Aqueous cathode slurry composition for cell cathode
The novel cathode slurry composition with a binder system of binder polymer, acidic polysaccharide, and lithiated polymer addresses the stability issues of high-nickel lithium-ion batteries by forming a stable CEI layer, enhancing cycle life and rate capacity, and enabling high voltage operation.
Patent Information
- Application Number
- PCT/EP2024/060388
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-24
AI Technical Summary
High-nickel cathode materials in lithium-ion batteries are prone to adverse phase transitions and nickel leaching, leading to battery instability and capacity fading, especially under high voltage conditions, due to limited knowledge on the cathode-electrolyte interphase (CEI) stability.
A novel cathode slurry composition incorporating a binder system comprising a binder polymer, an acidic polysaccharide, and a lithiated polymer, which forms a stable CEI layer, enhancing electrochemical and mechanical stability, and includes a lithiated polymer to act as a lithium ion reservoir and pH buffer, reducing adverse reactions and maintaining electrochemical performance.
The composition results in improved cycle life, rate capacity, and flexibility of lithium-ion batteries, allowing operation under high voltage conditions while maintaining electrochemical and mechanical stability, with enhanced adhesion to the conductive foil and reduced gas generation.
Smart Images

Figure EP2024060388_24102024_PF_FP_ABST
Abstract
Description
[0001] Aqueous cathode slurry composition for cell cathode
[0002] Field
[0003] The present disclosure relates to a cathode slurry composition, and its preparation, for use in a cathode, a cathode comprising the composition, a cell including the cathode and a battery pack including the cell.
[0004] Background
[0005] There has been significant interest in the use of rechargeable batteries for use in energy storage applications. In particular, lithium-ion batteries have been widely applied in diverse industries, such as electronic devices, power tools, satellites, utilityscale storage and electric vehicles.
[0006] Electrode-electrolyte interfaces are critical components in lithium-ion batteries that determine their cycle life, capacity retention and safety. While the solid-electrolyte interphase (SEI) at the anode has been well studied, knowledge on the nature of the cathode-electrolyte interphase (CEI) is limited, despite CEI formation and stability critically affecting battery performance.
[0007] Processes occurring at the CEI layer such as consumption of lithium ions, oxidative decomposition reactions, formation of side-reaction redox products and loss of transition metal cations from the cathode, can lead to battery instability and capacity fading. Therefore, there is significant interest in developing new electrode compositions and methods for producing stable and robust CEI layers in lithium-ion batteries. This would result in improved battery stability, cycle life and capacity retention.
[0008] High voltage lithium-ion batteries may offer advantages such as high energy density and capacity, longer lifespan, rapid charging capability and wide compatibility with devices. High-nickel cathode materials are also commercially attractive due to the improved performance in relation to cost. However, high-nickel cathode materials are prone to adverse phase transitions, nickel leaching and deterioration in battery performance when run at high voltage. In addition, cycling under high voltage conditions may result in oxidation and / or decomposition of binder materials. Therefore, there is a need for electrodes and lithium-ion batteries with prolonged cycle stability, such as electrochemical and mechanical stability, which may be manufactured using an environmentally friendly process. This disclosure relates to a novel electrode slurry composition, a method of preparation of such slurry composition, and electrodes, cells and battery packs formed from this slurry composition. The authors have discovered that this slurry composition leads to lithium-ion batteries with unexpectedly improved electrochemical performance and stability.
[0009] Brief Description
[0010] According to an aspect of the present disclosure, there is provided a slurry composition comprising: a cathode active material; a binder system; a dispersing medium; and optionally a conductive agent, wherein the binder system comprises: a binder polymer, an acidic polysaccharide, and a lithiated polymer.
[0011] According to a further aspect of the present disclosure, there is provided a method for forming a slurry composition comprising the steps of: a. providing a composition comprising a cathode active material, an acidic polysaccharide, a lithiated polymer, a binder polymer, optionally a conductive agent, and optionally a dispersing medium; and b. adding dispersing medium to the composition and mixing to provide a slurry composition having a solids content of from 60 wt% to 80 wt%; provided that when the binder polymer comprises acrylic polymer, the method comprises adding said acrylic polymer, optionally together with dispersing medium, to an intermediate slurry composition having solids content of from 65 wt% to 85 wt%, and mixing to provide a slurry composition having a solids content of from 60 wt% to 80 wt%.
[0012] According to a further aspect of the present disclosure, there is provided an electrode comprising: a cathode active material; a binder system; and optionally a conductive agent, wherein the binder system comprises: a binder polymer, an acidic polysaccharide, and a lithiated polymer.
[0013] According to a further aspect of the present disclosure, there is provided a binder system for an electrode comprising : a binder polymer, an acidic polysaccharide, and a lithiated polymer.
[0014] Brief description of the figures
[0015] Figure 1 shows the voltage and capacity for the half-cells of Example 1 and a sample without lithium polyacrylate during its formation cycle.
[0016] Figure 2 shows the capacity retention of half-cells of Example 1 and a sample without lithium polyacrylate after 50 cycles.
[0017] Figure 3 shows the voltage and capacity for the half-cells of Example 2 and a sample without lithium polyacrylate during its formation cycle.
[0018] Figure 4 shows the capacity retention of half-cells of Example 2 and a sample without lithium polyacrylate after 50 cycles.
[0019] The present disclosure will in the following be described in more detail.
[0020] Detailed Description
[0021] Unless otherwise indicated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains.
[0022] Binder system
[0023] The present disclosure relates to slurries used to form cathodes having a particular binder system, as well as electrodes formed from the same. The binder system of the present disclosure, when included in a cell, may form a stable CEI layer during cycling of the cell, resulting in a more stable cell that retains high coulombic efficiency. In addition, the binder system is compatible with an aqueous dispersing media, which provides a number of processing advantages such as reduced environmental impact and cost. Furthermore, the electrode formed using the binder system has excellent properties such as flexibility, life cycle performance and rate capacity, and should be capable of being operated under high voltage conditions while maintaining electrochemical and / or mechanical stability.
[0024] The binder system of the disclosure comprises a binder polymer, an acidic polysaccharide and a lithiated polymer. These components combine to provide a binder system that forms a CEI between the cathode and the electrolyte in the cell.
[0025] In some embodiments, the binder system comprises about 0.1 to 30 wt% of a binder polymer, about 55 to 97 wt% of an acidic polysaccharide and about 0.1 to 30 wt% of a lithiated polymer, based on the weight of the non-volatile content of the binder system.
[0026] In some embodiments, when the binder polymer is an acrylic polymer, the binder system comprises about 1 to 30 wt% of an acrylic polymer, about 55 to 95 wt% of an acidic polysaccharide and about 0.1 to 30 wt% of a lithiated polymer, based on the weight of the non-volatile content of the binder system.
[0027] In another embodiment, when the binder polymer is an acrylic polymer, the binder system comprises about 5 to 25 wt% of an acrylic polymer, about 65 to 90 wt% of an acidic polysaccharide and about 0.5 to 20 wt% of a lithiated polymer, based on the weight of the non-volatile content of the binder system.
[0028] In a preferred embodiment, when the binder polymer is an acrylic polymer, the binder system comprises about 10 to 20 wt% of an acrylic polymer, about 75 to 85 wt% of an acidic polysaccharide and about 1 to 10 wt% of a lithiated polymer, based on the weight of the non-volatile content of the binder system.
[0029] In some embodiments, when the binder polymer is an acrylamide copolymer, the binder system comprises about 0.1 to 30 wt% of an acrylamide copolymer, about 65 to 97 wt% of an acidic polysaccharide and about 0.1 to 30 wt% of a lithiated polymer, based on the weight of the non-volatile content of the binder system.
[0030] In another embodiment, when the binder polymer is an acrylamide copolymer, the binder system comprises about 0.5 to 20 wt% of an acrylamide copolymer, about 75 to 96 wt% of an acidic polysaccharide and about 0.5 to 20 wt% of a lithiated polymer, based on the weight of the non-volatile content of the binder system. In a preferred embodiment, when the binder polymer is an acrylamide copolymer, the binder system comprises about 1 to 10 wt% of an acrylamide copolymer, about 85 to 95 wt% of an acidic polysaccharide and about 1 to 10 wt% of a lithiated polymer, based on the weight of the non-volatile content of the binder system.
[0031] Without wishing to be bound by theory, it is proposed that the lithiated polymer component may improve the electrochemical performance and stability of the cell. The lithiated polymer may act as an additional reservoir of lithium ions. When a cell is fabricated using an electrode prepared with the binder system, the lithiated polymer may supply extra lithium ions to the electrode. Upon initial charge and discharge cycling of the cell, the lithiated polymer facilitates the formation of a stable and protective CEI layer on the cathode. Specifically, the lithiated polymer and the CEI layer may limit contact between the cathode active material and the electrolyte solution. The formation of a CEI layer prevents oxidative decomposition reactions occurring and degradation of the cathode and electrolyte species. It is proposed that the protective CEI layer mitigates reactions between the cathode active material and solution species from the electrolyte. Furthermore, the inclusion of a lithiated polymer may provide extra lithium ions that can compensate for the loss of active lithium ions from the cathode active material during cell cycling, such that the lithium ions in the lithiated polymer are consumed during formation of the CEI in preference to the lithium contained in the cathode active material. In addition, the lithiated polymer may have a high ionic conductivity, which facilitates transport of lithium ions during operation of the cell to and from the coated cathode active material. As a result, the impedance of the electrode remains low, and the rate capacity of the cell is retained.
[0032] Without wishing to be bound by theory, the acidic polysaccharide component is believed to interact with any lithium ions that may leach from the cathode active material when it is exposed to a dispersing medium such as water. It is proposed that the acidic groups of the acidic polysaccharide component in the binder system may react with the lithium ions of the cathode active material, which can result in a coating of the acidic polysaccharide on the surface of the cathode active material. This coating may then protect the cathode active material against any further degradation. The acidic polysaccharide provides the additional benefit that it can act both as a binder as well as increase the viscosity of the slurry.
[0033] Without wishing to be bound by theory, if the cathode active material, for example a lithium NMC (nickel manganese cobalt) material, is added to the dispersing medium, such as water, during cathode slurry preparation, the lithium can leach out of the cathode active material and react with water, which results in the formation of hydroxide ions and an increase in the pH of the slurry. This subsequently results in the formation of LiOH and IJ2CO3, which leads to a reduction in the capacity of the cell. Furthermore, the high pH may result in corrosion of the conductive foil. Therefore, the addition of acid to the slurry composition reduces the pH and mitigates the reaction of lithium with water and formation of unwanted by-products. The acid is able to form a complex with lithium upon addition to the cathode active material during preparation of the cathode slurry composition, thereby inhibiting unwanted side reactions of lithium.
[0034] Lithiated polymers provide additional benefits to the binder system during preparation of the slurry composition. Lithiated polymers may be basic and therefore may also act as a buffer when preparing the slurry composition. The acidic polysaccharide and lithiated polymer may react together to maintain the correct pH of the slurry composition. As a result, the pH of the slurry composition is maintained at a suitable level.
[0035] If a lithiated polymer is used in the preparation of the slurry composition without the addition of any acidic polysaccharide, lithium ions can react with water and form unwanted by-products. Therefore, the acidic polysaccharide is able to balance the pH of the aqueous cathode slurry, form a complex with the lithium ions and mitigate degradation of the cathode active material.
[0036] If the slurry composition does not comprise a lithiated polymer in the binder system, then the pH of the slurry composition may be too acidic. This subsequently leads to dissolution of transition metal ions from the cathode active material, and as a result leads to an inferior cathode and respective cell when said slurry composition is used in the cathode and cell. In particular, the cell capacity is lower for a cell comprising a cathode that is prepared using a slurry composition which is too acidic. Therefore, a lithiated polymer is required in the binder system and the slurry composition in order to act as a buffer (neutralising agent) and increase the pH of the slurry composition. A slurry composition comprising a lithiated polymer will result in the slurry composition being less acidic, and therefore can result in a cathode and subsequent cell comprising said cathode that displays a higher charge and discharge capacity.
[0037] Furthermore, the lithiated polymer may also function as a rheological modifier in the slurry composition. This can be useful for enhancing the viscosity of the slurry. This may subsequently be desirable for maintaining the preferred properties of the slurry composition, such as good dispersion properties, stability and coating ability.
[0038] The binder system additionally comprises a binder polymer which acts as a binder in the dried composition, providing flexibility and strength to the electrode formed from the slurry. The binder polymer additionally improves adhesion of the electrode to the foil. The resultant electrodes have excellent cycle life, rate capacity, as well as flexibility, allowing them to be rolled for incorporation into a cell, such as a cylindrical cell, prismatic cell, pouch cell, or coin cell.
[0039] The binder polymer in the binder provides flexibility to the final cathode, which enables rolling of the cathode during manufacture of the cell as well as better handling of cathodes during cell production / manufacture. The flexible properties are advantageous when preparing a cylindrical cell. Binders such as PVDF have typically been used in cathode slurries for lithium-ion batteries, since such compounds provide good flexibility. However, these binders contain fluorine, which may be harmful to the environment and to human health.
[0040] If the binder polymer is not added to the binder system, and the binder system contains only the lithiated polymer and the acidic polysaccharide, then this may result in a cathode which lacks flexibility. This can subsequently result in degradation of the cathode during cell operation, and poor life cycle stability.
[0041] The binder polymer also provides adhesive properties to the cathode, resulting in good adhesion of the cathode slurry composition to the conductive foil and improved peel strength. For example, a cathode comprising a binder polymer in the binder system may have a larger adhesion strength, such as peel strength, compared to a cathode that does not comprise a binder polymer. This leads to improved cycle life of the cell compared to a cathode that does not contain the acrylic component. Large volume changes of the cathode during charging and discharging under cell operation may lead to cathode delamination if there is poor adhesion between the cathode slurry composition and the conductive foil. The use of an acrylic component in the binder system prevents delamination of the cathode from the conductive foil, thereby improving cell cycle life.
[0042] For instance, the adhesion strength of an electrode to the conductive foil may be measured using a peel test. The peel strength of a cathode comprising a binder system comprising a binder polymer may be from about 10 to 120 N / m, for instance from about 30 to 100 N / m, whereas a cathode comprising a binder system without binder polymer may be from about 3 to 10 N / m. As such, the inclusion of binder polymer in the binder system results in a cathode displaying excellent adhesion strength to the conductive foil.
[0043] In some embodiments, the peel strength of a cathode comprising a binder system comprising a binder polymer may be from about 10 to 18 N / m, for instance from about 12 to 15 N / m.
[0044] The peel strength may be measured in accordance with ASTM D3330. The peel strength test may be carried out on a Universal Testing Machine (e.g. Instron 3345), for example, using an electrode sample having a width of 25 mm. Each of the electrode plates in which the coating layers were located on both surfaces of the current collectors may be cut to a size of 25 mmxl50 mm. After an adhesive was coated on a glass substrate at room temperature, the electrode plate was adhered to the adhesive and roll-pressed. After one end of the electrode plate was folded 180°, a force applied to the sample was measured while pulling the sample in a direction opposite to the one end at a speed of 100 mm / min. The peel strength may be an average of 20 samples.
[0045] The binder polymer is optimal for use in the cathode of a lithium-ion cell, since it has excellent electrochemical stability during cell operation and under the conditions to which the cathode is subjected during charge and discharge cycling. Other common binder materials, such as styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), hydrogenated butadiene rubber (HBR), and other rubbers, may be suitable for use in the anode, but are incompatible for use in the cathode due to the likelihood of electrochemical oxidation if used in the cathode. For example, such binders may have poor stability when used in the electrode of a cell operating at high voltage. If a cell is run at or above 4.2 V, there may be decomposition of the binder and / or delamination of the electrode.
[0046] The binder polymer of the disclosure may provide a cathode with excellent electrochemical and / or mechanical stability, in particular when the cathode is used in a cell operated under high voltage conditions. The binder system is particularly suitable for use in high voltage cells since the cathode may retains its adhesion strength while in use. A cell comprising a binder polymer, in particular wherein the cell comprises a high-nickel cathode active material, may be run under high voltage conditions without decomposition of the cell, cathode and / or binder system, while still retaining its electrochemical and / or mechanical performance, such as capacity and / or adhesion strength.
[0047] On the other hand, high-nickel cathode materials are considered to be promising cathode candidates due to advantages of high capacity, low cost and / or good cycle performance. In particular, high-nickel cathode materials allow for a reduced amount of cobalt (or even cobalt-free) in the cathode active material, and therefore a reduced cost. High-nickel cathode active materials may show improved capacity compared to those having a lower Ni-content. Therefore, a binder system allowing for the use of high-nickel cathode materials, for example that may be run at high voltage, while maintaining electrochemical and / or mechanical stability and / or performance, is of particular interest.
[0048] However, a high Ni content in NMC cathodes may compromise their chemical and structural stability, causing the battery to deteriorate faster than their lower Ni content counterparts. In particular, high Ni-NMC cathodes tend to evolve considerably more gas during storing than their lower Ni content counterparts. The binder system of the disclosure therefore may reduce gas generation for cathode active materials under storage.
[0049] Without wishing to be bound by theory, it is thought that if the lithiated polymer is not used in the binder, and only binder polymer and acidic polysaccharide are used, then the pH of the aqueous cathode slurry composition during the method of its preparation can be too low. This may result in the precipitation of the binder polymer, which leads to an inhomogeneous slurry that is difficult to coat onto the conductive foil, and thus a cathode with inferior properties.
[0050] The binder polymer is less stable under acidic conditions and will typically precipitate if the pH is too low. This will lead to a poorly mixed slurry composition. Therefore, a lithiated polymer is required in the slurry composition in order to act as a buffer or neutralising agent and increase the pH of the slurry and prevent precipitation of the binder polymer.
[0051] In some embodiments, the binder system is present in an amount of from about 0.1 to 8 wt%, for example about 0.2 to 7 wt%, for example about 0.5 to 5 wt%, such as about 2 to 5 wt%, for example about 1 to 4 wt%, for example about 1.6 to 3 wt%, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode). In some embodiments, when the binder system comprises an acrylic polymer, the binder system is present in an amount of from about 0.2 to 8 wt%, for example about 0.5 to 6 wt%, for example about 1 to 5 wt%, such as about 2 to 5 wt%, for example about 1.5 to 4 wt%, for example about 2 to 3 wt%, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0052] In some embodiments, when the binder system comprises an acrylamide copolymer, the binder system is present in an amount of from about 0.1 to 8 wt%, for example about 0.2 to 7 wt%, for example about 0.5 to 5 wt%, such as about 2 to 5 wt%, for example about 1 to 4 wt%, for example about 1.6 to 2.6 wt%, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0053] Each of these components will be described in turn.
[0054] Acidic polysaccharide
[0055] An "acidic polysaccharide" is a polysaccharide having acidic functional groups including carboxyl groups, phosphate groups, sulphuric ester groups, or mixtures thereof.
[0056] Preferably, the acidic polysaccharide has a pKa of from 1 to 10, more preferably from 1.5 to 6.
[0057] The acidic polysaccharide is a polymer that may comprise saccharide units bound together by glycosidic linkages. The acidic polysaccharide may comprise one or more repeating saccharide units, such as monosaccharide units, disaccharide units, trisaccharide units, or mixtures thereof. Preferably, the acidic polysaccharide comprises one or more monosaccharide units.
[0058] In some embodiments, the acidic polysaccharide is a linear polysaccharide, a branched polysaccharide, or a mixture thereof.
[0059] The acidic polysaccharide may comprise five-carbon monosaccharide units, six-carbon monosaccharide units, or mixtures thereof.
[0060] In some embodiments, the acidic polysaccharide comprises a copolymer containing more than one type of saccharide unit. For example, the acidic polysaccharide may comprise two or more different monosaccharide units, such as homopolymeric blocks of two or more different monosaccharide units. Preferably, the acidic polysaccharide is a copolymer. More preferably, the acidic polysaccharide is a block copolymer.
[0061] When the acidic polysaccharide is a saccharide having sulphuric ester groups, the acidic polysaccharide may comprise monosaccharide or disaccharide units that contain one or more sulphuric ester groups per monosaccharide or disaccharide unit. For example, the acidic polysaccharide may comprise sulphate esters of galactopyranose, sulphate esters of anhydrogalactopyranose, or mixtures thereof. In one embodiment, the acidic polysaccharide comprises carrageenan.
[0062] Preferably, the acidic polysaccharide is a polysaccharide comprising carboxyl groups. In some embodiments, the acidic polysaccharide comprises monosaccharide units that contain one or more carboxyl groups per monosaccharide unit.
[0063] The acidic polysaccharide may comprise sugar acid units, for example monosaccharide units having carboxyl groups that are linked by glycosidic bonds, such as an aldonic acid, a uronic acid, an ulosonic acid, an aldaric acid, or a mixture thereof. Preferably, the sugar acid units are selected from mannuronic acid, guluronic acid, gluconic acid, galacturonic acid, glucuronic acid, or mixtures thereof.
[0064] In one embodiment, the acidic polysaccharide is a derivative of cellulose comprising carboxyl groups.
[0065] In another embodiment, the acidic polysaccharide is a biopolymer. For example, the acidic polysaccharide may be extracted from a biological source. Alternatively, the acidic polysaccharide may be a biosynthetic polymer, i.e. a synthetic polymer that mimics a biopolymer found in nature. The acidic polysaccharide may be a synthetically modified biopolymer. In a further embodiment, the acidic polysaccharide may be a biopolymer derived from algae and / or seaweed.
[0066] Preferably, the acidic polysaccharide is selected from one or more of alginic acid, carboxymethyl cellulose, xanthan gum, guar gum, gum arabic, dextrin, hyaluronic acid, pectin, agar, glycogen, hydroxypropyl starch phosphate, hydroxyethyl cellulose, tragacanth, or mixtures thereof.
[0067] More preferably, the acidic polysaccharide is selected from one or more of alginic acid, carboxymethyl cellulose, xanthan gum, or mixtures thereof. Most preferably, the acidic polysaccharide is alginic acid.
[0068] Alginic acid has several properties that make it desirable for use in the binder system. This includes its compatibility with the dispersing medium, in particular water. Alginic acid may interact with any lithium ions that may leach from the cathode active material when it is exposed to a dispersing medium such as water. The carboxyl groups of alginic acid may react with the lithium ions of the cathode active material, which can result in a coating of alginic acid or its salt thereof on the surface of the cathode active material. The acidity and pKa of alginic acid is in an ideal region for tuning the pH of the slurry composition and mitigating the reaction of lithium (from the cathode active material) with water and formation of unwanted by-products. It also may act as a rheological modifier or thickening agent and enhance the viscosity of the slurry, which facilitates processing of the slurry composition.
[0069] The acidic polysaccharide, for example alginic acid, may be particularly suitable for stabilising the cathode active material, in particular high-nickel cathode materials, and prevent nickel and / or manganese leaching. Without wishing to be bound by theory, it is thought that the acidic polysaccharide (e.g. alginic acid) may bind with the nickel and / or manganese ions to form a gel, for example by producing a coating layer around the cathode active material, thereby reducing leaching of transition metals from the cathode active material. The driver for gel formation is replacement of the proton with the divalent cation leached from the cathode active material. The binder system of the disclosure therefore provides the protective coating on the CAM where and when it is needed.
[0070] In particular, if the cathode does not comprise an acidic polysaccharide (i.e. alginic acid) in the binder system, this may result in uncontrolled leaching of transition metal (e.g. Ni and / or Mn) from the cathode active material, which may lead to an inferior cathode and respective cell while in use.
[0071] Furthermore, alginic acid is an acidic polysaccharide derived from seaweed or algae. This provides a significant advantage, since it is biocompatible, abundant and relatively inexpensive.
[0072] When the acidic polysaccharide acid is alginic acid, it may have a number average molecular weight (Mn) of from about 10,000 to about 500,000 g / mol, for example from about 100,000 to about 300,000 g / mol, preferably from about 190,000 g / mol to about 250,000 g / mol.
[0073] The skilled person will understand that the molecular weight of the acidic polysaccharide will affect the viscosity of a solution or a slurry containing the acidic polysaccharide. An acidic polysaccharide with a high molecular weight will result in a solution or a slurry with a high viscosity, which can consequently affect other properties such as the dispersion stability of the slurry and the coating ability of the slurry, when coating the slurry composition onto the conductive foil. Therefore, the amount of acidic polysaccharide may be varied to tune the rheological properties of the aqueous cathode slurry. The acidic polysaccharide may therefore act as a rheological modifier as well as an acid in the slurry composition.
[0074] The acidic polysaccharide may be delivered as a solid powder.
[0075] The amount of acidic polysaccharide in the slurry composition depends on the pKa value of the acid. If the acidic polysaccharide has a high pKa value, for example if the acid is weak, then more acid may be required to reduce the pH of the slurry composition. If the acidic polysaccharide has a low pKa value, for example if the acid is strong, then less acid may be needed to reduce the pH of the slurry composition.
[0076] The acidic polysaccharide may be present in an amount of from about 0.05 to about 5 wt%, for example from about 0.05 to about 4 wt %, such as from about 0.5 to about 4 wt%, for example from about 1 to about 3 wt%, preferably from about 1.5 to about 2.5 wt% based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0077] Lithiated polymer
[0078] A "lithiated polymer" is a polymer comprising lithium ions.
[0079] In one embodiment, the lithiated polymer is a lithium salt and comprises a negatively charged polymer that is electrically balanced with positive lithium counterions.
[0080] In some embodiments, the lithiated polymer comprises carboxyl functional groups on the polymer. For example, the lithiated polymer may be a lithium salt of a polymer or copolymer comprising monomer units based on ethylenically unsaturated carboxylic acid derivatives. In another embodiment, the lithiated polymer is a lithium salt of a polymer or copolymer comprising monomer units selected from one or more of the following ethylenically unsaturated C3-C6 monocarboxylic acids, ethylenically unsaturated C4- C6 dicarboxylic acids, or mixtures thereof.
[0081] Preferably, the lithiated polymer is a lithium salt of a polymer or copolymer comprising monomer units selected from one or more of the following acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, 2-ethylpropenoic acid, maleic acid, itaconic acid, fumaric acid, citraconic acid, or mixtures thereof.
[0082] In other words, the lithiated polymer is preferably selected from lithium polyacrylate, lithium polymethacrylate, lithium polycrotonate, lithium polyisocrotonate, lithium poly- 2-ethylpropenate, lithium polymaleate, lithium polyitaconate, lithium polyfumate, or lithium polycitraconate.
[0083] More preferably, the lithiated polymer is a lithium salt of polyacrylic acid, i.e. the lithiated polymer is lithium polyacrylate (LiPAA).
[0084] The lithiated polymer has a molecular weight that allows coating of the cathode active material, yet is not so high that the viscosity of the slurry composition becomes too high, in order to allow the composition to be coated onto a foil. The lithiated polymer is not limited to only coating the cathode active material, but may also coat other components in the slurry composition. For example, lithium polyacrylate may coat the optional conductive agent.
[0085] The lithiated polymer may be delivered as a dispersion, preferably as a water-based dispersion, for example as a lithium polyacrylate water-based dispersion. The lithiated polymer dispersion may comprise from about 1 to about 30 wt% lithiated polymer, for example from about 2 to about 20 wt% lithiated polymer, such as from about 3 to about 10 wt% lithiated polymer, preferably from about 4 to about 6 wt% lithiated polymer.
[0086] The lithiated polymer dispersion may have a dynamic viscosity of from about 1,000 to about 100,000 mPa-s, for instance from about 5,000 to about 50,000 mPa-s, preferably from about 10,000 to about 40,000 mPa-s, as measured at 40 °C.
[0087] The lithiated polymer dispersion, when provided as a water-based dispersion, may have a pH from about 6 to about 10, for example from about 7 to about 9. Typical average molecular weights (Mn) of the lithiated polymer are from about 10,000 to about 500,000 g / mol, for example from about 15,000 to about 300,000 g / mol, preferably from about 20,000 to about 170,000 g / mol.
[0088] The lithiated polymer is present as a lithium salt. Preferably, the lithiated polymer is a fully-lithiated polymer, so that the acidic groups (e.g. the carboxyl groups) in the lithiated polymer are preferably all in salt form, i.e. the lithiated polymer preferably does not contain any free (carboxylic) acid groups.
[0089] It has been found that lithiated polymers, in particular lithium polyacrylate, provide several desirable properties. Lithium polyacrylate may facilitate the formation of a stable CEI on the electrode during the electrode preparation process. This acts as a passivation layer at the interface, thereby assisting with the retention of the cell's electrochemical performance by preventing electrolyte solution oxidation and dissolution of transition metal cations.
[0090] Lithium polyacrylate also provides additional features when used in the binder system. Lithium polyacrylate has good solubility in water, has excellent binding properties, provides good adhesive properties, can act as a rheological modifier and may also act as a buffering agent which can balance the pH of the slurry composition. Therefore, lithium polyacrylate may act both as a viscosity modifier and a neutralising agent.
[0091] Lithium polyacrylate is preferable over other lithium salts in the slurry composition, electrode and cell due to the unique and surprising combination of these features. Lithium polyacrylate is therefore preferable for use in the binder system over other lithium salts since it has good adhesive properties, it can create a uniform ionic conducting surface coating over the cathode active material, it may enhance the viscosity of the slurry composition and it can act as a neutralising agent. It is also able to act as an extra lithium source, compensate for Li-ion loss from the cathode active material during formation of a CEI layer and improve the electrochemical performance of the cell (e.g. capacity retention, cycle life and rate capacity).
[0092] Lithium polyacrylate is also preferable to use since it has a relatively low cost.
[0093] The lithiated polymer may be present in an amount of from about 0.001 to about 3 wt%, for example from about 0.05 to about 3 wt%, such as from about 0.001 to about 2 wt%, for example from about 0.005 to about 0.5 wt%, preferably from about 0.01 to about 0.1 wt%, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0094] The lithiated polymer may be formed by reacting a suitable polymer with a suitable base such as lithium hydroxide, in a solvent such as water.
[0095] Binder polymer
[0096] The binder polymer provides flexibility to the electrode, improves adhesion of the electrode to the foil, and reduces unwanted side reactions in the slurry prior to formation of the electrode.
[0097] In some embodiments, the binder polymer is present in an amount of from about 0.01 to about 5 wt%, such as from about 0.05 to about 4 wt%, such as from about 0.05 to about 3 wt%, for example from about 0.05 to about 2 wt%, such as from about 0.05 to about 1 wt%, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0098] In one embodiment the binder polymer has a number average molecular weight (Mn) of from about 300,000 to about 2,000,000 g / mol, for example from about 400,000 to about 1,500,000 g / mol. Preferably, the number average molecular weight is between 500,000-1,000,000 g / mol, for example between 600,000-900,000 g / mol.
[0099] The binder polymer typically has a pH (when dispersed in water) of from 5 to 10, for example from 6 to 10, preferably from 7 to 9.
[0100] The binder polymer may be an acrylic polymer and / or an acrylamide copolymer.
[0101] Preferably, the binder polymer consists of an acrylic polymer, an acrylamide copolymer, or a mixture thereof.
[0102] Preferably, the binder polymer, in particular the acrylic polymer, is in the form of a non-ionic polymer and / or non-acidic polymer. For example, preferably the acrylic polymer does not comprise free acid groups, such as carboxylic acid groups. In this way, the pH of the slurry composition does not become too acidic, thereby avoiding dissolution of transition metal from the cathode active material and / or precipitation of components of the slurry. By "acrylic polymer" is meant a polyacrylate ester polymer, or in other words a polymer formed from acrylic acid alkyl ester monomers, for example an acrylate alkyl ester monomer. Preferably, the acrylic polymer is a polyacrylate polymer wherein the acrylic groups are in the form of esters. More preferably, the acrylic polymer does not comprise an acidic group, such as a free carboxylic acid group.
[0103] The acrylic polymer may be selected from one or more of the following poly( methyl methacrylate), poly(methyl acrylate), poly(ethyl acrylate), poly(butyl acrylate), poly(2-ethylhexyl acrylate), or mixtures thereof.
[0104] The acrylic polymer may be a copolymer formed from two or more of methyl methacrylate, methyl acrylate, ethyl acrylate, butyl acrylate, or 2-ethylhexyl acrylate.
[0105] In some embodiments, the acrylic polymer is delivered as an aqueous solution and / or dispersion comprising from 20 to 60 wt% acrylic polymer, for example from 30 to 50 wt% acrylic polymer. Preferably, the acrylic polymer content in the aqueous solution and / or dispersion is from 35 to 45 wt%.
[0106] The acrylic polymer typically has a pH (in water) of from 6 to 10, for example from 6 to 9 and preferably from 8 to 9.
[0107] In some embodiments, the acrylic polymer in an aqueous solution and / or dispersion has a viscosity from 1 to 10,000 mPa-s, for example, from 10 to 1,000 mPa-s. Preferably, the acrylic polymer in an aqueous solution and / or dispersion has a viscosity from 20 to 200 mPa-s.
[0108] The viscosity of the acrylic polymer aqueous solution and / or dispersion is measured by a Brookfield viscometer. Preferably, the acrylic polymer content in the aqueous solution and / or dispersion is approximately from 35 to 45 wt% during the viscosity measurement.
[0109] In one embodiment, the acrylic polymer has a number average molecular weight (Mn) of from about 300,000 to about 2,000,000 g / mol, for example from about 400,000 to about 1,500,000 g / mol.
[0110] By "acrylamide copolymer" is meant a polymer formed from different monomers wherein one of the monomers is chosen from the group of (meth)acrylamide monomers. Preferably, the acrylamide copolymer comprises from about 20 to about 80 wt% (meth)acrylamide.
[0111] By "(meth)acrylamide" is meant acrylamide or methacrylamide, i.e. the parenthesis indicate that the methyl group may or may not be present.
[0112] The acrylamide copolymer typically comprises (meth)acrylamide and at least one acidic comonomer, preferably (meth)acrylamide and at least one comonomer selected from a carboxylic acid, a sulfonic acid, or mixtures thereof.
[0113] The acrylamide copolymer thus typically further comprises the inclusion of monomers of unsaturated organic acids selected from the group consisting of unsaturated carboxylic acids and unsaturated sulfonic acids and / or the alkali metal salt thereof.
[0114] Examples of unsaturated carboxylic acids include (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid and itaconic acid.
[0115] Examples of unsaturated sulfonic acids include o,B-ethylenically unsaturated sulfonic acid, such as vinylsulfonic acid, styrenesulfonic acid, (meth)allyl sulfonic acid, (meth)acrylamide t-butylsulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, 2-(meth)acrylamide-2-hydroxypropanesulfonic acid,
[0116] 3-sulfopropane(meth)acrylic ester, and bis-(3-sulfopropyl)itaconic ester.
[0117] Preferred unsaturated acid monomers include (meth)acrylic acid and (meth)allyl sulfonic acid.
[0118] Preferably, the acrylamide copolymer comprises from 5 to 50 wt% unsaturated organic acids and / or the alkali metal salt thereof, more preferably from 10 to 40 wt%.
[0119] The acid component is typically present in a mixture of the acid and alkali metal salt form, for instance with from 20% to 80%, preferably from 25% to 75%, of the acid groups present as the alkali metal salt.
[0120] Suitable alkali metals are selected from lithium, sodium or potassium, with lithium and sodium being preferred and lithium being particularly preferred. Optionally, the acrylamide copolymer comprises the inclusion of monomers of hydroxyl group-containing vinyl compounds. For example, the hydroxyl group-containing vinyl compound may be a hydroxyl-containing vinyl ether.
[0121] Optionally, the acrylamide copolymer comprises from 0 to 75 wt% hydroxyl group- containing vinyl compounds.
[0122] In some embodiments, the acrylamide copolymer is delivered as an aqueous solution comprising from 10 to 15 wt% acrylamide copolymer. Preferably, the acrylamide copolymer content in the aqueous solution is from 13 to 14 wt%, such as approximately 13.5 wt%.
[0123] In an embodiment, the acrylamide copolymer preferably has a pH (in water) from 5 to 10. Preferably, from 7 to 9. For example, the pH of the acrylamide copolymer can be altered by varying the amount of acid and metal salt thereof.
[0124] In some embodiments, the acrylamide copolymer in an aqueous solution has a viscosity from 10,000 to 30,000 mPa-s, for example, from 15,000 to 25,000 mPa-s. Preferably, the acrylamide copolymer in an aqueous solution has a viscosity from 17,000 to 23,000 mPa-s.
[0125] The viscosity of the acrylamide copolymer is measured by a B-type viscometer such as "B-type Viscometer Model BM" (product name) by Toki Sangyo Co., Ltd. Preferably, the acrylamide copolymer content in the aqueous solution is approximately 13.5 wt% during the viscosity measurement.
[0126] In one embodiment the acrylamide copolymer has a number average molecular weight (Mn) of from about 300,000 to about 2,000,000 g / mol, for example from about 400,000 to about 1,500,000 g / mol. Preferably, the number average molecular weight is between 500,000 to about 1,000,000 g / mol, for example between 600,000 and 900,000 g / mol.
[0127] In some embodiments, the acrylamide copolymer is present in an amount of from about 0.01 to about 2 wt%, such as from about 0.05 to about 1 wt%, preferably about 0.05 to about 0.7 wt%, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode). The binder polymer may have a glass transition temperature of from about -80 to about 65 °C, for example from about -60 to about 45 °C, such as from about -40 to about 25 °C. A glass transition temperature within this range may help to improve the electrode flexibility, which can subsequently lead to better cycle life performance and rate capacity of the cell.
[0128] In some embodiments, the acrylic polymer is present in an amount of from about 0.01 to about 5 wt%, such as from about 0.02 to about 4 wt%, for example from about 0.05 to about 3 wt%, such as from about 0.1 to about 2 wt%, preferably from about 0.1 to about 1 wt% based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0129] Dispersing medium
[0130] The slurry composition comprises a dispersing medium.
[0131] The dispersing media may include N-methyl pyrrolidone (NMP), water, or mixtures thereof.
[0132] Preferably, the dispersing medium comprises water. Other solvents may also be used in combination with water, such as organic solvents that are miscible with water may be used.
[0133] More preferably, the dispersing medium consists of water.
[0134] The use of aqueous solvents is preferred, since this can help to reduce costs by avoiding the use of a humidity-controlled environment and dry room conditions during cathode manufacture. Furthermore, the cost of the aqueous solvent itself may be cheaper compared to solvents such as NMP.
[0135] Cathode active material
[0136] The cathode active material may comprise a suitable material for use as an electrochemically active material in the cathode of a cell, particularly a lithium-ion cell.
[0137] The term "electrochemically active material" is to be understood as an electrochemical species which can be oxidised and reduced in a system which enables a cell to produce electric energy during discharge. The role of the cathode active material is to reversibly store, convert and / or alloy with lithium, e.g. via intercalation (or otherwise binding) ions (such as lithium ions) during cell charge and discharge cycles. The cathode active material may comprise an intercalation material, such as a lithium intercalation material, for example a lithium metal oxide which may include lithium and a transition metal.
[0138] The cathode active material may comprise any one or a mixture of two or more of lithium manganese oxide, lithium nickel oxide, lithium cobalt oxide, lithium nickel manganese oxide (LNMO), lithium nickel cobalt oxide, lithium nickel manganese cobalt (NMC) oxide, lithium iron phosphate (LFP), lithium iron manganese phosphate (LFMP) and lithium nickel cobalt aluminium oxide (NCA).
[0139] Preferably, the cathode active material is a LNMO or an NMC material, i.e. a lithium nickel manganese oxide or a lithium nickel manganese cobalt oxide. Even more preferably, the cathode active material is an NMC material intercalated with lithium or an "Li-NMC" material.
[0140] The cathode active material may comprise 80 mol% or more Ni, based on the total amount of non-lithium metals in the cathode active material, such as from about SO- 98 mol% Ni, for example from about 90-95 mol% Ni, such as from about 85-95 mol% Ni, such as from about 88-92 mol% Ni, based on the total amount of non-lithium metals in the cathode active material.
[0141] Exemplary cathode active materials include nickel-manganese-cobalt (NMC) composite oxides and lithium NMC (Li-NMC) composite oxides or lithium nickel manganese cobalt (NMC) oxides (LiNii-x-yCoxMnyO2 (0<x+y<0.2)).
[0142] In some embodiments, the cathode active material may comprise lithium nickel cobalt manganese oxides (NMC) (LibNii-x-y-zCoxMnyAzO2 (0<x+y+z<0.2)), where A is an element other than Li, Ni, Co, Mn or O and wherein 0<z<0.05, preferably 0<z<0.03, more preferably 0.001<z<0.01, and wherein 0.9<b<1.2. A is one or more chosen from the group Al, B, Zr, Ba, Ca, Ti, Mg, Ta, Nb, V, Fe, Ru, Re, Pt and Mo. Preferably, A is chosen from the group Al and Zr.
[0143] In preferred embodiments, the NMC cathode materials may be defined as LibNii-x-y-zCoxMnyAzO2, wherein 0<x+y+z<0.2, preferably 0<x+y+z<0.15, more preferably 0<x+y+z<0.12, and wherein 0<z<0.05, preferably 0.002<z<0.03, more preferably 0.001<z<0.01, and wherein 0.9<b<l.l. A is one or more chosen from the group Al, B, Zr, Ba, Ca, Ti, Mg, Ta, Nb, V, Fe, Ru, Re, Pt and Mo. Preferably, A is chosen from the group Al and Zr.
[0144] The cathode active material may comprise a lithium metal oxide material that is coated with another material. For example, a lithium metal oxide may be coated with a different lithium metal oxide, carbon, graphene, or a combination thereof. Furthermore, the coating material may have been coated using atomic layer deposition (ALD) as a non-limiting example.
[0145] The cathode active material may be present in an amount of from about 80 to about 99 wt%, for example from about 85 to about 99 wt%, such as from about 90 wt% to about 98 wt%, such as from about 95 to about 99 wt%, for example from about 95 to about 97 wt%, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0146] Conductive agent
[0147] The role of the conductive agent is to improve the electronic properties of the cathode and to provide an electrical connection between the particles of cathode active material in the cathode. As it is present merely to improve conductivity, it is optional as the inherent conductivity of the cathode active material may be sufficient.
[0148] For example, the conductive agent may comprise carbon black, acetylene black, graphene, graphite, mesocarbon microbead (MCMB), pitch-based carbon, coke powders, single-walled, thin-walled and / or multi-walled carbon nanotubes, metallic powders, or a combination thereof.
[0149] Preferred conductive agents are selected from carbon black, acetylene black, carbon nanotubes, or a combination thereof.
[0150] More preferably, the conductive agent is selected from carbon nanotubes.
[0151] In an embodiment, the conductive agent may be present in an amount of from about 0 wt% to about 6 wt%, for example from 0 wt% to about 4 wt%, such as from about 0 wt% to about 3 wt%, preferably from about 0.05 wt% to 2 wt%, or from about 0.1 wt% to 2 wt%, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode). Slurry composition
[0152] The slurry composition is formulated to a suitable viscosity to allow it to be processed into a cathode, for example by slot-die coating.
[0153] The slurry composition typically has a dynamic viscosity of from about 2 to about 40 Pa.s, for instance from about 5 to about 25 Pa.s, as measured at 25 °C.
[0154] The slurry composition typically contains from about 60 to 80 wt% solids, such as from about 65 to 75 wt% solids, preferably from about 68 to 73 wt% solids, more preferably from about 70 to 72 wt% solids, with the remainder being dispersing medium.
[0155] In some embodiments, the slurry composition does not comprise a group 13 element, such as boron, for example boric acid and / or boronic acid.
[0156] The method of formation of the slurry composition is not critical, and once formed it is typically stable at room temperature for at least one day, preferably at least one week. By "stable" in this context is meant that the solid particles do not settle.
[0157] While it may be possible to form the slurry composition by combining the ingredients in any order, for example the binder polymer may be added at any step in the method to form the slurry composition, best results are obtained when following the methods of the disclosure as described below.
[0158] There is provided a method for forming a slurry composition comprising the steps of: a. providing a composition comprising a cathode active material, an acidic polysaccharide, a lithiated polymer, a binder polymer, optionally a conductive agent, and optionally a dispersing medium; and b. adding dispersing medium to the composition and mixing to provide a slurry composition having a solids content of from 60 wt% to 80 wt%; provided that when the binder polymer comprises acrylic polymer, the method comprises adding said acrylic polymer, optionally together with dispersing medium, to an intermediate slurry composition having solids content of from 65 wt% to 85 wt%, and mixing to provide a slurry composition having a solids content of from 60 wt% to 80 wt%.
[0159] The intermediate slurry composition is prepared by adding dispersing medium to the composition of step a and mixing. The intermediate slurry composition may comprise a cathode active material, an acidic polysaccharide, a lithiated polymer, optionally a conductive agent, and a dispersing medium.
[0160] In the case of preparing the slurry composition wherein the binder polymer is an acrylic polymer, best results are obtained when following the method of the disclosure which comprises the steps of: i. providing a composition comprising cathode active material, an acidic polysaccharide, a lithiated polymer, optionally a conductive agent, and optionally a dispersing medium; ii. adding dispersing medium to the composition and mixing to provide an intermediate slurry composition having a solids content of from 65 wt% to 85 wt%; and iii. adding an acrylic polymer and optionally dispersing medium to the intermediate slurry composition to provide a slurry composition having a solids content of from 60 wt% to 80 wt%.
[0161] Step i. of the method comprises forming a mixture of cathode active material, (optional) conductive agent, acidic polysaccharide and lithiated polymer. These agents may be combined in any order, and may be dry mixed.
[0162] Typically, step i. comprises: forming a mixture of cathode active material and optional conductive agent; adding acidic polysaccharide and lithiated polymer and mixing, optionally in the presence of a dispersing medium.
[0163] The cathode active material and conductive agent may be dry mixed. However, the conductive agent (when present) is typically provided as a dispersion to aid in its processing. The first mixing step may therefore have small amounts of dispersing medium, which is typically water.
[0164] Likewise, the acidic polysaccharide and / or lithiated polymer may also be provided as dispersions, to aid in their processing. In view of this, step i. typically comprises providing a composition comprising cathode active material, an acidic polysaccharide, a lithiated polymer, a dispersing medium, and optionally a conductive agent, said composition having above 85 wt% solid content. Typically, the composition has a pH of from 5 to 8 after step i., for instance from about pH 6 to 7.
[0165] Step ii. comprises adding dispersing medium and mixing to decrease the solids content of the composition. During this step, the composition transitions through a clay-like solid to a free-flowing slurry.
[0166] The addition of dispersing medium is typically done stepwise, but may be continuous. The overall process is typically done at a rate which ensures even and thorough mixing of the dispersing medium into the composition. During this step, the lithiated polymer may begin to coat the cathode active material.
[0167] The pH of the composition after step ii. is typically from pH 6 to 8, for instance from about pH 6 to 7.
[0168] Step iii. comprises adding the acrylic polymer typically with dispersing medium under mixing to provide the final slurry composition.
[0169] Typically, the acrylic polymer is added as a dispersion to aid in its mixing into the composition.
[0170] Preferably, the acrylic polymer is added as an acrylic emulsion in the form of a waterbased dispersion. The pH of the slurry composition after step iii. is typically from pH 6 to 10, for instance from pH 7 to 10, for example from pH 7.5 to 9, preferably from pH 8 to 9.
[0171] Adding the acrylic polymer too early in the process may lead to poor coating properties and formation of bubbles. However, the acrylic polymer may be added at an earlier step in the process and still avoid the formation of bubbles, if the process, or part of the process, is carried out under vacuum. For example, the acrylic polymer may be added in step a. or step b.
[0172] Furthermore, adding the acrylic polymer too early in the process may lead to migration of the binder in the resulting cathode, i.e. binder migration to the edge of the cathode.
[0173] Additionally, if the acrylic polymer is exposed to very low pH compositions, it may precipitate resulting in poor integration into the slurry composition. In the case of preparing the slurry composition wherein the binder polymer is an acrylamide copolymer, best results are obtained when following the method of the disclosure which comprises the steps of:
[0174] 1) providing a composition comprising cathode active material, an acidic polysaccharide, a lithiated polymer, an acrylamide copolymer, optionally a conductive agent, and optionally a dispersing medium;
[0175] 2) adding dispersing medium to the composition and mixing to provide a slurry composition having a solids content of from 60 wt% to 80 wt%;
[0176] Step 1) of the method comprises forming a mixture of cathode active material, (optional) conductive agent, acidic polysaccharide, lithiated polymer and acrylamide copolymer. These agents may be combined in any order, and may be dry mixed.
[0177] Typically, step 1) comprises: forming a mixture of cathode active material and optional conductive agent; adding acidic polysaccharide, lithiated polymer and acrylamide copolymer and mixing, optionally in the presence of a dispersing medium.
[0178] When the binder polymer is only acrylamide copolymer, the method of making the slurry composition is simpler since the acrylamide copolymer may be combined and / or added together with the other components of the composition in the same step, i.e. in step 1). This results in a shorter processing time and lower operating cost.
[0179] Furthermore, the acrylamide copolymer does not display migration of the binder in the resulting cathode (e.g. migration of binder to the edge of the cathode), and so may be added during any step of the process. In addition, the acrylamide copolymer may be added at any step of the process without leading to bubble formation (although vacuum may still be used in the process).
[0180] The cathode active material and conductive agent may be dry mixed. However, the conductive agent (when present) is typically provided as a dispersion to aid in its processing. The first mixing step may therefore have small amounts of dispersing medium, which is typically water.
[0181] Likewise, the acidic polysaccharide and / or lithiated polymer may also be provided as dispersions, to aid in their processing. Typically, the acrylamide copolymer is added as a dispersion to aid in its mixing into the composition.
[0182] In view of this, step 1) typically comprises providing a composition comprising cathode active material, an acidic polysaccharide, a lithiated polymer, an acrylamide copolymer, a dispersing medium, and optionally a conductive agent, said composition having above 85 wt% solid content.
[0183] Typically, the composition has a pH of from 5 to 8 after step 1), for instance from about pH 6 to 7.
[0184] Step 2) comprises adding dispersing medium and mixing to decrease the solids content of the composition. During this step, the composition transitions through a clay-like solid to a free-flowing slurry having a solids content of from 60 to 80 wt%.
[0185] The addition of dispersing medium is typically done stepwise but may be continuous. The overall process is typically done at a rate which ensures even and thorough mixing of the dispersing medium into the composition. During this step, the alkali metal salt of the acidic polysaccharide may begin to coat the cathode active material.
[0186] The pH of the slurry composition after step 2) is typically from pH 6 to 10, for instance from pH 7 to 10, for example from pH 7.5 to 9, preferably from pH 8 to 9.
[0187] Typically, the slurry composition comprises at least 90 wt% cathode active material, preferably at least 95 wt% cathode active material, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0188] The slurry composition may be used to form a cathode in a cell using standard methodologies, such as by slot-die coating a conductive foil and drying the composition to form a cathode.
[0189] The cathode according to the disclosure (i.e. those containing the binder system of the disclosure, or formed from the slurry composition of the disclosure) display improved cycle life, good flexibility, and good adhesion to the conductive foil.
[0190] The remaining features of the cell of the disclosure will be briefly described. Conductive foil
[0191] The cell of the disclosure may comprise a first and second conductive foil. Said current foils act as one of a cathode or an anode current collector.
[0192] In a preferred embodiment, the first conductive foil acts as the cathode current collector and the second conductive foil acts as the anode current collector.
[0193] The cathode current collector may comprise a metal, such as aluminium, nickel or stainless steel. Preferably, the positive current collector is an aluminium foil.
[0194] The anode current collector may comprise a metal, such as copper, nickel or stainless steel. Preferably, the negative current collector is a copper foil.
[0195] The conductive foil may have a coating such as a carbon coating, which can improve conductivity at the interface with the electrode active material. The coating may also improve the peel strength (or adhesive properties) of layers coated thereon, reducing delamination of the electrode.
[0196] Anode
[0197] The cell may comprise an anode. The anode may comprise an anode active material, such as metallic lithium, lithium / aluminium alloys, lithium / tin alloys, carbon, graphite, black lead, silicon, silicon / silicon composite, or a combination thereof. The anode may further comprise a conductive agent and a binder.
[0198] The role of the anode active material is to reversibly bind the lithium. The mechanism of binding will vary, and may be by intercalation / deintercalation (for instance with graphite), alloying / dealloying (for instance with silicon), or by plating / stripping (for instance with metallic lithium), or combinations thereof.
[0199] Preferably, the anode comprises carbon and / or silicon.
[0200] Suitable anode active materials are selected from silicon, SiOx, silicon-carbon composites, prelithiated silicon or its composites and oxides, types of carbon, including natural and synthetic carbons, graphite, carbon black, active carbon, carbon fibres, cokes and other carbonaceous materials. The anode active material, conductive agent and binder may be coated on the second conductive foil (e.g. the copper foil). The anode active material, conductive agent and binder may be coated on the inner and outer sides of the second conductive foil.
[0201] Electrolyte
[0202] The cell of the disclosure further comprises an electrolyte. The electrolyte used in the cell according to the present disclosure may be a liquid electrolyte comprising at least one salt (particularly at least one lithium salt) and at least one or more solvents selected from the group consisting of carbonate solvents and their fluorinated equivalents, di-Ci-4-ethers and their fluorinated equivalents and ionic liquids. Alternatively, the electrolyte may be a solid electrolyte.
[0203] The lithium salt is preferably one or more selected from the group consisting of lithium hexafluorophosphate (LiPFe), lithium bis(fluorosulphonyl)imide (LiFSI), lithium bis(trifluoromethanesulphonyl)imide (LiTFSI), lithium
[0204] (fluorosulphonyl)(trifluoromethanesulphonyl)imide (LiFTFSI), lithium bis(pentafluoroethanesulphonyl)imide (LiBETI), lithium
[0205] (pentafluoroethanesulphonyl)(trifluoromethanesulphonyl)imide (LiPTFSI), lithium trifluoromethanesulphonate (LiOTf), lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LiDFOB), lithium difluorobis(oxalato)phosphate (LiDFOP), lithium tetrafluoro(oxalato)phosphate (LiTFOP), lithium tetrafluoroborate (UBF4), lithium nitrate (LiNOs) lithium 2-trifluoromethyl-4,5-dicyanoimidazole (LiTDI).
[0206] In one embodiment, the solvent is selected from the group consisting of 1,2- di methoxyethane (DME), N-propyl-N-methylpyrrolidinium bis(fluorosulphonyl)imide (PYR13-FSI), N-propyl-N-methylpyrrolidinium bis(trifluoromethanesulphonyl)imide (PYR13-TFSI), 1-butyl-l-methylpyrrolidinium bis(fluorosulphonyl)imide (PYR14-FSI), 1-butyl-l-methylpyrrolidinium bis(trifluoromethanesulphonyl)imide (PYR14-TFSI), 1- ethyl-3-methylimidazolium bis(fluorosulphonyl)imide (EMIM-FSI), l-ethyl-3- methylimidazolium bis(trifluoromethanesulphonyl)imide (EMIM-TFSI), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethylene carbonate (EC), and propylene carbonate (PC), and their fluorinated equivalents.
[0207] Separator
[0208] The cell of the disclosure may comprise one or more separators disposed between the anode and the cathode. The function of these separators is to prevent electrical contact between the cathode and the anode, whilst allowing the passage of ions. Any separator suitable for use in a cylindrical / pouch / prismatic / coin (e.g. lithium-ion) cell may be used.
[0209] For example, the separator may be made from a material such as glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or a combination thereof, and may be in the form of a nonwoven fabric or a woven fabric.
[0210] Optionally the separator is an integrated separator. For example, the separator may be integrated with a composite electrode to form an integrated electrode-separator (IES).
[0211] Cell
[0212] The cell may include at least a cathode, an anode and an electrolyte, wherein the cathode comprises the binder system described herein. The cell may include a separator.
[0213] The cell may be a cylindrical, prismatic, coin cell or pouch cell.
[0214] The cell may be a lithium-ion cell, such as a secondary lithium-ion cell.
[0215] Preferably, the cell is a cylindrical secondary lithium-ion cell.
[0216] Battery Pack
[0217] The battery pack may include one or more individual cells. The cells may be configured in a series, parallel, or a mixture thereof, in order to achieve the desired voltage, energy capacity and / or power density. The battery pack may include battery modules, wherein the battery modules include one or more individual cells. The battery pack may include interconnects which provide electrical conductivity between the cells. The battery pack may further include cooling and heating systems. The battery pack may also include software for managing the battery pack, for example a battery management system (BMS).
[0218] Vehicle
[0219] The disclosure also relates to a vehicle comprising the cell and / or battery pack of the disclosure. The vehicle is preferably an electric vehicle, such as a car, truck, bus, scooter, motorbike, bicycle, boat, plane or the like, preferably a car, truck or bus. The embodiments of the disclosure will be further described in the following nonlimiting examples:
[0220] Example 1
[0221] A coin half-cell was prepared using a cathode formed from the slurry composition described herein. Slurry compositions were prepared using water as the dispersing media. Alginic acid was used as the acidic polysaccharide and lithium polyacrylate was used as the lithiated polymer in the binder system. An acrylic polymer emulsion was used to provide the binder polymer. Lithium nickel manganese oxide (LiNio.75Mno.25O2) was used as the cathode active material.
[0222] The slurry composition comprised from about 95 to 99 wt% cathode active material, from about 0 to about 3 wt% conductive agent, from about 0.05 to 4 wt% acidic polysaccharide or salt thereof, from about 0.05 to 3 wt% lithiated polymer and from about 0.05 to 5 wt% acrylic polymer, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0223] The anode used in the coin half-cell was lithium. A ceramic-coated separator was used to separate the anode and cathode. Stainless steel was used for the positive and negative casing elements of the cell. The formation cycle results of the coin half-cell prepared using the slurry composition were compared to those using a slurry composition which did not comprise a lithium polyacrylate.
[0224] The voltage vs. capacity for the formation cycle of the coin half-cell is shown in Figure 1. The Figure shows a difference in properties between the electrodes formed with and without lithium polyacrylate during the charge and discharge cycles.
[0225] The coin half-cell prepared using the cathode slurry composition comprising lithium polyacrylate displayed better capacity retention after 50 cycles (1C / 1C) compared to the coin half-cell prepared using a slurry composition without lithium polyacrylate (Figure 2, Table 1). Table 1. Capacity retention of coin half-cells prepared using either a cathode slurry composition with lithium polyacrylate or a cathode slurry composition without lithium polyacrylate after 50 cycles.
[0226] Example 2
[0227] Coin half-cells were prepared using a cathode formed from slurry compositions described herein. The slurry compositions were prepared using water as the dispersing media. Alginic acid was used as the acidic polysaccharide and lithium polyacrylate was used as the lithiated polymer in the binder system. An acrylamide copolymer or an acrylic polymer were used as the binder polymer. Lithium nickel manganese oxide (LiNio.75Mno.25O2) was used as the cathode active material.
[0228] The slurry compositions comprised from about 95 to 99 wt% cathode active material, from about 0 to about 3 wt% conductive agent, from about 0.05 to 4 wt% acidic polysaccharide or salt thereof, from about 0.05 to 3 wt% lithiated polymer and from about 0.01 to 2 wt% acrylamide copolymer or from about 0.05 to 5 wt% acrylic polymer, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium, or alternatively the electrode).
[0229] The anode used in the coin half-cells was lithium. A ceramic- coated separator was used to separate the anode and cathode. Stainless steel was used for the positive and negative casing elements of the cells. The formation cycle results of the coin half-cells prepared using the slurry compositions were compared to those using a slurry composition which did not comprise a lithium polyacrylate. The results are based on data from an average of five cells in order demonstrate repeatability and reproducibility.
[0230] The formation cycle results of the coin half-cells prepared with lithium polyacrylate were superior to the coin half-cell prepared without lithium polyacrylate (Table 2). Table 2. Formation cycle results of coin half-cells prepared with or without lithium polyacrylate.
[0231] The voltage vs. capacity for the formation cycles of the coin half-cells is shown in Figure 3. The Figure shows a difference in properties between the electrodes formed with and without lithium polyacrylate during the charge and discharge cycles.
[0232] The coin half-cells prepared using the cathode slurry composition comprising lithium polyacrylate and acrylamide copolymer or acrylic polymer displayed better capacity retention after 50 cycles (1C / 1C) compared to the coin half-cell prepared using a slurry composition without lithium polyacrylate (Figure 4, Table 3).
[0233] Table 3. Capacity retention of coin half-cells prepared using either a cathode slurry composition with lithium polyacrylate and acrylic polymer or acrylamide copolymer, or a cathode slurry composition without lithium polyacrylate after 50 cycles.
[0234] Unless otherwise indicated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure pertains.
[0235] All embodiments of the disclosure and particular features mentioned herein may be taken in isolation or in combination with any other embodiments and / or particular features mentioned herein (hence describing more particular embodiments and particular features as disclosed herein) without departing from the disclosure of the disclosure. As used herein, the term "comprises" will take its usual meaning in the art, namely indicating that the component includes but is not limited to the relevant features (i.e. including, among other things). As such, the term "comprises" will include references to the component consisting essentially of the relevant substance(s).
[0236] Wherever the word 'about' is employed herein in the context of amounts, for example absolute amounts, weights, volumes, sizes, diameters etc., or relative amounts (e.g. percentages) of individual constituents in a composition or a component of a composition (including concentrations and ratios), timeframes, and parameters such as temperatures etc., it will be appreciated that such variables are approximate and as such may vary by ±10%, for example ±5% and preferably ±2% (e.g. ±1%) from the actual numbers specified herein. This is the case even if such numbers are presented as percentages in the first place (for example 'about 10%' may mean ±10% about the number 10, which is anything between 9% and 11%).'
Claims
Claims1. A slurry composition comprising: a cathode active material; a binder system; a dispersing medium; and optionally a conductive agent, wherein the binder system comprises: a binder polymer, an acidic polysaccharide, and a lithiated polymer.
2. The slurry composition according to claim 1, wherein the slurry composition has a solids content of from 65 to 75 wt%.
3. The slurry composition according to claim 1 or claim 2, wherein the binder system is present in an amount of from 2 to 5 wt% of the dry composition, based on the total weight of the dry composition (i.e. the slurry composition excluding the dispersing medium).
4. The slurry composition of any preceding claim, wherein the dispersing medium comprises water.
5. The slurry composition of any preceding claim, wherein the acidic polysaccharide is selected from one or more of alginic acid, carboxymethyl cellulose, xanthan gum, or mixtures thereof, for example wherein the acidic polysaccharide is selected from alginic acid.
6. The slurry composition of any preceding claim, wherein the lithiated polymer comprises lithium polyacrylate.
7. The slurry composition of any preceding claim, wherein the binder polymer is an acrylic polymer selected from one or more of poly(methyl methacrylate), poly(methyl acrylate), poly(ethyl acrylate), poly(butyl acrylate), poly(2-ethylhexyl acrylate), or mixtures thereof.
8. The slurry composition of any preceding claim, wherein the binder polymer is an acrylamide copolymer formed from different monomers comprising:a) 20 to 80 wt% (meth)acrylamide; b) 5 to 50 wt% unsaturated organic acids selected from carboxylic acids, sulfonic acids, or mixtures thereof, optionally present as alkali metal salts thereof; c) optionally, 0 to 75 wt% monomers of hydroxyl group-containing vinyl compounds such as hydroxyl-containing vinyl ethers.
9. The slurry composition of any preceding claim, wherein the cathode active material comprises a lithium nickel manganese cobalt oxide.
10. An electrode formed from the slurry composition of any preceding claim.
11. A method of making a slurry composition comprising the steps of: a. providing a composition comprising a cathode active material, an acidic polysaccharide, a lithiated polymer, a binder polymer, optionally a conductive agent, and optionally a dispersing medium; and b. adding dispersing medium to the composition and mixing to provide a slurry composition having a solids content of from 60 wt% to 80 wt%; provided that when the binder polymer comprises acrylic polymer, the method comprises adding said acrylic polymer, optionally together with dispersing medium, to an intermediate slurry composition having solids content of from 65 wt% to 85 wt%, and mixing to provide a slurry composition having a solids content of from 60 wt% to 80 wt%, wherein the intermediate slurry composition comprises a cathode active material, an acidic polysaccharide, a lithiated polymer, optionally a conductive agent, and a dispersing medium.
12. The method of claim 11, wherein the dispersing medium is according to claim 4, and / or wherein the acidic polysaccharide is according to claim 5, and / or wherein the lithiated polymer is according to claim 6, and / or wherein the binder polymer is according to claim 7 and / or claim 8, and / or wherein the cathode active material is according to claim 9.
13. An electrode comprising : a cathode active material; a binder system; and optionally a conductive agent, wherein the binder system comprises: a binder polymer, an acidic polysaccharide, anda lithiated polymer.
14. The electrode of claim 13, wherein the acidic polysaccharide is according to claim 5, and / or wherein the lithiated polymer is according to claim 6, and / or wherein the binder polymer is according to claim 7 and / or claim 8, and / or wherein the cathode active material is according to claim 9.
15. A cell comprising the electrode of claim 10, claim 13 or claim 14.
16. A battery pack comprising the cell of claim 15.
17. A vehicle comprising the battery pack of claim 16.
18. A method of making an electrode comprising providing a slurry composition according to any one of claims 1 to 9; and processing the slurry composition to form an electrode.
19. The method of claim 18, wherein the processing comprises coating a conductive foil with the slurry composition; and removing the dispersing medium to provide an electrode.
20. A binder system for an electrode comprising: a binder polymer, an acidic polysaccharide, and a lithiated polymer.
21. The binder system of claim 20, wherein the acidic polysaccharide is according to claim 5, and / or wherein the lithiated polymer is according to claim 6, and / or wherein the binder polymer is according to claim 7 and / or claim 8.
22. The binder system of claim 20 or claim 21, wherein the binder system comprises about 0.1 to 30 wt% of a binder polymer, about 55 to 97 wt% of an acidic polysaccharide and about 0.1 to 30 wt% of a lithiated polymer, based on the weight of the non-volatile content of the binder system.
Citation Information
Patent Citations
Cross-linking type aqueous binder for lithium ion battery and electrode prepared from cross-linking type aqueous binder
CN111106352A
Electrode for electrochemical devices and nonaqueous electrolyte secondary battery
EP4156332A1
Cross-linked binder composition for lithium ion batteries and methods for producing the same
US20150243995A1
Electrode slurry and electrode and lithium secondary battery including the same
US20190074516A1