Electrode material and method for producing electrode material

By employing Raney nickel from a specific NiAl alloy composition with controlled iron and cobalt proportions, the method enhances catalyst activity and suppresses ion elution, addressing performance issues in water electrolysis devices and improving electrode efficiency and stability.

WO2024219019A1PCT designated stage expired Publication Date: 2024-10-24TOYOTA INDUSTRIES CORP +1

Patent Information

Application Number
PCT/JP2023/046182
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2023-12-22
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Current water electrolysis devices face challenges in catalyst activity and efficiency due to the elution of iron and cobalt ions, which lead to increased resistance and internal short circuits, affecting the performance of the anode and cathode in water electrolysis devices.

Method used

The use of Raney nickel obtained from a specific NiAl alloy composition, with controlled proportions of iron and cobalt, through an alkali treatment and optional oxidation process, to enhance catalytic activity and suppress ion elution, thereby improving the stability and efficiency of the electrode material.

Benefits of technology

The method results in high catalytic activity for oxygen and hydrogen generation, with reduced risk of internal short circuits and increased resistance, leading to improved performance and longevity of the water electrolysis device electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023046182_24102024_PF_FP_ABST
    Figure JP2023046182_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This method for producing an electrode material used for an electrode of a water electrolysis device involves an alkali treatment step for treating a specific NiAl alloy with an alkaline material to elute aluminum from the specific NiAl alloy, thereby obtaining Raney nickel. The specific NiAl alloy is an alloy represented by the composition formula Al3Ni(n-(x+y))FexCoy (n is 1 or 2, and x and y are values satisfying 0 < n - (x + y) < 2, 0.005 ≤ x ≤ 0.8, and 0 ≤ y ≤ 0.8).
Need to check novelty before this filing date? Find Prior Art

Description

Electrode material and method for manufacturing electrode material

[0001] The present disclosure relates to an electrode material used in electrodes of a water electrolysis device, and a method for manufacturing the electrode material.

[0002] Water electrolysis is the electrolysis of water into hydrogen and oxygen, and is used, for example, as a technology for producing hydrogen. A water electrolysis device for generating hydrogen includes, for example, an electrolytic cell containing an electrolyte solution such as alkaline water, and an anode and a cathode disposed in the electrolytic cell with a separator sandwiched therebetween. In the water electrolysis device, oxygen is generated at the anode and hydrogen is generated at the cathode by passing a current between the anode and the cathode.

[0003] Patent Document 1 discloses a technology using Raney nickel as a catalyst for the anode of the water electrolysis device. Raney nickel is nickel that remains after dissolving and removing only aluminum from a NiAl alloy containing nickel and aluminum by alkali treatment. Raney nickel is a porous material with a large specific surface area in which numerous pores are formed by the dissolution of aluminum.

[0004] Special Publication No. 01-028837

[0005] As a result of extensive research, the present inventors have found that Raney nickel obtained from a NiAl alloy of a specific composition exhibits high activity as a catalyst for use in electrodes of a water electrolysis device.

[0006] In one aspect of the present disclosure, there is provided a method for producing an electrode material for use in electrodes of a water electrolysis device. The method includes an alkali treatment step of treating a NiAl alloy with an alkaline substance to dissolve aluminum from the NiAl alloy, thereby obtaining Raney nickel. The NiAl alloy has the composition formula Al 3 Ni (n-(x+y)) Fe x Co y (n is 1 or 2, and x and y are values ​​that satisfy the conditions 0<n-(x+y)<2, 0.005≦x≦0.8, and 0≦y≦0.8).

[0007] Another aspect of the present disclosure provides an electrode material for use in an electrode of a water electrolysis device, comprising Raney nickel having a molar ratio of nickel, iron, and cobalt (nickel:iron:cobalt) of (n-(x+y)):x:y (n is 1 or 2, and x and y are values ​​satisfying 0<n-(x+y)<2, 0.005≦x≦0.8, and 0≦y≦0.8).

[0008] In yet another aspect of the present disclosure, there is provided an electrode material for use in an electrode of a water electrolysis device. The electrode material has the composition formula Al 3 Ni (n-(x+y)) Fe x Co y (n is 1 or 2, and x and y are values ​​that satisfy 0<n-(x+y)<2, 0.005≦x≦0.8, 0≦y≦0.8)

[0009] Fig. 1 is a graph showing the evaluation results of catalytic activity in Test 1. Fig. 2 is a graph showing the evaluation results of catalytic activity in Test 2.

[0010] Hereinafter, one embodiment of the method for producing an electrode material according to the present disclosure will be described. In this specification, "A to B" used as a numerical range means "A or more and B or less." The electrode material produced by the production method according to this embodiment is a catalyst used in the electrodes of a water electrolysis device. The electrode material can be used in either the oxygen generating electrode, which is the anode, or the hydrogen generating electrode, which is the cathode of the water electrolysis device. It is particularly preferable to use the electrode material in the oxygen generating electrode, which is the anode.

[0011] The method for producing an electrode material according to this embodiment includes an alkali treatment step for obtaining Raney nickel from a NiAl alloy and an oxidation step for oxidizing the surface of the Raney nickel obtained in the alkali treatment step. The oxidation step can be omitted as necessary. Hereinafter, the Raney nickel obtained in the alkali treatment step before the oxidation step may be referred to as "first Raney nickel." The Raney nickel after the oxidation step may be referred to as "second Raney nickel."

[0012] <Alkali Treatment Step> The alkali treatment step is a step of treating a NiAl alloy of a specific composition (hereinafter referred to as specific NiAl alloy) with an alkaline substance to dissolve aluminum from the NiAl alloy, thereby obtaining first Raney nickel.

[0013] (Specific NiAl alloy) The specific NiAl alloy to be subjected to the alkali treatment step has the composition formula Al 3 Ni (n-(x+y)) Fe x Co y In the above formula, n is 1 or 2, and x and y are values ​​that satisfy the following: 0<n-(x+y)<2, 0.005≦x≦0.8, 0≦y≦0.8. 3 Ni (n-(x+y)) Fe x Co y The specific NiAl alloy represented by the formula (1) means an alloy of aluminum, nickel, and iron, or an alloy of aluminum, nickel, iron, and cobalt, in which the molar ratio of aluminum, nickel, iron, and cobalt in the entire alloy (aluminum:nickel:iron:cobalt) is 3:(n-(x+y)):x:y. Therefore, the specific NiAl alloy is an alloy of Al 3 Ni (n-(x+y)) Fe x Co y The alloy may be an alloy composed of a single phase, or an alloy composed of multiple phases, for example, an alloy including a main phase and a subphase.

[0014] In this specification, the term "main phase of a specific NiAl alloy" refers to one or two specific phases that occupy the majority of the specific NiAl alloy, and can be defined as a phase that satisfies at least one of the following volume and area conditions:

[0015] Volume condition: The volume ratio of a specific phase to the entire alloy, or the sum of the volume ratios of the two phases with the largest volume ratios to the entire alloy, exceeds 50%. Note that the above value regarding the volume condition may be 60% or more, 70% or more, 80% or more, or 90% or more. The volume of each phase constituting the alloy can be calculated, for example, by Rietveld analysis of X-ray diffraction (XRD) measurement data of the alloy.

[0016] Area condition: The area ratio of a specific phase in any cross section formed by cutting the alloy, or the sum of the area ratios of the two phases with the largest area ratios in the cross section, exceeds 50%. Note that the above numerical value regarding the area condition may be 60% or more, 70% or more, 80% or more, or 90% or more. The area of ​​each phase in the cross section of the alloy can be calculated, for example, by image analysis of elemental mapping data of the alloy cross section obtained by scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX).

[0017] [First NiAl Alloy] An example of the specific NiAl alloy is a first NiAl alloy having the composition formula Al 3 Ni (2-x) Fe x In the above formula representing the first NiAl alloy, x is, for example, a value that satisfies 0.01≦x≦0.8, preferably a value that satisfies 0.03≦x≦0.7, more preferably a value that satisfies 0.05≦x≦0.6, and even more preferably a value that satisfies 0.1≦x≦0.4.

[0018] The single phase, the main phase, and the subphase constituting the first NiAl alloy include, for example, Al 3 Ni (2-x) Fe x phase, Al 3 Ni 2 phase, AlNi phase, Al 3 The first NiAl alloy may include a subphase that is inevitably formed during manufacturing. 3 Ni 2 phase and has a molar ratio (aluminum:nickel:iron) of 3:(2-x):x.

[0019] [Second NiAl Alloy] An example of the specific NiAl alloy is a NiAl alloy having the composition formula Al 3 Ni (1-x) Fe x In the above formula representing the second NiAl alloy, x is, for example, a value that satisfies 0.005≦x≦0.7, preferably a value that satisfies 0.05≦x≦0.3, and more preferably a value that satisfies 0.05≦x≦0.1.

[0020] The single phase, the main phase, and the subphase constituting the second NiAl alloy include, for example, Al 3 Ni (1-x) Fe x phase, Al 4 Ni 3 phase, Al 3 Ni phase, AlNi phase, Al 3 Fe phase, Al 5 FeNi phase, AlNiFe 2 The second NiAl alloy may include a subphase, which is a phase inevitably formed during manufacturing. The second NiAl alloy may include, for example, a NiAl alloy having a main phase of Al. 3 Ni 1 phase and has a molar ratio (aluminum:nickel:iron) of 3:(1-x):x.

[0021] [Third NiAl Alloy] An example of the specific NiAl alloy is a third NiAl alloy having the composition formula Al 3 Ni (2-(x+y)) Fe x Co y The alloy is represented by the formula (hereinafter referred to as the third NiAl alloy).

[0022] In the above formula representing the third NiAl alloy, x and y are, for example, values ​​that satisfy 0<2-(x+y)<2, 0.01≦x≦0.8, and 0<y≦0.8. In the above formula, x is preferably a value that satisfies 0.03≦x≦0.7, more preferably a value that satisfies 0.05≦x≦0.6, and even more preferably a value that satisfies 0.1≦x≦0.4. In the above formula, y is preferably a value that satisfies 0.1<y<0.8, more preferably a value that satisfies 0.2≦y≦0.7, and even more preferably a value that satisfies 0.2≦y≦0.6. The ratio of cobalt to nickel (y / (2-(x+y))) is, for example, 0.05 to 1.0, preferably 0.3 to 0.8. The ratio of cobalt to iron (y / x) is, for example, 0.25 to 12.0, and preferably 1.0 to 6.0.

[0023] The single phase, the main phase, and the subphase constituting the third NiAl alloy include, for example, Al 3 Ni (2-(x+y)) Fe x Co y phase, Al 3 Ni 2 phase, AlNi phase, Al 3 The third NiAl alloy may include, as a subphase, a phase inevitably formed during manufacturing. For example, the third NiAl alloy may include a subphase in which the main phase is Al. 3 Ni 2 phase and Al 4 Ni 3 phase and the molar ratio (aluminum:nickel:iron:cobalt) is 3:(2−(x+y)):x:y.

[0024] [Fourth NiAl Alloy] An example of the specific NiAl alloy is a fourth NiAl alloy having the composition formula Al 3 Ni (1-(x+y)) Fe x Co y The alloy is represented by the formula (hereinafter referred to as the fourth NiAl alloy).

[0025] In the above formula representing the fourth NiAl alloy, x and y are, for example, values ​​that satisfy 0<1-(x+y)<1, 0.005≦x≦0.3, and 0<y≦0.7. In the above formula, x is preferably a value that satisfies 0.05≦x≦0.3, and preferably a value that satisfies 0.05≦x≦0.1. In the above formula, y is preferably a value that satisfies 0.1≦y≦0.6, and more preferably a value that satisfies 0.2≦y≦0.6. The ratio of cobalt to nickel (y / (1-(x+y))) is, for example, 0.1 to 3, and preferably 0.25 to 3.0. The ratio of cobalt to iron (y / x) is, for example, 0.3 to 12.0.

[0026] The single phase, main phase, and subphase constituting the fourth NiAl alloy include, for example, Al 3 Ni (1-(x+y)) Fe x Co y phase, Al 4 Ni 3 phase, Al 3 Ni phase, AlNi phase, Al 3 Fe phase, Al 5 FeNi phase, AlNiFe 2 The fourth NiAl alloy may include a subphase that is inevitably formed during manufacturing. 3 Ni 1 phase and the molar ratio (aluminum:nickel:iron:cobalt) is 3:(1-(x+y)):x:y.

[0027] Here, Raney nickel used as an electrode material for a water electrolysis device exhibits catalytic activity by generating a complex (acid) hydroxide during operation. The complex (acid) hydroxide refers to a complex of at least two of Ni(O)OH, Fe(O)OH, Al(O)OH, and Co(O)OH, for example.

[0028] The Raney nickel obtained from the specific NiAl alloy having an iron content equal to or greater than the lower limit of each of the above ranges can produce a large amount of highly active Fe(O)OH during operation of the water electrolysis system, and is likely to form a core-shell structure containing a relatively large amount of Fe(O)OH on the surface side. Therefore, by setting the iron content equal to or greater than the lower limit of each of the above ranges, a highly active Raney nickel can be obtained.

[0029] The Raney nickel obtained from the specific NiAl alloy in which the iron content is set to be equal to or less than the upper limit of each of the above ranges can suppress the elution of iron ions into the electrolyte during operation of the water electrolysis device. Therefore, it is possible to suppress an increase in resistance caused by clogging of the separator by the eluted iron ions. Furthermore, the eluted iron ions react with the generated oxygen gas on the anode side to form iron oxides (e.g., Fe 2 O 3 ) on the anode surface. This iron oxide has a lower oxygen generation activity than the anode, so the deposition of iron oxide on the anode surface causes a decrease in the activity of the anode. In addition, the dissolved iron ions are converted into electron-conductive iron oxide (e.g., Fe 3 O 4 ) precipitates as dendrites on the cathode surface, which can cause internal short circuits. Therefore, by suppressing the elution of iron ions, it is possible to suppress the decrease in activity on the anode side and the occurrence of internal short circuits.

[0030] The Raney nickel obtained from the specific NiAl alloy having a cobalt content equal to or greater than the lower limit of each of the above ranges can produce a more highly active composite (acid) hydroxide during operation of the water electrolysis device, and is also likely to form a structure having many interfaces between NiOOH and CoOOH. Therefore, by setting the cobalt content equal to or greater than the lower limit of each of the above ranges, a highly active Raney nickel can be obtained.

[0031] Raney nickel obtained from a specific NiAl alloy having a cobalt content equal to or less than the upper limit of each of the above ranges can suppress the elution of cobalt ions into the electrolyte during operation of the water electrolysis device. Therefore, it is possible to suppress an increase in resistance caused by clogging of the separator by the eluted cobalt ions. Furthermore, the eluted cobalt ions may precipitate as metallic cobalt on the cathode surface in the form of dendrites, which may cause an internal short circuit. Therefore, suppressing the elution of cobalt ions can suppress an internal short circuit.

[0032] Furthermore, when the proportion of aluminum in the specific NiAl alloy is high, the first Raney nickel obtained by eluting the aluminum has a relatively high porosity, i.e., a high specific surface area. Therefore, from the viewpoint of obtaining a Raney nickel exhibiting higher activity, it is preferable to use a specific NiAl alloy in which n is 1. On the other hand, when the proportion of aluminum in the specific NiAl alloy is low, the first Raney nickel obtained by eluting the aluminum has a relatively low porosity. Therefore, from the viewpoint of obtaining a Raney nickel with high strength, it is preferable to use a specific NiAl alloy in which n is 2.

[0033] The method for producing the specific NiAl alloy is not particularly limited, and any known alloy production method can be applied, such as casting, quenching, mechanical alloying, and sputtering.

[0034] The specific NiAl alloy subjected to the alkali treatment step is, for example, in the form of powder. The average particle size of the specific NiAl alloy is, for example, 1 to 150 μm. The average particle size described in this specification means the particle size at an integrated value of 50% in the particle size distribution determined by a laser diffraction / scattering method.

[0035] (Treatment Conditions) The alkali treatment step is carried out by reacting the specific NiAl alloy with an alkaline aqueous solution containing an alkaline substance. The reaction with the alkaline aqueous solution causes aluminum in the specific NiAl alloy to dissolve, thereby obtaining a first Raney nickel, which is a porous body with a large specific surface area. Specific treatment methods include, for example, gradually adding the powdered specific NiAl alloy to the alkaline aqueous solution, and then stirring the alkaline aqueous solution at a predetermined temperature for a predetermined time. Alternatively, a treatment method may be employed in which the specific NiAl alloy, which has been supported on a predetermined substrate by thermal spraying or the like, is reacted with the alkaline aqueous solution.

[0036] The alkaline substance is, for example, an alkali metal hydroxide or an alkali metal salt. Examples of the alkali metal hydroxide include sodium hydroxide, potassium hydroxide, and lithium hydroxide. Examples of the alkali metal salt include sodium carbonate, potassium carbonate, and lithium carbonate. It is preferable that the alkaline substance is an alkali metal hydroxide.

[0037] The treatment temperature in the alkali treatment step is, for example, 100 to 140°C. The treatment time in the alkali treatment step is, for example, 60 to 360 minutes. The amount of alkaline substance used in the alkali treatment step can be appropriately set depending on the amount of aluminum contained in the specific NiAl alloy. The amount of the alkaline substance may be any amount that is less than, equal to, or in excess of the stoichiometric amount of aluminum contained in the specific NiAl alloy. Furthermore, the solid-liquid ratio of the specific NiAl alloy to the alkaline aqueous solution (specific NiAl alloy:alkaline aqueous solution) in the alkali treatment step is, for example, 1:10 to 1:500 by mass.

[0038] A preferred example of treatment conditions for the alkali treatment step is treatment at high temperature using an alkaline aqueous solution of a high concentration of alkali metal hydroxide. The concentration of the alkaline aqueous solution under these treatment conditions is, for example, 3 M or more, preferably 7 M or more, and more preferably 14 M or more. The concentration of the alkaline aqueous solution under these treatment conditions is 20 M or less. The treatment temperature under these treatment conditions is, for example, 100°C or more, preferably 110°C or more, and more preferably 140°C or more. The treatment temperature under these treatment conditions is, for example, 148°C or less. Note that, in order to increase the treatment temperature, it is necessary to increase the concentration of the alkaline aqueous solution so that the boiling point of the alkaline aqueous solution is equal to or higher than the treatment temperature. For example, when the treatment temperature is 100°C or higher, the concentration of the alkaline aqueous solution is preferably 3 M or more, and when the treatment temperature is 140°C or higher, the concentration of the alkaline aqueous solution is preferably 14 M or more. The alkali treatment step is preferably performed at atmospheric pressure. In this case, hydrogen generated during treatment can be more easily removed compared to when pressurized. In particular, it is possible to prevent the device for removing hydrogen generated during processing from becoming complicated.

[0039] In this case, a first Raney nickel exhibiting high activity can be obtained. In particular, the high treatment temperature allows iron atoms to migrate to the surface of the particles in the alkaline treatment step, making it easier to obtain a first Raney nickel having a core-shell structure with a relatively high iron content on the surface side. Furthermore, the reaction time between the alkaline aqueous solution and the specific NiAl alloy can be shortened. Under these treatment conditions, the reaction time between the alkaline aqueous solution and the specific NiAl alloy is, for example, 3 hours to 6 hours when the concentration of the alkaline aqueous solution is 3 M or more and the treatment temperature is 100°C or higher, and is, for example, 1 hour to 6 hours when the concentration of the alkaline aqueous solution is 14 M or more and the treatment temperature is 140°C or higher.

[0040] The treatment conditions for the alkali treatment step may be conditions that allow all of the aluminum contained in the specific NiAl alloy to be eluted, or may be conditions that allow a portion of the aluminum to remain without being eluted.

[0041] The first Raney nickel obtained by the above treatment can be recovered by performing a filtration treatment. At that time, a washing treatment may be performed as necessary. As the filtration treatment, a known solid-liquid separation treatment used in the production of Raney nickel can be applied. As the washing treatment, a known washing treatment used in the production of Raney nickel, for example, a water washing treatment, can be applied.

[0042] <Oxidation Step> The first Raney nickel obtained by the alkali treatment step has a high surface activity and may spontaneously combust in air. Therefore, it is difficult to handle during storage, etc., and it is necessary to handle it by storing it in a solvent or the like to avoid contact with air.

[0043] The oxidation step is a step of oxidizing the surface of the first Raney nickel obtained in the alkali treatment step. The second Raney nickel, which is the first Raney nickel with an oxidized surface, is suppressed from spontaneous combustion in air. Therefore, the second Raney nickel is easier to handle during storage, etc., than the first Raney nickel.

[0044] An example of the oxidation step is carried out by reacting the first Raney nickel with an acidic aqueous solution containing an acidic substance. A specific treatment method includes, for example, adding powdered first Raney nickel little by little to the acidic aqueous solution, and then stirring the mixture at a predetermined temperature for a predetermined time.

[0045] Examples of the acidic substance include hydrogen peroxide, sodium peroxide, sodium percarbonate, and sodium perborate. Among these, the acidic substance is preferably hydrogen peroxide.

[0046] The concentration of the acidic aqueous solution, and the treatment temperature and treatment time in the oxidation step can be set appropriately. The concentration of the acidic aqueous solution is, for example, 0.7 to 10 M. The treatment temperature in the oxidation step is, for example, 15 to 80°C. The treatment time in the oxidation step is, for example, 5 to 720 minutes. The solid-liquid ratio of the first Raney nickel to the acidic aqueous solution in the oxidation step (first Raney nickel:acidic aqueous solution) is, for example, 1:9 to 1:100 in mass ratio.

[0047] The second Raney nickel obtained by the above treatment can be recovered by performing a filtration treatment. At that time, a washing treatment may be performed as necessary. As the filtration treatment, a known solid-liquid separation treatment used in the production of Raney nickel can be applied. As the washing treatment, a known washing treatment used in the production of Raney nickel, for example, a water washing treatment, can be applied.

[0048] <Raney Nickel> The first Raney nickel and second Raney nickel (hereinafter sometimes referred to as the Raney nickel of this embodiment) produced by the above-described production method contain nickel and iron in a specific ratio, or contain nickel, iron, and cobalt in a specific ratio. The ratios of nickel, iron, and cobalt in the Raney nickel of this embodiment are equal to the ratios of nickel, iron, and cobalt in the specific NiAl alloy used in the production. Therefore, the molar ratio of nickel, iron, and cobalt in the Raney nickel of this embodiment is (n-(x+y)):x:y. In the above molar ratio, n is 1 or 2, and x and y are values ​​that satisfy 0<n-(x+y)<2, 0.005≦x≦0.8, and 0≦y≦0.8.

[0049] The Raney nickel of this embodiment may contain aluminum. In this case, the mass percentage of aluminum contained in the Raney nickel of this embodiment is, for example, 22 mass% or less, preferably 11 mass% or less. The mass percentage of aluminum is, for example, 0.6 mass% or more, preferably 1 mass% or more.

[0050] The Raney nickel of this embodiment is Ni (n-(x+y)) Fe x Co yThe alloy may be an alloy composed of a single phase consisting of a phase, or may be an alloy composed of multiple phases, for example, an alloy containing a main phase and a subphase. For example, the Raney nickel of this embodiment obtained from a specific NiAl alloy containing a main phase and a subphase may have a phase derived from the main phase of the specific NiAl alloy and a phase derived from the subphase of the specific NiAl alloy. The phase derived from the main phase of the specific NiAl alloy is, for example, a phase in which part or all of the aluminum has been removed from the main phase of the specific NiAl alloy. The phase derived from the subphase of the specific NiAl alloy is, for example, a phase in which part or all of the aluminum has been removed from the subphase of the specific NiAl alloy.

[0051] The Raney nickel of this embodiment obtained from the first NiAl alloy may be, for example, Ni (2-x) Fe x Single-phase alloys consisting of Al phases and Al alloys in which the main phase is Al 3 Ni 2 phase and Al 4 Ni 3 An example of such an alloy is an alloy having a Ni phase derived from the Ni phase and a molar ratio (nickel:iron) of (2−x):x.

[0052] The Raney nickel of this embodiment obtained from the second NiAl alloy may be, for example, Ni (1-x) Fe x Single-phase alloys consisting of Al phases and Al alloys in which the main phase is Al 3 Ni 1 An example of such an alloy is an alloy having a Ni phase derived from the Ni phase and a molar ratio (nickel:iron) of (1-x):x.

[0053] The Raney nickel of this embodiment obtained from the third NiAl alloy may be, for example, Ni (2-(x+y)) Fe x Co y Single-phase alloys consisting of Al phases and Al alloys in which the main phase is Al 3 Ni 2 phase and Al 4 Ni 3 and an alloy having a molar ratio (nickel:iron:cobalt) of (2−(x+y)):x:y.

[0054] The Raney nickel of this embodiment obtained from the fourth NiAl alloy may be, for example, Ni (1-(x+y)) Fex Co y Single-phase alloys consisting of Al phases and Al alloys in which the main phase is Al 3 Ni 1 and an alloy having a molar ratio (nickel:iron:cobalt) of (1−(x+y)):x:y.

[0055] The BET specific surface area of ​​the Raney nickel of this embodiment is, for example, 5 to 100 m 2 / g. The BET specific surface area is the N 2 It means the surface area per unit mass of Raney nickel measured by adsorption.

[0056] The average particle size of the Raney nickel of this embodiment is, for example, 0.1 to 100 μm. <Function> Next, the function of this embodiment will be described.

[0057] According to the production method of this embodiment, Raney nickel containing iron in a specific ratio or Raney nickel containing iron and cobalt in specific ratios can be obtained. When the Raney nickel of this embodiment is used as an electrode material for a water electrolysis device, i.e., as an electrode catalyst, it exhibits high catalytic activity due to the generation of a highly active complex (acid) hydroxide during operation.

[0058] In particular, the Raney nickel of this embodiment exhibits high activity when used as an anode material for a water electrolysis device, i.e., as a catalyst for an oxygen generation reaction. Specifically, when used as a catalyst for an oxygen generation reaction, the Raney nickel of this embodiment has a Tafel gradient of, for example, 50 to 226 mV / dec. The Tafel gradient can be determined from a Tafel plot in which the horizontal axis represents the logarithm of the oxygen generating current and the vertical axis represents the overpotential, which is the value obtained by subtracting the theoretical decomposition potential of the oxygen generation reaction from the working electrode potential. The Tafel gradient obtained from the Tafel plot in which the horizontal axis represents the logarithm of the oxygen generating current is the voltage required to increase the oxygen generating current by 10 times, and a smaller absolute value indicates higher catalytic activity for oxygen generation.

[0059] In detail, the composition formula Al 3 Ni (2-x) Fe xThe Raney nickel of this embodiment obtained from the specific NiAl alloy represented by the formula Al has a Tafel gradient of, for example, 121 to 226 mV / dec. 3 Ni (1-x) Fe x The Raney nickel of this embodiment obtained from the second specific NiAl alloy represented by the formula Al has a Tafel gradient of, for example, 75 to 120 mV / dec. 3 Ni (2-(x+y)) Fe x Co y The Raney nickel of this embodiment obtained from the third specific NiAl alloy represented by the formula Al has a Tafel gradient of, for example, 86 to 126 mV / dec. 3 Ni (1-(x+y)) Fe x Co y The Raney nickel of this embodiment obtained from the fourth specific NiAl alloy represented by the formula (I) has a Tafel gradient of, for example, 50 to 91 mV / dec. The Tafel gradient can be measured by the measurement method described in the examples.

[0060] <Effects> Next, the effects of this embodiment will be described. (1) The method for producing an electrode material used in the electrodes of a water electrolysis device includes an alkali treatment step in which a specific NiAl alloy is treated with an alkaline substance to dissolve aluminum from the specific NiAl alloy, thereby obtaining Raney nickel. The specific NiAl alloy has the composition formula Al 3 Ni (n-(x+y)) Fe x Co y (n is 1 or 2, and x and y are values ​​that satisfy the conditions 0<n-(x+y)<2, 0.005≦x≦0.8, and 0≦y≦0.8).

[0061] According to the above-mentioned configuration, it is possible to produce Raney nickel that exhibits high catalytic activity when used as an electrode material for a water electrolysis device. The produced Raney nickel exhibits high oxygen generation activity when used as an anode material for a water electrolysis device, and exhibits high hydrogen generation activity when used as a cathode material.

[0062] (2) The alkali treatment step includes a process of reacting an alkaline aqueous solution, which is an aqueous solution of an alkaline substance, with the specific NiAl alloy at a temperature of 100°C or higher. The alkaline substance is an alkali metal hydroxide. The concentration of the alkaline aqueous solution is 3M or higher. According to the above configuration, iron atoms migrate to the surface of the particles in the alkali treatment step, making it easier to obtain Raney nickel with a core-shell structure that contains a relatively large amount of iron on the surface side. In addition, the reaction time between the alkaline aqueous solution and the specific NiAl alloy can be shortened.

[0063] (3) The alkaline treatment step includes reacting an alkaline aqueous solution, which is an aqueous solution of an alkaline substance, with the specific NiAl alloy at a temperature of 140°C or higher. The alkaline substance is an alkali metal hydroxide. The concentration of the alkaline aqueous solution is 14M or higher. This configuration further improves the effect of (2) above.

[0064] (4) A method for producing an electrode material for use in electrodes of a water electrolysis device includes an oxidation step of oxidizing the surface of Raney nickel obtained by the alkali treatment step. This method can suppress spontaneous combustion of the obtained Raney nickel in air. This allows for the production of Raney nickel that is easy to handle during storage, etc.

[0065] Examples that further embody the above-described embodiment will be described below. <Test 1> In Test 1, the catalytic activity of Raney nickel obtained from the first NiAl alloy containing iron was evaluated.

[0066] (Preparation of Raney Nickel) A mixture of predetermined amounts of aluminum, nickel, and iron is heated and melted at 1600°C using a high-frequency melting furnace, and then cooled to obtain a Raney Nickel alloy whose main phase is Al. 3 Ni 2 phase, and has the composition formula Al 3 Ni (2-x) Fe xThe alloy ingots were prepared by varying the x in the above formula to 0, 0.05, 0.1, 0.2, 0.4, or 0.7. The obtained alloy ingots were pulverized to obtain NiAl alloy powders of the above composition. The average particle size of the obtained powders was measured by a laser diffraction / scattering method and found to be in the range of 40 to 60 μm.

[0067] Next, the obtained NiAl alloy powder (2 g) was immersed in a 14 M aqueous sodium hydroxide solution (30 g) and subjected to an alkali treatment for 3 hours at 140° C. Thereafter, a filtration treatment and a cleaning treatment with water were performed, thereby obtaining first Raney nickel in which aluminum was eluted from the NiAl alloy.

[0068] The obtained first Raney nickel powder (1.5 g) was immersed in a 5 mass % aqueous hydrogen peroxide solution (14 g) and subjected to oxidation treatment at 20° C. for 10 hours. Thereafter, filtration treatment and washing treatment with water were performed to obtain second Raney nickel powder with an oxidized surface.

[0069] (Evaluation of catalytic activity) The oxygen generating activity of the obtained second Raney nickel was evaluated using a three-electrode electrochemical measurement device.

[0070] A slurry was prepared by dispersing 2D Raney nickel powder, Ketjen black, and a 20% Nafion® dispersion (DE2020CS type: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) in a mixed solvent of water and ethanol. The prepared slurry was applied to a glassy carbon substrate to obtain an electrode body. The amount of 2D Raney nickel supported in the electrode body was 0.05 mg / cm. 2 It was decided.

[0071] A 7 mol / L aqueous potassium hydroxide solution was used as the electrolyte, and a platinum coil serving as the counter electrode and the fabricated working electrode were immersed in the electrolyte. A mercury-mercury oxide electrode was used as the reference electrode, and connected to the electrolyte via a liquid junction. The potential of the working electrode relative to the reference electrode was swept at 10 mV / s, and the oxygen evolution current versus electrode potential was measured at room temperature.

[0072] Next, a Tafel plot was created with the logarithm of the measured oxygen generating current (A) on the horizontal axis and the overvoltage (V), which is the value obtained by subtracting the theoretical decomposition potential of the oxygen generating reaction from the working electrode potential, on the vertical axis, and the Tafel gradient (mV / dec.) was determined from the created Tafel plot. The overvoltage was calculated assuming the theoretical decomposition voltage of the oxygen generating reaction to be 1.23 V. The results are shown in the graph in Figure 1. As described above, the Tafel gradient, obtained by plotting the logarithm of the oxygen generating current on the horizontal axis, is the amount of change in potential required to increase the oxygen generating current by 10 times. A smaller absolute value of the Tafel gradient indicates higher catalytic activity for oxygen generation.

[0073] Table 1 below is a table summarizing the Fe ratio and Tafel slope values ​​at each point in the graph shown in FIG. 1. The relative evaluation column of oxygen generating activity in Table 1 also shows the evaluation of the oxygen generating activity for each example with different Fe ratios. This evaluation is a relative evaluation with the Tafel slope value when the Fe ratio is "0" as the reference value. The evaluation criteria are as follows:

[0074] "=": The Tafel slope value is 98% or more and 102% or less of the above reference value, and the oxygen generating activity is equivalent to that when the Fe ratio is "0." "○": The Tafel slope value is 85% or more and less than 98% of the above reference value, and the oxygen generating activity is higher than that when the Fe ratio is "0."

[0075] "Excellent": The Tafel gradient value is less than 85% of the above reference value, and the oxygen generating activity is significantly higher than when the Fe ratio is "0".

[0076]

[0077] As shown in FIG. 1 and Table 1, the Tafel gradient is 3 Ni (2-x) Fe xAs the iron ratio x (Fe ratio) in the NiAl alloy increases, the curve becomes convex downward. From this result, it can be seen that Raney nickel obtained from NiAl alloys containing iron in the range of iron ratio x of 0.8 or less has higher oxygen generation activity than Raney nickel obtained from NiAl alloys not containing iron. In addition, the Tafel slope has a minimum value when the iron ratio x is around 0.2. From this result, it can be seen that among NiAl alloys containing iron, the Raney nickel obtained from the NiAl alloys with the composition formula Al 3 Ni (2-x) Fe x It can be seen that Raney nickel obtained from a NiAl alloy represented by the formula (x is a value satisfying 0.1≦x≦0.4) exhibits particularly high oxygen generation activity.

[0078] Test 2 In Test 2, the catalytic activity of Raney nickel obtained from the second NiAl alloy containing iron was evaluated.

[0079] (Preparation of Raney Nickel) A mixture of predetermined amounts of aluminum, nickel, and iron is heated and melted at 1550°C using a high-frequency melting furnace, and then cooled to obtain a Raney Nickel alloy whose main phase is Al. 3 Ni 1 phase, and has the composition formula Al 3 Ni (1-x) Fe x The alloy ingots were prepared by varying the x in the above formula to 0, 0.05, 0.1, 0.2, 0.3, or 0.7. The obtained alloy ingots were pulverized to obtain NiAl alloy powders of the above composition. The average particle size of the obtained powders was measured by a laser scattering method and found to be in the range of 50 to 70 μm.

[0080] Next, the obtained NiAl alloy powder was subjected to the same alkali treatment and oxidation treatment as in Test 1 to obtain a second Raney nickel powder. (Evaluation of catalytic activity) The oxygen generating activity of the obtained second Raney nickel was evaluated in the same manner as in Test 1. The results are shown in the graph of Figure 2. Table 2 below is a table summarizing the Fe ratio and Tafel slope values ​​at each point in the graph shown in Figure 2. The relative evaluation column of oxygen generating activity in Table 2 also shows the evaluation of the oxygen generating activity of each example with different Fe ratios. This evaluation is a relative evaluation with the Tafel slope value when the Fe ratio is "0" as the reference value. The evaluation criteria are as follows.

[0081] "=": The Tafel slope value is 98% or more and 102% or less of the above reference value, and the oxygen generating activity is equivalent to that when the Fe ratio is "0." "○": The Tafel slope value is 85% or more and less than 98% of the above reference value, and the oxygen generating activity is higher than that when the Fe ratio is "0."

[0082] "Excellent": The Tafel gradient value is less than 85% of the above reference value, and the oxygen generating activity is significantly higher than when the Fe ratio is "0".

[0083]

[0084] As shown in FIG. 2 and Table 2, the Tafel gradient is 3 Ni (1-x) Fe x As the iron ratio x (Fe ratio) in the NiAl alloy increases, the curve becomes convex downward. From this result, it can be seen that Raney nickel obtained from NiAl alloys containing iron in the range of iron ratio x of 0.8 or less has higher oxygen generating activity than Raney nickel obtained from NiAl alloys not containing iron. In addition, the Tafel slope has a minimum value when the iron ratio x is near 0.1. From this result, it can be seen that among NiAl alloys containing iron, the Raney nickel obtained from the NiAl alloys with the composition formula Al 3 Ni (1-x) Fe xIt can be seen that Raney nickel obtained from a NiAl alloy represented by the formula (x is a value satisfying 0.05≦x≦0.3) exhibits particularly high oxygen generation activity.

[0085] <Test 3> In Test 3, the catalytic activity of Raney nickel obtained from the second NiAl alloy containing iron and the fourth NiAl alloy containing iron and cobalt was evaluated. In this test, the Fe ratio of 0.1, which was the Fe ratio that showed the highest oxygen generation activity in Test 2, was used.

[0086] (Preparation of Raney Nickel) A mixture of predetermined amounts of aluminum, nickel, iron, and cobalt is heated and melted at 1550°C using a high-frequency melting furnace, and then cooled to form a Raney Nickel alloy whose main phase is Al. 3 Ni 1 phase, and has the composition formula Al 3 Ni 1 NiAl alloy (Test Example 1) represented by the formula: 3 Ni 1 phase, and has the composition formula Al 3 Ni 0.9 Fe 0.1 NiAl alloy (Test Example 2) represented by the formula: 3 Ni 1 phase, and has the composition formula Al 3 Ni 0.75 Co 0.25 NiAl alloy (Test Example 3) represented by the formula 3 Ni 1 phase, and has the composition formula Al 3 Ni 0.7 Fe 0.1 Co 0.2 The alloy ingots were then crushed to obtain NiAl alloy powders. The average particle size of the resulting powders was measured by a laser scattering method and found to be in the range of 40 to 60 μm.

[0087] Next, the obtained NiAl alloy powder was used to obtain a second Raney nickel powder by performing the same alkali treatment and oxidation treatment as in Test 1. (Evaluation of catalytic activity) The oxygen generation activity of the obtained second Raney nickel was evaluated in the same manner as in Test 1. The results are shown in Table 3.

[0088]

[0089] As shown in Table 3, the Raney nickel obtained from the NiAl alloy containing iron (Test Example 2) has a smaller Tafel slope value than the Raney nickel obtained from the NiAl alloy containing cobalt (Test Example 3). These results demonstrate that the inclusion of iron, as a metal to be contained in the NiAl alloy for enhancing oxygen generating activity, is more effective than the inclusion of other metals such as cobalt. Furthermore, the Raney nickel obtained from the NiAl alloy containing both iron and cobalt (Test Example 4) has a smaller Tafel slope value than the NiAl alloy containing iron (Test Example 2). These results demonstrate that the combined use of both iron and cobalt as metals to be contained in the NiAl alloy for enhancing oxygen generating activity is more effective.

[0090] <Test 4> In Test 4, the catalytic activity of Raney nickel obtained from a third NiAl alloy containing iron and cobalt was evaluated. In this test, the iron ratio in the NiAl alloy was kept constant. In this test, the Fe ratio was fixed at 0.2, which was the Fe ratio that showed the highest oxygen generation activity in Test 1, and the Co ratio was changed.

[0091] (Preparation of Raney Nickel) A mixture of predetermined amounts of aluminum, nickel, iron, and cobalt is heated and melted at 1600°C using a high-frequency melting furnace, and then cooled to form a Raney Nickel alloy whose main phase is Al. 3 Ni 2 phase and Al 4 Ni 3 phase, and has the composition formula Al 3 Ni (1.8-y) Fe 0.2 Co y The alloy ingots were prepared by varying the y in the above formula to 0, 0.1, 0.2, 0.4, and 0.6. The obtained alloy ingots were pulverized to obtain NiAl alloy powders with the above composition. The average particle size of the obtained powders was measured by laser scattering and found to be in the range of 50 to 70 μm.

[0092] Next, the obtained NiAl alloy powder was subjected to the same alkali treatment and oxidation treatment as in Test 1 to obtain a second Raney nickel powder. (Evaluation of catalytic activity) The oxygen generating activity of the obtained Raney nickel powder was evaluated in the same manner as in Test 1. The results are shown in Table 4. The details of the evaluation shown in the relative evaluation column of oxygen generating activity in Table 4 are the same as the evaluation shown in Table 1. The relative evaluation column of oxygen generating activity in Table 4 also shows the evaluation of the oxygen generating activity of each example with different Co ratios. The evaluation is a relative evaluation in which the value of the Tafel slope when the Fe ratio and the Co ratio are both "0" is used as the reference value. The evaluation criteria are as follows.

[0093] "=": The Tafel slope value is 98% or more and 102% or less of the above reference value, and the oxygen generating activity is equivalent to that when the Fe ratio is "0." "○": The Tafel slope value is 85% or more and less than 98% of the above reference value, and the oxygen generating activity is higher than that when the Fe ratio is "0."

[0094] "◎1": The value of the Tafel gradient is 50% or more and less than 85% of the above-mentioned reference value, and the oxygen generating activity is significantly higher than when the Fe ratio is "0." "◎2": The value of the Tafel gradient is less than 50% of the above-mentioned reference value, and the oxygen generating activity is significantly higher than when the Fe ratio is "0."

[0095]

[0096] As shown in Table 4, the Tafel slope of Raney nickel obtained from a NiAl alloy containing both iron and cobalt is lower than when the Fe ratio and cobalt ratio (Co ratio) are 0 (when the NiAl alloy does not contain iron or cobalt), and is approximately equal to or lower than when the Fe ratio is 0.2 and the Co ratio is 0. In particular, when cobalt is contained in a Co ratio range of 0.2 to 0.6, the Tafel slope is extremely small. These results show that even when cobalt is used in combination, the addition of iron can have the effect of improving oxygen generating activity, and that a Co ratio of 0.2 to 0.6 is effective in improving oxygen generating activity.

Claims

1. A method for producing an electrode material for use in electrodes of a water electrolysis device, comprising an alkali treatment step of treating a NiAl alloy with an alkaline substance to dissolve aluminum from the NiAl alloy to obtain Raney nickel, wherein the NiAl alloy has the composition formula Al 3 Ni (n-(x+y)) Fe x Co y (n is 1 or 2, and x and y are values ​​satisfying 0<n-(x+y)<2, 0.005≦x≦0.8, and 0≦y≦0.8).

2. The NiAl alloy has the composition formula Al 3 Ni (2-x) Fe x 2. The method for producing an electrode material according to claim 1, wherein the alloy is represented by the formula: (x is a value satisfying 0.01≦x≦0.8).

3. The NiAl alloy has the composition formula Al 3 Ni (1-x) Fe x 2. The method for producing an electrode material according to claim 1, wherein the alloy is represented by the formula: (x is a value satisfying 0.005≦x≦0.7).

4. The NiAl alloy has the composition formula Al 3 Ni (2-(x+y)) Fe x Co y 2. The method for producing an electrode material according to claim 1, wherein the alloy is represented by the formula: (x and y are values ​​satisfying 0<2-(x+y)<2, 0.01≦x≦0.8, and 0<y≦0.8).

5. The NiAl alloy has the composition formula Al 3 Ni (1-(x+y)) Fe x Co y 2. The method for producing an electrode material according to claim 1, wherein the alloy is represented by the formula: (x and y are values ​​satisfying 0<1-(x+y)<1, 0.005≦x≦0.3, and 0<y≦0.7).

6. A method for producing an electrode material according to any one of claims 1 to 5, wherein the alkaline treatment step includes a process for reacting an alkaline aqueous solution, which is an aqueous solution of the alkaline substance, with the NiAl alloy at a temperature of 100°C or higher, the alkaline substance being an alkali metal hydroxide, and the alkaline aqueous solution having a concentration of 3M or higher.

7. The method for producing an electrode material according to claim 6, wherein the alkaline treatment step includes a process for reacting an alkaline aqueous solution, which is an aqueous solution of the alkaline substance, with the NiAl alloy at a temperature of 140°C or higher, the alkaline substance being an alkali metal hydroxide, and the concentration of the alkaline aqueous solution being 14M or higher.

8. The method for producing an electrode material according to any one of claims 1 to 7, further comprising an oxidation step of oxidizing the surface of the Raney nickel obtained in the alkali treatment step.

9. An electrode material used in an electrode of a water electrolysis device, comprising Raney nickel in which the molar ratio of nickel, iron, and cobalt (nickel:iron:cobalt) is (n-(x+y)):x:y (n is 1 or 2, and x and y are values ​​that satisfy 0<n-(x+y)<2, 0.005≦x≦0.8, 0≦y≦0.8).

10. An electrode material used in an electrode of a water electrolysis device, having the composition formula Al 3 Ni (n-(x+y)) Fe x Co y (n is 1 or 2, and x and y are values ​​satisfying 0<n-(x+y)<2, 0.005≦x≦0.8, 0≦y≦0.8), 11. The electrode material according to claim 9, wherein the electrode is an anode and has a Tafel gradient of 50 to 226 mV / dec.

Citation Information

Patent Citations

  • In-situ growth type composite transition metal oxide oxygen evolution catalytic electrode material and preparation method and application thereof

    CN115094457A

  • Preparation method of high-entropy alkaline electrolysis water electrode

    CN115491692A

  • Prestressing Steel ancher nail method

    KR1020210056292A

  • On-demand hydrogen gas generation device

    US20090081501A1

Cited By

  • Oxygen-evolving anode and method for producing same

    WO2026063413A1