Implantable material and synthesis method therefor and prosthetic heart valve

By grafting functional branches on the hard segments of the polyurethane material, the mechanical properties and biocompatibility of the polyurethane material are improved, and the problem of reduced mechanical properties after the introduction of polydimethylsiloxane groups is solved, achieving better results. The stress conduction and tensile strength are improved.

WO2024216794A1PCT designated stage expired Publication Date: 2024-10-24VENUS MEDTECH (HANGZHOU) INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/112846
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2023-08-14
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The introduction of polydimethylsiloxane (PDMS) into polyurethane materials leads to a decrease in mechanical properties. This is mainly due to the large difference in solubility parameters between soft segments and hard segments, which results in the inability to conduct stress smoothly and affects the tensile strength of the material.

Method used

Using modified implantable materials, functional branches are grafted on the hard segments. The solubility parameters of the functional branches are 6 to 8, including dimethylsiloxane and polydimethylsiloxane. base, phosphocholine base, etc., to improve the compatibility and stress transmission of hard segments and soft segments.

Benefits of technology

It effectively improves the mechanical properties of polyurethane materials, avoids stress accumulation at the interface, and significantly improves tensile strength and biocompatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023112846_24102024_PF_FP_ABST
    Figure CN2023112846_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses an implantable material and a synthesis method therefor and a prosthetic heart valve. The implantable material uses polyurethane, the molecular chain structure of polyurethane comprises a soft segment and a hard segment, and a functional branched chain is grafted onto the hard segment; the solubility parameter of the functional branched chain is 6-8. According to the present application, by introducing the functional branched chain into the hard segment, the compatibility between the hard segment and the soft segment is improved and the stress transfer points between the hard segment and the soft segment are increased, so that the prepared implantable polymer material has excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Implantable material, synthesis method thereof, and artificial heart valve Technical Field

[0001] The present application relates to the technical field of artificial valves, and in particular to an implantable material and a synthesis method thereof, and an artificial heart valve. Background Art

[0002] Implantable polymer materials refer to polymer materials used to make artificial prostheses and that come into contact with the human physiological environment, such as polyurethane materials (PU). Technical issues

[0003] In order to improve the biocompatibility and biostability of polyurethane materials, polydimethylsiloxane diol is used as one of the soft segment raw materials. However, the introduction of polydimethylsiloxane (PDMS) will significantly reduce the mechanical properties of polyurethane materials. This is mainly due to the large difference in the solubility parameters of the soft segment (PDMS) and the hard segment (PU), which leads to the appearance of a clear interface between the two, hindering the conduction of stress from the soft segment to the hard segment. Stress accumulates at the interface, thereby affecting the mechanical properties of the PDMS-PU material, which is manifested as a significant decrease in tensile strength under the same elastic modulus. Technical Solutions

[0004] In view of the problems of the existing technology, the present application provides a modified implantable material that improves the mechanical properties of the material while ensuring biocompatibility and biostability.

[0005] The implantable material of the present application adopts polyurethane, the molecular chain structure of the polyurethane includes a soft segment and a hard segment, and the hard segment is grafted with a functional side chain; the solubility parameter of the functional side chain is 6-8.

[0006] Optionally, the functional side chain is at least one of a dimethylsiloxane group, a polydimethylsiloxane group (PDMS), a phosphorylcholine group, and a sulfonic acid group.

[0007] Optionally, the soft segment raw material is an oligomer diol. More preferably, the soft segment raw material is an oligomer diol, for example, at least one of polycarbonate diol, polyester diol, polyether diol, and polydimethylsiloxane diol.

[0008] Optionally, the polycarbonate diol is at least one of DURANOL T5651 and DURANOL T5652.

[0009] Optionally, the polyether glycol is at least one of polyethylene glycol (PHMO) and polytetramethylene glycol (PTMO).

[0010] Optionally, the polyester diol is at least one of adipic acid polyester diol and succinic acid polyester diol.

[0011] Optionally, the soft segment includes a first soft segment and a second soft segment.

[0012] Optionally, the molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7.

[0013] Optionally, the molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10, such as 8.5-9.5.

[0014] Optionally, the mass ratio of the first soft segment to the second soft segment in the polyurethane is 2.5 to 5:1.

[0015] Optionally, the hard segment includes:

[0016] A first backbone segment formed from isocyanate;

[0017] a second main chain segment formed by a chain extender;

[0018] The functional branch is grafted to at least one of the first main link and the second main link.

[0019] Optionally, the raw material of the first main chain segment is at least one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), terephthalate diisocyanate (PPDI), isophorone diisocyanate (IPDI), xylylene diisocyanate (XDI), and triphenylmethane triisocyanate.

[0020] Optionally, the raw material of the second main chain segment is selected from at least one of a small molecule diol and a small molecule diamine;

[0021] The small molecule diol is at least one of ethylene glycol, butanediol (BDO), hexanediol, and octanediol;

[0022] The small molecule diamine is at least one of ethylenediamine, butanediamine, and hexamethylenediamine. Optionally, the molecular weight of the functional side chain is 100 to 2000.

[0023] Optionally, the grafting position of the functional side chain includes the following three methods:

[0024] Grafted only to the first main link;

[0025] Grafted only to the second main link;

[0026] Grafted onto the first main chain segment and the second main chain segment. Optionally, when grafted onto the first main chain segment only, the first main chain segment grafted with the functional branched chain accounts for 5-20% of the total molar amount of all first main chain segments.

[0027] Optionally, when only the second main chain segments are grafted, the second main chain segments grafted with functional branches account for 5 to 20% of the total molar amount of all second main chain segments.

[0028] Optionally, when grafted onto the first main chain segment and the second main chain segment, the first main chain segment and the second main chain segment grafted with functional branches account for 5 to 20% of the total molar amount of all first main chain segments and the second main chain segments.

[0029] Optionally, the hard segment (including functional side chains) accounts for 35 to 55% of the total mass of the polyurethane.

[0030] Optionally, the isocyanate index R value of the polyurethane is 1.0 to 1.1.

[0031] Optionally, the solubility parameter of the hard segment is 11-14.

[0032] The present application also provides a method for synthesizing an implantable material, comprising: providing a soft segment raw material and a hard segment raw material, and reacting the raw material to generate the implantable material;

[0033] The hard segment raw material comprises isocyanate and a chain extender, at least one of the isocyanate and the chain extender is grafted with a functional side chain; the solubility parameter of the functional side chain is 6-8.

[0034] Optionally, the functional side chain is at least one of a dimethylsiloxane group, a polydimethylsiloxane group (PDMS), a phosphorylcholine group, and a sulfonic acid group.

[0035] Optionally, the molecular weight of the functional side chain is 100-2000.

[0036] Optionally, the functional side chains are pre-grafted onto isocyanate and / or chain extender as hard segment raw materials.

[0037] Optionally, the functional side chains are grafted during the reaction process.

[0038] Optionally, the synthesis method includes: mixing all raw materials and reacting them to generate the implantable material.

[0039] Optionally, the reaction temperature is 60-80° C. and the reaction time is 2-6 hours.

[0040] Optionally, the synthesis method comprises:

[0041] S100, prepolymerizing and capping the soft segment raw material using isocyanate to obtain a prepolymer;

[0042] S200, the prepolymer reacts under the action of a chain extender to obtain the implantable material.

[0043] Optionally, the isocyanate in step S100 is a first isocyanate, and a second isocyanate is further added in step S200 , wherein the first isocyanate and the second isocyanate have the same or different structures.

[0044] Optionally, the first isocyanate and the second isocyanate are each a single isocyanate or a mixture of multiple isocyanates.

[0045] Optionally, the mixture of the multiple isocyanates is composed of one of the following:

[0046] a. All are isocyanates without the functional side chains grafted thereto;

[0047] b. isocyanates that are all grafted with the functional side chains;

[0048] c. One part is isocyanate grafted with the functional side chain, and the other part is isocyanate not grafted with the functional side chain.

[0049] Optionally, in the mixture of the multiple isocyanates, the molar ratio of the isocyanate not grafted with the functional side chain to the isocyanate grafted with the functional side chain is 4 to 20:1.

[0050] Optionally, the isocyanate not grafted with the functional side chain is at least one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), terephthalate diisocyanate (PPDI), isophorone diisocyanate (IPDI), xylylene diisocyanate (XDI), and triphenylmethane triisocyanate.

[0051] Optionally, in step S100, the soft segment raw material includes a first soft segment raw material and a second soft segment raw material; the first soft segment raw material and the second soft segment raw material are both pre-polymerized and capped with isocyanate.

[0052] Optionally, the molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7.

[0053] Optionally, the molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10, such as 8.5-9.5.

[0054] Optionally, the first soft segment raw material is polydimethylsiloxane diol.

[0055] Optionally, the second soft segment raw material is at least one of polyether diol, polycarbonate diol, and polyester diol, for example, at least one of polyethylene glycol (PHMO), polytetramethylene glycol (PTMO), Duolane T5651, and Duolane T5652.

[0056] Optionally, the mass ratio of the first soft segment raw material to the second soft segment raw material is 2.5 to 5:1.

[0057] Optionally, in step S100, the first soft segment raw material and the second soft segment raw material are pre-mixed and then added.

[0058] Optionally, the chain extender includes a linear chain extender and a chain extender grafted with functional branches.

[0059] Optionally, the linear chain extender is at least one of a small molecule diol and a small molecule diamine, for example, at least one of ethylene glycol, propylene glycol, butanediol, hexanediol, octanediol, and ethylenediamine.

[0060] Optionally, the main chain of the chain extender grafted with functional branches is the same as that of the linear chain extender. The chain extender grafted with functional branches is at least one of 1-palmitoylpropanediol-3-phosphocholine, 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine, and sphingosine phosphocholine.

[0061] Optionally, the molar ratio of the linear chain extender to the chain extender grafted with functional branches is 4 to 20:1.

[0062] Optionally, a mixture of a linear chain extender and a chain extender grafted with functional branches is added in step S200.

[0063] Optionally, step S200 includes:

[0064] The first reaction stage is a process of adding a chain extender grafted with functional branches to react with the prepolymer;

[0065] The second reaction stage is the process of adding a linear chain extender and continuing the reaction after the first reaction stage.

[0066] Optionally, the temperature of the first reaction stage is 60-80° C., and the time is 1-2 hours.

[0067] Optionally, the temperature of the second reaction stage is 60-80° C., and the time is 1-2 hours.

[0068] Optionally, the chain extension reaction system further includes a solvent; the solvent is at least one of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), and toluene; preferably methylacetamide (DMAc), dimethylformamide (DMF) or tetrahydrofuran (THF).

[0069] Optionally, the prepolymerization temperature in step S100 is 60-80° C. and the prepolymerization time is 2-4 hours.

[0070] Optionally, the temperature of the pre-sealing in step S100 is 60-80° C. and the time is 2-4 hours.

[0071] Optionally, the reaction temperature in step S200 is 60-80° C., and the reaction time is 2-6 hours.

[0072] The present application also provides an artificial heart valve, comprising a stent and leaflets connected to the stent, wherein the leaflets are made of the implantable material; the leaflets are multiple and cooperate with each other to control the opening and closing of the blood flow channel.

[0073] The implantable material can be prepared into leaflets using existing technology, and the leaflets can also be annealed. The annealing conditions are keeping the temperature at 60-150° C. for 2-60 hours.

[0074] Optionally, the artificial heart valve further includes a covering connected to the inner side and / or outer side of the stent, and the covering is made of the implantable material. Beneficial effects

[0075] Compared with the prior art, the present application introduces functional branches into the hard segment. Due to the large steric hindrance of the functional branches, the branches will be preferentially arranged in the outer layer of the hard segment while ensuring sufficient chain movement, and will not affect the interaction between the hard segments. At the same time, compared with the hard segment, the branches have better compatibility with the soft segment. One end of the branches forms a chemical bond with the hard segment, and the other end is similarly compatible with the soft segment, which well connects the hard segment and the soft segment, thereby improving the compatibility between the hard segment and the soft segment and increasing the stress transfer points between the two. The stress is well transmitted between the hard segment and the soft segment, avoiding the accumulation of stress at the interface, so that the prepared implantable polymer material has excellent mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] FIG1 is a schematic structural diagram of a polyurethane molecular chain in one embodiment;

[0077] FIG2 is a schematic diagram of a polyurethane system in one embodiment;

[0078] FIG3 is a flow chart of a method for synthesizing an implantable material according to an embodiment;

[0079] FIG4 is a schematic diagram showing the synthesis principle of an implantable material according to an embodiment;

[0080] FIG5 is a flow chart of a method for synthesizing an implantable material in another embodiment. Modes for Carrying Out the Invention

[0081] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0082] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0083] In the field of polymer material synthesis, such as polyurethane material synthesis, the hard segment and soft segment in the molecular structure are relative concepts. From the perspective of raw materials, the hard segment is a structural chain segment formed by low-molecular polyols / amines and isocyanates, and the soft segment is a structural chain segment formed by large-molecular polyols; from the perspective of chain length, the molecular chain of the hard segment is relatively short, the number of functional groups per unit chain length is high, and the intermolecular force is strong, which manifests as rigidity, while the molecular chain of the soft segment is long, the number of functional groups per unit chain length is low, and the intermolecular force is relatively weak, which manifests as flexibility.

[0084] In a polyurethane system, the soft segment typically forms the continuous phase, while the hard segment serves as the dispersed phase, dispersed within the soft segment. Conventional polyurethane materials include polyether polyurethane (PEU), polyester polyurethane, polycarbonate polyurethane (PCU), and polydimethylsiloxane polyurethane (PDMS-PU). The hard segment raw materials for these four types are isocyanate and chain extender, and their nomenclature is primarily determined by the soft segment raw materials. Because the hard segment has strong intermolecular forces, it forms an ordered, densely packed structure, making it relatively stable. The soft segment is the most susceptible to external influences. Among them, the soft segment raw material of PEU is polyether, which is easily oxidized itself, and the polyurethane involved in the synthesis also has the problem of easy oxidation; the soft segment of polyester polyurethane is polyester, which is easily hydrolyzed itself, and the polyurethane formed with it has the problem of easy hydrolysis; the soft segment raw material of PCU is polycarbonate, which is more stable than polyether polyester, but it is still easily hydrolyzed, and the polyurethane formed with it also has the problem of easy hydrolysis; the soft segment raw material of PDMS-PU is polydimethylsiloxane, which has excellent biostability and biocompatibility. As a leaflet material, it has excellent antioxidant and hydrolysis resistance. However, due to the large difference in the solubility parameters of polydimethylsiloxane and the hard segment, a clear interface is formed, and stress cannot be transmitted at the interface and forms accumulation. Therefore, the prepared polyurethane has poor mechanical properties.

[0085] The existing technology for improving the mechanical properties of PDMS-PU can be roughly divided into the following three types:

[0086] (1) A second soft segment, such as polyether, is introduced, and part of the hard segment forms an intermediate phase, connecting the soft segment and the hard segment to improve the compatibility between the two.

[0087] (2) Changing the groups at both ends of the soft segment, for example, by attaching carbon chains to both ends of PDMS. The resulting alkyl end groups and part of the hard segment form an intermediate phase, thereby improving the compatibility between PDMS and the hard segment.

[0088] (3) Using a linear siloxane chain extender, such as 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane (BHTD), to introduce a siloxane group into the main chain (linear) of the hard segment, on the one hand, reduces the polarity of the hard segment and improves the compatibility of the hard segment with PDMS. On the other hand, the addition of BHTD reduces the orderliness of the hard segment (steric hindrance and structural influence), which increases the entropy of the hard segment itself and reduces the phase separation with PDMS, thereby improving the compatibility between the hard segment and the soft segment.

[0089] Compared with the improvement schemes (1) and (2), the reason why the PDMS-PU of the improvement scheme (3) has good biostability is that there are no polyether, polyester, and polycarbonate functional groups inside the polysiloxane, so it is more stable. Introducing carbon chains or introducing a second soft segment at both ends of the polysiloxane is a compromise to the mechanical properties (a balance of performance trade-offs), or it increases the instability factor and still cannot meet the application requirements of artificial valves.

[0090] The inventors of this application discovered that one of the main factors affecting the mechanical properties of polyurethanes is the significant difference in the solubility parameters of the hard and soft segments, resulting in poor compatibility between the two. This makes it difficult for stress to be smoothly transmitted between the two segments, leading to stress concentration in either the soft or hard segments. This, in turn, affects the mechanical properties of the polyurethanes, causing them to break or crack easily during application. Therefore, this application addresses the issue of improving the compatibility of solubility parameters by employing appropriate functional side chains and incorporating them into the hard segments, resulting in a polyurethane that achieves both mechanical properties and biocompatibility.

[0091] One embodiment of the present application provides an implantable material using polyurethane. The polyurethane molecular chain structure includes a hard segment and a soft segment, wherein the hard segment is grafted with a functional side chain, and the solubility parameter of the functional side chain is 6 to 8. Specifically, the functional side chain can be at least one of a dimethylsiloxane group, a polydimethylsiloxane group, a phosphorylcholine group, and a sulfonic acid group, such as PDMS, or a phosphorylcholine group.

[0092] The molecular weight of the polyurethane in this application is not strictly limited and can generally be above 50,000, for example, 50,000 to 300,000. It can be adjusted according to its performance requirements and can also be determined in combination with the molecular weight ranges of the soft segment and hard segment described below.

[0093] The present embodiment introduces functional side chains into the structural chain of the hard segment. On the one hand, it does not affect the length of the hard segment main chain, and thus does not cause a decrease in the strength of the hard segment. On the other hand, under the guidance of the lowest energy arrangement, the hard segment tends to form an orderly arranged internal block, and the functional side chains tend to be located at the periphery of the block. Structurally, one end of the functional side chain is chemically bonded to the hard segment, and the other end is mutually soluble with the soft segment on the principle of similar dissolving in similarity. This can well serve the purpose of connecting the soft segment and the hard segment, and further eliminate the stress at the interface between the two. At the same time, the functional side chain has the characteristics of lower surface energy, tends to migrate to the polyurethane surface, can better protect the soft segment, and at the same time makes the polyurethane exhibit the characteristics of good hydrophobicity, biostability and biocompatibility possessed by the side chain, thereby improving the mechanical properties of the polyurethane material. The molecular structure of the polyurethane of the present embodiment is:

[0094] Where X is the soft segment, [YZ] n is a hard segment, n is 1-4;

[0095] Y is the first main chain segment, Z is the second main chain segment, R is a functional branch chain, and at least one of Y and Z is grafted with R;

[0096] In different [YZ], Y and Z may be the same or different.

[0097] The soft segment raw material can be a polymer polyol, for example, an oligomer polyol, such as an oligomer diol, which can be at least one of polycarbonate diol, polyester diol, polyether diol, and polydimethylsiloxane diol, for example, polydimethylsiloxane diol with a molecular weight of 500 to 2000. Among them, the polycarbonate diol is at least one of Duonaile T5651 and Duonaile T5652; the polyether diol is at least one of polyethylene glycol (PHMO) and polytetramethylene glycol (PTMO), for example, polyethylene glycol with a molecular weight of 500 to 2000; the polyester diol is at least one of adipic acid polyester diol and succinic acid polyester diol.

[0098] The first main chain segment in the hard segment is formed by an isocyanate, and the second main chain segment is formed by a chain extender. Specifically, the raw material involved in forming the first main chain segment can be selected from at least one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), terephthalate diisocyanate (PPDI), isophorone diisocyanate (IPDI), xylylene diisocyanate (XDI), and triphenylmethane triisocyanate, such as MDI or triphenylmethane triisocyanate. The raw material involved in forming the second main chain segment is a small molecule diol, such as at least one of ethylene glycol, butanediol, hexanediol, octanediol, and ethylenediamine, such as ethylene glycol or ethylenediamine.

[0099] The functional side chains can be grafted onto the first main chain segment only, the second main chain segment only, or both. Taking the structure shown in Figure 1 as an example, the polyurethane backbone is linear, and the functional side chains can be grafted onto position "1" or positions "2" and "3" on the hard segment. This is merely an example; all short-chain diols (small molecule diols) and isocyanates are also possible grafting locations.

[0100] The content of functional branches in the polyurethane molecular structure is one of the key parameters affecting the mechanical properties of implantable materials. An appropriate amount of functional branches can significantly improve the mechanical properties of implantable materials. When grafted only to the first main chain segment, the first main chain segment grafted with the functional branches accounts for 5-20% of the total molar weight of all first main chain segments, for example, 10-20%, or 12.66%. When grafted only to the second main chain segment, the second main chain segment grafted with the functional branches accounts for 5-20% of the total molar weight of all second main chain segments, for example, 10-20%, or 19.23%. When grafted to the first and second main chains, the molar weight of the first and second main chains grafted with the functional branches accounts for 5-20% of the total molar weight of all first and second main chains, for example, 10-15%, or 12.66%. An appropriate amount of functional side chains can increase the compatibility between the hard segment and the soft segment, thereby improving the mechanical properties. If the number of functional side chains is too large, the steric hindrance in the polyurethane molecular structure will increase significantly and affect the orderly arrangement of the hard segment, resulting in a decrease in the stability of the hard segment, and then causing a decrease in the overall mechanical properties of the polyurethane material.

[0101] The molecular weight of the functional side chains themselves is 100-2000, for example, 500-1000. If the molecular weight is too low, they will not be able to link the hard and soft segments. If the molecular weight is too high, the steric hindrance formed by the functional side chains will be too great, making it difficult for the hard segments to be connected to the polyurethane chain, and the order of the hard segments will be significantly disrupted.

[0102] As shown in Figure 2, in a polyurethane system, a transitional interface, or mesophase, exists between the dispersed and continuous phases, enabling stress transfer between the two phases. Structurally, the mesophase is primarily composed of a portion of the hard and soft segments' terminal alkyl groups, along with functional side chains. The functional side chains, miscible with the soft segments through the principle of like dissolves like, further facilitate stress transfer between the dispersed and continuous phases, thereby enhancing the mechanical properties of the polyurethane material.

[0103] From the perspective of heat flow, the Tg of the intermediate phase is the Tg of the soft segment ~ Tg + 20 ° C. Generally, differential scanning calorimetry (DSC) will show three Tg curve results, namely the dispersed phase, the intermediate phase and the continuous phase, and the Tg curve of the intermediate phase will produce a certain deviation towards the Tg curve of the continuous phase, indicating that some hard segments participate in the formation of the intermediate phase.

[0104] In another embodiment, the molecular structure of polyurethane is:

[0105] Among them, [X1-X2] is the soft segment; [YZ] n is a hard segment, n is 1-4;

[0106] Y is the first main chain segment, Z is the second main chain segment, R is a functional branch chain, and at least one of Y and Z is grafted with R;

[0107] In different [YZ], Y and Z may be the same or different.

[0108] In this embodiment, the soft segment includes a first soft segment X1 and a second soft segment X2. The raw material for the first soft segment has a molecular weight of 500-2000 and a solubility parameter of 6-7. The raw material for the second soft segment has a molecular weight of 500-2000 and a solubility parameter of 8-10, for example, 8.5-9.5. The chemical properties (solubility parameter) of the second soft segment are intermediate between those of the soft segment and the hard segment, which can mitigate adverse effects between the soft and hard segments, such as poor compatibility and poor stress conduction.

[0109] In one embodiment, the mass ratio of the first soft segment to the second soft segment in the polyurethane is 2.5 to 5:1, for example, 2.5 to 4:1, and for example, 4:1. This can effectively adjust the solubility parameter of the soft segment, thereby improving the compatibility between the soft segment and the hard segment, thereby enhancing the mechanical properties of the polyurethane.

[0110] Considering the overall performance of the implantable material, the hard segment (including functional branches) in the molecular chain structure accounts for 35-55% of the total molecular weight of the polyurethane, such as 40-45%, and for example 45%, so that the implantable material has good mechanical strength and elasticity.

[0111] The R value of polyurethane, also known as the isocyanate index, refers to the molar ratio of isocyanate groups (-NCO) to hydroxyl groups (-OH). The R value significantly affects the performance of polyurethane, primarily influencing the material's glass transition temperature, degree of swelling, and tensile strength. In this application, the R value of the polyurethane is between 1.0 and 1.1, for example, 1.0 and 1.05, to achieve the desired performance. Combined with the improvements in the molecular structure of this application, it is particularly suitable for implantable devices and fatigue resistance requirements for long-term dynamic deformation, achieving fatigue resistance of 200 million cycles.

[0112] In terms of the dispersion uniformity of the polyurethane system, the solubility index difference between the soft segment and the hard segment should be controlled within a certain range. For example, the difference between the hard segment and the soft segment does not exceed 8. More preferably, the difference between the hard segment and the soft segment does not exceed 6, and the solubility parameter of the hard segment can be 11 to 14.

[0113] One embodiment of the present application provides a method for synthesizing an implantable material, comprising providing a soft segment raw material and a hard segment raw material, and reacting the raw material to form the implantable material. The hard segment raw material comprises an isocyanate and a chain extender, at least one of which is grafted with a functional side chain, wherein the solubility parameter of the functional side chain is between 6 and 8.

[0114] Specifically, the functional side chains can be at least one of dimethylsiloxane, polydimethylsiloxane (PDMS), phosphorylcholine, and sulfonic acid groups, such as PDMS and phosphorylcholine. Various grafting combinations of these functional side chains and the two hard segment materials can be employed, such as grafting dimethylsiloxane and / or polydimethylsiloxane groups onto isocyanate, and phosphorylcholine and / or sulfonic acid groups onto chain extenders; or grafting dimethylsiloxane and / or polydimethylsiloxane groups onto chain extenders, and phosphorylcholine and / or sulfonic acid groups onto isocyanate.

[0115] Functional branches can be introduced into the hard segment by providing a hard segment raw material grafted with functional branches. For example, the functional branches can be pre-grafted onto at least one of the isocyanate and chain extender used as the hard segment raw material. Alternatively, the functional branches can be grafted onto the segments formed by the hard segment raw material during the reaction.

[0116] For example, in one embodiment, isocyanate grafted with polydimethylsiloxane side chains is prepared by reacting polysiloxane monool / amine with isocyanate, such as reacting 3-((tert-butyldimethylsilyl)oxy)-propanol with triphenylmethane triisocyanate.

[0117] For example, in one embodiment, a chain extender grafted with functional branches can be prepared by oxidizing a double-bond raw material grafted with the corresponding functional groups to form an epoxy, followed by ring opening to form a diol. The double-bond raw material grafted with the corresponding functional groups can be at least one of 1,3-divinyl-1,3-dimethyl-1,3-diphenyldisiloxane (CAS: 2627-97-6), vinylpentamethyldisiloxane (CAS: 1438-79-5), and 1-vinyl-1,1,3,3-tetramethyldisiloxane (CAS: 55967-52-7). The double-bond raw material grafted with the corresponding functional groups can also be produced by an alcohol / halogenated hydrocarbon elimination reaction.

[0118] The chain extender grafted with functional branches can also be prepared by hydrolyzing a double bond raw material grafted with corresponding functional groups. The double bond raw material grafted with corresponding functional groups can be a diester raw material, for example, 1,2-dilauroyl-SN-glycero-3-phosphocholine (CAS: 18194-25-7) and / or 1,2-diacetyl-SN-glycero-3-phosphocholine (CAS: 56782-46-8).

[0119] Polyurethane synthesis methods mainly include one-step and two-step methods. The one-step method involves mixing all raw materials or completing the chemical reaction process continuously to produce polyurethane, which can be used as an implantable material. The reaction temperature is 60-80°C and the reaction time is 2-6 hours.

[0120] The two-step method is also known as the prepolymerization method. Usually, oligomer polyols and isocyanates are reacted first to form a low molecular weight prepolymer, and then a chain extender is added to react with the prepolymer to form polyurethane.

[0121] Referring to FIG3 , the present application provides a specific synthesis method of an implantable material based on the prepolymerization method, comprising the following steps:

[0122] Step S100, prepolymerizing and capping the soft segment raw material using isocyanate to obtain a prepolymer;

[0123] Step S200: The prepolymer reacts under the action of a chain extender.

[0124] In specific operations, the isocyanate in step S100 can be a first isocyanate, and a second isocyanate can be added in step S200. The specific reaction principle is shown in Figure 4. The first and second isocyanates are collectively referred to as the isocyanates in the hard segment raw materials described above. This description is merely to distinguish between different reaction stages during the synthesis process. Specifically, the first and second isocyanates can be the same or different.

[0125] Furthermore, the first isocyanate and the second isocyanate may each be a single isocyanate or a mixture of multiple isocyanates. The mixture of multiple isocyanates may be composed of one of the following: a) all isocyanates without grafted functional branches; b) all isocyanates with grafted functional branches; c) a portion of isocyanates with grafted functional branches and a portion of isocyanates without grafted functional branches.

[0126] In a specific embodiment, in the mixture of multiple isocyanates, the molar ratio of the isocyanate without grafted functional side chains to the isocyanate with grafted functional side chains is 4 to 20:1, for example 8 to 20:1, or even 10:1.

[0127] In one embodiment, the soft segment raw materials in step S100 include a first soft segment raw material and a second soft segment raw material, both of which are pre-polymerized and end-capped with isocyanate. The first soft segment raw material has a molecular weight of 500-2000 and a solubility parameter of 6-7. The first soft segment raw material can be polydimethylsiloxane diol, such as polydimethylsiloxane diol with a molecular weight of 500-2000. The second soft segment raw material has a molecular weight of 500-2000 and a solubility parameter of 8-10, such as 8.5-9.5. The second soft segment raw material can be selected from at least one of polyether diol, polycarbonate diol, and polyester diol, such as at least one of polyethylene glycol (PHMO), polytetramethylene glycol (PTMO), DONALO T5651, and DONALO T5652, or polyethylene glycol with a molecular weight of 700.

[0128] In one embodiment, the mass ratio of the first soft segment raw material to the second soft segment raw material is 2.5 to 5: 1, for example 2.5 to 4: 1, and for example 4: 1. The first soft segment raw material and the second soft segment raw material can be pre-mixed and then added.

[0129] In step S200, the chain extender includes a linear chain extender and a chain extender grafted with functional branches. The linear chain extender is at least one of a small molecule diol and a small molecule diamine, for example, at least one of ethylene glycol, butanediol, hexanediol, octanediol, and ethylenediamine. The main chain of the chain extender grafted with functional branches can be consistent with that of the linear chain extender. Specifically, the chain extender grafted with functional branches can be at least one of 1-palmitoylpropanediol-3-phosphocholine (CAS: 68124-68-5), 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine, and sphingosine phosphocholine (CAS: 1670-26-4), for example, 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine. In one embodiment, the molar ratio of the linear chain extender to the chain extender grafted with functional branches is 4 to 20:1, such as 8 to 20:1, and another example is 10:1.

[0130] In step S200, the chain extender can be added by adding a mixture of a linear chain extender and a chain extender grafted with functional branches, or by adding the chain extender grafted with functional branches and the linear chain extender sequentially in stages. For example, in one embodiment, step S200 includes a first reaction stage and a second reaction stage. The first reaction stage is the process of adding the chain extender grafted with functional branches to react with the prepolymer, and the second reaction stage is the process of adding the linear chain extender after the first reaction stage. More specifically, the temperature in the first reaction stage is 60-80°C for 1-2 hours. The temperature in the second reaction stage is 60-80°C for 1-2 hours. This sequential, staged addition method facilitates the incorporation of the chain extender grafted with functional branches into the polyurethane synthesis.

[0131] The chain extension reaction system also includes a solvent, which can be selected from at least one of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), and toluene, such as N,N-dimethylacetamide (DMAc). In step S200, the solvent can be pre-dissolved in the prepolymer and the second isocyanate, or added as needed to achieve a final solution of 10-30 (w / v)%, for example, 20 (w / v), before the chain extender is added.

[0132] In the synthesis method, the prepolymerization temperature is 60-80°C, for example, 80°C, and the time is 2-4 hours. The chain extension reaction temperature is 60-80°C, for example, 80°C, and the time is 2-6 hours. During the above synthesis process, an inert gas such as nitrogen is used for both the prepolymerization end-capping and the chain extension reaction.

[0133] Referring to FIG5 , in one embodiment, the synthesis method further comprises:

[0134] Step S300: drying the system after the chain extension reaction to obtain an implantable material.

[0135] Drying is performed to volatilize the solvent in the system, yielding an implantable material, such as a polyurethane film. The drying temperature can be 40°C to 80°C, for example, 60°C, and the drying time can be 6 to 24 hours, for example, 8 hours. An inert gas, such as nitrogen, can also be used during the drying process.

[0136] The polyurethane material synthesized based on the prepolymerization method has a molecular chain comprising the structure shown in the general formula III: -[L2-A-L2-B] n -;

[0137] Wherein, L2 is the first main chain segment (the characteristics of the raw materials or chain segments can be found above, and combined with the above, it is the first isocyanate), A is the soft segment; at least one of L2 and B is grafted with a functional side chain;

[0138] A is independently selected from at least one of polyether diol, polycarbonate diol, polyester diol, and polydimethylsiloxane diol;

[0139] The structural formula of the above B is: -[W1-L1] n1 W1-;

[0140] Wherein, n1 is a natural number from 0 to 5;

[0141] L1 is an isocyanate (combined with the above, the second isocyanate), for example, at least one of TDI, HDI, MDI, NDI, PPDI, IPDI, and XDI, wherein the hydrogen element position on each hydrocarbon group in the isocyanate may be replaced by a functional branched chain;

[0142] W1 is a chain extender (combined with the above, it is the second main chain segment), which can be independently selected from at least one of ethylene glycol, butanediol, hexanediol, octanediol, and ethylenediamine, and the position of the hydrogen element on each hydrocarbon group in X1 can be replaced by a functional branched chain;

[0143] At least one of L1 and W1 is partially grafted with a functional branched chain.

[0144] The present application provides several applications of implantable materials in the field of artificial heart valve materials.

[0145] The implantable material is applied to an artificial heart valve through processing. For example, the artificial heart valve provided in Example 1 includes a stent and leaflets connected to the stent. The leaflets are multiple and cooperate with each other to control the opening and closing of the blood flow channel. The leaflets are made of implantable materials.

[0146] In artificial heart valves, especially aortic valves, extremely high requirements are placed on the mechanical properties of the leaflets, such as tensile strength, elongation, elastic modulus, surface silicon content, surface phosphorylcholine groups, and surface sulfonic acid groups. Among them, higher silicon content, surface phosphorylcholine groups, and surface sulfonic acid groups generally represent better biocompatibility. At the same time, they have a certain protective effect on the inside of the leaflets, so their biological stability is relatively better. The leaflets prepared with the implantable material of the present application are particularly suitable for aortic valves. During the preparation process, annealing treatment can also be performed, wherein the annealing treatment conditions are 60-150°C for 2-60 hours, which can fully rearrange the internal molecular chains of the polyurethane so that the hard segments are arranged in a manner of minimum energy or close to minimum energy.

[0147] The above-mentioned implantable materials can also be used to process a coating, which is connected to the inner and / or outer sides of the stent to maintain sealing, prevent leakage and provide safety protection. The coating on the inner side of the stent is connected to the leaflets separately or as an integrated structure, and the coating on the outer side of the stent can also be formed by rolling up the inner coating as a whole.

[0148] The following provides a number of specific examples in combination with specific parameters. The raw materials used in each preparation example and embodiment can be dried according to the moisture or impurity requirements before use, for example, vacuum drying at 80° C. for 10 hours.

[0149] Preparation Example 1

[0150] Triphenylmethane triisocyanate (CAS: 2422-91-5) was placed in a three-necked flask. Under a nitrogen atmosphere and at 60°C, an equimolar amount of 3-((tert-butyldimethylsilyl)oxy)-propanol (CAS: 73842-99-6) was added dropwise using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to obtain intermediate product 1, i.e., isocyanate grafted with polysiloxane side chains:

[0151] Preparation Example 2

[0152] Triphenylmethane triisocyanate was placed in a three-necked flask. Under nitrogen atmosphere and at 60°C, an equimolar amount of isethionic acid (CAS: 107-36-8) was added dropwise into the flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to obtain intermediate product 2, i.e., isocyanate grafted with sulfonic acid groups.

[0153] Preparation Example 3

[0154] 10.50 g of 2-amino-2-methyl-1,3-propanediol (AMPD, CAS 115-69-5) was dissolved in a mixture of 50 mL of 1,4-dioxane and 50 mL of water with stirring in an ice-water bath. 25.92 g of di-tert-butyl dicarbonate ((Boc)2O, CAS 24424-99-5) was added and stirred at room temperature for 24 hours. After stirring, the solution was concentrated in vacuo to an oily residue, which was then recrystallized to obtain the product, BocAMP. 18.8 g of BocAMP and 25.4 mL of triethylamine were dissolved in 200 mL of anhydrous THF and cooled to 0°C. Under a nitrogen atmosphere, 14.5 mL of acetyl chloride was added dropwise to the mixture, which was heated to room temperature and stirred for 2 hours. After the reaction, the mixture was filtered and the THF was removed by rotary evaporation. The crude BDAPA was purified by silica gel column chromatography using ethyl acetate (EtOAc) / petroleum ether (1:3) to obtain the product, BDAPA.

[0155] 9.4 g of BDAPA was dissolved in 50 mL of ethyl acetate saturated with hydrogen chloride, allowed to stand at room temperature for 2 hours, and then concentrated under reduced pressure to obtain DAPA. DAPA, 4.6 mL of triethylamine, and 5.2 g of HDA were dissolved in a mixture of 50 mL of dimethylformamide and 200 mL of ethanol to obtain HDADEA.

[0156] 4.5 g of HDADEA and 1.73 mL of triethylamine were dissolved in a mixture of 100 mL of anhydrous ether and 30 mL of anhydrous acetonitrile. After cooling to 20°C, 1.78 g of 2-chloro-1,3,2-dioxaphosphole-2-oxide (COP, CAS 6609-64-9) dissolved in 10 mL of anhydrous ether was slowly added to the stirred solution over 20 minutes under a nitrogen atmosphere. The reaction system was kept at 20°C for 1 hour and then slowly warmed to room temperature. After the reaction, the triethylammonium chloride precipitate was filtered and washed with ether. The filtrate was evaporated in vacuo under a stream of nitrogen to yield a colorless oily residue. The residue was dissolved in 60 mL of anhydrous acetone nitrile and transferred to a 100 mL pressure bottle. After cooling the pressure bottle to 18°C, an excess of trimethylamine was quickly added to the solution. The pressure bottle was then closed and maintained at 55°C for 16 hours. The solution was then evaporated in vacuo to produce a viscous liquid. The viscous liquid was dissolved in methanol and an excess of ammonia was added. The mixture was stirred at room temperature for 24 hours and then concentrated under reduced pressure to obtain (9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine):

[0157] Example 1

[0158] The synthesis method of the implantable material specifically includes:

[0159] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol is used as the soft segment raw material, and the soft segment raw material is pre-polymerized and capped using the first isocyanate:

[0160] Calculated by mass percentage of the reaction system (excluding the solvent DMAc), 30 wt% MDI was placed in a three-necked flask. At 80°C, 55 wt% polydimethylsiloxane diol (molecular weight 1000) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to produce a prepolymer: MDI-PDMS-MDI.

[0161] (2) The intermediate product 1 of Preparation Example 1 was used as the second isocyanate, and the temperature was lowered to 50° C. 9 wt % of the second isocyanate was added to the system after the reaction in step (1), and the solution was pre-dissolved in DMAc to form a 20 (w / v) % solution, and stirred for 10 to 30 min.

[0162] (3) heating to 80° C., gradually adding 6 wt % of chain extender BDO to the solution of step (2), and carrying out the chain extension reaction for 2 h after the addition is complete;

[0163] (4) Drying at 60°C to obtain a polyurethane film. The synthesis process is carried out under a nitrogen atmosphere. Further, the polyurethane film can be used to prepare leaflets and annealed at 150°C for 2 hours.

[0164] Example 2

[0165] The synthesis method of the implantable material specifically includes:

[0166] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol and polyhexamethylene glycol (PHMO) are used as soft segment raw materials, and the first isocyanate is used to pre-polymerize and cap the soft segment raw materials:

[0167] Calculated by mass percentage of the reaction system (excluding the solvent DMAc), 30 wt% MDI was placed in a three-necked flask. At 80°C, a mixture of 44 wt% polydimethylsiloxane diol (molecular weight, 1000) and 11 wt% PHMO (molecular weight, 700) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to produce prepolymers 1: MDI-PDMS-MDI and MDI-PHMO-MDI.

[0168] (2) The intermediate product 1 of Preparation Example 1 was used as the second isocyanate, and the temperature was lowered to 50° C. 9 wt % of the second isocyanate was added to the system after the reaction in step (1), and pre-dissolved in DMAc to form a 20 (w / v) % solution, and stirred for 10 to 30 min.

[0169] (3) The temperature was raised to 80° C., and 6 wt % of the chain extender BDO was gradually added dropwise to the solution in step (2). After the addition was complete, the chain extension reaction was carried out for 2 h.

[0170] (4) Drying at 60°C to obtain a polyurethane film.

[0171] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0172] Example 3

[0173] The synthesis method of the implantable material specifically includes:

[0174] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol is used as the soft segment raw material, and the soft segment raw material is pre-polymerized and capped using the first isocyanate:

[0175] Calculated by mass percentage of the reaction system (excluding the solvent DMAc), 33.0 wt% MDI was placed in a three-necked flask. At 80°C, 54.0 wt% polydimethylsiloxane diol (molecular weight 1000) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to generate a prepolymer: MDI-PDMS-MDI.

[0176] (2) 7.0 wt% 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine was added dropwise to the system of step (1), and a chain extension reaction was carried out for 2 hours after the addition was completed.

[0177] (3) DMAc was added to form a 20 (w / v)% solution.

[0178] (4) At 80° C., 6.0 wt % of chain extender BDO was gradually added dropwise to the solution in step (3). After the addition was complete, the chain extension reaction was carried out for 2 h.

[0179] (5) After the chain extension reaction is completed, the polyurethane film is dried at 60°C to obtain a polyurethane film.

[0180] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0181] Example 4

[0182] The synthesis method of the implantable material specifically includes:

[0183] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol and polyhexamethylene glycol (PHMO) are used as soft segment raw materials, and the first isocyanate is used to pre-polymerize and cap the soft segment raw materials:

[0184] Calculated by mass percentage of the reaction system (excluding the solvent DMAc), 33 wt% MDI was placed in a three-necked flask. At 80°C, 43.2 wt% polydimethylsiloxane diol (molecular weight 1000) and 10.8 wt% PHMO (molecular weight 700) were added dropwise to the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to generate prepolymers: MDI-PDMS-MDI and MDI-PHMO-MDI.

[0185] (2) At 80° C., 7.0 wt % 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine was added dropwise, and a chain extension reaction was carried out for 2 h after the addition was completed.

[0186] (3) DMAc was added to form a 20 (w / v)% solution.

[0187] (4) At 80° C., 6.0 wt % of chain extender BDO was gradually added dropwise to the solution in step (3). After the addition was complete, the chain extension reaction was carried out for 2 h.

[0188] (5) Drying at 60°C to obtain a polyurethane film.

[0189] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0190] Example 5

[0191] The synthesis method of the implantable material specifically includes:

[0192] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol and polyhexamethylene glycol (PHMO) are used as soft segment raw materials, and the first isocyanate is used to pre-polymerize and cap the soft segment raw materials:

[0193] Calculated by mass percentage of the reaction system (excluding the solvent DMAc), 32 wt% MDI was placed in a three-necked flask. At 80°C, a mixture of 40 wt% polydimethylsiloxane diol (molecular weight, 1000) and 10 wt% PHMO (molecular weight, 700) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to produce prepolymer 1: MDI-PDMS-MDI and MDI-PHMO-MDI.

[0194] (2) The intermediate product 1 of Preparation Example 1 was used as the second isocyanate, and the temperature was lowered to 50° C. 8 wt % of the second isocyanate was added to the system after the reaction in step (1), and pre-dissolved in DMAc to form a 20 (w / v) % solution, and stirred for 10 to 30 min.

[0195] (3) At 80° C., 5 wt % of a chain extender, 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine, was gradually added dropwise to the solution of step (2). After the addition was complete, a chain extension reaction was carried out for 2 h.

[0196] (4) At 80° C., 5 wt % of chain extender BDO was gradually added dropwise to the reaction system of step (3). After the addition was complete, the chain extension reaction was carried out for 2 h.

[0197] (5) Drying at 60°C to obtain a polyurethane film.

[0198] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0199] Example 6

[0200] The synthesis method of the implantable material specifically includes:

[0201] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol and polyhexamethylene glycol (PHMO) are used as soft segment raw materials, and the first isocyanate is used to pre-polymerize and cap the soft segment raw materials:

[0202] Calculated by mass percentage of the reaction system (excluding the solvent DMAc), 33 wt% MDI was placed in a three-necked flask. At 80°C, a mixture of 44 wt% polydimethylsiloxane diol (molecular weight, 1000) and 11 wt% PHMO (molecular weight, 700) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to produce prepolymers 1: MDI-PDMS-MDI and MDI-PHMO-MDI.

[0203] (2) Prepare the intermediate product 2 of Example 2 as the second isocyanate, cool to 50°C, add 6 wt% of the second isocyanate to the system after the reaction in step (1), and pre-dissolve it in DMAc to form a 20 (w / v)% solution, and stir for 10 to 30 minutes.

[0204] (3) The temperature was raised to 80° C., and 6 wt % of the chain extender BDO was gradually added dropwise to the solution in step (2). After the addition was complete, the chain extension reaction was carried out for 2 h.

[0205] (4) Drying at 60°C to obtain a polyurethane film.

[0206] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0207] Example 7

[0208] The synthesis method of the implantable material specifically includes:

[0209] (1) 30 wt% MDI, 44 wt% polydimethylsiloxane diol (molecular weight 1000), 11 wt% PHMO (molecular weight 700), 9 wt% intermediate 1, and 6 wt% chain extender BDO were added to a three-necked flask, calculated by mass percentage of the reaction system (excluding the solvent DMAc). DMAc was added to form a 20 (w / v)% solution, and the mixture was reacted at 80°C for 4 h.

[0210] (2) Drying at 60°C to obtain a polyurethane film.

[0211] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0212] Example 8

[0213] The synthesis method of the implantable material specifically includes:

[0214] (1) According to the mass percentage of the reaction system (excluding the solvent DMAc), 33 wt% MDI, 43.2 wt% polydimethylsiloxane diol (molecular weight of 1000), 10.8 wt% PHMO (molecular weight of 700), 6.0 wt% BDO, and 7.0 wt% 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine were added to a three-necked flask. DMAc was added to form a 20 (w / v)% solution. The mixture was reacted at 80°C for 4 h under a nitrogen atmosphere.

[0215] (2) Drying at 60°C to obtain a polyurethane film.

[0216] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0217] Comparative Example 1

[0218] (1) Based on the mass percentage of the reaction system (excluding the solvent DMAc), 39 wt% of MDI was placed in a three-necked flask. Under a nitrogen atmosphere and at 80°C, 55 wt% of polydimethylsiloxane diol with a molecular weight of 1000 was added to the three-necked flask using a dropping funnel. After completion of the addition, the mixture was reacted for 2 h to obtain an intermediate product 1, which is a prepolymer 1: MDI-PDMS-MDI.

[0219] (2) At 80°C, 6.0 wt% of chain extender BDO was gradually added dropwise. After the addition was complete, the chain extension reaction was carried out for 2 hours.

[0220] (3) DMAc was added to form a 20 (w / v)% solution.

[0221] (2) Drying at 60°C to obtain a polyurethane film.

[0222] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0223] Comparative Example 2

[0224] (1) According to the mass percentage of the reaction system (excluding the solvent DMAc), 39 wt% of MDI was placed in a three-necked flask. Under a nitrogen atmosphere and at 80°C, 44 wt% of polydimethylsiloxane diol with a molecular weight of 1000 and 11 wt% of polyethylene glycol (PHMO) with a molecular weight of 700 were added dropwise using a dropping funnel. After completion of the addition, the mixture was reacted for 2 h to obtain intermediate products 1, which were prepolymers 1: MDI-PDMS-MDI and MDI-PHMO-MDI.

[0225] (2) At 80°C, 6.0 wt% of chain extender BDO was gradually added dropwise. After the addition was complete, the chain extension reaction was carried out for 2 hours.

[0226] (3) DMAc was added to form a 20 (w / v)% solution.

[0227] (2) Drying at 60°C to obtain a polyurethane film.

[0228] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150°C for 2 hours.

[0229] Comparative Example 3

[0230] Commercially available Elast-Eon 2 TM 85A polyurethane material.

[0231] The raw materials used in each embodiment and comparative example are shown in Table 1:

[0232] Table 1 Raw materials used in various examples and comparative examples

[0233] The amounts of raw materials used in the examples and comparative examples are shown in Table 2:

[0234] Table 2 Amounts of raw materials used in various examples and comparative examples

[0235] Examples 1 to 6 all adopt the prepolymerization method to prepare the implantable materials, wherein:

[0236] In Example 1, MDI is an isocyanate without grafted functional branches, and intermediate product 1 is an isocyanate grafted with functional branches (dimethylsiloxane groups). The two respectively form independent first main chain sections, and the molar ratio is 7:1. Based on this molar ratio, it is calculated that the first main chain sections grafted with functional branches account for 12.50% of the total molar amount of all first main chain sections.

[0237] In Example 2, the molar ratio of polydimethylsiloxane diol to polyethylene glycol is 4:1. The molar ratio of MDI to intermediate product 1 is 7:1. Based on this molar ratio, the first main chain segments grafted with functional branches account for 12.50% of the total molar amount of all first main chain segments.

[0238] In Example 3, BDO is a chain extender without grafted functional branches, and 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine is a chain extender grafted with functional branches (phosphatidylcholine groups). The two independently form independent second main chain segments, and the molar ratio is 4.2:1. Based on this molar ratio, the second main chain segments grafted with functional branches account for 19.23% of the total molar amount of all second main chain segments.

[0239] In Example 4, the molar ratio of polydimethylsiloxane diol to polyethylene glycol was 4:1. BDO was a chain extender without grafted functional branches, and 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine was a chain extender grafted with functional branches (phosphatidylcholine groups). The two independently formed independent second backbone segments, and the molar ratio was 4.2:1. Based on this molar ratio, the second backbone segments grafted with functional branches accounted for 19.23% of the total molar weight of all second backbone segments.

[0240] In Example 5, MDI is an isocyanate without grafted functional branches, and intermediate product 1 is an isocyanate with grafted functional branches. The two respectively form independent first main chain sections, and the molar ratio is 8.9:1; BDO ​​is a chain extender without grafted functional branches, and 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine is a chain extender with grafted functional branches. The two respectively form independent second main chain sections, and the molar ratio is 4.9:1. Based on the two molar ratios, the first main chain sections and the second main chain sections grafted with functional branches account for 12.66% of the total molar amount of all first main chain sections and second main chain sections.

[0241] In Example 6, MDI is an isocyanate without grafted functional branches, and intermediate product 2 is an isocyanate with grafted functional branches (sulfonic acid groups). The molar ratio of the two is 10.85:1. Based on the molar ratio, the first main chain segments grafted with functional branches account for 8.4% of the total molar amount of all first main chain segments.

[0242] Examples 7 and 8 use a one-step synthesis method to prepare implantable materials, wherein:

[0243] In Example 7, MDI is an isocyanate without grafted functional branches, and intermediate product 1 is an isocyanate with grafted functional branches. The two respectively form independent first main chain sections, and the molar ratio is 7:1. The molar ratio is calculated to show that the first main chain sections grafted with functional branches account for 12.50% of the total molar amount of all first main chain sections.

[0244] In Example 8, BDO is a chain extender without grafted functional branches, and 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine is a chain extender with grafted functional branches. The two each form an independent second main chain segment with a molar ratio of 4.2:1. Based on the molar ratio, the second main chain segment grafted with functional branches accounts for 19.23% of the total molar amount of all second main chain segments.

[0245] The tensile strength, elongation, elastic modulus and surface silicon content of the leaflets prepared in each embodiment and comparative example were tested. The test results are shown in Table 3:

[0246] Table 3 Performance test results

[0247] Result Analysis

[0248] (1) Branching effect:

[0249] Based on the application scenario of the leaflet, it is required to have appropriate softness and strength. The softness is generally characterized by the elastic modulus, and the strength includes the tensile strength. Under the condition that the elastic modulus is basically the same, the greater the tensile strength, the better the mechanical properties of the leaflet.

[0250] As shown in Table 3, compared to Comparative Example 1, the results of Examples 1-6 demonstrate that the hard segment grafting has functional side chains with suitable solubility parameters, which can improve the tensile strength of the leaflets. Furthermore, from the perspective of elongation, the leaflets produced in Examples 1-6 all exhibited elongation exceeding 500%, meeting the requirements for leaflet applications.

[0251] (2) The second soft segment effect:

[0252] Compared with Example 1, Example 2 adds polyethylene glycol as the second soft segment mentioned above. Since the second soft segment plays a transitional role between the first soft segment and the hard segment, it is beneficial to further promote the conduction of stress between the hard segment and the soft segment, reduce the possibility of stress accumulation, and ultimately manifest itself in the improvement of the mechanical properties of the leaflet. Referring to Table 3, the tensile strength and elongation of Example 2 are significantly improved, which indicates that stress can be conducted more smoothly.

[0253] Similarly, compared with Example 3, the tensile strength and elongation of Example 4 are significantly improved, which indicates that stress can be transmitted relatively smoothly.

[0254] (3) Biocompatibility and stability:

[0255] Compared with Comparative Example 1, the introduction of polysiloxane side chains significantly increases the surface silicon content of the leaflets of Examples 1 and 2. Generally, the higher the silicon content, the better the biocompatibility and stability of the leaflets.

[0256] Examples 3, 4, and 5 partially replace BDO with a chain extender with phosphorylcholine side chains. The phosphorylcholine on the hard segment is soluble in PDMS, thereby increasing the compatibility between the hard and soft segments. Stress can be conducted between the hard and soft segments, reducing local stress concentration. The results show that the tensile strength is significantly improved. At the same time, phosphorylcholine is in the side chain and has a large steric hindrance with the surrounding groups, forcing it to tend to the surface. The results show that the surface silicon content decreases slightly, but the addition of phosphorylcholine groups changes the distribution of surface elements. Phosphatecholine is also a biocompatible and biostable group, so its tendency to the surface can further improve the biostability and biocompatibility of the membrane.

[0257] Example 6 uses an isocyanate with a sulfonic acid side chain. The sulfonic acid group on the hard segment is soluble in the soft segment, thereby increasing the compatibility of the hard segment and the soft segment. Stress can be conducted between the hard segment and the soft segment, reducing the concentration of local stress. From the results, the tensile strength is significantly improved. At the same time, the phosphorylcholine group is in the side chain and has a large steric hindrance with the surrounding groups, forcing it to tend to the surface. From the results, the surface silicon content decreases slightly, but the addition of the sulfonic acid group changes the distribution of surface elements, resulting in fewer polyether groups exposed on the surface, and the groups most susceptible to oxidative breakage are protected. Therefore, the biological stability of the polyurethane material is improved.

[0258] The technical features of the above-described embodiments may be combined in any manner. To simplify the description, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as no contradiction exists between these combinations of technical features, they should be considered to be within the scope of this specification. When technical features of different embodiments are embodied in the same drawing, it can be deemed that the drawing also discloses examples of combinations of the various embodiments involved.

[0259] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person skilled in the art may make various modifications and improvements without departing from the spirit of the present application, and such modifications and improvements are all within the scope of protection of the present application.

Claims

1. The implantable material is polyurethane, characterized in that: The molecular chain structure of the polyurethane comprises a soft segment and a hard segment, and a functional branch chain is grafted onto the hard segment; the solubility parameter of the functional branch chain is 6-8.

2. The implantable material according to claim 1, characterized in that The functional side chain is at least one of a dimethylsiloxane group, a polydimethylsiloxane group, a phosphorylcholine group, and a sulfonic acid group.

3. The implantable material according to claim 2, characterized in that The molecular weight of the functional side chain is 100-2000.

4. The implantable material according to claim 1, characterized in that The soft segment raw material is oligomer diol.

5. [Corrected 15.12.2023 according to Rule 91] An implantable material according to claim 4, characterized in that The oligomer diol is at least one of polycarbonate diol, polyester diol, polyether diol and polydimethylsiloxane diol.

6. The implantable material according to claim 5, characterized in that The polycarbonate diol is at least one of DONALO T5651 and DONALO T5652.

7. The implantable material according to claim 5, characterized in that The polyester diol is at least one of adipic acid polyester diol and succinic acid polyester diol.

8. The implantable material according to claim 5, characterized in that The polyether diol is at least one of polyethylene glycol and polytetrahydrofuran diol.

9. The implantable material according to claim 1, characterized in that The soft segment includes a first soft segment and a second soft segment; The molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7; The molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10.

10. The implantable material according to claim 9, characterized in that The mass ratio of the first soft segment to the second soft segment in the polyurethane is 2.5 to 5:

1.

11. The implantable material according to claim 1, characterized in that The hard segment comprises: A first backbone segment formed from isocyanate; A second main chain segment formed by a chain extender; The functional branch is grafted to at least one of the first main link and the second main link.

12. [Corrected 15.12.2023 according to Rule 91] An implantable material according to claim 11, characterized in that The raw material of the first main chain section is at least one of toluene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, p-phenylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, and triphenylmethane triisocyanate; The raw material of the second main chain segment is selected from at least one of small molecule diols and small molecule diamines.

13. [Corrected 15.12.2023 according to Rule 91] An implantable material according to claim 12, characterized in that The small molecule diol is at least one of ethylene glycol, butanediol (BDO), hexanediol and octanediol.

14. The implantable material according to claim 12, characterized in that The small molecule diamine is at least one of ethylenediamine, butanediamine and hexamethylenediamine.

15. The implantable material according to claim 11, characterized in that The grafting position of the functional side chain includes the following three methods: Grafted only to the first main link; Grafted only to the second main chain segment; Grafted onto the first main chain link and the second main chain link at the same time.

16. The implantable material according to claim 15, characterized in that The grafting position of the functional side chain is: Only the first main chain segments are grafted, and the first main chain segments grafted with functional branches account for 5 to 20% of the total molar amount of all first main chain segments; or Only the second main chain segments are grafted, and the second main chain segments grafted with functional branches account for 5 to 20% of the total molar amount of all second main chain segments; or The first main chain section and the second main chain section are grafted with functional branches at the same time, and the first main chain section and the second main chain section grafted with functional branches account for 5-20% of the total molar amount of all the first main chain sections and the second main chain sections.

17. The implantable material according to claim 1, characterized in that The isocyanate index R value of the polyurethane is 1.0-1.

1.

18. The implantable material according to claim 1, characterized in that The solubility parameter of the hard segment is 11-14.

19. The implantable material according to claim 1, characterized in that The hard segment accounts for 35-55% of the total mass of the polyurethane.

20. A method for synthesizing an implantable material according to any one of claims 1 to 19, characterized in that: include: Providing a soft segment raw material and a hard segment raw material, and reacting to generate the implantable material; The hard segment raw material comprises isocyanate and a chain extender, at least one of the isocyanate and the chain extender is grafted with a functional branch chain; the solubility parameter of the functional branch chain is 6-8.

21. The synthesis method according to claim 20, characterized in that: The functional side chain is at least one of a dimethylsiloxane group, a polydimethylsiloxane group, a phosphorylcholine group, and a sulfonic acid group; The molecular weight of the functional side chain is 100-2000.

22. The synthesis method according to claim 20, characterized in that: The functional side chains are pre-grafted onto isocyanate and / or chain extender as hard segment raw materials; Or the functional branched chains are grafted during the reaction process.

23. The synthesis method according to claim 20, characterized in that include: Mix all the raw materials to react and generate the implantable material; The reaction temperature is 60-80° C. and the reaction time is 2-6 hours.

24. The synthesis method according to claim 20, characterized in that: include: S100, prepolymerizing and capping the soft segment raw material using isocyanate to obtain a prepolymer; S200, the prepolymer reacts under the action of a chain extender to obtain the implantable material.

25. [Corrected 15.12.2023 in accordance with Rule 91] A method of synthesis according to claim 24, characterized in that The isocyanate in step S100 is a first isocyanate, and a second isocyanate is further added in step S200. The first isocyanate and the second isocyanate have the same or different structures.

26. The synthesis method according to claim 25, characterized in that The first isocyanate and the second isocyanate are each a single isocyanate or a mixture of a plurality of isocyanates.

27. The synthesis method according to claim 26, characterized in that The composition of the mixture of multiple isocyanates is one of the following: a. All are isocyanates without the functional side chains grafted thereto; b. all are isocyanates grafted with the functional side chains; c. One part is isocyanate grafted with the functional side chain, and the other part is isocyanate not grafted with the functional side chain.

28. The synthesis method according to claim 27, characterized in that In the mixture of the plurality of isocyanates, the molar ratio of the isocyanate not grafted with the functional side chain to the isocyanate grafted with the functional side chain is 4 to 20:

1.

29. [Corrected 15.12.2023 in accordance with Rule 91] The synthesis method according to claim 27, characterized in that The isocyanate not grafted with the functional side chain is at least one of toluene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, p-phenylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate and triphenylmethane triisocyanate.

30. The synthesis method according to claim 24, characterized in that: In step S100, the soft segment raw material includes a first soft segment raw material and a second soft segment raw material; the first soft segment raw material and the second soft segment raw material are both prepolymerized and capped with isocyanate.

31. The synthesis method according to claim 30, characterized in that The molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7; The molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10.

32. [Corrected 15.12.2023 in accordance with Rule 91] The synthesis method according to claim 30, characterized in that The first soft segment raw material is polydimethylsiloxane diol; The second soft segment raw material is at least one of polyether diol, polycarbonate diol and polyester diol.

33. The synthesis method according to claim 30, characterized in that The mass ratio of the first soft segment raw material to the second soft segment raw material is 2.5 to 5:

1.

34. The synthesis method according to claim 30, characterized in that In step S100, the first soft segment raw material and the second soft segment raw material are pre-mixed and then added.

35. The synthesis method according to claim 24, characterized in that The chain extender includes a straight chain extender and a chain extender grafted with a functional branched chain; The linear chain extender is at least one of a small molecule diol and a small molecule diamine; The main chain of the chain extender grafted with functional branches is the same as that of the linear chain extender.

36. The synthesis method according to claim 35, characterized in that The chain extender grafted with functional branches is at least one of 1-palmitoyl propanediol-3-phosphocholine, 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonyl phosphatidylcholine and sphingosine phosphorylcholine.

37. The synthesis method according to claim 35, characterized in that The molar ratio of the straight chain extender to the chain extender grafted with functional branches is 4 to 20:

1.

38. The synthesis method according to claim 35, characterized in that In step S200, a mixture of a linear chain extender and a chain extender grafted with functional branches is added.

39. The synthesis method according to claim 35, characterized in that Step S200 includes: The first reaction stage is a process of adding a chain extender grafted with functional branches to react with the prepolymer; The second reaction stage is the process of adding a linear chain extender and continuing the reaction after the first reaction stage.

40. The synthesis method according to claim 39, characterized in that The temperature of the first reaction stage is 60-80°C and the time is 1-2h; The temperature of the second reaction stage is 60-80° C., and the time is 1-2 hours.

41. The synthesis method according to claim 24, characterized in that The chain extension reaction system also includes a solvent; the solvent is at least one of N,N-dimethylacetamide, N,N-dimethylformamide, tetrahydrofuran, dimethyl sulfoxide, and toluene.

42. [Corrected 15.12.2023 according to Rule 91] The synthesis method according to claim 24, characterized in that The prepolymerization temperature in step S100 is 60-80° C. and the time is 2-4 hours; The reaction temperature in step S200 is 60-80° C. and the reaction time is 2-6 hours.

43. An artificial heart valve, characterized in that It comprises a stent and a leaflet connected to the stent, wherein the leaflet is made of any implantable material as claimed in claims 1 to 19; the leaflet is composed of multiple pieces and cooperates with each other to control the opening and closing of the blood flow channel.

44. The artificial heart valve according to claim 43, characterized in that The artificial heart valve further comprises a covering connected to the inner side and / or the outer side of the stent, and the covering is made of the implantable material.

Citation Information

Patent Citations

  • High-biocompatibility phosphorylcholine-modified polyurethane material and prepration method thereof

    CN106589290A

  • Polyether polyurethane material containing phosphorylcholine group on side chain and preparation method thereof

    CN106674484A

  • Polyurethane with biological stability and mechanical stability as well as preparation method and application thereof

    CN114456346A

  • Silicone-modified polyurethane elastomer and its production

    JP1998101766A

  • Polyurethanes

    US20070027285A1