Lithium ion battery fast-charging negative electrode sheet, electrochemical device and electronic device
By regulating the parameters and processes of the negative electrode diaphragm of lithium-ion batteries, the problem of lithium dendrite growth during fast charging of lithium-ion batteries is solved, the fast charging capability and high-rate cycle life of the battery are improved, and high energy density and long life are achieved. .
Patent Information
- Application Number
- PCT/CN2024/088554
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
Existing lithium-ion batteries are prone to lithium dendrite growth during fast charging, resulting in reduced battery power performance and shortened battery life, as well as increased safety risks and insufficient performance in high-rate cycle life.
By designing the parameters of the negative electrode diaphragm to satisfy the relational expression 1≤W≤9 in a specific value range, the preparation process parameters of the negative electrode active material and diaphragm are controlled, including the specific surface area, median particle size, specific capacity, Compact density and surface density, optimize the combination of negative electrode current collector and conductive agent, and prepare lithium-ion battery negative electrode sheets with excellent fast charging capability and large rate cycle life.
It achieves the excellent performance and high energy density of lithium-ion batteries during fast charging, and its cycle life reaches 4524 cycles, improving the overall performance of the battery.
Smart Images

Figure PCTCN2024088554-FTAPPB-I100001
Abstract
Description
A lithium-ion battery fast-charging negative electrode sheet, electrochemical device, and electronic device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to the Chinese invention patent application filed with the China Patent Office on April 18, 2023, with application number 202310425221.2. The entire contents of the patent application are incorporated into this application by reference. Technical Field
[0003] The present application relates to the technical field of lithium battery preparation, and in particular to a lithium-ion battery fast-charging negative electrode sheet, an electrochemical device, and an electronic device. Background Art
[0004] Lithium-ion secondary batteries are currently widely used in electronic products and new energy vehicles due to their high energy density, high voltage, low self-discharge, environmental friendliness, and low cost. However, the charging time and service life of lithium-ion secondary batteries are increasingly important to end consumers and are a significant factor limiting the widespread adoption of rechargeable batteries. To shorten charging time, batteries must be capable of rapid charging. Otherwise, forced rapid charging can easily lead to the growth of lithium dendrites on the negative electrode surface, resulting in reduced battery power performance and a drastic reduction in battery life. Furthermore, the continued growth of lithium dendrites during battery use can pierce the separator, causing internal short circuits and increasing safety risks.
[0005] The negative electrode material of lithium-ion secondary batteries has a significant impact on the fast-charging performance of the battery, which is related to how much current the battery can be repeatedly charged and discharged at, while reducing the degree of deterioration of battery performance and meeting the service life requirements of lithium-ion batteries in terminal products.
[0006] CN 110459743A discloses a method for preparing a negative electrode material for a lithium-ion battery with fast charge and discharge, comprising the following steps: dissolving graphene oxide and a bisamino-substituted aromatic compound in deionized water, heating the mixture to obtain a graphene hydrogel; adding FeCl3 to the graphene hydrogel, allowing the mixture to stand and drying to obtain a graphene composite material; providing graphite, mixing the graphene composite material with the graphene composite material, and then carbonizing and removing impurities to obtain the negative electrode material for a lithium-ion battery with fast charge and discharge.
[0007] CN 109273771A discloses a secondary battery, which includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer coated on at least one surface of the negative electrode current collector and containing a negative electrode active material. The secondary battery satisfies the following conditions: 0.12≤α / (β+γ)≤0.6, where α represents the excess capacity coefficient of the battery; β represents the compaction density of the negative electrode film layer, in units of g / cm3 ;γ represents the capacitance per unit area of the negative electrode film layer, unit mAh / cm 2 .
[0008] CN 110867581A discloses a high-voltage, high-energy-density, fast-charging soft-package lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte, and an aluminum-plastic film for lithium-ion battery packaging. The positive electrode sheet comprises a positive electrode material and a current collector, and the positive electrode material is coated on the surface of the current collector. The positive electrode material comprises lithium cobalt oxide, a positive electrode conductive agent, and a binder PVDF. The surface density of the positive electrode material coating is 252-288 g / m 2 The compaction density of the positive electrode is 3.9g / cm 3 The negative electrode sheet includes a negative electrode material and a current collector. The negative electrode material is coated on the surface of the current collector. The negative electrode material includes artificial graphite, a negative electrode conductive agent, a binder CMC and a binder SBR. The surface density of the negative electrode material coating is 140-160g / m 2 The compaction density of the negative electrode is 1.6g / cm 3 .
[0009] The above applications have all made some improvements to the performance of the negative electrode materials in fast-charging batteries, so that the prepared lithium-ion batteries have better charge and discharge capabilities, but there is still room for further improvement in the high-rate cycle life.
[0010] In view of the shortcomings of the existing technology, it is necessary to provide a negative electrode sheet that enables lithium-ion batteries to have excellent fast charging capability and high-rate cycle life.
[0011] Summary of the Invention
[0012] The purpose of this application is to provide a lithium-ion battery fast-charging negative electrode sheet, electrochemical device and electronic device. By exploring the design parameters of the negative electrode active material and the negative electrode membrane, a relationship related to the performance of the lithium-ion battery is obtained. When the relationship meets the requirements of a specific value range, the resulting lithium-ion battery can have both excellent fast charging capability and high-rate cycle life.
[0013] To achieve the purpose of this application, this application adopts the following technical solutions:
[0014] In a first aspect, the present application provides a lithium-ion battery fast-charging negative electrode sheet, the lithium-ion battery fast-charging negative electrode sheet comprising a negative electrode current collector and a negative electrode film containing a negative electrode active material coated on the surface of the negative electrode current collector;
[0015] The negative electrode membrane satisfies 1≤W≤9, W=0.01×(B+D v50 )×C / (P×S);
[0016] Wherein, B is the specific surface area of the negative electrode active material measured in a pure nitrogen atmosphere, in m2 / g;
[0017] D v50 is the median particle size of the negative electrode active material, in μm;
[0018] C is the specific capacity of the negative electrode active material, in mAh / g;
[0019] P is the compaction density of the negative electrode membrane, in g / cm 3 ;
[0020] S is the surface density of the negative electrode membrane, in mg / cm 2 .
[0021] The lithium-ion battery fast-charging negative electrode sheet provided in this application is configured to regulate the preparation process parameters of the negative electrode membrane and the design parameters of the negative electrode active material so that the negative electrode membrane satisfies the relationship within a specific value range. The lithium-ion battery further obtained has excellent fast-charging capability, energy density, and high high-rate cycle life.
[0022] The negative electrode membrane satisfies 1≤W≤9, for example, it can be 1, 3, 5, 7 or 9, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] When the negative electrode diaphragm meets the limited value range, the lithium-ion battery has excellent fast charging capability, energy density and high high-rate cycle life. If W is too small or too large, it will adversely affect the fast charging performance, energy density and cycle life of the lithium-ion battery.
[0024] Preferably, the range of B is 0.7≤B≤2.5, for example, it can be 0.7, 1, 1.5, 2 or 2.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] B is the specific surface area of the negative electrode active material measured in a pure nitrogen atmosphere, wherein the purity of the nitrogen is ≥99.9%. If the specific surface area is too small, the active sites for lithium ion reaction will be reduced. If the specific surface area is too large, the consumption of the dispersant will be increased when preparing the slurry and the side reactions will be increased during the first charge and discharge process.
[0026] Preferably, the D v50 The range is 7≤D v50 ≤18, for example, it can be 7, 10, 12, 15 or 18, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] The D v50It is the median particle size of the negative electrode active material. If the particle size is too small, the compaction density of the negative electrode membrane will be reduced. If the particle size is too large, the prepared negative electrode slurry will easily agglomerate particles. Therefore, the median particle size range of the negative electrode active material needs to be limited.
[0028] Preferably, the range of C is 330≤C≤370, for example, it can be 330, 340, 350, 360 or 370, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] The C is the specific capacity of the negative electrode active material. If the specific capacity is too small, the energy density of the lithium-ion battery will be reduced. If the specific capacity is too large, the cycle life of the lithium-ion battery will be significantly shortened.
[0030] Preferably, the range of P is 1.3≤P≤1.8, for example, it can be 1.3, 1.4, 1.5, 1.6 or 1.8, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] P is the compaction density of the negative electrode membrane. A too low compaction density will reduce the energy density of the lithium-ion battery. A too high compaction density will affect the electrolyte infiltration rate and reduce the porosity, thereby affecting lithium ion migration. Therefore, it is necessary to limit the compaction density range of the negative electrode membrane.
[0032] Preferably, the range of S is 5≤S≤15, for example, it can be 5, 8, 10, 12 or 15, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] The S is the surface density of the negative electrode membrane. If the surface density is too low, the energy density of the lithium-ion battery will be reduced. If the surface density is too high, the lithium ion insertion path will be increased, resulting in incomplete capacity utilization. Therefore, the surface density range of the negative electrode membrane needs to be strictly limited.
[0034] Preferably, the negative electrode active material includes any one or a combination of at least two of artificial graphite, natural graphite, hard carbon, soft carbon, silicon oxide material and silicon carbon material. Typical but non-limiting combinations include a combination of artificial graphite and natural graphite, a combination of hard carbon, soft carbon and silicon oxide material, a combination of artificial graphite, natural graphite, silicon oxide material and silicon carbon material, or a combination of artificial graphite, natural graphite, hard carbon, soft carbon, silicon oxide material and silicon carbon material.
[0035] Preferably, the negative electrode current collector comprises copper foil.
[0036] Preferably, ≥30 wt% of the negative electrode active material is in secondary particle morphology, for example, 30 wt%, 32 wt%, 35 wt%, 40 wt% or 45 wt%, but not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] The secondary particles are particles formed after agglomeration. Such particles have good isotropy. When ≥30 wt% of the negative electrode active material is in the form of secondary particles, the reaction path of lithium ions can be effectively shortened, thereby improving the overall performance of lithium-ion batteries.
[0038] Preferably, the method for preparing the lithium-ion battery fast-charging negative electrode sheet comprises the following steps:
[0039] (1) dry-mixing the negative electrode active material, the conductive agent, and the dispersant, and then adding a binder and a solvent to obtain a negative electrode slurry;
[0040] (2) The negative electrode slurry obtained in step (1) is evenly coated on the front and back surfaces of the negative electrode current collector and then dried, and then rolled, slit and cut into pieces to obtain the lithium ion battery fast charging negative electrode sheet.
[0041] In a second aspect, the present application provides an electrochemical device, which includes the lithium-ion battery fast-charging negative electrode sheet described in the first aspect.
[0042] In a third aspect, the present application provides an electronic device, which includes the electrochemical device described in the second aspect.
[0043] Compared with the prior art, this application has the following beneficial effects:
[0044] The lithium-ion battery fast-charging negative electrode sheet provided in the present application, by regulating the preparation process parameters of the negative electrode membrane and the design parameters of the negative electrode active material, makes the negative electrode membrane meet the relationship under the requirements of a specific value range. The obtained lithium-ion battery has excellent fast charging capability, energy density and high high-rate cycle life, the rate can reach 4.5C, the energy density is high, and the cycle performance is as high as 4524 cycles. DETAILED DESCRIPTION
[0045] To make the above-mentioned objects, features, and advantages of the present application more clearly understood, the specific embodiments of the present application are described in detail below with reference to the accompanying drawings. The following description sets forth many specific details to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the scope of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0046] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0047] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of such features. Throughout the description of this application, "plurality" means at least two, for example, two, three, etc., unless otherwise specifically defined.
[0048] In this application, unless otherwise specified or limited, the terms "installed," "connected," "connect," "fixed," etc. should be understood in a broad sense. For example, they can refer to fixed connection, detachable connection, or integration; mechanical connection or electrical connection; direct connection or indirect connection through an intermediate medium; internal communication between two elements or interaction between two elements, unless otherwise specified. Those skilled in the art will understand the specific meanings of the above terms in this application based on specific circumstances.
[0049] In this application, unless otherwise expressly specified or limited, when a first feature is "above" or "below" a second feature, it may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Furthermore, when a first feature is "above," "above," or "above" a second feature, it may mean that the first feature is directly above or diagonally above the second feature, or simply means that the first feature is at a higher level than the second feature. When a first feature is "below," "below," or "below" a second feature, it may mean that the first feature is directly below or diagonally below the second feature, or simply means that the first feature is at a lower level than the second feature.
[0050] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element. The terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only implementation methods.
[0051] Example 1
[0052] This embodiment provides a lithium-ion battery fast-charging negative electrode sheet, which includes a copper foil and a negative electrode film containing artificial graphite coated on the surface of the copper foil;
[0053] The specific capacity C of the artificial graphite is 351 mAh / g, and the median particle size D v50 The specific surface area B measured in pure nitrogen atmosphere is 1.4m 2 / g; 90wt% of the artificial graphite is in the form of secondary particles.
[0054] The method for preparing the lithium-ion battery fast-charging negative electrode sheet comprises the following steps:
[0055] (1) Artificial graphite, superconducting carbon black conductive agent, and sodium carboxymethyl cellulose were dry-mixed for 30 minutes, and then styrene-butadiene rubber and water were added and mixed for 6 hours to obtain a negative electrode slurry with a solid content of 48% and a viscosity of 5000 mPa·s;
[0056] The weight of the artificial graphite, superconducting carbon black conductive agent, and sodium carboxymethyl cellulose are 96 wt%, 1 wt%, and 1.5 wt% of the total solid amount of the negative electrode slurry, respectively;
[0057] (2) The negative electrode slurry obtained in step (1) was evenly coated on the front and back surfaces of the negative electrode current collector with a thickness of 6 mm until the surface density S of the negative electrode film reached 8 mg / cm 2 , then passed through a 20m long 110℃ oven at a speed of 1m / s, and then rolled to a compaction density P of 1.65g / cm 3 , cutting and cutting to obtain the lithium ion battery fast charging negative electrode sheet.
[0058] Example 2
[0059] This embodiment provides a lithium-ion battery fast-charging negative electrode sheet, which includes a copper foil and a negative electrode film containing artificial graphite coated on the surface of the copper foil;
[0060] The specific capacity C of the artificial graphite is 359 mAh / g, and the median particle size Dv50 The specific surface area B measured in pure nitrogen atmosphere is 2.5m 2 / g; 35wt% of the artificial graphite is in the form of secondary particles.
[0061] The method for preparing the lithium-ion battery fast-charging negative electrode sheet comprises the following steps:
[0062] (1) Artificial graphite, superconducting carbon black conductive agent, and sodium carboxymethyl cellulose were dry-mixed for 25 minutes, and then styrene-butadiene rubber and water were added and mixed for 6.2 hours to obtain a negative electrode slurry with a solid content of 47% and a viscosity of 5200 mPa·s;
[0063] The weight of the artificial graphite, superconducting carbon black conductive agent, and sodium carboxymethyl cellulose are 96 wt%, 1 wt%, and 1.5 wt% of the total solid amount of the negative electrode slurry, respectively;
[0064] (2) The negative electrode slurry obtained in step (1) was evenly coated on the front and back surfaces of the negative electrode current collector with a thickness of 5.8 mm until the surface density S of the negative electrode film reached 15 mg / cm 2 , then passed through a 20m long 108℃ oven at a speed of 1.4m / s, and then rolled to a compaction density P of 1.8g / cm 3 , cutting and cutting to obtain the lithium ion battery fast charging negative electrode sheet.
[0065] Example 3
[0066] This embodiment provides a lithium-ion battery fast-charging negative electrode sheet, which includes a copper foil and a negative electrode film containing artificial graphite coated on the surface of the copper foil;
[0067] The specific capacity C of the artificial graphite is 330 mAh / g, and the median particle size D v50 The specific surface area B measured in pure nitrogen atmosphere is 0.7m 2 / g; 30wt% of the artificial graphite is in the form of secondary particles.
[0068] The method for preparing the lithium-ion battery fast-charging negative electrode sheet comprises the following steps:
[0069] (1) Artificial graphite, superconducting carbon black conductive agent, and sodium carboxymethyl cellulose were dry-mixed for 35 minutes, and then styrene-butadiene rubber and water were added and mixed for 5.8 hours to obtain a negative electrode slurry with a solid content of 49% and a viscosity of 4800 mPa·s;
[0070] The weight of the artificial graphite, superconducting carbon black conductive agent, and sodium carboxymethyl cellulose are 96 wt%, 1 wt%, and 1.5 wt% of the total solid amount of the negative electrode slurry, respectively;
[0071] (2) The negative electrode slurry obtained in step (1) was evenly coated on the front and back surfaces of the negative electrode current collector with a thickness of 6.2 mm until the surface density S of the negative electrode film reached 5 mg / cm 2 , then passed through a 21m long 112℃ oven at a speed of 3.1m / s, and then rolled to a compaction density P of 1.4g / cm 3 , cutting and cutting to obtain the lithium ion battery fast charging negative electrode sheet.
[0072] Example 4
[0073] This embodiment provides a fast-charging negative electrode sheet for a lithium-ion battery. The difference from Example 1 is that 60 wt% of the artificial graphite has a secondary particle morphology, and the rest is the same as Example 1.
[0074] Comparative Example 1
[0075] This comparative example provides a lithium ion battery fast charging negative electrode sheet, which is different from Example 1 in that the specific capacity C of the artificial graphite is adjusted to 332 mAh / g and the median particle size D is 0. v50 The specific surface area B measured under pure nitrogen atmosphere was adjusted to 9 μm and 1.2 m 2 / g, and the surface density S of the negative electrode film coated in step (2) is adjusted to 21 mg / cm 2 , the rest are the same as in Example 1.
[0076] Comparative Example 2
[0077] This comparative example provides a lithium ion battery fast charging negative electrode sheet, which is different from Example 1 in that the specific capacity C of the artificial graphite is adjusted to 358 mAh / g and the median particle size D is 0. v50 The specific surface area B measured under pure nitrogen atmosphere was adjusted to 2.4 m 2 / g, and the surface density S of the negative electrode film coated in step (2) is adjusted to 5 mg / cm 2 , roll-press until the compaction density P of the negative electrode membrane is adjusted to 1.4g / cm 3 , the rest are the same as in Example 1.
[0078] Performance evaluation: The lithium-ion battery fast-charging negative electrode sheets and positive electrode sheets provided in Examples 1-4 and Comparative Examples 1 and 2 were assembled, injected, and formed into lithium-ion batteries, and the obtained lithium-ion batteries were subjected to dynamic performance tests and cycle performance tests.
[0079] Dynamic performance test: At 25°C, the lithium-ion battery was fully charged at 0.5xC (3≤x≤12) and fully discharged at 1C 20 times. The lithium-ion battery was then fully charged at 0.5xC (3≤x≤12). The negative electrode was then disassembled and the lithium deposition on the negative electrode surface was observed. Where x is an integer, and x is tested from large to small. The charge rate when the area of lithium deposition on the negative electrode surface is less than 5% is the fast charge capability. The results are shown in Table 1.
[0080] Cycling performance test: At 25℃, fully charge the lithium-ion battery at 2C, discharge it at 1C to the cut-off voltage, record the discharge capacity as C1, leave it for 30 minutes, then charge and discharge it at 2C / 1C, record the discharge capacity C2, and repeat this cycle until C n / C1 is less than 0.8, and the number of cycles n is recorded. The results are shown in Table 1;
[0081] Energy density test: At 25°C, the lithium-ion battery was fully charged at 1C and fully discharged at 1C, and the actual discharge energy at this time was recorded; at 25°C, the lithium-ion battery was weighed using an electronic balance; the ratio of the actual discharge energy of the lithium-ion battery at 1C to the weight of the lithium-ion battery was the actual energy density of the lithium-ion battery; when the actual energy density was less than 90% of the expected energy density, the battery was considered to have a low actual energy density; when the actual energy density was greater than or equal to 90% of the expected energy density and less than 100% of the expected energy density, the battery was considered to have a medium actual energy density; when the actual energy density was greater than 100% of the expected energy density, the battery was considered to have a high actual energy density. The results are shown in Table 1.
[0082] Table 1
[0083] From Table 1 we can see that:
[0084] Comparison of Example 1 with Examples 2 and 3 shows that the surface density and compaction density of the negative electrode membrane and the design parameters of the negative electrode active material are within the specified range, and the negative electrode membrane also satisfies the relationship under the requirements of the specific value range. The prepared lithium-ion battery has good fast charging capability and excellent cycle performance.
[0085] From the comparison between Example 1 and Example 4, it can be seen that, under the condition that other conditions remain unchanged, increasing the proportion of secondary particles can improve the fast charging capability, because the secondary particles can increase the lithium ion embedding angle and shorten the lithium ion embedding path;
[0086] From the comparison between Example 1 and Comparative Example 1, it can be seen that W is less than 1, and the energy density is medium, but the compaction density of the negative electrode membrane reaches the limit, which reduces the pores in the negative electrode membrane, which is not conducive to the liquid phase conduction of lithium ions. At the same time, the surface density of the negative electrode membrane is too high, which increases the transmission path of lithium ions and makes it difficult to fully utilize the capacity of the negative electrode active material; from the comparison between Example 1 and Comparative Example 2, it can be seen that W is greater than 9, and the larger specific surface area of artificial graphite leads to more side reactions, which has an adverse effect on the cycle life. The smaller surface density of the negative electrode membrane leads to a decrease in energy density.
[0087] In summary, the lithium-ion battery fast-charging negative electrode sheet provided in this application, by regulating the preparation process parameters of the negative electrode membrane and the design parameters of the negative electrode active material, makes the negative electrode membrane meet the relationship under the requirements of a specific value range, and further controls the proportion of secondary particles. The lithium-ion battery obtained has excellent fast charging capability, energy density and high high-rate cycle life, the rate can reach 4.5C, the energy density is high, and the cycle performance is as high as 4524 cycles.
[0088] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0089] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and these modifications and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.
Claims
1. A fast-charging negative electrode sheet for lithium-ion batteries, It is characterized in that The lithium-ion battery fast-charging negative electrode sheet comprises a negative electrode current collector and a negative electrode film containing a negative electrode active material coated on the surface of the negative electrode current collector; The negative electrode film satisfies 1≤W≤9, W=0.01×(B+D v50 )×C / (P×S); Wherein, B is the specific surface area of the negative electrode active material measured in a pure nitrogen atmosphere, in m 2 / g; D v50 is the median particle size of the negative electrode active material, in μm; C is the specific capacity of the negative electrode active material, in mAh / g; P is the compaction density of the negative electrode membrane, in g / cm 3 ; S is the surface density of the negative electrode membrane, in mg / cm 2 .
2. The lithium-ion battery fast-charging negative electrode sheet according to claim 1, It is characterized in that The range of B is 0.7≤B≤2.
5.
3. The lithium-ion battery fast-charging negative electrode sheet according to claim 2, It is characterized in that The B is 0.7, 1, 1.5, 2 or 2.
5.
4. The lithium-ion battery fast-charging negative electrode sheet according to any one of claims 1 to 3, It is characterized in that The D v50 The range is 7≤D v50 ≤18.
5. The lithium-ion battery fast-charging negative electrode sheet according to claim 4, It is characterized in that The D v50 7, 10, 12, 15 or 18.
6. The lithium-ion battery fast-charging negative electrode sheet according to any one of claims 1 to 5, It is characterized in that The range of C is 330≤C≤370.
7. The lithium-ion battery fast-charging negative electrode sheet according to claim 6, It is characterized in that The C is 330, 340, 350, 360 or 370.
8. The lithium-ion battery fast-charging negative electrode sheet according to any one of claims 1 to 7, It is characterized in that The range of P is 1.3≤P≤1.
8.
9. The lithium-ion battery fast-charging negative electrode sheet according to claim 8, It is characterized in that The P is 1.3, 1.4, 1.5, 1.6 or 1.
8.
10. The lithium-ion battery fast-charging negative electrode sheet according to any one of claims 1 to 9, It is characterized in that The range of S is 5≤S≤15.
11. The lithium-ion battery fast-charging negative electrode sheet according to claim 10, It is characterized in that The S is 5, 8, 10, 12 or 15.
12. The lithium-ion battery fast-charging negative electrode sheet according to any one of claims 1 to 11, It is characterized in that The negative electrode active material includes any one of artificial graphite, natural graphite, hard carbon, soft carbon, silicon-oxygen material and silicon-carbon material, or a combination of at least two thereof.
13. The lithium-ion battery fast-charging negative electrode sheet according to claim 12, It is characterized in that ≥30wt% of the negative electrode active material is in the form of secondary particles.
14. The fast-charging negative electrode sheet for a lithium-ion battery according to claim 13, wherein 30wt%, 32wt%, 35wt%, 40wt% or 45wt% of the negative electrode active material is in the form of secondary particles.
15. The lithium-ion battery fast-charging negative electrode sheet according to any one of claims 1 to 14, It is characterized in that The negative electrode current collector includes copper foil.
16. An electrochemical device, It is characterized in that The electrochemical device comprises the lithium-ion battery fast-charging negative electrode sheet according to any one of claims 1 to 15.
17. An electronic device, It is characterized in that The electronic device comprises the electrochemical device according to claim 16.
Citation Information
Patent Citations
Composite anode material for lithium ion battery, and preparation method and application of composite anode material
CN105261734A
Preparation method of lithium ion battery
CN108832183A
Anode and secondary battery comprising said anode
CN113614950A
Negative plate and lithium ion battery comprising same
CN114122329A
Negative active material, negative plate containing negative active material and lithium ion battery
CN114156446A
Cited By
Lithium battery negative pole piece, preparation method and application thereof, and lithium ion secondary battery
CN119864364A
Battery control method, controller, battery pack and electric equipment