Semi-aromatic polyamide resin, composite material, preparation method therefor, and use thereof

By introducing branched benzoic acid compounds and combining flame retardants and reinforcing materials into semi-aromatic polyamide materials, the contradiction between material fluidity and temperature resistance is solved, and high fluidity, flame retardancy and resistance are achieved. High-temperature composite materials are suitable for high-temperature electronic components such as connectors.

WO2024217376A1PCT designated stage expired Publication Date: 2024-10-24ZHUHAI WANTONG SPECIAL ENG PLASTICS CO LTD

Patent Information

Application Number
PCT/CN2024/087740
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-15
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

When improving the fluidity of existing semi-aromatic polyamide materials, it is easy to cause problems such as reduced temperature resistance, casting, foaming and high temperature resistance, making it difficult to meet the miniaturization and high-temperature application requirements of connector products.

Method used

By introducing a branched benzoic acid compound as an end-capping agent to spread the chain segments and improve the fluidity of the material, and combining flame retardants and reinforcing materials in the composite material, a composite material with ultra-high fluidity and resistance to reflow soldering is produced. Semi-aromatic polyamide resin and composite materials with foaming properties and high heat resistance.

Benefits of technology

The material has achieved ultra-high fluidity, a flame retardant grade of V-0, a melting point exceeding 304.3°C, and no foaming, meeting the requirements of SMT processes and high-temperature applications, while simplifying the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024087740_24102024_PF_FP_ABST
    Figure CN2024087740_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a semi-aromatic polyamide resin, a composite material, a preparation method therefor, and the use thereof, belonging to the technical field of polymer materials. The semi-aromatic polyamide resin provided by the present invention contains a diamine unit, a diacid unit, and an end-capping structure derived from formula 1, wherein the molar ratio of the compound of formula 1 to the diacid unit is (0.01-0.03):1. When the semi-aromatic polyamide resin prepared by the present invention is applied to preparation of a semi-aromatic polyamide composite material, the obtained composite material has the characteristics of ultrahigh fluidity, flame retardance, high-temperature resistance and foaming resistance, can be applied to manufacturing of new energy, 5G communication and electronic and electrical parts, and satisfies the requirements of an SMT process. In addition, the preparation method provided by the present invention is simple and facilitates actual production.
Need to check novelty before this filing date? Find Prior Art

Description

A semi-aromatic polyamide resin and composite material and preparation method and application thereof Technical Field

[0001] The present invention belongs to the technical field of polymer materials, and in particular relates to a semi-aromatic polyamide resin and composite material, and a preparation method and application thereof. Background Art

[0002] In recent years, with the increasing density and miniaturization of electronic products, lead-free surface mount technology (SMT) has become a crucial assembly method. Its application requires components to withstand temperatures of 250-280°C. Traditional engineering plastics such as PA66 and PBT simply cannot meet this requirement, leading to the emergence of high-temperature-resistant engineering plastics. Semi-aromatic polyamide (PPA) is widely used in connectors due to its high melting point, high heat deformation temperature, and high strength.

[0003] Due to the miniaturization of connector products, extremely high requirements are placed on the fluidity of PPA materials. Generally speaking, there are two main methods to improve the fluidity of the material: one is to reduce the molecular weight of the resin, thereby reducing its viscosity, to achieve a high fluidity effect, such as CN 201910128425. However, this method easily reduces the thermal stability of the material, and continuous injection molding at high temperatures can easily produce a large amount of mold deposits, and even cause bubbling during the SMT process. Another method is to add a third or even a fourth monomer to PPA to lower the melting point of the material to achieve the effect of meeting the high fluidity requirement; however, if the addition amount is small, it will not improve the processing effect, and if the addition amount is large, it will easily lead to a low melting point and poor thermal stability. There are even attempts to add aliphatic nylon to the system, and then improve the compatibility of high-temperature nylon and aliphatic nylon by adding a compatibilizer, such as CN201610892639. However, these methods all reduce the material's heat resistance and even increase its water absorption. While this improves processing performance, it can also lead to casting (due to the significant difference in processing temperature between semi-aromatic and aliphatic nylons) and blistering (due to the high-temperature injection molding of aliphatic nylons producing large amounts of gas). Other approaches, such as CN202110730705, improve the material's fluidity by adding lubricants like hyperbranched materials. However, hyperbranched materials have low heat resistance and are prone to decomposition during PPA extrusion and processing, leading to blistering during the SMT process.

[0004] That is, in the prior art, although the fluidity of the material can be improved to a certain extent through various methods, it is inevitable that the material will experience phenomena such as casting, bubbling, and heat resistance.

[0005] Summary of the Invention

[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a semi-aromatic polyamide resin with ultra-high fluidity, resistance to reflow soldering blistering, and high heat resistance, and at the same time provide a semi-aromatic polyamide composite material that has ultra-high fluidity, resistance to reflow soldering blistering, and high heat resistance on the basis of flame retardancy, as well as its preparation method and application.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a semi-aromatic polyamide resin, wherein the semi-aromatic polyamide resin has a diamine unit, a diacid unit, and an end-capping structure derived from Formula 1;

[0008] Wherein, R1, R2 and R3 are each independently at least one of a hydrogen atom, an alkane group having 1 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms, and R1, R2 and R3 are not hydrogen atoms at the same time.

[0009] The semi-aromatic polyamide resin provided by the present invention incorporates specific end-capping groups, specifically a branched benzoic acid compound, as an end-capping agent, which acts to expand the chain segments, thereby achieving ultra-high fluidity. Furthermore, when subsequently applied to semi-aromatic polyamide composites, the resin meets flame retardancy and high-temperature resistance requirements, while also exhibiting blister resistance. The resulting semi-aromatic polyamide composites all achieved a V-0 flame retardancy rating, flowability exceeding 38 mm, a melting point above 304.3°C, and exhibited no blistering during testing.

[0010] As a preferred embodiment of the semi-aromatic polyamide resin of the present invention, the molar ratio of the compound of formula 1 to the diacid unit is (0.01-0.03):1.

[0011] Preferably, the molar ratio of the compound of formula 1 to the diacid unit is 0.03:1.

[0012] The inventors have found that when the molar ratio of the compound of formula 1 to the diacid unit is further selected to be (0.01-0.03):1, especially when the molar ratio of the compound of formula 1 to the diacid unit is further preferably 0.03:1, when it is applied to the subsequent preparation of a composite material, the overall effect of the obtained composite material is even better.

[0013] As a preferred embodiment of the semi-aromatic polyamide resin of the present invention, the amine-carboxyl ratio of the diamine unit to the diacid unit is (1.005-1.08):1.

[0014] As a preferred embodiment of the semi-aromatic polyamide resin of the present invention, the alkyl group having 1 to 6 carbon atoms is at least one of methyl, ethyl, n-butyl, tert-butyl, n-pentyl, and isopentyl; the alkoxy group having 1 to 6 carbon atoms is at least one of methoxy, ethoxy, propoxy, and butoxy.

[0015] As a preferred embodiment of the semi-aromatic polyamide resin of the present invention, the compound represented by Formula 1 is a compound represented by the following structural formulas I-V:

[0016] As a preferred embodiment of the semi-aromatic polyamide resin of the present invention, the compound represented by Formula 1 is a compound represented by Structural Formula III and Structural Formula IV.

[0017] The inventors have found that when the structural formula of the end-capping agent is further preferably the compound represented by Structural Formula III and Structural Formula IV, it can better play the role of stretching the chain segments, thereby achieving better fluidity; and thus, when the obtained semi-aromatic polyamide resin is used in the subsequent preparation of a semi-aromatic polyamide composite material, the overall performance of the obtained composite material is even better. Specifically, the flow performance of the obtained composite material is above 58 mm.

[0018] As a preferred embodiment of the semi-aromatic polyamide resin of the present invention, the diamine unit is at least one monomer of an aliphatic diamine having a carbon number ≥ 9, the diacid unit is 45-100% of an aromatic dicarboxylic acid and 0-55% of an aliphatic dicarboxylic acid; the aliphatic diamine is selected from 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2-methyl-1,8-octanediamine, 5- The present invention relates to a method for preparing an aromatic dicarboxylic acid selected from at least one of terephthalic acid, isophthalic acid, 2-methylterephthalic acid, 2,5-dichloroterephthalic acid, 2,6-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, and 2,2'-biphenyl dicarboxylic acid; and the present invention relates to a method for preparing an aromatic dicarboxylic acid selected from at least one of 1,4-butanediol, 1,6-hexanediol, 1,8-octanedioic acid, 1,9-nonanediol, 1,10-decanedioic acid, 1,11-undecanedioic acid, and 1,12-dodecane dicarboxylic acid.

[0019] Preferably, the diamine unit is at least one monomer of an aliphatic diamine having 9 to 12 carbon atoms.

[0020] As a preferred embodiment of the semi-aromatic polyamide resin of the present invention, the aliphatic diamine is selected from at least one of 1,9-nonanediamine, 1,10-decanediamine, and 1,12-dodecanediamine, and the aromatic dicarboxylic acid is selected from at least one of terephthalic acid and isophthalic acid.

[0021] Preferably, the aliphatic diamine is selected from at least one of 1,10-decanediamine and 1,12-dodecanediamine, and the aromatic dicarboxylic acid is selected from terephthalic acid.

[0022] The inventors have found that when aliphatic diamines and aromatic dicarboxylic acids are further preferred as the above substances, the obtained resin has better fluidity; and when the obtained semi-aromatic polyamide resin is used in the subsequent preparation of semi-aromatic polyamide composite materials, the comprehensive performance of the obtained composite material is even better.

[0023] In addition, the present invention also provides a method for preparing the semi-aromatic polyamide resin, which comprises the following steps:

[0024] (1) adding measured amounts of diamine units, diacid units, end-capping agents, antioxidants, and catalysts into an autoclave, and polymerizing under pressure and heating under inert gas protection to obtain a prepolymer;

[0025] (2) The prepolymer is solid-phase thickened to obtain a semi-aromatic polyamide resin.

[0026] As a preferred embodiment of the preparation method of the present invention, in step (1), the amount of antioxidant added is 1-4‰ of the total mass of the substance, and the amount of catalyst added is 0.5-2‰ of the total mass of the substance.

[0027] Preferably, the antioxidant is 1098 antioxidant, and the catalyst is sodium hypophosphite catalyst.

[0028] As a preferred embodiment of the preparation method of the present invention, in step (1), the polymerization reaction temperature is 230-240° C., the polymerization reaction pressure is 2.9-3.1 MPa, and a constant pressure of 2.9-3.1 MPa is maintained during the polymerization reaction by removing the formed water.

[0029] As a preferred embodiment of the preparation method of the present invention, in step (2), the temperature of solid phase viscosity enhancement is 240-250° C., and the time is 1-3 hours.

[0030] In addition, the present invention also provides a semi-aromatic polyamide composite material, which includes the following components in parts by mass: 35-50 parts of the semi-aromatic polyamide resin, 12-22 parts of the flame retardant, and 15-50 parts of the reinforcing material; the flame retardant is at least one of a phosphinate flame retardant and a dialkyl phosphinate flame retardant.

[0031] The inventors have found that using the semi-aromatic polyamide resin provided by the present invention as a component to prepare a semi-aromatic polyamide resin composite material can make the obtained composite material have ultra-high fluidity, flame retardancy, high temperature resistance, and excellent anti-foaming performance.

[0032] As a preferred embodiment of the semi-aromatic polyamide composite material of the present invention, the semi-aromatic polyamide composite material includes the following components in parts by mass: 40 parts of semi-aromatic polyamide resin, 15-20 parts of flame retardant, and 20-30 parts of reinforcing material.

[0033] The inventors have found that when the addition amount of the components is further preferably within the above range, the comprehensive performance of the obtained composite material is even better.

[0034] As a preferred embodiment of the semi-aromatic polyamide composite material of the present invention, the reinforcing material is at least one of glass fiber, carbon fiber, asbestos fiber, wollastonite fiber, ceramic fiber, potassium titanate whisker, basic magnesium sulfate whisker, silicon carbide whisker, aluminum borate whisker, silica, aluminum silicate, silicon oxide, calcium carbonate, titanium dioxide, talc, wollastonite, diatomaceous earth, clay, kaolin, spherical glass, mica, and gypsum.

[0035] Preferably, the reinforcing material is glass fiber; the inventors have found that when the reinforcing material is further preferably glass fiber, the comprehensive performance of the obtained product is even better.

[0036] In addition, the present invention also provides a method for preparing the semi-aromatic polyamide composite material, which comprises the following steps: mixing the raw materials, melt-extruding, cooling, air-drying, and granulating to obtain the semi-aromatic polyamide composite material.

[0037] As a preferred embodiment of the preparation method of the present invention, the preparation process is specifically as follows: a semi-aromatic polyamide resin is added to an extruder from a main feed port, a reinforcing material is added to the extruder from a first side feed port, and a flame retardant is added to the extruder from a second side feed port. After the addition is completed, the mixture is melt-blended at 250-350°C, and then cooled, air-dried, and granulated to obtain a semi-aromatic polyamide composite material.

[0038] In addition, the present invention also provides an application of the semi-aromatic polyamide composite material in the preparation of components for new energy, 5G communications, and electronic and electrical applications. For example, the semi-aromatic polyamide composite material of the present invention is used in DDR connectors and high-voltage connectors.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The semi-aromatic polyamide resin provided by the present invention introduces a branched benzoic acid compound as a capping agent to achieve the effect of stretching chain segments, thereby achieving an ultra-high fluidity effect. When the obtained semi-aromatic polyamide resin is used in a subsequent semi-aromatic polyamide resin composite material, the obtained composite material can also have ultra-high fluidity, meet the requirements of flame retardancy and high temperature resistance, and has the characteristics of foaming resistance. Specifically, the obtained semi-aromatic polyamide composite materials have a flame retardancy grade of V-0, a fluidity of more than 38 mm, a melting point of more than 304.3°C, and do not produce serious deformation during testing. Therefore, the obtained semi-aromatic polyamide composite materials can be used in the preparation of parts for electronic, electrical or electrical products, and meet the requirements of the SMT process. At the same time, the preparation method provided by the present invention is simple and conducive to actual production. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] FIG1 is a schematic diagram of thin-walled elongated strips used in the flowability test process of the effect example;

[0042] FIG2 is a diagram showing the effect of the foaming test in which no foaming occurs;

[0043] FIG3 is a diagram showing the foaming phenomenon in the foaming test in the effect example;

[0044] FIG4 is a diagram showing a severe deformation in a foaming test in an effect example. DETAILED DESCRIPTION

[0045] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0046] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0047] PA66: PA66 EPR24, Shenma Group, China;

[0048] Flame retardant 1: aluminum diethylphosphinate, commercially available;

[0049] Flame retardant 2: zinc diethylphosphinate, commercially available;

[0050] Flame retardant 3: melamine polyphosphate, commercially available;

[0051] Reinforcement material: Glass fiber, commercially available.

[0052] Example 1

[0053] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-1, wherein the diamine unit is 1,10-decanediamine, the diacid unit is terephthalic acid, and the end-capping agent is a compound represented by structural formula I;

[0054] The preparation method of PA10T-1 comprises the following steps: adding measured materials (the amine-carboxyl ratio of the diamine unit to the diacid unit is 1.05, and the amount of the end-capping agent is 0.03 times the molar amount of the diacid unit) into a 20 L autoclave; and adding 2‰ (total mass) of 1098 antioxidant and 1‰ (total mass) of sodium hypophosphite catalyst. After the addition is completed, vacuuming and nitrogen replacement are performed, and then heating to a predetermined temperature of 235° C. while maintaining a constant pressure of 3.0 MPa by removing formed water. After the reaction is completed, the pressure is released to normal pressure to obtain a prepolymer; and the prepolymer is subjected to solid-phase viscosity-increasing in a rotary drum at 245° C. for 2 hours to obtain PA10T-1.

[0055] Example 2

[0056] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-2, wherein the diamine unit is 1,10-decanediamine, the diacid unit is terephthalic acid, and the end-capping agent is a compound represented by structural formula II. The preparation method of the PA10T-2 is the same as that of Example 1.

[0057] Example 3

[0058] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-3, wherein the diamine unit is 1,10-decanediamine, the diacid unit is terephthalic acid, and the end-capping agent is a compound represented by structural formula III. The preparation method of the PA10T-3 is the same as that of Example 1.

[0059] Example 4

[0060] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-4, wherein the diamine unit is 1,10-decanediamine, the diacid unit is terephthalic acid, and the end-capping agent is a compound represented by structural formula IV. The preparation method of the PA10T-4 is the same as that of Example 1.

[0061] Example 5

[0062] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-5, wherein the diamine unit is 1,10-decanediamine, the diacid unit is terephthalic acid, and the end-capping agent is a compound represented by structural formula V. The preparation method of the PA10T-5 is the same as that of Example 1.

[0063] Example 6

[0064] The embodiment of the present invention provides a semi-aromatic polyamide resin PA12T, wherein the diamine unit is 1,12-dodecanediamine, the diacid unit is terephthalic acid, and the end-capping agent is a compound represented by structural formula IV. The preparation method of the PA12T is the same as that of Example 1.

[0065] Example 7

[0066] An embodiment of the present invention provides a semi-aromatic polyamide resin PA6T / 66, wherein the diamine unit is hexamethylenediamine, the diacid units are 1,6-adipic acid and terephthalic acid (the molar ratio of terephthalic acid to 1,6-adipic acid is 60:40), and the end-capping agent is a compound represented by structural formula IV. The preparation method of the PA6T / 66 is the same as that in Example 1.

[0067] Example 8

[0068] The embodiment of the present invention provides a semi-aromatic polyamide resin PA9T, wherein the diamine unit is 1,9-nonanediamine, the diacid unit is terephthalic acid, and the end-capping agent is a compound represented by structural formula IV. The preparation method of PA9T is the same as that of Example 1.

[0069] Example 9

[0070] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-7. The only difference between the embodiment of the present invention and Example 1 is that the amount of the end-capping agent added during the preparation of the semi-aromatic polyamide resin is 0.01 times the molar amount of the diacid unit.

[0071] Example 10

[0072] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-8. The only difference between the embodiment of the present invention and Example 1 is that the amount of the end-capping agent added during the preparation of the semi-aromatic polyamide resin is 0.02 times the molar amount of the diacid unit.

[0073] Example 11

[0074] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-9. The only difference between the embodiment of the present invention and Example 1 is that the amount of the end-capping agent added during the preparation of the semi-aromatic polyamide resin is 0.008 times the molar amount of the diacid unit.

[0075] Example 12

[0076] The embodiment of the present invention provides a semi-aromatic polyamide resin PA10T-10. The only difference between the embodiment of the present invention and Example 1 is that the amount of the end-capping agent added during the preparation of the semi-aromatic polyamide resin is 0.04 times the molar amount of the diacid unit.

[0077] Comparative Example 1

[0078] The comparative example of the present invention provides a semi-aromatic polyamide resin PA10T-6, wherein the diamine unit is 1,10-decanediamine, the diacid unit is terephthalic acid, and the end-capping agent is benzoic acid. The preparation method of the PA10T-6 is the same as that of Example 1.

[0079] Examples 13-29 and Comparative Examples 2-6

[0080] Examples 13-29 of the present invention and comparative examples 2-6 provide a semi-aromatic polyamide composite material, the component contents of the semi-aromatic polyamide composite material are shown in Table 1-2;

[0081] Table 1

[0082] Table 2

[0083] The preparation methods of the semi-aromatic polyamide composite materials provided in Examples 13-29 and Comparative Examples 2-6 are as follows:

[0084] The semi-aromatic polyamide resin is added into the extruder from the main feeding port, the reinforcing material is added into the extruder from the first side feeding port, and the flame retardant is added into the extruder from the second side feeding port. After the addition is completed, the mixture is melt-blended at 250-350°C, and then cooled, air-dried, and granulated to obtain a semi-aromatic polyamide composite material.

[0085] Effect Examples

[0086] This effect example tests the properties of the semi-aromatic polyamide composite materials prepared in Examples 13-29 and Comparative Examples 2-6; specifically, the following tests are included:

[0087] 1. Flame retardant performance test: The semi-aromatic polyamide composite material was dried at 120°C for 4 hours and then injection molded according to the standard test. The flame retardant performance test was conducted on the specimen with a thickness of 0.8 mm according to the UL-94 standard;

[0088] 2. Flowability Test: The pellets were molded into thin-walled elongated strips using an injection molding machine equipped with a thin-walled elongated strip mold at a barrel temperature of 20°C above the melting point, a mold temperature of 120°C, an injection pressure of 90 MPa, and an injection speed of 75% to obtain elongated strips with a wall thickness of 0.5 mm. The flowability of the polymer composition was observed by measuring the sample length. The thin-walled elongated strips are shown in Figure 1.

[0089] 3. Blistering test: Injection mold a 60*60*1.0mm square plate and place it under high temperature and high humidity conditions of 85℃ / 85%RH for 168 hours. Then place the test piece in a SER-710A equipment from Unisplendour Suneast Technology (Shenzhen) Co., Ltd. and heat it from room temperature to 150℃ in 45 seconds, then from 150℃ to 200℃ in 135 seconds. Then, heat it to 260℃ at a maximum temperature rise rate of 3℃ / s, with the temperature above 255℃ for 20-40 seconds. Then, cool it to room temperature at a maximum temperature drop rate of 6℃ / s. Remove the test piece and observe whether there is any blistering (Figure 2 shows no blistering, Figure 3 shows blistering, and Figure 4 shows severe deformation).

[0090] 4. Melting point test: According to ISO 11357-1 / -3-2011, place the sample in a NETZSCH DSC214 and, under a nitrogen atmosphere, heat the sample from room temperature to the melting point + 20°C at a rate of 10°C / min, then cool the sample to room temperature at a rate of 10°C / min, and then heat the sample to the melting point + 20°C at a rate of 10°C / min. Measure the data for the second heating cycle.

[0091] The test results are shown in Table 3;

[0092] Table 3

[0093] As can be seen from the data in Table 3, when the technical solution of the present invention is adopted, the obtained semi-aromatic polyamide composite material has not only flame retardancy, but also ultra-high fluidity, high heat resistance and blister resistance. Specifically, the obtained fluidity data is above 38 mm, the obtained melting point is above 304.3°C, and the obtained product does not produce serious deformation in the blister resistance test.

[0094] It can be seen from Examples 13-17 and Comparative Examples 2-3 that the addition ratio of the semi-aromatic polyamide resin, flame retardant, and reinforcing material will affect the performance of the product. When the addition ratio of the semi-aromatic polyamide resin is further preferably 40 parts, the flame retardant is 15-20 parts, and the reinforcing material is 20-30 parts, the comprehensive performance of the obtained product is more excellent. Specifically, the obtained fluidity is above 46 mm and the melting point is above 314.3°C. When the addition ratio of the components is not within the range given in the present invention, the comprehensive performance of the obtained product shows a significant downward trend. For example, when the addition ratio of the flame retardant in Comparative Example 2 is too low, the flame retardant performance of the obtained product is significantly reduced, and only V-2 cannot be achieved. For example, when the addition ratio of the reinforcing material in Comparative Example 3 is too low, the fluidity and melting point of the obtained product are better, but the blistering resistance of the product is significantly reduced, and the test results show that blistering occurs.

[0095] It can be seen from Example 13, Example 18 and Comparative Example 4 that the choice of flame retardant will also affect the performance of the product. When the flame retardant provided by the present invention is not selected, the comprehensive performance of the obtained product is significantly reduced, which is reflected in the significant reduction in flame retardancy, which is only less than V-2.

[0096] It can be seen from Example 13, Examples 19-22 and Comparative Example 5 that when the end-capping agent provided by the present invention is used as the end-capping group, the comprehensive performance of the obtained product is excellent, especially when the compounds represented by Structural Formula III and Structural Formula IV are further selected, the comprehensive performance of the obtained product is even better. Specifically, the fluidity of the obtained product is above 58 mm and the melting point is above 312.3° C.; when benzoic acid is used as the end-capping agent, the fluidity of the obtained product is significantly reduced, and the reduction rate is 25.53% compared with Example 11;

[0097] As can be seen from Example 21 and Examples 23-25, the selection of diamine units and diacid units in the semi-aromatic polyamide resin also affects the performance of the product. When PA10T, PA9T, and PA12T are further selected as the semi-aromatic polyamide resin, the overall performance of the obtained product is even better, and no foaming occurs in the foaming resistance test. In particular, when PA10T is further selected as the semi-aromatic polyamide resin, the overall performance is even better, and the obtained flowability can reach 63 mm and the melting point is 312.3°C.

[0098] As can be seen from the examples and comparative example 6, the products obtained by the present invention have better flame retardancy and fluidity than traditional engineering plastics, and will not produce serious deformation during the bubble resistance test;

[0099] It can be seen from Example 13 and Examples 26-29 that, in the process of preparing the semi-aromatic polyamide resin, the amount of the end-capping agent used will also affect the performance of the product.

[0100] Finally, it should be noted that the above embodiments are intended to illustrate the technical solutions of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A semi-aromatic polyamide resin, characterized in that The semi-aromatic polyamide resin has a diamine unit, a diacid unit, and an end-capping structure derived from Formula 1; Wherein, R1, R2 and R3 are each independently at least one of a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms, and R1, R2 and R3 are not hydrogen atoms at the same time.

2. The semi-aromatic polyamide resin according to claim 1, characterized in that The molar ratio of the compound of formula 1 to the diacid unit is (0.01-0.03):

1.

3. The semi-aromatic polyamide resin according to claim 1, characterized in that The compound represented by formula 1 is a compound represented by the following structural formula I-V, 4. The semi-aromatic polyamide resin according to claim 3, characterized in that The compound represented by formula 1 is a compound represented by structural formula III and structural formula IV.

5. The semi-aromatic polyamide resin according to claim 1, characterized in that The diamine unit is at least one of aliphatic diamines having a carbon number of ≥ 9, and the diacid unit is 45-100% of an aromatic dicarboxylic acid and 0-55% of an aliphatic dicarboxylic acid; The aliphatic diamine is selected from 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2-methyl-1,8-octanediamine, The aromatic dicarboxylic acid is selected from at least one of terephthalic acid, isophthalic acid, 2-methylterephthalic acid, 2,5-dichloroterephthalic acid, 2,6-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, and 2,2'-biphenyl dicarboxylic acid; the aliphatic dicarboxylic acid is selected from at least one of 1,4-succinic acid, 1,6-hexanedicarboxylic acid, 1,8-octanedioic acid, 1,9-nonane diamine, 1,10-decanedioic acid, 1,11-undecanedioic acid, and 1,12-dodecane dioic acid.

6. The method for preparing a semi-aromatic polyamide resin according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) adding measured amounts of diamine units, diacid units, end-capping agents, antioxidants and catalysts into an autoclave, and polymerizing under pressure and heating under inert gas protection to obtain a prepolymer; (2) The prepolymer is solid-phase thickened to obtain a semi-aromatic polyamide resin.

7. A semi-aromatic polyamide composite material, characterized in that: The semi-aromatic polyamide composite material comprises the following components in parts by weight: 35-50 parts of the semi-aromatic polyamide resin according to any one of claims 1 to 5, 12-22 parts of a flame retardant, and 15-50 parts of a reinforcing material; The flame retardant is at least one of a phosphinate flame retardant and a dialkylphosphinate flame retardant.

8. The semi-aromatic polyamide composite material according to claim 7, characterized in that: The semi-aromatic polyamide composite material comprises the following components in parts by mass: 40 parts of semi-aromatic polyamide resin, 15-20 parts of flame retardant, and 20-30 parts of reinforcing material.

9. The method for preparing a semi-aromatic polyamide composite material according to claim 7 or 8, characterized in that: The preparation method comprises the following steps: mixing the raw materials, melting and extruding, cooling, air-drying and granulating to obtain a semi-aromatic polyamide composite material.

10. Application of the semi-aromatic polyamide composite material as claimed in claim 7 or 8 in the preparation of new energy, 5G communication and electronic and electrical components.

Citation Information

Patent Citations

  • Semi-aromatic polyamide preparation method capable of reducing diamine monomer loss, semi-aromatic polyamide and molding composition

    CN114058009A

  • Semi-aromatic polyamide resin and composite material as well as preparation method and application of semi-aromatic polyamide resin and composite material

    CN116355208A

  • Multi-layer bottle and method for producing the same

    JP2016169027A

  • Polyamide resin composition, and molded body obtained by molding the same

    JP2021167384A

Cited By

  • Syndiotactic polystyrene composition, application thereof and automobile connector

    CN122404972A