Positive electrode active material and preparation method therefor, positive electrode sheet, secondary battery and electrical device
By using a hollow secondary particle structure in the cathode active material, distributing specific elements M and doping elements A, and regulating the residual alkali content, the problem of impaired cycle performance of nickel cobalt lithium manganate ternary cathode materials when improving power performance is solved. problem, achieving a balance of high power and high cycle performance.
Patent Information
- Application Number
- PCT/CN2023/139148
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2023-12-15
- Publication Date
- 2024-10-24
AI Technical Summary
When improving the power performance of existing lithium nickel cobalt manganate ternary cathode materials, the cycle performance is usually damaged, and it is difficult to effectively improve the ion transmission rate at the grain boundary.
The cathode active material uses a hollow secondary particle structure. By distributing specific elements M and doping elements A at the grain boundaries, and regulating the residual alkali content, the bonding strength and ion transmission rate of the particles are improved, and internal resistance and side reactions are reduced.
It is possible to improve power performance while maintaining high cycle performance, reduce particle cracking and breakage, improve ion transmission rate at grain boundaries, and increase electrochemical activity and gram capacity.
Smart Images

Figure CN2023139148_24102024_PF_FP_ABST
Abstract
Description
Positive electrode active material, preparation method thereof, positive electrode sheet, secondary battery and electrical equipment
[0001] Cross-reference
[0002] This application claims the priority of the Chinese patent application with the application number 202310436352.0 and the invention title "Positive electrode active material, preparation method thereof, positive electrode sheet, secondary battery and electrical equipment" filed on April 21, 2023, the content of which is incorporated herein by reference. Technical field
[0003] This application relates to the technical field of secondary batteries, and in particular, to a positive electrode active material, a preparation method thereof, a positive electrode sheet, a secondary battery and electrical equipment. Background technique
[0004] Developing power-type lithium-ion batteries with high power performance and high cycle stability is an urgent need in the current market. However, in the current research on nickel-containing positive electrode active materials such as lithium nickel cobalt manganese oxide ternary positive electrode materials, when the power performance is effectively improved, the cycle performance is usually impaired.
[0005] Summary of the invention
[0006] In view of the above problems, this application provides a positive electrode active material, a preparation method thereof, a positive electrode sheet, a secondary battery and electrical equipment, which can effectively improve the power performance while maintaining good cycle performance.
[0007] In a first aspect, an embodiment of this application provides a positive electrode active material, the positive electrode active material includes hollow secondary particles; the hollow secondary particles include Li
[0007] Ni x [[ID=2⑨]]Co y Mn z A q M p O b , 0.2 ≤ a ≤ 1.2, 1.8 ≤ b ≤ 2, 0.3 ≤ x ≤ 0.6, 0 ≤ y ≤ 0.4, 0 < z ≤ 0.4, 0 ≤ q ≤ 0.02, 0 < p ≤ 0.02, the element A includes one or more of Al, Ti, Zr, Sr, B, La and Y, and the element M includes one or more of W, Mo, Nb, Y, Ta, La, Zr and Co; the atomic percentage of the element M at the grain boundary ≥ the atomic percentage of the element M in the bulk part of the primary particle, and the distance from the bulk part to the surface of the primary particle is equal to 5% of the volume average particle size Dv50 of the primary particle; the element A is distributed in the hollow secondary particles in a bulk doping manner.
[0008] In the technical solution of the embodiment of the present application, the hollow structure of the hollow secondary particles is beneficial to reducing the internal resistance of the particles and shortening the lithium ion diffusion path, which is conducive to accelerating the ion transport inside the particles and improving the power performance. The positive electrode active material contains a certain amount of element M. On the one hand, it is beneficial to stabilizing the crystal structure of the primary particles and improving the bonding strength between the primary particles, reducing the cracking and fragmentation of the hollow secondary particles during cycling, and thus improving the cycling performance. On the other hand, it is beneficial to improving the ion transport rate at the grain boundaries, thereby improving the power performance. Among them, element M is more distributed at the grain boundaries of the hollow secondary particles. Compared with element M being more distributed in the bulk phase of the primary particles, element M mainly distributed at the grain boundaries can better cooperate with the residual alkali of the positive electrode active material, which is beneficial to strengthening the bonding strength of element M to the grain boundaries, further stabilizing the structure of the hollow secondary particles and improving the cycling performance; it is also beneficial to increasing the ion transport rate at the grain boundaries and improving the power performance.
[0009] Optionally, when a small amount of element A is doped in the positive electrode active material, it is also beneficial to stabilizing the crystal structure, thereby improving the power performance and cycling performance.
[0010] In some embodiments, the residual alkali in the positive electrode active material includes Li2CO3 and LiOH; in the positive electrode active material, the content of Li2CO3 is s, and the content of LiOH is t, 0.05wt% ≤ s ≤ 3wt%, 0 < t ≤ 0.4wt%; optionally, at least one of the following conditions (a1) and (a2) is satisfied; (a1) 0.05wt% ≤ s ≤ 0.4wt%; (a2) 0 < t ≤ 0.25wt%. In this embodiment, the positive electrode active material has a certain content of residual alkali. On the one hand, it can better cooperate with element M mainly distributed at the grain boundaries, which is beneficial to improving the cycling performance; on the other hand, it can provide certain lithium ion transport sites, which is beneficial to improving the power performance; on the other hand, it can attract acidic substances in the electrolyte and reduce the side reaction between the hollow secondary particles and the electrolyte, which is beneficial to improving the cycling performance. The positive electrode active material having a certain content of residual alkali can provide certain lithium ion transport sites, reduce the side reaction between the hollow secondary particles and the electrolyte, and cooperate with element M to strengthen the bonding strength of the grain boundaries and stabilize the structure of the hollow secondary particles; at the same time, a suitable content of residual alkali can control the gas generation amount, thereby further improving the cycling performance.
[0011] In some embodiments, 0 < q ≤ 0.005. In this embodiment, doping a suitable amount of element A in the positive electrode active material is beneficial to stabilizing the crystal structure, thereby improving the power performance and cycling performance; at the same time, a suitable amount of element A further improves the specific capacity of the positive electrode active material.
[0012] In some embodiments, 0 < p ≤ 0.01. In this embodiment, doping the positive electrode active material with an appropriate amount of element M is beneficial to stabilizing the crystal structure of the primary particles, improving the adhesion strength between the primary particles to reduce cracking and fragmentation of the hollow secondary particles during cycling, improving the ion transport rate at the grain boundaries, and cooperating well with the residual alkali; at the same time, an appropriate amount of element M further improves the specific capacity of the positive electrode active material.
[0013] In some embodiments, at least one of the following conditions (b1) to (b5) is satisfied; (b1) The volume average particle size Dv50 of the hollow secondary particles is 2 μm to 5 μm; (b2) The volume average particle size Dv50 of the hollow secondary particles is 2.5 μm to 3.5 μm; (b3) The wall thickness of the hollow secondary particles is 0.2 μm to 1.6 μm; (b4) The ratio of the cavity diameter of the hollow secondary particles to the volume average particle size Dv50 of the hollow secondary particles is k, 0.1 ≤ k ≤ 0.8; (b5) The ratio of the cavity diameter of the hollow secondary particles to the volume average particle size Dv50 of the hollow secondary particles is k, 0.5 ≤ k ≤ 0.8. In this embodiment, when the hollow secondary particles satisfy a specific volume average particle size, the hollow secondary particles have appropriate particle size and specific surface area, can maintain appropriate electrochemical activity, and thus can achieve better power performance; at the same time, side reactions can be effectively controlled. When the hollow secondary particles meet the specific wall thickness requirement, the hollow secondary particles have a lower wall thickness, resulting in lower internal resistance and shorter lithium ion diffusion path of the hollow secondary particles, and lithium ions can be transmitted inside the hollow secondary particles faster, thus achieving better power performance; when the ratio k of the cavity diameter to the volume average particle size of the hollow secondary particles satisfies a specific range, the hollow secondary particles have appropriate relative wall thickness, can reduce the internal stress of the material, and are beneficial to maintaining the structural stability and power performance of the material; at the same time, better power performance can be maintained.
[0014] In some embodiments, the positive electrode active material further includes a coating layer, and the coating layer is distributed on at least part of the surface of the hollow secondary particles; the coating layer includes element Al and / or element B. In this embodiment, the coating layer can reduce the contact area between the hollow secondary particles and the electrolyte, and reduce the side reactions between the hollow secondary particles and the electrolyte, which is beneficial to improving the cycle performance.
[0015] In some embodiments, in the positive electrode active material, the total content of the Al element and / or the B element in the coating layer has a mass ratio b to the positive electrode active material, satisfying at least one of the following conditions (c1) and (c2): (c1) 0 < b ≤ 5 wt%; (c2) 0.1 wt% ≤ b ≤ 2 wt%. In this embodiment, the specified elements in the coating layer satisfy an appropriate mass ratio in the positive electrode active material, effectively reducing side reactions between the hollow secondary particles and the electrolyte while effectively maintaining the gram capacity of the positive electrode active material.
[0016] In some embodiments, the coating layer satisfies at least one of the following conditions (d1) and (d2): (d1) the mass ratio of Al to B is 1 to 5; (d2) the mass ratio of Al to B is 2 to 2.5. In this embodiment, the coating layer includes both Al and B. The Al-containing compound can effectively reduce side reactions, and the B-containing compound can effectively enhance the conductivity of the material. The combination of Al and B in an appropriate mass ratio effectively improves cycle performance while also improving power performance.
[0017] In some embodiments, the true density of the positive electrode active material is ≥4.6 g / cm 3 In this embodiment, the true density of the positive electrode active material is higher than a specific standard, so that the positive electrode active material has a higher energy density.
[0018] In a second aspect, an embodiment of the present application provides a positive electrode plate, including the positive electrode plate of the above embodiment.
[0019] In a third aspect, an embodiment of the present application provides a secondary battery comprising the positive electrode sheet of the above embodiment.
[0020] In a fourth aspect, an embodiment of the present application provides an electrical device comprising the secondary battery of the above embodiment.
[0021] In a fifth aspect, an embodiment of the present application provides a method for preparing a positive electrode active material as described in the above embodiment, comprising: heating a solution containing a transition metal salt to form a carbonate core; causing a precipitation reaction on the surface of the carbonate core to obtain a precursor having a core including a carbonate and an outer shell including a hydroxide; mixing the precursor, a lithium salt, a material containing element A, and a raw material containing element M, and sintering the mixture to obtain hollow secondary particles.
[0022] In some embodiments, at least one of the following conditions (e1) to (e3) is satisfied: (e1) the pH value of the solution containing the transition metal salt is 10.5 to 12; (e2) the time for heating the solution containing the transition metal salt is 14 to 25 hours; (e3) the time for the precipitation reaction to occur is 20 to 28 hours; (e4) the molar ratio of the precursor to the lithium salt is 1:(1 to 1.2). In this embodiment, when at least one of the pH value of the solution containing the transition metal salt, the time for heating the solution containing the transition metal salt, and the time for the precipitation reaction to occur meets specific requirements, it is beneficial to form a positive electrode active material in which the ratio k of the cavity diameter to the volume average particle diameter of the hollow secondary particles meets an appropriate range; the appropriate mass ratio of the precursor to the lithium salt is beneficial to regulating the residual alkali content in the positive electrode active material.
[0023] In some embodiments, the method for preparing the positive electrode active material further comprises: mixing the hollow secondary particles with a raw material for a coating layer, and sintering the mixture to produce a positive electrode active material having a coating layer distributed on at least a portion of the surface of the hollow secondary particles; the coating layer comprises Al and / or B. In this embodiment, the coating layer is formed on at least a portion of the surface of the hollow secondary particles. The coating layer can reduce the contact area between the hollow secondary particles and the electrolyte, thereby reducing side reactions between the hollow secondary particles and the electrolyte, thereby facilitating improved cycling performance.
[0024] The above description is only an overview of the technical solutions of the embodiments of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0026] FIG1 is a schematic structural diagram of a vehicle provided in some embodiments of the present application;
[0027] FIG2 is an exploded view of a battery provided in some embodiments of the present application;
[0028] FIG3 is an exploded view of a secondary battery provided in some embodiments of the present application;
[0029] FIG4 is a schematic diagram of the structure of a positive electrode sheet provided in some embodiments of the present application;
[0030] FIG5 is a process flow chart of a method for preparing a positive electrode active material according to some embodiments of the present application;
[0031] FIG6 is a process flow chart of a method for preparing a positive electrode active material according to some embodiments of the present application;
[0032] FIG7 is a SEM image of the surface of the positive electrode active material prepared in Example 1 of the present application;
[0033] FIG8 is a SEM image of a cross section of the positive electrode active material prepared in Example 1 of the present application;
[0034] FIG9 is another SEM image of the positive electrode active material prepared in Example 1 of the present application;
[0035] FIG10 is the energy spectrum at position 20 in the spectrum of FIG9 .
[0036] Icon: 1000-Vehicle; 100-Battery; 200-Controller; 300-Motor; 10-Case; 11-First part; 12-Second part; 13-Accommodation space; 20-Secondary battery; 21-Casing; 22-Electrode assembly; 23-Electrode terminal; 24-Pressure relief structure; 211-Casing; 212-Cover; 221-Positive electrode sheet; 2211-Positive current collector; 2212-Positive active material layer. DETAILED DESCRIPTION
[0037] To make the purpose, technical solutions and advantages of the examples of the present application clearer, the technical solutions in the examples of the present application will be described clearly and completely below. Where specific conditions are not specified in the examples, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0038] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.
[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0040] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.
[0041] In the description of the embodiments of the present application, the technical term "and / or", such as "Feature 1 and / or Feature 2", means that it can be "Feature 1" alone, it can be "Feature 2" alone, or it can be "Feature 1" plus "Feature 2".
[0042] In the description of the embodiments of the present application, unless otherwise specified, the “multiple” in “one or more” means two or more than two.
[0043] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0044] In the embodiments of this application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components in different embodiments are omitted. It should be understood that the heights, lengths, widths, and other dimensions of the various components in the embodiments of this application, as well as the overall heights, lengths, widths, and other dimensions of the integrated device shown in the drawings are merely illustrative and do not constitute any limitation on this application.
[0045] Market developments indicate that power batteries are becoming increasingly widely used. They are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. As power battery applications continue to expand, market demand is also growing.
[0046] The secondary battery disclosed in the embodiments of the present application can be used, but is not limited to, in electrical equipment such as vehicles, ships, or aircraft. The embodiments of the present application provide an electrical device that uses a battery as a power source. The electrical device can be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery-powered vehicle, an electric car, a ship, a spacecraft, and the like. Among them, the electric toy can include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and the spacecraft can include airplanes, rockets, space shuttles, and spacecraft, and the like.
[0047] For the convenience of explanation, the following embodiments are described by taking a vehicle as an example of an electrical device in the embodiments of the present application.
[0048] Refer to Figure 1, which is a structural schematic diagram of a vehicle 1000 provided in some embodiments of the present application. The vehicle 1000 can be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle can be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is provided inside the vehicle 1000, and the battery 100 can be provided at the bottom, head or tail of the vehicle 1000. The battery 100 can be used to power the vehicle 1000. For example, the battery 100 can serve as an operating power source for the vehicle 1000. The vehicle 1000 may also include a controller 200 and a motor 300. The controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the vehicle 1000.
[0049] In some embodiments of the present application, the battery 100 can not only serve as the operating power source of the vehicle 1000, but also serve as the driving power source of the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.
[0050] In this application, battery 100 refers to a single physical module that includes multiple secondary batteries 20 to provide higher voltage and capacity. It can be in the form of a battery pack, battery module, etc. Battery 100 can include a housing 10 for enclosing the multiple secondary batteries 20. Housing 10 can prevent liquids or other foreign matter from affecting the charging or discharging of the secondary batteries 20.
[0051] Referring to FIG. 2 , FIG. 2 is an exploded view of a battery 100 provided in some embodiments of the present application. The battery 100 includes a housing 10 and a plurality of secondary batteries 20, wherein the plurality of secondary batteries 20 are housed within the housing 10. The housing 10 is used to house the secondary batteries 20, and the housing 10 may have various structures. In some embodiments, the housing 10 may include a first portion 11 and a second portion 12, wherein the first portion 11 and the second portion 12 overlap each other, and the first portion 11 and the second portion 12 together define a housing space 13 for accommodating the secondary batteries 20. The second portion 12 may be a hollow structure with one end open, and the first portion 11 may be a plate-like structure, and the first portion 11 overlaps the open side of the second portion 12 to form the housing 10 having the housing space 13. The first portion 11 and the second portion 12 may also be hollow structures each with one end open, and the open side of the first portion 11 overlaps the open side of the second portion 12 to form the housing 10 having the housing space 13. Of course, the first part 11 and the second part 12 can be in various shapes, such as a cylinder, a cuboid, etc.
[0052] In the battery 100, multiple secondary batteries 20 can be connected in series, in parallel, or in a hybrid configuration. A hybrid configuration refers to multiple secondary batteries 20 being connected both in series and in parallel. Multiple secondary batteries 20 can be directly connected in series, in parallel, or in a hybrid configuration, and then the entire structure of the multiple secondary batteries 20 is housed within the housing 10. Alternatively, multiple secondary batteries 20 can be first connected in series, in parallel, or in a hybrid configuration to form a module, and then the modules can be connected in series, in parallel, or in a hybrid configuration to form a complete structure, which is then housed within the housing 10. The battery 100 may also include other structures. For example, multiple secondary batteries 20 can be electrically connected via a busbar to enable parallel, series, or hybrid configurations of the multiple secondary batteries 20.
[0053] The secondary battery 20 is the smallest unit of the battery pack and can be a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, but is not limited thereto.
[0054] 3 , the secondary battery 20 may include a housing 21 , an electrode assembly 22 , and an electrolyte, both of which are accommodated in the housing 21 .
[0055] The outer shell 21 may include a shell 211 and a cover 212. The shell 211 is a component used to cooperate with the cover 212 to form an internal sealed space of the secondary battery 20, wherein the formed sealed space can be used to accommodate the electrode assembly 22, electrolyte and other components. The cover 212 refers to a component that covers the opening of the shell 211 to isolate the internal environment of the secondary battery 20 from the external environment. The shape of the cover 212 can be adapted to the shape of the shell 211 to cooperate with the shell 211. Functional components such as electrode terminals 23 and pressure relief structures 24 can also be provided on the cover 212. A sealing ring can be configured between the opening of the shell 211 and the cover 212 to achieve a seal between the shell 211 and the cover 212.
[0056] The shell 211 and the cover 212 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shapes of the shell 211 and the cover 212 can be determined according to the specific shape and size of the electrode assembly 22. The material of the shell 211 and the cover 212 can be various, such as but not limited to metals such as copper, iron, aluminum, stainless steel, and aluminum alloy. The material of the sealing ring can be various, such as but not limited to PP (polypropylene), PC (polycarbonate), PET (polyethylene terephthalate) and other materials that are resistant to electrolyte corrosion, high toughness and fatigue resistance. A coating can be formed on the outer surface of the shell 211, and the material of the coating can be various, such as but not limited to corrosion-resistant materials such as Ni and Cr.
[0057] The secondary battery 20 may also be in the form of a soft pack, such as a pouch-type soft pack. The soft pack may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0058] The electrode assembly 22 can be composed of a positive electrode sheet 221, a negative electrode sheet, and a separator. The secondary battery 20 mainly relies on the movement of metal ions between the positive electrode sheet 221 and the negative electrode sheet to operate. During the charge and discharge process, active ions are embedded and released back and forth between the positive electrode sheet 221 and the negative electrode sheet; the separator is arranged between the positive electrode sheet 221 and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. The electrode assembly 22 can be a wound structure or a laminated structure, and the embodiments of the present application are not limited to this.
[0059] Referring to Figure 4 , the positive electrode sheet 221 includes a positive current collector 2211 and a positive active material layer 2212 disposed on the surface of the positive current collector 2211. The positive current collector 2211 has two surfaces that face each other in its thickness direction, and the positive active material layer 2212 is disposed on either or both of the two opposing surfaces of the positive current collector 2211. The positive current collector 2211 can be a metal foil or a composite current collector. The metal foil of the positive current collector 2211 can be made of aluminum. The composite current collector can include a polymer base layer and a metal layer formed on at least one surface of the polymer base layer. The composite current collector can be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer substrate (such as a substrate made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), or polyethylene (PE)). The positive electrode active material in the positive electrode active material layer 2212 may include the positive electrode active material provided in the embodiment of the present application, and may also include positive electrode active material materials such as lithium cobaltate, lithium iron phosphate, lithium manganate, lithium sulfur, etc. In some embodiments, the positive electrode active material layer 2212 may also optionally include a binder. As an example, the binder may include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. In some embodiments, the positive electrode active material layer 2212 may also optionally include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0060] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector. The negative electrode current collector has two opposing surfaces along its thickness, and the negative electrode active material layer is disposed on either or both of the opposing surfaces. The negative electrode current collector can be a metal foil or a composite current collector. The metal foil can be made of copper. The composite current collector can include a polymer base layer and a metal layer formed on at least one surface of the polymer base. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer base layer (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.). The negative electrode active material in the negative electrode active material layer can be carbon, silicon, or other negative electrode active material. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials; other conventional materials that can be used as negative electrode active materials may also be used. These negative electrode active materials may be used alone or in combination of two or more. In some embodiments, the negative electrode active material layer may also optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). In some embodiments, the negative electrode active material layer may also optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the negative electrode active material layer may further include other additives, such as a thickener (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0061] The embodiments of the present application have no particular limitation on the type of isolation membrane, and any known isolation membrane with a porous structure having good chemical stability and mechanical stability can be selected.
[0062] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0063] The electrolyte serves to conduct ions between the positive electrode sheet 221 and the negative electrode sheet. In some embodiments, the electrolyte includes an electrolyte salt and a solvent, wherein the types of the electrolyte salt and the solvent are not specifically limited and can be selected according to needs.
[0064] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0065] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0066] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain properties of the secondary battery 20, such as additives that improve the overcharge performance of the secondary battery 20, and additives that improve the high or low temperature performance of the secondary battery 20.
[0067] With the continued strength of the new energy vehicle market, the demand for power batteries is growing. The development of power lithium-ion batteries with high power performance and high cycle stability has become an urgent need in the current market. Among them, nickel-containing positive electrode active materials, such as nickel-cobalt-manganese oxide ternary positive electrode materials, have attracted much attention due to their advantages such as high specific capacity, high energy density, and high output power.
[0068] In order to improve the power performance and cycle stability of nickel-containing positive electrode active materials such as nickel-cobalt-manganese oxide ternary positive electrode materials, some studies have focused on: regulating particle size to enhance electrochemical reaction activity, doping to stabilize the crystal structure, coating to inhibit side reactions, and constructing porous or hollow polycrystalline particles to increase ion transport rate. However, the increase in reaction activity will lead to more serious side reactions, and the inhibitory effect of the coating layer on side reactions is very limited. Polycrystalline particles with porous or hollow structures are prone to cracking and shattering during repeated charge and discharge at high voltage; at the same time, improving the ion transport rate at the grain boundaries of polycrystalline particles remains a major problem. In other words, in some solutions, the power performance and cycle performance cannot be effectively improved; while in other solutions, when the power performance is effectively improved, the cycle performance is usually impaired.
[0069] Based on this, an embodiment of the present application provides a cathode active material, which includes hollow secondary particles, and a certain amount of a specific element M mainly distributed at the grain boundaries of the hollow secondary particles. Optionally, a small amount of a specific element A is doped, and optionally, the residual alkali with a certain content in the cathode active material is regulated. Among them, the hollow structure of the hollow secondary particles is beneficial to reducing the internal resistance of the particles and shortening the lithium ion diffusion path, which is beneficial to accelerating the ion transport inside the particles and improving the power performance. On the basis of the hollow structure, the element M or the compound containing M is beneficial to improving the bonding strength between primary particles and reducing the cracking and fragmentation of the hollow secondary particles during cycling; a certain amount of residual alkali can also cooperate with the element M or the compound containing M, which is beneficial to strengthening the bonding strength of the element M or the compound containing M to the grain boundaries, thereby effectively improving the cycling performance. In addition, the element A is also beneficial to stabilizing the crystal structure and improving the cycling performance; the element M or the compound containing M also has the function of stabilizing the crystal structure of primary particles and improving the ion transport rate at the grain boundaries, which is beneficial to improving the power performance and cycling performance; a certain amount of residual alkali can provide certain lithium ion transport sites, can attract acidic substances in the electrolyte and reduce the side reactions between the hollow secondary particles and the electrolyte, which is beneficial to improving the power performance and cycling performance.
[0070] Next, the cathode active material and its preparation method proposed in the embodiment of the present application will be elaborated in detail.
[0071] In the first aspect, an embodiment of the present application provides a cathode active material, and the cathode active material includes hollow secondary particles; the hollow secondary particles include Li a Ni x Co y Mn z A q M p O b , where 0.2 ≤ a ≤ 1.2, 1.8 ≤ b ≤ 2, 0.3 ≤ x ≤ 0.6, 0 ≤ y ≤ 0.4, 0 < z ≤ 0.4, 0 ≤ q ≤ 0.02, 0 < p ≤ 0.02, the element A includes one or more of Al, Ti, Zr, Sr, B, La, and Y, and the element M includes one or more of W, Mo, Nb, Y, Ta, La, Zr, and Co; the atomic percentage of the element M at the grain boundaries ≥ the atomic percentage of the element M inside the bulk part of the primary particles, and the distance from the bulk part to the surface of the primary particle is equal to 5% of the volume average particle size Dv50 of the primary particle; the element A is distributed in the hollow secondary particles in a bulk doping manner.
[0072] The hollow secondary particles refer to secondary particles with a cavity inside and agglomeration, and the secondary particles are aggregated by primary particles; the primary particles refer to non-agglomerated particles, that is, single fine grains. The hollow secondary particles are particles with a cavity inside formed by the agglomeration of single fine grains.
[0073] In the embodiment of the present application, the hollow secondary particles include Li a Ni x Co y Mn z A q M p O b The component testing method of the molecular formula can refer to the conventional method. As an example, ICP emission spectroscopy is used for testing.
[0074] It should be noted that the ratio of each element in the positive electrode active material in the present application refers to the ratio of each element in the positive electrode active material before the positive electrode active material is made into a positive electrode plate 221 and assembled into a secondary battery 20 for formation. Those skilled in the art can understand that in the positive electrode plate 221, the secondary battery 20, and the electrical equipment, some elements will be consumed due to processes such as formation and circulation. Therefore, even if the corresponding element ratio of the positive electrode active material is measured to be outside the above range, it should fall within the scope of the present application.
[0075] It should be noted that, in the positive electrode sheet 221, the secondary battery 20, and the electrical device, lithium ions are consumed during the formation and circulation processes, and therefore the measured lithium content a in the positive electrode active material may be less than 1. Furthermore, if the positive electrode sheet 221 and the negative electrode sheet are supplemented with lithium, after the formation and circulation processes, the measured lithium content a in the positive electrode active material may be greater than 1.
[0076] In the embodiments of the present application, the molar coefficient a of the Li (lithium) element is, for example but not limited to, any one of 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.95, 1, 1.05, 1.1, 1.15 and 1.2, or a range between any two of them.
[0077] It should be noted that in the positive electrode sheet 221, the secondary battery 20, and the electrical equipment, due to the loss of oxygen in the positive electrode active material during the cycle process, the measured oxygen content b in the positive electrode active material may be less than 2.
[0078] In the embodiment of the present application, the value of the molar coefficient b of the O (oxygen) element is, for example but not limited to, any one of 1.8, 1.85, 1.9, 1.95 and 2, or a range of values between any two of them.
[0079] The value of the molar coefficient x of the Ni (nickel) element is, for example but not limited to, any one of 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 and 0.6, or a range of values between any two of them.
[0080] The molar coefficient y of the Co (cobalt) element can be 0, which means that the molecular formula of the hollow secondary particles may not contain the Co element. The value of the coefficient y is, for example but not limited to, any point value among 0, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 and 0.4, or a range value between any two of them.
[0081] The molar coefficient z of the Mn (manganese) element can be, for example but not limited to, any one of 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 and 0.4, or a range between any two of them.
[0082] Element A refers to a specific element that is, for example, bulk-doped in the primary particles. The molar coefficient q of element A can be 0, meaning that the molecular formula of the hollow secondary particles does not contain element A. The coefficient q can be, for example, but not limited to, any one of 0, 0.005, 0.01, 0.015, and 0.02, or a range therebetween.
[0083] Element M refers to another type of specified element, which is mainly distributed at the grain boundaries of the hollow secondary particles; the value of the molar coefficient p of element M is, for example but not limited to, any point value among 0.005, 0.01, 0.015 and 0.02, or a range value between any two of them.
[0084] The element A is distributed in the hollow secondary particles in a bulk doping manner, which means that the content of the element A in various locations inside the hollow secondary particles is similar, and the element A is distributed in the entire hollow secondary particles in a relatively uniform manner.
[0085] The atomic percentage of element M at the grain boundaries is ≥ the atomic percentage of element M in the bulk of the primary particles, that is, element M is more distributed at the grain boundaries of the hollow secondary particles.
[0086] The test method for the atomic percentage of element M at different positions can refer to conventional methods. As an example, a SEM image of the cross section of the positive electrode active material can be obtained, and the atomic percentage of element M at different positions can be obtained by analyzing the spectrum.
[0087] The volume average particle size Dv50 refers to the particle size corresponding to 50% in the volume distribution, and can be measured by conventional methods. As an example, referring to GB / T 19077-2016 / ISO 13320:2009 particle size distribution laser diffraction method, the measurement is performed using the Malvern 3000 equipment.
[0088] The distance from the bulk to the surface of the primary particle is equal to the volume average particle diameter Dv50 of the primary particle multiplied by 5%, that is, the diameter of the bulk is 90% of the volume average particle diameter Dv50 of the primary particle.
[0089] In some embodiments of the present application, the grain boundaries of the positive electrode active material include: grain boundaries located outside the hollow secondary particles, grain boundaries located inside the hollow secondary particles and at the junction with the hollow cavity, and grain boundaries in contact between primary particles located inside the hollow secondary particles.
[0090] It should be noted that, in some embodiments of the present application, the element M may be, for example, an oxide MO. n1 or lithium metal oxide Li n2 MO n3 (n1, n2 and n3 are all greater than 0), therefore, when the molecular formula of the hollow secondary particles is confirmed by ICP emission spectroscopy, the detection results show that x+y+z+q<1 and x+y+z+q+p>1.
[0091] In the technical solution of the embodiment of the present application, the hollow structure of the hollow secondary particles is beneficial to reducing the internal resistance of the particles, shortening the lithium ion diffusion path, and accelerating the transmission of ions inside the particles to improve power performance.
[0092] The positive electrode active material contains a certain amount of element M. While maintaining a high discharge capacity of the material, on the one hand, it is beneficial to stabilize the crystal structure of the primary particles, improve the bonding strength between the primary particles and reduce the cracking and breakage of the hollow secondary particles during the cycle, thereby improving the cycle performance; on the other hand, it is beneficial to improve the ion transfer rate at the grain boundary, thereby improving the power performance.
[0093] Among them, element M is more distributed at the grain boundaries of the hollow secondary particles. Compared with element M which is more distributed in the bulk of the primary particles, element M mainly distributed at the grain boundaries can better cooperate with the residual alkali of the positive electrode active material, which is beneficial to strengthen the bonding strength of element M to the grain boundaries, thereby further stabilizing the structure of the hollow secondary particles and improving the cycle performance; it is also beneficial to increase the ion transfer rate at the grain boundaries and improve the power performance.
[0094] Optionally, when a small amount of element A is doped into the positive electrode active material, it is also beneficial to stabilize the crystal structure, thereby improving the power performance and cycle performance.
[0095] In some embodiments, the residual alkali in the positive electrode active material includes Li2CO3 and LiOH; in the positive electrode active material, the content of Li2CO3 is s, and the content of LiOH is t, where 0.05 wt% ≤ s ≤ 3 wt% and 0 < t ≤ 0.4 wt%. Optionally, at least one of the following conditions (a1) and (a2) is satisfied; (a1) 0.05 wt% ≤ s ≤ 0.4 wt%; (a2) 0 < t ≤ 0.25 wt%.
[0096] In some embodiments of the present application, the residual alkali is mainly distributed at the grain boundaries of the hollow secondary particles. The content of the residual alkali in the positive electrode active material can be detected by a conventional method. As an example, it can be determined by the general method for the determination of acidity and alkalinity of chemical reagents (GB / T 9724-2007). The content s of Li2CO3 in the positive electrode active material is, for example but not limited to, any one of the point values of 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, and 4 wt% or the range value between any two of them.
[0097] The content t of LiOH in the positive electrode active material is, for example but not limited to, any one of the point values of 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, and 0.4 wt% or the range value between any two of them.
[0098] Regarding condition (a1), optionally, 0.1 wt% ≤ s ≤ 0.4 wt%.
[0099] Regarding condition (a2), optionally, 0.05 wt% < t ≤ 0.25 wt%.
[0100] In this embodiment, the positive electrode active material has a certain content of residual alkali. On the one hand, it can better cooperate with the element M mainly distributed at the grain boundaries, which is beneficial to improving the cycling performance; on the other hand, it can provide certain lithium ion transport sites, which is beneficial to improving the power performance; on the other hand, it can attract acidic substances in the electrolyte and reduce the side reaction between the hollow secondary particles and the electrolyte, which is beneficial to improving the cycling performance. The positive electrode active material having a certain content of residual alkali can provide certain lithium ion transport sites, can reduce the side reaction between the hollow secondary particles and the electrolyte, and can cooperate with the element M to strengthen the bonding strength of the grain boundaries and stabilize the structure of the hollow secondary particles; at the same time, an appropriate amount of residual alkali content can control the gas generation amount, thereby further improving the cycling performance.
[0101] In some embodiments, 0 <q≤0.005。
[0102] As an example, the value of q is, but not limited to, any one of 0.001, 0.002, 0.003, 0.004 and 0.005, or a range of values between any two of them.
[0103] In this embodiment, doping the positive electrode active material with an appropriate amount of element A is beneficial to stabilizing the crystal structure, thereby improving power performance and cycle performance; at the same time, the appropriate amount of element A further improves the gram capacity of the positive electrode active material.
[0104] In some embodiments, 0 <p≤0.01。
[0105] As an example, the value of p is, but not limited to, any one of 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009 and 0.01, or a range of values between any two of them.
[0106] In this embodiment, doping the positive electrode active material with an appropriate amount of element M is beneficial to stabilizing the crystal structure of the primary particles, improving the bonding strength between the primary particles and reducing the cracking and breakage of the hollow secondary particles during the cycle, improving the ion transfer rate at the grain boundaries, and better coordination with the residual alkali; at the same time, the appropriate amount of element M further improves the gram capacity of the positive electrode active material.
[0107] In some embodiments, the element M is mainly added and distributed in the form of a compound containing the element M, and in the positive electrode active material, the content of the compound containing the element M is 0<≤2 wt %.
[0108] Compounds containing element M include, for example, MO n1 He Li n2 MO n3 (n1, n2 and n3 are all greater than 0) or more.
[0109] As an example, the content of the compound containing element M in the positive electrode active material is, but is not limited to, any one of 0.5 wt %, 1 wt %, 1.5 wt % and 2 wt %, or a range between any two of them.
[0110] In some embodiments, at least one of the following conditions (b1) to (b5) is met; (b1) the volume average particle size Dv50 of the hollow secondary particles is 2 μm to 5 μm; (b2) the volume average particle size Dv50 of the hollow secondary particles is 2.5 μm to 3.5 μm; (b3) the wall thickness of the hollow secondary particles is 0.2 μm to 1.6 μm; (b4) the ratio of the cavity diameter of the hollow secondary particles to the volume average particle size Dv50 of the hollow secondary particles is k, 0.1≤k≤0.8; (b5) the ratio of the cavity diameter of the hollow secondary particles to the volume average particle size Dv50 of the hollow secondary particles is k, 0.5≤k≤0.8.
[0111] Regarding the volume average particle size Dv50 of the hollow secondary particles, its value is, for example but not limited to, any one of 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm and 5 μm, or a range between any two of them.
[0112] The wall thickness of hollow secondary particles refers to the wall thickness from the inner interface to the outer surface of the hollow secondary particles. It can be calculated by subtracting the size of the hollow cavity of the hollow secondary particles from the volume average particle diameter Dv50 of the hollow secondary particles, and then dividing by 2. The test results can be obtained by first obtaining multiple calculation results and then taking the average. The size of the hollow cavity refers to the size corresponding to the line extending through the center of the hollow cavity and extending to the two ends of the hollow cavity.
[0113] Regarding the wall thickness of the hollow secondary particles, its value can be, for example but not limited to, any point value among 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm and 1.6μm, or a range value between any two of them.
[0114] Regarding the k value, its value can be, for example but not limited to, any one of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or a range of values between any two of them.
[0115] As an example, the hollow secondary particles meet the following conditions: the volume average particle size Dv50 of the hollow secondary particles is 2.5 μm to 3.5 μm; the wall thickness of the hollow secondary particles is 0.2 μm to 1.6 μm; the ratio of the cavity diameter of the hollow secondary particles to the volume average particle size Dv50 of the hollow secondary particles is k, 0.5≤k≤0.8.
[0116] In this embodiment, when the hollow secondary particles meet a specific volume average particle diameter, they have a more suitable particle size and specific surface area, can maintain suitable electrochemical activity, and thus achieve better power performance and improve side reaction issues. When the hollow secondary particles meet specific wall thickness requirements, the hollow secondary particles have a lower wall thickness, resulting in lower internal resistance and a shorter lithium ion diffusion path, allowing lithium ions to be transported more quickly within the hollow secondary particles, thereby achieving better power performance. When the ratio k of the hollow secondary particle cavity diameter to the volume average particle diameter meets a specific range, the hollow secondary particles have a suitable relative wall thickness, which can reduce internal stress in the material, which is beneficial for maintaining the structural stability and power performance of the material; at the same time, it can maintain good power performance.
[0117] In some embodiments, the positive electrode active material further includes a coating layer, which is distributed on at least a portion of the surface of the hollow secondary particles; the coating layer includes Al element and / or B element.
[0118] The coating layer is distributed on at least a portion of the surface of the main material. That is, the coating layer can partially cover the surface of the main material or completely cover the surface of the main material.
[0119] The coating layer may include Al (aluminum) element, B (boron) element, or both Al and B elements.
[0120] The Al element is added to the coating layer in the form of an Al-containing compound such as γ-Al2O3, and the final coating layer contains Al in the form of γ-Al2O3 and / or LiAlO2; the B element is added to the coating layer in the form of a B-containing compound such as H3BO3, and the final coating layer contains B in the form of H3BO3 and / or Li3BO3.
[0121] In some embodiments of the present application, the coating layer serves as a structure that coats at least a portion of the surface of the hollow secondary particles. Between the coating layer and the hollow secondary particles, it can be observed that part of the coating material is distributed in the form of small particles on the surface of the hollow secondary particles. The interface between the two can be determined by conventional means, such as directly observing the cross section of the material using a scanning electron microscope.
[0122] In this embodiment, the coating layer can reduce the contact area between the hollow secondary particles and the electrolyte, and can reduce the side reactions between the hollow secondary particles and the electrolyte, thereby facilitating improved cycle performance.
[0123] In some embodiments, in the positive electrode active material, the total content of Al element and / or B element in the coating layer accounts for a mass ratio of b to the positive electrode material, satisfying at least one of the following conditions (c1) and (c2); (c1) 0<b≤5wt%; (c2) 0.1wt%≤b≤2wt%.
[0124] As an example, the total content of Al element and / or B element in the coating layer accounts for the mass ratio b of the positive electrode material, for example but not limited to, any one of 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% and 5wt%, or a range between any two of them.
[0125] In this embodiment, the specified elements in the coating layer satisfy an appropriate mass ratio in the positive electrode active material, which can effectively reduce the side reaction between the hollow secondary particles and the electrolyte while better maintaining the gram capacity of the positive electrode active material.
[0126] In some embodiments, in the coating layer, at least one of the following conditions (d1) and (d2) is satisfied: (d1) the mass ratio of Al to B is 1 to 5; (d2) the mass ratio of Al to B is 2 to 2.5.
[0127] As an example, the mass ratio of Al to B is, for example but not limited to, any one of 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 and 5, or a range of values therebetween.
[0128] In this embodiment, the coating layer includes both Al and B. The compound containing the Al element can effectively reduce side reactions, and the compound containing the B element can effectively enhance the conductivity of the material. Al and B are combined in a suitable mass ratio, which not only effectively improves the cycle performance, but also helps to improve the power performance.
[0129] In some embodiments, the true density of the positive electrode active material is greater than 4.6 g / cm 3 .
[0130] The true density of the positive electrode active material refers to the actual mass of the solid material per unit volume of the positive electrode active material in an absolutely dense state, which can be measured by, for example but not limited to, an immersion method, a gas volumetric method, or the like.
[0131] In this embodiment, the true density of the positive electrode active material is higher than a specific standard, so that the positive electrode active material has a higher energy density.
[0132] In a second aspect, an embodiment of the present application provides a positive electrode plate 221 , including the positive electrode plate 221 of the above embodiment.
[0133] In a third aspect, an embodiment of the present application provides a secondary battery 20 , comprising the positive electrode plate 221 of the above embodiment.
[0134] In a fourth aspect, an embodiment of the present application provides an electrical device, comprising the secondary battery 20 of the above embodiment.
[0135] In a fifth aspect, an embodiment of the present application provides a method for preparing a positive electrode active material as described in the above embodiment, see Figure 5, comprising: heating a solution containing a transition metal salt to form a carbonate core; a precipitation reaction occurs on the surface of the carbonate core to obtain a precursor having a core including a carbonate and an outer shell including a hydroxide; mixing the precursor, a lithium salt, a material containing element A (referred to as A source), and a raw material containing element M (referred to as M source), and sintering them to obtain hollow secondary particles.
[0136] In the solution containing transition metal salts, the type of transition metal can be formulated according to the chemical formula of the hollow secondary particles. For example, the salts of nickel, cobalt and manganese can be regulated so that the nickel, cobalt and manganese elements meet a specific molar ratio; wherein the molar proportions of cobalt and manganese can each independently be 0.
[0137] In the process of heating a solution containing a transition metal salt to form a carbonate core, for example, a carbonate solution of a certain concentration is used as a first-stage precipitant, and ammonia water of a certain concentration is used as a complexing agent. The solution is heated under protective gas conditions and stirred for a period of time to form a carbonate core with a loose structure.
[0138] During the precipitation reaction on the carbonate core surface, sodium hydroxide solution is used as a second-stage precipitant to continue the precipitation reaction. The product is then washed, filtered, and dried to obtain a precursor having a loose carbonate core and a dense hydroxide shell.
[0139] It should be noted that in the process of mixing the precursor, lithium salt, material containing element A, and raw material containing element M, the lithium salt includes one or more of lithium carbonate and lithium hydroxide; when the molar coefficient q of element A in the chemical formula of the hollow secondary particles is 0, the amount of material containing element A is 0; when the molar coefficient p of element M in the chemical formula of the hollow secondary particles is 0, the amount of material containing element M is 0.
[0140] In some embodiments, at least one of the following conditions (e1) to (e3) is met; (e1) the pH value of the solution containing the transition metal salt is 10.5 to 12; (e2) the time for heating the solution containing the transition metal salt is 14 hours to 25 hours; (e3) the time for the precipitation reaction to occur is 20 hours to 28 hours; (e4) the molar ratio of the precursor to the lithium salt is 1:(1 to 1.2).
[0141] Regarding condition (e1), the pH value of the solution containing the transition metal salt is, for example but not limited to, any one of 10.5, 11, 11.5 and 12, or a range between any two of them.
[0142] Regarding condition (e2), the time for heating the solution containing the transition metal salt is, for example but not limited to, any one of 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, 21 h, 22 h, 23 h, 24 h and 25 h, or a range between any two of them.
[0143] Optionally, during the process of heating the solution containing the transition metal salt, the heating temperature is 30° C. to 80° C., accompanied by stirring at a rotation speed of 200 rpm to 800 rpm.
[0144] Regarding condition (e3), the time for the precipitation reaction to occur is, for example but not limited to, any one of 20 h, 21 h, 22 h, 23 h, 24 h, 25 h, 26 h, 27 h and 28 h, or a range between any two of them.
[0145] Optionally, during the precipitation reaction, the pH value of the system is 11.2 to 12.8, the heating temperature is 30° C. to 80° C., and the stirring speed is 400 rpm to 900 rpm.
[0146] Regarding condition (e4), the molar ratio of the precursor to the lithium salt is, for example but not limited to, any one of 1:1, 1:1.05, 1:1.1, 1:1.15 and 1:1.2, or a range between any two of them.
[0147] Optionally, in an embodiment of the present application, during the process of sintering to obtain the hollow secondary particles, the sintering temperature is 700° C. to 950° C., and the sintering time is 9 h to 14 h.
[0148] In this embodiment, when at least one of the pH value of the solution containing the transition metal salt, the time for heating the solution containing the transition metal salt, and the time for the precipitation reaction to occur meets specific requirements, it is beneficial to form a positive electrode active material in which the ratio k of the cavity diameter of the hollow secondary particles to the volume average particle size meets an appropriate range; a suitable mass ratio of the precursor to the lithium salt is beneficial to regulating the residual alkali content in the positive electrode active material.
[0149] Referring to Figure 6, in some embodiments, in an embodiment where the positive electrode active material also includes a coating layer, as an example, the method for preparing the positive electrode active material also includes: mixing the hollow secondary particles with the raw materials of the coating layer, and sintering to obtain a positive electrode active material in which the coating layer is distributed on at least a portion of the surface of the hollow secondary particles.
[0150] Optionally, in an embodiment of the present application, during the process of sintering to obtain the positive electrode active material having the coating layer distributed on at least a portion of the surface of the hollow secondary particles, the sintering temperature is 350° C. to 500° C., and the sintering time is 4 h to 8 h.
[0151] In this embodiment, a coating layer is formed on at least part of the surface of the hollow secondary particles. The coating layer can reduce the contact area between the hollow secondary particles and the electrolyte, and can reduce the side reactions between the hollow secondary particles and the electrolyte, thereby facilitating improved cycle performance.
[0152]
[0153] Some specific embodiments are listed below to better illustrate the present application.
[0154] 1. Preparation of secondary batteries
[0155] (1) Preparation of positive electrode active materials
[0156] Example 1
[0157] 1) A transition metal salt solution containing the corresponding transition metal salts was prepared at a molar ratio of 3:3:3 between nickel, cobalt, and manganese. The total metal concentration of the transition metal salt solution was 2 mol / L, and the addition rate was 12 L / h. A 1.6 mol / L sodium carbonate solution was prepared as a first-stage precipitant at a rate of 20 L / h. Simultaneously, 25% aqueous ammonia was added as a complexing agent at a rate of 2 L / h. The three solutions were added to a reactor containing 95 L of deionized water at 50°C under a nitrogen atmosphere. The stirring rate was controlled at 450 rpm, and the reaction pH was adjusted to a stable value of 11.5. The reaction was stirred continuously for 18 hours to obtain a loosely structured carbonate core.
[0158] 2) Using 4.5 mol / L sodium hydroxide solution as the second-stage precipitant, the addition rate was controlled to 9 L / h, the reaction pH was adjusted to 11.8, and the reaction was stirred at 600 rpm at 50°C under a nitrogen atmosphere for 26 hours. After aging for 2 hours, the mixture was washed, filtered, and dried to obtain a precursor with a loose carbonate as the core and a dense hydroxide as the shell.
[0159] 3) The obtained precursor, lithium hydroxide (LiOH) and titanium oxide (TiO2) are weighed according to a molar ratio of 1:1.15:0.001, and 0.65wt% of the precursor mass of tungsten trioxide (WO3) is added and stirred evenly. Then, in an air or oxygen atmosphere, the temperature is increased to 900°C at a heating rate of 2°C / min, the heat preservation time is 12h, and finally naturally cooled to room temperature to obtain hollow secondary particles after primary sintering.
[0160] 4) The hollow secondary particles obtained after the primary sintering, Al element (derived from γ-Al2O3) and B element (derived from H3BO3) are evenly mixed in a mass ratio of 1:0.004:0.002, and the mixture is heated to 450°C at a heating rate of 2°C / min, kept at this temperature for 6 hours, and finally naturally cooled to room temperature to obtain a positive electrode active material with a coating layer.
[0161] Example 2 to Example 5
[0162] The difference from Example 1 is that in step 1), the pH value and the heating and stirring reaction time of the solution containing the transition metal salt are different, and the positive electrode active materials with different k values of the hollow secondary particles are obtained.
[0163] Example 6 to Example 8
[0164] The difference from Example 1 is that: step 1) the heating and stirring reaction time is different; step 2) the precipitation reaction time is different, and the volume average particle size Dv50 of the hollow secondary particles obtained is different.
[0165] Example 9 to Example 11
[0166] The difference from Example 1 is that the molar ratio of nickel, cobalt and manganese elements added in step 1) is different, and the sintering temperatures in step 3) are modified to 830° C., 850° C. and 890° C. respectively.
[0167] Example 12
[0168] The difference from Example 1 is that the heating and stirring reaction time in step 1) is different from the heating and stirring time in step 2).
[0169] Example 13-Example 14
[0170] The difference from Example 1 is that the pH values of the solution containing the transition metal salt in step 1) are different, namely 10.0 and 9.5.
[0171] Example 15-Example 16
[0172] The difference from Example 1 is that the molar ratios of the precursor added in step 3) to titanium oxide (TiO2) are different, namely 1:0.02 and 1:0.01, respectively.
[0173] Example 17 to Example 18
[0174] The difference from Example 1 is that the titanium oxide (TiO2) added in step 3) is replaced by zirconium oxide (ZrO2) and yttrium oxide (Y2O3) respectively.
[0175] Example 19 to Example 21
[0176] The difference from Example 1 is that the content of the M source (WO3) added in step 3) is changed to 1.5wt%, 1.0wt% and 0.1wt%, respectively.
[0177] Example 22 to Example 24
[0178] The difference from Example 1 is that the M source (WO3) added in step 3) is replaced by oxidized Nb2O5, MoO3 and ZrO2 respectively.
[0179] Example 25
[0180] The difference from Example 1 is that in step 2), no material containing element A is added.
[0181] Example 26 to Example 27
[0182] The difference from Example 1 is that the molar ratios of the precursor material added in step 3) to lithium hydroxide are 1:1.18 and 1:1.13 respectively.
[0183] Example 28
[0184] The difference from Example 1 is:
[0185] The sintering temperature in step 3) is 800°C.
[0186] Example 29
[0187] The difference from Example 1 is that the sintering temperature in step 3) is 1000°C.
[0188] Example 30
[0189] The difference from Example 1 is that the molar ratio of the precursor material added in step 3) to lithium hydroxide is 1:1.
[0190] Example 31 to Example 41
[0191] The difference from Example 1 is that the amount and ratio of the Al element (derived from γ-Al2O3) and the B element (derived from H3BO3) added in step 4) are different.
[0192] Comparative Example 1
[0193] The difference from Example 1 is that in step 2), no material containing element M is added.
[0194] Comparative Example 2
[0195] The difference from Example 1 is that in step 1), 1 wt% (NH4)6W7O is simultaneously mixed into the transition metal salt. 24In the preparation step 2), no material containing element M is added, and the sintering temperature is changed to 850° C. to avoid segregation of element M during the sintering process and ensure that element M is mainly present in the bulk phase.
[0196] The above description of the various embodiments and comparative examples tends to emphasize the differences between the various embodiments and comparative examples. The same or similar points can be referenced to each other and will not be described in detail herein for the sake of brevity.
[0197] (2) Preparation of positive electrode sheet
[0198] The positive electrode slurry prepared above was prepared by mixing the positive electrode active material, conductive agent (super-P), carbon nanotubes (CNT), and polyvinylidene fluoride (PVDF) in a mass ratio of 94:1.5:0.5:3, and coated on a 13 μm Al foil. The positive electrode sheet was obtained after vacuum drying at 120°C, cold pressing, and cutting into strips.
[0199] (3) Preparation of negative electrode sheet
[0200] A negative electrode slurry was prepared by mixing graphite negative electrode material, conductive agent (Super P), binder (SBR), and thickener (CMC-Na) in a mass ratio of 96.2:0.8:1.8:1.2, and coated on an 8μm copper foil. The negative electrode sheet was obtained after vacuum drying at 120°C, cold pressing, and cutting into strips.
[0201] (4) Assemble the battery
[0202] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the anode and cathode to play an isolating role. After winding, they are placed in the outer packaging, injected with the prepared electrolyte, and packaged, injected, formed, and vented to obtain a lithium-ion battery.
[0203] Those skilled in the art will understand that, in the above methods of the specific embodiments and comparative examples, the writing order of the steps does not mean a strict execution order and does not constitute any limitation on the implementation process. The specific execution order of the steps should be determined by their functions and possible internal logic.
[0204] 2. Test Method
[0205] 1) Gram capacity test
[0206] Assemble a button cell using the positive electrode sheet from "I. Preparing a Secondary Battery" as the positive electrode and the lithium sheet as the negative electrode. Test the charge and discharge capacity at 2.8V to 4.2V at a current density of 1C at 25°C.
[0207] At the same time, the coulombic efficiency is calculated based on the charge and discharge capacity: first-cycle coulombic efficiency = first-cycle discharge capacity / first-cycle charge capacity × 100%.
[0208] 2) Power performance test
[0209] At 25°C, fully charge the lithium-ion batteries described in "I. Preparation of Secondary Batteries" at a current density of 1C. Then, discharge them at current densities of 1C and 20C, respectively. Using the 1C capacity as a reference, measure the discharge capacity of the lithium-ion batteries and determine their capacity retention. Here, 20C capacity retention = 20C capacity retention / 1C discharge capacity × 100%.
[0210] 3) Cyclic performance test
[0211] The lithium-ion batteries described in "Preparation of Secondary Batteries" were subjected to charge and discharge cycle testing at 25°C and a current density of 5C, with a voltage range of 2.8V to 4.2V. Capacity retention = discharge capacity at the first cycle / discharge capacity at 1000 cycles × 100%.
[0212] 4) Chemical composition test
[0213] Confirmation of molecular formula: The molecular formula of the hollow secondary particles was determined by ICP emission spectroscopy.
[0214] The mass content of Li2CO3 and LiOH can be determined using the General Method for the Determination of Acidity and Alkalinity of Chemical Reagents (GB / T 9724-2007). Using dilute hydrochloric acid as the titrant, the filtrate undergoes an automated two-step potentiometric titration. The following reactions occur: LiOH + HCl = LiCl + H2O, and Li2CO3 + HCl = LiHCO3 + LiCl. With the continued addition of dilute hydrochloric acid, all of the lithium hydroxide is converted to lithium chloride and water, and all of the Li2CO3 is converted to lithium bicarbonate and lithium chloride. At this point, the pH is approximately 4.0-5.0, and the potentiometric titrator exhibits an electrode potential jump, EP1. With continued addition of dilute hydrochloric acid, LiHCO3 + HCl = LiCl + CO2↑ + H2O. At this point, the pH is approximately 8.0-9.0, and the potentiometric titrator exhibits an electrode potential jump, EP2. The amounts of dilute hydrochloric acid consumed corresponding to EP1 and EP2 can be used to calculate the Li2CO3 and LiOH contents in the sample.
[0215] 3. Experimental conditions and test results
[0216] The main experimental conditions and test results in each experimental group are shown in Tables 1 to 3 and Figures 8 to 10. For experimental conditions not described, refer to the above description of the specific embodiments and comparative examples and will not be repeated herein.
[0217] Table 1.1
[0218] Table 1.2
[0219] Table 2.1
[0220] Table 2.2
[0221] The molar proportion of element A refers to its molar proportion in the mixed material in step 3).
[0222] Table 3
[0223] FIG7 is a SEM image of the surface of the positive electrode active material prepared in Example 1 of the present application; as can be seen from FIG7 , the positive electrode active material prepared in Example 1 exhibits a polycrystalline particle morphology composed of a plurality of primary small particles.
[0224] FIG8 is a SEM image of a cross section of the positive electrode active material prepared in Example 1 of the present application. As can be seen from FIG8 , the positive electrode active material prepared in Example 1 has a hollow structure.
[0225] The positive electrode active material presents a polycrystalline particle morphology composed of multiple primary small particles, and has good sphericity and roundness.
[0226] Figure 9 is another SEM image of the positive electrode active material prepared in Example 1 of the present application; Figure 10 is the energy spectrum at point 20 in the spectrum diagram of Figure 9 (point 20 in the spectrum diagram is used as an example, and the same method is used to analyze other points).
[0227] 9 and 10 , the weight percentage, weight percentage variance, and atomic percentage of the element M corresponding to each site in the cross section of the positive electrode active material are shown in Table 4.
[0228] Table 4
[0229] According to Table 4, in the positive electrode active material prepared in Example 1 of the present application, the content of element M at the grain boundary is greater than the content in the bulk of the primary particles.
[0230] Combined with the above Tables 1 to 3, a brief analysis is as follows:
[0231] In Examples 1 to 14:
[0232] In Examples 1 to 11, the pH value of the solution containing the transition metal salt, the heating time of the solution containing the transition metal salt, and the precipitation reaction time are appropriately controlled in the preparation process, so that the k value of the hollow secondary particles can be well controlled within the range of 0.5 to 0.8; in Example 12, the heating time of the solution containing the transition metal salt is relatively long and the precipitation reaction time is relatively short, and the k value of the hollow secondary particles obtained is relatively high; in Examples 13 to 14, the pH value of the solution containing the transition metal salt is relatively low, and the k value of the hollow secondary particles obtained is relatively low.
[0233] Compared with Examples 1 to 5, the volume average particle size Dv50 of the hollow secondary particles in Example 12 is similar, the k value of the hollow secondary particles in Example 12 is relatively high, and Examples 1 to 5 have higher power performance and cycle performance.
[0234] Compared with Examples 1 to 5, the volume average particle size Dv50 of the hollow secondary particles in Examples 13 to 14 is similar, the k value of the hollow secondary particles in Examples 13 to 14 is relatively low, and Examples 1 to 5 have higher power performance and cycle performance.
[0235] Compared with Examples 1 to 5, the k values of the hollow secondary particles in Examples 6 to 8 are similar. The volume average particle size Dv50 of the hollow secondary particles in Examples 1 to 5 is in the range of 2.5 μm to 3.5 μm, and the volume average particle size Dv50 of the hollow secondary particles in Examples 6 to 8 is not in the range of 2.5 μm to 3.5 μm. Examples 1 to 5 have higher power performance and cycle performance.
[0236] Compared with Examples 1 to 5, Examples 9 to 11 mainly differ in the ratio of nickel, cobalt and manganese. All Examples have good power performance and cycle performance.
[0237] In Example 1 and Examples 15 to 27:
[0238] Compared with Example 1, Example 15-Example 16 and Example 25, Example 1 and Example 15-Example 16 added an appropriate amount of source A, and the power performance and cycle performance were improved. Among them, compared with Example 1 and Example 15-Example 16, the amount of source A added in Example 15-Example 16 was relatively high, and Example 1 had better cycle performance and power performance.
[0239] Compared with Example 1 and Example 17 to Example 18, different A sources are used, and each example has better power performance and cycle performance.
[0240] Compared with Comparative Example 1, Example 19 to Example 21, an appropriate amount of M source and an appropriate amount of residual alkali are added to Example 1 and Example 19 to Example 21, and the power performance and cycle performance are significantly improved.
[0241] Compared with Example 1 and Examples 22 to 24, different M sources are used, and each example has better power performance and cycle performance.
[0242] Compared with Example 1 and Comparative Example 2, in Example 1, the M source is more distributed at the grain boundaries, and in Example 27, the M source is bulk-doped. Example 1 can better cooperate with an appropriate amount of residual alkali and has better power performance and cycle performance.
[0243] In Example 1, Example 26 to Example 30:
[0244] According to the comparison between Example 1 and Examples 26 to 30, it can be seen that the lithium salt ratio and the sintering temperature will affect the residual alkali content in the positive electrode active material.
[0245] The positive electrode active materials in Example 1 and Examples 26 to 29 all contain a certain amount of Li2CO3 and LiOH, which can be well coordinated with the element M, and the power performance and cycle performance are significantly improved.
[0246] Compared with Example 1, Example 30 has a lower content of Li2CO3, and Example 1 has significantly better power performance and cycle performance.
[0247] In Example 1 and Examples 31 to 41:
[0248] Compared with Example 1, Examples 31 to 40 and Example 41, Example 41 has no coating layer. Example 1 and Examples 31 to 40 have better power performance and cycle performance.
[0249] Compared with Example 1, Example 37 to Example 38 and Example 39 to Example 40, the coating layer in Example 39 includes Al but not B, the coating layer in Example 40 includes B but not Al, the coating layers in Example 1 and Example 37 to Example 38 include Al and B, Example 1 and Example 37 to Example 38 have better power performance than Example 39, and Example 1 and Example 37 to Example 38 have better cycle performance than Example 40.
[0250] Compared with Example 1 and Examples 31 to 32, the content of the coating layer in Examples 33 to 34 is relatively high, and Example 1 has higher gram capacity and power performance.
[0251] Compared with Example 1 and Examples 36 to 38, Al and B in Example 1 have a more appropriate mass ratio, and Example 1 has higher gram capacity and power performance.
[0252] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A positive electrode active material, characterized in that: The positive electrode active material includes hollow secondary particles; The hollow secondary particles include Li a Ni x Co y Mn z A q M p O b , 0.2 ≤ a ≤ 1.2, 1.8 ≤ b ≤ 2, 0.3 ≤ x ≤ 0.6, 0 ≤ y ≤ 0.4, 0 < z ≤ 0.4, 0 ≤ q ≤ 0.02, 0 < p ≤ 0.02, the element A includes one or more of Al, Ti, Zr, Sr, B, La, and Y, and the element M includes one or more of W, Mo, Nb, Y, Ta, La, Zr, and Co; The atomic percentage of the element M at the grain boundary is ≥ the atomic percentage of the element M in the bulk phase of the primary particle, and the distance from the bulk phase to the surface of the primary particle is equal to the volume average particle size Dv50 of the primary particle multiplied by 5%; the element A is distributed in the hollow secondary particle in the form of bulk doping.
2. The positive electrode active material according to claim 1, characterized in that The residual alkali in the positive electrode active material includes Li2CO3 and LiOH; in the positive electrode active material, the content of Li2CO3 is s, the content of LiOH is t, 0.05wt%≤s≤3wt%, 0 <t≤0.4wt%; Optionally, at least one of the following conditions (a1) and (a2) is satisfied; (a1)0.05wt%≤s≤0.4wt%; (a2)0 <t≤0.25wt%。 3. The positive electrode active material according to claim 1 or 2, characterized in that: 0<q≤0.005。 4. The positive electrode active material according to any one of claims 1 to 3, characterized in that 0<p≤0.01。 5. The positive electrode active material according to any one of claims 1 to 4, characterized in that Satisfy at least one of the following conditions (b1) to (b5); (b1) the volume average particle size Dv50 of the hollow secondary particles is 2 μm to 5 μm; (b2) the volume average particle size Dv50 of the hollow secondary particles is 2.5 μm to 3.5 μm; (b3) the wall thickness of the hollow secondary particles is 0.2 μm to 1.6 μm; (b4) the ratio of the cavity diameter of the hollow secondary particles to the volume average particle diameter Dv50 of the hollow secondary particles is k, 0.1≤k≤0.8; (b5) The ratio of the cavity diameter of the hollow secondary particles to the volume average particle diameter Dv50 of the hollow secondary particles is k, and 0.5≤k≤0.
8.
6. The positive electrode active material according to any one of claims 1 to 5, characterized in that The positive electrode active material further includes a coating layer, and the coating layer is distributed on at least a portion of the surface of the hollow secondary particle; The coating layer includes Al element and / or B element.
7. The positive electrode active material according to claim 6, characterized in that In the positive electrode active material, the total content of the Al element and / or the B element in the coating layer accounts for a mass ratio of b to the positive electrode active material, satisfying at least one of the following conditions (c1) and (c2); (c1) 0<b≤5wt%; (c2)0.1wt%≤b≤2wt%.
8. The positive electrode active material according to claim 6 or 7, characterized in that: In the coating layer, at least one of the following conditions (d1) and (d2) is satisfied; (d1) the mass ratio of Al to B is 1 to 5; (d2) The mass ratio of the Al to the B is 2 to 2.
5.
9. The positive electrode active material according to any one of claims 1 to 8, characterized in that The true density of the positive electrode active material is ≥4.6 g / cm 3 .
10. A positive electrode sheet, characterized in that: The invention comprises the positive electrode active material as claimed in any one of claims 1 to 9.
11. A secondary battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 10.
12. An electrical equipment, characterized in that: Comprising the secondary battery as claimed in claim 11.
13. A method for preparing a positive electrode active material according to any one of claims 1 to 9, characterized in that: include: Heating a solution containing a transition metal salt to form a carbonate core; A precipitation reaction occurs on the surface of the carbonate inner core to obtain a precursor having an inner core including carbonate and an outer shell including hydroxide; The precursor, lithium salt, the material containing the element A, and the raw material containing the element M are mixed and sintered to obtain the hollow secondary particles.
14. The preparation method according to claim 13, characterized in that: Satisfy at least one of the following conditions (e1) to (e3); (e1) the pH value of the solution containing the transition metal salt is 10.5 to 12; (e2) heating the solution containing the transition metal salt for 14 to 25 hours; (e3) The precipitation reaction takes place for 20 to 28 hours; (e4) The molar ratio of the precursor to the lithium salt is 1:(1-1.2).
15. The preparation method according to claim 13 or 14, characterized in that: Also includes: The hollow secondary particles are mixed with raw materials for the coating layer, and sintered to obtain a positive electrode active material having the coating layer distributed on at least a portion of the surface of the hollow secondary particles; The coating layer includes Al element and / or B element.
Citation Information
Patent Citations
Positive electrode material precursor for lithium batteries and preparation method thereof
CN110817978A
Nickel-cobalt-manganese ternary positive electrode material and preparation method thereof
CN113258061A
Lithium ion battery positive electrode material with non-hollow porous structure as well as preparation method and application of lithium ion battery positive electrode material
CN114744188A
Porous-structure precursor, hollow-structure oxide and application of porous-structure precursor and hollow-structure oxide in positive electrode material
CN114772556A
A waterless, high-rate hollow high-nickel cathode material, its preparation method and application
CN114937769A
Cited By
Positive electrode material and secondary battery
CN119764416A
Lithium-metal composite oxide powder, positive electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secodary battery