Nonaqueous-electrolyte secondary battery and separator for nonaqueous-electrolyte secondary battery

The introduction of a spacer with a convex and skirt design in the separator for nonaqueous electrolyte secondary batteries addresses deformation issues, improving cycle characteristics and preventing short circuits, thereby enhancing battery performance.

WO2024219289A1PCT designated stage expired Publication Date: 2024-10-24PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014396
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-09
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Nonaqueous electrolyte secondary batteries face challenges in maintaining high cycle characteristics due to separator deformation during charging and discharging, leading to potential short circuits and decreased battery performance.

Method used

A separator design featuring a base material with a spacer that includes a convex portion and a thinner skirt portion at its outer edge, which helps to minimize deformation and prevent short circuits by maintaining a consistent distance between electrodes.

Benefits of technology

The proposed separator design enhances the cycle characteristics of nonaqueous electrolyte secondary batteries by reducing the likelihood of short circuits and maintaining battery performance over repeated charge and discharge cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014396_24102024_PF_FP_ABST
    Figure JP2024014396_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The disclosed nonaqueous-electrolyte secondary battery includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a nonaqueous electrolyte. The negative electrode is a negative electrode on which one or more metals including at least one selected from the group consisting of lithium and sodium precipitate during charge and from which the metals dissolve out during discharge. The separator (50) comprises a base (51) and spacers (52) formed on the base (51). The spacers (52) each comprise a protrusion (52a) and a skirt (52b) which is provided at the outer edge of the protrusion (52a) and which is thinner than the protrusion (52a).
Need to check novelty before this filing date? Find Prior Art

Description

Non-aqueous electrolyte secondary battery and separator for non-aqueous electrolyte secondary battery

[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery and a separator for the non-aqueous electrolyte secondary battery.

[0002] Lithium secondary batteries (lithium metal secondary batteries) are known as one type of non-aqueous electrolyte secondary battery. In lithium secondary batteries, lithium metal precipitates on the negative electrode during charging, and the lithium metal dissolves in the non-aqueous electrolyte during discharging. Various proposals have been made for lithium secondary batteries.

[0003] Claim 1 of Patent Document 1 (JP 2020-077497 A) describes, "A separator for use in a non-aqueous electrolyte battery, the separator comprising a substrate and a convex pattern provided on at least one surface of the substrate, the pattern including end regions disposed at both ends in a planar direction of the convex shape and a central region disposed between the opposing end regions, the end regions having an apex protruding in a thickness direction perpendicular to the planar direction and disposed at the boundary with the central region, the central region having a recessed portion having a thickness smaller than that of the apex."

[0004] Japanese Patent Application Laid-Open No. 2020-077497

[0005] Currently, there is a demand for further improvements in the characteristics of non-aqueous electrolyte secondary batteries. One of the objects of the present disclosure is to provide a non-aqueous electrolyte secondary battery with excellent cycle characteristics.

[0006] One aspect of the present disclosure relates to a non-aqueous electrolyte secondary battery, the non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, a non-aqueous electrolyte, the negative electrode being an electrode on which a metal containing at least one selected from the group consisting of lithium and sodium is deposited during charging and from which the metal dissolves during discharging, the separator including a substrate and a spacer formed on the substrate, the spacer including a protrusion and a skirt disposed around the outer edge of the protrusion and thinner than the protrusion.

[0007] Another aspect of the present disclosure relates to a separator for a non-aqueous electrolyte secondary battery, the separator including a substrate and a spacer formed on the substrate, the spacer including a protrusion and a skirt portion disposed on an outer edge of the protrusion and thinner than the protrusion.

[0008] According to the present disclosure, a non-aqueous electrolyte secondary battery with excellent cycle characteristics can be obtained. The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0009] FIG. 1A is a top view schematically showing an example of a separator of Embodiment 1. FIG. 1B is a cross-sectional view schematically showing a portion of the separator shown in FIG. 1A. FIG. 2 is a top view schematically showing another example of the separator of Embodiment 1. FIG. 3 is a top view schematically showing another example of the separator of Embodiment 1. FIG. 4A is a cross-sectional view schematically showing an example of a manufacturing process for the separator of Embodiment 1. FIG. 4B is a cross-sectional view schematically showing an example of a process subsequent to the process of FIG. 4A. FIG. 5 is a longitudinal cross-sectional view schematically showing an example of a nonaqueous electrolyte secondary battery of Embodiment 2. FIG. 6 is a cross-sectional view schematically showing a portion of the lithium secondary battery shown in FIG. 5.

[0010] Below, embodiments according to the present disclosure will be described using examples, but the embodiments according to the present disclosure are not limited to the examples described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and other materials may be applied as long as the invention according to the present disclosure can be implemented. In this specification, the expression "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits are exemplified for numerical values ​​of specific physical properties or conditions, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit.

[0011] (Non-aqueous electrolyte secondary battery) Hereinafter, the non-aqueous electrolyte secondary battery according to this embodiment may be referred to as a "nonaqueous electrolyte secondary battery (B)" or a "secondary battery (B)." The secondary battery (B) includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte. The negative electrode is an electrode into which a metal containing at least one selected from the group consisting of lithium and sodium is deposited during charging, and the metal dissolves during discharging. The separator includes a substrate and a spacer formed on the substrate. The spacer includes a protrusion and a skirt portion disposed on the outer edge of the protrusion and thinner than the protrusion.

[0012] When using a negative electrode in which metal (negative electrode active material) precipitates during charging, a spacer has traditionally been used to ensure space for the metal to precipitate. In the secondary battery (B), the spacer ensures the space between the positive electrode and the negative electrode. This prevents the electrode group from expanding during repeated charge and discharge. As a result, deterioration in cycle characteristics can be suppressed. Note that expansion of the electrode group can sometimes lead to deterioration in cycle characteristics due to reasons such as breakage of the electrode plates.

[0013] As a result of their investigation, the present inventors have newly discovered that separators with spacers may deteriorate. When using a negative electrode in which metal (negative electrode active material) precipitates and dissolves during charge and discharge, the separator deforms with charge and discharge. When a separator has a substrate and a spacer formed on the substrate, when the separator deforms, the force applied to the substrate at the corners of the lower end of the spacer increases. As a result, the substrate in contact with the corners becomes thinner, making it more likely for micro-short circuits to occur. Micro-short circuits result in a deterioration of battery characteristics (e.g., cycle characteristics).

[0014] As a result of further investigation, the inventors of the present application have newly discovered that the use of spacers having a bottom portion can suppress deterioration of the substrate caused by the spacers. The present disclosure is based on this new finding.

[0015] The metal deposited during charging may contain lithium. The metal deposited during charging may be lithium metal. The lithium metal may contain trace amounts of other metal elements or may be a lithium alloy.

[0016] A lithium secondary battery in which lithium metal is deposited on the negative electrode during charging is also called a lithium metal secondary battery. In the negative electrode of a lithium secondary battery, lithium metal is deposited during charging and dissolves during discharging. The negative electrode has at least a negative electrode current collector, and lithium metal is deposited on the negative electrode current collector. Hereinafter, a lithium secondary battery that is a secondary battery (B) may be referred to as a "lithium secondary battery (LB)."

[0017] In a lithium secondary battery (LB), for example, 70% or more of the rated capacity is achieved by the deposition and dissolution of lithium metal. The movement of electrons at the negative electrode during charging and discharging is mainly due to the deposition and dissolution of lithium metal at the negative electrode. Specifically, 70 to 100% (e.g., 80 to 100% or 90 to 100%) of the movement of electrons (or current from another perspective) at the negative electrode during charging and discharging is due to the deposition and dissolution of lithium metal. In other words, the negative electrode of a lithium secondary battery (LB) differs from a negative electrode in which the movement of electrons at the negative electrode during charging and discharging is mainly due to the absorption and release of lithium ions by the negative electrode active material (e.g., graphite).

[0018] The bottom is formed so as to connect to the outer edge of the convex portion. The bottom is preferably formed over almost the entire outer edge of the convex portion. For example, when the convex portion is a linear convex portion, the bottom is preferably formed on both sides of the linear convex portion in the width direction. When the convex portion is a dot-shaped convex portion, the bottom is preferably formed over the entire outer periphery of the dot-shaped convex portion. The bottom is preferably located over 70% or more, 80% or more, 90% or more, or 95% or more of the outer edge of the convex portion.

[0019] The width Wf of the bottom portion may be 1 μm or more, 5 μm or more, or 10 μm or more, and may be 40 μm or less, or 20 μm or less. The width Wf of the bottom portion may be in the range of 1 μm to 40 μm (e.g., in the range of 5 μm to 20 μm). The width Wc of the convex portion may be 100 μm or more, or 500 μm or more, and may be 5000 μm or less, or 1000 μm or less. The width Wc of the convex portion may be in the range of 100 μm to 5000 μm (e.g., in the range of 500 μm to 1000 μm).

[0020] The ratio Wf / Wc of the width Wf of the base to the width Wc of the convex portion may be 0.001 or more, 0.006 or more, 0.02 or more, or 0.08 or more. The ratio Wf / Wc may be 0.6 or less, 0.4 or less, 0.12 or less, or 0.08 or less. The ratio Wf / Wc may be in the range of 0.001 to 0.4 (e.g., 0.006 to 0.12 or 0.006 to 0.08). By setting the ratio Wf / Wc to 0.001 or more, deterioration of the separator can be particularly suppressed. By setting the ratio Wf / Wc to 0.4 or less, a decrease in permeability to liquids and ions can be suppressed.

[0021] The average height Hf of the skirt may be 0.5 μm or more, 1 μm or more, or 2 μm or more, and may be 10 μm or less, or 5 μm or less. The average height Hf of the skirt may be in the range of 0.5 μm to 10 μm (for example, in the range of 1 μm to 5 μm).

[0022] The average height Hc of the convex portions may be 10 μm or more, or 20 μm or more, or may be 100 μm or less, 50 μm or less, 40 μm or less, or 30 μm or less. Note that the height of the convex portions may be approximately constant across the separator so that the gap between the electrodes formed by the spacers is approximately constant.

[0023] The ratio Hf / Hc of the average height Hf of the base to the average height Hc of the peaks may be 0.005 or more, 0.01 or more, or 0.05 or more, and may be 0.25 or less, or 0.15 or less. The ratio Hf / Hc may be in the range of 0.005 to 0.25 (for example, 0.01 to 0.15).

[0024] The average height of one skirt portion can be determined from an image of the cross section of the skirt portion. Specifically, the cross-sectional area of ​​the skirt portion and the length of the base of the skirt portion are measured from the image, and the average height of one skirt portion can be determined by dividing the cross-sectional area by the length of the base. The average skirt height Hf is determined by determining the average height from 20 or more (e.g., 20) cross-sectional images of the skirt portion selected at random, and then arithmetically averaging the obtained average heights from the 20 or more locations.

[0025] The height of a single convex portion can be determined by measuring the height of the highest part of the convex portion in an image of the cross section of the spacer. The average height Hc of the convex portions can be determined by determining the height of each convex portion from cross-sectional images of 20 or more arbitrarily selected convex portions (for example, 20 positions) and then arithmetically averaging the heights obtained at the 20 or more positions.

[0026] The bottom portion may be gradually thinner with increasing distance from the protrusion. This configuration particularly prevents damage to the substrate caused by the corners of the protrusion. The bottom portion may be formed to have a substantially constant thickness.

[0027] The ratio Sa / Ss of the area Ss of the spacers to the area Sa of the main surface on which the spacers are formed, of the two main surfaces of the separator substrate, may be 0.001 or more, or 0.01 or more, and may be 0.25 or less, 0.10 or less, or 0.05 or less. By setting the ratio Sa / Ss to 0.25 or less, it is possible to reduce disadvantages caused by the area occupied by the spacers becoming too large.

[0028] The material of the protrusions and the material of the bottom portion may be different or the same. By using the same material for the protrusions and the bottom portion, the adhesion between the bottom portion and the protrusions can be improved. The protrusions and the bottom portion may contain the same resin. The protrusions and the bottom portion may contain the same resin and the same filler.

[0029] The method for producing the secondary battery (B) is not particularly limited except for the use of the separator described above. The secondary battery (B) may be produced by a production method similar to a known production method. The secondary battery (B) can be produced by enclosing an electrode group including a positive electrode, a negative electrode, and a separator, and a non-aqueous electrolyte in an exterior case.

[0030] (Separator) Hereinafter, the separator according to this embodiment may be referred to as a "separator (S)." The separator (S) is a separator for a non-aqueous electrolyte secondary battery. The separator (S) includes a substrate and a spacer formed on the substrate, and the spacer includes a protrusion and a skirt portion that is disposed on the outer edge of the protrusion and is thinner than the protrusion.

[0031] The separator (S) can be the same as the separator for the secondary battery (B). The matters described for the separator for the secondary battery (B) can be applied to the separator (S), so duplicated explanations may be omitted. The separator (S) can be used as the separator for the secondary battery (B). The matters described for the separator (S) can also be applied to the separator for the secondary battery (B).

[0032] (Spacer) The spacer may contain a resin (for example, an insulating resin), or may contain a resin and a filler. The spacer may be made of only a resin, or may be made of a resin and a filler.

[0033] Examples of resin materials include fluorine-containing resins (polyvinylidene fluoride (PVdF), polytetrafluoroethylene, etc.), fluorine-containing rubbers (vinylidene fluoride-tetrafluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, etc.), rubbers (styrene-butadiene copolymer or its hydrogenated product, acrylonitrile-butadiene copolymer or its hydrogenated product, methacrylic acid ester-acrylic acid ester copolymer, styrene-acrylic acid ester copolymer, acrylonitrile-acrylic acid ester copolymer, ethylene propylene rubber, polyvinyl alcohol, polyvinyl acetate, etc.), cellulose derivatives, Examples of suitable resins include polymers (ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, etc.), acrylic resins (acrylic acid-methacrylic acid copolymers, etc.), polyphenylene ether, polysulfone, polyether sulfone, polyphenylene sulfide, polyetherimide, polyimide, polyamide (wholly aromatic polyamide (aramid) etc.), polyamideimide, polyacrylonitrile, polyvinyl alcohol, polyether, polyacrylic acid, polymethacrylic acid, polyester, polyolefin, silicone resin, urethane resin, melamine resin, urea resin, and epoxy resin.

[0034] The resin content Cr in the spacer may be 10% by volume or more, 30% by volume or more, 40% by volume or more, or 50% by volume or more, or may be 100% by volume or less, 90% by volume or less, 80% by volume or less, or 60% by volume or less. By making the content Cr 30% by volume or more, deformation of the spacer due to compression can be suppressed.

[0035] The filler contained in the spacer is not particularly limited. The filler may be an insulating filler. The filler may be an inorganic filler, an organic filler, or a mixture thereof. Examples of filler materials include oxides, nitrides, carbides, etc. Examples of oxides include aluminum oxide (alumina), magnesium oxide, titanium oxide, zirconium oxide, silicon oxide, etc. Examples of nitrides include silicon nitride, aluminum nitride, titanium nitride, etc. Examples of carbides include silicon carbide, etc.

[0036] The shape of the filler may be spherical or non-spherical. The average particle size of the filler is not particularly limited, but may be 0.1 μm or more or 0.5 μm or more, and may be 10 μm or less, 5 μm or less, or 2 μm or less. The average particle size can be measured using the following method. First, a cross-section of the spacer is photographed using an electron microscope to obtain an image of the cross-section. Next, the image is subjected to image processing such as binarization to identify the particle portion. Next, the diameter of a circle having the same area as the cross-section area of ​​each particle (equivalent circle diameter) is determined, and the arithmetic mean of the determined equivalent circle diameters can be used as the average particle size. The arithmetic mean can be determined from, for example, 20 particles. The average particle size of other particles contained in the electrode plate and separator can also be determined using a similar method.

[0037] The spacer may be formed on the main surface of the substrate on the positive electrode side or on the main surface of the substrate on the negative electrode side. When the spacer is formed on the main surface of the substrate on the positive electrode side, the substrate is significantly deformed due to precipitation of metal (negative electrode active material) during charging. Therefore, the technology of the present disclosure is particularly preferably used when the spacer is formed on the main surface of the substrate on the positive electrode side.

[0038] The shape of the convex portion included in the spacer is not particularly limited as long as it can form a space in at least one region. The convex portion may include at least one type selected from the group consisting of linear convex portions and dot-shaped convex portions.

[0039] The spacer may include linear protrusions arranged in a mesh pattern. The mesh pattern may be a pattern combining polygons (triangles, squares, hexagons, etc.). For example, the mesh pattern may be a honeycomb pattern. The spacer may include a plurality of linear protrusions arranged in a stripe pattern. The spacer may include a plurality of dot-shaped protrusions regularly arranged at regular intervals.

[0040] The shape of the cross section of the linear protrusions (a cross section perpendicular to the direction in which the linear protrusions extend) is not particularly limited, and may be rectangular, trapezoidal, or semicircular.

[0041] The spacer may have a non-porous structure that is impermeable to ions of the metal (e.g., lithium ions) that are the negative electrode active material. Such a spacer can be realized by forming the spacer under conditions that prevent the spacer from becoming porous. The method for forming a spacer having a non-porous structure is not particularly limited, and known methods may be used. For example, a spacer having a non-porous structure may be formed by printing the spacer's constituent material as ink on a separator. In this specification, "lithium ions do not permeate" means that an amount of lithium ions that would affect the battery's characteristics or shape does not permeate, and includes cases where an amount of lithium ions that is considered to be substantially not permeating moves within the spacer.

[0042] (Substrate) The substrate is a sheet that can be used as a separator for a non-aqueous electrolyte secondary battery. The substrate may be composed of only a substrate layer. Alternatively, the substrate may include a substrate layer and a composite material layer formed on the substrate layer. The composite material layer contains a polymer and inorganic particles. When the substrate includes a substrate layer and a composite material layer, the separator may be disposed so that the composite material layer faces the positive electrode, or so that the composite material layer faces the negative electrode. When the substrate includes a substrate layer and a composite material layer, a spacer may be formed on the substrate layer or on the composite material layer. Forming a spacer on the composite material layer particularly enhances the effect of suppressing thermal shrinkage of the substrate layer.

[0043] If the temperature of an electrode assembly composed of a positive electrode, a negative electrode, and a separator rises excessively, the substrate layer will shrink, which will likely cause a short circuit between the positive electrode and the negative electrode, further increasing the temperature of the electrode assembly. By laminating a composite material layer on the substrate layer, it is possible to suppress the substrate layer from shrinking when the temperature of the electrode assembly rises. As a result, it is possible to suppress a further temperature rise in the electrode assembly.

[0044] The substrate layer is made of a porous sheet having ion permeability and insulating properties. Examples of porous sheets include porous membranes, woven fabrics, and nonwoven fabrics. The separator material is not particularly limited, but may be a polymeric material. Examples of polymeric materials include polyolefin resins, polyamide resins, and cellulose. Examples of polyolefin resins include polyethylene, polypropylene, and copolymers of ethylene and propylene. The substrate layer may contain additives as needed. Examples of additives include inorganic fillers. The substrate layer may be made of a sheet used as a separator in a nonaqueous electrolyte secondary battery (e.g., a lithium secondary battery).

[0045] The composite material layer includes a polymer (hereinafter sometimes referred to as "polymer (PL)") and inorganic particles. The inorganic particles may include first particles and / or second particles. The first particles are particles of a lithium-containing phosphate. The second particles are particles other than the first particles. The composite material layer is a layer that allows lithium ions to pass through.

[0046] The phosphate constituting the first particles is lithium phosphate (Li 3 P.O. 4 ), dilithium hydrogen phosphate (Li 2 HPO 4 ), and lithium dihydrogen phosphate (LiH 2 P.O. 4 Among these, lithium phosphate is preferred because it is highly effective in suppressing heat generation in the battery during abnormal conditions.

[0047] A preferred example of the second particles (inorganic particles) is a particle made of an insulating inorganic compound that does not melt or decompose when the battery generates abnormal heat. The second particles may be inorganic particles commonly used as inorganic fillers. Examples of materials for the second particles include aluminum oxide, boehmite, talc, titanium oxide, magnesium oxide, and silicon oxide.

[0048] The polymer (PL) is preferably a polymer having higher heat resistance than the main component of the separator substrate layer. The polymer (PL) may contain at least one selected from the group consisting of aromatic polyamide, aromatic polyimide, and aromatic polyamideimide. These are known as polymers with high heat resistance. Aramid (wholly aromatic polyamide) is preferred from the viewpoint of heat resistance.

[0049] The inorganic particles may include the first particles and second particles other than phosphate. In this case, the composite material layer may include a first layer including the first particles and a second layer including the second particles. This configuration can particularly enhance the effect of suppressing excessive temperature rise in the electrode group. Note that the composite material layer may be composed of only the first layer or only the second layer.

[0050] The first layer and the second layer may be laminated on the main surface of the substrate layer that faces the positive electrode, on the main surface of the substrate layer that faces the negative electrode, or on different main surfaces. For example, the separator and the spacer may have a laminate structure of substrate layer / first layer / second layer / spacer, substrate layer / second layer / first layer / spacer, first layer / second layer / substrate layer / spacer, or second layer / first layer / substrate layer / spacer. Alternatively, the first layer and the second layer may be disposed on different main surfaces of the substrate layer. For example, the separator and the spacer may have a laminate structure of first layer / substrate layer / second layer / spacer, or second layer / substrate layer / first layer / spacer.

[0051] The thickness of the substrate is not particularly limited and may be 5 μm or more, or 10 μm or more, and may be 50 μm or less, or 40 μm or less. When the substrate includes a substrate layer and a composite material layer, the thickness of the substrate layer may be 5 μm or more, or 10 μm or more, and may be 50 μm or less, or 40 μm or less.

[0052] (Method for manufacturing separator (S)) The separator (S) can be manufactured by forming spacers on a substrate. The method for forming the spacers is not particularly limited. The bottom portion and the convex portion may be formed simultaneously or separately. As described below, the bottom portion and the convex portion may be formed integrally.

[0053] The bottom and protrusions may be formed by applying a coating liquid and then drying it. The coating liquid can be prepared by mixing the components of each part with a liquid medium (dispersion medium). The liquid medium used to form the coating liquid is not particularly limited. Examples of liquid media include organic solvents (N-methyl-2-pyrrolidone, etc.). The coating liquid may be applied using a dispenser or by known printing methods such as gravure printing, inkjet printing, and screen printing. Drying may also be performed by known methods such as drying by heating or natural drying.

[0054] An example of a method for forming a spacer is described below. This method includes steps (i) and (ii). In step (i), a first layer that will become the base and the bottom of the convex portions is formed on the substrate. In step (ii), a second layer that will become the portion of the convex portions other than the bottom of the convex portions is formed on the first layer. The first and second layers can be formed, for example, by applying a coating liquid to the substrate and then drying it.

[0055] Another example of a method for forming a spacer will be described below. In this method, first, either the bottom portion or the protrusion portion is formed, and then the other of the bottom portion and the protrusion portion is formed. In this manner, the spacer can be formed.

[0056] When the substrate includes a substrate layer and a composite material layer, the substrate may be produced by the following method: First, a substrate layer is prepared. A commercially available substrate layer may be used as the substrate layer. Next, a composite material layer is formed on the substrate layer.

[0057] There is no particular limitation on the method for forming the composite material layer, and it may be formed by the following method. First, a coating liquid is formed by mixing the components of the composite material layer with a liquid medium (dispersion medium). Next, the coating liquid is applied to the substrate layer to form a coating film, and the coating film is then dried. In this manner, the composite material layer can be formed. There is no particular limitation on the liquid medium used to form the coating liquid. Examples of the liquid medium include organic solvents (such as N-methyl-2-pyrrolidone).

[0058] There are no particular limitations on the steps in forming the composite material layer, and known methods can be used. For example, the coating of the coating liquid may be performed by a known method such as a method using a bar coater. Furthermore, the drying may be performed by a known method such as drying by heating or natural drying.

[0059] Examples of each component of the secondary battery (B) will be specifically described below. Note that the components described below are merely examples, and the components of the secondary battery (B) of this embodiment are not limited to the following components. Known components may be used for components other than those characteristic of the secondary battery (B) of this embodiment. The following mainly describes the case where the secondary battery (B) is a lithium secondary battery (lithium secondary battery (LB)). If the secondary battery (B) is a battery other than a lithium secondary battery, components (positive electrode, negative electrode, non-aqueous electrolyte, etc.) appropriate for that battery may be used. The separator and spacer have been described above, so redundant description will be omitted.

[0060] The shape of the secondary battery (B) is not particularly limited, and examples of the shape of the secondary battery (B) include a cylindrical shape, a coin shape, a square shape, a sheet shape, and a flat shape.

[0061] The negative electrode is disposed opposite the positive electrode. The separator is disposed between the positive electrode and the negative electrode. The positive electrode, the negative electrode, and the separator may be wound together so that the separator is disposed between the positive electrode and the negative electrode. When forming a wound electrode assembly, a strip-shaped positive electrode, a strip-shaped negative electrode, and a strip-shaped separator are used. Alternatively, the positive electrode, the negative electrode, and the separator may be stacked. For example, a flat positive electrode, a flat negative electrode, and a flat separator may be stacked. That is, the electrode assembly may be a wound electrode assembly or a stacked electrode assembly.

[0062] (Negative Electrode) The negative electrode includes a negative electrode current collector. In a lithium secondary battery (LB), lithium metal is deposited on the negative electrode current collector upon charging. More specifically, lithium ions contained in the non-aqueous electrolyte receive electrons on the negative electrode current collector upon charging, becoming lithium metal, which is then deposited on the negative electrode current collector. The lithium metal deposited on the negative electrode current collector dissolves as lithium ions in the non-aqueous electrolyte upon discharging. The lithium ions contained in the non-aqueous electrolyte may be derived from a lithium salt added to the non-aqueous electrolyte, may be supplied from the positive electrode active material upon charging, or may be both.

[0063] The negative electrode current collector may be a conductive sheet. When the electrode group is a wound type, a strip-shaped conductive sheet is used. Examples of the conductive sheet include a conductive film and a metal foil.

[0064] The material of the negative electrode current collector (conductive sheet) may be any conductive material other than lithium metal and lithium alloys. The conductive material may be a metal. The conductive material is preferably a material that does not react with lithium. The conductive material preferably does not form either an alloy or an intermetallic compound with lithium. Examples of such conductive materials include copper (Cu), nickel (Ni), iron (Fe), alloys containing these metal elements, or graphite with a preferentially exposed basal surface. Examples of alloys include copper alloys and stainless steel (SUS). In terms of high conductivity, the conductive material is preferably copper and / or a copper alloy. The thickness of the negative electrode current collector is not particularly limited and may be in the range of 5 to 300 μm.

[0065] A negative electrode mixture layer may be formed on the surface of the negative electrode current collector. The negative electrode mixture layer is formed, for example, by applying a paste containing a negative electrode active material such as graphite to at least a portion of the surface of the negative electrode current collector. However, from the viewpoint of achieving a high-capacity lithium secondary battery exceeding that of a lithium ion battery, the thickness of the negative electrode mixture layer is set to be sufficiently thin so that lithium metal can be precipitated on the negative electrode.

[0066] The negative electrode may include a negative electrode current collector and a sheet-like lithium metal or lithium alloy disposed on the negative electrode current collector. That is, the negative electrode current collector may be provided with a base layer (a layer of lithium metal or lithium alloy) containing lithium metal in advance. The lithium alloy may contain elements such as aluminum, magnesium, indium, and zinc in addition to lithium. By providing the base layer in advance and depositing lithium metal on it during charging, dendritic deposition can be more effectively suppressed. The thickness of the base layer is not particularly limited, but may be, for example, in the range of 5 μm to 25 μm.

[0067] (Positive Electrode) The positive electrode may include a positive electrode current collector and a positive electrode mixture layer supported on the positive electrode current collector. The positive electrode mixture layer includes a positive electrode active material. The positive electrode mixture layer may include a positive electrode active material, a conductive material, and a binder. The positive electrode mixture layer may be formed on only one side of the positive electrode current collector, or may be formed on both sides. The positive electrode can be formed, for example, by applying a positive electrode mixture slurry containing the positive electrode active material, a conductive material, and a binder to the positive electrode current collector, drying the coating, and then rolling it.

[0068] The positive electrode active material is a material that absorbs and releases lithium ions. Examples of the positive electrode active material include lithium-containing transition metal oxides, transition metal fluorides, polyanions, fluorinated polyanions, and transition metal sulfides. Among these, lithium-containing transition metal oxides are preferred because of their low production cost and high average discharge voltage.

[0069] Examples of transition metal elements contained in the lithium-containing transition metal oxide include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, and W. The lithium-containing transition metal oxide may contain one or more transition metal elements. The transition metal element may be Co, Ni, and / or Mn. The lithium-containing transition metal oxide may contain one or more typical elements as needed. Examples of typical elements include Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, and Bi. The typical element may be Al, etc.

[0070] The conductive material is, for example, a carbon material, such as carbon black (acetylene black, ketjen black, etc.), carbon nanotubes, and graphite.

[0071] Examples of the binder include fluororesin, polyacrylonitrile, polyimide resin, acrylic resin, polyolefin resin, rubber polymer, etc. Examples of the fluororesin include polytetrafluoroethylene, polyvinylidene fluoride, etc.

[0072] The positive electrode current collector may be a conductive sheet, such as a foil or film, and the surface of the positive electrode current collector may be coated with a carbon material.

[0073] Examples of materials for the positive electrode current collector (conductive sheet) include metal materials containing Al, Ti, Fe, etc. The metal material may be Al, an Al alloy, Ti, a Ti alloy, an Fe alloy, etc. The Fe alloy may be stainless steel (SUS). The thickness of the positive electrode current collector is not particularly limited and may be in the range of 5 to 300 μm.

[0074] (Non-aqueous electrolyte) The non-aqueous electrolyte having lithium ion conductivity contains, for example, a non-aqueous solvent and lithium ions and anions dissolved in the non-aqueous solvent. The non-aqueous electrolyte may be in a liquid state or a gel state.

[0075] The liquid non-aqueous electrolyte is prepared by dissolving a lithium salt in a non-aqueous solvent, which generates lithium ions and anions.

[0076] The gel-like non-aqueous electrolyte contains a lithium salt and a matrix polymer, or a lithium salt, a non-aqueous solvent, and a matrix polymer. The matrix polymer is, for example, a polymer material that absorbs the non-aqueous solvent and gels. Examples of the polymer material include fluororesin, acrylic resin, and polyether resin.

[0077] As the lithium salt or anion, any known material used in non-aqueous electrolytes for lithium secondary batteries can be used. Specifically, BF 4 - , ClO 4 - , P.F. 6 - , C.F. 3 SO 3 - , C.F. 3 CO 2 - , anions of imides, anions of oxalate complexes, etc. Examples of the anions of imides include N(SO 2 CF 3 ) 2 - , N(C m F 2m+1 SO 2 ) x (C n F2n+1 SO 2 ) y - (m and n are each independently an integer of 0 or 1 or more, and x and y are each independently 0, 1, or 2, satisfying the relationship x+y=2.) The anion of the oxalate complex may contain boron and / or phosphorus. Examples of the anion of the oxalate complex include bisoxalate borate anion, BF 2 (C 2 O 4 ) - , P.F. 4 (C 2 O 4 ) - , P.F. 2 (C 2 O 4 ) 2 - The non-aqueous electrolyte may contain one of these anions alone or two or more of them.

[0078] From the viewpoint of suppressing the deposition of lithium metal in a dendrite-like form, the non-aqueous electrolyte preferably contains an anion of an oxalate complex. The interaction between the anion of the oxalate complex and lithium facilitates the uniform deposition of lithium metal in the form of fine particles. This facilitates the suppression of local deposition of lithium metal. The anion of the oxalate complex may be combined with another anion. The other anion may be PF 6 - and / or an anion of an imide.

[0079] The non-aqueous electrolyte contains LiBF as a solute (lithium salt). 2 (C 2 O 4 ) (lithium difluorooxalatoborate).

[0080] Examples of non-aqueous solvents include esters, ethers, nitriles, amides, and halogen-substituted derivatives thereof. The non-aqueous electrolyte may contain one or more of these non-aqueous solvents. Examples of halogen-substituted derivatives include fluorides.

[0081] Examples of esters include carbonate esters and carboxylic acid esters. Examples of cyclic carbonate esters include ethylene carbonate, propylene carbonate, and fluoroethylene carbonate (FEC). Examples of chain carbonate esters include dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate. Examples of cyclic carboxylic acid esters include γ-butyrolactone and γ-valerolactone. Examples of chain carboxylic acid esters include ethyl acetate, methyl propionate, and methyl fluoropropionate.

[0082] Examples of the ether include cyclic ethers and chain ethers. Examples of the cyclic ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, and 2-methyltetrahydrofuran. Examples of the chain ethers include 1,2-dimethoxyethane, diethyl ether, ethyl vinyl ether, methyl phenyl ether, benzyl ethyl ether, diphenyl ether, dibenzyl ether, 1,2-diethoxyethane, and diethylene glycol dimethyl ether.

[0083] The concentration of the lithium salt in the non-aqueous electrolyte is, for example, 0.5 mol / L or more and 3.5 mol / L or less. The concentration of the anion in the non-aqueous electrolyte may be 0.5 mol / L or more and 3.5 mol / L or less. Furthermore, the concentration of the anion of the oxalate complex in the non-aqueous electrolyte may be 0.05 mol / L or more and 1 mol / L or less.

[0084] The non-aqueous electrolyte may contain an additive. The additive may form a coating on the negative electrode. The formation of a coating derived from the additive on the negative electrode makes it easier to suppress the formation of dendrites. Examples of such additives include vinylene carbonate, FEC, and vinyl ethyl carbonate (VEC).

[0085] (Others) The secondary battery (B) usually includes an exterior body that houses an electrode group and a non-aqueous electrolyte. The exterior body is not particularly limited, and known exterior bodies can be used.

[0086] Below, examples of the separator (S) and nonaqueous electrolyte secondary battery (B) of this embodiment will be specifically described with reference to the drawings. The components described above can be applied to the components of the examples described below. Furthermore, the components of the examples described below can be modified based on the above description. Furthermore, the matters described below may be applied to the above embodiment. Furthermore, in the separator and secondary battery described below, components that are not essential for the separator and secondary battery according to the present disclosure may be omitted. Note that the scale of the components has been changed in the following figures to facilitate understanding.

[0087] (Embodiment 1) In embodiment 1, an example of a separator (S) will be described. FIG. 1A shows a top view of a separator 50 of embodiment 1. The separator 50 includes a substrate 51 and a spacer 52 formed on the substrate 51. FIG. 1B shows a cross-sectional view of the separator 50 at a portion where the spacer 52 is present. Note that hatching of the spacer 52 is omitted in FIG. 1B for ease of viewing. The cross-section of FIG. 1B is a cross-sectional view taken along a direction perpendicular to the extension direction of the linear protrusions 52a. As shown in FIG. 1B, the spacer 52 includes linear protrusions 52a and two skirts 52b arranged on either side of the protrusions 52a. As shown in FIG. 1A, the spacer 52 (linear protrusions 52a) is formed in a honeycomb pattern. FIG. 1B also shows the height Hx of the protrusions 52a, the width Wc of the protrusions 52a, and the width Wf of one skirt 52b.

[0088] The skirt portion 52b is connected to the outer edge of the protrusion 52a and is thinner than the protrusion 52a. The skirt portion 52b has a tapered shape that becomes thinner as it moves away from the protrusion 52a. The angle α between the surface 52bs of the skirt portion 52b and the surface 51s of the substrate 51 is smaller than the angle β between the side surface 52as of the protrusion 52a and the surface 51s of the substrate 51. An inflection point 52p, where the angle between the surface of the spacer 52 and the surface 51s of the substrate 51 changes significantly, can be defined as the boundary between the protrusion 52a and the skirt portion 52b. If a clear inflection point 52p does not exist, the region where the angle α is 45° or less can be defined as the skirt portion 52b, and the remaining region can be defined as the protrusion 52a.

[0089] Another example of the arrangement of the spacers 52 (protrusions 52 a) is shown in Figures 2 and 3. In the arrangement shown in Figure 2, a plurality of linear spacers 52 spaced apart from one another are formed on the substrate 51. A gap P exists between the linear spacers 52. In the arrangement shown in Figure 3, a plurality of linear spacers 52 arranged in a stripe pattern are formed on the substrate 51.

[0090] An example of a method for forming the spacer 52 will be described. First, a first coating liquid is prepared by dispersing the material (e.g., resin, filler) that will primarily form the bottom portion 52b in a liquid medium (dispersion medium). The liquid medium is not particularly limited, and an organic solvent (e.g., N-methyl-2-pyrrolidone) may be used. Next, the first coating liquid is thinly applied to the area where the protrusions 52a and bottom portion 52b are to be formed and dried, thereby forming a first layer 52x on the substrate 51, as shown in FIG. 4A. The shape of the bottom portion 52b can be changed by, for example, adjusting the concentration of the first coating liquid. For example, by thinning the first coating liquid, it is possible to make the bottom portion 52b more likely to have a tapered shape.

[0091] Next, a second coating liquid is prepared by dispersing the material (e.g., resin, filler) that will primarily form the convex portions 52a in a liquid medium (dispersion medium). The liquid medium is not particularly limited, and an organic solvent (e.g., N-methyl-2-pyrrolidone) may be used. Next, the second coating liquid is applied thickly to the region where the convex portions 52a are to be formed and dried, thereby forming a second layer 52y on the first layer 52x, as shown in FIG. 4B . In this manner, the spacer 52 is formed. The portion of the first layer 52x that is directly below the second layer 52y and the second layer 52y constitute the convex portions 52a. The portion of the first layer 52x that is not directly below the second layer 52y constitutes the skirt portion 52b.

[0092] The coating liquid may be applied using a dispenser or a known printing method such as gravure printing, inkjet printing, screen printing, etc. The coating liquid may be dried by a known method such as drying by heating or natural drying.

[0093] (Embodiment 2) In Embodiment 2, an example of a lithium secondary battery will be described as an example of a nonaqueous electrolyte secondary battery (B). Fig. 5 is a longitudinal sectional view schematically showing a nonaqueous electrolyte secondary battery according to Embodiment 2. Note that in Fig. 5, the spacers and the spaces formed by the spacers are not shown.

[0094] The cylindrical secondary battery (nonaqueous electrolyte secondary battery) 10 shown in Fig. 5 includes a cylindrical battery case, and a wound electrode group 14 and a nonaqueous electrolyte (not shown) housed within the battery case. The battery case includes a case body 15, which is a cylindrical metal container with a bottom, and a sealing body 16 that seals the opening of the case body 15. A gasket 27 is disposed between the case body 15 and the sealing body 16. The gasket 27 ensures the airtightness of the battery case. Within the case body 15, insulating plates 17 and 18 are disposed at both ends of the electrode group 14 in the winding axis direction.

[0095] Case body 15 has a step 21 formed, for example, by pressing a portion of the side wall of case body 15 from the outside. Step 21 may be formed in an annular shape along the circumferential direction of case body 15 on the side wall of case body 15. In this case, sealing body 16 is supported by the surface of step 21 on the opening side.

[0096] The sealing body 16 includes a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cap 26. These members are stacked in this order in the sealing body 16. The above-mentioned members constituting the sealing body 16 are, for example, disk-shaped or ring-shaped. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective centers, and an insulating member 24 is interposed between their respective peripheral edges. The filter 22 and the lower valve body 23 are connected to each other at their respective peripheral edges. The upper valve body 25 and the cap 26 are connected to each other at their respective peripheral edges. In other words, all members except the insulating member 24 are electrically connected to each other.

[0097] A vent hole (not shown) is formed in the lower valve body 23. Therefore, if the internal pressure of the battery case increases due to abnormal heat generation or the like, the upper valve body 25 bulges toward the cap 26 and separates from the lower valve body 23. This cuts off the electrical connection between the lower valve body 23 and the upper valve body 25. If the internal pressure increases further, the upper valve body 25 breaks, and gas is discharged from an opening formed in the cap 26.

[0098] 6 is an enlarged view of a portion of the electrode group 14. FIG. 6 includes a portion near the positive electrode surrounded by region II in FIG. 5 and a portion near the negative electrode surrounded by region III in FIG.

[0099] The electrode group 14 includes a positive electrode 11, a negative electrode 12, and a separator 50. The positive electrode 11, the negative electrode 12, and the separator 50 are all strip-shaped. The separator 50 is the separator described in embodiment 1. The electrode group 14 is formed by winding the positive electrode 11, the negative electrode 12, and the separator 50 such that the separator 50 is disposed between the positive electrode 11 and the negative electrode 12.

[0100] The positive electrode 11 includes a positive electrode current collector 11a and a positive electrode composite layer 11b. The positive electrode current collector 11a is electrically connected to a cap 26, which functions as a positive electrode terminal, via a positive electrode lead 19. In FIG. 6, the negative electrode 12 is shown as a negative electrode (negative electrode current collector) on which no lithium metal is deposited. The negative electrode 12 is electrically connected to a case body 15, which functions as a negative electrode terminal, via a negative electrode lead 20.

[0101] 6 , the spacer 52 is formed on one of the two main surfaces of the substrate 51, the main surface on the positive electrode 11 side, but may also be formed on the main surface on the negative electrode 12 side. The spacer 52 forms a space 14s between the positive electrode 11 and the negative electrode 12.

[0102] In the secondary battery 10, lithium metal is deposited on the negative electrode 12 during charging. In the configuration shown in FIG. 6 , the deposition of lithium metal on the negative electrode 12 causes the substrate 51 in the portion without the protrusion 52 a to move toward the space 14 s. Because the space 14 s exists between the positive electrode 11 and the negative electrode 12, the volume change of the electrode group 14 associated with the deposition of lithium metal is reduced, improving the cycle characteristics. Although the substrate 51 deforms significantly during charging and discharging, the spacer 52 has a bottom portion 52 b, which prevents the spacer 52 from damaging the substrate 51.

[0103] (Additional Notes) The above embodiments disclose the following technologies. (Technology 1) A nonaqueous electrolyte secondary battery comprising: a positive electrode; a negative electrode; a separator disposed between the positive electrode and the negative electrode; and a nonaqueous electrolyte, wherein the negative electrode deposits a metal containing at least one selected from the group consisting of lithium and sodium during charging and dissolves the metal during discharging, and the separator comprises a substrate and a spacer formed on the substrate, and the spacer comprises protrusions and skirts disposed on the outer edges of the protrusions and thinner than the protrusions. (Technology 2) The nonaqueous electrolyte secondary battery according to Technology 1, wherein the width Wf of the skirts is in the range of 1 μm to 40 μm. (Technology 3) The nonaqueous electrolyte secondary battery according to Technology 1 or 2, wherein the ratio Wf / Wc of the width Wf of the skirts to the width Wc of the protrusions is in the range of 0.001 to 0.4. (Technology 4) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 3, wherein the average height Hf of the bottom portion is in the range of 0.5 μm to 10 μm. (Technology 5) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 4, wherein the ratio Hf / Hc of the average height Hf of the bottom portion to the average height Hc of the protrusions is in the range of 0.005 to 0.25. (Technology 6) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 5, wherein the bottom portion becomes thinner with increasing distance from the protrusions. (Technology 7) A separator for a nonaqueous electrolyte secondary battery, comprising: a substrate; and a spacer formed on the substrate, wherein the spacer includes protrusions and bottom portions disposed on the outer edges of the protrusions and thinner than the protrusions. (Technology 8) The separator according to Technology 7, wherein the width of the bottom portion is in the range of 1 μm to 40 μm. (Technology 9) A separator according to Technology 7 or 8, wherein the ratio Wf / Wc of the width Wf of the bottom portion to the width Wc of the convex portion is in the range of 0.001 to 0.4. (Technology 10) A separator according to any one of Technology 7 to 9, wherein the average height of the bottom portion is in the range of 0.5 μm to 10 μm. (Technology 11) A separator according to any one of Technology 7 to 10, wherein the ratio Hf / Hc of the average height Hf of the bottom portion to the average height Hc of the convex portion is in the range of 0.005 to 0.25.(Technology 12) The separator according to any one of Techniques 7 to 11, wherein the bottom portion becomes thinner with increasing distance from the protrusion.

[0104] [Examples] The secondary battery (B) according to this embodiment will be specifically described below based on examples. In the following examples, a plurality of lithium secondary batteries with different separators were fabricated and evaluated.

[0105] (Preparation of Separator SA1) First, a strip-shaped porous polyethylene film (average thickness 10 μm) was prepared as a substrate layer. Next, a porous composite material layer (average thickness 2 μm) was formed on one side of the substrate layer. The composite material layer was formed by forming the second layer and the first layer in this order on the substrate layer.

[0106] The second layer was formed as follows. First, N-methyl-2-pyrrolidone (NMP) and calcium chloride were mixed in a mass ratio of 94.2:5.8. This mixture was heated to approximately 80°C to completely dissolve the calcium chloride. Then, this solution was returned to room temperature, and 2200 g of it was collected. 0.6 mol of paraphenylenediamine (PPD) was added and completely dissolved. While maintaining this solution at approximately 20°C, 0.6 mol of terephthalic acid dichloride (TPC) was added in small portions. The resulting solution was aged at approximately 20°C for 1 hour to obtain a polymerized solution. Next, 100 g of this polymerized solution was mixed with an N-methyl-2-pyrrolidone solution containing 5.8% by mass of calcium chloride to obtain a solution (coating liquid) containing 2% by mass of paraphenylene terephthalamide (PPTA), an aromatic polyamide (aramid).

[0107] The coating solution was then applied to a substrate layer using a slot die method to form a coating film. The substrate layer on which the coating film was formed was then left to stand for 1 hour in an atmosphere at a temperature of 25°C and a relative humidity of 70% to precipitate the aromatic polyamide. The NMP and calcium chloride in the coating film were then removed by rinsing with water. The coating film was then dried at 60°C for 5 minutes to form a second layer.

[0108] The first layer was formed as follows: First, lithium phosphate (Li 3 P.O. 4Particles of lithium phosphate (LiPO4) and poly(N-vinylacetamide) (PNVA) were mixed in a mass ratio of 100:8 to obtain a mixture. The lithium phosphate particles used had a volume-based median diameter of 0.19 μm. Water (ion-exchanged water) was added to the resulting mixture and stirred to prepare a slurry (coating liquid) with a solids concentration of 12 mass%. The slurry was then applied to the second layer by microgravure coating to form a coating film. The coating film was then dried in a drying oven attached to the coating machine. In this manner, the first layer was formed. In this manner, a composite material layer was formed.

[0109] Next, spacers were formed on the composite material layer in a honeycomb pattern as shown in FIG. 3. Specifically, first, a first layer 52x was formed on the composite material layer as shown in FIG. 4A. Next, a second layer 52y was formed on the first layer 52x as shown in FIG. 4B. Each layer was formed so that the average height Hc of the convex portions, the average height Hf of the base portions, and the ratio Wf / Wc of the base width Wf to the convex width Wc were the values ​​shown in Table 1. The convex width Wc was 500 μm. The first layer 52x and the second layer 52y were formed using a coating liquid containing resin and alumina particles (inorganic filler). In this manner, a separator SA1 having spacers was formed.

[0110] (Fabrication of Other Separators) Separators SA2 to SA4 were fabricated using the same method and conditions as for the fabrication of separator SA1, except that spacers were formed so that the ratio Wf / Wc was the value shown in Table 1. In this case, the width Wc of the convex portion was set to 500 μm, the same as for separator SA1. Separator SC1 was fabricated using the same method and conditions as for the fabrication of separator SA1, except that spacers were formed that were composed only of the convex portion and not including the bottom portion.

[0111] (Battery A1) A lithium secondary battery A1 was fabricated according to the following procedure. (1) Fabrication of Positive Electrode A rock-salt lithium-containing transition metal oxide (NCA: positive electrode active material) containing Li, Ni, Co, and Al (the molar ratio of Li to the total of Ni, Co, and Al was 1.0) and having a layered structure was prepared. This lithium-containing transition metal oxide (NCA), acetylene black (AB: conductive material), and polyvinylidene fluoride (PVdF: binder) were mixed in a mass ratio of NCA:AB:PVdF = 95:2.5:2.5, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added and stirred to prepare a positive electrode composite slurry. Next, the resulting positive electrode composite slurry was applied to both sides of a strip-shaped Al foil (positive electrode current collector) and then dried to form a coating of the positive electrode composite. Next, the coating film was rolled using a roller. Finally, the resulting laminate of the positive electrode current collector and the positive electrode composite was cut to a predetermined electrode size. In this way, a positive electrode including a positive electrode current collector and positive electrode composite layers disposed on both sides of the positive electrode current collector was produced.

[0112] (2) Preparation of Negative Electrode A negative electrode was prepared by providing a rolled lithium metal layer (thickness: 25 μm) on both sides of a strip of copper foil (thickness: 12 μm).

[0113] (3) Preparation of non-aqueous electrolyte Ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed in a volume ratio of EC:DMC=30:70. LiPF 6 The concentration of LiBF becomes 1 mol / L. 2 (C 2 O 4 ) were dissolved in water so that the concentration of the non-aqueous electrolyte was 0.1 mol / L to prepare a liquid non-aqueous electrolyte.

[0114] (4) Battery Fabrication An aluminum tab was attached to the positive electrode obtained above. A nickel tab was attached to the negative electrode. The positive electrode and negative electrode were spirally wound in an inert gas atmosphere with the separator SA1 interposed therebetween to fabricate a wound electrode group. The separator SA1 was positioned so that the spacer was in contact with the positive electrode. In this manner, a battery A1 was fabricated.

[0115] (Batteries A2 to A4 and C1) Batteries A2 to A4 and C1 were fabricated under the same conditions and by the same method as for fabricating Battery A1, except that separators SA2 to SA4 or separator SC1 were used instead of separator SA1.

[0116] A charge-discharge test was carried out on each of the batteries fabricated as described above. In the charge-discharge test, the batteries were charged in a thermostatic chamber at 25° C. under the following conditions, then rested for 20 minutes, and discharged under the following conditions.

[0117] (Charging) The battery was charged at a constant current of 2.15 mA per unit area (cm 2 ) of the electrode until the battery voltage reached 4.1 V, and then charged at a constant voltage of 4.1 V until the current value per unit area of ​​the electrode reached 0.54 mA.

[0118] (Discharge) Constant current discharge was carried out at a current of 2.15 mA per unit area of ​​the electrode until the battery voltage reached 3.75 V.

[0119] (Capacity Retention Rate) In the charge-discharge test, the discharge capacity C(1) at the first cycle and the discharge capacity C(200) at the 200th cycle were measured. The capacity retention rate was calculated using the following formula: Capacity retention rate (%) = 100 × C(200) / C(1).

[0120] (Air Resistance of Separator) The air resistance (Gurley seconds) of each of the produced separators was measured by the Gurley tester method.

[0121] The spacer formation conditions and the evaluation results of the separator and battery are shown in Table 1. The air permeability resistance (Gurley seconds) in Table 1 is a relative value when the value for separator SC1 is set to 100%. The higher the air permeability resistance value, the lower the separator's breathability. The higher the capacity retention rate, the better the cycle characteristics.

[0122]

[0123] Batteries A1 to A4 are secondary batteries (B) according to the present disclosure, and Battery C1 is a comparative example. The capacity retention rates of Batteries A1 to A4 were higher than that of Battery C1. This is thought to be due to the effect of forming a bottom portion. As the Wf / Wc value increased, the capacity retention rate tended to decrease. This is thought to be due to the fact that the breathability of the separator decreases as the Wf / Wc value increases.

[0124] The present disclosure can be used for non-aqueous electrolyte secondary batteries and separators for non-aqueous electrolyte secondary batteries. Although the present invention has been described with reference to presently preferred embodiments, such disclosure should not be interpreted as limiting. Various modifications and alterations will undoubtedly become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. Therefore, the appended claims should be construed to cover all modifications and alterations without departing from the true spirit and scope of the present invention.

[0125] REFERENCE SIGNS LIST 10: Secondary battery (nonaqueous electrolyte secondary battery) 11: Positive electrode 11a: Positive electrode current collector 11b: Positive electrode composite layer 12: Negative electrode 14: Electrode group 14s: Space 50: Separator 51: Substrate 52: Spacer 52a: Convex portion 52b: Bottom portion

Claims

1. A non-aqueous electrolyte secondary battery comprising: a positive electrode; a negative electrode; a separator disposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte, wherein the negative electrode is an electrode into which a metal containing at least one selected from the group consisting of lithium and sodium is deposited during charging and wherein the metal dissolves during discharging, the separator comprises a substrate and a spacer formed on the substrate, and the spacer comprises a protrusion and a skirt portion disposed on an outer edge of the protrusion and which is thinner than the protrusion.

2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the width Wf of the bottom portion is in the range of 1 μm to 40 μm.

3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the ratio Wf / Wc of the width Wf of the base to the width Wc of the protrusion is in the range of 0.001 to 0.

4.

4. The nonaqueous electrolyte secondary battery according to claim 1, wherein the average height Hf of the bottom portion is in the range of 0.5 μm to 10 μm.

5. The nonaqueous electrolyte secondary battery according to claim 1, wherein the ratio Hf / Hc of the average height Hf of said base portions to the average height Hc of said projections is in the range of 0.005 to 0.

25.

6. The nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein the bottom portion becomes thinner with increasing distance from the protruding portion.

7. A separator for a non-aqueous electrolyte secondary battery, comprising: a substrate; and a spacer formed on the substrate, the spacer including a protrusion and a bottom portion disposed on an outer edge of the protrusion and thinner than the protrusion.

8. The separator according to claim 7, wherein the width Wf of the bottom portion is in the range of 1 μm to 40 μm.

9. The separator according to claim 7 or 8, wherein the ratio Wf / Wc of the width Wf of the bottom portion to the width Wc of the convex portion is in the range of 0.001 to 0.

4.

10. The separator according to claim 7 or 8, wherein the average height Hf of the bottom portion is in the range of 0.5 μm to 10 μm.

11. The separator according to claim 7 or 8, wherein the ratio Hf / Hc of the average height Hf of said base portions to the average height Hc of said projections is in the range of 0.005 to 0.

25.

12. The separator according to claim 7 or 8, wherein the bottom portion becomes thinner with increasing distance from the protruding portion.

Citation Information

Patent Citations

  • Separator having fine pattern, wound body, and nonaqueous electrolyte battery

    JP2020077497A

  • Separator and nonaqueous electrolyte battery

    JP2013137984A

  • Lithium secondary battery

    WO2022224872A1