Binder composition for non-aqueous secondary battery electrodes, slurry composition for non-aqueous secondary battery electrodes, electrode for non-aqueous secondary batteries, and non-aqueous secondary battery
The binder composition for non-aqueous secondary battery electrodes addresses the challenges of cycle and peel characteristics by optimizing acid content and metal impurities, resulting in improved stability and performance for non-aqueous secondary batteries.
Patent Information
- Application Number
- PCT/JP2024/014785
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-24
AI Technical Summary
Non-aqueous secondary batteries, such as lithium ion batteries, face challenges in maintaining cycle characteristics and peel characteristics, and require improved storage stability in their binder compositions for electrodes.
A binder composition for non-aqueous secondary battery electrodes is developed, comprising a particulate polymer with specific oxidation-reduction potential, acid content, and metal impurity levels, along with a water-soluble polymer, to enhance cycle and peel characteristics and storage stability.
The binder composition improves the cycle characteristics, peel strength, and storage stability of non-aqueous secondary battery electrodes, reducing contamination during production and maintaining battery performance over time.
Smart Images

Figure JP2024014785_24102024_PF_FP_ABST
Abstract
Description
Binder composition for non-aqueous secondary battery electrodes, slurry composition for non-aqueous secondary battery electrodes, electrodes for non-aqueous secondary batteries, and non-aqueous secondary batteries
[0001] The present invention relates to a binder composition for a non-aqueous secondary battery electrode, a slurry composition for a non-aqueous secondary battery electrode, an electrode for a non-aqueous secondary battery, and a non-aqueous secondary battery.
[0002] A non-aqueous secondary battery such as a lithium ion secondary battery generally includes battery components such as a positive electrode, a negative electrode, and a separator that separates the positive electrode from the negative electrode to prevent short circuits between the positive electrode and the negative electrode. These battery components are often formed as a layered structure.
[0003] The positive and negative electrodes of non-aqueous secondary batteries can be formed by applying a slurry composition containing an electrode active material, a binder, and a dispersion medium to a suitable substrate such as a current collector and then volatilizing the dispersion medium. While organic solvents are sometimes used as the dispersion medium, aqueous dispersion media containing water as the main component are sometimes used for ease of operation and to reduce environmental impact. Particulate polymers are often used as binders. Various aqueous slurry compositions containing aqueous dispersion media and binder compositions for preparing such slurry compositions have been proposed (e.g., Patent Documents 1 to 6).
[0004] International Publication No. WO 2015 / 098008, International Publication No. WO 2015 / 129257, International Publication No. WO 2015 / 098507, International Publication No. WO 2013 / 191239, International Publication No. WO 2019 / 188722 (corresponding publication: U.S. Patent Application Publication No. 2020 / 411870, JP 2022-064465 A (corresponding publication: U.S. Patent Application Publication No. 2022 / 115665, JP 2022-064465 A)
[0005] Further improvements in the performance of non-aqueous secondary batteries are required. For example, the cycle characteristics of batteries, i.e., the ability to maintain capacity even after multiple charge / discharge cycles, are required to be further improved. In addition, electrodes are required to have excellent peel characteristics, i.e., excellent adhesion of the electrode mixture layer to the current collector. Furthermore, since the binder composition for forming the slurry is required to be prepared in advance and used when forming the slurry, high storage stability is required.
[0006] Therefore, an object of the present invention is to provide a binder composition for non-aqueous secondary battery electrodes that is capable of realizing a non-aqueous secondary battery with high cycle characteristics and an electrode with high peel characteristics and that has high storage stability; an electrode that is capable of realizing a non-aqueous secondary battery with high cycle characteristics and that has high peel characteristics; and a non-aqueous secondary battery with high cycle characteristics.
[0007] In order to solve the above-mentioned problems, the present inventors have conducted studies and found that the above-mentioned problems can be solved by setting the value of the oxidation-reduction potential in the binder composition and the sum of the amount of acid on the surface of the particulate polymer in the binder composition and the amount of acid in the aqueous phase within specific ranges, and have thus completed the present invention. That is, according to the present invention, the following is provided.
[0008] (1) A binder composition for a non-aqueous secondary battery electrode, comprising a particulate polymer and a dispersion medium, and having an aqueous phase and a solid phase, wherein the binder composition has an oxidation-reduction potential value of 90 to 280 mV, and the sum of the amount of acid on the surface of the particulate polymer and the amount of acid in the aqueous phase is 0.15 mmol / g or more and 1.5 mmol / g or less. (2) The binder composition for a non-aqueous secondary battery electrode according to (1), wherein the contents of Fe, Cu, Zn, Co, Ni, and Cr are all less than 0.5 ppm. (3) The binder composition for a non-aqueous secondary battery electrode according to (1) or (2), wherein the value obtained by dividing the amount of acid contained in the aqueous phase by the sum of the amount of acid on the surface of the particulate polymer and the amount of acid in the aqueous phase is 0.2 or more and 0.6 or less. (4) The binder composition for a non-aqueous secondary battery electrode according to any one of (1) to (3), wherein the particulate polymer comprises one or more units selected from the group consisting of styrene monomer units, butadiene monomer units, (meth)acrylic acid ester monomer units, and acidic group-containing monomer units. (5) The binder composition for a non-aqueous secondary battery electrode according to any one of (1) to (4), further comprising a water-soluble polymer. (6) A slurry composition for a non-aqueous secondary battery electrode, comprising an electrode active material and the binder composition for a non-aqueous secondary battery electrode according to any one of (1) to (5). (7) A non-aqueous secondary battery electrode, comprising an electrode mixture layer formed using the slurry composition for a non-aqueous secondary battery electrode according to (6). (8) A non-aqueous secondary battery, comprising a positive electrode, a negative electrode, a separator, and an electrolytic solution, wherein at least one of the positive electrode and the negative electrode is the non-aqueous secondary battery electrode according to (7).
[0009] According to the present invention, there are provided a binder composition for non-aqueous secondary battery electrodes that can realize a non-aqueous secondary battery with high cycle characteristics and an electrode with high peel characteristics and that has high storage stability; an electrode that can realize a non-aqueous secondary battery with high cycle characteristics and that has high peel characteristics; and a non-aqueous secondary battery with high cycle characteristics.
[0010] FIG. 1 is a graph showing the relationship between the cumulative amount (mmol) of hydrochloric acid added and electrical conductivity (mS) in the measurements of the surface acid amount of a particulate polymer and the acid amount of an aqueous phase of a binder composition in Examples and Comparative Examples of the present application.
[0011] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents.
[0012] In the following description, the term "(meth)acrylic" is meant to encompass "acrylic", "methacrylic" and combinations thereof, for example, (meth)acrylic acid means acrylic acid, methacrylic acid or a mixture thereof.
[0013] In a polymer produced by copolymerizing multiple types of monomers, the ratio of structural units formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of the certain monomer to all the monomers used in the polymerization of the polymer, unless otherwise specified.
[0014] In this application, the "solid content" of a mixture in which a solid is dispersed in a liquid, such as a binder composition or a slurry composition, is defined as the components remaining after the dispersion medium and solvent in the composition evaporate and the composition hardens, and the "solid content concentration" is defined as the concentration of such components. When such a composition consists of water and components dissolved or dispersed in water, the solid content concentration is the concentration of components other than water.
[0015] (Binder composition) The binder composition of the present invention contains a particulate polymer and a dispersion medium, and has an aqueous phase and a solid phase. The aqueous phase consists of water and a water-soluble component, and the solid phase is a particulate polymer, or a particulate polymer and other water-insoluble solid phase. Here, the particulate polymer is preferably a water-insoluble particle. Unless otherwise specified, in this specification, the term "water-insoluble" for polymer particles means that when 0.5 g of the polymer is dissolved in 100 g of water at a temperature of 25°C, the insoluble content is 90 mass% or more. On the other hand, unless otherwise specified, the term "water-soluble" for a polymer means that when 0.5 g of the polymer is dissolved in 100 g of water at a temperature of 25°C, the insoluble content is less than 1.0 mass%.
[0016] (Particulate polymer) The particulate polymer functions as a binder when the binder composition is added to the slurry composition. When such a slurry composition is used to form an electrode mixture layer, the particulate polymer binds the components in the mixture layer together or the components to the current collector in the electrode mixture layer. As the particulate polymer, a polymer dispersible in an aqueous medium such as water can be used.
[0017] Here, examples of the particulate polymer include known polymers, such as diene polymers, acrylic polymers, fluoropolymers, silicone polymers, etc. These polymers may be used alone or in combination of two or more types in any ratio.
[0018] Specifically, it is preferable to use a diene polymer, particularly a copolymer having an aliphatic conjugated diene monomer unit and an aromatic vinyl monomer unit, or a hydrogenated product thereof, as the particulate polymer. This is because a particulate polymer made of a copolymer having an aliphatic conjugated diene monomer unit, which is a repeating unit with low rigidity and flexibility and can enhance binding ability, and an aromatic vinyl monomer unit, which can reduce the solubility of the polymer in the electrolyte solution and thereby enhance the stability of the particulate polymer in the electrolyte solution, can exhibit good function as a binder.
[0019] Here, when a copolymer having an aliphatic conjugated diene monomer unit and an aromatic vinyl monomer unit is used as the particulate polymer, the aliphatic conjugated diene monomer capable of forming the aliphatic conjugated diene monomer unit is not particularly limited, and 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadiene, substituted and side-chain conjugated hexadienes, etc. The aliphatic conjugated diene monomer may be used alone or in combination of two or more types in any ratio.
[0020] In the particulate polymer, the content of the aliphatic conjugated diene monomer unit is preferably 20% by mass or more, more preferably 30% by mass or more, and preferably 70% by mass or less, more preferably 60% by mass or less. If the content of the aliphatic conjugated diene monomer unit is 20% by mass or more, the flexibility of the negative electrode formed using the slurry composition can be increased. Furthermore, if the content of the aliphatic conjugated diene monomer unit is 70% by mass or less, the binding strength of the particulate polymer is sufficiently high, and the components constituting the negative electrode mixture layer and the negative electrode mixture layer and the current collector can be well bound together, thereby increasing the peel strength of the negative electrode.
[0021] The aromatic vinyl monomer capable of forming the aromatic vinyl monomer unit is not particularly limited, and examples thereof include styrene, α-methylstyrene, vinyltoluene, divinylbenzene, etc. The aromatic vinyl monomer may be used alone or in combination of two or more kinds in any ratio.
[0022] The content of the aromatic vinyl monomer units in the particulate polymer is preferably 5% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and preferably 80% by mass or less, more preferably 70% by mass or less. If the content of the aromatic vinyl monomer units is 30% by mass or more, the electrolyte resistance of the negative electrode formed using the binder composition can be improved. Furthermore, if the content of the aromatic vinyl monomer units is 80% by mass or less, the binding strength of the particulate polymer made of the copolymer is sufficiently high, and the components constituting the negative electrode mixture layer and the negative electrode mixture layer and the current collector can be well bound together, thereby increasing the peel strength of the negative electrode.
[0023] The copolymer having an aliphatic conjugated diene monomer unit and an aromatic vinyl monomer unit preferably contains a 1,3-butadiene unit as the aliphatic conjugated diene monomer unit and a styrene unit as the aromatic vinyl monomer unit (i.e., it is a styrene-butadiene copolymer or a hydrogenated styrene-butadiene copolymer).
[0024] From the viewpoint of imparting a desired surface acidity to the particulate polymer, the copolymer (particulate polymer) having an aliphatic conjugated diene monomer unit and an aromatic vinyl monomer unit preferably contains an acidic group-containing monomer unit. Examples of the acidic group-containing monomer unit include an ethylenically unsaturated carboxylic acid monomer unit and an unsaturated monomer unit having a sulfonic acid group. Among these, the particulate polymer preferably contains an ethylenically unsaturated carboxylic acid monomer unit.
[0025] Examples of ethylenically unsaturated carboxylic acid monomers that can form ethylenically unsaturated carboxylic acid monomer units include ethylenically unsaturated monocarboxylic acids and derivatives thereof, ethylenically unsaturated dicarboxylic acids and acid anhydrides thereof, and derivatives thereof. Examples of ethylenically unsaturated monocarboxylic acids and derivatives thereof include acrylic acid, methacrylic acid, crotonic acid, 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, and β-diaminoacrylic acid. Examples of ethylenically unsaturated dicarboxylic acids and derivatives thereof include maleic acid, fumaric acid, itaconic acid, methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, diphenyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleate. Examples of acid anhydrides of ethylenically unsaturated dicarboxylic acids include maleic anhydride, diacrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride. Among these, ethylenically unsaturated monocarboxylic acids are preferred, and acrylic acid is particularly preferred. These may be used alone or in combination of two or more in any ratio.
[0026] Furthermore, examples of unsaturated monomers having a sulfonic acid group that can form unsaturated monomer units having a sulfonic acid group include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)acrylic acid sulfonic acid, styrene sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, etc. These may be used alone or in combination of two or more in any ratio.
[0027] The content of the acidic group-containing monomer units in the particulate polymer is preferably 1% by mass or more, more preferably 2% by mass or more, particularly preferably 3% by mass or more, and is preferably 15% by mass or less, more preferably 13% by mass or less, particularly preferably 10% by mass or less. When the content of the acidic group-containing monomer units is equal to or greater than the lower limit, the surface acid amount of the particulate polymer can be easily increased to the desired range of the present application, and the battery characteristics of the lithium ion secondary battery can be improved while suppressing swelling of the negative electrode. On the other hand, when the content of the acidic group-containing monomer units is equal to or less than the upper limit, the particulate polymer can be easily prepared.
[0028] Furthermore, the copolymer (particulate polymer) having the above-mentioned aliphatic conjugated diene monomer units and aromatic vinyl monomer units preferably contains (meth)acrylic acid ester monomer units. In particular, it is preferable to contain hydroxyl group-containing (meth)acrylic acid ester monomer units having a (meth)acrylic acid ester structure and equipped with hydroxyl groups. Here, examples of hydroxyl group-containing (meth)acrylic acid ester monomers capable of forming hydroxyl group-containing (meth)acrylic acid ester monomer units include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, and 3-chloro-2-hydroxypropyl methacrylate. Of these, 2-hydroxyethyl acrylate is preferred. These may be used alone or in combination of two or more types in any ratio.
[0029] The content of the hydroxyl group-containing (meth)acrylic acid ester monomer units in the particulate polymer is preferably 0.5% by mass or more, more preferably 0.7% by mass or more, particularly preferably 0.8% by mass or more, and preferably 10% by mass or less, more preferably 4% by mass or less, particularly preferably 3% by mass or less. When the content of the hydroxyl group-containing (meth)acrylic acid ester monomer units is above the lower limit, the copolymerization property of an acidic group-containing monomer such as an ethylenically unsaturated carboxylic acid monomer with other monomers can be improved. On the other hand, when the content of the hydroxyl group-containing (meth)acrylic acid ester monomer units is below the upper limit, the polymerization of the hydroxyl group-containing (meth)acrylic acid ester monomers with each other to form a polymer is suppressed, and the copolymerization property of the ethylenically unsaturated carboxylic acid monomer into the particulate polymer is improved, so that the copolymerization of the above-mentioned monomers can be smoothly progressed.
[0030] Furthermore, the copolymer having the aliphatic conjugated diene monomer unit and the aromatic vinyl monomer unit described above may contain any other repeating units in addition to those described above, as long as the effects of the present invention are not significantly impaired. The content ratio of the other repeating units is not particularly limited, but the upper limit is preferably 30% by mass or less, more preferably 4% by mass or less, and particularly preferably 2% by mass or less in total.
[0031] The content ratio of the particulate polymer in the binder composition of the present invention can be a desired ratio suitable for preparing a slurry composition. It can also be appropriately adjusted to improve storage stability. Specifically, the ratio of the particulate polymer to 100 parts by mass of the electrode active material is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 7 parts by mass or less.
[0032] The particulate polymer can be prepared by polymerizing a monomer composition containing the above-mentioned monomers in an aqueous solvent. Here, in the present invention, the content ratio of each monomer in the monomer composition can be determined according to the content ratio of the monomer unit (repeating unit) in the particulate polymer.
[0033] The aqueous solvent is not particularly limited as long as it can disperse the particulate polymer in a particulate state, but water is particularly preferred from the viewpoints that it is non-flammable and that a dispersion of particulate polymer particles can be easily obtained. Water may be used as the main solvent, and a solvent other than water may be mixed therewith within a range in which the dispersed state of the particulate polymer particles can be ensured.
[0034] The polymerization method is not particularly limited, and any method such as solution polymerization, suspension polymerization, bulk polymerization, or emulsion polymerization can be used. The polymerization method can be any method such as ionic polymerization, radical polymerization, or living radical polymerization. From the viewpoint of production efficiency, emulsion polymerization is particularly preferred because it is easy to obtain a high molecular weight product, and the polymer is obtained in a state dispersed in water as is, eliminating the need for redispersion treatment and allowing it to be directly used in the production of the binder composition or slurry composition of the present invention. Emulsion polymerization can be carried out according to a conventional method. Furthermore, seed polymerization using seed particles may be employed in emulsion polymerization.
[0035] The emulsifier, dispersant, polymerization initiator, polymerization aid, and the like used in the polymerization may be those generally used, and the amounts used should be the amounts generally used.
[0036] In addition, to produce the particulate polymer used in the present invention, batch polymerization or semi-batch polymerization can be used, but it is preferable to use semi-batch polymerization in which a monomer is continuously or intermittently added to a reaction system.By using semi-batch polymerization, the surface acid amount of the particulate polymer can be easily controlled compared with the case of using batch polymerization in which an acidic group-containing monomer such as an ethylenically unsaturated carboxylic acid monomer is added to a reaction system all at once from the beginning.
[0037] A preferred method for preparing a particulate polymer using semi-batch polymerization is, for example, when the particulate polymer is a copolymer having the above-mentioned aliphatic conjugated diene monomer units and aromatic vinyl monomer units. A first monomer composition containing an aliphatic conjugated diene monomer, an aromatic vinyl monomer, and an acidic group-containing monomer is continuously or intermittently added to a reaction system. Once the monomer composition addition rate reaches 70% or more, the addition of a second monomer composition containing a hydroxyl group-containing (meth)acrylic acid monomer is initiated to obtain the particulate polymer. "Continuous or intermittent addition" refers to adding the monomer composition to the reaction system over a certain period of time (e.g., 30 minutes or more) rather than all at once. Furthermore, "addition rate of the monomer composition" refers to the proportion (mass%) of the monomer already added to the reaction system relative to the total monomer composition used in the polymerization.
[0038] The "primary monomer composition" is a monomer composition added to the reaction system from the initiation stage of polymerization. Of the total monomer composition used in the polymerization, the primary monomer composition preferably comprises 80 to 99 mass%, more preferably 90 to 99 mass%. The primary monomer composition preferably contains an aromatic vinyl monomer, an aliphatic conjugated diene monomer, and an acidic group-containing monomer, and preferably does not substantially contain a hydroxyl group-containing (meth)acrylic acid ester monomer.
[0039] In preparing a particulate polymer using semi-batch polymerization, for example, a mixture obtained by adding an emulsifier, a chain transfer agent, and water to the primary monomer composition as appropriate, and a separately prepared polymerization initiator are added to a single reaction vessel to initiate the polymerization reaction. The reaction conditions are not particularly limited, but the reaction temperature is preferably 60 to 90°C. The time from the start of polymerization until the addition rate of the monomer composition reaches 70% is not particularly limited, but is preferably 2 to 6 hours, more preferably 3 to 5 hours.
[0040] Then, once the addition rate of the monomer composition reaches 70% or more (i.e., once 70% by mass of the total monomer composition to be used in the polymerization has been added to the reaction system), the addition of the secondary monomer composition containing the hydroxyl group-containing (meth)acrylic acid ester monomer is started. The time from the start of addition of the secondary monomer composition to the end of addition of the secondary monomer composition is not particularly limited, but is preferably 1 to 3 hours. By adding the hydroxyl group-containing (meth)acrylic acid ester monomer later in this manner, copolymerization of the acid group-containing monomer with other monomers can be smoothly progressed, and the magnitude of the surface acidity can be easily controlled.
[0041] The addition of the primary monomer composition and the secondary monomer composition may be completed separately or simultaneously. The time from the start of polymerization to the completion of the addition of the entire monomer composition is not particularly limited, but is preferably 3 to 8 hours, more preferably 4 to 7 hours. After the completion of the addition of the entire monomer composition, the reaction is preferably carried out at 0 to 90°C for 3 to 9 hours.
[0042] Thereafter, when the polymerization conversion rate reaches a sufficient level (e.g., 95% or higher), the reaction is stopped by cooling. After the above-described polymerization, the resulting aqueous dispersion may be adjusted to a pH of typically 5 or higher and typically 10 or lower, preferably 9 or lower, using a basic aqueous solution containing, for example, a hydroxide of an alkali metal (e.g., Li, Na, K, Rb, or Cs), ammonia, an inorganic ammonium compound (e.g., NH4Cl), or an organic amine compound (e.g., ethanolamine or diethylamine), to form an aqueous dispersion of particulate polymer. Among these, pH adjustment using an alkali metal hydroxide is preferred because it improves the peel strength of the negative electrode. Furthermore, after the pH adjustment, it is preferable to remove unreacted monomers by heated, reduced-pressure distillation.
[0043] (Dispersion medium and components constituting the aqueous phase) The binder composition of the present invention contains a dispersion medium. In the binder composition, the dispersion medium and components soluble therein constitute the aqueous phase. Usually, in the binder composition of the present invention, the particulate polymer is dispersed in the dispersion medium. In the binder composition of the present invention, the dispersion medium may be water or a mixture of water and a water-soluble organic solvent, and is preferably water.
[0044] The binder composition of the present invention may contain a water-soluble polymer as a component constituting the aqueous phase. The water-soluble polymer is usually dissolved in water as a dispersion medium to form the aqueous phase.
[0045] As an example of a water-soluble polymer, a polymer containing a monomer unit having an acidic group is preferred from the viewpoint of effectively adjusting the acid content in the aqueous phase. As a monomer having an acidic group capable of forming a monomer unit having an acidic group, (meth)acrylic acid is preferred. Specifically, the water-soluble polymer is preferably poly(meth)acrylic acid or a copolymer of (meth)acrylic acid and any other monomer. Examples of such optional monomers include nitrile-group-containing vinyl monomers such as acrylonitrile and acrylamide. The proportion of (meth)acrylic acid monomer units in 100% by mass of the water-soluble polymer is preferably 50% by mass or more and 100% by mass or less. The proportion of nitrile-group-containing vinyl monomer units in the water-soluble polymer is preferably 1% by mass or more and 29% by mass or less. By adjusting the proportion within this range, a binder composition having a desired acid content in the aqueous phase can be easily prepared, and the desired effects of the present invention can be effectively achieved.
[0046] The content of the water-soluble polymer in the binder composition of the present invention can be appropriately adjusted so that the acid content can be within a desired range. Specifically, the proportion of the water-soluble polymer relative to 100 mass% of the total amount of the binder composition is preferably 0.5 mass% or more, and preferably 2.0 mass% or less. The content of the water-soluble polymer in the binder composition can also be specified relative to the mass of the particulate polymer. When the binder composition contains a water-soluble polymer, the amount of the water-soluble polymer relative to 100 mass parts of the particulate polymer can be more than 0 mass parts and 10 mass parts or less.
[0047] (Other Components) In addition to the above components, the binder composition of the present invention may contain components such as a reinforcing material, a leveling agent, an electrolyte additive, and cellulose nanofibers. These components can be appropriately selected from those that do not affect the battery reaction. For example, known components, specifically those described in International Publication No. 2012 / 115096, can be used. These components may be used alone or in combination of two or more in any ratio.
[0048] (Surface Acid Amount and Aqueous Phase Acid Amount) In the binder composition of the present invention, the sum of the acid amount on the surface of the particulate polymer and the acid amount in the aqueous phase is a value within a specific range. The acid amount on the surface of the particulate polymer may be simply referred to as the "surface acid amount" hereinafter. The "acid amount" is an index reflecting the number of acidic groups per 1 g of the solid content of the binder composition. Therefore, when the binder composition is composed of, for example, a particulate polymer, a water-soluble polymer, and water, the surface acid amount is an index of the number of acidic groups on the surface of the particulate polymer per 1 g of the particulate polymer and the water-soluble polymer, and the acid amount in the aqueous phase is an index of the number of acidic groups in the substance in the aqueous phase per 1 g of the particulate polymer and the water-soluble polymer.
[0049] The sum of the surface acid amount and the acid amount in the aqueous phase is 0.15 mmol / g or more, preferably 0.20 mmol / g or more, more preferably 0.25 mmol / g or more, and is 1.5 mmol / g or less, preferably 1.45 mmol / g or less, more preferably 1.40 mmol / g or less.
[0050] In the binder composition of the present invention, the ratio of the acid amount in the aqueous phase to the total of the surface acid amount and the acid amount in the aqueous phase is preferably within a specific range. Specifically, the value obtained by dividing the acid amount in the aqueous phase by the total of the surface acid amount and the acid amount in the aqueous phase is preferably 0.2 or more, more preferably 0.25 or more, even more preferably 0.30 or more, and is preferably 0.6 or less, more preferably 0.55 or less, even more preferably 0.50 or less, and even more preferably 0.40 or less.
[0051] The amount of acid on the particulate polymer surface and the amount of acid in the aqueous phase of the binder composition can be measured by the following method. The binder composition, diluted with water as necessary, is placed in a glass container washed with distilled water, and a solution conductivity meter is set and stirred. Stirring is then continued until the addition of hydrochloric acid, described below, is completed. A 0.1 N aqueous solution of sodium hydroxide is added to the aqueous dispersion containing the particulate polymer so that the electrical conductivity of the binder composition becomes 2.5 to 3.0 mS. Six minutes later, the electrical conductivity is measured. This value is the electrical conductivity at the start of measurement. 0.5 mL of 0.1 N hydrochloric acid is added to this binder composition, and the electrical conductivity is measured after 30 seconds. Then, 0.5 mL of 0.1 N hydrochloric acid is added again, and the electrical conductivity is measured after 30 seconds. In this manner, the addition of hydrochloric acid and the measurement of the electrical conductivity after 30 seconds are repeated until the electrical conductivity of the binder composition becomes equal to or higher than the electrical conductivity at the start of measurement. The obtained electrical conductivity data is plotted on a graph with electrical conductivity (unit: mS) as the vertical axis (Y-axis) and the cumulative amount of hydrochloric acid added (unit: mmol) as the horizontal axis (X-axis). This results in a hydrochloric acid amount-electrical conductivity curve with three change points (points where the graph bends), as shown in Figure 1. The X-coordinates of the three change points and the X-coordinate at the end of hydrochloric acid addition are designated P1, P2, P3, and P4, respectively, in ascending order. Approximate straight lines L1, L2, L3, and L4 are determined by the least squares method for the data in the X-coordinate range from zero to P1, the range from P1 to P2, the range from P2 to P3, and the range from P3 to P4. The X-coordinate of the intersection of L1 and L2 is designated A1 (mmol), the X-coordinate of the intersection of L2 and L3 is designated A2 (mmol), and the X-coordinate of the intersection of L3 and L4 is designated A3 (mmol). The amount of surface acid of the particulate polymer per 1 g of the solid content of the binder composition and the amount of acid in the aqueous phase of the binder composition per 1 g of the solid content of the binder composition can be calculated as milliequivalents (mmol / g) titrated with hydrochloric acid from the formula (a) and the formula (b), respectively.Formula (a): Amount of surface acid of the particulate polymer per 1 g of solid content of the binder composition (mmol / g)=(A2-A1) / (mass (g) of solid content of the binder composition) Formula (b): Amount of acid in the aqueous phase per 1 g of solid content of the binder composition (mmol / g)=(A3-A2) / (mass (g) of solid content of the binder composition).
[0052] The surface acid content of the particulate polymer can be adjusted by changing the type and amount of monomers used in the production of the polymer used as the particulate polymer. Specifically, the surface acid content can be increased by increasing the amount of an acidic group-containing monomer, such as a carboxylic acid group-containing monomer, used. The acid content in the aqueous phase can be adjusted by changing the type and amount of components, such as a water-soluble polymer, present in a dissolved state in the aqueous phase.
[0053] (Oxidation-Reduction Potential) The binder composition of the present invention has an oxidation-reduction potential within a specific range. Specifically, the oxidation-reduction potential is 90 mV or more, preferably 100 mV or more, and more preferably 110 mV or more, and 280 mV or less, preferably 270 mV or less, and more preferably 250 mV or less.
[0054] The redox potential can be measured using a potentiometer equipped with an appropriate electrode. Specifically, the measurement can be performed at 25°C by immersing a platinum composite ORP electrode (e.g., HORIBA composite electrode 9300-10D).
[0055] The oxidation-reduction potential of the binder composition is affected by the amount of surface acid, the amount of acid in the aqueous phase, the sum of these, and the proportion of the amount of acid in the aqueous phase. Therefore, the oxidation-reduction potential of the binder composition can be adjusted by changing the type and amount of components added to the particulate polymer and the aqueous phase (especially the type and content ratio of the acid group-containing monomer units contained therein). In addition, the oxidation-reduction potential of the binder composition is affected by the content of the metal component, the timing of addition of each component when preparing the binder composition, etc., so that the oxidation-reduction potential can sometimes be adjusted to a desired value by appropriately controlling these factors.
[0056] The inventors have found that the storage stability of the binder composition can be improved by ensuring that the sum of the surface acid amount of the particulate polymer in the binder composition and the acid amount in the aqueous phase, as well as the redox potential, falls within the specific ranges described above. Furthermore, the peel properties of an electrode fabricated using the binder composition can be improved. Furthermore, the cycle characteristics of a non-aqueous secondary battery equipped with an electrode fabricated using the binder composition can be improved. Furthermore, when forming an electrode using the binder composition, the degree of roll contamination during operations in which the roll comes into contact with the electrode mixture layer, such as pressing with a roll in a roll press, can be reduced. While the mechanism by which such effects are achieved is unclear, it is believed that satisfying the above-described conditions for the acid amount and redox potential can reduce the amount of low-molecular-weight components, such as free oligomers, thereby improving storage stability, peel characteristics, and the like. Furthermore, it is believed that the amount of low-molecular-weight components that migrate to the layer surface due to frictional heat generated during the pressing process of the electrode mixture layer in the manufacture of an electrode using a slurry containing the binder composition can be reduced, thereby improving peel properties, cycle characteristics, and roll contamination.
[0057] The above-mentioned effect can be further improved by ensuring that the proportion of the acid amount in the aqueous phase to the total of the surface acid amount and the acid amount in the aqueous phase is within the above-mentioned specific range. Although the principle behind such an effect is not clear, one possible reason is that if the acid amount in the aqueous phase is excessive, the viscosity of the binder composition tends to increase over time, impairing storage stability and ultimately adversely affecting cycle characteristics, etc., and such adverse effects can be avoided by ensuring that the proportion of the acid amount in the aqueous phase is within the above-mentioned specific range.
[0058] (Metal Content) The binder composition of the present invention preferably has a low metal content. Specifically, since elements that generally have a substantial effect on the metal content are Fe, Cu, Zn, Co, Ni, and Cr, it is preferable to measure the content of each of these elements and find that each is less than 0.5 ppm. The metal content can be measured using ICP-MS after subjecting the binder composition to an appropriate pretreatment. The lower limit of the metal content is ideally 0 ppm, but may be greater than 0 ppm.
[0059] By limiting the metal content to the small amount described above, the oxidation-reduction potential can be adjusted to a desired value, and the capacity of a battery produced using the binder composition can be increased.
[0060] Methods for reducing the metal content of a binder composition to less than 0.5 ppm include using a material with a low metal content to prepare the binder composition, as well as removing metal components from the prepared binder composition. An example of a method for removing metal components is removing magnetic substances using magnetism. Since the main metal component is a magnetic metal such as iron, the metal content can be reduced by removing magnetic substances. Examples of magnetic substance removal devices include a magnetic separator sold by Nippon Magnetics Co., Ltd. and a magnetic filter sold by Toc Engineering Co., Ltd.
[0061] (Slurry composition for non-aqueous secondary battery electrode) The slurry composition for non-aqueous secondary battery electrode of the present invention contains an electrode active material and the binder composition for non-aqueous secondary battery electrode of the present invention. The slurry composition of the present invention can be used as a slurry composition for a negative electrode or a slurry composition for a positive electrode, but is particularly preferably used as a slurry composition for a negative electrode. Below, specific examples of the slurry composition for a negative electrode will be mainly described.
[0062] The amount of binder composition added to the slurry composition can be appropriately adjusted so that the ratio of the particulate polymer to the active material in the slurry composition is the desired value. Specifically, the ratio of the particulate polymer is preferably 0.5 parts by mass or more and preferably 5.0 parts by mass or less per 100 parts by mass of the active material. By setting the amount of the particulate polymer within the above range, the above-described effects of the present invention can be effectively achieved. Furthermore, by setting the amount of the particulate polymer to be equal to or greater than the above lower limit, the components constituting the electrode mixture layer and the electrode mixture layer and the current collector can be effectively bound together, thereby increasing the peel strength of the electrode. Furthermore, by setting the amount of the particulate polymer to be equal to or less than the above upper limit, the productivity of the slurry composition and the cycle characteristics of the secondary battery can be ensured.
[0063] (Active Material) The active material that can be contained in the slurry composition of the present invention can be appropriately selected from materials used in ordinary non-aqueous secondary batteries. Examples of the negative electrode active material include carbon-based negative electrode active materials, non-carbon-based negative electrode active materials, and active materials that are combinations of these.
[0064] Examples of carbon-based negative electrode active materials include carbonaceous materials and graphitic materials. Carbonaceous materials are materials with a low degree of graphitization (i.e., low crystallinity) obtained by carbonizing a carbon precursor through heat treatment at 2000°C or less. The lower limit of the heat treatment temperature during carbonization is not particularly limited, but can be, for example, 500°C or higher. Examples of carbonaceous materials include graphitic carbon, whose carbon structure can be easily changed depending on the heat treatment temperature, and non-graphitic carbon, which has a structure similar to an amorphous structure, such as glassy carbon. Examples of graphitic carbon include carbon materials made from tar pitch obtained from petroleum or coal. Specific examples include coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fiber, and pyrolytic vapor-grown carbon fiber. Examples of non-graphitic carbon include phenolic resin sintered bodies, polyacrylonitrile-based carbon fiber, pseudoisotropic carbon, furfuryl alcohol resin (PFA) sintered bodies, and hard carbon.
[0065] The graphite material is a material with high crystallinity similar to that of graphite, obtained by heat-treating graphitizable carbon at 2000°C or higher. The upper limit of the heat treatment temperature is not particularly limited, but can be, for example, 5000°C or lower. Examples of graphite materials include natural graphite and artificial graphite. Examples of artificial graphite include artificial graphite obtained by heat-treating carbon containing graphitizable carbon mainly at 2800°C or higher, graphitized MCMB obtained by heat-treating MCMB at 2000°C or higher, and graphitized mesophase pitch-based carbon fiber obtained by heat-treating mesophase pitch-based carbon fiber at 2000°C or higher.
[0066] In addition to the above, known carbon-based negative electrode active materials include a composite carbon material described in JP 2013-45714 A, which is formed by forming a coating of low-crystalline carbon on the surface of core particles made of highly crystalline carbon.
[0067] The non-carbon-based negative electrode active material is an active material other than a carbon-based negative electrode active material, and examples of the non-carbon-based negative electrode active material include metal-based negative electrode active materials.
[0068] The metal-based negative electrode active material is an active material containing a metal, and usually refers to an active material that contains an element capable of inserting lithium in its structure and has a theoretical electric capacity per unit mass of 500 mAh / g or more when lithium is inserted. Examples of the metal-based negative electrode active material include lithium metal, elemental metals that can form lithium alloys (e.g., Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.), and alloys thereof, as well as oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. thereof.
[0069] Among metal-based negative electrode active materials, silicon-containing active materials (silicon-based negative electrode active materials) are preferred. This is because the use of silicon-based negative electrode active materials can increase the capacity of lithium-ion secondary batteries. Examples of silicon-based negative electrode active materials include silicon (Si), silicon-containing alloys, SiO, SiOx, and composites of Si-containing materials and conductive carbon, which are obtained by coating or compounding Si-containing materials with conductive carbon. Note that these silicon-based negative electrode active materials may be used alone or in combination of two or more types.
[0070] Examples of alloys containing silicon include alloy compositions containing silicon and at least one element selected from the group consisting of titanium, iron, cobalt, nickel, and copper. Examples of alloys containing silicon also include alloy compositions containing silicon, aluminum, and a transition metal such as iron, and further containing tin and a rare earth element such as yttrium.
[0071] SiOx is a compound containing at least one of SiO and SiO2 and Si, where x is usually 0.01 or more and less than 2. SiOx can be formed, for example, by utilizing the disproportionation reaction of silicon monoxide (SiO). Specifically, SiOx can be prepared by heat-treating SiO, optionally in the presence of a polymer such as polyvinyl alcohol, to produce silicon and silicon dioxide. The heat treatment can be carried out by pulverizing and mixing SiO and, optionally, a polymer, in an atmosphere containing organic gas and / or steam at a temperature of 900°C or higher, preferably 1000°C or higher.
[0072] Examples of composites of Si-containing materials and conductive carbon include compounds obtained by heat-treating a pulverized mixture of SiO, a polymer such as polyvinyl alcohol, and optionally a carbon material in an atmosphere containing an organic gas and / or steam. Furthermore, composites can also be obtained by known methods, such as a method of coating the surfaces of SiO particles with an organic gas or the like by chemical vapor deposition, or a method of forming composite particles (granulation) from SiO particles and graphite or artificial graphite by mechanochemical treatment.
[0073] When the electrode slurry composition of the present invention is a negative electrode slurry composition containing both a carbonaceous negative electrode active material and a non-carbonaceous negative electrode active material, the proportion of the non-carbonaceous negative electrode active material in the total of 100 mass % is preferably more than 0 mass % and 20 mass % or less. By setting the proportion in this manner, the effects of the present invention can be favorably obtained.
[0074] (Preparation of Slurry Composition) The slurry composition for a secondary battery electrode of the present invention can be prepared by dispersing the above-mentioned components in an aqueous medium as a dispersion medium. Specifically, the slurry composition can be prepared by mixing the above-mentioned components with the aqueous medium using a mixer such as a ball mill, sand mill, bead mill, pigment disperser, crusher, ultrasonic disperser, homogenizer, planetary mixer, or Filmix. Here, water is typically used as the aqueous medium, but an aqueous solution of any compound or a mixed solution of a small amount of organic medium and water may also be used. The solids concentration of the slurry composition can be a concentration that allows the components to be uniformly dispersed, for example, 30% by mass to 90% by mass. Furthermore, the mixing of the above-mentioned components with the aqueous medium can typically be performed at a temperature range of room temperature to 80°C for 10 minutes to several hours.
[0075] (Secondary Battery Electrode) The secondary battery electrode of the present invention can be manufactured using the slurry composition for a secondary battery electrode of the present invention. Here, the secondary battery electrode of the present invention comprises a current collector and an electrode mixture layer formed on the current collector, and the electrode mixture layer is obtained from the slurry composition for a secondary battery electrode of the present invention. Note that the components contained in the electrode mixture layer are the same as those contained in the slurry composition for a secondary battery electrode of the present invention, and the preferred abundance ratios of the components are the same as the preferred abundance ratios of the components in the slurry composition for a secondary battery electrode. Furthermore, the secondary battery electrode of the present invention can suppress cell swelling of the secondary battery while allowing the secondary battery to exhibit excellent cycle characteristics.
[0076] (Method for manufacturing electrode for secondary battery) The electrode for secondary battery of the present invention is manufactured, for example, through a step of applying the above-described slurry composition for a secondary battery electrode onto a current collector (application step), and a step of drying the slurry composition for a secondary battery electrode applied onto the current collector to form an electrode mixture layer on the current collector (drying step).
[0077] (Coating Step) The method for applying the slurry composition for a secondary battery electrode onto a current collector is not particularly limited, and known methods can be used. Specifically, examples of the coating method include a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, and a brush coating method. In this case, the slurry composition may be applied to only one side of the current collector, or may be applied to both sides. The thickness of the slurry film on the current collector after application and before drying can be appropriately set depending on the thickness of the electrode mixture layer obtained by drying.
[0078] Here, a material having electrical conductivity and electrochemical durability is used as the current collector to which the slurry composition is applied. Specifically, the current collector may be made of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, or the like. Among these, copper foil is particularly preferred as the current collector used for the electrode. Note that the above-mentioned materials may be used alone or in combination of two or more types in any ratio.
[0079] (Drying step) The method for drying the slurry composition on the current collector is not particularly limited and any known method can be used, for example, drying with warm air, hot air, or low-humidity air, vacuum drying, or drying by irradiation with infrared rays or electron beams, etc. By drying the slurry composition on the current collector in this manner, an electrode mixture layer can be formed on the current collector, and a secondary battery electrode including the current collector and the electrode mixture layer can be obtained.
[0080] After the drying step, the electrode mixture layer may be subjected to pressure treatment using a mold press, a roll press, etc. Pressure treatment can improve the peel strength of the electrode.
[0081] (Secondary Battery) The secondary battery of the present invention comprises a positive electrode, a negative electrode, an electrolyte, and a separator, and uses the secondary battery electrode of the present invention as at least one of the positive electrode and the negative electrode. Because the secondary battery of the present invention uses the secondary battery electrode of the present invention, cell swelling is suppressed and the battery characteristics, such as rate characteristics, are excellent. Below, the positive electrode, electrolyte, and separator will be described using an example in which the secondary battery is a lithium ion secondary battery and the negative electrode is the secondary battery electrode of the present invention, but the present invention is not limited to these examples.
[0082] (Positive Electrode) As the positive electrode, a known positive electrode used as a positive electrode for a lithium ion secondary battery can be used. Specifically, as the positive electrode, for example, a positive electrode formed by forming a positive electrode composite layer on a current collector can be used. Note that the current collector can be made of a metal material such as aluminum. Furthermore, as the positive electrode composite layer, a layer containing a known positive electrode active material, a conductive material, and a binder can be used.
[0083] (Electrolyte) The electrolyte may be an electrolyte solution prepared by dissolving an electrolyte in a solvent. Here, an organic solvent capable of dissolving the electrolyte may be used as the solvent. Specifically, the solvent may be an alkyl carbonate solvent such as ethylene carbonate, propylene carbonate, or γ-butyrolactone to which a viscosity-adjusting solvent such as 2,5-dimethyltetrahydrofuran, tetrahydrofuran, diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, methyl acetate, dimethoxyethane, dioxolane, methyl propionate, or methyl formate has been added. The electrolyte may be a lithium salt. For example, the lithium salts described in JP 2012-204303 A may be used. Among these lithium salts, LiPF6, LiClO4, and CF3SO3Li are preferred as electrolytes because they are easily soluble in organic solvents and exhibit a high degree of dissociation.
[0084] (Separator) As the separator, for example, those described in JP 2012-204303 A can be used. Among these, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred because it allows the thickness of the entire separator to be thin, thereby increasing the ratio of electrode active material in the lithium ion secondary battery and increasing the capacity per volume.
[0085] (Method for manufacturing secondary battery) The secondary battery of the present invention can be manufactured, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, rolling or folding the resulting assembly as needed according to the battery shape, placing it in a battery container, injecting an electrolyte into the battery container, and sealing it. To prevent internal pressure rise and overcharging / discharging, etc., a fuse, an overcurrent prevention element such as a PTC element, an expanded metal, a lead plate, etc. may be provided as needed. The shape of the secondary battery may be, for example, any of a coin type, a button type, a sheet type, a cylindrical type, a rectangular type, a flat type, etc.
[0086] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified. Furthermore, the operations described below were performed under conditions of room temperature and normal pressure unless otherwise specified.
[0087] [Evaluation Method] (Oxidation-Reduction Potential) 50 g of the binder composition was placed in a sealed thermostatic chamber at 25°C and left for 30 minutes, and then a platinum composite ORP electrode (HORIBA, Ltd., composite electrode 9300-10D) was immersed in the binder composition to measure the oxidation-reduction potential (mV).
[0088] (Amount of Surface Acid of Particulate Polymer and Amount of Acid of Aqueous Phase of Binder Composition) The amount of surface acid (mmol / g) of the particulate polymer per 1 g of solid content of the binder composition and the amount of acid (mmol / g) in the aqueous phase of the binder composition per 1 g of solid content of the binder composition were measured by the following procedure. A 150 ml glass container was washed with distilled water. 50 g of the binder composition diluted with water to a solid content concentration of 2% was placed in this container, and the container was set in a solution conductivity meter (Kyoto Electronics Manufacturing Co., Ltd.: CM-117, cell type: K-121) and stirred. Stirring was continued until the addition of hydrochloric acid was completed. 0.1 N sodium hydroxide (Wako Pure Chemical Industries: special grade reagent) was added to the binder composition so that the electrical conductivity of the binder composition would be 2.5 to 3.0 (mS), and then the electrical conductivity was measured 6 minutes later. This value was defined as the electrical conductivity at the start of the measurement. To this binder composition, 0.5 ml of 0.1 N hydrochloric acid (Wako Pure Chemical Industries, Ltd.: special grade reagent) was added, and the electrical conductivity was measured 30 seconds later. Immediately after the measurement, 0.5 ml of 0.1 N hydrochloric acid was added again, and the electrical conductivity was measured 30 seconds later. In this manner, the addition of hydrochloric acid and the measurement of the electrical conductivity 30 seconds later were repeated until the electrical conductivity of the binder composition reached or exceeded the electrical conductivity at the start of the measurement.
[0089] Generally, when such titration is performed on a binder composition in which acid is present on both the particulate polymer surface and the aqueous phase, and the resulting electrical conductivity data is plotted on a graph with electrical conductivity (mS) on the vertical axis and the cumulative amount (mmol) of hydrochloric acid added on the horizontal axis, a hydrochloric acid amount-electrical conductivity curve having three change points (points where the graph bends) is obtained, as shown in Figure 1. The X coordinates of the three change points and the X coordinate at the end of hydrochloric acid addition were designated P1, P2, P3, and P4, respectively, in order from smallest to largest. Approximate straight lines L1, L2, L3, and L4 were determined by the least squares method for the data in each of the X coordinate sections from zero to P1, P1 to P2, P2 to P3, and P3 to P4. The X coordinate of the intersection of L1 and L2 was designated A1 (mmol), the X coordinate of the intersection of L2 and L3 was designated A2 (mmol), and the X coordinate of the intersection of L3 and L4 was designated A3 (mmol).
[0090] The amount of surface acid of the particulate polymer per 1 g of solid content of the binder composition and the amount of acid in the aqueous phase of the binder composition per 1 g of solid content of the binder composition were calculated as milliequivalents (mmol / g) converted to hydrochloric acid using the formulas (a) and (b), respectively. Formula (a): Amount of surface acid of the particulate polymer per 1 g of solid content of the binder composition (mmol / g) = (A2 - A1) / (mass of solid content of binder composition (g)) Formula (b): Amount of acid in the aqueous phase per 1 g of solid content of the binder composition (mmol / g) = (A3 - A2) / (mass of solid content of binder composition (g))
[0091] (Metal Content) The metal content of the binder composition was measured using ICP-MS. The metal elements measured were Fe, Cu, Zn, Co, Ni, and Cr.
[0092] (Peel Strength) The fabricated negative electrode for a lithium ion secondary battery was cut out to obtain a rectangular test piece measuring 1.0 cm wide x 10 cm long. The test piece was fixed with the surface facing the negative electrode composite layer facing up. Cellophane tape was then applied to the surface of the negative electrode composite layer of the test piece. The cellophane tape used was specified in JIS Z1522. The stress was then measured when the cellophane tape was peeled from one end of the test piece in a 180° direction (toward the other end of the test piece) at a rate of 50 mm / min. The measurement was performed 10 times, and the average stress was calculated. This was designated as the peel strength (N / m) and evaluated according to the following criteria. A higher peel strength indicates better adhesion of the negative electrode composite layer to the current collector. A: Peel strength is 8 N / m or more. B: Peel strength is 5 N / m or more and less than 8 N / m. C: Peel strength is 3 N / m or more and less than 5 N / m. D: Peel strength is less than 3 N / m.
[0093] (Storage Stability) The viscosity (unit: mPa s) of the binder composition was measured using a Brookfield viscometer, and then the composition was stored in an oven heated to 40°C for one week. After storage, the viscosity was measured again using the Brookfield viscometer, and the viscosity change was calculated using the following formula and evaluated according to the following evaluation criteria: Viscosity change (%) = (viscosity of binder composition after storage) / (viscosity of binder composition before storage) × 100 A: Less than 110% B: 110% or more and less than 120% C: 120% or more and less than 130% D: 130% or more
[0094] (Cycle Characteristics) The secondary battery was left standing at 25°C for 6 hours. It was then charged for 100 minutes at 0.1 C in a 25°C environment. It was then aged for 12 hours at 60°C. It was then charged to a cell voltage of 4.20 V at 0.5 C in a 25°C environment, and discharged to a cell voltage of 2.75 V, and the initial capacity C0 was measured. This charge / discharge cycle was further repeated, and the capacity C1 after 50 cycles was measured. The capacity retention C2 was then calculated according to the following formula: C2 (%) = (C1 / C0) x 100. A larger value for the capacity retention C2 indicates better cycle characteristics. A: Capacity retention C2 is 90% or more. B: Capacity retention C2 is 85% or more but less than 90%. C: Capacity retention C2 is 80% or more but less than 85%. D: Capacity retention C2 is less than 80%.
[0095] (Example 1) (1-1. Preparation of Particulate Polymer A) 99 parts of a monomer composition, 0.25 parts of tert-dodecyl mercaptan as a chain transfer agent, and 0.35 parts of sodium lauryl sulfate as an emulsifier were placed in a container A to prepare a mixture containing a monomer composition. The monomer composition was a composition consisting of 42.0 parts of styrene as an aromatic vinyl monomer, 54.0 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, and 3.0 parts of itaconic acid as an acidic group-containing monomer. Meanwhile, 1 part of potassium persulfate was prepared as a polymerization initiator.
[0096] The mixture was gradually added from vessel A to pressure vessel B, and at the same time, the polymerization initiator was gradually added to pressure vessel B to initiate the polymerization reaction. The reaction temperature was maintained at 75°C.
[0097] After adding about 70% of the entire monomer composition, 1 part of 2-hydroxyethyl acrylate as a hydroxyl group-containing (meth)acrylic acid ester monomer was gradually added to pressure vessel B. Five and a half hours after the start of polymerization, the addition of the entire amount of the monomer composition was completed, and then the mixture was further heated to 85°C to continue the reaction.
[0098] When the polymerization conversion rate reached 97%, the mixture was cooled to stop the reaction, and a mixture containing a particulate polymer was obtained. A 5% aqueous solution of sodium hydroxide was added to the mixture containing the particulate polymer to adjust the pH to 8. Thereafter, unreacted monomers were removed by heating and vacuum distillation. Thereafter, the mixture was further cooled to obtain an aqueous dispersion containing particulate polymer A.
[0099] (1-2. Preparation of Water-Soluble Polymer) 100 parts of a monomer composition for a water-soluble polymer was placed in a polymerization vessel, and the temperature inside the system was raised to 85° C. The monomer composition for the water-soluble polymer was a composition consisting of 75.0 parts of acrylic acid as a (meth)acrylic acid monomer and 25.0 parts of acrylonitrile as a nitrile group-containing vinyl monomer.
[0100] During the temperature increase, when the temperature in the system reached 60°C, 1.3 parts of 2,2'-azobis(2-methyl-N-2-hydroxyethylpropionamide) was added as a polymerization initiator. Thereafter, the mixture was stirred at a temperature of 85°C. When the monomer conversion rate reached 90% or more, the mixture was cooled to terminate the reaction. Thereafter, the pH was adjusted to 8.0 with a 4% aqueous sodium hydroxide solution, and unreacted monomer was removed by heating and distillation under reduced pressure, yielding an aqueous solution of a water-soluble polymer.
[0101] (1-3. Binder Composition) 0.5 parts (based on the mass of the water-soluble polymer) of the aqueous solution of the water-soluble polymer obtained in (1-2) was added to 100 parts (based on the solid content) of the aqueous dispersion containing the particulate polymer A obtained in (1-1), and the mixture was passed through a magnetic filter. Water was further added to adjust the concentration. In this way, an aqueous dispersion containing the particulate polymer A and the water-soluble polymer was obtained as a binder composition. The solid content concentration of the binder composition was set to 40%. The oxidation-reduction potential, surface acid amount, acid amount in the aqueous phase, and metal content of this binder composition were measured. In addition, the storage stability of this binder composition was evaluated. The results are shown in Table 1.
[0102] (1-4. Carbon-Based Negative Electrode Active Material) As a carbon-based negative electrode active material, artificial graphite (average particle size: 24.5 μm, graphite interlayer distance (plane spacing (d value) of (002) plane by X-ray diffraction method): 0.354 nm) was prepared.
[0103] (1-5. Slurry Composition for Lithium-Ion Secondary Battery Negative Electrode) In a planetary mixer equipped with a disperser, 85 parts of the carbon-based negative electrode active material A obtained in (1-4) as a negative electrode active material, 15 parts of a silicon-carbon composite active material as a Si-based active material, 1.5 parts in terms of solid content of carboxymethyl cellulose (viscosity of 1% by mass aqueous solution: 250 mPa s), and acetylene black (BET specific surface area: 68 m) as a conductive material were added. 2 1 part of ethanol (1 / g) was added. The mixture was adjusted to a solids concentration of 56% with ion-exchanged water, and then mixed at 25° C. for 60 minutes. Next, the mixture was adjusted to a solids concentration of 52% with ion-exchanged water, and then further mixed at 25° C. for 15 minutes to obtain a mixed solution.
[0104] To the above mixture, 1.6 parts of the binder composition obtained in (1-3) in terms of solid content (i.e., based on the mass of the particulate polymer A) and ion-exchanged water were added to adjust the final solid content concentration to 50%, and the mixture was further mixed for 10 minutes. This was subjected to a degassing treatment under reduced pressure to obtain a slurry composition for a lithium-ion secondary battery negative electrode.
[0105] (1-6. Lithium-ion secondary battery negative electrode) The slurry composition for lithium-ion secondary battery negative electrode obtained in (1-5) was applied to a copper foil current collector having a thickness of 15 μm using a comma coater in an amount of 9 to 10 mg / cm. 2 The copper foil coated with the lithium ion secondary battery negative electrode slurry composition was dried by conveying it at a speed of 0.5 m / min through an oven at a temperature of 60° C. for 2 minutes. Thereafter, the copper foil was heat-treated in an oven at a temperature of 120° C. for 2 minutes to obtain a negative electrode blank.
[0106] The obtained negative electrode blank was pressed with a roll press until the density of the negative electrode mixture layer was 1.6 to 1.7 g / cm 3 The negative electrode for a lithium ion secondary battery was then pressed so that the peel strength was 0.01 mm. The peel strength of the negative electrode for a lithium ion secondary battery was evaluated. The results are shown in Table 1.
[0107] (1-7. Lithium-ion secondary battery positive electrode) A planetary mixer was used, and LiCoO 2A slurry composition for a lithium ion secondary battery positive electrode was prepared by mixing 100 parts of cellulose acetate, 2 parts of acetylene black (HS-100, manufactured by Denki Kagaku Kogyo Co., Ltd.) as a conductive material, 2 parts of PVDF (polyvinylidene fluoride, KF-1100, manufactured by Kureha Chemical Co., Ltd.) as a binder, and further adding 2-methylpyrrolidinone so that the total solids concentration was 67%.
[0108] The obtained slurry composition for lithium ion secondary battery positive electrodes was applied to a 20 μm-thick aluminum foil current collector using a comma coater. The aluminum foil coated with the slurry composition for lithium ion secondary battery positive electrodes was dried by conveying it at a speed of 0.5 m / min in an oven at a temperature of 60° C. for 2 minutes. Thereafter, the aluminum foil was heat-treated in an oven at a temperature of 120° C. for 2 minutes to obtain a positive electrode blank.
[0109] The obtained positive electrode raw sheet is pressed with a roll press until the density of the positive electrode mixture layer becomes 3.40 to 3.50 g / cm 3 The electrode was pressed to obtain a positive electrode for a lithium ion secondary battery.
[0110] (1-8. Lithium-ion secondary battery) A single-layer polypropylene separator (width 65 mm, length 500 mm, thickness 25 μm; produced by a dry process; porosity 55%) was cut out to obtain a 50 mm × 200 mm rectangular separator. The positive electrode obtained in (1-7) was cut out to obtain a 45 mm × 150 mm rectangular positive electrode. The negative electrode obtained in (1-6) was cut out to obtain a 47 mm × 155 mm rectangular negative electrode.
[0111] A rectangular positive electrode, a rectangular separator, and a rectangular negative electrode were stacked in this order with their longitudinal directions aligned, and then wound up to prepare a wound body.
[0112] The wound body was placed in an aluminum packaging. Then, LiPF 5 with a concentration of 1.0 M was added as an electrolyte to the aluminum packaging. 6A solution (the solvent was a mixed solvent of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (volume ratio), containing 2 mass% vinylene carbonate as an additive) was filled into the battery. The opening of the aluminum packaging exterior was then sealed by heat sealing at 150°C, thereby producing a lithium ion secondary battery. The capacity retention rate of the obtained lithium ion secondary battery was evaluated. The results are shown in Table 1.
[0113] (Example 2) In the preparation of the water-soluble polymer (1-2), a composition consisting of only 100.0 parts of acrylic acid (not containing acrylonitrile) was used as the monomer composition for the water-soluble polymer, and the same procedures as in Example 1 were carried out to obtain and evaluate a binder composition, a negative electrode, and a lithium ion secondary battery. The results are shown in Table 1.
[0114] (Example 3) (3-1. Particulate Polymer B - Binder Composition) 100 parts of a monomer composition, 0.25 parts of tert-dodecyl mercaptan as a chain transfer agent, and 0.35 parts of sodium lauryl sulfate as an emulsifier were placed in a container A to prepare a mixture containing a monomer composition. The monomer composition was a composition consisting of 35.0 parts of styrene as an aromatic vinyl monomer, 51.0 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 10.0 parts of acrylonitrile as a nitrile group-containing vinyl monomer, and 4.0 parts of itaconic acid as an acidic group-containing monomer. Meanwhile, 1 part of potassium persulfate was prepared as a polymerization initiator.
[0115] The mixture was gradually added from vessel A to pressure vessel B, and at the same time, the polymerization initiator was gradually added to pressure vessel B, thereby initiating the polymerization reaction. The reaction temperature was maintained at 75°C. Five and a half hours after the start of polymerization, the addition of all of the monomer compositions was completed, and the mixture was then further heated to 85°C and reacted for 6 hours.
[0116] When the polymerization conversion rate reached 97%, the mixture was cooled to stop the reaction, yielding a mixture containing a particulate polymer. A 5% aqueous sodium hydroxide solution was added to the mixture containing the particulate polymer, adjusting the pH to 8. Unreacted monomers were then removed by heating and vacuum distillation. The mixture was then cooled and passed through a magnetic filter. This yielded an aqueous dispersion containing particulate polymer B as a binder composition. The solids concentration of the binder composition was 40%. The oxidation-reduction potential, surface acid amount, aqueous acid amount, and metal content of this binder composition were measured. Additionally, the storage stability of this binder composition was evaluated. The results are shown in Table 1.
[0117] (3-2. Negative electrode and lithium ion secondary battery) A negative electrode and a lithium ion secondary battery were obtained and evaluated in the same manner as in (1-4) to (1-8) of Example 1, except that the binder composition obtained in (3-1) was used instead of the binder composition obtained in (1-3) of Example 1. The results are shown in Table 1.
[0118] (Example 4) (4-1. Particulate polymer C) In a reactor equipped with a stirrer, 96.0 parts of butyl acrylate as a (meth)acrylic acid ester monomer, 2.0 parts of acrylonitrile as a vinyl cyanide monomer, 2.0 parts of methacrylic acid as an acidic group-containing monomer, 0.3 parts of sodium dodecylbenzenesulfonate as an emulsifier, 0.3 parts of ammonium persulfate as a polymerization initiator, and 300 parts of ion-exchanged water were placed, thoroughly stirred, and then heated to 70 ° C. to proceed with the reaction for 4 hours, and further heated to 80 ° C. and aged for 3 hours to complete the reaction. Thereafter, the reaction mixture was cooled to 30 ° C. or less, and an aqueous dispersion containing particulate polymer C was obtained.
[0119] (4-2. Binder Composition) 90.0 parts (based on the mass of the particulate polymer) of the aqueous dispersion containing the particulate polymer A obtained in (1-1) of Example 1 and 10.0 parts (based on the mass of the particulate polymer) of the aqueous dispersion containing the particulate polymer C obtained in (4-1) were mixed and then passed through a magnetic filter. As a result, an aqueous dispersion containing the particulate polymers A and C was obtained as a binder composition.
[0120] (4-3. Negative electrode and lithium ion secondary battery) A negative electrode and a lithium ion secondary battery were obtained and evaluated in the same manner as in (1-4) to (1-8) of Example 1, except that the binder composition obtained in (4-2) was used instead of the binder composition obtained in (1-3) of Example 1. The results are shown in Table 1.
[0121] (Example 5) In preparing the particulate polymer B of (3-1), a composition consisting of 9.0 parts of styrene, 56.0 parts of butadiene, 25.0 parts of acrylonitrile, and 10.0 parts of acrylic acid was used as the monomer composition, and the same operation as in Example 3 was used to obtain a binder composition, a negative electrode, and a lithium ion secondary battery, and the evaluations were carried out. The results are shown in Table 1.
[0122] (Comparative Example 1) In preparing the particulate polymer B of (3-1), a composition consisting of 51.0 parts of styrene, 49.0 parts of butadiene and 0.1 parts of itaconic acid was used as the monomer composition in a total amount of 100.1 parts, and the same operation as in Example 3 was carried out to obtain a binder composition, a negative electrode and a lithium ion secondary battery, and the evaluations were carried out. The results are shown in Table 1.
[0123] (Comparative Example 2) In preparing the particulate polymer B of (3-1), a composition consisting of 45.0 parts of styrene, 40.0 parts of butadiene, 3.0 parts of methyl methacrylate and 12.0 parts of acrylic acid was used as the monomer composition, and the same operation as in Example 3 was used to obtain a binder composition, a negative electrode and a lithium ion secondary battery, and the evaluations were carried out. The results are shown in Table 1.
[0124] (Comparative Example 3) A binder composition, a negative electrode, and a lithium ion secondary battery were obtained and evaluated by the same procedures as in Example 3, except for the following changes. The results are shown in Table 1. In preparing the particulate polymer B of (3-1), a composition consisting of 24.0 parts of styrene, 72.0 parts of butadiene, and 4.0 parts of itaconic acid was used as the monomer composition. In preparing the particulate polymer B of (3-1), the step of passing through a magnetic filter was not performed.
[0125] Comparative Example 4 A binder composition, a negative electrode, and a lithium ion secondary battery were obtained and evaluated in the same manner as in Example 1, except that in the preparation of the water-soluble polymer of (1-2), a composition consisting of 40.0 parts of acrylic acid and 60.0 parts of acrylonitrile was used as the monomer composition for the water-soluble polymer. The results are shown in Table 1.
[0126]
[0127] St parts by mass: parts by mass of styrene used BD parts by mass: parts by mass of 1,3-butadiene used Ester parts by mass: parts by mass of (meth)acrylic acid ester monomer (2-hydroxyethyl acrylate) used Other (AN) parts by mass: parts by mass of other monomers (acrylonitrile) used Acidic group-containing monomer parts by mass: parts by mass of acidic group-containing monomers (itaconic acid, methacrylic acid, acrylic acid) used AA parts by mass: parts by mass of acrylic acid used AN parts by mass: parts by mass of acrylonitrile used Metal content (ppm): contents of Fe, Cu, Zn, Co, Ni, and Cr measured using ICP-MS. "0.5>": All less than 0.5 ppm. "1.0>": Any one or more elements are 0.5 ppm or more and less than 1.0 ppm.
[0128] From the above results, it can be seen that the binder compositions of the Examples have higher storage stability than the binder compositions of the Comparative Examples, and can realize electrodes with excellent peel properties, and can also realize nonaqueous secondary batteries with excellent cycle properties.
[0129] In addition to the above evaluations, the degree of roll contamination during the pressing operation using a roll press machine in the production of the negative electrode was visually evaluated. As a result, there was no contamination and good pressing operation was possible in Examples 1 to 5, Comparative Example 1, and Comparative Example 4, but the roll was contaminated and required frequent cleaning in Comparative Examples 2 and 3. Furthermore, such roll contamination is thought to be one of the causes of the decrease in peel strength.
Claims
1. A binder composition for a non-aqueous secondary battery electrode, comprising a particulate polymer and a dispersion medium, and having an aqueous phase and a solid phase, wherein the binder composition has an oxidation-reduction potential value of 90 to 280 mV, and the sum of the amount of acid on the surface of the particulate polymer and the amount of acid in the aqueous phase is 0.15 mmol / g or more and 1.5 mmol / g or less.
2. A binder composition for non-aqueous secondary battery electrodes according to claim 1, wherein the content of Fe, Cu, Zn, Co, Ni and Cr is each less than 0.5 ppm.
3. The binder composition for a non-aqueous secondary battery electrode according to claim 1, wherein the amount of acid contained in the aqueous phase divided by the sum of the amount of acid on the surface of the particulate polymer and the amount of acid in the aqueous phase is 0.2 or more and 0.6 or less.
4. The binder composition for a non-aqueous secondary battery electrode according to claim 1, wherein the particulate polymer contains at least one selected from the group consisting of styrene monomer units, butadiene monomer units, (meth)acrylic acid ester monomer units, and acidic group-containing monomer units.
5. The binder composition for a non-aqueous secondary battery electrode according to claim 1, further comprising a water-soluble polymer.
6. A slurry composition for a non-aqueous secondary battery electrode, comprising an electrode active material and the binder composition for a non-aqueous secondary battery electrode according to any one of claims 1 to 5.
7. A non-aqueous secondary battery electrode comprising an electrode mixture layer formed using the slurry composition for a non-aqueous secondary battery electrode according to claim 6.
8. A non-aqueous secondary battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein at least one of the positive electrode and the negative electrode is the electrode for a non-aqueous secondary battery according to claim 7.
Citation Information
Patent Citations
Electrode for secondary battery, and secondary battery
WO2011001848A1
Method for preserving aqueous binder composition for lithium secondary cell
WO2015029835A1
Binder composition for lithium ion secondary battery, slurry composition for lithium ion secondary battery, method for manufacturing electrode for secondary battery, and lithium ion secondary battery
WO2015098507A1
Binder composition for lithium ion secondary battery electrode, slurry composition for lithium ion secondary battery negative electrode, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
WO2015129257A1