Gas adsorption sheet for secondary battery with cover film
The gas adsorption sheet with a cover film addresses handling and moisture issues in non-aqueous secondary batteries by using a sheet form of gas adsorption materials, ensuring effective gas management and extended battery life.
Patent Information
- Application Number
- PCT/JP2023/044446
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2023-12-12
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional gas adsorbents for non-aqueous secondary batteries, such as those made of zeolite, have poor handling properties due to their granular or powdered form, leading to aggregation and dispersion issues, and their gas adsorption performance is compromised by moisture, necessitating improved solutions for effective gas management in batteries.
A gas adsorption sheet with a cover film is developed, comprising a heat-resistant base material and a gas adsorption layer made of a binder resin and inorganic porous material, where the gas adsorption particles are dispersed in a sheet form, enhancing handling and preventing moisture-induced deterioration, with optional intermediate and adhesive layers for improved adhesion and stability.
The sheet form of gas adsorption materials allows for better handling and application, maintains gas adsorption performance by preventing moisture damage, and can be easily integrated into existing battery manufacturing processes, extending battery life and ensuring reliable gas management.
Smart Images

Figure JP2023044446_24102024_PF_FP_ABST
Abstract
Description
Gas absorption sheet for secondary batteries with cover film
[0001] The present invention relates to a gas adsorbent sheet with a cover film for a secondary battery.
[0002] Conventionally, non-aqueous secondary batteries, such as lithium ion batteries, have been widely used in various fields. In non-aqueous secondary batteries using a non-aqueous electrolyte, CO is produced by electrolysis of carbonate ester contained in the non-aqueous electrolyte. 2 Gases such as these are likely to be generated, and the generated gases can cause deformation of the housing, an increase in internal resistance, a decrease in safety, and the like.
[0003] Various techniques have been investigated to prevent the above-described problems, and one such technique is a gas adsorbent made of zeolite with fine pores, capable of encapsulating and adsorbing gases (Patent Document 1). This gas adsorbent exhibits excellent gas adsorption performance and significantly improves the safety of non-aqueous secondary batteries. Furthermore, the use of this gas adsorbent also makes it possible to omit the degassing step in the secondary battery manufacturing process.
[0004] However, the gas adsorbents are provided in granular or powder form, which presents problems of poor handling. Furthermore, the granular or powder form also presents problems of difficulty in disposing the desired amount at the desired location, due to factors such as aggregation or unwanted dispersion. Furthermore, there is also the problem that the gas adsorption performance of the gas adsorbent is reduced due to the influence of moisture.
[0005] JP 2015-162457 A
[0006] The present invention has been made to solve the above-mentioned conventional problems, and an object of the present invention is to provide a gas adsorption sheet for secondary batteries that contains gas adsorption particles with excellent gas adsorption properties, and that allows the gas adsorption performance of the gas adsorption particles to be fully exhibited.
[0007] [1] A gas adsorption sheet for a secondary battery with a cover film according to an embodiment of the present invention comprises a gas adsorption sheet for a secondary battery including a heat-resistant substrate and a gas adsorption layer disposed on at least one side of the heat-resistant substrate; and a cover film disposed on the gas adsorption layer opposite the heat-resistant substrate. The gas adsorption layer is composed of a binder resin and an inorganic porous material having micropores and contains gas adsorption particles capable of adsorbing gas. [2] The gas adsorption sheet for a secondary battery with a cover film described in [1] above may further comprise an intermediate layer disposed between the heat-resistant substrate and the gas adsorption layer. [3] In the gas adsorption sheet for a secondary battery with a cover film described in [1] or [2] above, the gas adsorption particles may have a surface treated with silicone. [4] In the gas adsorption sheet for a secondary battery with a cover film described in [3] above, the silicone may have an ethoxysilane group or a methoxysilane group. [5] In the gas adsorption sheet for a secondary battery with a cover film described in [4] above, the silicone may be a silane coupling agent containing an epoxy group or an amino group. [6] In the gas adsorption sheet for a secondary battery with a cover film described in any one of [1] to [5] above, the binder resin may be an acrylic resin. [7] In the gas adsorption sheet for a secondary battery with a cover film described in [6] above, the binder resin may contain a structural unit derived from a (meth)acrylic acid alkyl ester, and the (meth)acrylic acid alkyl ester may have a linear or branched alkyl group having 4 to 12 carbon atoms. [8] In the gas adsorption sheet for a secondary battery with a cover film described in any one of [1] to [5] above, the binder resin may be butyl rubber, isoprene rubber, polyisobutylene rubber, ethylene propylene rubber, or a silicone resin. [9] In the gas adsorbent sheet for a secondary battery with a cover film according to any one of [1] to [8] above, the content of the gas adsorbent particles may be 10 parts by weight to 90 parts by weight per 100 parts by weight of the gas adsorbent sheet for a secondary battery.
[10] In the gas adsorption sheet for a secondary battery with a cover film described in any one of [1] to [9] above, the material constituting the heat-resistant substrate may be polyamideimide, polyetherimide, polyphenylene sulfide, polyethylene naphthalate, polyimide, or polyether ether ketone.
[11] In the gas adsorption sheet for a secondary battery with a cover film described in any one of [1] to
[10] above, the cover film may include a substrate and a pressure-sensitive adhesive layer disposed on at least one side of the substrate.
[12] In the gas adsorption sheet for a secondary battery with a cover film described in
[11] above, the pressure-sensitive adhesive layer may be formed from a pressure-sensitive adhesive containing a base polymer, and the content of structural units derived from organic acid monomers may be preferably 0.5 parts by weight or less per 100 parts by weight of the base polymer.
[13] In the gas adsorption sheet for a secondary battery with a cover film described in any one of [1] to
[12] above, the cover film may be peelable.
[0008] According to the present invention, by forming gas adsorption particles into a sheet in combination with a heat-resistant substrate, a gas adsorbent (gas adsorption sheet) with excellent handleability can be obtained. In this gas adsorption sheet, the gas adsorption performance inherent to the gas adsorption particles can be fully exhibited, and deterioration of the gas adsorption performance due to moisture can be prevented.
[0009] 1 is a schematic cross-sectional view of a gas adsorbent sheet for a secondary battery according to one embodiment of the present invention.
[0010] A. Overall Configuration of a Gas Adsorption Sheet for a Secondary Battery with a Cover Film FIG. 1 is a schematic cross-sectional view of a gas adsorption sheet for a secondary battery with a cover film (hereinafter also referred to as a gas adsorption sheet with a cover film) according to one embodiment of the present invention. The gas adsorption sheet with a cover film 100 comprises a gas adsorption sheet for a secondary battery 110 including a heat-resistant substrate 10 and a gas adsorption layer 20 disposed on at least one side of the heat-resistant substrate 10, and a cover film 120 disposed on the opposite side of the gas adsorption layer 20 from the heat-resistant substrate 10. The gas adsorption layer includes a binder resin and gas adsorption particles. The gas adsorption particles are composed of an inorganic porous material having pores. The gas adsorption particles exhibit high gas adsorption performance due to the inclusion action. Gases adsorbed by the gas adsorption particles include, for example, CO, CO 2 and the like. In one embodiment, the gas adsorption sheet 110 further includes an intermediate layer 30 between the heat-resistant substrate 10 and the gas adsorption layer 20. The formation of the intermediate layer can prevent the gas adsorption layer from falling off. In another embodiment, the cover film 120 includes a substrate 41 and an adhesive layer 51 disposed on at least one side of the substrate 41. The adhesive layer 51 can be laminated so as to face the gas adsorption layer 20. In this specification, the gas adsorption sheet for a secondary battery with a cover film is also simply referred to as a gas adsorption sheet with a cover film, and the gas adsorption sheet for a secondary battery is also simply referred to as a gas adsorption sheet. The gas adsorption sheet with a cover film and the gas adsorption sheet may include any appropriate other layer as long as the effects of the present invention are obtained. For example, the gas adsorption sheet may include an adhesive layer disposed on one or both outer surfaces (not shown) of the gas adsorption sheet.
[0011] According to the present invention, a gas adsorption sheet that is easy to handle and applicable to various applications can be obtained by dispersing gas adsorption particles in a binder resin, forming a gas adsorption layer composed of the gas adsorption particles and the binder resin, and forming the sheet. Furthermore, by providing a heat-resistant substrate, the effect of improving handleability becomes even more pronounced. Furthermore, by using a heat-resistant substrate as the substrate, the gas adsorption sheet can be heated (e.g., heated at 200°C for 24 hours) before use. Heating before use can remove unnecessary substances adhering to the gas adsorption particles, allowing the gas adsorption particles to fully exhibit their performance during use.
[0012] The gas adsorption sheet can be suitably used, for example, as a gas adsorbent for a non-aqueous secondary battery. Specifically, it can be used in the form of an insulating sheet, insulating plate, insulating tape, or the like, which is placed in a non-aqueous electrolyte. The gas adsorption sheet can adsorb CO and CO 2 In addition, the gas adsorption sheet can also adsorb moisture, hydrogen fluoride, etc., and applying the gas adsorption sheet to a battery can extend its lifespan. Furthermore, by providing the gas adsorbent in sheet form, it becomes possible to apply the gas adsorbent to a battery using existing battery manufacturing equipment. Furthermore, using the gas adsorption sheet makes it easy to arrange a desired amount of gas adsorption particles in a desired position.
[0013] Furthermore, in the present invention, by providing a cover film, it is possible to prevent deterioration of the gas adsorption layer due to moisture, for example, during storage. Even in a dry room (e.g., a dew point temperature of −50° C.), and even in a gas adsorption sheet having a gas adsorption layer that is susceptible to moisture deterioration, the above-described configuration can prevent deterioration of the gas adsorption layer due to moisture (e.g., a decrease in gas absorbency).
[0014] The thickness of the gas adsorbent sheet with cover film is preferably 15 μm to 1100 μm, more preferably 30 μm to 550 μm, and even more preferably 30 μm to 200 μm.
[0015] B. Gas Adsorption Sheet The gas adsorption sheet may have adhesive properties on one or both sides, or may be a gas adsorption sheet without adhesive properties. Examples of gas adsorption sheets with adhesive properties include a gas adsorption layer having adhesive properties and a gas adsorption sheet having an adhesive layer disposed on the outermost surface thereof.
[0016] When the gas adsorption sheet has adhesive properties, the adhesive strength of the gas adsorption sheet to a stainless steel plate at 25°C is preferably 0.1 N / 20 mm to 10 N / 20 mm, more preferably 0.5 N / 20 mm to 5 N / 20 mm. Within these ranges, the gas adsorption sheet can be suitable for battery applications. In this specification, adhesive strength refers to adhesive strength measured by a method in accordance with JIS Z 0237:2000, in which an adhesive tape is applied to an adherend (SUS304BA) by rolling a 2 kg roller back and forth once, and the adhesive tape is left to stand at 25°C for 30 minutes, and then peeled off at a peel angle of 180° and a peel rate (tensile speed) of 300 mm / min.
[0017] The thickness of the gas adsorption sheet is preferably 10 μm to 1000 μm, more preferably 20 μm to 500 μm, even more preferably 20 μm to 150 μm, and even more preferably 20 μm to 130 μm. Within these ranges, a gas adsorption sheet with excellent gas adsorption performance and handleability can be obtained.
[0018] B-1. Gas Adsorption Layer As described above, the gas adsorption layer contains a binder resin and gas adsorption particles dispersed in the binder resin. In the present invention, this configuration makes it possible to form the gas adsorption layer by coating using a coating liquid containing the binder resin and the gas adsorption particles. As a result, a gas adsorption layer with excellent dispersibility of the gas adsorption particles can be formed, and a gas adsorption sheet with excellent gas adsorption performance can be obtained.
[0019] The thickness of the gas adsorption layer is preferably 5 μm to 150 μm, more preferably 5 μm to 120 μm, and even more preferably 10 μm to 100 μm. Within this range, the gas adsorption layer can fully exhibit the performance of the gas adsorption particles. Furthermore, a gas adsorption sheet with excellent handleability can be obtained.
[0020] (Gas-adsorbing particles) The gas-adsorbing particles are made of an inorganic porous material having pores. In one embodiment, the gas-adsorbing particles are made of zeolite. The zeolite may be A-type zeolite, X-type zeolite, or LSX-type zeolite. Preferably, the cation moiety of the zeolite is A-type zeolite ion-exchanged with Li, or A-type zeolite ion-exchanged with Ca. The ratio of Si to Al (Si / Al) constituting the gas-adsorbing particles is preferably 1 to 5. If the Si / Al ratio is less than 1, the gas-adsorbing particles may be structurally unstable. Furthermore, if the Si / Al ratio exceeds 5, the adsorption performance may be reduced.
[0021] The volume average particle diameter D50 (median diameter) of the gas-adsorbed particles is preferably 50 μm or less, more preferably 20 μm or less. Within this range, a gas-adsorbed layer with a high gas adsorption capacity can be formed. The volume average particle diameter D50 (median diameter) can be measured using a laser diffraction / scattering particle size distribution analyzer.
[0022] The specific surface area of the gas adsorption particles is preferably 100 m 2 / g to 3000m 2 / g. Within this range, gas-adsorbed particles having excellent gas adsorption performance and mechanical strength can be obtained. Gas-adsorbed particles having a large specific surface area are prone to aggregation, but according to the present invention, a gas-adsorbed layer can be formed with good dispersibility of the gas-adsorbed particles.
[0023] The gas-adsorbing particles have pores, the size of which is preferably 3 Å to 10 Å, and the pores are preferably present over the entire surface of the gas-adsorbing particles.
[0024] The CO2 The adsorption amount is preferably 15 mL / g or more, more preferably 20 mL / g or more, and even more preferably 30 mL / g or more. 2 The adsorption amount is the amount of CO per 1 g of gas adsorption particles. 2 It means the amount of CO adsorption. 2 The method for measuring the amount of adsorption is as follows. 2 Method for measuring the amount of adsorption> The gas-adsorbing particles are immersed in a lithium-ion battery electrolyte (composition: lithium hexafluorophosphate (1 mol / l) ethylene carbonate solution / ethyl methyl carbonate = 3 / 7 (volume ratio)) in a predetermined sealed glass container in an environment with a dew point of -40°C so that the electrolyte amount per 1 g of gas-adsorbing particles is 80 ml / g, and then stored at 60°C for 24 hours. 2 The same procedure as above was repeated except that no gas adsorption particles were added, that is, only the electrolyte solution for a lithium ion battery was sealed in a glass container and stored at 60°C for 24 hours. 2 The concentration B was measured (concentration B = 0.43 v / v%), and CO 2 Concentration A and CO 2 The gas adsorption amount of the gas adsorption particles (gas adsorption amount per 1 g of gas adsorption particles (mL / g)) is evaluated from the difference with concentration B.
[0025] In one embodiment, the gas-adsorbing particles have a surface-treated surface. The surface treatment may be a treatment for adjusting the affinity between the gas-adsorbing particles and the binder resin. By using gas-adsorbing particles having a surface-treated surface, a gas-adsorbing layer having excellent mechanical strength and resistance to shedding can be formed. The gas-adsorbing sheet with a cover film laminated thereon is particularly preferred in that damage to the gas-adsorbing layer can be prevented when the cover film is peeled off during use of the gas-adsorbing sheet. Furthermore, by using gas-adsorbing particles having a surface-treated surface, a gas-adsorbing sheet having excellent processability during cutting can be obtained. For example, damage to the gas-adsorbing layer can be prevented when punching the gas-adsorbing sheet with a blade such as a Thomson blade. The surface-treated surface may be the entire surface of the gas-adsorbing particles, or a portion of the surface. Examples of surface treatments include silane coupling agent treatment, isocyanate compound treatment, thiol compound treatment, acid compound treatment, alcohol compound treatment, and epoxy compound treatment. In one embodiment, the surface treatment may be a coupling treatment. The use of coupling-treated gas adsorbent particles significantly prevents the gas adsorbed layer from being separated and improves processability.
[0026] In one embodiment, gas adsorption particles having a surface treated with silicone are used. In one embodiment, the silicone has an ethoxysilane group or a methoxysilane group. Use of such a silicone allows for the formation of a gas adsorption layer that is excellent in mechanical strength and resistant to shedding. The silicone may be a silane coupling agent. Preferably, the silane coupling agent contains an epoxy group and / or an amino group. Use of such a silane coupling agent allows for the formation of a gas adsorption layer that is excellent in mechanical strength and resistant to shedding. The gas adsorption particles, i.e., gas adsorption particles surface-treated with silicone (silane coupling agent), can be obtained by contacting the silane coupling agent with the gas adsorption particle surface to react organic groups (e.g., hydroxyl groups) present on the surface with silanol groups generated by hydrolysis of the silane coupling agent, or by bonding oligomers generated by condensation of the silanol groups to the gas adsorption particles.
[0027] Examples of the silane coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-amino N-propylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl)-2-aminopropyltrimethoxysilane hydrochloride, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-isocyanatopropyltriethoxysilane, dithioltriazinepropyltriethoxysilane, and the like.
[0028] The content of the gas adsorption particles is preferably 10 to 90 parts by weight, more preferably 30 to 80 parts by weight, and even more preferably 40 to 70 parts by weight, relative to 100 parts by weight of the gas adsorption sheet. Within such a range, a gas adsorption sheet having excellent gas adsorption performance and easy handling can be obtained.
[0029] The content of the gas adsorption particles is preferably 10 to 2,000 parts by weight, more preferably 50 to 1,500 parts by weight, even more preferably 100 to 1,000 parts by weight, and particularly preferably 280 to 1,000 parts by weight, relative to 100 parts by weight of the binder resin constituting the gas adsorption layer. Within this range, a gas adsorption layer can be obtained from which the gas adsorption particles are resistant to desorption. Furthermore, a gas adsorption sheet can be obtained that exhibits excellent gas adsorption performance, handleability, and electrolyte resistance.
[0030] (Binder Resin) Any appropriate resin can be used as the binder resin as long as the effects of the present invention can be obtained. Examples of binder resins include acrylic resins; rubber-based resins such as butyl rubber, isoprene rubber, polyisobutylene rubber, and ethylene propylene rubber; silicone-based resins; urethane-based resins; epoxy-based resins; alkyd-based resins; polyester-based resins; melamine-based resins; polyamide-based resins; polyimide-based resins; ethylene-vinyl acetate copolymer resins; and polyvinyl alcohol-based resins. In one embodiment, an acrylic resin is preferably used. The use of an acrylic resin makes it possible to form a gas adsorption layer that exhibits excellent dispersibility of gas adsorption particles. Furthermore, the use of an acrylic resin makes it possible to form a gas adsorption layer that is difficult to desorb. Furthermore, it makes it possible to form a gas adsorption layer that allows the gas adsorption performance of the gas adsorption particles to be fully exhibited. In another embodiment, butyl rubber, isoprene rubber, polyisobutylene rubber, ethylene propylene rubber, or a silicone-based resin is used. The use of these resins makes it possible to form a gas adsorption layer that exhibits excellent dispersibility of gas adsorption particles.
[0031] The binder resin preferably has gas permeability. By using a binder resin having gas permeability, a gas adsorption sheet suitable for battery applications can be obtained. Examples of resins with excellent gas permeability include acrylic resins; rubber-based resins such as butyl rubber, isoprene rubber, polyisobutylene rubber, and ethylene propylene rubber; silicone-based resins; urethane-based resins; epoxy-based resins; alkyd-based resins; polyester-based resins; melamine-based resins; polyamide-based resins; and polyimide-based resins. 2 The permeability is preferably 1500 cm 3 / m 2 24 hrs atm or more, more preferably 3000 cm 3 / m 2 ・24 hrs·atm or more. CO in the gas adsorption layer 2 The permeation amount can be measured in an environment at a temperature of 23°C according to JIS K 7126 (isobaric method).
[0032] The binder resin preferably exhibits high affinity for the non-aqueous electrolyte solution. For example, the binder resin may have an SP value of 8 cal / cm 3 ~15.4cal / cm 3 (preferably 9 cal / cm 3 ~13.2cal / cm 3 In addition, the binder resin preferably has high resistance to a non-aqueous electrolyte solution.
[0033] Examples of acrylic resins include acrylic resins containing one or more structural units derived from (meth)acrylic acid alkyl esters. The content of the structural units derived from (meth)acrylic acid alkyl esters is preferably 50 to 97 parts by weight, more preferably 70 to 94 parts by weight, per 100 parts by weight of the acrylic resin.
[0034] Preferably, the (meth)acrylic acid alkyl ester has a linear or branched alkyl group having 1 to 24 carbon atoms (more preferably 3 to 20, and even more preferably 6 to 18).
[0035] In one embodiment, the (meth)acrylic acid alkyl ester preferably has a linear or branched alkyl group having 4 to 12 carbon atoms, and more preferably has a linear or branched alkyl group having 6 to 12 carbon atoms. Forming a gas adsorption layer using an acrylic resin having such a (meth)acrylic acid alkyl ester as a main structural unit can provide a gas adsorption sheet that is inhibited from discoloring and swelling in an electrolyte solution. Furthermore, a gas adsorption layer that is difficult to desorb can be formed. In one embodiment, the content of structural units derived from linear or branched alkyl groups having 4 to 12 carbon atoms in the acrylic resin is preferably 20 to 100 parts by weight, more preferably 30 to 100 parts by weight, even more preferably 50 to 100 parts by weight, and particularly preferably 70 to 100 parts by weight, per 100 parts by weight of structural units derived from the (meth)acrylic acid alkyl ester.
[0036] Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and eicosyl (meth)acrylate.
[0037] In one embodiment, a (meth)acrylic acid alkyl ester having a branched alkyl group is used as the (meth)acrylic acid alkyl ester. By using a (meth)acrylic acid alkyl ester having a branched alkyl group, a gas adsorption layer can be formed that can fully exhibit the gas adsorption performance of the gas adsorption particles. A (meth)acrylic acid alkyl ester having a linear alkyl group and a (meth)acrylic acid alkyl ester having a branched alkyl group may be used in combination. Furthermore, a (meth)acrylic acid alkyl ester having a branched alkyl group may be used alone as the (meth)acrylic acid alkyl ester.
[0038] In one embodiment, in the acrylic resin, the content of structural units derived from (meth)acrylic acid alkyl esters having a branched alkyl group is preferably 20 to 100 parts by weight, more preferably 30 to 100 parts by weight, even more preferably 50 to 100 parts by weight, and particularly preferably 70 to 100 parts by weight, per 100 parts by weight of structural units derived from (meth)acrylic acid alkyl esters (including methyl (meth)acrylate and ethyl (meth)acrylate) having a linear alkyl group and a (meth)acrylic acid alkyl ester having a branched alkyl group (100 parts by weight). Within such a range, a gas adsorption sheet having particularly excellent electrolyte resistance can be obtained.
[0039] Examples of (meth)acrylic acid alkyl esters having a branched alkyl group include isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, stearyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, and 2-methylbutyl (meth)acrylate. Of these, 2-ethylhexyl (meth)acrylate is preferred.
[0040] The acrylic resin may contain, as necessary, a structural unit derived from another monomer copolymerizable with the alkyl (meth)acrylate, for the purpose of modifying properties such as cohesive strength, heat resistance, and crosslinkability. Examples of such other monomers include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; phosphoric acid group-containing monomers such as 2-hydroxyethyl acryloyl phosphate; sulfonic acid group-containing monomers such as styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl methacrylate. hydroxyl group-containing monomers; (N-substituted) amide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; aminoalkyl (meth)acrylate monomers such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; methoxyethyl (meth)acrylate, (Meth)acrylate alkoxyalkyl monomers such as ethoxyethyl (meth)acrylate; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide;succinimide-based monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyoctamethylene succinimide; vinyl-based monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinylcarboxylic acid amides, styrene, α-methylstyrene, and N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and (meth)acrylate. Examples of suitable monomers include glycol-based acrylic ester monomers such as methoxypolypropylene glycol acrylate; acrylic ester monomers having heterocycles, halogen atoms, silicon atoms, etc., such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, and silicone (meth)acrylate; polyfunctional monomers such as hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; olefin-based monomers such as isoprene, butadiene, and isobutylene; and vinyl ether-based monomers such as vinyl ether. These monomer components may be used alone or in combination of two or more.
[0041] The content of the structural units derived from the other monomers is preferably 20 parts by weight or less, more preferably 15 parts by weight or less, and even more preferably 1 to 10 parts by weight, relative to 100 parts by weight of the acrylic resin.
[0042] The weight-average molecular weight of the acrylic resin is preferably 300,000 to 2,000,000, and more preferably 500,000 to 1,500,000. The weight-average molecular weight can be measured by GPC (solvent: THF).
[0043] (Additives) The gas adsorption layer may contain any appropriate additives as needed, such as crosslinkers, tackifiers (e.g., rosin-based tackifiers, terpene-based tackifiers, hydrocarbon-based tackifiers, etc.), plasticizers (e.g., trimellitic ester-based plasticizers, pyromellitic ester-based plasticizers), pigments, dyes, antioxidants, conductive materials, antistatic agents, light stabilizers, release modifiers, softeners, surfactants, flame retardants, antioxidants, ultraviolet absorbers, particles, etc.
[0044] B-2. Heat-Resistant Substrate In this specification, a heat-resistant substrate refers to a substrate that can withstand heating for 24 hours in an atmosphere at a temperature of 150°C and a pressure of -100 kPa to 0 kPa (preferably, 24 hours in an atmosphere at a temperature of 200°C and a pressure of -100 kPa to 0 kPa), and specifically refers to a substrate that undergoes a dimensional change of 5% or less when heated for 24 hours in an atmosphere at a temperature of 150°C and a pressure of -100 kPa (preferably, 24 hours in an atmosphere at a temperature of 200°C and a pressure of -100 kPa). Furthermore, when the heat-resistant substrate is formed from a resin, the heat-resistant substrate refers to a substrate made of a resin having a glass transition temperature of 80°C or higher (preferably, 100°C or higher, more preferably, 150°C or higher). The term "glass transition temperature" refers to the temperature at which the loss tangent (tan δ) peaks when measured by the DMA method (tensile method) under the following conditions: a temperature rise rate of 5°C / min, a sample width of 5 mm, a chuck distance of 20 mm, and a frequency of 10 Hz.
[0045] Any suitable material can be used as the material for the heat-resistant substrate as long as the effects of the present invention can be obtained. Preferably, the heat-resistant substrate is made of a resin. Examples of materials for the heat-resistant substrate include polyamideimide (PAI), polyetherimide (PEI), polyphenylene sulfide (PPS), polyethylene naphthalate (PEN), polyimide (PI), and polyether ether ketone (PEEK). These resins have excellent heat resistance and excellent electrolyte resistance.
[0046] The thickness of the heat-resistant substrate is preferably 5 μm to 500 μm, more preferably 10 μm to 300 μm, and even more preferably 15 μm to 100 μm. Within such a range, a gas adsorbent sheet with particularly excellent handleability can be obtained.
[0047] B-3. Intermediate Layer The intermediate layer contains any appropriate resin. Examples of resins forming the intermediate layer include acrylic resins, rubber resins, and silicone resins. Among these, acrylic resins are preferably used. Furthermore, an active energy ray-curable acrylic resin may be used as the adhesive. Examples of resins forming the intermediate layer include the binder resins described above. In one embodiment, the resin forming the intermediate layer is the same as the binder resin forming the gas adsorption layer. The intermediate layer does not contain gas adsorption particles.
[0048] By forming the intermediate layer, it is possible to obtain a gas adsorbing sheet in which the gas adsorbing layer is less likely to desorb.
[0049] The thickness of the intermediate layer is preferably 1 μm to 50 μm, more preferably 2 μm to 30 μm, and even more preferably 2 μm to 20 μm.
[0050] The intermediate layer may contain any appropriate additives as needed, such as a crosslinking agent, a tackifier, a plasticizer (e.g., a trimellitic ester-based plasticizer or a pyromellitic ester-based plasticizer), a pigment, a dye, a filler, an antioxidant, a conductive agent, an ultraviolet absorber, a light stabilizer, a release adjuster, a softener, a surfactant, a flame retardant, an antioxidant, and a solvent.
[0051] C. Cover Film In one embodiment, the cover film includes a substrate and a pressure-sensitive adhesive layer disposed on at least one side of the substrate.
[0052] In one embodiment, the cover film is disposed in a releasable manner. In one embodiment, the cover film is releasable from the gas adsorption sheet after heat drying at 110°C for 3 hours. The releasability of such a cover film can be controlled by adjusting the adhesive strength of the cover film, for example, by adjusting the composition of the adhesive layer.
[0053] The adhesive strength of the cover film to a stainless steel plate at 25°C is preferably 0.05 N / 20 mm to 5 N / 20 mm, more preferably 0.1 N / 20 mm to 3 N / 20 mm, more preferably 0.15 N / 20 mm to 2 N / 20 mm, and even more preferably 0.15 N / 20 mm to 1 N / 20 mm.
[0054] After drying the cover film-attached gas adsorption sheet at 110°C under a reduced pressure of -100 kPa for 3 hours, the peel strength when peeling the cover film from the gas adsorption sheet is preferably 0.01 N / 50 mm to 5 N / 50 mm, more preferably 0.02 N / 50 mm to 3 N / 50 mm, and even more preferably 0.05 N / 50 mm to 2.5 N / 50 mm. Within these ranges, the cover film can be peeled off while preventing damage to the gas absorbing layer. The peel strength can be measured using a method in accordance with JIS Z 0237:2000. That is, the peel strength is measured by peeling the cover film of the cover film-attached gas adsorption sheet from the gas adsorption sheet under the following conditions: a measurement temperature of 25°C, a peel angle of 180°, and a peel rate (tensile speed) of 300 mm / min.
[0055] C-1. Substrate The substrate can be made of any appropriate material. Various sheet-like materials can be used as the substrate, such as resin film, paper, cloth, nonwoven fabric, metal foil, or plastic laminates thereof, or laminates of plastics. Among these, resin film is most preferable from the standpoints of handleability and cost. The material constituting the resin film can be selected as needed from the standpoints of strength, heat resistance, and the like. Examples include olefin-based resins containing α-olefins as monomer components, such as polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, and ethylene-vinyl acetate copolymer (EVA); polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); polyvinyl chloride (PVC); polyphenylene sulfide (PPS); amide-based resins such as polyamide (nylon) and wholly aromatic polyamide (aramid); polyether ether ketone (PEEK), polyimide, polyetherimide, polystyrene, and acrylic resin. These materials can be used alone or in combination of two or more. The plastic film may be any of an unstretched film, a uniaxially oriented film, and a biaxially oriented film. These films may be laminated films consisting of two or more film layers, or may contain a lubricant such as inert particles added thereto for ease of handling.
[0056] The thickness of the substrate is preferably 200 μm or less, more preferably 1 μm to 200 μm, even more preferably 5 μm to 100 μm, particularly preferably 10 μm to 100 μm, particularly preferably 20 μm to 100 μm, and most preferably 30 μm to 100 μm. Within such a range, lifting is prevented when the substrate is formed into a roll, and a gas adsorbent sheet with a cover film that is easy to work with can be obtained.
[0057] The moisture permeability of the substrate is preferably 500 g / m 2 24 hours or less, more preferably 100 g / m 2The moisture permeability can be determined in accordance with the moisture permeability test (cup method) of JIS Z 0208.
[0058] The substrate may be subjected to a surface treatment, such as corona treatment, chromic acid treatment, ozone exposure, flame exposure, high-voltage shock exposure, ionizing radiation treatment, or coating with a primer.
[0059] C-2. Pressure-sensitive adhesive layer The thickness of the pressure-sensitive adhesive layer is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. The lower limit of the thickness of the pressure-sensitive adhesive layer is, for example, 1 μm (preferably 0.5 μm).
[0060] The pressure-sensitive adhesive layer includes any suitable pressure-sensitive adhesive. Any suitable pressure-sensitive adhesive can be used as the pressure-sensitive adhesive as long as the effects of the present invention can be obtained. For example, a pressure-sensitive adhesive can be used as the pressure-sensitive adhesive.
[0061] Examples of pressure-sensitive adhesives include acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, and styrene-diene block copolymer adhesives. Among these, acrylic adhesives or rubber adhesives are preferred, and acrylic adhesives are even more preferred. The above-mentioned adhesives may be used alone or in combination of two or more. In one embodiment, from the viewpoint of ultraviolet absorption, an adhesive containing a base polymer having an aromatic ring and / or a double bond is used. From this perspective, acrylic adhesives may be preferably used.
[0062] Examples of the acrylic adhesive include an acrylic adhesive having as a base polymer an acrylic polymer (homopolymer or copolymer) using one or more (meth)acrylic acid alkyl esters as a monomer component. Specific examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and methyl (meth)acrylate. Examples of (meth)acrylic acid C1-20 alkyl esters include nonyl acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. Of these, (meth)acrylic acid alkyl esters having a linear or branched alkyl group having 4 to 18 carbon atoms can be preferably used.
[0063] The acrylic polymer may contain, as necessary, units corresponding to other monomer components copolymerizable with the alkyl (meth)acrylate, for the purpose of modifying properties such as cohesive strength, heat resistance, and crosslinkability. Examples of such monomer components include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itanoic anhydride; hydroxyl group-containing monomers such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl methacrylate; sulfonic acid group-containing monomers such as styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; (N-substituted) amide monomers such as methylol (meth) acrylamide, N,N-dimethyl (meth) acrylamide, N-butyl (meth) acrylamide, N-methylol (meth) acrylamide, and N-methylol propane (meth) acrylamide; aminoalkyl (meth) acrylate monomers such as aminoethyl (meth) acrylate, N,N-dimethylaminoethyl (meth) acrylate, and t-butylaminoethyl (meth) acrylate; alkoxyalkyl (meth) acrylate monomers such as methoxyethyl (meth) acrylate and ethoxyethyl (meth) acrylate; maleimide monomers such as N-cyclohexyl maleimide, N-isopropyl maleimide, N-lauryl maleimide, and N-phenyl maleimide; itaconimide monomers such as N-methyl itaconimide, N-ethyl itaconimide, N-butyl itaconimide, N-octyl itaconimide, N-2-ethylhexyl itaconimide, N-cyclohexyl itaconimide, and N-lauryl itaconimide;succinimide-based monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyoctamethylene succinimide; vinyl-based monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinylcarboxylic acid amides, styrene, α-methylstyrene, and N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and (meth)acrylate. Examples of suitable monomers include glycol-based acrylic ester monomers such as methoxypolypropylene glycol acrylate; acrylic ester monomers having heterocycles, halogen atoms, silicon atoms, etc., such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, and silicone (meth)acrylate; polyfunctional monomers such as hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; olefin-based monomers such as isoprene, butadiene, and isobutylene; and vinyl ether-based monomers such as vinyl ether. These monomer components may be used alone or in combination of two or more.
[0064] In one embodiment, the content of structural units derived from organic acid monomers (e.g., (meth)acrylic acid group-containing monomers, carboxyl group-containing monomers) in the base polymer (e.g., acrylic polymer) is preferably 0.5 parts by weight or less, more preferably 0.3 parts by weight or less, per 100 parts by weight of the base polymer. Within this range, a cover film can be obtained that is less likely to destroy the gas adsorption layer of the gas adsorption sheet when peeled from the gas adsorption sheet. This effect is particularly pronounced when surface-treated (preferably coupling-treated) gas adsorption particles are used. In one embodiment, an acrylic polymer that does not contain structural units derived from organic acid monomers is used.
[0065] In one embodiment, the content of the nitrogen-containing monomer-derived structural unit in the base polymer (e.g., acrylic polymer) is preferably 20 parts by weight or less, and more preferably 15 parts by weight or less, per 100 parts by weight of the base polymer. Within this range, a cover film can be obtained that is less likely to destroy the gas adsorption layer of the gas adsorption sheet when the gas adsorption sheet is peeled off.
[0066] The pressure-sensitive adhesive may contain any suitable additives as needed, such as crosslinkers, tackifiers (e.g., rosin-based tackifiers, terpene-based tackifiers, hydrocarbon-based tackifiers, etc.), plasticizers (e.g., trimellitate ester-based plasticizers, pyromellitate ester-based plasticizers), pigments, dyes, antioxidants, conductive materials, antistatic agents, light stabilizers, release modifiers, softeners, surfactants, flame retardants, antioxidants, ultraviolet absorbers, particles, etc.
[0067] Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, and amine-based crosslinking agents. Among these, isocyanate-based crosslinking agents and epoxy-based crosslinking agents are preferred. In one embodiment, from the viewpoint of ultraviolet absorption, a crosslinking agent having an aromatic ring and / or a double bond (e.g., an aromatic isocyanate-based crosslinking agent) is used.
[0068] Specific examples of the isocyanate-based crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, trade name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, trade name "Coronate HX"). The content of the isocyanate-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the base polymer.
[0069] Examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500NP"), ethylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500NP"), and ethylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500NP"). Licor diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 40E"), propylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 70P"), polyethylene glycol diglycidyl ether (manufactured by NOF Corporation, trade name "Epiol E-400"), polypropylene glycol diglycidyl ether (manufactured by NOF Corporation, trade name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol") Examples of suitable crosslinking agents include glycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. The content of the epoxy crosslinking agent can be set at any appropriate amount depending on the desired adhesive strength, and is typically 0.01 to 10 parts by weight, and more preferably 0.03 to 5 parts by weight, per 100 parts by weight of the base polymer.
[0070] Examples of the tackifier include rosin-based resins (e.g., rosin ester resins), terpene-based resins (e.g., terpene-phenol copolymers (terpene-modified phenolic resins), hydrogenated terpene resins), coumarone-indene resins, alicyclic saturated hydrocarbon-based resins, petroleum-based resins (e.g., hydrocarbon-based petroleum resins such as aliphatic / aromatic copolymer petroleum resins and aromatic petroleum resins), and phenol-based resins. In one embodiment, from the viewpoint of ultraviolet absorption, a crosslinker having an aromatic ring and / or a double bond (e.g., rosin-based resin) is used. The content of the tackifier can be set to any appropriate amount depending on the desired adhesive strength, and is typically 1 to 50 parts by weight, more preferably 10 to 30 parts by weight, per 100 parts by weight of the base polymer.
[0071] D. Method for Manufacturing Gas Adsorption Sheet The gas adsorption sheet can be manufactured by any appropriate method. In one embodiment, the gas adsorption sheet is manufactured by coating (applying and drying) a gas adsorption layer-forming composition containing the binder resin and gas adsorption particles on a heat-resistant substrate. Forming a gas adsorption layer by coating can provide a gas adsorption sheet with excellent dispersibility of the gas adsorption particles and excellent gas adsorption performance. When the gas adsorption sheet includes an intermediate layer, the sheet can be manufactured by coating a heat-resistant substrate with a composition for forming an intermediate layer to form the intermediate layer, and then forming the gas adsorption layer.
[0072] The gas-adsorbing layer-forming composition may further contain any appropriate additives in addition to the binder resin and gas-adsorbing particles. Alternatively, the intermediate layer-forming composition may further contain any appropriate additives in addition to the resin. Examples of additives include crosslinkers, tackifiers, plasticizers (e.g., trimellitate ester-based plasticizers, pyromellitate ester-based plasticizers), pigments, dyes, fillers, antioxidants, conductive agents, UV absorbers, light stabilizers, release modifiers, softeners, surfactants, flame retardants, and antioxidants. Examples of crosslinkers include isocyanate-based crosslinkers, epoxy-based crosslinkers, melamine-based crosslinkers, and peroxide-based crosslinkers, as well as urea-based crosslinkers, metal alkoxide-based crosslinkers, metal chelate-based crosslinkers, metal salt-based crosslinkers, carbodiimide-based crosslinkers, oxazoline-based crosslinkers, aziridine-based crosslinkers, and amine-based crosslinkers. Among these, isocyanate-based crosslinkers and epoxy-based crosslinkers are preferred. The gas adsorbing layer-forming composition may also contain a solvent such as toluene or ethyl acetate.
[0073] Examples of methods for applying the gas adsorption layer-forming composition and intermediate layer-forming composition include coating methods such as air doctor coating, blade coating, knife coating, reverse coating, transfer roll coating, gravure roll coating, kiss coating, cast coating, spray coating, slot orifice coating, calendar coating, electrodeposition coating, dip coating, and die coating; and printing methods such as relief printing methods such as flexographic printing, intaglio printing methods such as direct gravure printing and offset gravure printing, lithographic printing methods such as offset printing, and stencil printing methods such as screen printing.
[0074] The gas adsorbent sheet with a cover film can be obtained by laminating the cover film on the gas adsorbing layer of the gas adsorbing sheet by any appropriate method. The cover film can be obtained by applying the pressure-sensitive adhesive to the substrate by any appropriate method.
[0075] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Evaluation methods in the examples are as follows. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0076] [Production Example 1] Production method of cover film A Monomers (2-ethylhexyl acrylate / ethyl acrylate / methyl methacrylate / hydroxyethyl acrylate = 30 parts by weight / 70 parts by weight / 5 parts by weight / 4 parts by weight), 0.2 parts by weight of benzoyl peroxide as an initiator, and 244 parts by weight of toluene were charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was maintained at around 60 ° C. to carry out a polymerization reaction for about 6 hours, thereby obtaining a resin composition A containing an acrylic copolymer A. To the obtained resin composition A containing 100 parts by weight of acrylic copolymer A, 3 parts by weight of an isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., trade name "Takenate D-101E") and ethyl acetate were added to prepare a pressure-sensitive adhesive A with a base of 15%. Pressure-sensitive adhesive A was applied to a 75 μm-thick substrate (polyester film, manufactured by Toray Industries, Inc., product name "Lumirror S10") so that the thickness of the pressure-sensitive adhesive layer after drying would be 10 μm, thereby obtaining a cover film A (substrate / pressure-sensitive adhesive layer A).
[0077] [Production Example 2] Method for producing cover films B to Q Cover films B to Q were obtained in the same manner as in Production Example 1, except that the base material shown in Table 1 was used, the monomers shown in Table 1 were used as the material monomers for the acrylic copolymer instead of <2-ethylhexyl acrylate / ethyl acrylate / methyl methacrylate / hydroxyethyl acrylate=30 parts by weight / 70 parts by weight / 5 parts by weight / 4 parts by weight>, the type and amount of crosslinking agent were as shown in Table 1, and the thickness of the pressure-sensitive adhesive layer was as shown in Table 1. Details of each component are as follows. (Monomers) 2EHA: 2-ethylhexyl acrylate EA: ethyl acrylate MMA: methyl methacrylate HEA: hydroxyethyl acrylate BA: butyl acrylate 4HBA: 4-hydroxybutyl acrylate AA: acrylic acid NVP: N-vinylpyrrolidone (Base material) Torefane BO: polypropylene film Lumirror S1N: polyester film (Crosslinking agent) Tetrad C: epoxy-based crosslinking agent, manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "Tetrad C"
[0078]
[0079] Example 1 A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with 100 parts by weight of gas-adsorbing particles (manufactured by Union Showa K.K., product name "Molecular Sieve 3AB Powder"), 4 parts by weight of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-4803"), 150 parts by weight of tetrahydrofuran, and 1.3 parts by weight of distilled water. Nitrogen gas was introduced while gently stirring, and a coupling reaction was carried out for approximately 6 hours while the liquid temperature in the flask was maintained at around 60°C, to obtain surface-treated gas-adsorbing particles (1). A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser was charged with 2-ethylhexyl acrylate / acrylic acid (95 parts by weight / 5 parts by weight), 0.2 parts by weight of an initiator (benzoyl peroxide), and 120 parts by weight of ethyl acetate. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was maintained at around 60°C, allowing a polymerization reaction to occur for approximately 6 hours, yielding a resin composition (1) containing an acrylic copolymer (1). 3 parts by weight of an isocyanate crosslinking agent (manufactured by Mitsui Chemicals, Inc., trade name "Takenate D-101E") and ethyl acetate were added to the resin composition (1) containing 100 parts by weight of the acrylic copolymer (1), to prepare an intermediate layer-forming composition (1) with a base of 18%. The obtained intermediate layer-forming composition (1) was applied to a heat-resistant substrate (polyimide film, manufactured by Toray DuPont Co., Ltd., trade name "Kapton 100H", thickness: 25 μm) to a thickness of 10 μm after drying, thereby obtaining a heat-resistant substrate (1) with an intermediate layer. 1 part by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "Tetrad C"), ethyl acetate, and 900 parts by weight of the gas adsorption particles (1) were added to a resin composition (1) containing 100 parts by weight of an acrylic copolymer (1) to prepare a 50% base gas adsorption layer-forming composition (1). The obtained gas adsorption layer-forming composition (1) was applied to a release-treated film (manufactured by Fujiko Co., Ltd., trade name "CA0", thickness: 75 μm) to a thickness of 80 μm after drying, thereby obtaining a gas adsorption layer (1). The obtained gas adsorption layer (1) was transferred to the intermediate layer of the intermediate layer-forming composition (1), thereby obtaining a gas adsorption sheet (1). The cover film A was laminated on the gas adsorption sheet (1) so that the gas adsorption layer (1) and the pressure-sensitive adhesive layer A faced each other, to obtain a gas adsorption sheet with a cover film.
[0080] Examples 2 to 19, Comparative Examples 1 to 3 Gas adsorbent sheets with cover films were obtained in the same manner as in Example 1, except that the type and amount of coupling agent used when preparing gas adsorbent particles were as shown in Table 2; the thickness of the intermediate layer was as shown in Table 2; the type and amount of crosslinking agent added to the gas adsorbing layer was as shown in Table 2; and a cover film as shown in Table 2 was used. In the comparative examples, pressure-sensitive adhesive sheets were obtained without laminating a cover film, and the pressure-sensitive adhesive sheets were subjected to the evaluations described below. Furthermore, in comparative example 1, a heat-resistant substrate (polyimide film, manufactured by Toray DuPont Co., Ltd., product name "Kapton 100H", thickness: 25 μm) was used instead of the heat-resistant substrate with an intermediate layer, and the gas adsorbing layer-forming composition was applied to the heat-resistant substrate to obtain a gas adsorbent sheet. Details of each component are as follows: (Coupling Agent) KBM903: manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM903" KBM3033: manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM3033" KBM13: manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM13" KBM403: manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM403"
[0081]
[0082] <Evaluation> The gas adsorption sheets with cover films obtained in the examples and comparative examples were subjected to the following evaluations. The results are shown in Table 2. (1) Cover film peel strength The gas adsorption sheet with cover film was dried at 110°C under a reduced pressure of -100 kPa for 3 hours, and then the cover film was peeled from the gas adsorption sheet with cover film, and the peel strength was measured. Test speed: 300 mm / min Peel angle: 180° Measurement temperature: 25°C
[0083] (2) Cover film peelability (peeling ability after drying) The failure mode in the above evaluation (1) was evaluated. ◯: Peeling was possible at the interface between the cover film and the gas adsorption layer. △: The surface layer of the gas adsorption layer was transferred to the cover film side. ×: The entire gas adsorption layer was transferred to the cover film side.
[0084] (3) Gas adsorption layer strength The gas adsorption sheet with cover film was dried at 110°C under reduced pressure of -100 kPa for 3 hours, and then the cover film was peeled off from the gas adsorption sheet with cover film. Nitto Denko No. 31B was attached to the exposed surface of the gas adsorption layer, and the peel strength was measured, which was taken as the gas adsorption layer strength. Bonding conditions: Bonded in a 25°C environment with a 2 kg roller going back and forth once. Test speed: 300 mm / min Peel angle: 180 degrees Measurement temperature: 25°C
[0085] (4) Adhesion of Gas Adsorption Layer The failure mode in the above evaluation (3) was evaluated. ◯: Cohesive failure mode of the gas adsorption layer ×: Anchor failure mode of the gas adsorption layer
[0086] (5) Heat Resistance of Cover Film The gas adsorption sheet with cover film was dried at 110°C under reduced pressure of -100 kPa for 3 hours, and then the state of the cover film was evaluated. ◯: No exposure of the gas adsorption layer due to lifting, peeling, or shrinkage. ×: Exposure of the gas adsorption layer due to lifting, peeling, or shrinkage occurred.
[0087] (6) Processability The gas adsorption sheet with cover film was punched using a Thomson blade (5 mm × 20 mm size, blade thickness 0.7 mm, R: 0.2), and the state of the gas adsorption sheet was evaluated. ◯: No chipping in the gas adsorption layer Δ: No chipping in the gas adsorption layer, but lifting or peeling of the cover film observed ×: Chip in the gas adsorption layer observed
[0088] (7) Moisture resistance A gas adsorption sheet with a cover film was dried for 3 hours at 110°C under reduced pressure of -100 kPa in a dry room with a dew point temperature of -50°C and a room temperature of 23°C, and then stored in the dry room, and the change in moisture content due to moisture absorption was measured. ◯: Moisture content maintained at 1% or less for 8 hours or more in the dry room. ×: Moisture content cannot be maintained at 1% or less for 8 hours in the dry room. - Moisture content measurement method (Karl Fischer method) - Moisture content measurement instrument: AQ-2100 manufactured by HIRANUMA Corporation
[0089] (8) Cover Film Adhesion The obtained cover film was attached to a SUS304BA plate, and the peel strength when peeled was measured, and this was defined as the cover film adhesion. Attachment conditions: 25°C environment, 1 round trip with a 2 kg roller. Test speed: 300 mm / min. Peel angle: 180°. Measurement temperature: 25°C.
[0090] (9) Handling Efficiency: Evaluate any problems that occur when winding the gas adsorption sheet with cover film onto a 3-inch core made of ABS resin. ◯: No problems ×: There is chipping in the gas adsorption layer during transportation, or the cover film is lifted after winding.
[0091] The gas adsorbent sheet of the present invention can be suitably used as a gas adsorbent for non-aqueous secondary batteries.
[0092] 10 Heat-resistant substrate 20 Gas adsorption layer 30 Intermediate layer 100 Gas adsorption sheet with cover film
Claims
1. A gas adsorption sheet for a secondary battery with a cover film, comprising: a heat-resistant substrate and a gas adsorption layer disposed on at least one side of the heat-resistant substrate; and a cover film disposed on the side of the gas adsorption layer opposite the heat-resistant substrate; the gas adsorption layer is made of a binder resin and an inorganic porous material having pores, and contains gas adsorption particles capable of adsorbing gas.
2. The gas adsorption sheet for a secondary battery with a cover film according to claim 1, further comprising an intermediate layer disposed between said heat-resistant substrate and said gas adsorption layer.
3. The gas adsorbing sheet for a secondary battery with a cover film according to claim 1, wherein the gas adsorbing particles have a surface treated with silicone.
4. The gas adsorbing sheet for a secondary battery with a cover film according to claim 3, wherein the silicone has an ethoxysilane group or a methoxysilane group.
5. The gas adsorption sheet for a secondary battery with a cover film according to claim 4, wherein the silicone is a silane coupling agent containing an epoxy group or an amino group.
6. The gas adsorption sheet for a secondary battery with a cover film according to claim 1, wherein the binder resin is an acrylic resin.
7. The gas adsorption sheet for a secondary battery with a cover film according to claim 6, wherein the binder resin contains a structural unit derived from an alkyl (meth)acrylate ester, and the alkyl (meth)acrylate ester has a linear or branched alkyl group having 4 to 12 carbon atoms.
8. The gas adsorption sheet for a secondary battery with a cover film according to claim 1, wherein the binder resin is butyl rubber, isoprene rubber, polyisobutylene rubber, ethylene propylene rubber or a silicone-based resin.
9. The gas adsorption sheet for a secondary battery with a cover film according to claim 1, wherein the content of said gas adsorption particles is 10 to 90 parts by weight per 100 parts by weight of the gas adsorption sheet for a secondary battery.
10. The gas adsorption sheet for a secondary battery with a cover film according to claim 1, wherein the material constituting the heat-resistant substrate is polyamideimide, polyetherimide, polyphenylene sulfide, polyethylene naphthalate, polyimide or polyether ether ketone.
11. The gas adsorbing sheet for a secondary battery with a cover film according to claim 1, wherein the cover film comprises a substrate and an adhesive layer disposed on at least one side of the substrate.
12. The gas adsorption sheet for a secondary battery with a cover film according to claim 11, wherein the adhesive layer is formed from an adhesive containing a base polymer, and the content of structural units derived from an organic acid monomer is preferably 0.5 parts by weight or less per 100 parts by weight of the base polymer.
13. The gas adsorbing sheet for a secondary battery with a cover film according to claim 11, wherein the cover film is peelable.
Citation Information
Patent Citations
Material capable of absorbing carbon monoxide and carbon dioxide, power storage device arranged by use thereof, and method for producing material capable of absorbing carbon monoxide and carbon dioxide
JP2015162457A
Non-aqueous electrolyte cell
JP2001155790A
Sheet for formalin absorption
JP2009156791A
Adhesive tape for electrochemical devices
JP2012226992A
Outer case, laminate film for outer case, and battery module
JP2015179618A