosene and 58g / t of MIBC.
[0182] S7: The tailings are acid-leached together with a reducing agent to remove impurities and extract nickel, cobalt, manganese and the remaining lithium to obtain qualified nickel, cobalt, manganese and lithium products.
[0183] Example 2
[0184] The difference between this embodiment and embodiment 1 is that in S2, the calcination temperature is 450°C.
[0185] Example 3
[0186] The difference between this embodiment and embodiment 1 is that in S3, the water immersion temperature is 25°C.
[0187] Example 4
[0188] The difference between this embodiment and embodiment 1 is that in S3, the stirring speed of the water immersion is 500 rpm.
[0189] Example 5
[0190] The difference between this embodiment and embodiment 1 is that in S6, no stabilizer (aluminum sulfate) is added during the roughing.
[0191] Example 6
[0192] The difference between this embodiment and embodiment 1 is that in S6, the amount of kerosene and MIBC used in the roughing is reduced. Specifically, the amount of kerosene used is 106 g / t, and the amount of MIBC used is 116 g / t.
[0193] Example 7
[0194] The difference between this embodiment and embodiment 1 is that in S6, no pH regulator (calcium oxide) is added during the roughing.
[0195] Example 8
[0196] The difference between this embodiment and embodiment 1 is that step S5 is not performed, that is, ultrasonic dispersion is not performed before flotation, and the water-soaked residue is directly subjected to flotation.
[0197] Example 9
[0198] The difference between this embodiment and embodiment 1 is that in S6, no stabilizer (aluminum sulfate) and pH regulator (calcium oxide) are added during the roughing.
[0199] Example 10
[0200] The difference between this embodiment and embodiment 1 is that in S6, the flotation agent used in the roughing process includes a pH regulator (calcium carbonate and calcium hydroxide, the mass ratio of the two is 1:1, 200 g / t), a stabilizer (ferric chloride, 200 g / t), a flocculant (sodium carboxymethyl cellulose, 500 g / t), a graphite collector (diesel, 50 g / t), and a foaming agent (pine oil, 50 g / t).
[0201] The amount of diesel used in each selection was 10 g / t, and the amount of pine oil used in each selection was 10 g / t.
[0202] The amount of diesel used in each sweep is 10 g / t, and the amount of pine oil used in each sweep is 10 g / t.
[0203] Example 11
[0204] The difference between this embodiment and embodiment 1 is that in S6, the flotation agent used in the roughing process includes a pH regulator (sodium carbonate and sodium hydroxide, the mass ratio of the two is 1:1, 4000 g / t), a stabilizer (magnesium nitrate, 2000 g / t), a flocculant (dextrin, 2000 g / t), a graphite collector (kerosene, 500 g / t), and a foaming agent (octanol, 400 g / t).
[0205] The amount of kerosene used in each selection is 150g / t, and the amount of octanol used in each selection is 150g / t.
[0206] The amount of kerosene used in each sweep was 150 g / t, and the amount of octanol used in each sweep was 150 g / t.
[0207] Example 12
[0208] The difference between this embodiment and embodiment 1 is that in S6, the number of selections is 2.
[0209] Example 13
[0210] The difference between this embodiment and embodiment 1 is that in S6, the number of selections is 3.
[0211] Example 14
[0212] The difference between this embodiment and embodiment 1 is that in S6, the number of scans is 1.
[0213] Example 15
[0214] The difference between this embodiment and embodiment 1 is that in S2, the calcination temperature is 800°C.
[0215] Comparative Example 1
[0216] The difference between this comparative example and Example 1 is that in S6, no flocculant (starch) is added during the roughing.
[0217] Comparative Example 2
[0218] The difference between this comparative example and Example 1 is that in S6, no flocculant (starch) and pH regulator (calcium oxide) were added during the roughing.
[0219] Comparative Example 3
[0220] The difference between this comparative example and Example 1 is that in S6, no flocculant (starch) and stabilizer (aluminum sulfate) were added during the roughing.
[0221] Comparative Example 4
[0222] The difference between this comparative example and Example 1 is that the amount of kerosene used in the roughing process is 100 g / t.
[0223] Comparative Example 5
[0224] The difference between this comparative example and Example 1 is that the amount of kerosene used in the roughing process is 600 g / t.
[0225] Comparative Example 6
[0226] The difference between this comparative example and Example 1 is that in the roughing process, the amount of MIBC used is 20 g / t.
[0227] Comparative Example 7
[0228] The difference between this comparative example and Example 1 is that in the roughing process, the amount of MIBC used is 450 g / t.
[0229] Comparative Example 8
[0230] The difference between this comparative example and Example 1 is that the amount of corn starch used in the roughing process is 400 g / t.
[0231] Comparative Example 9
[0232] The difference between this comparative example and Example 1 is that the amount of corn starch used in the roughing process is 2400 g / t.
[0233] Comparative Example 10
[0234] The difference between this comparative example and Example 1 is that in the roughing process, the amount of calcium oxide used is 150 g / t.
[0235] Comparative Example 11
[0236] The difference between this comparative example and Example 1 is that in the roughing process, the amount of calcium oxide used is 4200 g / t.
[0237] Comparative Example 12
[0238] The difference between this comparative example and Example 1 is that in the roughing process, the amount of aluminum sulfate used is 2400 g / t.
[0239] Comparative Example 13
[0240] The difference between this comparative example and Example 1 is that the amount of kerosene used in each cleaning is 0 g / t.
[0241] Comparative Example 14
[0242] The difference between this comparative example and Example 1 is that the amount of kerosene used in each cleaning is 200 g / t.
[0243] Comparative Example 15
[0244] The difference between this comparative example and Example 1 is that the amount of MIBC used in each concentration is 0 g / t.
[0245] Comparative Example 16
[0246] The difference between this comparative example and Example 1 is that the amount of MIBC used in each concentration is 200 g / t.
[0247] Comparative Example 17
[0248] The difference between this comparative example and Example 1 is that the amount of kerosene used in each sweep is 0 g / t.
[0249] Comparative Example 18
[0250] The difference between this comparative example and Example 1 is that the amount of kerosene used in each sweep is 200 g / t.
[0251] Comparative Example 19
[0252] The difference between this comparative example and Example 1 is that the amount of MIBC used in each sweep is 0 g / t.
[0253] Comparative Example 20
[0254] The difference between this comparative example and Example 1 is that the amount of MIBC used in each sweep is 200 g / t.
[0255] Comparative Example 21
[0256] The difference between this comparative example and Example 1 is that in S2, the calcination temperature is 300°C.
[0257] Comparative Example 22
[0258] The difference between this comparative example and Example 1 is that in S2, the calcination temperature is 1000°C.
[0259] Test example
[0260] The above examples and comparative examples were subjected to the following tests:
[0261] ①. The Li content in the raw material (battery black powder) and the leachate and leaching residue obtained in each leaching process was tested to obtain the corresponding leaching rate. The results are shown in Table 1.
[0262] ②. The fixed carbon content in the feed ore (battery black powder) and the tailings and concentrate obtained during the flotation process was tested to obtain the corresponding recovery rates. The results are shown in Table 2.
[0263] Table 1 Water immersion test results
[0264] Table 2 Flotation test results
[0265] As can be seen from Table 1, the method provided by the present disclosure can effectively extract Li, and the Li leaching rate is high. As can be seen from Table 2, the method provided by the present disclosure can effectively recover graphite, with a high graphite recovery rate, and the recovered graphite product has a high fixed carbon content.
[0266] In summary, the full-chain integrated method for recycling lithium and graphite from waste batteries provided by the present invention is simple and easy to implement, and can effectively recycle lithium and graphite from waste batteries. The recovery rates of lithium and graphite are both high, thus avoiding waste of resources.
[0267] The above are merely preferred embodiments of the present disclosure and are not intended to limit the present disclosure. Those skilled in the art will readily appreciate that various modifications and variations of the present disclosure are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present disclosure shall be included within the scope of protection of the present disclosure. Industrial Applicability
[0268] The method for recycling lithium and graphite from waste batteries provided by the present invention is simple and easy to implement, and can effectively recycle lithium and graphite from waste batteries. The recovery rates of lithium and graphite are both high, and the recovered graphite has a high fixed carbon content, thus avoiding waste of resources.
Claims
1. A full-chain integrated method for recycling lithium and graphite from waste batteries. It is characterized in that The following steps are involved: The battery black powder obtained from the waste battery is roasted and water-leached to extract lithium, and the water-leached residue is floated; The flotation comprises: using a flotation agent to perform a roughing on the water-leached residue to obtain a roughing foam material and a roughing slurry; performing at least one fine separation on the roughing foam material to finally obtain a carbonaceous concentrate; The flotation agent includes a graphite collector, an adjusting agent and a frother; and the adjusting agent includes a flocculant.
2. The method according to claim 1, It is characterized in that The graphite collector comprises at least one of kerosene and diesel; And / or, the flocculant includes at least one of starch, sodium carboxymethyl cellulose and dextrin; And / or, the foaming agent includes at least one of methyl isobutyl carbinol, pine oil and octanol.
3. The method according to claim 1 or 2, It is characterized in that The amount of the graphite collector is 50g / t-500g / t; and / or the amount of the flocculant is 500g / t-2000g / t; and / or the amount of the foaming agent is 50g / t-400g / t.
4. The method according to any one of claims 1 to 3, It is characterized in that The regulator also includes at least one of a pH adjuster and a stabilizer.
5. The method according to claim 4, It is characterized in that The pH regulator includes at least one of calcium oxide, calcium carbonate, calcium hydroxide, sodium carbonate and sodium hydroxide; And / or, the stabilizer includes at least one of aluminum sulfate, aluminum nitrate, aluminum chloride, polyaluminum chloride, ferric sulfate, ferric nitrate, ferrous sulfate, ferric chloride, ferrous chloride, magnesium nitrate, magnesium chloride and magnesium sulfate.
6. The method according to claim 4 or 5, It is characterized in that The pH adjuster is used in an amount of 200 g / t-4000 g / t, and / or the stabilizer is used in an amount of 200 g / t-2000 g / t.
7. The method according to any one of claims 1 to 6, It is characterized in that The number of times of selection is n, where n≥2 and is an integer; in the first n-1 selection processes, the n-1th selected foam material and the n-1th selected middlings are obtained after each selection; the n-1th selected foam material is used as the raw material to be selected for the nth selection.
8. The method according to claim 7, It is characterized in that When n=2, the first concentrated middlings obtained in the first concentration are returned to the roughing process as the raw material to be selected.
9. The method according to claim 7 or 8, It is characterized in that When n=2, the second concentrated middlings obtained from the second concentration are returned to the first concentration process as raw materials to be selected.
10. The method according to claim 7, It is characterized in that When n≥3, the n-1th concentrated middlings obtained in the n-1th concentration are returned to the n-2th concentration process as raw materials to be selected.
11. The method according to claim 7 or 10, It is characterized in that The nth concentrated middlings obtained from the nth concentration are returned to the n-1th concentration process as raw materials to be selected.
12. The method according to claim 9 or 10, It is characterized in that When the selected middlings are returned to the second selection process as raw materials to be selected, the foam material from the first selection is combined with the middlings from the third selection for grinding and scrubbing before the second selection.
13. The method according to claim 12, It is characterized in that The scrubbing time is 2min-15min.
14. The method according to any one of claims 1 to 13, It is characterized in that The concentrator used in each concentrating step independently includes a graphite collector and a frother.
15. The method according to claim 14, It is characterized in that The graphite collector used in each beneficiation process includes at least one of kerosene and diesel; And / or, the foaming agent used in each beneficiation process includes at least one of methyl isobutyl carbinol, pine oil and secondary octanol.
16. The method according to claim 14 or 15, It is characterized in that The amount of graphite collector used in each concentration process is 0-150 g / t; and / or the amount of foaming agent used in each concentration process is 0-150 g / t.
17. The method according to any one of claims 1 to 16, It is characterized in that The flotation further comprises: subjecting the roughing slurry to at least one scavenging process to finally obtain carbon-containing tailings.
18. The method according to claim 17, It is characterized in that The number of sweeping is m times, m≥2 and is an integer; in the first m-1 sweeping processes, after each sweeping, the m-1th sweeping residual slurry and the m-1th sweeping foam middlings are obtained respectively; the m-1th sweeping residual slurry is used as the raw material to be selected for the mth sweeping.
19. The method according to claim 18, It is characterized in that When m=2, the first scavenging foam middlings obtained in the first scavenging are returned to the roughing process as the raw material to be selected.
20. The method according to claim 18 or 19, It is characterized in that When m=2, the second scavenging foam middlings obtained in the second scavenging are returned to the first scavenging process as the raw material to be selected.
21. The method according to claim 18, It is characterized in that When m≥3, the m-1th scavenging foam middlings obtained in the m-1th scavenging are returned to the m-2th scavenging process as the raw material to be selected.
22. The method according to claim 18 or 21, It is characterized in that The m-th scavenging foam middlings obtained in the m-th scavenging are returned to the m-1-th scavenging process as raw materials to be selected.
23. The method according to any one of claims 17 to 22, It is characterized in that The scavenging agent used in each scavenging process independently includes a graphite collector and a foaming agent.
24. The method according to claim 23, It is characterized in that The graphite collector used in each sweeping process includes at least one of kerosene and diesel; And / or, the foaming agent used in each scanning process includes at least one of methyl isobutyl carbinol, pine oil and secondary octanol.
25. The method according to claim 23 or 24, It is characterized in that The amount of graphite collector used in each scavenging process is 0-150 g / t; and / or the amount of foaming agent used in each scavenging process is 0-150 g / t.
26. The method according to any one of claims 17 to 25, It is characterized in that The number of rough selection is 1 time, the number of fine selection is 4 times, and the number of sweep selection is 2 times.
27. The method according to any one of claims 1 to 26, It is characterized in that The main sources of the battery black powder include positive electrode materials containing lithium and negative electrode materials containing graphite.
28. The method according to claim 27, It is characterized in that The source of the battery black powder also includes at least one of a current collector and battery impurities.
29. The method according to claim 28, It is characterized in that The current collector includes copper foil or aluminum foil.
30. The method according to any one of claims 1 to 29, It is characterized in that In terms of mass percentage, the battery black powder has a fixed carbon content of 30%-55%, a Li content of 3%-7%, a Ni content of 10%-35%, a Co content of 2%-5%, a Mn content of 2%-5%, a Cu content of 0.055-1%, an Al content of 0.05%-1% and a Fe content of 0.05%-1%.
31. The method according to any one of claims 1 to 30, It is characterized in that The preparation of the battery black powder comprises: discharging, crushing, cracking and screening the waste batteries.
32. The method according to any one of claims 1 to 31, It is characterized in that Roasting includes at least one of the following features: Feature 1: Calcination temperature is 400℃-800℃; Feature 2: Calcination time is 30min-180min; Feature 3: Calcination is carried out in an oxygen-free environment.
33. The method according to claim 32, It is characterized in that The oxygen-free environment is provided by nitrogen or inert gas.
34. The method according to any one of claims 1 to 33, It is characterized in that Lithium extraction by water leaching includes a water leaching process, and the water leaching includes at least one of the following characteristics: Feature 1: The solid-liquid ratio of water immersion is 1:3-1:10; Feature 2: The water immersion temperature is 25℃-90℃; Feature 3: The immersion time is 30min-120min; Feature 4: Water immersion is carried out under stirring conditions.
35. The method according to claim 34, It is characterized in that The stirring speed during the water immersion process is 500rpm-2000rpm.
36. The method according to claim 34 or 35, It is characterized in that Lithium extraction by water leaching also includes a lithium extraction process, and the lithium extraction method includes evaporating the leaching liquid obtained by the water leaching process.
37. The method according to claim 36, It is characterized in that The evaporation was carried out by water bath evaporation.
38. The method according to claim 37, It is characterized in that The temperature of water bath evaporation is 80℃-100℃.
39. The method according to any one of claims 1 to 38, It is characterized in that Before flotation, the water-soaked residue is dispersed.
40. The method according to claim 39, It is characterized in that The dispersion method is ultrasonic dispersion.
41. The method according to claim 40, It is characterized in that Ultrasonic dispersion includes at least one of the following features: Feature 1: Ultrasonic dispersion is carried out by mixing the water-leached residue with water at a liquid-to-solid ratio of 1:3-1:10; Feature 2: Ultrasonic stirring intensity is 300rpm-1000rpm; Feature 3: Ultrasonic dispersion time is 5min-20min.
42. The method according to any one of claims 1 to 41, It is characterized in that After flotation, it also includes post-processing of the flotation tailings products; Post-treatment includes acid leaching, impurity removal and extraction.
Citation Information
Patent Citations
Recovery method of waste lithium ion battery negative electrode material
CN111430831A
Method for recovering copper, aluminum and graphite from waste ternary lithium ion battery
CN111468284A
Separation and smelting combined comprehensive recovery method and device for waste lithium ion batteries
CN111534697A
Method for recovering all components of waste lithium ion battery
CN112510281A
Cited By
Regeneration method of lithium ion battery negative electrode waste slurry
CN119029376A