Separator, battery cell, battery, and electric device

By using a swollen polymer isolation film with compression resistance and high liquid absorption capacity in the battery cell, and setting a recessed area in the electrode assembly, the problem of electrolyte being squeezed out is solved and the reliability and cycle of the battery are improved. performance.

WO2024217092A1PCT designated stage expired Publication Date: 2024-10-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2024/072431
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-01-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The reliability and cycle performance of battery cells are poor, mainly because the electrolyte is easily squeezed out during the charge and discharge process, resulting in a lack of liquid in the electrode assembly, which affects the dynamic performance and life of the battery.

Method used

A separator membrane including a swollen polymer is used. The membrane has excellent compression resistance and liquid absorption capacity, and can store the electrolyte and prevent it from being extruded. The liquid storage space is increased by setting a recessed area in the electrode assembly to ensure electrolysis. uniform infiltration of liquid and reduce the risk of leakage.

Benefits of technology

It improves the reliability and cycle performance of battery cells, extends the life of the battery, reduces the risk of electrolyte leakage, and enhances the dynamic performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024072431_24102024_PF_FP_ABST
    Figure CN2024072431_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a separator, a battery cell, a battery, and an electric device. The separator comprises two surfaces opposite each other in a thickness direction of the separator, at least one of the surface of the separator and the interior of the separator comprises a pore structure, and the separator further comprises a swelling polymer; and the separator satisfies: when a pressure of 1.25 MPa is applied in the thickness direction of the separator, a compression ratio ΔV of the separator is ≤ 25%.
Need to check novelty before this filing date? Find Prior Art

Description

Separator, battery cell, battery and electrical device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310409606.X filed on April 17, 2023, entitled “Separation membrane, battery cell, battery and electrical device,” the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the field of battery technology, and more specifically, to a separator, a battery cell, a battery, and an electrical device. Background Art

[0004] Battery cells have the characteristics of high capacity and long life, and are therefore widely used in electronic devices such as mobile phones, laptops, electric vehicles, electric airplanes, electric boats, electric toy cars, electric toy boats, electric toy airplanes and power tools, etc.

[0005] As battery applications become increasingly widespread, the requirements for battery cell performance are becoming increasingly stringent. To improve battery cell performance, optimization and improvement are often performed on the battery cells; however, the reliability and cycle performance of battery cells remain poor.

[0006] Summary of the Invention

[0007] The present application is made in view of the above-mentioned problems, and its object is to provide a separator, a battery cell, a battery, and an electrical device.

[0008] In the first aspect, the present application proposes an isolation membrane, which includes two surfaces opposite to each other along its own thickness direction, at least one of the surface of the isolation membrane and the interior of the isolation membrane includes a pore structure, and the isolation membrane also includes a swelling polymer; the isolation membrane satisfies: when a pressure of 1.25 MPa is applied along the thickness direction of the isolation membrane, the compression rate ΔV of the isolation membrane is ≤25%.

[0009] Therefore, when the isolation membrane of the embodiment of the present application meets the above conditions, the isolation membrane can simultaneously have good liquid absorption capacity and excellent compression resistance, and the pore structure will basically not undergo compression deformation, so that the electrolyte can be stored in the pore structure, thereby reducing the risk of the electrolyte being squeezed out of the electrode assembly and improving the reliability and cycle performance of the battery cell.

[0010] In some embodiments, at least one surface of the isolation membrane includes a pore structure, and the pore structure includes a first recessed area.

[0011] In some embodiments, the isolation film further satisfies:

[0012] Take an isolation film with an area of ​​5 cm × 10 cm and record its mass ms1 in g;

[0013] The separator was immersed in excess electrolyte at 25°C for 7 days, and then the separator was taken out and placed vertically until there was no droplet. After 5 minutes, the mass ms2 was recorded in g.

[0014] Then, ((ms2-ms1) / ms1)×100%≥10%.

[0015] Therefore, when the embodiment of the present application satisfies the above range, the liquid absorption capacity of the separator is relatively strong, which is conducive to adsorbing the electrolyte into the swollen polymer molecular chain, thereby improving the cycle performance of the battery cell.

[0016] In some embodiments, the swelling ratio of the swellable polymer is ≥ 100%. When the swelling ratio of the swellable polymer is within the above range, the electrolyte is more easily diffused into the polymer molecular chains of the separator, thereby making the separator have better liquid absorption capacity.

[0017] In some embodiments, the compression modulus of the separator is ≥45 MPa. When the separators of the embodiments of the present application meet the above conditions, they have excellent compression resistance and their pore structures are substantially free of compression deformation, thereby reducing the risk of electrolyte being squeezed out of the electrode assembly and improving the reliability and cycle performance of the battery cells.

[0018] In some embodiments, the separator includes a first porous base membrane including the swollen polymer.

[0019] In some embodiments, the pore structure is disposed inside the first porous base membrane.

[0020] In some embodiments, the surface of the first porous base membrane includes at least one first recessed area.

[0021] In some embodiments, the separator includes a second porous base membrane and a coating layer disposed on at least one side of the second porous base membrane, wherein the coating layer includes the swelling polymer.

[0022] In some embodiments, the surface of the coating layer facing away from the second porous base membrane includes at least one of the first recessed areas.

[0023] In some embodiments, the first recessed area is formed between the coating layer and the second porous base membrane.

[0024] In some embodiments, the swelling polymer includes at least one of a first fluorinated polymer, a first ester polymer, and a first ether polymer. These polymers have excellent swelling properties and compression modulus, which facilitates electrolyte absorption. Furthermore, they are not easily compressed during the charge and discharge process of the battery cell, thereby reducing the amount of electrolyte flowing out of the electrode assembly.

[0025] In a second aspect, the present application further proposes a battery cell comprising an electrode assembly and an electrolyte, wherein the electrode assembly comprises a separator as described in any embodiment of the first aspect of the present application.

[0026] In some embodiments, the battery cell satisfies: V0 / (m / ρ)≥1;

[0027] Where,

[0028] V0 represents the pore volume and interlayer gap volume in the electrode assembly, and its unit is mL;

[0029] m represents the difference between the mass of the battery cell before drying and the mass after drying, and its unit is g;

[0030] ρ represents the density of the electrolyte, and its unit is g / mL.

[0031] Therefore, when the battery cell of the embodiment of the present application satisfies the above formula, there can be sufficient space in the electrode assembly to provide storage space for the electrolyte, thereby reducing the risk of the electrolyte flowing out of the electrode assembly and improving the cycle performance of the battery cell.

[0032] In some embodiments, the electrode assembly includes a first electrode piece and a second electrode piece, wherein the first electrode piece and the second electrode piece have opposite polarities. The separator is disposed between the first electrode piece and the second electrode piece, and the surface of the first electrode piece facing the separator has at least one second recessed area. The second recessed area can increase liquid storage space, reduce the risk of electrolyte leakage into the electrode assembly, and improve the cycling performance of the battery cell.

[0033] In some embodiments, the battery cell further includes an electrolyte, and the electrolyte is located in the electrode assembly;

[0034] Optionally,

[0035] The battery cell satisfies: (m / ρ) / V 总孔 ≥80%;

[0036] V 总孔 A value representing the pore volume of the electrode assembly, in mL;

[0037] m represents the difference between the mass of the battery cell before drying and the mass after drying, and its unit is g;

[0038] ρ represents the density of the electrolyte, and its unit is g / mL.

[0039] Therefore, when the battery cell of the embodiment of the present application meets the above conditions, most of the electrolyte is located in the pore structure of the electrode assembly, that is, the electrode assembly itself has good liquid absorption and liquid retention capabilities, which is conducive to the transmission of active ions and improves the kinetic performance of the battery cell; a small part of the electrolyte can diffuse into the swelling polymer and release liquid during the battery cell's cyclic charge and discharge process. Since the amount of released liquid is relatively small, the electrolyte is not easy to flow out of the electrode assembly, and the electrolyte can make the electrode assembly more uniformly infiltrated, thereby improving the cycle performance of the battery cell.

[0040] In some embodiments, the battery cell satisfies:

[0041] 0≤y / Ah≤15%;

[0042] y represents the volume of free electrolyte in the battery cell, in mL;

[0043] Ah represents the value of the nominal capacity of the battery cell, and its unit is Ah.

[0044] Therefore, when the battery cell of the embodiment of the present application meets the above conditions, the free electrolyte content in the battery cell is extremely small, or even substantially free electrolyte is contained in the battery cell, thereby significantly improving the reliability and cycle performance of the battery cell.

[0045] In some embodiments, the battery cell satisfies:

[0046] 0≤y / V 总孔 ≤15%;

[0047] y represents the volume of free electrolyte in the battery cell, in mL;

[0048] V 总孔 The value representing the pore volume of the electrode assembly, with the unit being mL.

[0049] Therefore, when the battery cell of the embodiment of the present application meets the above conditions, the free electrolyte content in the battery cell is extremely small, or even substantially free electrolyte is contained in the battery cell, thereby significantly improving the reliability and cycle performance of the battery cell.

[0050] In some embodiments, after the battery cell is subjected to a linear frequency sweep vibration test, it is charged to 100% state of charge (SOC). A hole is opened on the battery cell, and the hole is located at the lowest point in the vertical direction. The volume of electrolyte flowing out of the battery cell is recorded as M1, where 0 mL ≤ M1 ≤ 0.5 mL. Optionally, M1 is 0 mL.

[0051] in,

[0052] The vibration direction of the linear sweep vibration test is: single vibration up and down;

[0053] The vibration frequency of the linear sweep vibration test is: 10Hz~55Hz;

[0054] The maximum acceleration of the linear sweep vibration test is: 30m / s 2 ;

[0055] The number of sweep cycles of the linear sweep vibration test is: 10 times;

[0056] The vibration time of the linear sweep frequency vibration test is 3 hours.

[0057] When the battery cell of the embodiment of the present application meets the above conditions, the free electrolyte content in the battery cell is extremely small, or even substantially free electrolyte is contained in the battery cell, thereby significantly improving the reliability and cycle performance of the battery cell.

[0058] In some embodiments, after the battery cell is subjected to the linear sweep vibration test, the electrode assembly is removed, and after the electrode assembly is subjected to the extrusion test, the volume of the electrolyte flowing out of the electrode assembly is recorded as M2, 0 mL≤M2≤0.5 mL, optionally, M2 is 0 mL; wherein,

[0059] The extrusion direction of the extrusion test is: perpendicular to the thickness direction of the electrode assembly;

[0060] The extrusion degree of the extrusion test is: the extrusion force is 0.35 MPa.

[0061] When the battery cell of the embodiment of the present application meets the above conditions, after extrusion, the free electrolyte content in the battery cell is extremely small, or even substantially free electrolyte is contained in the battery cell, thereby significantly improving the reliability and cycle performance of the battery cell.

[0062] In a third aspect, the present application proposes a battery, comprising a battery cell as described in any embodiment of the second aspect of the present application.

[0063] In a fourth aspect, the present application proposes an electrical device comprising the battery as described in the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0065] FIG1 is a schematic diagram of an isolation membrane according to an embodiment of the present application.

[0066] FIG2 is a schematic diagram of another embodiment of the isolation membrane of the present application.

[0067] FIG. 3 is a schematic diagram of the isolation film shown in FIG. 2 at another angle.

[0068] FIG4 is a schematic diagram of another embodiment of the isolation membrane of the present application.

[0069] FIG5 is a schematic diagram of another embodiment of the isolation membrane of the present application.

[0070] FIG6 is a schematic diagram of another embodiment of the isolation membrane of the present application.

[0071] FIG. 7 is a schematic diagram of an embodiment of an electrode assembly of a battery cell of the present application.

[0072] FIG8 is a schematic diagram of another embodiment of an electrode assembly of a battery cell of the present application.

[0073] FIG9 is a schematic diagram of another embodiment of an electrode assembly of a battery cell of the present application.

[0074] FIG. 10 is a schematic diagram of a battery cell according to an embodiment of the present application.

[0075] FIG. 11 is an exploded schematic diagram of the embodiment of the battery cell of FIG. 10 .

[0076] FIG12 is a schematic diagram of an embodiment of a battery module of the present application.

[0077] FIG13 is a schematic diagram of an embodiment of a battery pack of the present application.

[0078] FIG. 14 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 13 .

[0079] FIG15 is a schematic diagram of an embodiment of an electric device including the battery cell of the present application as a power source.

[0080] The drawings are not necessarily drawn to scale.

[0081] The accompanying drawings are marked as follows: 1. Battery pack; 2. Upper case; 3. Lower case; 4. Battery module; 5. Battery cell; 51. Shell; 52. Electrode assembly; 53. Cover plate; 6. Electrical device; 7. Isolation membrane; 71. First recessed area; 711. Second porous base membrane; 712. Coating; 8. First pole piece; 81. Second recessed area; 9. Second pole piece. DETAILED DESCRIPTION

[0082] Below, the embodiments of the separator, battery cell, battery, and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially identical structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0083] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0084] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0085] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0086] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0087] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0088] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0089] The battery cell includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator. The separator is arranged between the positive electrode sheet and the negative electrode sheet. Its main function is to prevent the positive electrode sheet and the negative electrode sheet from short-circuiting, while allowing active ions to pass freely to form a loop.

[0090] During the charge and discharge cycle of the battery cell, the volume of the electrode assembly may change (such as expansion and deformation) due to the embedding or removal of active ions from the active material, resulting in the electrolyte infiltrated in the electrode assembly being continuously squeezed out. It is difficult to absorb the squeezed electrolyte back, and sufficient time is required to be completely absorbed back into the electrode assembly. This leads to liquid shortage and bridge breakage in application scenarios such as fast charging cycles where there is not enough standing time. Since the electrolyte bridge is broken, the active material cannot be fully infiltrated, and the local lack of liquid in the active material makes it impossible to cycle charge and discharge in this area. Its kinetic performance will deteriorate sharply, causing metal precipitation at the interface and increasing the risk of dendrites. As the dendrites grow, the dendrites may pierce the isolation membrane, causing a short circuit between the positive and negative pole pieces, thereby deteriorating the reliability and cycle performance of the battery cell.

[0091] In view of the above problems, the present application proposes a separator membrane comprising a swellable polymer having a strong affinity for the electrolyte. Upon contact between the two, the swellable polymer can lock the electrolyte between the polymer molecular chains through physical adsorption. When the separator membrane is applied to a battery cell, even if the battery cell is in a highly expanded state, the electrolyte adsorbed in the swellable polymer may be squeezed out. The squeezed-out electrolyte can be stored in a first recessed area on the surface of the separator membrane, i.e., this first recessed area forms a liquid storage space. Due to the compression resistance of the separator membrane, the liquid storage space will basically not deform, thereby reducing the risk of the electrolyte being squeezed out of the electrode assembly and improving the reliability and cycle performance of the battery cell. The technical solution of the present application is now described in detail.

[0092] Isolation film

[0093] In a first aspect, the present application provides an isolation membrane.

[0094] As shown in Figures 1 to 3, the isolation membrane 7 includes two surfaces opposite to each other along its own thickness direction, at least one of the surface of the isolation membrane 7 and the interior of the isolation membrane includes a pore structure, and the isolation membrane 7 also includes a swelling polymer; the isolation membrane 7 satisfies: when a pressure of 1.25 MPa is applied along the thickness direction of the isolation membrane 7, the compression rate ΔV of the isolation membrane 7 is ≤25%.

[0095] In some embodiments, the interior of the isolation membrane 7 includes a pore structure. As some examples, the pore structure can be understood as the isolation membrane 7 being a porous structure, the swollen polymer being located inside the isolation membrane 7, and adsorbing and storing the electrolyte inside the isolation membrane 7, and being able to release the swollen polymer to the pore structure of the isolation membrane 7. As other examples, the swollen polymer can be prepared as an isolation membrane having a pore structure, which is conducive to adsorbing the electrolyte and storing the electrolyte inside the isolation membrane 7. In the above structure, the pore structure can be a three-dimensional cross-linked pore structure; or, the pore structure can be a blind hole, through hole, or other structure opened in the isolation membrane. The isolation membrane can be prepared as an isolation membrane with pores (for example, a bubble pore isolation membrane) by a phase inversion method or an extraction method, and the isolation membrane can also be pore-forming by fiber spinning (for example, biaxial stretching).

[0096] In some embodiments, at least one surface of the isolation membrane 7 includes a pore structure. The pore structure can be understood as a blind hole structure, that is, it does not penetrate the isolation membrane 7. Optionally, the pore structure includes a first recessed area 71 (blind hole structure).

[0097] The separator 7 comprises a swellable polymer, which exhibits good lyophilicity and a strong affinity for the electrolyte. The swellable polymer can physically adsorb the electrolyte between its molecular chains. As the battery cell expands, some of the electrolyte may be squeezed out, flowing into the pore structure. This pore structure, acting as a liquid reservoir, effectively reduces the amount of electrolyte flowing out of the electrode assembly and ensures good and uniform wetting of the electrode assembly, improving the reliability and cycling performance of the battery cell.

[0098] The pore structure inside the separator 7 can adsorb the electrolyte inside the separator 7 , and even if the electrolyte separates from the swollen polymer, it will flow into the pore structure inside the separator 7 and will basically not flow out of the separator 7 .

[0099] The first recessed area 71 refers to the space formed by a portion of the surface of the isolation membrane 7 being recessed toward the interior of the isolation membrane 7. The first recessed area 71 serves as a storage space for the electrolyte. When the volume of the battery cell expands, components in the electrode assembly, such as the isolation membrane 7, are subjected to a certain extrusion force, and the electrolyte locked in the polymer may be squeezed out. The electrolyte is fluid. Since the isolation membrane 7 has good lyophilicity, it will guide the electrolyte to flow into the storage space, thereby reducing the risk of the electrolyte flowing out of the electrode assembly and achieving good and uniform infiltration of the electrode assembly.

[0100] When the isolation membrane 7 of the embodiment of the present application meets the above conditions, the isolation membrane 7 has excellent compression resistance, and the pore structure basically does not undergo compression deformation, making it difficult for the electrolyte to separate from the swollen polymer. Even if the electrolyte flows out of the swollen polymer, it can be stored in the pore structure, thereby reducing the risk of the electrolyte being squeezed out of the electrode assembly and improving the reliability and cycle performance of the battery cell.

[0101] The compressibility of the separator 7 is well known in the art and can be tested using equipment and methods known in the art, such as testing in accordance with the national standard GB / T 1041-2008 for testing the compression properties of plastics. Specifically, the separator 7 may be derived from the separator 7 itself or from a battery cell. If the separator 7 is derived from the separator 7 itself, the compression properties can be tested directly without drying. If the separator 7 is derived from a battery cell, the separator 7 must be dried before the compression properties are tested. The drying process is as follows: disassemble the battery cell, remove the separator 7, and dry it in a 60°C oven for 2 hours. The compression properties test is as follows: lay the separator 7 flat on a flat aluminum foil surface and cover it with a layer of aluminum foil to ensure the flatness of the separator 7. Cut 50 sets of separator 7 samples of a fixed area (e.g., 5 cm x 5 cm). Cover the upper and lower surfaces of each separator 7 sample with aluminum foil. Stack the 50 sets of samples together for subsequent compression testing. Cut 100 pieces of aluminum foil of the same size and stack them together to serve as a blank. Tests were performed using a universal tensile machine in compression mode at a speed of 0.5 mm / min. The stress-strain curves were recorded to determine the compression ratio of the separator 7 samples.

[0102] In some embodiments, the compression rate ΔV of the isolation membrane 7 can be 25%, 24%, 23%, 22%, 21%, 20%, 19%, 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 02%, 0.1% or a range consisting of any two of the above values.

[0103] In some embodiments, the isolation film 7 further satisfies:

[0104] Take an isolation film 7 with an area of ​​5 cm × 10 cm and record its mass ms1;

[0105] Immerse the separator 7 in excess electrolyte (mass ratio of separator to electrolyte ≥ 1:100) at 25°C for 7 days, then take out the separator 7 and set it vertically until there is no droplet for 5 minutes, and record its mass ms2.

[0106] Then, ((ms2-ms1) / ms1)×100%≥10%.

[0107] The unit of ms1 is g, and the unit of ms2 is g.

[0108] In the embodiment of the present application, ((ms2-ms1) / ms1)×100% can be understood as the liquid absorption rate of the isolation membrane 7, which can characterize the ability of the isolation membrane 7 to absorb electrolyte. As the liquid absorption rate increases, the ability of the isolation membrane 7 to absorb electrolyte becomes stronger; as the liquid absorption rate decreases, the ability of the isolation membrane 7 to absorb electrolyte becomes weaker. When the embodiment of the present application meets the above range, the liquid absorption capacity of the isolation membrane 7 is relatively strong, which is conducive to adsorbing the electrolyte into the swollen polymer molecular chain, thereby improving the cycle performance of the battery cell. The electrolyte in which the isolation membrane 7 is immersed uses a standard electrolyte, or uses the composition of the electrolyte of Example 1.

[0109] Exemplarily, the liquid absorption rate of the isolation film 7 can be 10%, 12%, 15%, 16%, 18%, 20%, 22%, 23%, 24%, 25%, 26%, 28%, 30%, 32%, 34%, 35%, 36%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 56%, 58%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 92%, 95%, 96%, 97%, 98% or a range consisting of any two of the above values.

[0110] In some embodiments, the swelling ratio of the swellable polymer is ≥ 100%.

[0111] When the swelling ratio of the swelling polymer is within the above range, the electrolyte is more easily diffused between the polymer molecular chains of the isolation membrane 7, thereby making the isolation membrane 7 have better liquid absorption capacity. For example, the swelling ratio of the swelling polymer 7 can be 100%, 105%, 108%, 110%, 112%, 115%, 118%, 120%, 125%, 130%, 135%, 140%, 145%, 150%, 155%, 160%, 165%, 170%, 175%, 180%, 185%, 190%, 195%, 200%, 210%, 220%, 250%, 280%. , 300%, 320%, 350%, 380%, 400%, 420%, 450%, 480%, 490%, 500%, 520%, 550%, 580%, 600%, 620%, 650%, 680%, 700%, 720%, 750%, 800%, 820%, 850%, 900%, 920%, 950%, 980%, 1000% or a range consisting of any two of the above values.

[0112] The swelling rate is well known in the art and can be measured using commonly used equipment and methods in the art, for example,

[0113] When the isolation membrane is mainly made of a swellable polymer (the swellable polymer is the main material of the substrate), the isolation membrane can be used as a test sample.

[0114] When the separator includes a coating containing a swellable polymer, the separator can be immersed in N-methylpyrrolidone (NMP) (mass ratio of separator to NMP: 1:20) and stirred at 2000 rpm for 2 hours to fully dissolve or peel off the swellable polymer on the separator surface, thereby obtaining an NMP solution of the swellable polymer. This solution can then be prepared into a film, which serves as the test sample. For example, after stirring at 1200 rpm for 2 hours and then drying at 130°C for ≥8 hours, a polymer film with a width of 10 mm, a length of 10 mm, and a thickness of 1 mm can be obtained.

[0115] Take a test sample with a width of 10 mm and a length of 10 mm as the specimen and record its mass as the initial mass;

[0116] The sample was added to an excess of dimethyl carbonate (DMC) (the mass ratio of the sample to DMC was 1:100), and after standing at 25°C for 7 days, the swollen sample was obtained, and its mass was recorded as the swollen mass.

[0117] The swelling ratio of a swollen polymer is (swollen mass - initial mass) multiplied by 100 percent.

[0118] In some embodiments, a pressure of 1.25 MPa is applied along the thickness direction of the isolation membrane 7 , and the compression modulus of the isolation membrane 7 is ≥45 MPa.

[0119] When the separator 7 of the embodiment of the present application meets the above conditions, the separator 7 has excellent compression resistance, and the pore structure, such as the first recessed area 71, is substantially free of compression deformation, thereby reducing the risk of electrolyte being squeezed out of the electrode assembly and improving the reliability and cycle performance of the battery cell. For example, the compression modulus of the separator 7 can be 45 MPa, 46 MPa, 48 MPa, 50 MPa, 52 MPa, 55 MPa, 58 MPa, 60 MPa, 62 MPa, 65 MPa, 68 MPa, 70 MPa, 72 MPa, 75 MPa, 80 MPa, 85 MPa, 90 MPa, 95 MPa, 100 MPa, 110 MPa, 120 MPa, 130 MPa, 150 MPa, or a range consisting of any two of the above values.

[0120] The compression modulus of the isolation film 7 is well known in the art and can be tested using known equipment and methods, such as those described in the national standard GB / T 1041-2008 for testing the compression properties of plastics. For example, the isolation film 7 can be cut into a fixed area (e.g., 5 cm x 5 cm) and a set of 500 layers (approximately 5 mm thick) can be used for compression testing.

[0121] The separator 7 of the embodiment of the present application includes two surfaces, one of which is located near the positive electrode tab of the battery cell, and the other is located near the negative electrode tab of the battery cell. One of the two surfaces may include a first recessed area 71, or both surfaces may include a first recessed area 71. Exemplarily, the surface near the negative electrode tab of the two surfaces includes a first recessed area 71. The surface near the positive electrode tab of the two surfaces includes a first recessed area 71. Optionally, both surfaces of the separator 7 include at least one first recessed area 71.

[0122] In some embodiments, the projection profile of the first recessed area 71 along the thickness direction of the isolation film 7 may be polygonal, circular, elliptical, sector-shaped, semi-elliptical, irregular, etc.

[0123] Exemplarily, the polygon can be a regular polygon or an irregular polygon; for example, the polygon can be a triangle, a trapezoid, a quadrilateral, a pentagon or a hexagon. Specifically, the polygon is a quadrilateral, and the first recessed area 71 can be a long strip extending along the length direction or width direction of the isolation membrane 7, etc.

[0124] Exemplarily, the sector may be a portion of a circle, such as a semicircle, 1 / 3 of a circle, and so on.

[0125] The number of the first recessed area 71 may be one or more.

[0126] When there are multiple first recessed areas 71, the projection contour shapes of the first recessed areas 71 may be the same or different. For example, the projection contour shape of one of the first recessed areas 71 may be circular, and the projection contour shape of another first recessed area 71 may be a strip, etc.

[0127] When the projection contour shape of the first recessed area 71 can be a long strip, the extension direction of the first recessed area 71 is parallel or approximately parallel to the width direction of the isolation membrane 7, or the extension direction of the first recessed area 71 is parallel or approximately parallel to the length direction of the isolation membrane 7.

[0128] In some embodiments, the angle between the extension direction of the first recessed area 71 and the length direction of the isolation membrane 7 is -45° to 45°. For example, the angle between the extension direction of the first recessed area 71 and the length direction of the isolation membrane 7 can be -45°, -30°, -25°, -20°, -15°, -10°, -5°, -2°, -1°, 0°, 1°, 2°, 5°, 10°, 15°, 20°, 25°, 30°, 45°, or a range consisting of any two of the above values. It can be optionally -20° to 20°, -15° to 15°, -10° to 10°, or -5° to 5°. In the embodiment of the present application, when the angle between the extension direction of the first recessed area 71 and the length direction of the isolation membrane 7 is 0°, it means that the extension direction of the first recessed area 71 is parallel to the length direction of the isolation membrane 7.

[0129] In some embodiments, the angle between the extension direction of the first recessed area 71 and the width direction of the isolation membrane 7 is -45° to 45°. For example, the angle between the extension direction of the first recessed area 71 and the width direction of the isolation membrane 7 can be -45°, -30°, -25°, -20°, -15°, -10°, -5°, -2°, -1°, 0°, 1°, 2°, 5°, 10°, 15°, 20°, 25°, 30°, 45°, or a range consisting of any two of the above values. It can be optionally -20° to 20°, -15° to 15°, -10° to 10°, or -5° to 5°. In the embodiment of the present application, when the angle between the extension direction of the first recessed area 71 and the width direction of the isolation membrane 7 is 0°, it means that the extension direction of the first recessed area 71 is parallel to the width direction of the isolation membrane 7.

[0130] In the case that there is only one first recessed region 71 , the extending direction of the first recessed region 71 may be unique, for example, the first recessed region 71 extends along the length direction of the isolation film 7 .

[0131] In the case of multiple first recessed regions 71, the extension direction of each first recessed region 71 may be unique, for example, extending along the length direction of the isolation membrane 7, with the multiple first recessed regions 71 arranged in parallel. The extension direction of the first recessed regions 71 may also include multiple directions, for example, the extension direction of one first recessed region 71 is parallel to the length direction of the isolation membrane 7, while the extension direction of another first recessed region 71 forms an angle of 5° with the length direction of the isolation membrane 7. In this arrangement, the extension directions of the two first recessed regions 71 may intersect.

[0132] In the case where there are multiple first recessed areas 71, the first recessed areas 71 can be arranged at intervals or continuously. When the first recessed areas 71 are arranged at intervals, they can be arranged in an array or in a non-uniform manner. The multiple first recessed areas 71 are arranged at intervals. On the one hand, it can increase the overall occupied volume of the multiple first recessed areas 71, increase the mechanical strength of the isolation membrane 7, and improve the structural stability of the isolation membrane 7. When the volume of the battery cell expands, the isolation membrane 7 is not easily deformed, so that the first recessed area 71 (liquid storage space) is relatively stable and not easily deformed. The continuous arrangement of the first recessed areas 71 can be understood as the continuous arrangement of the projections of two adjacent first recessed areas 71 along the thickness direction of the isolation membrane 7. This structure is conducive to increasing the overall occupied volume of the multiple first recessed areas 71 and increasing the occupied volume of the liquid storage space.

[0133] In some embodiments, the separator 7 includes a first porous base membrane including a swellable polymer.

[0134] The swellable polymer can be used as the main material of the first porous substrate and prepared into a first porous base membrane with pores (such as bubble pores) by phase inversion or extraction. The pores can also be formed by fiber spinning (such as biaxial stretching).

[0135] The main material of the first porous substrate may also include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The main material of the first porous substrate and the swelling polymer are blended to prepare the first porous base membrane.

[0136] The first porous base film may have a pore structure inside. FIG1 shows such a structure of a separator, which may not include a coating layer.

[0137] Optionally, the first porous base film includes two surfaces facing each other along the thickness direction of the separator 7, and at least one of the two surfaces includes at least one first recessed area 71. Figures 2 and 3 show this structure of the separator.

[0138] Further optionally, both surfaces of the first porous base membrane include at least one first recessed area 71 .

[0139] This type of isolation membrane 7 can be understood as the first porous base membrane no longer having an additional coating 712 on its surface. Since the first porous base membrane is added with a swelling polymer, the first porous base membrane has the ability to absorb liquid, attracting and locking the electrolyte into the first porous base membrane, thereby reducing the amount of free electrolyte and improving the reliability of the battery cell.

[0140] The first porous substrate in the embodiment of the present application can be a single-layer film or a multi-layer composite film. When the first porous substrate is a multi-layer composite film, the materials of each layer can be the same or different.

[0141] As shown in FIG. 4 to FIG. 6 , in other embodiments, the separator 7 includes a second porous base membrane 711 and a coating layer 712 disposed on at least one side of the second porous base membrane 711 , wherein the coating layer 712 includes a swelling polymer.

[0142] The coating layer 712 may be provided as a continuous whole film layer, in which case the surface of the coating layer 712 facing away from the second porous base film 711 includes at least one first recessed region 71. Figure 4 shows a schematic diagram of the coating layer 712 being a whole film layer.

[0143] The coating 712 can be set continuously. In this case, the coating 712 may not be a whole film layer. The local area is too thin or even has no coating 712, so that part of the surface of the second porous base membrane 711 is exposed. The cavity corresponding to the exposed surface is the first recessed area 71, that is, the first recessed area 71 is formed between the coating 712 and the second porous base membrane 711.

[0144] The coating 712 can also be provided discontinuously. In this case, the coating 712 is not a whole film layer, and part of the surface of the second porous base membrane 711 is exposed. The cavity corresponding to the exposed surface is the first recessed area 71, that is, the coating 712 and the second porous base membrane 711 enclose the first recessed area 71. For example, the coating 712 includes a plurality of protrusions, and the second porous base membrane 711 and the plurality of protrusions enclose the first recessed area 71. Figure 5 shows that the coating 712 is a strip-like structure provided at intervals. Figure 6 shows that the coating 712 can be distributed in a dotted manner, and the dotted distribution can be an array distribution, or a non-uniform distribution.

[0145] The coating 712 can be provided on one side of the second porous base membrane 711 or on both sides of the second porous base membrane 711. The coating 712 can be provided directly on the surface of the second porous base membrane 711 or indirectly on the surface of the second porous base membrane 711. When the coating 712 is provided indirectly on the surface of the second porous base membrane 711, other functional layers such as a heat-resistant coating 712 can be provided between the coating 712 and the second porous base membrane 711. In this type of separator 7, the surface of the second porous base membrane 711 is provided with the coating 712. Since the coating 712 contains a swelling polymer, it has liquid absorption capacity, attracting and locking the electrolyte into the coating 712, thereby reducing the amount of free electrolyte and improving the reliability of the battery cell.

[0146] In the embodiment of the present application, the main material of the second porous base film 711 is not particularly limited. Any known substrate with good chemical and mechanical stability can be selected, such as at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The first porous base film can be a single-layer film or a multi-layer composite film. When the first porous base film is a multi-layer composite film, the materials of each layer can be the same or different.

[0147] In some embodiments, the second porous base membrane 711 may further include a swelling polymer. In this case, the material and structure of the second porous base membrane 711 are as described in the first porous base membrane section and are not repeated here.

[0148] In some embodiments, the swelling polymer includes at least one of a first fluorinated polymer, a first ester polymer, and a first ether polymer.

[0149] The polymer has excellent swelling properties and compression modulus, which is conducive to the adsorption of electrolyte. In addition, it is not easily compressed during the charge and discharge process of the battery cell, thereby reducing the amount of electrolyte flowing out of the electrode assembly.

[0150] [First Fluorinated Polymer]

[0151] In some embodiments, the first fluorinated polymer comprises at least one of the structural units represented by formula (AI) to the structural units represented by formula (AIII),

[0152] In formula (AI) and formula (AII), R 11 、R 12 、R 13 and R 14 Each independently includes a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted alkoxy group, and R 11 、R 12 、R 13 and R 14 At least one of them contains a fluorine atom.

[0153] Optionally, R 11 、R 12 、R 13 and R 14 Each independently includes a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted C1-C10 alkyl group, or a substituted or unsubstituted C1-C10 alkoxy group.

[0154] Alternatively, when substituted, the substituent may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, a halogen atom.

[0155] In formula (aIII), R 15 Includes single bonds, substituted or unsubstituted alkyl groups; when substituted, substituents include fluorine atoms.

[0156] In some embodiments, p is a positive integer selected from 1 to 3.

[0157] In some embodiments, R 11 、R 12 、R 13 and R 14 Each independently includes a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted alkoxy group.

[0158] Optionally, R 11 、R 12 、R 13 and R 14 Each independently includes a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted C1-C10 alkyl group, or a substituted or unsubstituted C1-C10 alkoxy group.

[0159] Further optionally, R 11 、R 12 、R 13 and R 14 Each independently includes a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, a fluoromethyl group, a methoxy group or a perfluoromethoxy group.

[0160] In some embodiments, when substituted, the substituent may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0161] In some embodiments, the first fluorinated polymer includes at least one of the structural units represented by formula (AI-1) to the structural units represented by formula (AI-11),

[0162] In some embodiments, the first fluorinated polymer includes at least one of the structural units represented by formula (AII-1) to the structural units represented by formula (AII-5),

[0163] In some embodiments, the first fluorinated polymer includes at least one of the structural units represented by formula (AIII-1) to the structural units represented by formula (AIII-3),

[0164] Illustratively, the fluorinated polymer includes one or more of polyperfluoroethylene (PTFE), polyvinylidene fluoride (PVDF), perfluoroethylene propylene copolymer (FEP), perfluoroalkoxy polymer (PFA), perfluoropolyether (PFPE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyvinylidene fluoride-trifluoroethylene copolymer (PVDF-TrFE) and perfluoro (1-butenyl vinyl ether) polymer (CYTOP for short).

[0165] Optionally, the fluorinated polymer includes one or more of polyperfluoroethylene (PTFE), polyvinylidene fluoride (PVDF), perfluoroethylene propylene copolymer (FEP), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polyvinylidene fluoride-trifluoroethylene copolymer (PVDF-TrFE).

[0166] The fluoropolymer may be derived from one or more of the following monomers: fluorocycloethane, vinyl fluoride, 1,2-difluoroethylene, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, hexafluoropropylene, 3,3,3-trifluoropropylene, trifluoropropylene, tetrafluoropropylene, and pentafluoropropylene. Alternatively, the fluoropolymer may be derived from at least two of the following monomers: fluorocycloethane, vinyl fluoride, 1,2-difluoroethylene, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, hexafluoropropylene, 3,3,3-trifluoropropylene, trifluoropropylene, tetrafluoropropylene, and pentafluoropropylene.

[0167] In the embodiments of the present application, the polymer may also be obtained by copolymerizing the above-mentioned structural groups with a small amount of other types of structural groups (e.g., olefin structural units, ester monomers, nitrile monomers such as acrylonitrile, amide monomers such as acrylamide, acrylic acid, etc.). Such small amounts of monomers have relatively poor lyophilic properties, and copolymerizing the above-mentioned fluorinated polymer monomers with such monomers can improve the swelling ratio and compression modulus of the swollen polymer.

[0168] In some embodiments, the molecular weight of the swelling polymer is 2×10 5 g / mol to 1.2×10 6 g / mol.

[0169] The present application can adjust at least one of the swelling ratio and compression modulus of the swelling polymer by adjusting the molecular weight.

[0170] For example, the molecular weight of the polymer may be 2×10 5 g / mol, 5×10 5 g / mol, 8×10 5 g / mol, 1×10 6g / mol, 1.2×10 6 g / mol or a range consisting of any two of the above values.

[0171] [First ether polymer]

[0172] In some embodiments, the first ether polymer comprises a structural unit represented by formula (BI),

[0173] In formula (BI), R 21 and R 22 Each independently includes a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted alkoxy group; R 23 This includes single bonds, and substituted or unsubstituted methylene groups.

[0174] Optionally, R 21 and R 22 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, or a substituted or unsubstituted C1-C10 alkoxy group.

[0175] Optionally, R 23 It includes single bonds, substituted or unsubstituted C1-C10 methylene groups.

[0176] In some embodiments, when substituted, the substituent may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0177] Illustratively, the first ether polymer includes at least one of the structural units represented by formula (BI-1) to the structural units represented by formula (BI-8),

[0178] In some embodiments, the first ether polymer comprises a structural unit represented by formula (BII),

[0179] In formula (BII), R 24 to R 27 Each independently includes a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkoxy group or an ether group, and R 24 to R 27 At least one of them contains a substituted or unsubstituted alkoxy group or an ether group.

[0180] Optionally, R 24 to R 27 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C1-C10 alkoxy group or an ether group.

[0181] In some embodiments, the first ether polymer includes at least one of the structural units represented by formula (BII-1) to the structural units represented by formula (BII-7),

[0182] The above-mentioned polymers are only examples of the structural groups of the main molecular chain. In the embodiments of the present application, the polymers can also be obtained by copolymerizing the above-mentioned structural groups with a small amount of other types of structural groups (such as olefin structural units, ester monomers, nitrile monomers such as acrylonitrile, amide monomers such as acrylamide, acrylic acid and other structural units, etc.).

[0183] When the above groups are substituted, the substituents may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0184] In some embodiments, the molecular weight of the swelling polymer is 2×10 5 g / mol to 1.2×10 6 g / mol.

[0185] The present application can adjust at least one of the swelling ratio and compression modulus of the swelling polymer by adjusting the molecular weight.

[0186] For example, the molecular weight of the polymer may be 2×10 5 g / mol, 5×10 5 g / mol, 8×10 5 g / mol, 1×10 6 g / mol, 1.2×10 6 g / mol or a range consisting of any two of the above values.

[0187] [First ester polymer]

[0188] In some embodiments, the first ester polymer comprises a structural unit represented by formula (CI),

[0189] In formula (CI), R 31 、R 32 and R 33 Each independently includes a hydrogen atom, or a substituted or unsubstituted alkyl group; R 34 It includes a substituted or unsubstituted alkyl group, or a substituted or unsubstituted hydroxyalkyl group.

[0190] Optionally, R 31 、R 32 and R 33 Each independently includes a hydrogen atom, or a substituted or unsubstituted C1-C10 alkyl group.

[0191] In some embodiments, R 34 It includes substituted or unsubstituted C1-C10 alkyl groups, or substituted or unsubstituted C1-C10 hydroxyalkyl groups.

[0192] In some embodiments, R 31 This includes a hydrogen atom, or a substituted or unsubstituted methyl group.

[0193] In some embodiments, R 32 and R 33 Each independently includes a hydrogen atom.

[0194] In some embodiments, when substituted, the substituent may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0195] Illustratively, the first ester polymer includes at least one of the structural units represented by formula (CI-1) to the structural units represented by formula (CI-15),

[0196] In some embodiments, the ester polymer comprises a structural unit represented by formula (CII),

[0197] In formula (CII), R 35 This includes substituted or unsubstituted methylene groups.

[0198] Optionally, R 35 This includes substituted or unsubstituted C1-C10 methylene groups.

[0199] Illustratively, the first ester polymer includes at least one of the structural units represented by formula (CII-1) to the structural units represented by formula (CII-5),

[0200] In some embodiments, the first ester polymer comprises a compound represented by formula (CIII),

[0201] In formula (CIII), R 36 、R 37 and R 38 Each independently includes a hydrogen atom, or a substituted or unsubstituted C1-C8 alkyl group; R 39 Including substituted or unsubstituted C1-C8 alkyl;

[0202] Optionally, R 36 、R 37 and R 38 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C4 alkyl group.

[0203] Illustratively, the ester polymer includes at least one of the compounds represented by formula (CIII-1) to the compounds represented by formula (CIII-5),

[0204] The above-mentioned polymers are only examples of the structural groups of the main molecular chain. In the embodiments of the present application, the polymers can also be obtained by copolymerizing the above-mentioned structural groups with a small amount of other types of structural groups (such as olefin structural units, ester monomers, nitrile monomers such as acrylonitrile, amide monomers such as acrylamide, acrylic acid and other structural units, etc.).

[0205] When the above groups are substituted, the substituents may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0206] In some embodiments, the molecular weight of the swelling polymer is 2×10 5 g / mol to 1.2×10 6 g / mol.

[0207] The present application can adjust at least one of the swelling ratio and compression modulus of the swelling polymer by adjusting the molecular weight.

[0208] For example, the molecular weight of the polymer may be 2×10 5 g / mol, 5×10 5 g / mol, 8×10 5 g / mol, 1×10 6 g / mol, 1.2×10 6 g / mol or a range consisting of any two of the above values.

[0209] In some embodiments, the coating layer 712 may further include a heat-resistant filler, thereby improving the overall heat resistance of the isolation film 7 .

[0210] In some embodiments, the separator 7 may further include a heat-resistant coating 712 , which is located between the second porous base membrane 711 and the coating 712 , and includes a heat-resistant filler.

[0211] In some embodiments, the decomposition temperature of the filler may be above 200° C., so that the filler has good thermal stability and is not easily decomposed, thereby further improving the heat resistance of the isolation membrane 7 .

[0212] The inorganic particles have the characteristics of high thermal stability and non-decomposability. Optionally, the inorganic particles include at least one of inorganic particles with a dielectric constant of 5 or greater, inorganic particles with ion conductivity but not storing ions, and inorganic particles capable of undergoing electrochemical reactions.

[0213] Optionally, the inorganic particles having a dielectric constant of 5 or more include boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, magnesium aluminum silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate, barium titanate, Pb(Zr,Ti)O3 (abbreviated as PZT), Pb 1-m La m Zr 1-n Ti n O3 (abbreviated as PLZT, 0<m<1, 0<n<1), Pb(Mg3Nb 2 / 3 )O3-PbTiO3 (abbreviated as PMN-PT), and at least one of their respective modified inorganic particles. Optionally, the modification method of each inorganic particle may be chemical modification and / or physical modification. The chemical modification method includes coupling agent modification (for example, using silane coupling agent, titanate coupling agent, etc.), surfactant modification, polymer grafting modification, etc. The physical modification method may be mechanical force dispersion, ultrasonic dispersion, high energy treatment, etc. The modification treatment can reduce the agglomeration of inorganic particles, thereby enabling them to form a more stable and uniform spatial network structure with nanocellulose; in addition, by selecting coupling agents, surfactants or polymer-modified inorganic particles with specific functional groups, it is also helpful to improve the wetting properties of the coating 712 to the electrolyte and improve the bonding strength between the coating 712 and the substrate.

[0214] Optionally, the inorganic particles having ion conductivity but not storing ions include Li3PO4, lithium titanium phosphate Li x1 Ti y1 (PO4)3, lithium aluminum titanium phosphate Li x2 Al y2 Ti z1 (PO4)3, (LiAlTiP) x3 O y3 Type glass, lanthanum lithium titanate Li x4 La y4 TiO3, lithium germanium thiophosphate Li x5 Ge y5 P z2 S w , lithium nitride Li x6 N y6、SiS2 type glass Li x7 Si y7 S z3 and P2S5 glass Li x8 P y8 S z4 At least one of the following: 0<x1<2, 0<y1<3, 0<x2<2, 0<y2<1, 0<z1<3, 0<x3<4, 0<y3<13, 0<x4<2, 0<y4<3, 0<x5<4, 0<y5<1, 0<z2<1, 0<w<5, 0<x6<4, 0<y6<2, 0<x7<3, 0<y7<2, 0<z3<4, 0<x8<3, 0<y8<3, 0<z4<7. This can further improve the ion transport characteristics of the separator 7.

[0215] The organic particles have good thermal stability and are not easy to decompose, thereby improving the heat resistance of the isolation membrane 7; at the same time, when the internal temperature of the battery cell reaches the melting point of the organic particles due to overcharge abuse, heat abuse, etc., the organic particles can also melt and be absorbed into the micropores of the substrate due to capillary action to play the role of closing the pores and breaking the circuit, which is beneficial to ensure that the battery cell has high safety performance.

[0216] In some embodiments, the organic particles include but are not limited to at least one of polyethylene particles, polypropylene particles, polystyrene particles, melamine resin particles, phenolic resin particles, polyester particles (e.g., polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate), polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles, polyaryletherketone particles, and copolymers of butyl acrylate and ethyl methacrylate (e.g., cross-linked polymers of butyl acrylate and ethyl methacrylate).

[0217] battery cells

[0218] In a first aspect, the present application provides a battery cell, which includes an electrode assembly and an electrolyte, wherein the electrode assembly includes a separator according to any embodiment of the first aspect of the present application.

[0219] In some embodiments, the battery cell satisfies: V0 / (m / ρ)≥1;

[0220] V0 represents the value of the pore volume and interlayer gap volume in the electrode assembly, and its unit is mL;

[0221] m represents the difference between the mass of the battery cell before drying and the mass after drying, and its unit is g;

[0222] ρ represents the density of the electrolyte, and its unit is g / mL.

[0223] When the battery cell satisfies the above formula, there can be sufficient space in the electrode assembly 52 to provide storage space for the electrolyte, thereby reducing the risk of the electrolyte flowing out of the electrode assembly 52 and improving the cycle performance of the battery cell.

[0224] As shown in Figures 7 and 8 , the electrode assembly 52 includes a first electrode piece 8, a second electrode piece 9, and a separator 7. The first electrode piece 8 and the second electrode piece 9 have opposite polarities, and the separator 7 is disposed between the first and second electrode pieces 8, 9. The first electrode piece 8, the second electrode piece 9, and the separator 7 each have a porous structure. The pore volume of the electrode assembly 52 is the sum of the pore volume of the first electrode piece 8, the pore volume of the second electrode piece 9, and the pore volume of the separator 7. The interlayer gap volume of the electrode assembly 52 is the sum of the gap volume between the first electrode piece 8 and the separator 7, and the gap volume between the second electrode piece 9 and the separator 7. Generally speaking, the interlayer gap volume of the electrode assembly 52 is relatively small. However, in the present embodiment, given the compressibility of the separator 7, during the charge and discharge process of the battery cell, the separator 7 undergoes a certain degree of deformation, which increases the gap volume between the separator 7 and the electrode pieces.

[0225] V0 can be considered to be equal to the sum of the pore volume V1 of the first pole piece 8, the pore volume V2 of the second pole piece 9, the pore volume of the isolation membrane and the interlayer gap volume V3, that is, V0=V1=V2+V3.

[0226] V3=S×(D0-d1-d2)×(1-ΔV);

[0227] Wherein, S represents the facing area of ​​the first pole piece 8 and the second pole piece 9;

[0228] D0 represents the total thickness of the electrode assembly 52;

[0229] d1 represents the thickness of the first pole piece 8;

[0230] d2 represents the thickness of the second pole piece 9;

[0231] ΔV represents the compression rate of the separator.

[0232] As shown in FIG9 , when the surface of the first electrode piece 8 includes a second recessed area 81 (groove), the gap volume of the electrode assembly 52 needs to be further added with the total volume of the second recessed area 81. Specifically, V3 also includes the total volume of the second recessed area 81.

[0233] Furthermore, when the surface of the second electrode piece 9 includes a second recessed area 81 (groove), the gap volume of the electrode assembly 52 needs to be further added with the total volume of the second recessed area 81. Specifically, V3 also includes the total volume of the second recessed area 81.

[0234] The first electrode piece 8 may be a positive electrode piece, and correspondingly, the second electrode piece 9 may be a negative electrode piece; or the first electrode piece 8 may be a negative electrode piece, and correspondingly, the second electrode piece 9 may be a positive electrode piece.

[0235] m can be understood as the total amount of electrolyte in the battery cell. After the electrolyte is injected into the battery cell, the electrolyte mainly exists in the following forms: one is adsorbed in the pore structure of the electrode and / or the separator 7, and the other is diffused into the swollen polymer. The total amount of electrolyte can be measured by the following method: take a fresh battery cell and fully discharge it to 0% SOC state of charge, and weigh the battery cell. The weighed mass is the mass of the battery cell before drying; open a hole with a diameter of The battery cell is placed on top of a container with the hole facing downward and directly above the container, so that the free electrolyte inside the battery cell can drip into the container below. The battery cell is left to stand for 3 to 5 hours so that all the free electrolyte inside can drip into the container. Of course, there may be no free electrolyte. The battery cell is then dried at 60°C to 95°C for 24 to 48 hours, and the battery cell is immersed in dimethyl carbonate (DMC) solvent for 12 hours. The battery cell is then dried at 60°C to 95°C for 24 to 48 hours. The dried battery cell is weighed, and the weighed mass is the mass of the dried battery cell. For example, the battery cell is dried at 60°C for 5 hours, and the dried battery cell is weighed. In the embodiment of the present application, the fresh battery cell can be a battery cell that has just left the factory (not subjected to charge and discharge cycles after formation), or a battery cell that is assembled on an electrical device and has been cycled for less than 10 cycles.

[0236] In the embodiment of the present application, when there is free electrolyte in the battery cell, the electrolyte density ρ can be measured by the following method: a predetermined mass of electrolyte can be poured out from multiple battery cells in the battery, for example 10, and the volume of the poured electrolyte can be measured. The ratio of the predetermined mass to the volume is the electrolyte density ρ. When there is no free electrolyte in the battery cell, the electrolyte density ρ is the density of the electrolyte injected into the battery cell.

[0237] When the battery cell meets the above range, the electrode assembly 52 can provide space for the electrolyte, which is conducive to the electrolyte being completely located in the electrode assembly 52, reducing the risk of the electrolyte being free outside the electrode assembly 52, and improving the reliability and cycle performance of the battery cell.

[0238] Optionally, V0 / (m / ρ)≥1; V0 / (m / ρ)≥1.2; V0 / (m / ρ)≥1.5; V0 / (m / ρ)≥1.8; V0 / (m / ρ)≥2.0; V0 / (m / ρ)≥2.2; V0 / (m / ρ)≥2.5; V0 / (m / ρ)≥2.8; or V0 / (m / ρ)≥3, etc.

[0239] In some embodiments, the first pole piece 8 includes two surfaces opposite to each other along its own thickness direction, which can also be understood as the surface of the first pole piece 8 facing the isolation membrane 7, and at least one of the two surfaces has at least one second recessed area 81, that is, one of the two surfaces has at least one second recessed area 81, or both surfaces have at least one second recessed area 81.

[0240] The second recessed area 81 refers to the space formed by the recess of part of the surface of the first pole piece 8 toward the interior of the first pole piece 8. The second recessed area 81 can also serve as a storage space for the electrolyte. When the volume of the battery cell expands, the components in the electrode assembly 52, such as the isolation membrane 7, are subjected to a certain extrusion force. The electrolyte locked in the polymer may be squeezed out, and the electrolyte flows to the second recessed area 81, thereby reducing the risk of the electrolyte flowing out of the electrode assembly 52 and achieving good and uniform infiltration of the electrode assembly 52.

[0241] For example, the first electrode piece 8 may be a positive electrode piece, i.e., the surface of the positive electrode piece has at least one second recessed area 81. Correspondingly, the second electrode piece 9 may be a negative electrode piece, and the surface of the negative electrode piece may have at least one second recessed area 81. Of course, the surface of the negative electrode piece may also be a flat surface, i.e., the surface of the negative electrode piece does not have the second recessed area 81.

[0242] For example, the first electrode piece 8 may be a negative electrode piece, i.e., the surface of the negative electrode piece has at least one second recessed area 81. Correspondingly, the second electrode piece 9 may be a positive electrode piece, and the surface of the positive electrode piece may be a flat surface, i.e., the surface of the negative electrode piece does not have the second recessed area 81.

[0243] The number of the second recessed area 81 may be one or more.

[0244] The specific configuration of the second recessed area 81 is as described in the first recessed area, and will not be repeated here.

[0245] In some embodiments, the projection of the first recessed region along the thickness direction of the electrode assembly 52 overlaps with the projection of the second recessed region 81 along the thickness direction of the electrode assembly 52. ​​In this case, it can also be understood that the first recessed region can be arranged opposite the second recessed region 81. After the electrolyte is released from the swollen polymer, it can flow into the liquid storage space formed by the first recessed region and the second recessed region 81, further reducing the risk of the electrolyte flowing out of the electrode assembly 52.

[0246] In other embodiments, the projection of the first recessed region along the thickness direction of the electrode assembly 52 does not overlap with the projection of the second recessed region 81 along the thickness direction of the electrode assembly 52. ​​In this case, it can also be understood that the first recessed region can be staggered with the second recessed region 81. The second recessed region 81 is arranged opposite the protruding surface of the separator 7 (the protruding surface corresponding to the first recessed region). The protruding surface has a large amount of swollen polymer with electrolyte locked in it. When the battery cell expands in volume, the electrolyte is released, and some of the electrolyte flows into the second recessed region 81 corresponding to the protruding surface, while the other part of the electrolyte flows along the separator 7 into the first recessed region, further reducing the risk of electrolyte flowing out of the electrode assembly 52.

[0247] In some further embodiments, there are multiple first recessed areas 71 and multiple second recessed areas 81. For example, the first recessed area 71 includes a recessed area a and a recessed area b, and the second recessed area 81 includes a recessed area c and a recessed area d. The recessed area a is arranged opposite to the recessed area c, and the recessed area b and the recessed area d are staggered.

[0248] In some embodiments, the electrolyte is located within the electrode assembly 52 .

[0249] The electrolyte has fluidity, which makes it easier to flow around the active material particles and improve the transmission rate of active ions. In the related art, the electrolyte usually has the following forms in the battery cell: one is to diffuse into the pore structure of the electrode assembly 52, such as in the pores of the electrode piece and / or the separator 7; the other is to be free in the battery cell. The electrolyte of the embodiment of the present application has the following forms: one is to diffuse into the pore structure of the electrode assembly 52, such as in the pores of the electrode piece and / or the separator 7; the second is to be located in the gap structure of the electrode assembly 52, such as the gap space between the first electrode piece 8 and the separator 7, and the gap space between the second electrode piece 9 and the separator 7; the third is to diffuse into the swelling polymer, so that the electrolyte of the embodiment of the present application is basically all located inside the electrode assembly 52, and there is basically no free electrolyte in the battery cell, which can significantly improve the reliability and cycle performance of the battery cell.

[0250] In some embodiments, the battery cell also satisfies 0≤y / V总孔 ≤15%;

[0251] y represents the volume of free electrolyte in the battery cell, in mL;

[0252] V 总孔 The value representing the pore volume of the electrode assembly 52 is in mL.

[0253] When calculating a formula, only the numerical value is substituted for the calculation, without substituting the unit for the calculation.

[0254] When the battery cell meets the above conditions, the content of free electrolyte in the battery cell is extremely small, or even the battery cell basically contains no free electrolyte, which can significantly improve the reliability and cycle performance of the battery cell.

[0255] For example, y / V 总孔 It can be 0%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, or a range consisting of any two of the above values. 总孔 A value of 0 indicates that the amount of free electrolyte is 0 mL, that is, there is basically no free electrolyte in the battery cell.

[0256] The electrode assembly 52 includes a first electrode piece 8, a second electrode piece 9 and a separator 7. The pore volume V of the electrode assembly 52 is 总孔 The pore volume includes the sum of the pore volume of the first pole piece 8, the pore volume of the second pole piece 9, and the pore volume of the separator 7. In the embodiments of the present application, the pore volume has a meaning well known in the art and can be detected using equipment and methods well known in the art. For example, it can be obtained by a gas displacement method. The pore volume is (vm), where v represents the apparent volume (i.e., the total volume) and m represents the true volume.

[0257] In some embodiments, the battery cell satisfies: (m / ρ) / V 总孔 ≥80%;

[0258] V 总孔 represents the pore volume of the electrode assembly 52, in mL;

[0259] m represents the difference between the mass of the battery cell before drying and the mass after drying, and its unit is g.

[0260] ρ represents the density of the electrolyte, and its unit is g / mL.

[0261] In the embodiments of the present application, m can be understood as the total amount of electrolyte in the battery cell, and the specific testing method is as described above.

[0262] When the battery cell meets the above conditions, most of the electrolyte is located in the pore structure of the electrode assembly 52, that is, the electrode assembly 52 itself has good liquid absorption and liquid retention capabilities, which is conducive to the transmission of active ions and improves the dynamic performance of the battery cell; a small part of the electrolyte can diffuse into the swelling polymer and release during the battery cell's cyclic charge and discharge process. Since the amount of released liquid is relatively small, the electrolyte is not easy to flow out of the electrode assembly 52, and the electrolyte can make the infiltration of the electrode assembly 52 more uniform, thereby improving the cycle performance of the battery cell.

[0263] For example, (m / ρ) / V 总孔 ≥80% 、 (m / ρ) / V 总孔 ≥82%, (m / ρ) / V 总孔 ≥85%, (m / ρ) / V 总孔 ≥86%, (m / ρ) / V 总孔 ≥88%, (m / ρ) / V 总孔 ≥90%, (m / ρ) / V 总孔 ≥92% or (m / ρ) / V 总孔 ≥95%.

[0264] In some embodiments, the battery cell further satisfies: 0≤y / Ah≤15%;

[0265] y represents the volume of free electrolyte in the battery cell, in mL;

[0266] Ah represents the value of the nominal capacity of the battery cell, and its unit is Ah.

[0267] When calculating a formula, only the numerical value is substituted into the formula without its unit.

[0268] The volume of free electrolyte y (mL) can be measured by the following method: take a fresh battery cell and discharge it to 0% SOC state of charge, and open a hole with a diameter of The battery cell is placed on top of a container with the hole facing downward and directly above the container, so that the free electrolyte inside the battery cell can drip into the container below. The battery cell is left to stand for 3 to 5 hours to allow all the free electrolyte inside to drip into the container. The volume of the electrolyte in the container is then measured to obtain y. In the embodiments of the present application, a fresh battery cell can be a battery cell that has just left the factory (has not been charged and discharged after formation) or a battery cell that has been assembled in an electrical device and has been cycled less than 10 times.

[0269] When the battery cell meets the above conditions, the content of free electrolyte in the battery cell is extremely small, or even the battery cell basically contains no free electrolyte, which can significantly improve the reliability and cycle performance of the battery cell.

[0270] For example, y / Ah can be 0%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, or a range consisting of any two of the foregoing values. A y / Ah of 0 indicates zero free electrolyte, i.e., substantially no free electrolyte is present in the battery cell.

[0271] In some embodiments, after the battery cell is subjected to a linear frequency sweep vibration test, it is charged to 100% state of charge (SOC). A hole is opened on the battery cell, and the hole is located at the lowest point in the vertical direction. The volume of electrolyte flowing out of the battery cell is recorded as M1, where 0 mL ≤ M1 ≤ 0.5 mL. Optionally, M1 is 0 mL.

[0272] in,

[0273] The vibration direction of the linear sweep vibration test is: single vibration up and down;

[0274] The vibration frequency of the linear sweep vibration test is: 10Hz~55Hz;

[0275] The maximum acceleration of the linear sweep vibration test is: 30m / s 2 ;

[0276] The number of sweep cycles of the linear sweep vibration test is: 10 times;

[0277] The vibration time of the linear sweep frequency vibration test is 3 hours.

[0278] In the related art, during use, the battery cell may vibrate under the action of external forces, and the electrolyte in the electrode assembly 52 may be separated from the electrode assembly 52 under the action of vibration, forming free electrolyte. The free electrolyte in the battery cell may leak, causing corrosion to the battery cell, leading to risks such as battery cell failure. However, the embodiment of the present application can effectively gather and throw out the electrolyte inside the battery cell by subjecting the battery cell to static and vibration treatment, thereby more accurately judging whether there is flowing electrolyte between the battery cell shell and the electrode assembly 52, and determining the content of free electrolyte. When the battery cell of the embodiment of the present application meets the above conditions, the content of free electrolyte in the battery cell is extremely small, or even basically contains no free electrolyte in the battery cell, which can significantly improve the reliability and cycle performance of the battery cell.

[0279] For example, M1 can be 0 mL, 0.05 mL, 0.1 mL, 0.15 mL, 0.2 mL, 0.25 mL, 0.3 mL, 0.35 mL, 0.4 mL, 0.45 mL, 0.5 mL, or a range consisting of any two of the foregoing values. M1 of 0 mL indicates that the amount of free electrolyte is zero, meaning that there is essentially no free electrolyte inside the battery cell after the linear frequency sweep vibration test.

[0280] In some embodiments, after the battery cell undergoes the above-mentioned linear sweep vibration test, the shell is removed, the electrode assembly is taken out and subjected to an extrusion test, and the volume of the electrolyte flowing out of the electrode assembly is recorded as M2 (the extrusion equipment is suspended, and a weighing balance and an electrolyte collection container are set at the bottom), 0 mL ≤ M2 ≤ 0.5 mL, optionally, M2 is 0 mL;

[0281] in,

[0282] The extrusion direction of the extrusion test is: perpendicular to the thickness direction of the electrode assembly 52;

[0283] The extrusion degree of the extrusion test is: the extrusion force is 0.35 MPa.

[0284] In the related art, during use, the battery cell may be subjected to external squeezing, and the electrolyte located in the electrode assembly 52 may be separated from the electrode assembly 52 under the squeezing action, forming free electrolyte. The free electrolyte in the battery cell may leak, causing corrosion to the battery cell, leading to risks such as battery cell failure. However, the embodiment of the present application can effectively squeeze out the electrolyte inside the battery cell by performing an squeezing test on the battery cell, thereby more accurately judging whether there is flowing electrolyte between the battery cell shell and the electrode assembly 52, and determining the content of free electrolyte. When the battery cell of the embodiment of the present application meets the above conditions, after squeezing, the content of free electrolyte in the battery cell is extremely small, or even the battery cell basically contains no free electrolyte, which can significantly improve the reliability and cycle performance of the battery cell.

[0285] For example, M2 can be 0 mL, 0.05 mL, 0.1 mL, 0.15 mL, 0.2 mL, 0.25 mL, 0.3 mL, 0.35 mL, 0.4 mL, 0.45 mL, 0.5 mL, or a range consisting of any two of the foregoing values. An M2 of 0 mL indicates zero free electrolyte, meaning that substantially no free electrolyte remains within the battery cell after the extrusion test.

[0286] In some embodiments, a voltage of 200 V is provided to the battery cell to form a loop for 4 hours, and the absolute value of the temperature change of the battery cell is ≤ 4°C.

[0287] For example, when the negative terminal and outer casing of a battery cell are connected to a 200V voltage to form a current loop, the battery cell's temperature fluctuates within 4°C over a 4-hour period, without any failures such as fire or explosion. In particular, when the free electrolyte y = 0, the temperature fluctuation range is minimal, significantly improving the reliability of the battery cell.

[0288] In order to further enhance the liquid absorption and storage capabilities of the electrode assembly 52 , a liquid-retaining polymer may be added to at least one of the first electrode piece 8 and the second electrode piece 9 .

[0289] In some embodiments, the first electrode 8 includes a current collector and a film layer disposed on at least one surface of the current collector, the film layer comprising a liquid-retaining polymer and active material particles. The liquid-retaining polymer may be disposed only in the first electrode 8 or only in the second electrode 9, or both. The first electrode 8 may be a positive electrode, and accordingly, the second electrode 9 may be a negative electrode; alternatively, the first electrode 8 may be a negative electrode, and accordingly, the second electrode 9 may be a positive electrode.

[0290] As some examples, the liquid-retaining polymer is distributed on the surface of the active material particles; it can be understood that the active material particles and the binder are solidified into an active material layer on the surface of the current collector, and the liquid-retaining polymer is arranged on the surface of the active material layer away from the current collector. Such a configuration allows the electrolyte to quickly diffuse between the molecular chains of the liquid-retaining polymer and be wrapped by the molecular chains, forming a gel-like substance on the surface of the active material particles and adhering to the surface of the active material particles to protect the active material particles. This closely connects the active material particles and the electrolyte, improves the solid-liquid interface performance, can reduce side reactions between the active material particles and the electrolyte, and improves the reliability and electrical performance (such as cycle performance and storage performance) of the battery cell.

[0291] Specifically, the electrode preparation process includes:

[0292] adding active material particles into a solvent to prepare an active slurry;

[0293] Applying the active slurry to the surface of the current collector and drying and solidifying it into an active material layer;

[0294] A liquid-retaining polymer is placed on the surface of the active material layer to form an electrode.

[0295] As other examples, there are multiple active material particles, and there are pores between two adjacent active material particles. The liquid-retaining polymer is distributed in the pores between the active material particles. This setting can improve the liquid storage capacity of the active material layer, that is, the ability to lock the electrolyte, thereby improving the reliability and electrical performance of the battery cell.

[0296] Specifically, the preparation process of an embodiment of a pole piece includes:

[0297] dispersing the liquid-retaining polymer in the solvent to form a mixed system;

[0298] Adding active material particles into the mixed system to prepare a slurry;

[0299] The slurry is applied to the surface of the current collector and dried and solidified to form a pole piece.

[0300] Specifically, the preparation process of another embodiment of the pole piece includes:

[0301] Dispersing the liquid-retaining polymer and active material particles in a solvent to prepare a slurry;

[0302] The slurry is applied to the surface of the current collector and dried and solidified to form a pole piece.

[0303] As some further examples, the liquid-retaining polymer is distributed on the surface of the active material particles, and the liquid-retaining polymer is distributed in the pores between the active material particles.

[0304] Specifically, the preparation process of an embodiment of a pole piece includes:

[0305] Dispersing the liquid-retaining polymer and active material particles in a solvent to prepare a slurry;

[0306] Applying the slurry on the surface of the current collector and drying and solidifying it into an active material layer;

[0307] A liquid-retaining polymer is placed on the surface of the active material layer to form an electrode.

[0308] In some embodiments, the liquid-retaining polymer may include at least one of a second fluoropolymer, a second ether polymer, a second ester polymer, and a ketone-aldehyde polymer. The liquid-retaining polymer and the electrolyte have good affinity, and the electrolyte can quickly diffuse between the molecular chains of the liquid-retaining polymer and be wrapped by the molecular chains. After swelling and adsorption, an elastic porous slow-release electrolyte is obtained. The slow-release electrolyte can absorb the free electrolyte in the battery cell and reduce the presence of the free electrolyte. Since the free electrolyte is locked, the risk of the free electrolyte being squeezed out is reduced, thereby reducing the risk of short-circuiting the positive and negative pole pieces due to dendrite formation, and improving the reliability and cycle performance of the battery cell. In addition, the absorbed free electrolyte forms a new condensed electrolyte with the elastic porous slow-release electrolyte, which can ensure that the electrolyte has a higher conductivity, thereby improving the electrical performance of the battery cell.

[0309] [Second fluorinated polymer]

[0310] In some embodiments, the liquid-retaining polymer comprises a second fluoropolymer having a crystallinity of X 0.001 ... C1 %,0<X C1 ≤30; the melting temperature of the second fluorinated polymer is T m1 , its unit is ℃, 0<T m1 ≤140.

[0311] Crystallization refers to the process in which atoms, ions or molecules in a material are arranged in a certain spatial order to form an orderly structure. The conformation of the polymer in the crystallization is determined by both intramolecular and intermolecular factors. The intermolecular force will affect the packing density between molecular chains. C1 % is used to characterize the degree of crystallinity in the material, which can be measured by differential scanning calorimetry (DSC). Specifically, the test steps are as follows: take 0.5g to 0.8g of sample, place the sample in a carrier crucible, and perform temperature rise and fall treatment on the sample under a nitrogen atmosphere, with a heating rate of 10℃ / min from the intrinsic T g1 The initial temperature is 20℃ lower and then heated to the intrinsic T m1 The cut-off temperature of the process is 20℃ higher. The actual glass transition temperature T of the material is determined according to the endothermic and exothermic peak or transition point of the material in the process. g1 and melting temperature T m1 wait.

[0312] As a result, the second fluoropolymer has a relatively low crystallinity and melting temperature, so that the molecular chain arrangement tends to be loose, the interaction force between the molecular chains is small, adjacent molecular chains are easily opened, and chain segment movement is achieved through intermolecular internal rotation, forming a molecular chain structure with high flexibility; and the second fluoropolymer and the electrolyte in the battery cell can form a gel-like substance, thereby improving the reliability and cycle performance of the battery cell.

[0313] For example, the crystallinity X of the second fluorinated polymer measured by differential scanning calorimetry is C1 % can be 5%, 10%, 15%, 20%, 25%, 30% or a range consisting of any two of the above values.

[0314] Illustratively, the melting temperature of the second fluorinated polymer may be 10° C., 20° C., 50° C., 70° C., 90° C., 100° C., 120° C., 140° C., or a range consisting of any two of the foregoing values.

[0315] In some embodiments, the glass transition temperature of the second fluoropolymer is T g1 , its unit is ℃, -150≤T g1 ≤60.

[0316] The glass transition temperature is the temperature at which the chain segments of a polymer transition from freezing to movement. The glass transition temperature has a certain influence on the flexibility of the polymer molecular chain. The lower the glass transition temperature, the better the flexibility of the polymer molecular chain at room temperature. The higher the glass transition temperature, the worse the flexibility of the molecular chain at room temperature. The glass transition temperature can be measured by differential scanning calorimetry (DSC). The glass transition temperature of a polymer is relatively low, the segment flexibility of the molecular chain is better, and adjacent molecular chains are easier to open. For example, the glass transition temperature of the second fluorinated polymer can be -150°C, -120°C, -100°C, -80°C, -60°C, -30°C, 0°C, 30°C, 60°C, or a range consisting of any two of the above values.

[0317] The structural units of the second fluorinated polymer are the same as those of the first fluorinated polymer described above, but the substituents of the side chains of the two are not exactly the same.

[0318] In some embodiments, the second fluorinated polymer comprises at least one of the structural units represented by formula (AI) to the structural units represented by formula (AIII),

[0319] In formula (AI) and formula (AII), R 11 、R 12 、R 13 and R 14 Each independently includes a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted C1-C3 alkyl group, or a substituted or unsubstituted C1-C3 alkoxy group, and R 11 、R 12 、R 13 and R 14 At least one of them contains a fluorine atom;

[0320] When substituted, the substituent may include one or more of a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0321] In formula (AIII), R 15 Includes single bonds, substituted or unsubstituted C1-C3 alkyl groups; when substituted, the substituents include fluorine atoms.

[0322] In some embodiments, p is a positive integer selected from 1 to 3.

[0323] In some embodiments, the degree of polymerization n of the second fluoropolymer is selected from a positive integer ranging from 1,000 to 30,000.

[0324] In some embodiments, R 11 、R 12 、R 13 and R14 Each independently includes a hydrogen atom, a fluorine atom, a chlorine atom, a substituted or unsubstituted C1-C2 alkyl group or a substituted or unsubstituted C1-C2 alkoxy group; further optionally, R 11 、R 12 、R 13 and R 14 Each independently includes a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, a fluoromethyl group, a methoxy group or a perfluoromethoxy group.

[0325] In some embodiments, when substituted, the substituent may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0326] In some embodiments, the second fluorinated polymer comprises at least one of the structural units represented by formula (AI-1) to the structural units represented by formula (AI-11),

[0327] In some embodiments, the second fluorinated polymer includes at least one of the structural units represented by formula (AII-1) to the structural units represented by formula (AII-5),

[0328] In some embodiments, the second fluorinated polymer includes at least one of the structural units represented by formula (AIII-1) to the structural units represented by formula (AIII-3),

[0329] Exemplarily, the second fluorinated polymer includes one or more of polyperfluoroethylene (PTFE), polyvinylidene fluoride (PVDF), perfluoroethylene propylene copolymer (FEP), perfluoroalkoxy polymer (PFA), perfluoropolyether (PFPE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyvinylidene fluoride-trifluoroethylene copolymer (PVDF-TrFE) and perfluoro (1-butenyl vinyl ether) polymer (CYTOP for short).

[0330] Optionally, the second fluorinated polymer includes one or more of polyperfluoroethylene (PTFE), polyvinylidene fluoride (PVDF), perfluoroethylene propylene (FEP), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), and polyvinylidene fluoride-trifluoroethylene (PVDF-TrFE).

[0331] The second fluoropolymer may be derived from one or more of the following monomers: fluorocycloethane, vinyl fluoride, 1,2-difluoroethylene, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, hexafluoropropylene, 3,3,3-trifluoropropylene, trifluoropropylene, tetrafluoropropylene, and pentafluoropropylene. Alternatively, the fluoropolymer may be derived from at least two of the following monomers: fluorocycloethane, vinyl fluoride, 1,2-difluoroethylene, vinylidene fluoride, trifluoroethylene, chlorotrifluoroethylene, tetrafluoroethylene, hexafluoropropylene, 3,3,3-trifluoropropylene, trifluoropropylene, tetrafluoropropylene, and pentafluoropropylene.

[0332] The monomers used in the above-mentioned second fluorinated polymer are all short-chain monomers, which are conducive to polymerization to form a straight-chain linear structure or a short-chain branched structure. This type of structure has a low degree of entanglement, which is conducive to improving the flexibility of the molecular chain. The molecular chain can fully stretch in the electrolyte, thereby further improving the interfacial performance of the active material.

[0333] In some embodiments, the degree of polymerization n of the second fluoropolymer is selected from a positive integer ranging from 5,000 to 20,000.

[0334] In some embodiments, the molecular weight of the liquid retaining polymer is 2×10 5 g / mol to 1.5×10 6 g / mol.

[0335] When the molecular weight of the liquid-retaining polymer is within the above range, the interaction between the molecular chains is relatively weak, which is conducive to the solvent molecules in the electrolyte opening the molecular chains and entering between the molecular chains, thereby facilitating the active ions to enter the active material through the solvent, thereby achieving smooth and rapid migration of the active ions. For example, the molecular weight of the polymer can be 2×10 5 g / mol, 5×10 5 g / mol, 8×10 5 g / mol, 1×10 6 g / mol, 1.5×10 6 g / mol or a range consisting of any two of the above values.

[0336] [Second ether polymer]

[0337] In some embodiments, the liquid-retaining polymer includes a second ether polymer, and the second ether polymer is made into a sheet structure; the sheet structure is (T m2 The elastic modulus G'-energy loss modulus G" curve was obtained by dynamic frequency sweep test at +20)℃. The slope of the elastic modulus G'-energy loss modulus G" curve is K1, 1<K1<∞, T m2 °C represents the melting temperature of the second ether polymer.

[0338] Specifically, the sheet structure is prepared as follows: the second ether polymer is vacuum dried at 80°C for 12 hours. The dried ether polymer is hot-pressed into a sheet by a flat vulcanizer, and the hot-pressing temperature is set to (T m2 The sample is then removed from the press after 2 minutes of calendering and placed on another vulcanizing press of the same model for cold pressing at a pressure of 10 MPa. A polymer disc (sheet structure) of fixed size is obtained using a circular mold with a diameter of 25 mm. For example, the sheet structure can be a disc with a thickness of 1-2 mm and a diameter of 25 mm; alternatively, a sample can be prepared according to the sample standard required by the test equipment.

[0339] According to the conclusions of classical linear viscoelasticity, for polymers, especially linear polymers, the elastic modulus G'-dissipation modulus G" in the terminal region of the elastic modulus G'-dissipation modulus G" curve (the interval approaching the maximum angular velocity) conforms to frequency dependence, and the longest chain of the polymer plays a role in the viscoelastic behavior.

[0340] The specific steps of the dynamic frequency sweep test are as follows: The dynamic frequency sweep test was performed using a TA-AR2000EX rotational rheometer (TAinstruments, USA) with a parallel plate diameter of 25 mm and a thickness of 0.9 mm. To ensure that the test was in the linear point-bounce region, the strain during the dynamic frequency sweep test was 2% and the test temperature was T m2 +20℃, test frequency sweep range: 500rad / s≤w 2 ≤0.05rad / s, so as to obtain data in the lowest possible frequency range.

[0341] The dynamic frequency sweep test can characterize the degree of entanglement of molecular chains under solid-phase melting (melt state). Compared with linear structures or short-chain branched structures, long-branched structures, network structures, and low-crosslinked structures have a high degree of entanglement, which will show deviation from linear terminal behavior. Ether polymers exhibit solid-phase behavior. When the ether polymers of the present application meet the above range, the entanglement state of the molecular chains can be further reduced, which is conducive to the diffusion of solvent molecules in the electrolyte between the molecular chains; moreover, the ether polymers still maintain a certain degree of molecular chain entanglement and can form a gel-like substance with the electrolyte, thereby improving the cycle performance and storage performance of the battery cell.

[0342] In some embodiments, 1<K1≤100; alternatively, 1<K1≤10. For example, K1 can be 0.8, 0.9, 1, 2, 5, 10, 15, 20, 30, 50, 100, 200, 500, 1000, 5000, 10000, or a range consisting of any two of the above values.

[0343] In some embodiments, the glass transition temperature of the second ether polymer is T g2 , its unit is ℃, -100≤T g2 ≤50; optionally, -80≤T g2 ≤30. For example, the glass transition temperature of the ether polymer may be -100°C, -80°C, -60°C, -30°C, 0°C, 30°C, 50°C, or a range consisting of any two of the above values.

[0344] In some embodiments, the structural unit of the second ether polymer is the same as the structural unit of the first ether polymer described above, but the substituents of the side chains of the two are not exactly the same.

[0345] In some embodiments, the second ether polymer comprises a structural unit represented by formula (BI),

[0346] In formula (BI), R 21 and R 22 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C3 alkyl group, or a substituted or unsubstituted C1-C3 alkoxy group; R 23 This includes substituted or unsubstituted C1-C5 methylene groups.

[0347] In some embodiments, R 21 and R 22 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C2 alkyl group.

[0348] In some embodiments, R 23 It includes single bonds, substituted or unsubstituted C1-C4 methylene groups.

[0349] In some embodiments, when substituted, the substituent may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0350] Illustratively, the second ether polymer includes at least one of the structural units represented by formula (BI-1) to the structural units represented by formula (BI-8),

[0351] In some embodiments, the second ether polymer comprises a structural unit represented by formula (BII),

[0352] In formula (BII), R 24 to R 27 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C3 alkoxy group or an ether group, and R 24 to R27 At least one of them contains a substituted or unsubstituted C1-C3 alkoxy group or an ether group.

[0353] Optionally, R 24 to R 27 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C2 alkyl group, a substituted or unsubstituted C1-C2 alkoxy group or an ether group, and R 24 to R 27 At least one of them contains a substituted or unsubstituted C1-C2 alkoxy group or an ether group.

[0354] In some embodiments, the second ether polymer includes at least one of the structural units represented by formula (BII-1) to the structural units represented by formula (BII-7),

[0355] The above polymers are merely examples of the structural groups of the main molecular chain. In the embodiments of the present application, the polymers may also be obtained by copolymerizing the above structural groups with other types of structural groups (such as olefin structural units, acrylonitrile structural units, etc.).

[0356] When the above-mentioned groups are substituted, the substituents may include one or more of a nitrile group (-CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom. These substituents are high-pressure-resistant substituents, which are more conducive to stabilizing the structure of the polymer. Halogen atoms may include fluorine atoms, chlorine atoms, bromine atoms, and the like.

[0357] In some embodiments, the degree of polymerization n of the second ether polymer is a positive integer selected from 1,500 to 25,000.

[0358] Optionally, the polymerization degree n of the second ether polymer is a positive integer selected from 3,000 to 18,000.

[0359] In some embodiments, the molecular weight of the second ether polymer is 1.2×10 5 g / mol to 1.0×10 6 g / mol.

[0360] For example, the molecular weight of the polymer may be 1.2×10 5 g / mol, 2×10 5 g / mol, 5×10 5 g / mol, 8×10 5 g / mol, 1×10 6 g / mol or a range consisting of any two of the above values.

[0361] [Second ester polymer]

[0362] In some embodiments, the liquid-retaining polymer includes a second ester polymer, wherein the second ester polymer is made into a sheet structure; the sheet structure is (T m3 The elastic modulus G'-energy loss modulus G" curve was obtained by dynamic frequency sweep test at +20)℃. The slope of the elastic modulus G'-energy loss modulus G" curve is K2, 1<K2<∞, T m3 °C represents the melting temperature of the second ester polymer.

[0363] When the second ester polymer of the present application meets the above range, the entanglement state of the molecular chains can be further reduced, which is beneficial to the diffusion of solvent molecules in the electrolyte between the molecular chains; and the ether polymer still maintains a certain molecular chain entanglement state, and can form a gel-like substance with the electrolyte, thereby improving the cycle performance and storage performance of the battery cell.

[0364] In some embodiments, 1<K2≤100; optionally, 1<K2≤10.

[0365] Illustratively, K2 may be 1.01, 1.1, 1.2, 1.5, 2, 5, 10, 15, 20, 30, 50, 100, 200, 500, 1000, 5000, 10000, or a range consisting of any two of the above values.

[0366] In some embodiments, the glass transition temperature of the second ester polymer is T g3 , its unit is ℃, -100≤T g3 ≤50; optionally, -80≤T g3 ≤30.

[0367] For example, the glass transition temperature of the second ester polymer may be -100°C, -90°C, -80°C, -60°C, -30°C, 0°C, 30°C, 50°C, or a range consisting of any two of the above values.

[0368] In some embodiments, the structural unit of the second ester polymer is the same as the structural unit of the first ester polymer described above, but the substituents of the side chains of the two are not exactly the same.

[0369] In some embodiments, the second ester polymer comprises a structural unit represented by formula (CI),

[0370] In formula (CI), R 31 、R 32 and R 33 Each independently includes a hydrogen atom, or a substituted or unsubstituted C1-C8 alkyl group; R 34It includes substituted or unsubstituted C1-C8 alkyl groups, or substituted or unsubstituted C1-C8 hydroxyalkyl groups.

[0371] In some embodiments, R 34 It includes substituted or unsubstituted C1-C6 alkyl groups, or substituted or unsubstituted C1-C6 hydroxyalkyl groups.

[0372] In some embodiments, R 31 This includes a hydrogen atom, or a substituted or unsubstituted methyl group.

[0373] In some embodiments, R 32 and R 33 Each independently includes a hydrogen atom.

[0374] In some embodiments, R 34 It includes substituted or unsubstituted C1-C4 alkyl groups, or substituted or unsubstituted C1-C4 hydroxyalkyl groups.

[0375] In some embodiments, when substituted, the substituent may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0376] Illustratively, the second ester polymer includes at least one of the structural units represented by formula (CI-1) to the structural units represented by formula (CI-15),

[0377] In some embodiments, the second ester polymer comprises a structural unit represented by formula (CII),

[0378] In formula (CII), R 35 This includes substituted or unsubstituted C2-C6 methylene groups.

[0379] In some embodiments, R 35 Each independently includes a substituted or unsubstituted C2-C4 methylene group.

[0380] Illustratively, the second ester polymer includes at least one of the structural units represented by formula (CII-1) to the structural units represented by formula (CII-5),

[0381] In some embodiments, the second ester polymer comprises a compound represented by formula (CIII),

[0382] In formula (CIII), R 36 、R 37 and R38 Each independently includes a hydrogen atom, or a substituted or unsubstituted C1-C8 alkyl group; R 39 Including substituted or unsubstituted C1-C8 alkyl;

[0383] Optionally, R 36 、R 37 and R 38 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C4 alkyl group.

[0384] Illustratively, the ester polymer includes at least one of the compounds represented by formula (CIII-1) to the compounds represented by formula (CIII-5),

[0385] The above-mentioned polymers are only examples of the structural groups of the main molecular chain. In the embodiments of the present application, the polymers can also be obtained by copolymerizing the above-mentioned structural groups with other types of structural groups (such as olefin structural units, acrylonitrile structural units, maleic anhydride and other monomers with functional groups).

[0386] When the above groups are substituted, the substituents may include one or more of a nitrile group, a nitro group, a sulfonyl group, a carboxyl group, an ester group, a chlorine atom, a fluorine atom, and a bromine atom. The above substituents are high-pressure-resistant substituents, which are more conducive to stabilizing the structure of the polymer.

[0387] In some embodiments, the degree of polymerization n of the second ester polymer is a positive integer selected from 800 to 20,000.

[0388] In some embodiments, the degree of polymerization n of the second ester polymer is a positive integer selected from 1,000 to 15,000.

[0389] In some embodiments, the molecular weight of the second ester polymer is 1.2×10 5 g / mol to 1.0×10 6 g / mol.

[0390] For example, the molecular weight of the second ester polymer may be 1.2×10 5 g / mol, 2×10 5 g / mol, 5×10 5 g / mol, 8×10 5 g / mol, 1×10 6 g / mol, 1.5×10 6 g / mol or a range consisting of any two of the above values.

[0391] [Ketone-aldehyde polymers]

[0392] In some embodiments, the liquid-retaining polymer comprises an aldehyde-ketone polymer, wherein the aldehyde-ketone polymer is made into a sheet structure; the sheet structure is (T m4 The elastic modulus G'-energy loss modulus G" curve was obtained by dynamic frequency sweep test at +20)℃. The slope of the elastic modulus G'-energy loss modulus G" curve is K3, 0.8≤K3<∞, T m4 °C represents the melting temperature of the aldehyde-ketone polymer.

[0393] In some embodiments, 0.8≤K3≤100; optionally, 0.8≤K3≤10.

[0394] Illustratively, K3 may be 0.8, 0.9, 1, 2, 5, 10, 15, 20, 30, 50, 100, 200, 500, 1000, 5000, 10000, or a range consisting of any two of the above values.

[0395] In some embodiments, the glass transition temperature of the aldehyde-ketone polymer is T g4 , its unit is ℃, -100≤T g4 ≤50; optionally, -80≤T g4 ≤30.

[0396] For example, the glass transition temperature of the aldehyde-ketone polymer may be -100°C, -90°C, -80°C, -60°C, -30°C, 0°C, 30°C, 50°C, or a range consisting of any two of the above values.

[0397] In some embodiments, the liquid-retaining polymer comprises an aldehyde-ketone polymer, wherein the aldehyde-ketone polymer comprises a structural unit represented by formula (DI),

[0398] In formula (DI), R 41 Including single bonds, substituted or unsubstituted C1-C6 methylene; R 42 This includes a hydrogen atom, and a substituted or unsubstituted C1-C6 alkyl group.

[0399] Optionally, R 41 It includes single bonds, substituted or unsubstituted C1-C2 methylene groups.

[0400] Optionally, R 42 This includes a hydrogen atom, and a substituted or unsubstituted C1-C3 alkyl group.

[0401] In the embodiments of the present application, a single bond indicates that the group does not exist, and the atoms on both sides of the group are connected by a single bond, for example, R 41 is a single bond, indicating R 41 The carbon atoms on both sides are connected by single bonds.

[0402] In some embodiments, when substituted, the substituent may include one or more of a nitrile group (—CN), a nitro group, a sulfonic acid group, a sulfonyl group, an amide group, a carboxyl group, an ester group, and a halogen atom.

[0403] Illustratively, the aldehyde-ketone polymer includes at least one of the structural units represented by formula (DI-1) to the structural units represented by formula (DI-6),

[0404] Illustratively, the aldehyde-ketone polymer includes a structural unit represented by formula (DII),

[0405] In formula (DII), R 43 to R 46 Each independently includes a hydrogen atom, a hydroxyl group, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C3 hydroxyalkyl group, or a substituted or unsubstituted C1-C3 alkoxy group; r and s are each independently selected from an integer from 0 to 5, and at least one of r and s is selected from a positive integer.

[0406] Optionally, R 43 to R 46 Each independently includes a hydrogen atom, a hydroxyl group, a substituted or unsubstituted C1-C3 alkyl group, a substituted or unsubstituted C1-C2 hydroxyalkyl group, or a substituted or unsubstituted C1-C2 alkoxy group.

[0407] In some embodiments, the aldehyde-ketone polymer includes at least one of the structural units represented by formula (DII-1) to the structural units represented by formula (DII-4),

[0408] The above polymers are only examples of the structural groups of the main molecular chain. In the embodiments of the present application, the polymers can also be obtained by copolymerizing the above structural groups with other types of structural groups (such as olefin structural units, enol structural units, acrylonitrile structural units, etc.).

[0409] When the above-mentioned groups are substituted, the substituents may include one or more of a nitrile group (-CN), a nitro group, a sulfonyl group, a carboxyl group, an ester group, a chlorine atom, a fluorine atom, and a bromine atom. These substituents are high-pressure-resistant substituents and are more conducive to stabilizing the structure of the polymer.

[0410] In some embodiments, the degree of polymerization n of the aldehyde-ketone polymer is a positive integer selected from 500 to 15,000.

[0411] Optionally, the degree of polymerization n of the aldehyde-ketone polymer is selected from a positive integer ranging from 500 to 10,000.

[0412] In some embodiments, the molecular weight of the aldehyde-ketone polymer is 1.2×10 5 g / mol to 1.0×10 6 g / mol.

[0413] For example, the molecular weight of the aldehyde-ketone polymer may be 1.2×10 5 g / mol, 2×10 5 g / mol, 5×10 5 g / mol, 8×10 5 g / mol, 1×10 6 g / mol, 1.0×10 6 g / mol or a range consisting of any two of the above values.

[0414] The relevant parameters of the liquid-retaining polymer according to the embodiment of the present application can be detected by the following methods:

[0415] The groups of the liquid-retaining polymer of the embodiment of the present application can be detected by infrared spectrophotometry IR. Specifically, the liquid-retaining polymer is tested using a Thermo Nicolet Nexus 670 attenuated total reflectance Fourier transform infrared spectrometer (FTIR-ATR), and then tested in accordance with the standard GB / T6040-2002. The test range is: ATR method 600-4000 cm -1 ; Repeatability: ±2cm -1 ; Resolution: better than 4cm -1 ; Transmission depth 0.2~0.6μm.

[0416] The structure of the liquid-retaining polymer according to the embodiment of the present application can be tested by nuclear magnetic resonance (NMR). Specifically, 1H NMR and 13C NMR are performed on a Varian Mercury Plus-400 NMR spectrometer at a test temperature of 20° C., TMS as an internal standard, CDCl 3 as a solvent, and a proton resonance frequency of 400 MHz.

[0417] The polymer monomer type of the liquid-retaining polymer in the embodiment of the present application (especially suitable for monomers that account for a relatively small proportion in the polymer) can be tested by pyrolysis-gas chromatography-mass spectrometry. The specific testing steps are as follows: accurately weigh 0.5 mg of sample and put it into the sample cup. After fixing it to the injection rod, it is loaded into the pyrolyzer installed near the GC (gas chromatography) injection port. After the pyrolyzer temperature reaches the set temperature, press the injection button, and the sample cup falls rapidly into the core of the pyrolysis furnace by free fall. In the inert gas N2 atmosphere, the volatile components are instantly vaporized and carried into the gas chromatography column by the carrier gas for separation. Finally, it is detected by a flame ionization detector FID or a mass spectrometer MS to obtain a gas chromatogram or a total ion current diagram.

[0418] The molecular weight of the liquid-retaining polymer in the embodiment of the present application is well known in the art and can be measured using commonly used equipment and methods in the art. Gel permeation chromatography (GPC) testing can be used. The specific testing steps are as follows: take an appropriate amount of the sample to be tested (the sample concentration is sufficient to ensure 8%-12% shading), add 20 ml of deionized water, and simultaneously ultraviolet (53KHz / 120W) for 5 minutes to ensure that the sample is completely dispersed. Then, the sample is measured in accordance with the GB / T19077-2016 / ISO 13320:2009 standard.

[0419] Alternatively, a multi-angle laser light scattering (MALLS) instrument was used for testing. Specifically, a GPC coupled with a Dawn Heleos II multi-angle laser light scattering device, an Optilab T-rEX refractive index (RI) detector, and a Visco Star II viscometer (Wyatt Technology Corporation, USA) was used. Testing was conducted at 30°C, using tetrahydrofuran as the mobile phase at a flow rate of 1.0 ml / min. SEC-SAMLL data were processed using the commercial ASTRA6 software to obtain molecular weight parameters.

[0420] The above-mentioned polymers are only examples of the structural groups of the main molecular chains. In the embodiments of the present application, the polymers can also be obtained by copolymerizing the above-mentioned structural groups with a small amount of other types of structural groups (such as olefin structural units, ester monomers, nitrile monomers, amide monomers and other structural units).

[0421] [Positive electrode]

[0422] The battery cell includes a positive electrode plate, and the positive electrode plate includes a positive electrode current collector and a positive electrode film layer arranged on the positive electrode current collector.

[0423] In some embodiments, the positive electrode film layer includes a positive electrode active material.

[0424] In other embodiments, the positive electrode film layer includes a positive electrode active material and a liquid-retaining polymer.

[0425] As some examples, the positive electrode film layer includes a polymer layer containing a liquid-retaining polymer and a positive electrode active material layer containing positive electrode active material particles, the positive electrode active material layer is arranged on at least one surface of the positive electrode collector, and the polymer layer is arranged on the surface of the positive electrode active material layer away from the positive electrode collector.

[0426] As some other examples, there are a plurality of positive electrode active material particles, a pore exists between two adjacent positive electrode active material particles, and the liquid-retaining polymer is distributed in the pore.

[0427] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is disposed on either or both of the two facing surfaces of the positive electrode current collector.

[0428] The positive electrode active material layer includes a positive electrode active material, which can be a positive electrode active material commonly known in the art for use in battery cells. For example, the positive electrode active material includes at least one of a lithium-containing positive electrode active material and a sodium-containing positive electrode active material, and can include at least one of the following materials: a lithium-containing phosphate compound, a lithium-containing transition metal oxide, a sodium-containing phosphate compound, and a sodium-containing transition metal oxide.

[0429] For example, the general formula of the olivine-type phosphate active material (lithium-containing phosphate compound) is: Li x A y Me a M b P 1-c X c Y z , wherein 0≤x≤1.3, 0≤y≤1.3, and 0.9≤x+y≤1.3; 0.9≤a≤1.5, 0≤b≤0.5, and 0.9≤a+b≤1.5; 0≤c≤0.5; 3≤z≤5; A includes one or more of Na, K, and Mg; Me includes one or more of Mn, Fe, Co, and Ni; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; X includes one or more of S, Si, Cl, B, C, and N; and Y includes one or more of O and F. Specifically, the olivine-type phosphate active material includes one or more of LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4.

[0430] For example, lithium transition metal oxides (layered materials such as ternary, lithium nickelate / sodium, lithium cobaltate / sodium, lithium manganate / sodium, lithium-rich layered and rock salt phase layered materials). The general formula of the layered structure positive electrode active material is: Li x A y Ni a Co b Mn c M (1-a-b-c) Y z, wherein 0≤x≤2.1, 0≤y≤2.1, and 0.9≤x+y≤2.1; 0≤a≤1, 0≤b≤1, 0≤c≤1, and 0.1≤a+b+c≤1; 1.8≤z≤3.5; A includes one or more of Na, K, and Mg; M includes one or more of B, Mg, Al, Si, P, S, Ca, Sc, Ti, V, Cr, Fe, Cu, Zn, Sr, Y, Zr, Nb, Mo, Cd, Sn, Sb, Te, Ba, Ta, W, Yb, La, and Ce; Y includes one or more of O and F. Optionally, y=0. Specifically, the layered structure positive electrode active material may include lithium cobalt oxide LCO, lithium nickel oxide LNO, lithium manganese oxide LMO, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NML33), LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523),LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 One or more of O2 (NCM811) and NCA.

[0431] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil or an aluminum alloy foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include a combination of one or more selected from aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. The polymer material base layer may include a combination of one or more selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0432] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode conductive agent. The present application does not particularly limit the type of positive electrode conductive agent. For example, the positive electrode conductive agent may include a combination of one or more selected from superconducting carbon, conductive carbon black, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the positive electrode conductive agent is less than 5% based on the total mass of the positive electrode active material layer.

[0433] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode binder. The embodiments of the present application do not particularly limit the type of positive electrode binder. As an example, the positive electrode binder may include a combination of one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylic resin. In some embodiments, based on the total mass of the positive electrode active material layer, the mass percentage of the positive electrode binder is less than 5%. Compared to the crystallinity of the fluorinated polymer in the embodiment of the present application, the crystallinity of the positive electrode binder is higher.

[0434] The positive electrode active material layer is typically formed by coating a positive electrode slurry onto a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional liquid-retaining polymer, an optional conductive agent, an optional binder, and any other components in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP). Of course, the preparation of the positive electrode sheet is not limited to the above method; the preparation methods described above can also be used.

[0435] [Negative electrode]

[0436] The battery cell includes a negative electrode plate.

[0437] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces that are opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.

[0438] In some embodiments, the negative electrode film layer includes a negative electrode active material.

[0439] As some examples, the negative electrode film layer includes a polymer layer containing a liquid-retaining polymer and a negative electrode active material layer containing negative electrode active material particles, the negative electrode active material layer is arranged on at least one surface of the negative electrode collector, and the polymer layer is arranged on the surface of the negative electrode active material layer away from the negative electrode collector.

[0440] As some other examples, there are a plurality of negative electrode active material particles, a gap exists between two adjacent negative electrode active material particles, and the liquid-retaining polymer is distributed in the gap.

[0441] The negative electrode active material can be any negative electrode active material known in the art for use in battery cells. For example, the negative electrode active material may include, but is not limited to, at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may include at least one of elemental silicon, silicon oxide, a silicon-carbon composite, a silicon-nitrogen composite, and a silicon alloy. The tin-based material may include at least one of elemental tin, tin oxide, and a tin alloy.

[0442] In some embodiments, the negative electrode active material layer may further optionally include a negative electrode conductive agent. The present embodiments do not particularly limit the type of the negative electrode conductive agent. For example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the negative electrode conductive agent is ≤5% based on the total mass of the negative electrode active material layer.

[0443] In some embodiments, the negative electrode active material layer may further optionally include a negative electrode binder. The present application embodiment does not particularly limit the type of the negative electrode binder. As an example, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the negative electrode binder based on the total mass of the negative electrode active material layer is ≤5%.

[0444] In some embodiments, the negative electrode active material layer may optionally include other additives. For example, these additives may include thickeners, such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, and the like. In some embodiments, the weight percentage of these other additives is ≤ 2% based on the total weight of the negative electrode active material layer.

[0445] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of copper, a copper alloy, nickel, a nickel alloy, titanium, a titanium alloy, silver, and a silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0446] The negative electrode active material layer is typically formed by coating a negative electrode slurry onto a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional liquid-retaining polymer, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring them uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water. Of course, the preparation of the negative electrode sheet is not limited to the above method; the preparation method described above may also be used.

[0447] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode active material layer. For example, in some embodiments, the negative electrode plate described herein further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode active material layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode plate described herein further includes a protective layer covering the surface of the negative electrode active material layer.

[0448] [Electrolyte]

[0449] The battery cells include an electrolyte.

[0450] During the charge and discharge process of a battery cell, active ions are embedded and released back and forth between the positive and negative electrodes, and the electrolyte conducts the active ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and it can be selected according to actual needs.

[0451] The electrolyte solution includes an electrolyte salt and a solvent. The types of the electrolyte salt and the solvent are not particularly limited and can be selected according to actual needs.

[0452] When the battery cell of the present application is a lithium-ion battery, as an example, the electrolyte salt may include but is not limited to at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0453] When the battery cell of the present application is a sodium ion battery, as an example, the electrolyte salt may include but is not limited to at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobis(oxalatophosphate) (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP).

[0454] As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0455] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature power performance.

[0456] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet may be formed into an electrode assembly through a winding process and / or a lamination process.

[0457] In some embodiments, the battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0458] In some embodiments, the outer packaging of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery cell may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0459] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet may be formed into an electrode assembly by a winding process or a lamination process.

[0460] The present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square, or any other shape. FIG9 shows a battery cell 5 with a square structure as an example.

[0461] In some embodiments, as shown in Figures 10 and 11, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, which can be adjusted according to demand.

[0462] The manufacturing method of the battery cell of the present application is well known. In some embodiments, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, separator, and negative electrode sheet can be wound or laminated to form an electrode assembly. The electrode assembly is then placed in an outer packaging, dried, and then injected with electrolyte. The battery cell is then vacuum packaged, allowed to stand, formed, and shaped to obtain a battery cell.

[0463] In some embodiments of the present application, the battery cells according to the present application can be assembled into a battery module. The battery module can contain multiple battery cells, and the specific number can be adjusted according to the application and capacity of the battery module.

[0464] Figure 12 is a schematic diagram of an exemplary battery module 4. As shown in Figure 12 , within the battery module 4, multiple battery cells 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple battery cells 5 may be secured together using fasteners.

[0465] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.

[0466] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0467] Both the battery module 4 and the battery pack can be used as specific examples of batteries in the embodiments of the present application.

[0468] Figures 13 and 14 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 13 and 14, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery box.

[0469] Electrical devices

[0470] On the third aspect, the present application provides an electrical device, which includes at least one of the battery cells, battery modules and battery packs of the present application. The battery cells, battery modules and battery packs can be used as power sources for the electrical device, and can also be used as energy storage units for the electrical device. The electrical device may be, but is not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc. In some embodiments, the battery cell includes an injection hole for injecting electrolyte; when the battery cell is applied to the electrical device, the injection hole is located at the bottom of the battery cell in the vertical direction. Since the amount of free electrolyte in the battery cell is extremely small, or even no free electrolyte, when the injection hole is set at the bottom of the battery cell in the vertical direction, the reliability of the battery cell can also be improved, thereby improving the reliability of the electrical device.

[0471] The electric device can select a battery cell, a battery module or a battery pack according to its usage requirements. Figure 15 is a schematic diagram of an electric device as an example. The electric device 6 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the electric device, a battery pack 1 or a battery module can be used. As another example, the electric device can be a mobile phone, a tablet computer, a laptop computer, etc. The electric device usually requires to be lightweight and thin, and a battery cell can be used as a power source.

[0472] Example

[0473] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0474] Example 1 Preparation of lithium-ion battery

[0475] (1) Preparation of positive electrode sheet:

[0476] The positive electrode active material LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), conductive agent carbon black, binder polyvinylidene fluoride (PVDF) are added to N-methylpyrrolidone (NMP) and mixed to prepare positive electrode slurry. 0.6 Co 0.2 Mn 0.2 The mass ratio of O2 (NCM622), conductive carbon black, and PVDF is 97.5:2:0.5. The positive electrode slurry is coated on the current collector aluminum foil and dried at 85°C before cold pressing. After trimming, cutting, and slitting, it is dried under vacuum at 85°C for 4 hours to produce the positive electrode sheet.

[0477] (2) Preparation of negative electrode sheet:

[0478] The negative electrode slurry was prepared by adding artificial graphite (the negative electrode active material), carbon black (the conductive agent), styrene-butadiene rubber (SBR) (the binder), and sodium carboxymethyl cellulose (CMC) (the thickener) to deionized water at a weight ratio of 94.9:5.5:0.5:0.1 and mixing them evenly. The negative electrode slurry was then coated onto the current collector copper foil and dried at 85°C. The negative electrode sheet was then cold-pressed, trimmed, cut, and slit, and then dried at 120°C under vacuum for 12 hours.

[0479] (3) Preparation of electrolyte:

[0480] In an environment with a water content of less than 10ppm, the non-aqueous organic solvents ethylene carbonate EC and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 3:7 to obtain an electrolyte solvent. Subsequently, the lithium salt LiPF6 and the mixed solvent are mixed to prepare an electrolyte with a lithium salt concentration of 1 mol / L.

[0481] (4) Preparation of isolation membrane

[0482] A 16 μm polyethylene film (PE) is used as a base film of the separator, and a coating is uniformly dotted on the surface of the base film, the coating comprising a swelling polymer.

[0483] (5) Preparation of lithium-ion batteries:

[0484] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive electrode sheet and the negative electrode sheet to serve as an isolation, and then wound to obtain an electrode assembly; the electrode assembly is placed in an outer packaging shell, dried, and then injected with electrolyte, and after vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.

[0485] Example 2

[0486] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the positive electrode sheet of Example 2 was prepared as follows:

[0487] Liquid-holding polymer, positive electrode active material LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), conductive agent carbon black, binder polyvinylidene fluoride (PVDF) are added to N-methylpyrrolidone (NMP) and mixed to form positive electrode slurry. 0.6 Co 0.2 Mn 0.2 The mass ratio of O2 (NCM622), conductive carbon black, and PVDF is 0.2:97.3:2:0.5. The positive electrode slurry is coated on the current collector aluminum foil and dried at 85°C before cold pressing. After trimming, cutting, and slitting, the positive electrode sheet is then dried at 85°C under vacuum for 4 hours.

[0488] The preparation of the negative electrode sheet is as follows:

[0489] The negative electrode slurry was prepared by adding a liquid-retaining polymer, artificial graphite (the negative electrode active material), carbon black (the conductive agent), styrene-butadiene rubber (SBR) (the binder), and sodium carboxymethyl cellulose (CMC) (the thickener) to deionized water at a weight ratio of 2.5:94.9:2:0.5:0.1 and mixing them evenly. The negative electrode slurry was then coated onto the current collector copper foil and dried at 85°C. The negative electrode sheet was then cold-pressed, trimmed, cut, and slit, and then dried at 120°C under vacuum for 12 hours.

[0490] Example 3

[0491] A lithium-ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the monomers of Example 3 were different from those of Example 1. Specifically, the monomers of Example 3 additionally included acrylamide, and the molar percentage of acrylamide was 1%.

[0492] Example 4

[0493] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the negative electrode sheet of Example 4 was prepared as follows:

[0494] The negative electrode slurry was prepared by adding a liquid-retaining polymer, artificial graphite (the negative electrode active material), carbon black (the conductive agent), styrene-butadiene rubber (SBR) (the binder), and sodium carboxymethyl cellulose (CMC) (the thickener) to deionized water at a weight ratio of 2.5:94.9:2:0.5:0.1 and mixing them evenly. The negative electrode slurry was then coated onto the current collector copper foil and dried at 85°C. The negative electrode sheet was then cold-pressed, trimmed, cut, and slit, and then dried at 120°C under vacuum for 12 hours.

[0495] Example 5

[0496] A lithium-ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the isolation membrane of Example 5 was prepared as follows:

[0497] A 16 μm polyethylene film (PE) is used as a base film of the separator, and a coating having a plurality of stripe structures is uniformly and spaced apart on the surface of the base film, wherein the coating comprises a swelling polymer.

[0498] Example 6

[0499] A lithium-ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the isolation membrane of Example 5 was prepared as follows:

[0500] Vinylidene fluoride (VDF) and perfluoropropylene (HFP) are used as main materials, with the molar ratio of VDF to HFP being 90%:10%. A bubble-shaped isolation membrane is prepared through a phase inversion method.

[0501] Example 7

[0502] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, a groove (second recessed area) was provided on the surface of the positive electrode sheet of Example 7. The preparation method of the positive electrode sheet was as follows:

[0503] The positive electrode active material LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), conductive agent carbon black, binder polyvinylidene fluoride (PVDF) are added to N-methylpyrrolidone (NMP) and mixed to prepare positive electrode slurry. 0.6 Co 0.2 Mn 0.2 The mass ratio of O2 (NCM622), conductive carbon black, and PVDF is 97.5:2:0.5. The positive electrode slurry is coated on the current collector aluminum foil and dried at 85°C before cold pressing to form the positive electrode film. The positive electrode film is partially rolled to form grooves. After trimming, cutting, and slitting, it is dried under vacuum conditions at 85°C for 4 hours to form the positive electrode sheet.

[0504] Example 8

[0505] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, a groove (second recessed area) was provided on the surface of the negative electrode plate of Example 8. The preparation method of the negative electrode plate was as follows:

[0506] The negative electrode slurry is prepared by adding artificial graphite (the negative electrode active material), carbon black (the conductive agent), styrene-butadiene rubber (SBR) (the binder), and sodium carboxymethyl cellulose (CMC) (the thickener) to deionized water at a weight ratio of 94.9:5.5:0.5:0.1 and mixing them evenly. The negative electrode slurry is then coated onto a current collector copper foil and dried at 85°C. It is then cold-pressed to form a negative electrode film. The film is then partially rolled to form grooves. After trimming, cutting, and slitting, the negative electrode is dried at 120°C under vacuum for 12 hours to form the negative electrode sheet.

[0507] Comparative Example 1

[0508] A lithium-ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the material of the swelling polymer was replaced in Comparative Example 1. In Comparative Example 1, a 16 μm polyethylene film (PE) was used as the base film of the isolation membrane, and a coating was uniformly applied in dots on the surface of the base film. The coating included polyvinylidene fluoride (VDF as a monomer).

[0509] Test section

[0510] 1. Battery cell capacity retention test

[0511] Taking Example 1 as an example, the battery capacity retention rate test process is as follows: The corresponding lithium-ion battery of Example 1 is charged to 4.25V at an equivalent current of 1C at 45°C, then charged at a constant voltage of 4.25V to a current of 0.05C, left for 5 minutes, and then discharged at 1C to 2.8V. The resulting capacity is recorded as the initial capacity C0. The above steps are repeated for the same battery, and the battery discharge capacity Cn after the nth cycle is recorded. The battery capacity retention rate after each cycle is Pn = Cn / C0*100%. The 1600 points P1, P2, ..., P1600 are used as the vertical axis and the corresponding cycle number is used as the horizontal axis to obtain a curve of the battery capacity retention rate and cycle number corresponding to the polymer of Example 1.

[0512] During the test, the first cycle corresponds to n=1, the second cycle corresponds to n=2, ..., and the 1600th cycle corresponds to n=1600. The battery capacity retention rate data corresponding to Example 1 in Table 1 is the data measured after 1600 cycles under the above test conditions, that is, the value of P1600.

[0513] The testing procedures of Comparative Example 1 and other embodiments are the same as above.

[0514] 2. Battery cell DC impedance test

[0515] The lithium-ion batteries (NCM622, design voltage 2.8-4.4V, operating voltage 2.8-4.25V) prepared in the Examples and Comparative Examples were charged at 1C constant current to 4.25V at 45°C. They were then charged at 4.25V constant voltage to a current of 0.05C. After 5 minutes, the voltage V1 was recorded. The battery was then discharged at 1C for 30 seconds, and the voltage V2 was recorded. The internal resistance DCR1 of the battery after the first cycle was calculated as (V2-V1) / 1 / 3C. The above steps were repeated for the same battery, and the internal resistance DCRn of the battery after the nth cycle (n=1, 2, 3, ..., 1600) was recorded. The 1600 points (DCR1, DCR2, DCR3, ..., DCR1200) were plotted as the ordinate, and the corresponding cycle number as the abscissa, to produce a graph of the discharge DCIR of the batteries corresponding to the ester polymers in the Examples and Comparative Examples versus the cycle number.

[0516] During this test, the first cycle corresponds to n=1, the second cycle corresponds to n=2, ..., and the 1600th cycle corresponds to n=1200. For example, the internal resistance increase ratio of the battery of Example 1 in Table 1 = (DCRn-DCR1) / DCR1*100%. The test procedures for Comparative Example 1 and other examples are the same as above.

[0517] The data in Table 3 were measured after 1600 cycles under the above test conditions.

[0518] Test results

[0519] The test results are shown in Tables 1 to 3.

[0520] Table 1

[0521] In Table 1, the compression rate of 25%@1.25 MPa indicates that the compression rate of the separator is 25% at 1.25 MPa.

[0522] 90% vinylidene fluoride + 10% hexafluoropropylene in the monomer means that, based on the total mass of the monomer, the mass content of vinylidene fluoride is 90% and the mass content of hexafluoropropylene is 10%.

[0523] The amount of the liquid-retaining polymer added to the positive electrode sheet is 0.2%, which means that the mass content of the liquid-retaining polymer is 0.2% based on the total mass of the positive electrode film layer.

[0524] The amount of the liquid-retaining polymer added to the positive electrode sheet is 0.0%, indicating that no liquid-retaining polymer is added to the positive electrode film layer.

[0525] Table 2

[0526] In Table 2, M1 is the amount of electrolyte measured by the linear frequency sweep vibration test of the battery cell.

[0527] M2 is the amount of electrolyte measured by first performing a linear frequency sweep vibration test on the battery cell and then performing an extrusion test.

[0528] y represents the amount of free electrolyte measured in the battery cell without undergoing a linear frequency sweep vibration test or an extrusion test.

[0529] V 总孔 It is the pore volume of the electrode assembly, that is, the sum of the pore volume V1 of the positive electrode sheet, the pore volume V2 of the negative electrode sheet and the pore volume of the separator.

[0530] The positive electrode groove volume refers to the total volume of the second recessed area set in the positive electrode plate.

[0531] The negative electrode groove volume refers to the total volume of the second recessed area provided in the negative electrode sheet.

[0532] The compression volume of the isolation diaphragm refers to the spatial volume generated by the compression of the isolation diaphragm when it is subjected to a pressure of 1.25 MPa.

[0533] Table 3

[0534] As can be seen from Table 3, the isolation membrane of Comparative Example 1 does not add a swelling polymer. During the cycle of the lithium-ion battery, due to the volume change of the lithium-ion battery, the electrolyte in the electrode assembly may be squeezed out, causing a liquid shortage problem, thereby increasing the risk of lithium dendrites and deteriorating the reliability and cycle performance of the lithium-ion battery.

[0535] The embodiment of the present application adds a swelling polymer to the isolation membrane. The swelling polymer can lock the electrolyte and release the electrolyte during the charge and discharge process, thereby improving the liquid retention capacity of the electrode assembly and the wettability of the electrolyte to the electrode assembly, thereby improving the reliability and cycle performance of the lithium-ion battery.

[0536] Furthermore, adding a liquid-retaining polymer to at least one of the positive electrode sheet and the negative electrode sheet can further improve the reliability and cycle performance of the lithium-ion battery.

[0537] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions, and modifications may be made to the embodiments without departing from the spirit, principles, and scope of the present application.

Claims

1. A separator, comprising two surfaces opposite to each other along its own thickness direction, at least one of the surface of the separator and the interior of the separator comprising a pore structure, and the separator further comprising a swelling polymer; The isolation film satisfies: when a pressure of 1.25 MPa is applied along the thickness direction of the isolation film, the compression rate ΔV of the isolation film is ≤25%.

2. The isolation film according to claim 1, wherein: At least one surface of the isolation film includes a pore structure, and the pore structure includes a first recessed area.

3. The isolation film according to claim 1 or 2, wherein: The isolation film also satisfies: Take an isolation film with an area of ​​5cm×10cm and record its mass ms1 in g; The separator is immersed in excess electrolyte at 25°C for 7 days, then taken out and placed vertically until there is no droplet for 5 minutes, and its mass ms2 is recorded in g. Then, ((ms2-ms1) / ms1)×100%≥10%.

4. The separator according to any one of claims 1 to 3, wherein: The swelling ratio of the swelling polymer is ≥100%.

5. The separator according to any one of claims 1 to 4, wherein: The compression modulus of the isolation film is ≥45 MPa.

6. The separator according to any one of claims 1 to 5, wherein: The separator includes a first porous base film including the swollen polymer.

7. The isolation film according to claim 6, wherein: The pore structure is arranged inside the first porous base membrane; and / or The surface of the first porous base membrane includes at least one first recessed area.

8. The separator according to any one of claims 1 to 7, wherein: The isolation membrane includes a second porous base membrane and a coating layer disposed on at least one side of the second porous base membrane, wherein the coating layer includes the swelling polymer. The surface of the coating layer facing away from the second porous base membrane includes at least one of the first recessed areas; or The first recessed area is formed between the coating layer and the second porous base film.

9. The separator according to any one of claims 1 to 8, wherein: The swelling polymer includes at least one of a first fluorinated polymer, a first ester polymer, and a first ether polymer. 10 . A battery cell comprising an electrode assembly and an electrolyte, wherein the electrode assembly comprises the separator according to claim 1 .

11. The battery cell according to claim 10, wherein the battery cell satisfies: V0 / (m / ρ)≥1; In the formula, V0 represents the pore volume and interlayer gap volume in the electrode assembly, and its unit is mL; m represents the difference between the mass of the battery cell before drying and the mass after drying, and its unit is g; ρ represents the density of the electrolyte, and its unit is g / mL.

12. According to the battery cell according to claim 10 or 11, the electrode assembly includes a first pole piece and a second pole piece, the first pole piece and the second pole piece have opposite polarities, the isolation membrane is arranged between the first pole piece and the second pole piece, and the surface of the first pole piece facing the isolation membrane has at least one second recessed area. 13 . The battery cell according to claim 10 , further comprising an electrolyte, wherein the electrolyte is located in the electrode assembly.

14. The battery cell according to any one of claims 10 to 13, wherein: The battery cell satisfies: (m / ρ) / V 总孔 ≥80%; V 总孔 A value representing the pore volume of the electrode assembly, in mL; m represents the difference between the mass of the battery cell before drying and the mass after drying, and its unit is g; ρ represents the numerical value of the density of the electrolyte, and its unit is g / mL.

15. The battery cell according to any one of claims 10 to 14, wherein: The battery cell meets the following requirements: 0≤y / Ah≤15%; y represents the volume of free electrolyte in the battery cell, in mL; Ah represents the value of the nominal capacity of the battery cell, and its unit is Ah.

16. The battery cell according to any one of claims 10 to 15, wherein: The battery cell satisfies: 0≤y / V 总孔 ≤15%; y represents the volume of free electrolyte in the battery cell, in mL; V 总孔 A numerical value representing the pore volume of the electrode assembly, with the unit being mL.

17. The battery cell according to any one of claims 10 to 16, wherein: After the linear frequency sweep vibration test, the battery cell is charged to 100% state of charge SOC, a hole is opened on the battery cell, and the hole is set at the lowest point in the vertical direction, and the volume of the electrolyte flowing out of the battery cell is recorded as M1, 0mL≤M1≤0.5mL; in, The vibration direction of the linear frequency sweep vibration test is: single vibration up and down; The vibration frequency of the linear sweep vibration test is: 10Hz~55Hz; The maximum acceleration of the linear sweep vibration test is: 30m / s 2 ; The number of sweep frequency cycles of the linear sweep frequency vibration test is: 10 times; The vibration time of the linear frequency sweep vibration test is 3h.

18. The battery cell according to any one of claims 10 to 17, wherein: After the linear frequency sweep vibration test, the battery cell is charged to 100% state of charge SOC, a hole is opened on the battery cell, and the hole is set at the lowest point in the vertical direction, and the volume of the electrolyte flowing out of the battery cell is recorded as M1, and M1 is 0 mL.

19. The battery cell according to claim 18, wherein: After the battery cell is subjected to the linear frequency sweep vibration test, the electrode assembly is taken out. After the electrode assembly is subjected to the extrusion test, the volume of the electrolyte flowing out of the electrode assembly is recorded as M2, 0 mL ≤ M2 ≤ 0.5 mL; in, The extrusion direction of the extrusion test is: perpendicular to the thickness direction of the electrode assembly; The extrusion degree of the extrusion test is: the extrusion pressure is 0.35 MPa.

20. The battery cell according to claim 19, wherein: After the battery cell is subjected to the linear frequency sweep vibration test, the electrode assembly is taken out. After the electrode assembly is subjected to the extrusion test, the volume of the electrolyte flowing out of the electrode assembly is recorded as M2, and M2 is 0 mL.

21. A battery comprising the battery cell according to any one of claims 1 to 20.

22. An electrical device comprising the battery as claimed in claim 21.

Citation Information

Patent Citations

  • Isolating membrane, lithium ion battery, battery module, battery pack and electric device

    CN115566361A

  • Battery module, battery cell, secondary battery, and electric device

    CN115810873A

  • Separator, preparation method therefor and related secondary battery thereof, battery module, battery pack and device

    WO2022110224A1

  • Isolation membrane, secondary battery comprising same, and related battery module, battery pack and device

    WO2022110225A1

  • Separator, preparation method therefor, and secondary battery, battery module, battery pack and device related thereto

    WO2022110226A1

Cited By

  • Battery cell manufacturing method, end cap assembly, battery cell and battery device

    CN119833701A