Lithium supplementing material and method for preparing same, positive electrode piece and secondary battery
By arranging nano-scale deposition layers and pre-coating layers on the lithium-replenishing materials of lithium-ion batteries, the problem of the materials being prone to deterioration in humid environments is solved, its water absorption resistance and stability are improved, the storage time is extended and the Battery performance.
Patent Information
- Application Number
- PCT/CN2024/087182
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Existing lithium-replenishing materials have poor water absorption resistance and structural stability, resulting in easy deterioration in humid environments, affecting their storage and transportation, and limiting the application of lithium-ion batteries.
By setting a sub-nanoscale deposition layer on the outer core layer of the lithium-supplemented material, combined with the pre-coating layer, the density and water absorption resistance of the material are improved, and the storage time is extended.
It significantly improves the water absorption resistance and stability of lithium-replenishing materials, extends its storage time, and improves the electrochemical performance of lithium-ion batteries.
Smart Images

Figure CN2024087182_24102024_PF_FP_ABST
Abstract
Description
Lithium supplement material and preparation method thereof, positive electrode sheet and secondary battery
[0001] This disclosure claims priority to the Chinese patent application filed with the China Patent Office on April 21, 2023, with application number 202310459303.9, the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0002] The present disclosure relates to the technical field of secondary batteries, and in particular to a lithium supplement material and a preparation method thereof, a positive electrode sheet, and a secondary battery. Background Art
[0003] During the initial charging process of a lithium-ion battery, a large amount of solid electrolyte interface film forms on the surface of the battery's negative electrode, consuming the battery's limited lithium ions and electrolyte, resulting in irreversible capacity loss, reducing the energy density of the lithium-ion secondary battery and limiting its application. In existing technologies, adding lithium-supplementing materials to the positive electrode material can effectively compensate for this initial irreversible capacity loss.
[0004] However, existing lithium-ion supplementation materials have poor water absorption resistance and structural stability. They easily absorb water in humid environments, causing deterioration. This ultimately weakens the structural strength of the lithium-ion supplementation materials and reduces their electrochemical performance. This makes existing lithium-ion supplementation materials unsuitable for long-term storage or long-distance transportation. Therefore, improving the water absorption resistance and stability of lithium-ion supplementation materials has become a key issue.
[0005] Summary of the Invention
[0006] The purpose of the present disclosure is to provide a lithium supplement material and a preparation method thereof, a positive electrode plate and a secondary battery.
[0007] The present disclosure provides the following technical solutions:
[0008] In a first aspect, the present disclosure provides a lithium supplement material, comprising a core and a deposition layer, wherein the core comprises a lithium-rich compound; the deposition layer is coated on the outer layer of the core, and the deposition layer is a film layer below the nanometer scale.
[0009] The lithium-supplementing material provided by the present disclosure has a deposition layer arranged on the outer layer of the inner core, so that the deposition layer can isolate the lithium-rich compound in the inner core from the external environment, thereby preventing water vapor in the external environment from invading the inner core, thereby enabling the lithium-supplementing material to have better resistance to water absorption and stability; at the same time, the deposition layer provided by the present disclosure is a film layer below the nanometer level, which has a higher density than the existing coating layer, so that the deposition layer can further control the absorption of water from the outer core of the lithium-supplementing material, thereby extending the storage time of the lithium-supplementing material.
[0010] In one embodiment, the deposited layer includes a single atomic deposition layer and / or an oxide nanofilm layer obtained by atomic layer deposition technology.
[0011] In one embodiment, the density ρ1 of the deposited layer satisfies the relationship: 2 g / cm 3 ≤ρ1≤4.2g / cm 3 By controlling the density of the deposited layer within the above range, the deposited layer can have a higher density, thereby further controlling the absorption of water from the core from the outside, and the lithium supplement material can have a longer storage time.
[0012] In one embodiment, the lithium-supplementing material further includes a pre-coating layer, the pre-coating layer is coated on the outer surface of the inner core, and the deposition layer is coated on the outer surface of the inner core and the pre-coating layer. By pre-coating the outer surface of the inner core composed of the lithium-rich compound with nano-scale oxide particles, the specific surface area of the lithium-supplementing material is increased, providing an excellent environment for the subsequent arrangement of the deposition layer; the pre-coating layer formed by the oxide particles can have a higher roughness and specific surface area than the outer surface of the inner core, and can avoid the uneven coating phenomenon caused by the deposition layer being directly arranged on the outer surface of the inner core; the pre-coating layer is arranged between the deposition layer and the inner core, which can make the coating of the deposition layer more uniform, ensure the integrity and sealing of the outer surface, so that the lithium-supplementing material provided by the present disclosure can have better anti-water absorption ability and stability.
[0013] In one embodiment, the lithium supplement material further includes a carbon layer, and the carbon layer is coated on the outer layer of the deposition layer.
[0014] In one embodiment, the core is a secondary particle, the secondary particle includes a plurality of primary particles, there is sediment between the primary particles in the secondary particle, and the sediment includes sediment particles below the nanometer level.
[0015] In one embodiment, the density ρ2 of the pre-coating layer satisfies the relationship: 1.5 g / cm 3 ≤ρ2≤3g / cm 3 .
[0016] In one embodiment, the density of the deposited layer is greater than the density of the pre-coating layer.
[0017] In one embodiment, the particle size D10 of the core satisfies the relationship: D10 ≥ 2 μm. When the particle size D10 of the core satisfies the above range, the core can have a size larger than the oxide particles, and the area of the outer surface of the core is also larger, making it easier for nano-scale oxide particles to adhere, or easier for atoms to deposit, further reducing the difficulty of the preparation process; further, when the core satisfies the above range, the oxide particles can also use a wider particle size range (the upper limit of the particle size of the oxide particles is larger), which is conducive to the selection of oxide particles and reduces the cost of the preparation process. When the particle size of the core is smaller than the above range, the particle size of the core is too small, which will make it difficult for the nano-scale oxide to adhere, resulting in uneven coating.
[0018] In one embodiment, the specific surface area S1 of the core satisfies the relationship: S1≤3m 2 / g. Controlling the specific surface area of the core within an appropriate range is intended to provide a more suitable adhesion environment for the oxide particles. It is understood that a larger specific surface area of the core allows for greater outer surface roughness, which is more conducive to oxide particle adhesion compared to a smoother surface, thereby further reducing the difficulty of the preparation process.
[0019] In one embodiment, the deposition layer is made of a material selected from the group consisting of aluminum oxide, silicon dioxide, and titanium dioxide.
[0020] In one embodiment, the pre-coating layer has gaps, and at least a portion of the deposited layer fills the gaps. Specifically, the pre-coating layer may be formed by a plurality of oxide particles interconnected on the outer surface of the core. Therefore, the pre-coating layer may have some gaps, which may be caused by insufficient connection between the oxide particles. At least a portion of the deposited layer fills the gaps in the pre-coating layer, thereby reducing the size of the gaps and preventing moisture from the external environment from intruding into the core through the gaps in the pre-coating layer.
[0021] In one embodiment, at least a portion of the deposited layer directly coats the outer surface of the core. Due to the gaps in the pre-coating layer, at least a portion of the atomic deposition agent can pass through the gaps and deposit on the outer surface of the core. By directly coating at least a portion of the deposited layer on the outer surface of the core, the advantage is that it not only fills the gaps formed, but also directly coats the core, improving the lithium-replenishing material's resistance to water absorption. Furthermore, when using the same mass of atomic deposition agent, the outermost deposited layer can be thinned.
[0022] In one embodiment, the pre-coating layer includes oxide particles and a lubricant mixed with each other.
[0023] In one embodiment, the oxide particles include one or more of aluminum oxide, silicon dioxide, and titanium dioxide.
[0024] In one embodiment, the particle size of the oxide particles is 1 nm to 100 nm. The particle size of the oxide particles through the pores is beneficial to controlling the thickness of the pre-coating layer formed, as well as controlling the lithium replenishing effect of the lithium replenishing material. It can be understood that the pre-coating layer is formed by interconnected oxide particles, so compared with the same number of oxide particles, the smaller the particle size of the oxide particles, the thinner the pre-coating layer formed. In addition, controlling the oxide particles within the above range can also control the proportion of gaps formed in the pre-coating layer.
[0025] In one embodiment, the specific surface area S2 of the oxide particles satisfies the relationship: S2 ≥ 50m 2 / g. The specific surface area of the oxide particles is controlled within the above range, on the one hand, to improve the adhesion between them and the core, and on the other hand, to provide a good environment for the adhesion of the deposited layer. It can be understood that when the specific surface area of the oxide particles is larger, the outer surface roughness of the oxide particles can be greater, which is more conducive to combining with the core compared to a smooth surface, thereby improving the structural stability of the pre-coating layer. Similarly, the rough outer surface also reduces the difficulty of forming the deposited layer, provides an excellent environment for the atomic deposition agent, and facilitates deposition and forming.
[0026] In one embodiment, the lubricant includes at least one of graphite and boron nitride.
[0027] In one embodiment, the mass ratio of the oxide particles to the lubricant is 1:(0.1-0.8). By controlling the ratio of oxide particles to lubricant, the uniformity of the oxide particle coating on the outer surface of the core can be controlled. It is understandable that when the lubricant ratio is lower than the above ratio, the lubrication level will be insufficient, and the oxide particles will easily accumulate, thus still failing to form a relatively uniform pre-coating layer; when the lubricant ratio is higher than the above ratio, lubricant accumulation will occur, that is, some oxide particles will not be able to form a continuous deposition to form a coordinated deposition layer.
[0028] In one embodiment, the mass ratio of the core, the pre-coating layer, and the deposited layer is 100:(0.01-10):(0.01-5). By controlling the mass ratio of the core, the pre-coating layer, and the deposited layer within an appropriate range, not only can the thickness of the pre-coating layer and the deposited layer be adjusted to provide a good sealing environment for the pre-coating layer and the deposited layer, but also can ensure that the lithium-supplementing material can maintain good electrochemical performance.
[0029] In one embodiment, the thickness A1 of the pre-coating layer is 1 nm to 200 nm. The pre-coating layer is intended to create an environment for the deposition layer without affecting the efficiency of lithium ion extraction from the core. Therefore, after ensuring that the pre-coating layer has a certain thickness for deposition, it should be avoided that the pre-coating layer is too thick. The thickness of the pre-coating layer within the above range can meet the deposition requirements without affecting the efficiency of lithium ion extraction.
[0030] In one embodiment, the thickness A2 of the deposited layer is 1 nm to 200 nm. The deposited layer is used to achieve a dense wrapping, thereby protecting the core. The thickness of the deposited layer within the above range can protect the core without affecting the efficiency of lithium ion extraction.
[0031] In one embodiment, the thicknesses of the pre-coating layer and the deposited layer satisfy the relationship: 1≤A1 / A2≤40. Controlling the thickness ratio of the pre-coating layer to the deposited layer within the above range facilitates controlling the thickness of the pre-coating layer or the deposited layer, thereby ensuring complete coverage of the pre-coating layer while avoiding excessive thickness of the deposited layer.
[0032] In one embodiment, the chemical formula of the lithium-rich compound includes Li x M y O z He Li w At least one of A; wherein, 0<x≤6, 0<y≤3, 0<z≤4, 0<w≤5; M is at least one element selected from Fe, Co, Ni, Mn, V, Cu, Mo, Al, Ti, and Mg, and A is at least one element selected from C, N, O, P, S, F, B, and Se.
[0033] In a second aspect, the present disclosure provides a method for preparing a lithium-supplementing material, comprising: uniformly mixing a lithium source and a first metal source and sintering them together to obtain a lithium-rich compound; arranging a sediment on the outer layer of the lithium-rich compound to obtain a lithium-supplementing material; the lithium-supplementing material comprises a core and a sediment layer, the core comprising the lithium-rich compound, and the sediment forming the sediment layer.
[0034] In a third aspect, the present disclosure further provides a positive electrode plate, which includes a current collector and an active material layer arranged on the current collector, wherein the active material layer includes a positive electrode material and the lithium-supplementing material described in any one of the embodiments of the first aspect, or the active material layer includes a positive electrode material and a lithium-supplementing material obtained by the preparation method of the lithium-supplementing material described in any one of the embodiments of the second aspect.
[0035] In a fourth aspect, the present disclosure further provides a secondary battery, comprising a negative electrode plate, a separator, and the positive electrode plate described in the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0037] FIG1 is a schematic cross-sectional view of a lithium-supplementing material in one embodiment;
[0038] FIG2 is a partial cross-sectional schematic diagram of a lithium-supplementing material in one embodiment;
[0039] FIG3 is a partial cross-sectional schematic diagram of a lithium-supplementing material including a lubricant in one embodiment;
[0040] FIG4 is a schematic diagram of a cross-sectional structure of a lithium supplement material in the form of secondary particles in one embodiment;
[0041] FIG5 is a flow chart of a method for preparing a lithium supplement material in one embodiment;
[0042] FIG6 is a specific flow chart of step S20 in FIG5 ;
[0043] FIG7 is a SEM image of a pre-coating layer of a lithium supplementing material in one embodiment;
[0044] Figure 8 is a TEM image of the lithium-replenishing material from another perspective. DETAILED DESCRIPTION
[0045] The following will be combined with the accompanying drawings in the embodiments of the present disclosure to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the embodiments described are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present disclosure.
[0046] It should be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may be an intermediate component. When a component is referred to as being "connected to" another component, it may be directly connected to the other component or there may be an intermediate component.
[0047] Unless otherwise defined, all technical and scientific terms used in this disclosure have the same meanings as those commonly understood by those skilled in the art to which this disclosure belongs. The terms used in the specification of this disclosure are for the purpose of describing specific embodiments only and are not intended to limit this disclosure. The term "and / or" as used in this disclosure includes any and all combinations of one or more of the relevant listed items.
[0048] The following describes some embodiments of the present disclosure in detail with reference to the accompanying drawings. In the absence of conflict, the following embodiments and features therein may be combined with each other.
[0049] In a first aspect, the present disclosure provides a lithium-supplementing material comprising a core and a deposition layer, wherein the core comprises a lithium-rich compound; the deposition layer is coated on the outer surface of the core, and the deposition layer is a sub-nanometer-scale film layer. It should be noted that the deposition layer can be directly coated on the outer surface of the lithium-supplementing material; alternatively, another layer can be provided between the core and the deposition layer. Specifically, the outer surface of the core is coated with another coating layer, and the deposition layer is further coated on the outer surfaces of the core and the coating layer.
[0050] Specifically, the core of the lithium-supplementing material can be mainly composed of a lithium-rich compound. The lithium-rich compound is the core of the lithium-supplementing material for providing lithium ions, and the chemical formula of the lithium-rich compound is not specifically limited. Optionally, the shape of the core can be spherical or spherical-like structure or other irregular shapes. The lithium-supplementing material with a lithium-rich compound as the core is added to the electrode, so that during the first cycle of charging, it acts as a "sacrificial agent" to release all the lithium ions contained in it at one time as much as possible to replenish the irreversible lithium ions consumed by the formation of the SEI film at the negative electrode, thereby maintaining the abundance of lithium ions in the battery system and improving the first efficiency and overall electrochemical performance of the battery.
[0051] In one embodiment, the chemical formula of the lithium-rich compound includes Li x M y O z He Li w At least one of A; wherein, 0<x≤6, 0<y≤3, 0<z≤4, 0<w≤5; M is at least one element selected from Fe, Co, Ni, Mn, V, Cu, Mo, Al, Ti, Mg, and A is at least one element selected from C, N, O, P, S, F, B, and Se. In a specific embodiment, the lithium-rich compound may be Li5FeO4, Li6MnO4, Li6CoO4, Li6ZnO4, Li2NiO2, Li2CuO2, Li2CoO2, Li2MnO2, Li2Ni 0.5 Mn 1.5 It should be noted that some of the above lithium-rich compounds can be directly used as lithium-rich positive electrode materials, such as Li2NiO2, Li2CuO2, Li2CoO2, Li2MnO2, Li2Ni 0.5 Mn 1.5 O4.
[0052] The deposited layer is a film layer composed of nano-scale and smaller-than-nanoscale deposits. Specifically, the nano-scale deposits include nanoparticles, and the smaller-than-nanoscale deposits include atomic or molecular-scale particles.
[0053] In one embodiment, the deposited layer includes a single atomic deposition layer and / or an oxide nanofilm layer obtained by atomic layer deposition technology. Specifically, the deposited layer can be a single atomic deposition layer obtained by atomic layer deposition technology, and the level can be a single atomic layer or nanolayer composed of atoms or molecules. Optionally, when the deposited layer is a single atomic deposition layer, different atomic deposition agents can be selected according to the different materials thereof, including but not limited to one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, tetrakis(diethylamino)titanium, triethylsilane, tetraethylsilane, and tetrakis(ethylmethylamino)zirconium.
[0054] Alternatively, the deposited layer may be an oxide nanofilm. For example, the oxide nanofilm may be formed by reacting the aforementioned monoatomic deposition layer with oxygen, and may be made of materials such as aluminum oxide, titanium dioxide, silicon dioxide, or zirconium dioxide. Alternatively, a nanoscale oxide layer may be formed directly on the outer layer of the core using vapor deposition technology. Of course, the oxide nanofilm may also be formed using other techniques.
[0055] Optionally, the deposited layer may be a multilayer; for example, it may include both a single atomic deposition layer and an oxide nanofilm layer; or it may include at least one single atomic deposition layer or oxide nanofilm layer.
[0056] It is understood that the deposition layer should be composed of atomic, molecular, or nanoscale particles. Furthermore, the specific formation method of the deposition layer is not limited. By controlling the composition of the deposition layer to the aforementioned size levels, it is easier to obtain a denser layer, thereby achieving a dense coating of the core, thereby further reducing the ingress of external water into the core.
[0057] The lithium-supplementing material provided by the present disclosure has a sedimentary layer arranged on the outer layer of the inner core, so that the sedimentary layer can isolate the lithium-rich compound in the inner core from the external environment, thereby preventing water vapor in the external environment from invading the inner core, thereby enabling the lithium-supplementing material to have better resistance to water absorption and stability; the sedimentary layer provided by the present disclosure has a higher density than the existing coating layer, so that the lithium-supplementing material can further control the water absorption of the inner core from the outside by using the sedimentary layer as the outer coating layer, so that the lithium-supplementing material can have a longer storage time.
[0058] In one embodiment, the density ρ1 of the deposited layer satisfies the relationship: 2 g / cm 3 ≤ρ1≤4.2g / cm 3By controlling the density of the deposited layer within the above range, the deposited layer can have a higher density, thereby further controlling the absorption of water from the core from the outside, and the lithium-supplemented material can have a longer storage time. It can be understood that when the density of the deposited layer is higher, the density of the deposited layer is higher, and the tightness of the film layer is better.
[0059] In one embodiment, referring to FIG. 1 , the lithium supplement material further includes a pre-coating layer 20 , which is coated on the outer surface of the core 10 , and a deposition layer 30 is coated on the outer surfaces of the core 10 and the pre-coating layer 20 .
[0060] Specifically, the pre-coating layer 20 can be a continuous layer formed by connecting oxide particles 21. Optionally, the oxide particles 21 can be nano-sized particles prepared by vapor deposition. The oxide particles 21 include, but are not limited to, one or more of vapor-phase nano-alumina, vapor-phase nano-silicon dioxide, and vapor-phase nano-titanium dioxide. It is understandable that the pre-coating layer 20 can be formed by a plurality of oxide particles 21 connected to each other on the outer surface of the core 10, so there can be partial gaps in the pre-coating layer 20, which can be formed by the oxide particles 21 not being fully connected.
[0061] Optionally, the particle size of the oxide particles 21 should be smaller than that of the core 10, and the oxide particles 21 may have a larger particle size distribution range. This allows the oxide particles 21 to form a denser pre-coating layer 20 while also reducing the gap ratio in the pre-coating layer 20, thereby preventing moisture from the external environment from invading the core 10 through the gaps in the pre-coating layer 20.
[0062] Optionally, the material of the deposition layer 30 can be the same as or different from that of the pre-coating layer 20. For example, the pre-coating layer 20 can be composed of vapor-phase nano-alumina particles, while the deposition layer 30 can be composed of molecular-level aluminum oxide; the deposition layer 30 can also be composed of molecular-level silicon dioxide.
[0063] Optionally, part of the sediment can pass through the gaps in the pre-coating layer 20 and directly coat the outer surface of the core 10. It will be appreciated that because the sediment is smaller than the oxide particles 21 and potentially smaller than the width of the gaps in the pre-coating layer 20, it can pass through the gaps and directly connect to the core 10 during the deposition process. This has the advantage of filling the gaps in the pre-coating layer 20 with the sediment, thereby reducing the size of the gaps and preventing moisture from the external environment from intruding into the core 10 through the gaps in the pre-coating layer 20.
[0064] The present disclosure increases the specific surface area of the lithium-supplementing material by pre-coating the outer surface of the inner core composed of a lithium-rich compound with nano-scale oxide particles, providing an excellent environment for the subsequent arrangement of a deposition layer; the pre-coating layer formed by the oxide particles can have a higher roughness and specific surface area than the outer surface of the inner core, and can avoid the uneven coating phenomenon that occurs when the deposition layer is directly arranged on the outer surface of the inner core; the pre-coating layer is arranged between the deposition layer and the inner core, which can make the coating of the deposition layer more uniform, ensure the integrity and sealing of the outer surface, and thus enable the lithium-supplementing material provided by the present disclosure to have more excellent water absorption resistance and stability.
[0065] In one embodiment, the lithium-replenishing material further includes a carbon layer (not shown), which is coated on the outer layer of the deposited layer. Specifically, the carbon layer is composed of a carbon material, including one or more of graphite, carbon black, hard carbon, soft carbon, amorphous carbon, etc.
[0066] In one embodiment, the core 10 is a secondary particle, and the secondary particle includes a plurality of primary particles, and there is sediment between the primary particles in the secondary particles. Specifically, the core 10 can be a secondary particle composed of a plurality of primary particles, so the core 10 can have a gap formed by connecting a plurality of primary particles. The sediment can be the main substance constituting the sedimentation layer 30, and the sediment can be deposited in the gap between the plurality of primary particles, and the sediment can even form a coating on the primary particles, as shown in Figure 4. Preferably, in the structure in which the core 10 is a secondary particle, metal elements can be doped inside the core or in the interface layer by atomic layer deposition technology, thereby improving the conductivity inside the core.
[0067] In one embodiment, the density ρ2 of the pre-coating layer satisfies the relationship: 1.5 g / cm 3 ≤ρ2≤3g / cm 3 .
[0068] In one embodiment, the density of the deposited layer is greater than that of the pre-coating layer. Specifically, the density of the deposited layer is set to be greater than that of the pre-coating layer to ensure that the deposited layer has a higher density, thereby protecting the core from external water vapor erosion.
[0069] In one embodiment, the particle size D10 of the inner core satisfies the relationship: D10 ≥ 2 μm. Wherein, D10 refers to the particle size corresponding to a volume smaller than 10% of the total volume on the particle size distribution curve. Preferably, the specific range of the particle size D10 of the inner core can be 2 μm to 8 μm. The particle size of the inner core is controlled in order to provide a more suitable attachment environment for particles at the nanometer level and below, and it is also easier to carry out atomic deposition. It can be understood that when the particle size D10 of the inner core satisfies the above range, the inner core can have a size larger than the oxide particles, and the area of the outer surface of the inner core is also larger, making it easier for nanometer-scale oxide particles to adhere, further reducing the difficulty of the preparation process; further, when the inner core satisfies the above range, the oxide particles can also use a wider particle size range (the upper limit of the particle size of the oxide particles is larger), which is conducive to the selection of oxide particles and reduces the cost of the preparation process.
[0070] When the core particle size D10 is smaller than the above range, the small core size can make it difficult for the oxide particles to adhere, and the range of oxide particles available is narrowed. Furthermore, the small core size increases the difficulty of core preparation, hindering the cost of lithium-supplementing materials. When the core particle size D10 is larger than the above range, the compaction density of the positive electrode sheet made from the lithium-supplementing material is low, hindering the capacity of the lithium-supplementing battery.
[0071] In one embodiment, the specific surface area S1 of the core satisfies the relationship: S1≤3m 2 / g. Preferably, the specific range of the specific surface area of the kernel can be 0m 2 / g~1m 2 / g. Specifically, the specific surface area S1 of the core can be, but is not limited to, 0.1m 2 / g, 0.2m 2 / g, 0.5m 2 / g, 0.8m 2 / g、1m 2 / g, 2m 2 / g、3m 2 / g. Controlling the specific surface area of the core within an appropriate range is intended to provide a more suitable adhesion environment for the oxide particles. It is understood that a larger specific surface area of the core allows for greater outer surface roughness, which is more conducive to oxide particle adhesion compared to a smoother surface, thereby further reducing the difficulty of the preparation process.
[0072] In one embodiment, the material of the deposited layer is a combination of one or more of aluminum oxide, silicon dioxide, and titanium dioxide. Specifically, based on the above embodiment, the deposited layer can be formed by reacting the aforementioned atomic deposition agent with oxygen. Therefore, the material of the deposited layer depends on the selected atomic deposition agent. It is understood that the deposition layer can be formed by placing the atomic deposition agent on the pre-coating layer and waiting for the atomic deposition agent to completely react with oxygen to form the final deposition layer. Of course, to speed up the reaction, high-temperature reaction can also be used to accelerate the reaction.
[0073] In one embodiment, referring to FIG2 , the pre-coating layer 20 has gaps, and at least a portion of the deposited layer 30 fills these gaps. Specifically, the pre-coating layer 20 may be formed by a plurality of interconnected oxide particles 21 on the outer surface of the core 10. Therefore, the pre-coating layer 20 may have some gaps, which may be caused by insufficient connection between the oxide particles 21. At least a portion of the deposited layer 30 fills the gaps in the pre-coating layer 20, thereby reducing the size of the gaps and preventing moisture from the external environment from invading the core 10 through the gaps in the pre-coating layer 20.
[0074] In one embodiment, referring to FIG2 , at least a portion of the deposition layer 30 is directly coated on the outer surface of the core 10. It will be appreciated that due to the presence of gaps in the pre-coating layer 20, at least a portion of the atomic deposition agent can pass through the gaps and be deposited on the outer surface of the core 10. By directly coating at least a portion of the deposition layer 30 on the outer surface of the core 10, the advantage is that while filling the gaps, it can also directly coat the core 10, improving the lithium-replenishing material's resistance to water absorption. Furthermore, when using the same mass of atomic deposition agent, the outermost deposition layer 30 can be thinned.
[0075] In one embodiment, referring to FIG3 , the pre-coating layer 20 includes oxide particles 21 and a lubricant 22 that are mixed with each other, and the lubricant 22 includes at least one of graphite and boron nitride. Specifically, the lubricant 22 can be added together with the oxide particles 21 when making the pre-coating layer 20, so that there can be residual lubricant 22 in the formed pre-coating layer 20. The purpose of adding the lubricant 22 is to enhance mixing, because the method for making the pre-coating layer 20 can use solid-phase mixing, that is, directly mixing the core 10 and the oxide particles 21, so in order to reduce static electricity between the solid particles and make the mixing more complete, a lubricant 22 (such as graphite or boron nitride) can be used. In this way, the gas-phase nano-scale oxide particles 21 can be more evenly distributed on the surface of the lithium-replenishing particles. Of course, in other embodiments, the lubricant 22 can also be paraffin or other volatile substances, so there may be no lubricant 22 remaining in the final lithium-replenishing material.
[0076] In one embodiment, the particle size of the oxide particles is 1 nm to 100 nm. Specifically, the particle size of the oxide particles can be, but is not limited to, 8 nm, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, 30 nm, 50 nm, 80 nm, and 100 nm. The particle size of the oxide particles through the pores is beneficial to controlling the thickness of the pre-coating layer formed, as well as controlling the lithium replenishing effect of the lithium replenishing material. It can be understood that the pre-coating layer is formed by interconnecting oxide particles, so compared to the same number of oxide particles, the smaller the particle size of the oxide particles, the thinner the pre-coating layer formed. In addition, controlling the oxide particles within the above range can also control the proportion of gaps formed in the pre-coating layer. When the particle size of the oxide particles is smaller than the above range, it becomes more difficult to obtain the oxide particles, and the oxide particles are more likely to form local accumulation, which will lead to uneven thickness of the pre-coating layer and is not conducive to the formation of the pre-coating layer; when the particle size of the oxide particles is larger than the above range, the overall thickness of the pre-coating layer will be thicker, and the weight ratio of the pre-coating layer will increase, but since the oxide particles do not contribute lithium ions, the overall gram capacity of the lithium-supplementing material will be reduced, resulting in deviations in the lithium-supplementing effect of the lithium-supplementing material.
[0077] In one embodiment, the specific surface area S2 of the oxide particles satisfies the relationship: S2 ≥ 50m 2 / g. Preferably, the specific range of the oxide particle specific surface area S2 can be 50m 2 / g~200m 2 / g. Specifically, the specific surface area S2 of the oxide particles can be, but is not limited to, 50m 2 / g、80m 2 / g、100m 2 / g, 150m 2 / g, 200m 2 / g. The specific surface area of the oxide particles is controlled within the above range, on the one hand, to improve the adhesion between them and the core, and on the other hand, to provide a good environment for the adhesion of the deposited layer. It can be understood that when the specific surface area of the oxide particles is larger, the outer surface roughness of the oxide particles can be greater, which is more conducive to combining with the core compared to a smooth surface, thereby improving the structural stability of the pre-coating layer. Similarly, the rough outer surface also reduces the difficulty of forming the deposited layer, provides an excellent environment for the atomic deposition agent, and facilitates deposition and forming.
[0078] In one embodiment, in the pre-coating layer of the lithium-supplementing material, the mass ratio of the oxide particles to the lubricant is 1: (0.1 to 0.8). Specifically, the mass ratio of the oxide particles to the lubricant can be, but is not limited to, 1: 0.1, 1: 0.2, 1: 0.3, 1: 0.4, 1: 0.5, 1: 0.6, 1: 0.7, 1: 0.8. It should be noted that in the preparation process of the pre-coating layer of the lithium-supplementing material, the amount of lubricant added needs to be more. This is because some lubricants such as paraffin will evaporate at high temperatures, and another part of the lubricant such as graphite may also be partially consumed during the preparation process. Preferably, the mass ratio of the oxide particles to the lubricant added during the preparation process is 1: (0.1 to 5). By controlling the ratio of oxide particles to lubricant, the uniformity of the oxide particles coating the outer surface of the inner core can be controlled. It is understandable that when the lubricant ratio is lower than the above ratio, the lubrication level will be insufficient, the oxide particles will easily accumulate, and thus it will still be impossible to form a relatively uniform pre-coating layer. When the lubricant ratio is higher than the above ratio, lubricant accumulation will occur, that is, some oxide particles will not form a continuous deposition and form a combination with the deposition layer. At the same time, if a non-conductive lubricant (such as boron nitride) is used, when the lubricant ratio is high, the overall conductivity of the lithium supplement material will be poor due to the lubricant's lack of conductivity, making it difficult for lithium ions to be inserted and removed.
[0079] In one embodiment, the pre-coating layer includes a sub-coating layer (not shown in the figure). The sub-coating layer can be formed by the lubricant in the above-mentioned embodiment, coating a portion of the outer surface of the core, or coating the outer surface of the oxide particles. It is understood that when the proportion of the lubricant approaches the upper limit in the above-mentioned embodiment, part of the lubricant can be interconnected to form a sub-coating layer. The advantage of this structure is that it can not only further protect the core from external water vapor corrosion, but also provide a conductive environment (such as graphite), thereby increasing the lithium ion insertion and extraction efficiency of the lithium supplement material.
[0080] In one embodiment, the mass ratio of the core, the pre-coating layer, and the deposited layer is 100:(0.01-10):(0.01-5). Specifically, the mass ratio of the core, the pre-coating layer, and the deposited layer may be, but is not limited to, 100:0.01:0.01, 100:0.01:5, 100:10:0.01, 100:5:3, 100:5:5, and 100:10:3. By controlling the mass ratio of the core, the pre-coating layer, and the deposited layer within an appropriate range, not only can the thickness of the pre-coating layer and the deposited layer be adjusted so that the pre-coating layer and the deposited layer provide a good sealing environment, but it can also ensure that the lithium supplement material can maintain good electrochemical properties. When the proportion of the inner core is smaller than the above range, the specific gravity of the pre-coating layer or the deposited layer is too large, and since the pre-coating layer or the deposited layer does not contribute lithium ions, the overall gram capacity of the lithium supplement material will be reduced; when the proportion of the inner core is larger than the above range, the specific gravity of the pre-coating layer or the deposited layer is too small, which may cause the layer thickness of the pre-coating layer or the deposited layer to be too thin, or the coating to be incomplete, which is not conducive to creating a good sealing environment.
[0081] Preferably, the mass ratio of the core, the pre-coating layer, and the deposition layer is 100:(0.01-5):(0.01-3). More preferably, it is 100:(0.01-3):(0.01-1).
[0082] In one embodiment, the thickness A1 of the pre-coating layer is 1nm to 200nm. Specifically, the thickness A1 of the pre-coating layer can be, but is not limited to, 1nm, 2nm, 3nm, 5nm, 8nm, 10nm, 15nm, 30nm, 50nm, 80nm, 120nm, 150nm, and 200nm. It can be understood that the pre-coating layer is to create an environment for the deposition layer and does not affect the efficiency of lithium ion extraction in the core. Therefore, after ensuring that the pre-coating layer has a certain thickness for deposition, the pre-coating layer should be avoided from being too thick; and the thickness of the pre-coating layer within the above range can meet the deposition requirements while not affecting the efficiency of lithium ion extraction. When the thickness of the pre-coating layer is less than the above range, the particle size requirements for the oxide particles are higher (smaller particle size is required), the difficulty of obtaining the oxide particles increases, and the difficulty of making the pre-coating layer also increases accordingly (the accumulation rate of small particles increases); when the thickness of the pre-coating layer is greater than the above range, since the pre-coating layer does not contribute lithium ions, the overall gram capacity of the lithium supplement material will be reduced.
[0083] In one embodiment, the thickness A2 of the deposited layer is 1 nm to 200 nm. Specifically, the thickness A2 of the deposited layer may be, but is not limited to, 1 nm, 2 nm, 3 nm, 5 nm, 8 nm, 10 nm, 15 nm, 30 nm, 50 nm, 80 nm, 120 nm, 150 nm, and 200 nm. The deposited layer is used to achieve dense wrapping, thereby protecting the core. The thickness of the deposited layer within the above range can meet the requirements of protecting the core without affecting the efficiency of lithium ion extraction. When the thickness of the deposited layer is less than the above range, the requirements for atomic deposition are higher (higher precision), which is not conducive to improving the yield rate of the lithium supplement material; when the thickness of the deposited layer is greater than the above range, since the deposited layer does not contribute lithium ions, the overall gram capacity of the lithium supplement material will be reduced.
[0084] In one embodiment, the thickness of the pre-coating layer and the deposited layer satisfies the relationship: 1≤A1 / A2≤40. Specifically, A1 / A2 can be, but is not limited to, 1, 2, 5, 8, 12, 20, 30, 40. By controlling the thickness ratio of the pre-coating layer and the deposited layer within the above range, it is beneficial to control the thickness of the pre-coating layer or the deposited layer, thereby avoiding the phenomenon of the deposited layer being too thick while ensuring that the pre-coating layer is completely coated. When it is less than the range of the above relationship, it means that the pre-coating layer is too thin, and the difficulty of making the pre-coating layer increases; when it is greater than the range of the above relationship, it means that the deposited layer is too thin, and it is easy to have incomplete coating or loose coating.
[0085] In a second aspect, the present disclosure further provides a method for preparing a lithium-supplementing material, as shown in FIG5 , which is specifically used for preparing the lithium-supplementing material in the first aspect. The preparation method comprises the following steps:
[0086] Step S10: uniformly mix the lithium source and the first metal source and then sinter them together to obtain a lithium-rich compound.
[0087] Step S20 , placing a sediment on the outer layer of the lithium-rich compound to obtain a lithium-supplementing material.
[0088] The lithium supplement material includes a core and a sediment layer. The core includes a lithium-rich compound, and the sediment forms a sediment layer. The density ρ1 of the sediment layer satisfies the relationship: 2g / cm 3 ≤ρ1≤4.2g / cm 3 .
[0089] Specifically, please refer to FIG6 , step S20 includes:
[0090] In step S21 , a lithium-rich compound and oxide particles are mixed in a solid phase and then treated at high temperature to obtain a first lithium-supplementing material. The first lithium-supplementing material includes a core containing a lithium-rich compound and a pre-coating layer containing oxide particles. The pre-coating layer is coated on the outer surface of the core.
[0091] Step S22 , placing a sediment on the outer surface of the first lithium-supplementing material, and the sediment forms a sediment layer to obtain a second lithium-supplementing material.
[0092] Optionally, in step S10, the lithium-rich compound can be formed by sintering a lithium source and a first metal source together, and the specific chemical formula can be as provided in the first aspect. The lithium source can be one or more of lithium oxide, lithium hydroxide, lithium acetate, lithium carbonate, lithium fluoride, and lithium chloride. Preferably, the first metal source can be an iron source, a manganese source, and a nickel source; the iron source can be one or more of ferric acetate, ferric nitrate, ferric sulfate, ferric hydroxide, ferric chloride, and ferric oxide. The manganese source can be one or more of manganese acetate, manganese nitrate, manganese monoxide, manganese sulfate, manganese hydroxide, and manganese dichloride. The nickel source can be one or more of nickel acetate, nickel nitrate, nickel oxide, nickel sulfate, nickel hydroxide, and nickel chloride. Preferably, the above-mentioned lithium source and the first metal source can be mixed in a liquid phase, and the solvent used can be one or more of methanol, glycerol, ethanol, and water.
[0093] Optionally, the oxygen content in the sintering environment of the lithium-rich compound needs to be controlled below 50 ppm to prevent Mn 2+ and Ni 2+ Therefore, it should be carried out under a protective atmosphere, specifically one or more of nitrogen, helium, argon, and neon.
[0094] Optionally, the oxide particles in step S21 may be those provided in the first aspect, which will not be described in detail here.
[0095] Optionally, a lubricant may also be added in step S21. The lubricant includes one or more of paraffin wax, graphite, boron nitride, silicone oil, glycerin, tetrabutyl titanate, propylene glycol, and molybdenum disulfide. It is understood that volatile lubricants such as paraffin wax evaporate after high-temperature sintering and therefore do not remain in the lithium-supplementing material, while less volatile lubricants such as graphite and boron nitride remain in the lithium-supplementing material.
[0096] Optionally, the oxide particles and lubricant can be added in steps. For example, after the oxide particles and lubricant are mixed, they can be divided into three batches, namely the first batch, the second batch and the third batch, and the three batches are added and mixed with the lithium-rich compound in chronological order. The weight of the oxide particles and lubricant in the first batch is the largest, and then decreases in the third batch. The advantage of this addition method is that the oxide particles can coat the core more evenly, avoiding the particle accumulation phenomenon that occurs after a one-time addition.
[0097] Optionally, in step S21 , the temperature of the high temperature treatment may be 400° C. to 700° C., and the time of the high temperature treatment may be 1 hour to 6 hours.
[0098] Optionally, in step S22, a first lithium-replenishing material may be pre-placed in a reaction chamber of an atomic deposition apparatus. An atomic deposition agent may be heated and vaporized to obtain a vapor-phase atomic deposition agent. The vapor-phase atomic deposition agent is then pulsed into the first lithium-replenishing material to deposit the first lithium-replenishing material, thereby obtaining a second lithium-replenishing material. The second lithium-replenishing material includes a core, a pre-coating layer, and a deposition layer. The structure of the lithium-replenishing material described in the first aspect may be referred to in detail and will not be further described here.
[0099] Optionally, in step S22 , the atomic deposition agent includes one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, tetrakis(diethylamino)titanium, triethylsilane, tetraethylsilane, and tetrakis(ethylmethylamino)zirconium.
[0100] Optionally, in step S22, the temperature of the deposition environment is between -10°C and 200°C. Preferably, the temperature of the deposition environment is between 50°C and 150°C. Controlling the deposition environment within this temperature range results in a better coating effect after deposition. When the temperature is below this range, the coating effect is poor; when the temperature is above this range, the atomic deposition agent reacts too quickly, making the deposition rate difficult to control and potentially dangerous.
[0101] In a third aspect, the present disclosure further provides a positive electrode plate, comprising a current collector and an active material layer disposed on the current collector, wherein the active material layer comprises a positive electrode material and the lithium-supplementing material of the first aspect, or the active material layer comprises the positive electrode material and a lithium-supplementing material obtained by the preparation method of the lithium-supplementing material of the second aspect. The positive electrode plate provided by the present disclosure, because it contains the above-mentioned lithium-supplementing material, and the lithium-supplementing material can provide active lithium ions that compensate for the formation of the SEI film during the first charge of the battery, thereby effectively maintaining the gram capacity of the positive electrode plate and improving the capacity retention rate of the positive electrode plate; at the same time, the lithium-supplementing material can release lithium polysulfide to eliminate lithium plating, thereby not only maintaining the performance of the positive electrode plate, but also improving the service life of the positive electrode plate.
[0102] In one embodiment, the positive electrode sheet includes a positive electrode current collector, and the positive electrode current collector has a positive electrode active layer. The positive electrode active layer includes components such as a positive electrode material, a conductive agent, and a binder. The present disclosure does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive electrode current collector includes but is not limited to any one of copper foil and aluminum foil. The positive electrode active material can be a phosphate positive electrode active material and a ternary positive electrode active material. In a specific embodiment, it includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, fluorolithium vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60, and carbon nanotubes, and the content of the conductive agent in the positive electrode active layer is 3wt%-5wt%. The types of binders include one or more of polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives, and the content of the binder in the positive electrode active layer is 2wt%-4wt%.
[0103] In one embodiment, the content of the lithium-supplementing material in the positive electrode material can be controlled at 1%-6% of the mass of the positive electrode active material. This ratio can just compensate for the loss of active lithium in the battery during the first charge. If the amount of lithium-supplementing material added to the positive electrode sheet is too low, the active lithium lost in the positive electrode material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of lithium-supplementing material added to the positive electrode material is too high, it may cause lithium plating at the negative electrode to become serious and increase costs. In some specific embodiments, the mass percentage of the lithium-supplementing material in the positive electrode material can be 1%, 2%, 4%, 6%, etc.
[0104] In a fourth aspect, the present disclosure further provides a secondary battery, comprising a negative electrode plate, a separator and the above-mentioned positive electrode plate.
[0105] In one embodiment, the secondary battery is a lithium-ion secondary battery.
[0106] The disclosed embodiment of the present invention performs a surface treatment process on the lithium-supplementing material, specifically pre-coating the surface of the lithium-supplementing material and then performing atomic layer deposition to ensure the integrity and sealing of the surface packaging of the lithium-supplementing material and effectively improve the density of the lithium-supplementing material coating layer. The lithium-supplementing material that has undergone the above surface treatment has a water absorption rate of less than 50ppm / s at 25°C and 30-35% relative humidity in air, and preferably less than 10ppm / s; the water absorption rate at 25°C and 20-25% relative humidity in air is less than 20ppm / s, and more preferably less than 5ppm / s. The lithium-ion battery assembled with the lithium-supplementing material has an initial charge capacity greater than 500mAh / g, preferably greater than 600mAh / g, and can even reach more than 750mAh / g.
[0107] The technical solution of the present disclosure is described in detail below through specific embodiments.
[0108] Example 1
[0109] This embodiment provides a lithium-supplementing material and a preparation method thereof, wherein the lithium-supplementing material comprises a core, a pre-coating layer and a deposition layer. Referring to FIG7 and FIG8 , the chemical formula of the lithium-rich compound is Li 3.5 Fe 0.5 Ni 0.4 Mn 0.1 O3, the material of the pre-coating layer is titanium dioxide, and the deposited layer is an aluminum oxide nanofilm layer.
[0110] The preparation method of the lithium supplement material comprises the following steps:
[0111] (1) A certain amount of lithium hydroxide, ferric acetate, nickel acetate, and manganese acetate were weighed in a molar ratio of 3.5:0.5:0.4:0.1, and an appropriate amount of methanol solvent was added to perform liquid phase mixing. A precursor with a nano-scale porous structure was prepared using a sol-gel or coprecipitation method.
[0112] (2) The precursor prepared in (1) was sintered in a nitrogen atmosphere for 7 h at a temperature of 800 ° C and an oxygen content of less than 50 ppm to prepare Li 3.5 Fe 0.5 Ni 0.4 Mn 0.1 O3 lithium-rich compounds.
[0113] (3) The lithium-rich compound prepared in (2) is sieved and classified, and a lithium-rich compound having a particle size D10 ≥ 2 μm is selected. The lithium-rich compound, gas-phase nano-sized titanium dioxide, and graphite are solid-phase mixed in a mass ratio of 100:9:1. The mixture is then subjected to high-temperature treatment under a nitrogen atmosphere at a temperature of 600° C. for 3 hours. Thus, a first lithium-supplementing material having a core coated with a pre-coating layer is obtained.
[0114] (3) The first lithium-replenishing material prepared in (3) is placed in a reaction chamber of an atomic deposition apparatus, trimethylaluminum is first heated and vaporized to obtain gaseous trimethylaluminum, and then gaseous trimethylaluminum is introduced in a pulsed manner to deposit the first lithium-replenishing material to obtain a second lithium-replenishing material. The deposition temperature is 100° C.
[0115] In the second lithium supplement material, the mass ratio of the core, the pre-coating layer and the deposition layer is 100:10:1, the thickness of the pre-coating layer is 200 nm, the particle size of titanium dioxide is 80 nm, and the thickness of the deposition layer is 40 nm.
[0116] Example 2
[0117] The lithium-supplementing material provided in this embodiment is different from the lithium-supplementing material in Example 1 only in that, in the lithium-supplementing material provided in this embodiment, the mass ratio of the core, the pre-coating layer and the deposited layer is 100:10:5, the thickness of the pre-coating layer is 200 nm, the particle size of titanium dioxide is 80 nm, and the thickness of the deposited layer is 200 nm.
[0118] Example 3
[0119] The lithium-supplementing material provided in this embodiment is different from the lithium-supplementing material in Example 1 only in that, in the lithium-supplementing material provided in this embodiment, the mass ratio of the core, the pre-coating layer and the deposited layer is 100:10:3, the thickness of the pre-coating layer is 200 nm, the particle size of titanium dioxide is 80 nm, and the thickness of the deposited layer is 120 nm.
[0120] Example 4
[0121] The lithium-supplementing material provided in this embodiment is different from the lithium-supplementing material in Example 1 only in that the particle size of titanium dioxide in the pre-coating layer in this embodiment is 40 nm.
[0122] Example 5
[0123] The lithium-supplementing material provided in this embodiment is different from the lithium-supplementing material in Example 1 only in that the particle size of titanium dioxide in the pre-coating layer in this embodiment is 60 nm.
[0124] Example 6
[0125] The lithium-supplementing material provided in this embodiment is different from the lithium-supplementing material in Example 1 only in that the deposited layer in this embodiment is an aluminum oxide nanofilm layer.
[0126] Example 7
[0127] The lithium-supplementing material provided in this embodiment is different from the lithium-supplementing material in Example 1 only in that the lithium-supplementing material in this embodiment includes a core and a deposition layer, but does not include a pre-coating layer.
[0128] Comparative Example 1
[0129] The lithium-supplementing material provided in this comparative example is different from the lithium-supplementing material in Example 1 only in that the lithium-supplementing material in this comparative example does not contain a pre-coating layer and a deposition layer.
[0130] Comparative Example 2
[0131] The lithium-supplementing material provided in this comparative example is different from the lithium-supplementing material in Example 1 only in that the lithium-supplementing material in this example includes a core and a coating layer, does not contain a deposition layer, and the coating layer is a carbon layer.
[0132] Test 1:
[0133] The lithium supplement materials provided in Examples 1 to 7 and the lithium supplement materials provided in Comparative Examples 1 to 2 were subjected to water absorption tests according to the following method:
[0134] (1) The ambient temperature of the experimental chamber is controlled at 25°C and the relative humidity is controlled at 20%-25% or 30%-35%.
[0135] (2) Weigh the same mass of the sample to be tested into a container and spread the sample to be tested to increase the contact area. Place the container and the sample to be tested together on the analytical balance. After the reading stabilizes, turn on the timer and record the mass of the analytical balance as the value at 0 min.
[0136] (3) Then, record the values displayed by the analytical balance at 5 min, 10 min, 15 min, and 20 min respectively, and calculate the average absorption data from 10 min to 20 min.
[0137] The calculation formula for the water absorption rate of lithium supplement materials is as follows:
[0138] V=(W t2 -W t1 ) / (W0·(T2-T1)); unit: ppm / s;
[0139] Where W0 is the initial weight of the sample to be tested, W t1 is the weight at T1 (10 min), W t2 is the weight at T2 (20 min).
[0140] Test 2:
[0141] The lithium supplement materials provided in Examples 1 to 7 and the lithium supplement materials provided in Comparative Examples 1 and 2 were assembled into positive electrodes and lithium-ion batteries respectively according to the following methods:
[0142] Positive electrode: The lithium supplement material, SP and PVDF were mixed in a mass ratio of 90:4:6 to prepare a positive electrode slurry. The positive electrode slurry was coated on the surface of aluminum foil, vacuum dried at 110°C overnight, and roller pressed to obtain a positive electrode sheet.
[0143] Negative electrode: lithium sheet;
[0144] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte. The concentration of LiPF6 was 1 mol / L.
[0145] Diaphragm: Polypropylene microporous separator;
[0146] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of graphite negative electrode sheet - diaphragm - electrolyte - positive electrode sheet.
[0147] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery embodiment was tested under the following test conditions:
[0148] Constant current and constant voltage charging, the first cycle charge and discharge voltage is 2.5-4.3V, the current is 0.1C, and the cut-off current is 0.01C.
[0149] The test results of the above lithium supplement materials and lithium ion batteries are shown in Table 1 below:
[0150] Table 1
[0151] It can be seen from the SEM image and TEM image of Example 1 (Figures 7 and 8) that the method provided by the present invention can achieve good coating of lithium-rich compounds. Among them, the SEM image of Figure 7 shows a state in which the lithium-replenishing material is only coated with a pre-coating layer, and its outer surface is relatively rough, so it can provide a good environment for the subsequent coating of the sedimentary layer; and because the pre-coating layer provides more attachment sites for the sedimentary layer, a more uniform coating of the sedimentary layer can be achieved. The TEM image of Figure 8 shows a state in which the lithium-replenishing material is coated with a sedimentary layer, wherein A is the core, B is the pre-coating layer, and C is the sedimentary layer. It can be seen from the figure that the pre-coating layer and the sedimentary layer achieve uniform and complete coating of the core, thereby concluding that pre-setting a pre-coating layer is beneficial to improving the uniformity of the sedimentary layer.
[0152] The test results of Example 1, Example 7, and Comparative Example 1 in Table 1 show that the water absorption rate of the lithium-supplementing material coated with the deposited layer has been significantly reduced, while still maintaining high electrochemical performance. Furthermore, the use of a pre-coating layer further enhances the lithium-supplementing material's resistance to water absorption, demonstrating that the provision of a pre-coating layer can enhance the coating effect of the deposited layer. Therefore, the lithium-supplementing material provided by the present disclosure can have a longer shelf life and exhibit superior product performance after storage.
[0153] The test results of Example 1 and Comparative Example 2 in Table 1 show that lithium-supplementing materials with only a pre-coating layer cannot achieve high resistance to water absorption. In other words, the pre-coating layer cannot provide dense protection for the core. Therefore, it is necessary to combine the pre-coating layer with the deposition layer to obtain a lithium-supplementing material with high resistance to water absorption.
[0154] From the test results of Examples 1 to 3 in Table 1, it can be seen that the thickness of the deposited layer is directly related to the water absorption resistance of the lithium-supplementing material. When the thickness of the deposited layer is greater (or the mass ratio of the deposited layer is greater), the water absorption rate of the material is slower (the water absorption resistance is stronger). However, the thickness of the deposited layer is inversely proportional to the capacity of the secondary battery; this is because the thicker the deposited layer, the stronger the hindrance to lithium ion release, which will lead to a decrease in the electrical performance of the secondary battery. Therefore, in industrial production, the thickness of the deposited layer can be appropriately adjusted according to the required storage time of the lithium-supplementing material or the required electrochemical performance of the lithium-supplementing material.
[0155] The test results of Examples 1 and 4-5 in Table 1 show that the size of the nano-oxide particles used in the pre-coating layer is also related to the lithium-supplementing material's resistance to water absorption. Specifically, the smaller the nano-oxide particle size, the better the lithium-supplementing material's resistance to water absorption.
[0156] It can be seen from the test results of Example 1 and Example 6 in Table 1 that the solution provided by the present disclosure can be applied to deposition layers composed of different materials.
[0157] In the description of the embodiments of the present disclosure, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", and "outside" are based on the orientation or positional relationship of the accompanying drawings, which is only for the convenience of describing the present disclosure and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present disclosure.
[0158] The above disclosure is only a preferred embodiment of the present disclosure, and it is certainly not intended to limit the scope of the rights of the present disclosure. A person skilled in the art can understand that all or part of the processes of the above embodiment and equivalent changes made in accordance with the claims of the present disclosure are still within the scope of the present disclosure.
Claims
1. A lithium supplement material, It is characterized in that include: a core including a lithium-rich compound; The deposition layer is coated on the outer layer of the inner core, and the deposition layer is a film layer below the nanometer level.
2. The lithium supplement material according to claim 1, It is characterized in that The deposited layer includes a single atomic deposited layer and / or an oxide nanofilm layer obtained by atomic layer deposition technology; and / or the density ρ1 of the deposited layer satisfies the relationship: 2 g / cm 3 ≤ρ1≤4.2g / cm 3 .
3. The lithium supplement material according to claim 1, It is characterized in that The lithium supplement material further includes a pre-coating layer, which is coated on the outer surface of the inner core, and the deposition layer is coated on the outer surfaces of the inner core and the pre-coating layer.
4. The lithium supplement material according to claim 3, It is characterized in that The pre-coating layer is a continuous layer formed by connecting a plurality of oxide particles to each other.
5. The lithium supplement material according to claim 4, It is characterized in that The particle size of the oxide particles is smaller than the particle size of the core.
6. The lithium supplement material according to claim 5, It is characterized in that The deposition layer is a film layer composed of nano-scale and smaller-than-nano-scale depositions, and the particle size of the depositions is smaller than the particle size of the oxide.
7. The lithium supplement material according to claim 3, It is characterized in that The density ρ2 of the pre-coating layer satisfies the relationship: 1.5 g / cm 3 ≤ρ2≤3g / cm 3 ; and / or, the density of the deposited layer is greater than the density of the pre-coating layer; And / or, the particle size D10 of the core satisfies the relationship: D10 ≥ 2 μm; And / or, the specific surface area S1 of the core satisfies the relationship: S1≤3m 2 / g.
8. The lithium supplement material according to claim 3, It is characterized in that The pre-coating layer has a gap, and at least a portion of the deposited layer fills the gap; And / or, at least a portion of the deposited layer is directly coated on the outer surface of the inner core.
9. The lithium supplement material according to claim 3, It is characterized in that The pre-coating layer includes oxide particles and a lubricant mixed with each other.
10. The lithium supplement material according to claim 9, It is characterized in that and / or, the mass ratio of the oxide particles to the lubricant is 1:(0.1-0.8); And / or, the particle size of the oxide particles is 1 nm to 100 nm; And / or, the specific surface area S2 of the oxide particles satisfies the relationship: S2 ≥ 50m 2 / g.
11. The lithium supplement material according to claim 9, It is characterized in that The lubricant includes at least one of graphite and boron nitride.
12. The lithium supplement material according to any one of claims 3 to 11, It is characterized in that The mass ratio of the core, the pre-coating layer and the deposition layer is 100:(0.01-10):(0.01-5); and / or, the thickness A1 of the pre-coating layer is 1 nm to 200 nm; And / or, the thickness A2 of the deposited layer is 1 nm to 200 nm; And / or, the thickness of the pre-coating layer and the deposition layer satisfy the relationship: 1≤A1 / A2≤40.
13. The lithium supplement material according to claim 1, It is characterized in that The lithium supplement material further includes a carbon layer, and the carbon layer is coated on the outer layer of the deposition layer; And / or, the inner core is a secondary particle, the secondary particle includes a plurality of primary particles, and there are sediments between the primary particles in the secondary particles.
14. A method for preparing a lithium supplement material, It is characterized in that include: The lithium source and the first metal source are uniformly mixed and then sintered together to obtain a lithium-rich compound; The sediment is arranged on the outer layer of the lithium-rich compound to obtain a lithium-supplementing material; the lithium-supplementing material comprises a core and a sedimentation layer, the core comprises the lithium-rich compound, and the sediment forms the sedimentation layer.
15. The method for preparing the lithium supplement material according to claim 14, It is characterized in that The step of placing the sediment on the outer layer of the lithium-rich compound to obtain the lithium-supplementing material comprises: The lithium-rich compound and the oxide particles are mixed in a solid phase and then treated at a high temperature to obtain a first lithium supplement material, wherein the first lithium supplement material includes the core and a pre-coating layer coated on the outer surface of the core; The sediment is disposed on the outer surface of the first lithium supplementing material to obtain a second lithium supplementing material, and the sediment layer is coated on the outer surface of the inner core and the pre-coating layer.
16. The method for preparing the lithium supplement material according to claim 15, It is characterized in that The step of mixing the lithium-rich compound and the oxide particles in a solid phase and then subjecting them to high temperature treatment further comprises: The lithium-rich compound, oxide particles and lubricant are mixed in a solid phase and then treated at high temperature.
17. The method for preparing the lithium supplement material according to claim 16, It is characterized in that The high temperature treatment temperature after solid phase mixing of the lithium-rich compound, the oxide particles and the lubricant is 400° C. to 700° C., and the high temperature treatment time is 1 hour to 6 hours.
18. The method for preparing the lithium supplement material according to claim 15, It is characterized in that The step of placing the deposit on the outer surface of the first lithium supplementing material further comprises: The first lithium-replenishing material is placed in a reaction chamber of an atomic deposition device, and the atomic deposition agent is first heated and vaporized to obtain the atomic deposition agent in gas phase, and then the atomic deposition agent in gas phase is introduced in a pulse form to deposit the first lithium-replenishing material, wherein the atomic deposition agent is a precursor of the deposit.
19. A positive electrode sheet, It is characterized in that The positive electrode plate includes a current collector and an active material layer arranged on the current collector, the active material layer includes a positive electrode material and a lithium supplement material as described in any one of claims 1 to 13; or, the active material layer includes a positive electrode material and a lithium supplement material obtained by the preparation method of a lithium supplement material as described in any one of claims 14 to 18.
20. A secondary battery, It is characterized in that The secondary battery comprises a negative electrode sheet, a separator and the positive electrode sheet as claimed in claim 19.
Citation Information
Patent Citations
Positive electrode lithium supplementing material with core-shell structure as well as preparation and application of material
CN111682181A
Positive electrode lithium supplementing material and preparation method and application thereof
CN115000536A
Lithium supplement additive and preparation method and application thereof
CN115188957A
Positive electrode lithium supplement composite additive and preparation method and application thereof
CN115312768A
Lithium supplement material and preparation method thereof, positive pole piece and secondary battery
CN116525825A
Cited By
Positive pole piece and preparation method thereof, battery and power-related equipment
CN120784270A
Lithium supplement agent and preparation method thereof
CN122338074A
A lithium supplement and a method for preparing the same
CN122338074B