Printed plate with three-dimensional wood grain effect on patterned surface, and preparation method therefor
By adding pre-processing and post-processing steps to 3D printing sheet technology, the problem of unclean removal of the embossed layer is solved, delicate and natural textures and clear 3D patterns are achieved, and the beauty and touch of stone plastic flooring are improved.
Patent Information
- Application Number
- PCT/CN2024/086763
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-24
AI Technical Summary
It is difficult to remove the embossed layer with the existing 3D printing plate technology, resulting in the three-dimensional wood grain structure on the surface of the stone plastic floor being not delicate and natural enough, the 3D pattern being unclear, the visual decoration effect being poor, and the touch feeling unreal.
Add a pre-treatment step to solidify the resin liquid on the surface of the wood grain bottom layer and then apply a pre-treatment agent to reduce the hardness and viscosity of the embossed layer, improve the steel brush scraping effect, and add a post-treatment step after removal to remove the residual resin Liquid, forming a more natural wood grain edge and an accurate three-dimensional wood grain structure.
The surface texture of the pattern layer is delicate and natural, the 3D pattern is clear, the visual decoration effect is good, the wood grain edges are sharp, and the touch is real, which improves the aesthetics and quality of the product.
Smart Images

Figure CN2024086763_24102024_PF_FP_ABST
Abstract
Description
A printing plate with a pattern surface having a three-dimensional wood grain effect and a preparation method thereof Technical Field
[0001] The present invention belongs to the technical field of 3D printing plates, and particularly relates to a printing plate with a pattern surface having a three-dimensional wood grain effect and a preparation method thereof. Background Art
[0002] Wood flooring primarily includes solid wood flooring, laminate flooring, and engineered wood flooring. Solid wood flooring has a natural grain, offering a natural, soft, and inviting feel. It's also warm in winter and cool in summer, and pleasant to the touch. However, using large quantities of solid wood flooring consumes a lot of wood, resulting in high costs and potentially causing serious damage to the environment. Engineered wood flooring, made by interlacing and laminating planks of different tree species, overcomes the shortcomings of solid wood flooring, which tends to swell and shrink when wet, offering lower shrinkage and better dimensional stability. It also retains the natural wood grain and comfortable feel of solid wood flooring. However, engineered wood flooring has a complex structure and requires sophisticated production processes. Furthermore, its grain pattern is not wear-resistant and easily fades. Water damage is irreparable, resulting in high costs. Furthermore, the production of engineered wood flooring requires glue, which can easily release harmful gases such as formaldehyde, posing potential health risks.
[0003] Laminate flooring is made of one or more layers of specialized paper impregnated with thermosetting amino resin, applied to the surface of a wood-based panel such as particleboard or high-density fiberboard. A balanced moisture-proof layer is added to the back, and a wear-resistant and decorative layer is added to the front. The flooring is then hot-pressed and formed. Laminate flooring offers excellent resistance to pollution, corrosion, compression, wear, impact, and flame retardancy, as well as good stability, ease of care, and low cost. Laminate flooring is typically decorated by affixing printed paper to its surface, but this paper can easily fall off and become damaged, and the texture lacks fidelity, resulting in poor simulation and decorative effects. The affixed wear-resistant paper can easily become detached from the flooring substrate due to footsteps and vibrations during use, reducing the wood floor's service life and diminishing its quality and grade.
[0004] With the advancement of science and technology, plastics are increasingly being used in our daily lives. SPC flooring, primarily made of PVC, is gaining popularity among consumers. SPC flooring (stone plastic composite), also known as stone plastic flooring (its formal name should be "PVC sheet flooring"), is a high-quality, high-tech, new flooring material developed through research and development. It utilizes a high-density, high-fiber mesh structure to create a solid base layer of stone powder, covered with a special, technologically processed, transparent, high-molecular-weight PVC wear-resistant layer for exceptional wear resistance. SPC flooring is environmentally friendly and typically installed using a snap-on installation method. It avoids the use of formaldehyde-containing adhesives, making it non-toxic, harmless, and non-radioactive. It is a recyclable, environmentally friendly product. SPC flooring is a popular product in Europe, America, Japan, and South Korea, and has become a global phenomenon. After entering the Chinese market, it has gained widespread acceptance and popularity. SPC flooring is widely used in a variety of settings, including homes, hospitals with high traffic, high-speed rail stations, office buildings, factories, supermarkets, shopping malls, and stadiums, and is increasingly popular. Furthermore, stone plastic flooring is waterproof and moisture-resistant, retaining its shape when exposed to water. Furthermore, its flame retardant insulation, acid and alkali corrosion resistance, and high safety have led to its rapid growth in mainstream markets both domestically and internationally in recent years. Stone plastic flooring is a new type of flooring material widely used worldwide, enjoying widespread popularity in Europe, the US, and the Asia-Pacific markets. It is also very popular in China, with promising prospects for further development.
[0005] With the exception of solid wood floors, which have a natural grain, all other types of flooring require a printed pattern on the substrate, followed by a surface treatment such as varnishing to achieve wear and scratch resistance. However, the surface decorative wood grain achieved through this method is a flat pattern, lacking the visual impact of real wood grain. Furthermore, the texture of this decorative wood grain is rough and unnoticeable, appearing rigid and lacking the sense of wood. Therefore, when reproducing the texture of wood on a stone-plastic flooring substrate (i.e., SPC substrate), in addition to reproducing the flat color pattern, it is also necessary to reproduce a three-dimensional wood grain structure with a rich, concave and convex feel on the SPC substrate surface. This creates a three-dimensional wood grain decorative effect that more closely resembles the feel of natural wood, further resulting in a stone-plastic floor with a fine, realistic, tactile, comfortable, and three-dimensional wood texture.
[0006] In order to obtain natural, delicate wood grain and patterns to enhance visual aesthetics, traditional 3D printing board technology uses veneer and other film layers laminated to the surface of the substrate to simulate the wood grain effect through the laminated veneer and other film layers, thereby replacing solid wood floors to a certain extent. For example, patent CN107740554 provides a solid wood stone plastic floor and a preparation method thereof. The solid wood stone plastic floor comprises a stone plastic substrate layer and a solid wood epidermis layer. The solid wood epidermis layer is bonded to the stone plastic substrate layer with hot melt adhesive, making the product look very natural. The overall structure is similar to that of solid wood flooring, while having the fragrance of real wood and being more environmentally friendly. Because the solid wood epidermis layer is only a thin layer on the surface of the stone plastic floor, and the solid wood epidermis layer is easily warped and deformed when it becomes damp or loses water, the defective rate during the production and processing of the stone plastic floor is too high. For example, patent CN111231437B discloses an indoor flooring product based on a polyolefin-biomass composite material and its production process. This flooring utilizes a core material made from polyolefin and biomass materials, which is then laminated with a veneer. Because the veneer itself has wood grain and a certain thickness, the overall product possesses a strong woody feel. However, rare veneer materials are often in short supply and are expensive, presenting significant limitations in flooring production.
[0007] Existing 3D printing sheet technology uses a flatbed inkjet printer to print a flat color pattern on a substrate. Based on the desired texture effect, a transparent / translucent ink / lacquer layer is then sprayed on specific locations. After curing, the desired 3D pattern with a three-dimensional wood grain structure is obtained. For example, patent CN112739463A provides a method for creating a three-dimensional surface on a substrate. This method first coats the substrate with a layer of resin A. Then, while resin A is liquid or partially cured, liquid B is sprayed on resin A in the areas where the concave-convex 3D structure is desired. Resin A and liquid B are then polymerized separately. The polymerized liquid B is then mechanically removed to produce a 3D textured surface formed by liquid B on resin A. Mechanical removal methods include brushing with a steel brush. For example, patent CN110773403A provides a 3D-printed sheet material with a brushed surface. The production steps include: roller-coating an adhesive primer and drying; roller-coating a white primer and drying; roller-coating a transition layer and drying; printing color; roller-coating a wear-resistant layer and drying; 3D printing the texture; brushing; and UV topcoat and drying. The brushed surface effect is achieved by using a wood grain brushing machine to brush the uncured areas of the sheet material.
[0008] However, during the development of the manufacturing process for SPC flooring with 3D wood textures, researchers discovered that applying a resin liquid onto the printed flat pattern layer, then spraying and curing the embossing liquid used to create the three-dimensional wood grain structure on the SPC pattern layer using digital printing technology, and then mechanically removing the embossing layer (e.g., scraping with a steel brush roller / belt) was difficult and incomplete. The embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid remained and deposited in the concave or convex areas of the three-dimensional wood grain layer. This resulted in a three-dimensional wood grain structure on the SPC flooring surface that differed significantly from real wood grain, felt flatter to the touch, had less distinct concavities and convexities, and lacked sharp edges, resulting in an unrealistic feel. Furthermore, the three-dimensional wood grain on the SPC flooring surface lacked a delicate and natural texture, the 3D pattern was unclear, and the visual decorative effect was poor, seriously affecting the aesthetics of the SPC flooring with 3D wood textures.
[0009] Therefore, researchers hope to find a new method to completely remove the embossed layer to obtain a 3D wood texture stone plastic floor with a delicate and natural three-dimensional wood grain structure, a realistic touch, a clear 3D pattern, and a good decorative effect. This method is efficient, easy to operate, and has a low application cost. However, this problem has not yet been solved. Summary of the Invention
[0010] The present invention aims to overcome the defects in the prior art of preparing stone-plastic flooring with 3D wood texture, in which it is difficult to remove the embossed layer mechanically, which easily leads to the three-dimensional wood grain texture on the surface of the stone-plastic flooring being not delicate and natural, the 3D pattern being unclear, the visual decorative effect being poor, and the tactile feeling being unreal. The present invention provides a printed plate with a three-dimensional wood grain effect on the pattern surface and a preparation method thereof.
[0011] According to one aspect of the present invention, the applicant provides a method for generating three-dimensional wood grain on a pattern surface by adding a pretreatment step.
[0012] According to the first aspect, in order to achieve the above-mentioned object of the invention, the present invention is implemented through the following technical solutions:
[0013] The method for generating three-dimensional wood grain on a pattern surface comprises the following steps:
[0014] (1) a step of covering at least a portion of the surface of the pattern layer with a resin liquid;
[0015] (2) a step of solidifying at least a portion of the resin liquid on the surface of the pattern layer to form a wood grain bottom layer;
[0016] (3) a step of covering at least a portion of the surface of the wood grain bottom layer with at least one layer of resin liquid;
[0017] (4) applying embossing liquid to at least a portion of the surface of the resin liquid on the wood grain bottom surface along the color pattern, so that the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid form an embossing layer;
[0018] (5) a step of solidifying the resin liquid except for the embossed layer formed in the previous step;
[0019] (6) further comprising a pre-treatment step of causing the embossed layer to be infiltrated with a pre-treatment agent;
[0020] (7) A step of removing the embossed layer to form a three-dimensional wood grain layer on the surface of the wood grain base layer.
[0021] Preferably, in step (3), at least a portion of the surface of the wood grain bottom layer is covered with at least two layers of resin liquid.
[0022] Preferably, the embossing liquid in step (4) is applied to the surface of the resin liquid and / or penetrates downward into the interior of the resin liquid.
[0023] Preferably, the surface tension of the embossing liquid in step (4) is higher than that of the resin liquid.
[0024] Preferably, the embossing liquid in step (4) comprises at least a curable resin.
[0025] Preferably, the curable resin contained in the embossing liquid has a surface energy lower than the surface energy of the three-dimensional wood grain layer after curing.
[0026] Preferably, the curable resin contained in the embossing liquid includes any one of fluorocarbon resin, fluorosilicone resin or silicone resin.
[0027] Preferably, the density of the embossing liquid is greater than the density of the resin liquid.
[0028] Preferably, the embossing liquid further comprises a density regulator for adjusting the density of the embossing liquid.
[0029] Preferably, the density regulator is an inorganic solid powder additive.
[0030] Preferably, the embossing liquid comprises at least two embossing liquids with different surface tensions.
[0031] Preferably, the step (6) further comprises the step of applying a pre-treatment agent to the embossed layer.
[0032] Preferably, the pretreatment agent includes at least an organic solvent.
[0033] Preferably, the organic solvent includes any one or more combinations of halogenated hydrocarbons, ketones, aromatic hydrocarbons, acrylates, alcohols, and ethers.
[0034] Preferably, the organic solvent includes any one or more combinations of dichloromethane, bromopropane, trichloroethane, acetone, toluene, methanol, ethanol, ether, and chloroform.
[0035] Preferably, the pretreatment agent further comprises a resin monomer.
[0036] Preferably, the resin monomer is any one of an acrylic monomer and an epoxy monomer, or a combination of the two.
[0037] Preferably, the application amount of the pretreatment agent is 1~5g / m2.
[0038] Preferably, the pretreatment process in step (6) further includes a step of bringing the surface of the embossed layer into contact with a brush roller.
[0039] Preferably, the pretreatment process in step (6) further includes a transition treatment step for allowing the pretreatment agent to penetrate into the embossed layer after the pretreatment agent is applied to the embossed layer, and the embossed layer is removed after the transition treatment step is completed.
[0040] As a further preference, during the transition treatment process in which the pretreatment agent penetrates into the embossed layer, the hardness of the embossed layer decreases.
[0041] As a further preference, during the transition process in which the pretreatment agent penetrates into the embossed layer, the viscosity of the embossed layer decreases.
[0042] Preferably, after the embossed layer in step (7) is removed, a post-processing step is further included, and the post-processing step includes a step of applying a post-processing agent to the surface of the three-dimensional wood grain layer.
[0043] Preferably, the post-treatment agent includes at least a volatile organic solvent.
[0044] Preferably, the post-treatment agent further comprises water.
[0045] Preferably, the post-treatment agent further comprises a resin monomer.
[0046] Preferably, the post-treatment agent further comprises a surfactant and / or an emulsifier.
[0047] Preferably, the volatile organic solvent includes any one or more combinations of acetone, ethanol, methanol, N,N-dimethylformamide, and dimethyl sulfoxide.
[0048] Preferably, the application amount of the post-treatment agent is 5~20g / m2.
[0049] Preferably, in the post-processing process after the embossed layer is removed in step (7), a step of increasing the surface temperature of the three-dimensional wood grain layer is also included.
[0050] Preferably, in the post-processing process after the embossed layer is removed in step (7), the surface temperature of the three-dimensional wood grain layer is increased to 40-80°C.
[0051] Preferably, the resin liquid is cured by light curing, heat curing or electron beam curing.
[0052] Preferably, the resin liquid includes at least a photo-crosslinking resin and a photoinitiator.
[0053] Preferably, the embossing liquid in step (4) contains at least a polymerization inhibitor for preventing the polymerization of the photo-crosslinking resin.
[0054] Preferably, the photo-crosslinking resin includes any one or more combinations of unsaturated polyester, epoxy resin, acrylic resin, acrylic modified polyurethane resin, acrylic modified silicone resin, acrylic modified epoxy resin, water-based epoxy acrylate, water-based polyurethane acrylate, and water-based polyester acrylate.
[0055] Preferably, the photoinitiator includes any one of a free radical polymerization initiator, a cationic polymerization initiator, an energy transfer initiator, and an ion reaction initiator.
[0056] Preferably, the resin liquid at least includes a thermosetting resin.
[0057] Preferably, the thermosetting resin includes one or more combinations of epoxy resin, phenolic resin, melamine formaldehyde resin, furan resin, unsaturated polyester resin, silicone resin, and polybutadiene resin.
[0058] Preferably, the resin solution further comprises a curing agent for catalyzing the curing of the thermosetting resin.
[0059] According to another aspect of the present invention, the applicant provides a printed board with a three-dimensional wood grain effect.
[0060] According to the second aspect, in order to achieve the above-mentioned object of the invention, the present invention is implemented through the following technical solutions:
[0061] A printed board with a three-dimensional wood grain effect,
[0062] including substrates;
[0063] The surface of the substrate includes a wood grain base layer and a three-dimensional wood grain layer prepared by the method described above.
[0064] Preferably, the following are arranged in sequence between the substrate and the wood grain bottom layer:
[0065] A primer layer used to improve the bonding properties of the printed board surface;
[0066] A color paint layer provided on the surface of the primer layer to cover the color of the substrate;
[0067] The pattern layer is located on the surface of the color paint layer and is used to form a wood grain pattern.
[0068] Preferably, the outer surface of the three-dimensional wood grain layer is further covered with a topcoat layer, and at least a portion of the topcoat layer is lower than the upper surface of the three-dimensional wood grain layer.
[0069] According to another aspect of the present invention, the applicant provides a method for preparing a printed board having a three-dimensional wood grain effect.
[0070] According to the third aspect, in order to achieve the above-mentioned purpose of the invention, the present invention is implemented through the following technical solutions:
[0071] A method for preparing a printed board having a three-dimensional wood grain effect as described above,
[0072] The method at least comprises the steps of preparing a wood grain base layer and a three-dimensional wood grain layer according to the method described above.
[0073] According to another aspect of the present invention, the applicant provides an application method of a printed board with a three-dimensional wood grain effect.
[0074] According to the fourth aspect, in order to achieve the above-mentioned purpose of the invention, the present invention is implemented through the following technical solutions:
[0075] The printed board with three-dimensional wood grain effect as described above is used in flooring, decorative wall panels or ceiling panels.
[0076] Therefore, the present invention has the following beneficial effects:
[0077] (1) The present invention adds a pretreatment step so that the resin liquid on the surface of the wood grain bottom layer is solidified, and the hardness and / or viscosity of the embossed layer is reduced, which effectively improves the problem of the steel brush roller not scraping the embossed layer cleanly, thereby achieving a three-dimensional wood grain structure with fine and natural texture, clear 3D pattern, good visual decorative effect, realistic touch, sharp wood grain edges, and accurate pattern alignment on the surface of the color pattern layer;
[0078] (2) The present invention adds a post-processing step after the embossing layer is removed, thereby effectively removing the residual embossing liquid and / or a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid, and further obtaining a stone-plastic floor with a 3D wood texture and sharp wood grain edges and accurate patterns, thereby improving product quality and enhancing aesthetics. BRIEF DESCRIPTION OF THE DRAWINGS
[0079] FIG1 is a schematic representation of steps (1)-(7) of the method of the present invention.
[0080] Figure 2 is a schematic reproduction diagram of steps (S.9)-(S.12) in Example 9 of the present invention. DETAILED DESCRIPTION
[0081] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only a portion of the embodiments of the present invention, rather than all of the embodiments. Therefore, all other embodiments derived by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0082] According to one aspect of the present invention, the applicant provides a method for generating three-dimensional wood grain on a pattern surface by adding a pretreatment step.
[0083] As shown in FIG1 , according to the first aspect, in order to achieve the above-mentioned object of the invention, the present invention is implemented by the following technical solutions:
[0084] The method for generating three-dimensional wood grain on a pattern surface comprises the following steps:
[0085] (1) a step of covering at least a portion of the surface of the pattern layer with a resin liquid;
[0086] (2) a step of solidifying at least a portion of the resin liquid on the surface of the pattern layer to form a wood grain bottom layer;
[0087] (3) a step of covering at least a portion of the surface of the wood grain bottom layer with at least one layer of resin liquid;
[0088] (4) applying embossing liquid to at least a portion of the surface of the resin liquid on the wood grain bottom surface along the color pattern, so that the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid form an embossing layer;
[0089] (5) a step of solidifying the resin liquid except for the embossed layer formed in the previous step;
[0090] (6) further comprising a pre-treatment step of causing the embossed layer to be infiltrated with a pre-treatment agent;
[0091] (7) A step of removing the embossed layer to form a three-dimensional wood grain layer on the surface of the wood grain base layer.
[0092] During the development of a production process for SPC flooring with a 3D wood texture, after repeated experiments, the applicant discovered that applying an embossing liquid to at least a portion of the surface of the resin liquid on the wood grain base layer of the SPC flooring, along the color pattern, creates an embossed layer, thereby creating a three-dimensional wood grain structure on the patterned layer of the SPC flooring. The embossed layer is mixed with a partially curable resin liquid containing additives such as a photoinitiator, curing agent, leveling agent, wetting agent, slip agent, and rheology modifier. Over time, these additives will gradually precipitate, causing the composition of the embossed layer to change. When the embossed layer is not fully cured (uncured and / or partially cured), it appears as a viscous liquid. Rapid evaporation of the solvent in the embossed layer can easily increase the viscosity of the embossed layer, which in turn increases its surface tension. This increases the resistance of the embossed layer to the steel brush, further complicating mechanical scraping. At the same time, the embossed layer adheres to the remaining portion of the steel brush roller, forming a gel-like structure. The gel-like embossed layer has a high adhesion force, forming layers of sludge-like attachments that adhere to the steel brush roller. This covers the surface of the steel brush with sludge-like attachments, making it difficult to contact and thoroughly scrape the embossed layer. Furthermore, over time, as the amount of embossed layer adheres to the raised portions of the steel brush roller's surface gradually increases, once the solvent in the embossed layer evaporates completely, the large amount of embossed layer adhered to the steel brush roller crusts and dries, significantly increasing its adhesion, making the steel brush roller's surface increasingly smooth, further increasing the difficulty of scraping the embossed layer with the steel brush. Furthermore, when the embossed layer is fully solidified, it takes on a hard, solid state. Because the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid form long-chain molecules during solidification, these long-chain molecules are interconnected by chemical bonds or physical forces, forming a hard, dense, and high-strength polymer network structure. This network structure gives the surface of the embossed layer good mechanical strength and stability, so that it can resist external forces such as friction, wear, and scraping, making it difficult to clean the embossed layer by mechanical scraping.
[0093] Therefore, the applicant innovatively adds a pretreatment step, so that after the resin liquid on the surface of the wood grain base layer except for the formed embossed layer is cured, a pretreatment agent is applied on the surface of the embossed layer, so that the pretreatment agent penetrates into the interior of the embossed layer.
[0094] When the embossed layer is not fully cured (uncured and / or partially cured), it has high adhesion and appears as a viscous liquid. After the pretreatment agent penetrates the embossed layer, it can interact with unreacted monomers, oligomers, and other organic matter in the uncured (uncured and / or partially cured) embossed layer through physical or chemical adsorption. This weakens the interaction between the molecular chains of the embossed layer and increases the distance between molecules, causing the unreacted monomers, oligomers, and other organic matter to disperse and dissolve, effectively reducing the viscosity of the embossed layer. Simultaneously, the pretreatment agent also interacts with the crosslinking additives mixed in the embossed layer, loosening the crosslinked network structure formed in the embossed layer, increasing its fluidity, reducing the surface tension of the embossed layer, and preventing it from adhering to the steel brush roller. This further effectively improves the problem of the steel brush roller not being able to clean the embossed layer properly.
[0095] When the embossed layer is completely solidified, it takes on a relatively hard solid state. After the pretreatment agent penetrates into the interior of the embossed layer, the pores and capillaries in the solidified embossed layer allow the pretreatment agent to penetrate into the interior of the embossed layer, thereby causing the pretreatment agent to interact with the polymer molecules in the embossed layer, changing the molecular arrangement and void structure, causing the embossed layer to soften, further effectively reducing the hardness of the embossed layer surface, and making it easier to be scraped off with a steel brush. In addition, when the pretreatment agent penetrates into the interior of the embossed layer, it can break the non-covalent bonds between the resin and other polymers mixed in the embossed layer and interact with the functional groups in the resin and other polymers, thereby disrupting the interaction force between the polymer molecular chains, increasing the distance between the polymer molecular chains, and causing swelling. This causes the volume of the embossing liquid in the embossing layer and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid to expand, further reducing the viscosity of the embossing layer. This creates a three-dimensional wood grain structure on the surface of the color pattern layer with delicate and natural texture, clear 3D patterns, high pattern resolution, accurate pattern registration, good visual decorative effect, sharp wood grain edges, and real touch.
[0096] In addition, the applicant has added a post-treatment step after the embossing layer is removed, applying a post-treatment agent to the surface of the three-dimensional wood grain layer. This effectively removes residual embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid. This further effectively prevents the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid from being deposited in the depressions or projections of the three-dimensional wood grain layer, thereby forming residue on the surface. This alters the appearance of the three-dimensional wood grain layer, making the projections appear more rounded and the wood grain edges less sharp and less realistic. Concave areas, on the other hand, appear darker and darker, reducing the gloss of the three-dimensional wood grain layer and blurring the texture, affecting the visual effect and further compromising the overall quality and aesthetics of the three-dimensional wood grain layer. This further results in the final wood grain shape not matching the underlying color pattern layer, reducing the product quality of the stone-plastic flooring with a 3D wood texture.
[0097] In a preferred embodiment of the present invention, in step (3), at least a portion of the surface of the wood grain bottom layer is covered with at least two layers of resin liquid.
[0098] In step (3), at least two layers of resin liquid are coated on the surface of the wood grain bottom layer, so that a thicker three-dimensional wood grain layer is formed on the surface of the wood grain bottom layer, which effectively prevents the subsequent use of a steel brush to scrape off the embossed layer, resulting in part of the pattern layer being exposed, and further causing the exposed pattern layer to be easily worn or even peeled off by external forces. In step (3), the surface of the wood grain bottom layer is coated with multiple layers of resin liquid, which can effectively prevent the steel brush from scraping down too deep, causing the wood grain bottom layer to be scratched through, or even damaging the pattern layer below the wood grain bottom layer, causing the 3D pattern to be scratched, the clarity to be reduced, and the decorative effect to be worse. By controlling the amount of resin liquid applied, the embossing depth can be further freely adjusted, making the three-dimensional sense of the three-dimensional wood grain layer stronger.
[0099] In a preferred embodiment of the present invention, the embossing liquid in step (4) is applied to the surface of the resin liquid and / or penetrates downward into the interior of the resin liquid.
[0100] The embossing liquid in step (4) is applied to the surface of the resin liquid and / or penetrates downward into the interior of the resin liquid to form an embossing layer. When the resin liquid is a UV-curable resin liquid, a layer of embossing liquid that can prevent ultraviolet light from penetrating is covered on the surface of the uncured resin liquid, so that the resin liquid below the embossing liquid can remain in a liquid and uncured state, thereby forming an embossing layer. In the subsequent processing process, it is removed by mechanical cleaning (such as scraping with a steel brush) to obtain a highly simulated three-dimensional wood grain layer.
[0101] When the resin liquid is obtained using the principle of free radical polymerization, when the embossing liquid is applied to the surface of the uncured resin liquid or penetrates downward into the uncured resin liquid, the embossing liquid can absorb the free radicals used to polymerize the resin liquid to undergo free radical polymerization and curing, so that the resin liquid in the part containing the embossing liquid can remain in a liquid and uncured state. This part of the uncured resin liquid forms an embossing layer, which is removed by mechanical cleaning (such as scraping with a steel brush) during subsequent processing, thereby obtaining a highly simulated three-dimensional wood grain layer.
[0102] When the embossing liquid penetrates downward into the uncured resin liquid, it squeezes out the uncured resin liquid so that the occupied volume only contains the embossing liquid. The embossing liquid can be polymerizable or non-polymerizable. Finally, the embossing liquid is removed by mechanical cleaning (such as scraping with a steel brush) to obtain a highly simulated three-dimensional wood grain layer.
[0103] In a preferred embodiment of the present invention, the surface tension of the embossing liquid in step (4) is higher than that of the resin liquid.
[0104] The surface tension of the embossing liquid in step (4) is higher than that of the resin liquid, which helps the embossing liquid penetrate into the resin liquid while maintaining the shape of the area covered by the embossing liquid, thereby producing a more complex concave / convex structure. If the surface tension of the embossing liquid is too low relative to the surface tension of the resin liquid, the embossing liquid will easily wet the surface of the resin liquid, resulting in a reduction in the clarity of the final 3D pattern. The more significant the difference in surface tension between the embossing liquid and the resin liquid, the better the corresponding embossing effect.
[0105] In a preferred embodiment of the present invention, the embossing liquid in step (4) comprises at least a curable resin.
[0106] In a preferred embodiment of the present invention, the surface energy of the curable resin contained in the embossing liquid after curing is lower than the surface energy of the three-dimensional wood grain layer.
[0107] In a preferred embodiment of the present invention, the curable resin contained in the embossing liquid includes any one of fluorocarbon resin, fluorosilicone resin or organosilicon resin.
[0108] In another preferred embodiment of the present invention, the curable resin contained in the embossing liquid includes acrylic resin, epoxy resin or other curable resins.
[0109] Through the above arrangement, the adhesion between the curable resin included in the embossing liquid and the three-dimensional wood grain layer is reduced after curing, so that the embossing layer can be easily removed mechanically.
[0110] In a preferred embodiment of the present invention, the density of the embossing liquid is greater than the density of the resin liquid.
[0111] By adjusting the density of the embossing liquid to be greater than that of the resin liquid, the same volume of embossing liquid applied to at least a portion of the surface of the uncured resin liquid has a higher mass. This results in greater kinetic energy when the embossing liquid enters the uncured resin liquid, further increasing the depth of the resulting three-dimensional wood grain layer. Furthermore, the higher-density embossing liquid, once incorporated into the resin liquid, is more likely to quickly penetrate downward into the uncured resin liquid due to its own gravity.
[0112] In a preferred embodiment of the present invention, the embossing liquid further comprises a density regulator for adjusting the density of the embossing liquid.
[0113] In a preferred embodiment of the present invention, the density regulator is an inorganic solid powder additive.
[0114] In another preferred embodiment of the present invention, the density regulator is an inorganic solid additive.
[0115] In a further preferred embodiment of the present invention, the density regulator is any one of calcium carbonate and silicon dioxide or a combination of the two.
[0116] In a preferred embodiment of the present invention, the embossing liquid comprises at least two embossing liquids with different surface tensions.
[0117] In order to make the tactile feel of the three-dimensional wood grain layer closer to the feel of real wood, in addition to controlling the depth of the three-dimensional wood grain structure, it is also necessary to control the width of the three-dimensional wood grain structure. Currently, its width is mainly controlled by the amount of embossing liquid sprayed. Generally, the more embossing liquid sprayed or the larger the individual droplets of embossing liquid, the wider the wood grain gap is, while the less embossing liquid sprayed or the smaller the droplets of embossing liquid, the smaller the width of the wood grain gap formed. In order to form a three-dimensional wood grain structure with a wider width, more embossing liquid needs to be added, but the embossing liquid needs to be removed in the final step, resulting in excessive embossing liquid being wasted. In order to form a three-dimensional wood grain structure with a smaller width, a smaller amount of embossing liquid needs to be added, which can easily lead to the depth of the three-dimensional wood grain structure being too small. At the same time, the precision of the three-dimensional wood grain structure may be insufficient, resulting in unnatural three-dimensional wood grain defects. Therefore, the embossing liquid can include at least two types: embossing liquid for forming a three-dimensional wood grain structure with a larger width and embossing liquid for forming a three-dimensional wood grain structure with a smaller width.
[0118] The reason is that embossing liquid with a lower surface tension spreads more easily on the surface of the resin liquid on the wood grain base surface, and the contact angle between the embossing liquid and the surface of the resin liquid on the wood grain base surface is smaller. Because it can spread over a larger area under the same volume, it can achieve a wider three-dimensional wood grain structure with less embossing liquid. Embossing liquid with a higher surface tension has difficulty spreading on the surface of the resin liquid on the wood grain base surface, and the contact angle between the embossing liquid and the surface of the resin liquid on the wood grain base surface is larger. Under the same volume, the height of the droplet is higher. Therefore, when using a smaller amount of embossing liquid with a higher surface tension, it can achieve a finer and deeper three-dimensional wood grain structure.
[0119] In a preferred embodiment of the present invention, the step (6) further comprises the step of applying a pre-treatment agent to the embossed layer.
[0120] After the resin liquid on the wood-grain base layer, excluding the embossed layer, is cured, a pretreatment agent is applied to the embossed layer. This application allows the pretreatment agent to penetrate the embossed layer. When the embossed layer is not fully cured (uncured or partially cured), it exhibits high adhesion and a viscous liquid appearance. Once the pretreatment agent penetrates the embossed layer, it interacts with unreacted monomers, oligomers, and other organic matter in the uncured (uncured or partially cured) embossed layer through physical or chemical adsorption. This weakens the interactions between the molecular chains and increases the distance between molecules, causing the unreacted monomers, oligomers, and other organic matter to disperse and dissolve, effectively reducing the viscosity of the embossed layer. Simultaneously, the pretreatment agent interacts with the crosslinking additive in the embossed layer, loosening the crosslinked network structure and increasing its fluidity. This reduces the surface tension of the embossed layer, making it less likely to adhere to the steel brush roller, further effectively alleviating the problem of incomplete scraping of the embossed layer by the steel brush roller.
[0121] When the embossed layer is fully solidified, it takes on a relatively hard solid state. After the pretreatment agent penetrates into the interior of the embossed layer, the presence of certain pores and capillaries in the solidified embossed layer allows the pretreatment agent to penetrate into the interior of the embossed layer, thereby causing the pretreatment agent to interact with the polymer molecules in the embossed layer, changing the molecular arrangement and void structure, causing the embossed layer to soften, further effectively reducing the hardness of the embossed layer surface, and making it easier to be scraped off with a steel brush. In addition, when the pretreatment agent penetrates into the interior of the embossed layer, it can break the non-covalent bonds between the resin and other polymers mixed in the embossed layer and interact with the functional groups in the resin and other polymers, thereby disrupting the interaction forces between the polymer molecular chains, increasing the distance between the polymer molecular chains, and causing swelling. This causes the embossing liquid in the embossing layer and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid to expand in volume, protruding outward, making it easier to scrape off mechanically later. This creates a three-dimensional wood grain structure on the surface of the color pattern layer with delicate and natural texture, clear 3D patterns, high pattern resolution, accurate pattern registration, good visual decorative effect, sharp wood grain edges, and a real touch.
[0122] In a preferred embodiment of the present invention, the pretreatment agent at least includes an organic solvent.
[0123] When the embossed layer is not fully cured (uncured or partially cured), it has high adhesion and appears as a viscous liquid. The pretreatment agent contains an organic solvent. After penetrating the embossed layer, the organic solvent can interact with unreacted monomers, oligomers, and other organic matter in the uncured (uncured or partially cured) embossed layer through physical or chemical adsorption. This weakens the interaction between the molecular chains of the unreacted monomers, oligomers, and other organic matter, increases the distance between molecules, and causes the unreacted monomers, oligomers, and other organic matter to disperse, effectively reducing the viscosity of the embossed layer. Simultaneously, the organic solvent also interacts with the crosslinking agent mixed in the embossed layer, loosening the crosslinked network structure formed in the embossed layer, increasing its fluidity, reducing the surface tension of the embossed layer, and preventing it from adhering to the steel brush roller. This further effectively improves the problem of the steel brush roller not being able to clean the embossed layer properly.
[0124] When the embossed layer is completely solidified, it takes on a relatively hard solid state. After the organic solvent penetrates into the interior of the embossed layer, it causes the organic solvent to interact with the polymer molecules in the embossed layer, changing the molecular arrangement and void structure, causing the embossed layer to soften, further effectively reducing the hardness of the embossed layer surface, and making it easier to be scraped off with a steel brush. In addition, when the organic solvent penetrates into the interior of the embossed layer, it can break the non-covalent bonds between the resin and other polymers mixed in the embossed layer, and interact with the functional groups in the resin and other polymers, thereby disrupting the interaction force between the polymer molecular chains, increasing the distance between the polymer molecular chains, and causing swelling. This causes the embossing liquid in the embossed layer and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid to expand in volume and bulge outward, making it easier to scrape off mechanically later. This results in a three-dimensional wood grain structure with fine and natural texture, clear 3D patterns, high pattern resolution, accurate pattern alignment, good visual decorative effect, sharp wood grain edges, and a realistic touch.
[0125] In a preferred embodiment of the present invention, the organic solvent includes any one or more combinations of halogenated hydrocarbons, ketones, aromatic hydrocarbons, esters, alcohols, and ethers.
[0126] Halogenated hydrocarbons, ketones, aromatic hydrocarbons, esters, alcohols, and ethers are polar solvents with excellent solubility and compatibility with the resin, embossing fluid, and resin monomers present in the embossing layer. When these organic solvents penetrate into the uncured (uncured or partially cured) embossing layer, the polar sites in their molecules interact with those in the resin, embossing fluid, and resin monomers present in the embossing layer, forming various forces such as van der Waals forces and hydrogen bonds. This shortens the distance between molecules and creates a stable dissolution system. Furthermore, during the dissolution process, these organic solvents occupy the spaces between small molecule additives, such as the embossing fluid and resin monomers, weakening the mutual attraction between these small molecule additives and enhancing their solubility. Furthermore, organic solvent molecules such as halogenated hydrocarbons, ketones, aromatic hydrocarbons, esters, alcohols, and ethers can enter and intersect with polymer molecules such as resins, allowing them to penetrate the interstices within them. This alters the molecular structure and the interactions between adjacent molecules, further reducing the viscosity and increasing the fluidity of these molecules. This improves the dispersion and fluidity of the resin, embossing fluid, and resin monomers mixed in the embossing layer, reducing its viscosity and preventing adhesion. This effectively prevents the embossing layer from agglomerating and forming a large amount of sludge-like attachments that adhere to the steel brush roller and are difficult to scrape off, further affecting the visual effect of the three-dimensional wood grain layer.
[0127] When organic solvents such as halogenated hydrocarbons, ketones, aromatic hydrocarbons, esters, alcohols, and ethers penetrate into the fully solidified embossed layer, they interact with the resin and other polymer molecules in the embossed layer, changing the arrangement and void structure of the polymer molecules, resulting in a decrease in the polymer's glass transition temperature, further softening the embossed layer, and effectively reducing the hardness of the embossed layer's surface, making it easier to scrape off with a steel brush. Furthermore, when the organic solvent penetrates into the embossed layer, it can break the non-covalent bonds between the resin and other polymers mixed in the embossed layer and interact with the functional groups in the resin and other polymers, thereby disrupting the interaction forces between the polymer molecular chains, increasing the distance between the polymer molecular chains and causing swelling. This causes the embossing liquid in the embossed layer and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid to expand in volume, causing it to bulge outward, facilitating subsequent mechanical scraping. In addition, halogenated hydrocarbons, ketones, aromatic hydrocarbons, esters, alcohols, and ethers have good solubility, which can cause small molecules such as the embossing liquid and resin monomers mixed in the embossing layer to dissolve and diffuse into the solution, causing the embossing liquid, resin monomers, etc. mixed in the embossing layer to disperse from the embossing layer, making it easy to remove them later. In addition, halogenated hydrocarbons, ketones, aromatic hydrocarbons, esters, alcohols, and ethers are liquids at room temperature and pressure, have good fluidity, low viscosity, and strong volatility. After being applied to the embossing layer, they leave little or no residue on the surface of the three-dimensional wood grain layer, effectively avoiding corrosion and damage to the three-dimensional wood grain layer. This achieves a three-dimensional wood grain structure with delicate and natural texture, clear 3D patterns, high pattern resolution, accurate pattern registration, good visual decorative effect, sharp wood grain edges, and a realistic touch on the surface of the pattern layer.
[0128] In a preferred embodiment of the present invention, the organic solvent includes any one or more combinations of dichloromethane, bromopropane, trichloroethane, acetone, toluene, methanol, ethanol, ether, and chloroform.
[0129] In a preferred embodiment of the present invention, the pretreatment agent further comprises a resin monomer.
[0130] In a preferred embodiment of the present invention, the resin monomer is any one of an acrylic monomer and an epoxy monomer, or a combination of both.
[0131] In a preferred embodiment of the present invention, the application amount of the pretreatment agent is 1-5 g / m2.
[0132] When the pretreatment agent dosage is less than 1g / m², the resin, embossing fluid, and resin monomer mixed in the embossed layer have difficulty fully contacting and dissolving with the pretreatment agent. This leads to uneven dispersion of the components in the embossed layer, which can easily cause resin precipitation and poor leveling, resulting in agglomeration and adhesion to the mechanical equipment used to remove the embossed layer. Furthermore, a low dosage of pretreatment agent prolongs the reaction time of the pretreatment step, complicates the process flow, and further reduces production efficiency. When the pretreatment agent dosage exceeds 5g / m², excessive use of the pretreatment agent can easily lead to complete dissolution of the resin, embossing fluid, and resin monomer mixed in the embossed layer, resulting in excessive fluidity and thus disrupting the structure and shape of the three-dimensional wood grain layer. Furthermore, excessive pretreatment agent can penetrate and diffuse downward into the pattern layer below the three-dimensional wood grain layer, causing contamination, blurring, and blurring of the pattern, further compromising the quality of the 3D wood-textured SPC flooring. Furthermore, the pretreatment agent contains volatile and flammable substances, and excessive use may increase the risk of fire and explosion.
[0133] In a preferred embodiment of the present invention, the pretreatment process in step (6) further includes a step of bringing the surface of the embossed layer into contact with a brush roller.
[0134] During the pretreatment process in step (6), the pretreatment agent applied to the surface of the embossed layer is evenly spread by a brush roller so that the pretreatment agent is in full contact with the surface of the embossed layer, thereby facilitating the pretreatment agent to penetrate downward into the embossed layer.
[0135] In a preferred embodiment of the present invention, the pretreatment process in step (6) further includes a transition treatment step for allowing the pretreatment agent to penetrate into the embossed layer after the pretreatment agent is applied to the embossed layer, and the embossed layer is removed after the transition treatment step is completed.
[0136] In a further preferred embodiment of the present invention, the transition treatment step of allowing the pretreatment agent to penetrate into the interior of the embossed layer after the application of the pretreatment agent to the embossed layer is completed may include allowing the embossed layer to stand for a period of time to promote the pretreatment agent to enter the interior of the embossed layer and prolong the time for the pretreatment agent to enter and react with the interior of the embossed layer, thereby allowing the pretreatment agent to penetrate into the interior of the embossed layer more thoroughly and contact more fully.
[0137] In a further preferred embodiment of the present invention, the transition treatment step of allowing the pretreatment agent to penetrate into the interior of the embossed layer after the pretreatment agent is applied to the embossed layer may include adding appropriate surfactants, additives, etc. to the embossed layer, so that the surface of the embossed layer is easier to wet, thereby improving the affinity between its surface and the pretreatment agent, making it easier for the pretreatment agent to penetrate into the interior of the embossed layer.
[0138] In a further preferred embodiment of the present invention, the transition treatment step of allowing the pretreatment agent to penetrate into the interior of the embossed layer after the pretreatment agent is applied to the embossed layer may include increasing the surface temperature of the embossed layer so that the viscosity and surface tension of the embossing liquid, resin liquid, resin monomer, etc. mixed in the embossed layer decrease as the temperature rises, thereby enhancing the permeability of the embossed layer and making it easier for the pretreatment agent to penetrate into the interior of the embossed layer.
[0139] In a preferred embodiment of the present invention, after the embossed layer in step (7) is removed, a post-processing step is further included, and the post-processing step includes the step of applying a post-processing agent to the surface of the three-dimensional wood grain layer.
[0140] By adding a post-treatment step after the embossing layer is removed, a post-treatment agent is applied to the surface of the three-dimensional wood grain layer, effectively removing residual embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid. This further effectively prevents the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid from being deposited in the depressions or projections of the three-dimensional wood grain layer, thereby forming residue on the surface and altering the appearance of the three-dimensional wood grain layer. The projections appear visually more rounded, and the wood grain edges are less sharp and less realistic. Concave areas, on the other hand, appear darker and darker, reducing the gloss of the three-dimensional wood grain layer and blurring the texture, affecting the visual effect and further compromising the overall quality and aesthetics of the three-dimensional wood grain layer. This further results in the final wood grain shape not matching the underlying color pattern layer, reducing the product quality of the stone-plastic flooring with a 3D wood texture.
[0141] In a preferred embodiment of the present invention, the post-treatment agent includes at least a volatile organic solvent.
[0142] The post-treatment agent includes a volatile organic solvent, which quickly dilutes and dissolves the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid, remaining on the surface of the three-dimensional wood grain layer, improving removal efficiency. This also ensures that the surface of the three-dimensional wood grain layer is dry and free of solvent residue, preventing damage to the structure of the three-dimensional wood grain layer and affecting its aesthetic appearance, while providing high safety.
[0143] In a preferred embodiment of the present invention, the post-treatment agent further comprises at least water.
[0144] Water is a good solvent that can dissolve water-soluble dirt. The presence of water in the post-treatment agent helps it to contact and penetrate into the interior of the embossing liquid remaining on the surface of the three-dimensional wood grain layer and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid, thereby improving the removal effect of water-soluble dirt. At the same time, the presence of water in the post-treatment agent can effectively reduce the concentration of the post-treatment agent, further reducing its corrosion to the three-dimensional wood grain layer, and also helping to reduce the cost of the post-treatment agent. In addition, the water in the post-treatment agent, after mixing with the remaining embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid and the volatile organic solvent, will form a stable fluid due to emulsification, which is convenient for subsequent cleaning and discharge by flushing or wiping.
[0145] In a preferred embodiment of the present invention, the post-treatment agent further comprises a resin monomer.
[0146] In a preferred embodiment of the present invention, the post-treatment agent further comprises a surfactant and / or an emulsifier.
[0147] The surfactant can reduce the surface tension between the post-treatment agent and the remaining embossing fluid and / or at least a portion of the resin liquid mixed with the embossing fluid and / or at least a portion of the resin liquid covered by the embossing fluid, allowing the post-treatment agent to fully contact the post-treatment agent, more easily penetrate and dissolve the post-treatment agent, thereby improving its removal efficiency and preventing it from remaining on the surface of the three-dimensional wood grain layer. The surfactant can also act as a dispersant, causing the post-treatment agent to react with the remaining embossing fluid and / or at least a portion of the resin liquid mixed with the embossing fluid and / or at least a portion of the resin liquid covered by the embossing fluid to form a mixed liquid, effectively reducing the viscosity of the resulting mixed liquid and facilitating subsequent cleaning of the mixed liquid by flushing or other methods. The emulsifier can form an emulsion between the remaining embossing fluid and / or at least a portion of the resin liquid mixed with the embossing fluid and / or at least a portion of the resin liquid covered by the embossing fluid and the post-treatment agent, facilitating removal. Furthermore, the emulsifier can prevent the remaining embossing fluid and / or at least a portion of the resin liquid mixed with the embossing fluid and / or at least a portion of the resin liquid covered by the embossing fluid from redepositing on the surface of the three-dimensional wood grain layer.
[0148] In a preferred embodiment of the present invention, the volatile organic solvent includes any one or more combinations of acetone, ethanol, methanol, N,N-dimethylformamide, and dimethyl sulfoxide.
[0149] In a preferred embodiment of the present invention, the application amount of the post-treatment agent is 5-20 g / m2.
[0150] When the amount of post-treatment agent applied is less than 5g / m2, it is likely to cause insufficient reaction with the residual embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid, making it difficult to achieve the removal effect, further affecting the structure and aesthetics of the three-dimensional wood grain layer. At the same time, too little post-treatment agent applied can also lead to unstable and difficult-to-control production processes, extended production cycles, and reduced production efficiency. When the amount of post-treatment agent applied exceeds 20g / m2, the volatile organic solvents in the post-treatment agent evaporate and are released into the environment, which can easily cause environmental pollution. In addition, volatile organic solvents are flammable and explosive. When the amount of post-treatment agent added is too high, it can easily lead to safety hazards such as fire and explosion.
[0151] In a preferred embodiment of the present invention, the post-processing process after the embossed layer is removed in step (7) further includes a step of increasing the surface temperature of the three-dimensional wood grain layer.
[0152] In the post-processing process after the embossing layer is removed in step (7), the surface temperature of the three-dimensional wood grain layer is increased by heating. This can promote the interaction between the molecules of resin, embossing liquid, resin monomer, etc. in the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid on the surface of the three-dimensional wood grain layer and the solvent molecules in the post-processing agent, increase the mutual diffusion rate between the two, and make them more fully dissolved by the solvent, thereby accelerating the process of removing the surface residues of the three-dimensional wood grain layer. In addition, the heating treatment can effectively reduce the viscosity of the residual embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid, so that the solvent molecules in the post-processing agent can more easily penetrate into the molecules of resin, embossing liquid, resin monomer, etc. contained therein, thereby improving the removal efficiency. In addition, the heating treatment increases the solvent evaporation rate and simultaneously dries and removes the post-processing agent, effectively preventing the post-processing agent from remaining on the surface of the three-dimensional wood grain layer.
[0153] In a preferred embodiment of the present invention, during the post-processing process after the embossed layer is removed in step (7), the surface temperature of the three-dimensional wood grain layer is increased to 40-80°C.
[0154] During the post-processing process after the embossing layer is removed in step (7), when the surface temperature of the three-dimensional wood grain layer is too low (lower than 40°C), the volatilization rate and diffusion rate of the volatile organic solvent contained in the post-processing agent are slowed down, making it difficult for the solvent to penetrate into the residual embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid, resulting in insufficient mutual dissolution and poor removal of residues. The post-processing agent may even accumulate on the surface of the three-dimensional wood grain layer, further corroding or destroying the structure of the three-dimensional wood grain layer. When the surface temperature of the three-dimensional wood grain layer is too high (higher than 80°C), the three-dimensional wood grain layer may be easily deformed and cracked due to excessive thermal expansion, and may even cause the pattern of the stone plastic floor with 3D wood texture to change color, thereby affecting the product quality and visual effect of the stone plastic floor with 3D wood texture.
[0155] In a preferred embodiment of the present invention, the curing method of the resin liquid includes any one of light curing, heat curing or electron beam curing.
[0156] In a preferred embodiment of the present invention, the resin liquid at least includes a photo-crosslinking resin and a photoinitiator.
[0157] In a preferred embodiment of the present invention, the embossing liquid in step (4) contains at least a polymerization inhibitor for preventing the polymerization of the photo-crosslinking resin.
[0158] Adding a polymerization inhibitor to the embossing liquid can quench the free radicals generated by the decomposition of the photoinitiator under light, thereby effectively preventing the polymerization of the resin liquid containing the polymerization inhibitor or reducing the curing speed of the resin liquid containing the polymerization inhibitor, so that after the end of step (5), the resin liquid containing the polymerization inhibitor can still remain in a liquid or semi-solid state, thereby making it easier to remove the embossing layer.
[0159] In a preferred embodiment of the present invention, the photo-crosslinking resin includes any one or more combinations of unsaturated polyester, epoxy resin, acrylic resin, acrylic modified polyurethane resin, acrylic modified silicone resin, acrylic modified epoxy resin, water-based epoxy acrylate, water-based polyurethane acrylate, and water-based polyester acrylate.
[0160] In a preferred embodiment of the present invention, the photoinitiator includes any one of a free radical polymerization initiator, a cationic polymerization initiator, an energy transfer initiator, and an ion reaction initiator.
[0161] In a preferred embodiment of the present invention, the resin liquid at least includes a thermosetting resin.
[0162] In a preferred embodiment of the present invention, the thermosetting resin includes one or more combinations of epoxy resin, phenolic resin, melamine formaldehyde resin, furan resin, unsaturated polyester resin, silicone resin, and polybutadiene resin.
[0163] In a preferred embodiment of the present invention, the resin solution further includes a curing agent for catalyzing the curing of the thermosetting resin.
[0164] According to another aspect of the present invention, the applicant provides a printed board with a three-dimensional wood grain effect.
[0165] According to the second aspect, in order to achieve the above-mentioned object of the invention, the present invention is implemented through the following technical solutions:
[0166] A printed board with a three-dimensional wood grain effect,
[0167] including substrates;
[0168] The surface of the substrate includes a wood grain base layer and a three-dimensional wood grain layer prepared by the method described above.
[0169] In a preferred embodiment of the present invention, the following are further provided in sequence between the substrate and the wood grain bottom layer:
[0170] A primer layer used to improve the bonding properties of the printed board surface;
[0171] A color paint layer provided on the surface of the primer layer to cover the color of the substrate;
[0172] The pattern layer is located on the surface of the color paint layer and is used to form a wood grain pattern.
[0173] In a preferred embodiment of the present invention, the outer surface of the three-dimensional wood grain layer is further covered with a topcoat layer, and at least a portion of the topcoat layer is lower than the upper surface of the three-dimensional wood grain layer.
[0174] According to another aspect of the present invention, the applicant provides a method for preparing a printed board having a three-dimensional wood grain effect.
[0175] According to the third aspect, in order to achieve the above-mentioned purpose of the invention, the present invention is implemented through the following technical solutions:
[0176] A method for preparing a printed board having a three-dimensional wood grain effect as described above,
[0177] The method at least comprises the steps of preparing a wood grain bottom layer and a three-dimensional wood grain layer according to the method described above.
[0178] In another preferred embodiment of the present invention, a method for preparing the printed board having the three-dimensional wood grain effect as described above further comprises the following steps:
[0179] The step of covering at least a portion of the surface of the printed plate with a primer and curing the primer layer;
[0180] The step of covering at least a portion of the surface of the primer layer with color paint and curing the primer layer to obtain a color paint layer;
[0181] The step of covering at least a portion of the surface of the color paint layer with ink for forming a wood grain pattern and curing the ink to obtain a pattern layer;
[0182] The step of covering at least a portion of the surface of the pattern layer with the wood grain base layer and the three-dimensional wood grain layer prepared according to the above method;
[0183] The step of covering at least a portion of the surface of the three-dimensional wood grain layer with a topcoat and curing the topcoat layer.
[0184] In a further preferred embodiment of the present invention,
[0185] The coverage of the primer is 10-15 g / m2;
[0186] The coverage of the paint is 15-25 g / m2;
[0187] The coverage of the ink is 6-10 g / m2;
[0188] The coverage of the topcoat is 10~30g / m2.
[0189] In a further preferred embodiment of the present invention, the color paint layer is white.
[0190] In a further preferred embodiment of the present invention, the paint contains at least a photo-crosslinking resin, a photoinitiator and white pigment powder.
[0191] According to another aspect of the present invention, the applicant provides an application method of a printed board with a three-dimensional wood grain effect.
[0192] According to the fourth aspect, in order to achieve the above-mentioned purpose of the invention, the present invention is implemented through the following technical solutions:
[0193] The printed board with three-dimensional wood grain effect as described above is used in flooring, decorative wall panels or ceiling panels.
[0194] Example 1
[0195] The method for generating three-dimensional wood grain on a pattern surface comprises the following steps:
[0196] (S.1) Place an SPC sheet with a length, width and thickness of 1560mm*970mm*4.85mm on the surface of a conveyor moving in a fixed direction;
[0197] (S.2) The SPC sheet in step (S.1) is sequentially passed through a first roller coater and a second roller coater during transportation, so that 12 g / m2 of a primer (wherein the primer comprises: 90% light-curing clear varnish HYS01-1, 5% photoinitiator 184, 0.5% photoinitiator TPO, and 4.5% diluent hydroxyethyl acrylate) and 17 g / m2 of a light-curable white paint (wherein the white paint comprises: 50% light-curing epoxy HYS01-1, 30% titanium dioxide, 5% photoinitiator 184, 0.5% photoinitiator TPO, and 14.5% diluent hydroxyethyl acrylate) are sequentially coated on the surface of the SPC sheet while the SPC sheet is in contact with the coating rollers. The primer is cured using a 395 nm UV lamp and an 8 W / cm2 UV lamp, respectively, to form a primer layer, and a white color paint layer is formed on the surface of the primer layer.
[0198] (S.3) conveying the SPC sheet obtained in step (S.2) to a first inkjet printer, spraying 7 g / m2 of ink on the surface of the color paint layer by the first inkjet printer, and curing the ink to form a pattern layer having a wood grain pattern on the surface of the primer layer;
[0199] (S.4) The SPC sheet obtained in step (S.3) is conveyed to a third roller coater, and 45 g / m2 of a photocurable resin liquid (the resin liquid comprises: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, and 4.5% diluent hydroxyethyl acrylate) is roller-coated on the surface of the pattern layer. The resin liquid is then sequentially irradiated with a 395 nm UV lamp at 8 W / cm2 and a 160 W / cm2 Hg lamp to form a wood grain base layer;
[0200] (S.5) conveying the SPC sheet obtained in step (S.4) to a fourth roller coater, such that the coating roller of the fourth roller coater is rolled along the conveying direction of the SPC sheet (the roller itself rotates in a clockwise direction) to apply 75 g / m2 of a resin solution (the resin solution comprises: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, and 4.5% diluent hydroxyethyl acrylate) to the surface of the wood grain bottom layer;
[0201] (S.6) After applying the first layer of resin liquid, the SPC sheet is conveyed forward along the surface of the conveying equipment, and it is ensured that the fourth roller coater does not apply any force to the resin liquid before conveying it to the next roller coater;
[0202] (S.7) conveying the SPC sheet obtained in step (S.6) to a fifth roller coater, so that the coating roller of the fifth roller coater continues to roll-coat 80 g / m2 of the resin solution in the opposite direction of the SPC sheet conveyance (the roller itself rotates in a clockwise direction);
[0203] (S.8) The SPC sheet obtained in step (S.7) is conveyed to a second inkjet printer, where 8 g / m2 of embossing liquid (the embossing liquid comprises: 45.5% diacrylate monomer PEG600DA, 20.5% p-hydroxyanisole HQMME, 10% 2-tert-butylhydroquinone MTBHQ, and 24% diethylene glycol butyl ether) is sprayed on the surface of the resin liquid, and the embossing liquid is allowed to penetrate downward into the resin liquid and mix with the resin liquid to form an embossed layer;
[0204] (S.9) Deeply curing the resin liquid on the surface of the SPC sheet obtained in step (S.8) except for the embossed layer by sequentially irradiating the surface with a UV lamp of 395 nm and 8 W / cm2 and a Hg lamp of 160 W / cm2;
[0205] (S.10) conveying the SPC sheet obtained in step (S.9) to a sixth roller coater, so that 2 g / m2 of a pretreatment agent (wherein the pretreatment agent comprises 95% ethanol and 5% butyl acrylate) is roller-coated on the surface of the SPC sheet;
[0206] (S.11) conveying the SPC sheet obtained in step (S.10) to a cleaning device including a steel brush, so that the embossed layer is brushed out by the steel brush, thereby forming a three-dimensional wood grain layer;
[0207] (S.12) The SPC sheet obtained in step (S.11) is passed through a seventh roller coater and a UV lamp with a wavelength of 395 nm and 8 W / cm2, thereby coating the surface of the three-dimensional wood grain layer with a first topcoat of 12 g / m2, and curing the first topcoat to obtain a first topcoat layer;
[0208] (S.13) The SPC sheet obtained in step (S.12) is passed through an eighth roller coater and a UV lamp with a wavelength of 395 nm and 8 W / cm2, thereby coating the surface of the first topcoat layer with a second topcoat of 12 g / m2, and curing the second topcoat to obtain a second topcoat layer.
[0209] Example 2
[0210] The difference between this embodiment and embodiment 1 is that the roller coating amount of the pre-treatment agent in step (S.10) is 1 g / m2. The other conditions are the same as those in embodiment 1.
[0211] Example 3
[0212] The difference between this embodiment and embodiment 1 is that the roller coating amount of the pre-treatment agent in step (S.10) is 5 g / m2. The other conditions are the same as those in embodiment 1.
[0213] Example 4
[0214] The difference between this embodiment and embodiment 1 is that the pretreatment agent in step (S.10) contains 95% dichloromethane and 5% butyl acrylate. The other conditions are the same as those in embodiment 1.
[0215] Example 5
[0216] The difference between this embodiment and embodiment 1 is that the pretreatment agent in step (S.10) contains 95% chloroform and 5% butyl acrylate. The other conditions are the same as those in embodiment 1.
[0217] Example 6
[0218] This example differs from Example 1 in that the composition and curing method of the resin solution are modified in steps (S.4) to (S.9). A thermosetting resin system is used, specifically: 100 parts bisphenol A epoxy resin E-51, 30 parts methyltetrahydrophthalic anhydride, 15 parts butyl glycidyl ether (BGE), and 10 parts accelerator DMP30. The resulting thermosetting resin solution is applied to the surface of the SPC sheet. The ambient temperature of the SPC sheet is then raised to 140°C using infrared heating to cure the thermosetting resin solution. All other aspects remain the same as in Example 1.
[0219] Example 7
[0220] This embodiment differs from Example 1 in that, in step (S.8), 8 g / m² of embossing liquid (a polytetrafluoroethylene emulsion with a solids content of 60% and a density of 1.5 g / cm³) is sprayed onto the surface of the resin liquid. The embossing liquid is then allowed to penetrate and mix with the resin liquid, forming an embossed layer. All other steps are the same as in Example 1. Because the polytetrafluoroethylene emulsion is aqueous, it is immiscible with the resin liquid after infiltration. Consequently, after the resin liquid solidifies, some of the water in the polytetrafluoroethylene emulsion evaporates due to heat, forming a polytetrafluoroethylene layer. Due to the low surface energy of the polytetrafluoroethylene layer, it does not adhere to the solidified resin liquid, making it easier to remove.
[0221] Example 8
[0222] This embodiment differs from Example 1 in that the embossing liquid sprayed onto the surface of the resin liquid in step (S.8) is a polytetrafluoroethylene emulsion with a solid content of 60%. Nanosilica is added to the embossing liquid, increasing its density from 1.5 g / cm³ to 2.0 g / cm³. All other aspects are the same as in Example 1.
[0223] Comparative Example 1
[0224] This comparative example differs from Example 1 in that step (S.10) is omitted. That is, steps (S.11), (S.12), and (S.13) are performed directly after step (S.9), thereby eliminating the need for roller coating of the SPC sheet surface with a pretreatment agent. All other aspects are the same as in Example 1.
[0225] Comparative Example 2
[0226] This comparative example differs from Example 1 in that the pretreatment agent in step (S.10) contains ethanol and no butyl acrylate. All other aspects are the same as in Example 1.
[0227] Comparative Example 3
[0228] The difference between this comparative example and Example 1 is that the roller coating amount of the pre-treating agent in step (S.10) is 0.5 g / m2. The other conditions are the same as those in Example 1.
[0229] Comparative Example 4
[0230] The difference between this comparative example and Example 1 is that the roller coating amount of the pre-treating agent in step (S.10) is 6 g / m2. The other conditions are the same as those in Example 1.
[0231]
Product performance test
[0232] According to the methods in Examples 1 to 8 and Comparative Examples 1 to 4 above, 50 printing plates were respectively produced in batches and product performance tests were performed.
[0233] Clarity test: Tested in accordance with standard JIS K7374.
[0234] Wiredrawing Effect Grade Test: 20 assessors visually inspected the printed board surface to assess the sharpness of the wood grain edges. The results were recorded according to a scale, with the highest number of assessors determining the final grade. Visual inspection of the wood grain edges on the printed board surface is divided into five grades. The five grades, along with the scoring and evaluation criteria, are shown in Table 1.
[0235] Table 1 Wood grain edge sharpness level, scoring and standards
[0236]
[0237] Note: From level 1 to level 5, the sharpness of the wood grain edges gradually decreases.
[0238] Registration Accuracy Test: 20 assessors visually inspected the printed plate surface to assess the alignment accuracy. They visually observed the printed plate surface to detect any misalignment. The evaluation results were recorded according to a grade and score. The grade with the highest number of assessors was determined as the final grade for the printed plate. Visual inspection of the printed plate surface is divided into five grades. The five grades, along with the scoring and evaluation criteria, are shown in Table 2.
[0239] Table 2 Wood grain edge alignment accuracy grades, scores, and standards
[0240]
[0241] Note: From level I to level IV, the accuracy of flower matching gradually decreases.
[0242] The performance test results of the printed plates of Examples 1 to 8 and Comparative Examples 1 to 4 are shown in Table 3 below:
[0243] Table 3
[0244]
[0245] Analysis of the data in Table 3 shows that the addition of a pretreatment step, which solidifies the resin liquid on the wood grain base surface, excluding the embossed layer, and then applies a pretreatment agent to the embossed layer, effectively alleviates the problem of the steel brush roller not scraping the embossed layer cleanly. This results in a fine, natural texture on the pattern layer surface, with a pattern clarity of 83.5%, sharp wood grain edges, a brushed effect rating of Level 1, a realistic touch, and a pattern registration accuracy rating of Level 1 (as in Example 1), resulting in a three-dimensional wood grain structure with accurate pattern registration.
[0246] Example 9
[0247] The method for generating three-dimensional wood grain on a pattern surface comprises the following steps:
[0248] (S.1) Place an SPC sheet with a length, width and thickness of 1560mm*970mm*4.85mm on the surface of a conveyor moving in a fixed direction;
[0249] (S.2) The SPC sheet in step (S.1) is sequentially passed through a first roller coater and a second roller coater during transportation, so that 12 g / m2 of a primer (wherein the primer comprises: 90% light-curing clear varnish HYS01-1, 5% photoinitiator 184, 0.5% photoinitiator TPO, and 4.5% diluent hydroxyethyl acrylate) and 17 g / m2 of a light-curable white paint (wherein the white paint comprises: 50% light-curing epoxy HYS01-1, 30% titanium dioxide, 5% photoinitiator 184, 0.5% photoinitiator TPO, and 14.5% diluent hydroxyethyl acrylate) are sequentially coated on the surface of the SPC sheet while the SPC sheet is in contact with the coating rollers. The primer is cured using a 395 nm UV lamp and an 8 W / cm2 UV lamp, respectively, to form a primer layer, and a white color paint layer is formed on the surface of the primer layer.
[0250] (S.3) conveying the SPC sheet obtained in step (S.2) to a first inkjet printer, spraying 7 g / m2 of ink on the surface of the color paint layer by the first inkjet printer, and curing the ink to form a pattern layer having a wood grain pattern on the surface of the primer layer;
[0251] (S.4) The SPC sheet obtained in step (S.3) is conveyed to a third roller coater, and 45 g / m2 of a photocurable resin liquid (the resin liquid comprises: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, and 4.5% diluent hydroxyethyl acrylate) is roller-coated on the surface of the pattern layer. The resin liquid is then sequentially irradiated with a 395 nm UV lamp at 8 W / cm2 and a 160 W / cm2 Hg lamp to form a wood grain base layer;
[0252] (S.5) conveying the SPC sheet obtained in step (S.4) to a fourth roller coater, such that the coating roller of the fourth roller coater is rolled along the conveying direction of the SPC sheet (the roller itself rotates in a clockwise direction) to apply 75 g / m2 of a resin solution (the resin solution comprises: 90% Dow Corning 65 Additive, 5% photoinitiator 184, 0.5% photoinitiator TPO, and 4.5% diluent hydroxyethyl acrylate) to the surface of the wood grain bottom layer;
[0253] (S.6) After applying the first layer of resin liquid, the SPC sheet is conveyed forward along the surface of the conveying equipment, and it is ensured that the fourth roller coater does not apply any force to the resin liquid before conveying it to the next roller coater;
[0254] (S.7) conveying the SPC sheet obtained in step (S.6) to a fifth roller coater, so that the coating roller of the fifth roller coater continues to roll-coat 80 g / m2 of the resin solution in the opposite direction of the SPC sheet conveyance (the roller itself rotates in a clockwise direction);
[0255] (S.8) The SPC sheet obtained in step (S.7) is conveyed to a second inkjet printer, where 8 g / m2 of embossing liquid (the embossing liquid comprises: 45.5% diacrylate monomer PEG600DA, 20.5% p-hydroxyanisole HQMME, 10% 2-tert-butylhydroquinone MTBHQ, and 24% diethylene glycol butyl ether) is sprayed on the surface of the resin liquid, and the embossing liquid is allowed to penetrate downward into the resin liquid and mix with the resin liquid to form an embossed layer;
[0256] (S.9) Deeply curing the resin liquid on the surface of the SPC sheet obtained in step (S.8) except for the embossed layer by sequentially irradiating the surface with a UV lamp of 395 nm and 8 W / cm2 and a Hg lamp of 160 W / cm2;
[0257] (S.10) conveying the SPC sheet obtained in step (S.9) to a sixth roller coater, so that 2 g / m2 of a pretreatment agent (wherein the pretreatment agent comprises 95% ethanol and 5% butyl acrylate) is roller-coated on the surface of the SPC sheet;
[0258] (S.11) conveying the SPC sheet obtained in step (S.10) to a cleaning device including a steel brush, so that the embossed layer is brushed out by the steel brush, thereby forming a three-dimensional wood grain layer;
[0259] (S.12) The SPC sheet obtained in step (S.11) is conveyed to a seventh roller coater, where 13 g / m² of a post-treatment agent (comprising 48% water, 32% ethanol, 10% butyl acrylate, 7% polysorbate 80, and 3% isooctylphenoxypolyethoxyethanol) is roller-coated on the surface of the SPC sheet and heated to 55°C. Figure 2 shows a schematic diagram of steps (S.9)-(S.12) of this embodiment, which facilitates a better understanding of these four steps.
[0260] (S.13) The SPC sheet obtained in step (S.12) is passed through an eighth roller coater and a UV lamp with a wavelength of 395 nm and 8 W / cm2, thereby coating the surface of the three-dimensional wood grain layer with a first topcoat of 12 g / m2, and curing the first topcoat to obtain a first topcoat layer;
[0261] (S.14) The SPC sheet obtained in step (S.13) is passed through a ninth roller coater and a UV lamp with a wavelength of 395 nm and 8 W / cm2, thereby coating the surface of the first topcoat layer with a second topcoat of 12 g / m2, and curing the second topcoat layer to obtain the second topcoat layer.
[0262] Example 10
[0263] The difference between this embodiment and embodiment 9 is that the roller coating amount of the post-treatment agent in step (S.12) is 5 g / m2. Other aspects are the same as those in embodiment 9.
[0264] Example 11
[0265] The difference between this embodiment and embodiment 9 is that the roller coating amount of the post-treatment agent in step (S.12) is 20 g / m2. Other aspects are the same as those in embodiment 9.
[0266] Example 12
[0267] The difference between this embodiment and embodiment 9 is that in step (S.12), the post-treatment agent is roller-coated on the surface of the SPC plate and heated to 40° C. The rest is the same as in embodiment 9.
[0268] Example 13
[0269] The difference between this embodiment and embodiment 9 is that in step (S.12), the post-treatment agent is roller-coated on the surface of the SPC plate and heated to 80° C. The rest is the same as in embodiment 9.
[0270] Comparative Example 5
[0271] This comparative example differs from Example 9 in that the post-treatment agent in step (S.12) contains 80% ethanol, 10% butyl acrylate, 7% polysorbate 80, and 3% isooctylphenoxypolyethoxyethanol. In other words, the post-treatment agent does not contain water. All other conditions are the same as in Example 9.
[0272] Comparative Example 6
[0273] This comparative example differs from Example 9 in that the post-treatment agent in step (S.12) contains 53% water, 37% ethanol, and 10% butyl acrylate. In other words, the post-treatment agent does not contain polysorbate 80 or isooctylphenoxypolyethoxyethanol. All other conditions are the same as in Example 9.
[0274] Comparative Example 7
[0275] This comparative example differs from Example 9 in that the post-treatment agent in step (S.12) contains 48% water, 42% ethanol, 7% polysorbate 80, and 3% isooctylphenoxypolyethoxyethanol. In other words, the post-treatment agent does not contain butyl acrylate. All other conditions are the same as in Example 9.
[0276] Comparative Example 8
[0277] This comparative example differs from Example 9 in that the post-treatment agent in step (S.12) contains 48% water, 32% ethanol, 10% butyl acrylate, and 10% polysorbate 80. In other words, the post-treatment agent does not contain isooctylphenoxypolyethoxyethanol. All other conditions are the same as in Example 9.
[0278] Comparative Example 9
[0279] This comparative example differs from Example 9 in that the post-treatment agent in step (S.12) contains 48% water, 32% ethanol, 10% butyl acrylate, and 10% isooctylphenoxypolyethoxyethanol. In other words, the post-treatment agent does not contain polysorbate 80. All other conditions are the same as in Example 9.
[0280] Comparative Example 10
[0281] The difference between this comparative example and Example 9 is that the roller coating amount of the post-treatment agent in step (S.12) is 4 g / m2. Other aspects are the same as those in Example 9.
[0282] Comparative Example 11
[0283] The difference between this comparative example and Example 9 is that the roller coating amount of the post-treatment agent in step (S.12) is 25 g / m2. Other aspects are the same as those in Example 9.
[0284] Comparative Example 12
[0285] The difference between this comparative example and Example 9 is that in step (S.12), the post-treatment agent is roller-coated on the surface of the SPC plate and allowed to stand at room temperature (25°C). All other aspects are the same as in Example 9.
[0286] Comparative Example 13
[0287] The difference between this comparative example and Example 9 is that in step (S.12), the post-treatment agent is roller-coated on the surface of the SPC plate and heated to 85° C. The other steps are the same as in Example 9.
[0288]
Product performance test
[0289] According to the methods in Example 1, Examples 9 to 13, and Comparative Examples 5 to 13, 50 printing plates were respectively produced in batches and product performance tests were performed.
[0290] Clarity test: Tested in accordance with standard JIS K7374.
[0291] Wiredrawing Effect Grade Test: 20 assessors visually inspected the printed board surface to assess the sharpness of the wood grain edges. The results were recorded according to a scale, with the highest number of assessors determining the final grade. Visual inspection of the wood grain edges on the printed board surface is divided into five grades. The five grades, along with the scoring and evaluation criteria, are shown in Table 1.
[0292] Registration Accuracy Test: 20 assessors visually inspected the printed plate surface to assess the alignment accuracy. They visually observed the printed plate surface to detect any misalignment. The evaluation results were recorded according to a grade and score. The grade with the highest number of assessors was determined as the final grade for the printed plate. Visual inspection of the printed plate surface is divided into five grades. The five grades, along with the scoring and evaluation criteria, are shown in Table 2 above.
[0293] The performance test results of the printed plates of Example 1, Examples 9 to 13, and Comparative Examples 5 to 13 are shown in Table 4 below:
[0294] Table 4
[0295]
[0296] Analysis of the data in Table 4 shows that a pretreatment step was added to cure the resin liquid on the wood grain base layer, excluding the embossed layer, before applying a pretreatment agent to the embossed layer. A posttreatment step was then added after the embossed layer was removed, applying a posttreatment agent to the surface of the three-dimensional wood grain layer. This allowed the embossed layer to be scraped clean while simultaneously removing the remaining embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid. This resulted in a three-dimensional wood grain structure with a fine, natural texture, a pattern clarity of up to 85.7%, sharp wood grain edges, a more realistic brushed effect, a realistic feel, and more accurate pattern alignment.
[0297] The above description is only a detailed description of the preferred embodiments and principles of the present invention. For ordinary technicians in this field, based on the ideas provided by the present invention, there may be changes in the specific implementation methods, and these changes should also be considered as the scope of protection of the present invention.
Claims
1. A method for producing three-dimensional wood grain on a pattern surface, characterized in that: The following steps are involved: (1) a step of covering at least a portion of the surface of the pattern layer with a resin liquid; (2) a step of solidifying at least a portion of the resin liquid on the surface of the pattern layer to form a wood grain bottom layer; (3) a step of covering at least a portion of the surface of the wood grain bottom layer with at least one layer of resin liquid; (4) applying embossing liquid to at least a portion of the surface of the resin liquid on the wood grain bottom layer along the color pattern, so that the embossing liquid and / or at least a portion of the resin liquid mixed with the embossing liquid and / or at least a portion of the resin liquid covered by the embossing liquid form an embossing layer; (5) a step of solidifying the resin liquid except for the embossed layer formed in the previous step; (6) further comprising a pretreatment step of allowing the embossed layer to be infiltrated with a pretreatment agent; (7) A step of removing the embossed layer to form a three-dimensional wood grain layer on the surface of the wood grain base layer.
2. A method for generating three-dimensional wood grain on a pattern surface according to claim 1, characterized in that: In the step (3), at least a portion of the surface of the wood grain bottom layer is covered with at least two layers of resin liquid.
3. The method for generating three-dimensional wood grain on a pattern surface according to claim 1, characterized in that: The embossing liquid in step (4) is applied to the surface of the resin liquid and / or penetrates downward into the interior of the resin liquid.
4. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 3, characterized in that: The surface tension of the embossing liquid in the step (4) is higher than that of the resin liquid.
5. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 3, characterized in that: The embossing liquid in step (4) at least includes a curable resin.
6. The method for generating three-dimensional wood grain on a pattern surface according to claim 5, characterized in that: The curable resin contained in the embossing liquid has a surface energy lower than the surface energy of the three-dimensional wood grain layer after curing.
7. The method for generating three-dimensional wood grain on a pattern surface according to claim 5, characterized in that: The curable resin contained in the embossing liquid includes any one of fluorocarbon resin, fluorosilicone resin or organic silicone resin.
8. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 3, characterized in that: The density of the embossing liquid is greater than the density of the resin liquid.
9. The method for generating three-dimensional wood grain on a pattern surface according to claim 8, characterized in that: The embossing liquid also includes a density regulator for adjusting the density of the embossing liquid.
10. The method for generating three-dimensional wood grain on a pattern surface according to claim 9, characterized in that: The density regulator is an inorganic solid powder additive.
11. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 3, characterized in that: The embossing liquid comprises at least two embossing liquids with different surface tensions.
12. The method for generating three-dimensional wood grain on a pattern surface according to claim 1, characterized in that: The step (6) also includes the step of applying a pre-treatment agent to the embossed layer.
13. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 12, characterized in that: The pretreatment agent includes at least an organic solvent.
14. A method for generating three-dimensional wood grain on a pattern surface according to claim 13, characterized in that: The organic solvent includes any one or more combinations of halogenated hydrocarbons, ketones, aromatic hydrocarbons, esters, alcohols, and ethers.
15. The method for generating three-dimensional wood grain on a pattern surface according to claim 14, characterized in that: The organic solvent includes any one or more combinations of dichloromethane, bromopropane, trichloroethane, acetone, toluene, methanol, ethanol, ether, and chloroform.
16. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 12, characterized in that: The pretreatment agent further includes a resin monomer.
17. The method for generating three-dimensional wood grain on a pattern surface according to claim 16, characterized in that: The resin monomer is any one of an acrylic monomer and an epoxy monomer, or a combination of both.
18. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 12, characterized in that: The application amount of the pretreatment agent is 1~5g / m 2 .
19. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 12, characterized in that: The pretreatment process in step (6) also includes a step of bringing the surface of the embossed layer into contact with a brush roller.
20. A method for generating three-dimensional wood grain on a pattern surface according to claim 1 or 12, characterized in that: The pretreatment process in step (6) also includes a transition treatment step after the pretreatment agent is applied to the embossed layer, allowing the pretreatment agent to penetrate into the embossed layer, and the embossed layer is removed after the transition treatment step is completed.
21. The method for generating three-dimensional wood grain on a pattern surface according to claim 1, characterized in that: After the embossed layer in step (7) is removed, a post-treatment step is further included, and the post-treatment step includes a step of applying a post-treatment agent to the surface of the three-dimensional wood grain layer.
22. A method for generating three-dimensional wood grain on a pattern surface according to claim 21, characterized in that: The post-treatment agent at least includes a volatile organic solvent.
23. A method for generating three-dimensional wood grain on a pattern surface according to claim 21 or 22, characterized in that: The post-treatment agent also includes water.
24. A method for generating three-dimensional wood grain on a pattern surface according to claim 21 or 22, characterized in that: The post-treatment agent further includes a resin monomer.
25. A method for generating three-dimensional wood grain on a pattern surface according to claim 21 or 22, characterized in that: The post-treatment agent further comprises a surfactant and / or an emulsifier.
26. The method for generating three-dimensional wood grain on a pattern surface according to claim 22, characterized in that: The volatile organic solvent includes any one or more combinations of acetone, ethanol, methanol, N,N-dimethylformamide, and dimethyl sulfoxide.
27. The method for generating three-dimensional wood grain on a pattern surface according to claim 21, characterized in that: The application amount of the post-treatment agent is 5-20 g / m 2 .
28. The method for generating three-dimensional wood grain on a pattern surface according to claim 21, characterized in that: The post-processing process after the embossed layer is removed in step (7) also includes a step of increasing the surface temperature of the three-dimensional wood grain layer.
29. The method for generating three-dimensional wood grain on a pattern surface according to claim 28, characterized in that: In the post-processing process after the embossed layer is removed in step (7), the surface temperature of the three-dimensional wood grain layer is increased to 40-80°C.
30. A method for generating three-dimensional wood grain on a pattern surface according to claim 1, 2 or 3, characterized in that: The resin liquid is cured in any one of light curing, heat curing or electron beam curing.
31. A method for generating three-dimensional wood grain on a pattern surface according to claim 30, characterized in that: The resin solution at least includes a photo-crosslinking resin and a photoinitiator.
32. A method for producing three-dimensional wood grain on a pattern surface according to claim 1 or 3, characterized in that: The embossing liquid in the step (4) contains at least a polymerization inhibitor for preventing the polymerization of the photo-crosslinking resin.
33. The method for producing three-dimensional wood grain on a pattern surface according to claim 31, characterized in that: The photo-crosslinking resin includes any one or more combinations of unsaturated polyester, epoxy resin, acrylic resin, acrylic modified polyurethane resin, acrylic modified silicone resin, acrylic modified epoxy resin, water-based epoxy acrylate, water-based polyurethane acrylate, and water-based polyester acrylate.
34. The method for producing three-dimensional wood grain on a pattern surface according to claim 31, characterized in that: The photoinitiator includes any one of a free radical polymerization initiator, a cationic polymerization initiator, an energy transfer initiator, and an ion reaction initiator.
35. The method for generating three-dimensional wood grain on a pattern surface according to claim 30, characterized in that: The resin liquid at least includes a thermosetting resin.
36. A method for producing three-dimensional wood grain on a pattern surface according to claim 35, characterized in that: The thermosetting resin includes one or more of epoxy resin, phenolic resin, melamine formaldehyde resin, furan resin, unsaturated polyester resin, silicone resin, and polybutadiene resin.
37. The method for producing three-dimensional wood grain on a pattern surface according to claim 35, characterized in that: The resin solution also includes a curing agent for catalyzing the curing of the thermosetting resin.
38. A printed board with a three-dimensional wood grain effect, characterized in that: including substrates; The surface of the substrate comprises a wood grain base layer and a three-dimensional wood grain layer prepared by the method according to any one of claims 1 to 37.
39. The printed board with three-dimensional wood grain effect according to claim 38, characterized in that: The substrate and the wood grain bottom layer are also provided in sequence: A primer layer used to improve the bonding performance of the printed board surface; A color paint layer provided on the surface of the primer layer to cover the color of the substrate; The pattern layer is located on the surface of the color paint layer and is used to form a wood grain pattern.
40. The printed board with three-dimensional wood grain effect according to claim 38 or 39, characterized in that: The outer surface of the three-dimensional wood grain layer is also covered with a topcoat layer, and at least a portion of the topcoat layer is lower than the upper surface of the three-dimensional wood grain layer.
41. A method for preparing a printed board having a three-dimensional wood grain effect as claimed in any one of claims 38 to 40, characterized in that: It at least comprises the steps of preparing a wood grain base layer and a three-dimensional wood grain layer according to the method described in any one of claims 1 to 37.
42. Use of the printed board with three-dimensional wood grain effect as claimed in any one of claims 38 to 40 in flooring, decorative wall panels or ceiling panels.
Citation Information
Patent Citations
Solid wood stone plastic floor and preparation method thereof
CN107740554A
3D printing plate with surface drawing effect
CN110773403A
Indoor flooring based on polyolefin biomass composites and its preparation process
CN111231437B
Method and apparatus for generating superficial structure
CN110177691A
SPC-based 3D printing plate and preparation method thereof
CN111231430A