Method for manufacturing electrode assembly for secondary battery and method for manufacturing secondary battery including same
The method addresses non-uniformity in secondary battery electrode assemblies by varying active material loading and density in the electrode assembly's active material layer, ensuring uniformity and preventing winding-induced stress, thereby enhancing energy density and lifespan.
Patent Information
- Application Number
- PCT/KR2024/005272
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
AI Technical Summary
Secondary battery electrode assemblies with active material layers wound in a jelly-roll form often experience non-uniform active material density, leading to uneven energy density and lifespan characteristics due to winding-induced stress and material distribution deviations.
A method of manufacturing an electrode assembly with a preliminary electrode having regionally varied active material loading and density, where the active material layer is formed with a higher loading and density at one end and lower at the other, and potentially including intermediate regions to buffer changes, ensuring uniformity and preventing cracking during winding. This involves forming active material layers on both surfaces of the current collector and using different solvents for the slurry applications to maintain uniformity and prevent mixing disturbances.
The method achieves a substantially uniform active material density across the wound electrode assembly, enhancing both energy density and lifespan characteristics by distributing stress evenly and preventing peeling or cracking, thus improving the performance and reliability of secondary batteries.
Smart Images

Figure KR2024005272_24102024_PF_FP_ABST
Abstract
Description
Method for manufacturing an electrode assembly for a secondary battery and method for manufacturing a secondary battery including the same
[0001] The present disclosure relates to a method for manufacturing an electrode assembly for a secondary battery and a method for manufacturing a secondary battery including the electrode assembly for a secondary battery. More specifically, the present disclosure relates to a method for manufacturing an electrode assembly for a secondary battery having active material layers formed on both sides of a current collector and a secondary battery including the electrode assembly for a secondary battery.
[0002]
[0003] Secondary batteries, which can be repeatedly charged and discharged, are widely used as power sources for portable electronic communication devices such as camcorders, mobile phones, and laptops, thanks to the advancements in the information and communication and display industries. Furthermore, battery packs containing secondary batteries are being developed and applied as power sources for eco-friendly vehicles such as hybrid vehicles.
[0004] Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, and nickel-hydrogen batteries. Among these, lithium secondary batteries are being actively developed and applied due to their high operating voltage and energy density per unit weight, and their advantages in charging speed and weight reduction.
[0005] For example, a secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator, and an electrolyte that impregnates the electrode assembly. The secondary battery may further include an outer packaging material, for example, in the form of a pouch, that accommodates the electrode assembly and the electrolyte.
[0006] The above electrode assembly may have, for example, a jelly-roll shape in which the positive and negative electrodes are wound with a separator interposed therebetween.
[0007] However, the jelly roll-shaped electrode assembly may have a non-uniform active material density due to winding, which may result in non-uniform energy density and lifespan characteristics.
[0008]
[0009] An object of the present disclosure is to provide a method for manufacturing an electrode assembly for a secondary battery having improved life characteristics and energy density.
[0010] One object of the present disclosure is to provide a method for manufacturing a secondary battery including the electrode assembly for the secondary battery.
[0011]
[0012] In a method for manufacturing an electrode assembly for a secondary battery according to exemplary embodiments, an electrode current collector may be prepared. An active material layer including a first region on one end of the electrode current collector and a second region having a higher active material loading amount and density than the first region on the other end of the electrode current collector may be formed to form a reserve electrode. The reserve electrode may be wound together with the active material layer around the one end of the electrode current collector to form a wound electrode including a wound active material layer.
[0013] In some embodiments, the active material layer may include an intermediate region formed between the first region and the second region and having a greater active material loading amount and density than the first region and a lower active material loading amount and density than the second region.
[0014] In some embodiments, the active material layer may be formed such that the active material loading amount and density gradually or stepwise increase from the first region toward the second region.
[0015] In some embodiments, the active material loading amount and density of the winding active material layer can be uniform over the entire area of the electrode current collector.
[0016] In some embodiments, the thickness of the active material layer included in the preliminary electrode may be uniform over the entire area of the electrode current collector.
[0017] In some embodiments, forming the active material layer includes forming an upper active material layer and a lower active material layer on the upper and lower surfaces of the electrode current collector, respectively, and the average active material loading amount and average density of the lower active material layer may be smaller than those of the upper active material layer.
[0018] In some embodiments, winding the spare electrode may include winding the lower active material layer inward.
[0019] In some embodiments, forming the active material layer may include forming a first active material layer on a surface of the electrode current collector, and forming a second active material layer on the first active material layer, the second active material layer being spaced apart from the electrode current collector and the first active material layer.
[0020] In some embodiments, the active material loading amount in the first region of the first active material layer may be less than the active material loading amount in the second region, and the active material loading amount in the first region of the second active material layer may be greater than the active material loading amount in the second region.
[0021] In some embodiments, the thickness of the first active material layer in the first region may be smaller than the thickness in the second region, and the thickness of the second active material layer in the first region may be larger than the thickness in the second region.
[0022] In some embodiments, the active material loading amount of the first active material layer may gradually or stepwise increase from the first region to the second region, and the active material loading amount of the second active material layer may gradually or stepwise decrease from the first region to the second region.
[0023] In some embodiments, forming the first active material layer may include applying a first slurry comprising a first solvent and the active material, and forming the second active material layer may include applying a second slurry comprising a second solvent different from the first solvent and the active material on the first active material layer.
[0024] In some embodiments, the density of the first solvent may be greater than the density of the second solvent.
[0025] In some embodiments, the method may further include disposing the spare electrodes on the first and second opposing sides of the separator, respectively, and the separator may be wound together with the spare electrodes.
[0026] A method for manufacturing a secondary battery according to exemplary embodiments can prepare an electrode assembly manufactured according to the method for manufacturing an electrode assembly for a secondary battery. The electrode assembly can be accommodated in a case.
[0027]
[0028] According to exemplary embodiments, the active material layer of the pre-coil electrode can be formed to have a lower active material loading and density in a region including the center of the coiling than in a region including the end of the coiling. Accordingly, for example, a coiled electrode in a jelly roll state can have a substantially uniform active material density across the entire region. Accordingly, stress generated during the coiling operation can be distributed, thereby preventing cracking and detachment of the active material layer. Furthermore, the energy density and lifespan characteristics of the secondary battery can be uniform.
[0029] According to exemplary embodiments, the active material loading amount and density of the lower active material layer disposed inward during the winding operation can be reduced. Accordingly, the density of the winding active material layers disposed on the outer and inner sides of the winding can be substantially uniformly controlled, and electrode cracking / peeling due to variations in the distribution of the active material within the jelly roll can be prevented. Accordingly, the energy density and life characteristics of the secondary battery can be uniform.
[0030] In some embodiments, the active material layer may be formed to include a first active material layer and a second active material layer sequentially formed on the electrode current collector. The active material loading amounts of the first active material layer and the second active material layer may be gradually or stepwise changed from a first region corresponding to the winding center to a second region corresponding to the winding end. By utilizing a multi-layer structure, the density in the active material layer of the above-described preliminary electrode may be more uniform. In addition, by using different solvents in the slurries for forming the first active material layer and the second active material layer, mixing of the active materials and density disturbance between the first active material layer and the second active material layer may be prevented.
[0031] The method for manufacturing an electrode assembly for a secondary battery of the present disclosure and the secondary battery manufactured according to the method for manufacturing a secondary battery can be widely applied in green technology fields such as electric vehicles, battery charging stations, and other fields utilizing batteries, such as solar power generation and wind power generation. The negative active material for a lithium secondary battery of the present disclosure, the method for manufacturing the same, and the lithium secondary battery including the same can be used in eco-friendly electric vehicles, hybrid vehicles, etc. to prevent climate change by suppressing air pollution and greenhouse gas emissions.
[0032]
[0033] FIG. 1 and FIG. 2 are drawings for explaining a method for manufacturing an electrode assembly for a secondary battery according to exemplary embodiments.
[0034] Figures 3 and 4 are schematic cross-sectional views showing a spare electrode according to some exemplary embodiments.
[0035] FIG. 5 is a schematic plan view showing a secondary battery according to exemplary embodiments.
[0036]
[0037] Embodiments of the present disclosure provide a method for manufacturing an electrode assembly for a secondary battery, including winding a spare electrode having a region-specific variation in the loading amount or density of an active material layer. In addition, a method for manufacturing a secondary battery including the electrode assembly for a secondary battery is provided.
[0038] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the drawings. However, the following drawings attached to this disclosure illustrate preferred embodiments of the present disclosure and serve to further understand the technical concepts of the present disclosure. Therefore, this disclosure should not be interpreted as being limited to the matters described in such drawings.
[0039] The terms “upper”, “lower”, “top surface”, “lower surface”, etc. used in this disclosure are used in a relative sense to distinguish the positions of the components, and do not specify absolute positions.
[0040] FIG. 1 and FIG. 2 are drawings for explaining a method for manufacturing an electrode assembly for a secondary battery according to exemplary embodiments.
[0041] Referring to FIG. 1, a preliminary electrode (50) may be formed by forming an active material layer (110) on an electrode current collector (105). The active material layer (110) may include an active material that provides charge / discharge activity to the electrode of a secondary battery. For example, the active material may be dispersed in the active material layer (110) in the form of particles, as indicated by black dots in FIG. 1.
[0042] According to exemplary embodiments, the active material layer (110) may be formed such that the active material loading amount and density on one end of the electrode current collector (105) are greater than the active material loading amount and density on the other end of the electrode current collector (105).
[0043] For example, the electrode current collector (105) or the active material layer (110) may include a first region (I) and a second region (II). The first region (I) includes one end of the electrode current collector (105) and may have a predetermined width from the one end. The second region (II) includes the other end and may have a predetermined width from the other end.
[0044] According to exemplary embodiments, the first region (I) may have a lower active material loading and density than the second region (II).
[0045] In some embodiments, the active material layer (110) may further include an intermediate region (III) disposed between the first region (I) and the second region (II). The active material loading amount and density of the intermediate region (III) may be greater than those of the first region (I) and less than those of the second region (II).
[0046] As described above, the active material loading amount and density can be sequentially increased from the first region (I) to the second region (II) (or from one end of the electrode current collector (105) to the other end).
[0047] In one embodiment, the active material loading amount and density may gradually increase from the first region (I) to the second region (II). In this case, the active material loading amount and density may also gradually increase within the first region (I), the second region (II), and / or the intermediate region (III).
[0048] In one embodiment, the active material loading amount and density may be increased stepwise from the first region (I) to the second region (II). In this case, the active material loading amount and density may also be increased stepwise within the first region (I), the second region (II), and / or the intermediate region (III).
[0049] The intermediate region (III) serves as, for example, a buffer region and can prevent separation of the active material layer (110) and cracking of the active material during the winding process described later due to a sudden change in the active material loading amount and density from one end to the other end.
[0050] The thickness of the active material layer (110) can be substantially the same from one end to the other end of the electrode current collector (105). Accordingly, the active material loading amount and the density of the active material layer (110) can be easily controlled simply by adjusting the amount of active material input within a set thickness.
[0051] According to exemplary embodiments, the active material layer (110) may be formed on the upper and lower surfaces of the electrode current collector (105), respectively. For example, the active material layer (110) may include an upper active material layer (112) formed on the upper surface of the electrode current collector (105) and a lower active material layer (114) formed on the lower surface of the electrode current collector (105). As described above, each of the upper active material layer (112) and the lower active material layer (114) may have a regional variation in active material loading amount and density.
[0052] In some embodiments, the average active material loading and average density of the lower active material layer (114) may be less than the average active material loading and average density of the upper active material layer (112).
[0053] The active material layer (110) can be formed by coating a slurry containing the active material on an electrode current collector (105), followed by drying and rolling. For example, the slurry can be prepared by mixing the active material with a binder, a conductive agent, and / or a dispersant in a solvent.
[0054] The solvent may be a polar protic solvent, a polar aprotic solvent or a nonpolar solvent.
[0055] The polar aprotic solvent may include, for example, N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), acetonitrile, butylene carbonate, propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethylene carbonate (EC), ethyl bromide, tetrahydrofuran (THF), acetone, and the like.
[0056] The polar proton solvent may include, for example, deionized water, distilled water, ethanol, isopropanol, methanol, n-propanol, t-butanol, etc.
[0057] Examples of the non-polar solvent include hexane, heptane, carbon tetrachloride, benzene, toluene, ethylbenzene, xylene, 1,4-dioxane, etc. These may be used alone or in combination of two or more.
[0058] In some embodiments, the preliminary electrode (50) may be a preliminary electrode for a positive electrode. In this case, the active material included in the preliminary electrode (50) may include a compound capable of reversibly intercalating and deintercalating lithium ions. The active material may include lithium-transition metal composite oxide particles. For example, the lithium-transition metal composite oxide particles include nickel (Ni) and may further include at least one of cobalt (Co) and manganese (Mn).
[0059] For example, the lithium-transition metal composite oxide particles can be represented by the following chemical formula 1.
[0060] [Chemical Formula 1]
[0061] Li x Ni 1-y M y O 2+z
[0062] In chemical formula 1, 0.9≤x≤1.1, y may be 0≤y≤0.7, and z may be -0.1≤z≤0.1. M may represent one or more elements selected from Na, Mg, Ca, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Co, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, or Zr.
[0063] The positive electrode binder may include, for example, an organic binder such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, or an aqueous binder such as styrene-butadiene rubber (SBR). The positive electrode binder may be included together with a thickener such as carboxymethyl cellulose (CMC), for example.
[0064] For example, a PVDF series binder can be used as a positive electrode binder. In this case, the amount of binder for forming a positive electrode active material layer can be reduced and the amount of positive electrode active material can be relatively increased, thereby improving the output and capacity of the secondary battery (200).
[0065] The positive electrode collector (135) may include, for example, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof. For example, the positive electrode collector (135) may include aluminum or an aluminum alloy.
[0066] A cathode conductive material may be included to promote electron transfer between active material particles. For example, the cathode conductive material may include a carbon-based conductive material such as graphite, carbon black, graphene, carbon nanotubes, and / or a metal-based conductive material including a perovskite material such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3.
[0067] In some embodiments, the reserve electrode (50) may be a reserve electrode for the negative electrode. In this case, the active material included in the reserve electrode (50) may include a compound capable of adsorbing and desorbing lithium ions. For example, the active material may include carbon-based materials such as crystalline carbon, amorphous carbon, carbon composites, carbon fibers, lithium alloys, silicon (Si)-based compounds, or tin.
[0068] The amorphous carbon may include, for example, hard carbon, coke, mesocarbon microbeads (mesocarbon pitch-based carbon fiber: MPCF), etc. The crystalline carbon may include, for example, graphite-based carbon such as natural graphite, artificial graphite, coke, graphitized MCMB, etc. The elements included in the lithium alloy may include, for example, aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, indium, etc. The silicon-based compound may include, for example, silicon oxide (SiO x ) or a silicon-carbon composite oxide such as carbide (SiC).
[0069] The negative electrode binder may include, for example, an aqueous binder such as styrene-butadiene rubber (SBR) for compatibility with the carbon-based active material. The negative electrode binder may be included together with a thickener such as, for example, carboxymethyl cellulose (CMC).
[0070] The negative electrode current collector (145) may include gold, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof. For example, the negative electrode current collector (145) may include copper or a copper alloy.
[0071] The cathode conductive material may include a carbon-based conductive material such as carbon nanotubes, carbon black, Super P, etc.
[0072] Referring to FIG. 2, a spare electrode (50) can be wound to form an electrode assembly (100) including a wound electrode.
[0073] According to exemplary embodiments, the spare electrode (50) can be wound in the form of a jelly roll using the one end and the other end of the electrode current collector (105) as the winding center and the winding end, respectively.
[0074] The second region (II) of the above-mentioned other end or active material layer (110) can be tensioned by applying a winding tension. Accordingly, the active materials distributed in a relatively high loading amount in the second region (II) can be dispersed or expanded. Accordingly, the uniformity of the distribution of the active materials can be improved across the entire area of the active material layer (110).
[0075] The electrode assembly (100) includes a wound electrode, and the wound active material layer included in the wound electrode can have a substantially uniform active material loading amount and density.
[0076] In some embodiments, the lower active material layer (114) may be disposed on the inner side of the winding as described above, and the upper active material layer (112) may be disposed on the outer side of the winding. Accordingly, the density of the active material may increase as a shrinkage force is applied to the lower active material layer (114) having a relatively low active material loading, and the density of the active material may decrease as a tensile force is applied to the upper active material layer (112) having a relatively high active material loading.
[0077] Accordingly, a substantially uniform active material loading amount and density can be achieved throughout the active material layer in a wound state. Therefore, peeling of the active material layer and uneven energy density / lifespan characteristics due to differences in electrode expansion due to variations in active material distribution in the electrode assembly (100) state can be suppressed.
[0078] The above-described winding electrode may include an anode (130) and a cathode (140). In some embodiments, a separator (120) may be placed between the anode (130) and the cathode (140), and the anode (130) and the cathode (140) may be wound together using the separator (120).
[0079] The positive electrode (130) may include a positive electrode current collector (135) and an upper positive electrode active material layer (132) and a lower positive electrode active material layer (134) positioned with the positive electrode current collector (135) interposed therebetween. For example, the lower positive electrode active material layer (134) may be positioned on the inner side of the winding, and the upper positive electrode active material layer (132) may be positioned on the outer side of the winding.
[0080] The negative electrode (140) may include a negative electrode current collector (145) and an upper negative electrode active material layer (142) and a lower negative electrode active material layer (144) positioned with the negative electrode current collector (145) interposed therebetween. For example, the lower negative electrode active material layer (144) may be positioned on the inner side of the winding, and the upper negative electrode active material layer (142) may be positioned on the outer side of the winding.
[0081] The separator (120) may include a porous polymer film made of a polyolefin polymer, such as, for example, an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc. The separator (120) may also include a nonwoven fabric formed of high-melting-point glass fibers, polyethylene terephthalate fibers, etc.
[0082] Figures 3 and 4 are schematic cross-sectional views illustrating a preliminary electrode according to some exemplary embodiments. Detailed descriptions of structures / processes substantially identical or similar to those described with reference to Figures 1 and 2 are omitted.
[0083] Referring to FIG. 3, a first active material layer (110a) can be formed on an electrode current collector (105), and a second active material layer (110b) can be formed on the first active material layer (110a) to form an active material layer (110) having a multi-layer structure.
[0084] For example, the second active material layer (110b) can be formed spaced apart from the electrode current collector (105) with the first active material layer (110a) interposed therebetween.
[0085] According to exemplary embodiments, the amount of active material loading in the first region (I) of the electrode current collector (105) of the first active material layer (110a) may be less than the amount of active material loading in the second region (II) of the electrode current collector (105).
[0086] In some embodiments, the active material loading amount of the first active material layer (110a) in the intermediate region (III) may be greater than that of the first region (I) and less than that of the second region (II). Accordingly, the active material loading amount of the first active material layer (110a) may sequentially increase from the first region (I) to the second region (II).
[0087] In one embodiment, the active material loading amount of the first active material layer (110a) may gradually increase in the direction from the first region (I) to the second region (II). In this case, the active material loading amount of the first active material layer (110a) may also gradually increase within the first region (I), the second region (II), and / or the intermediate region (III).
[0088] According to exemplary embodiments, the active material loading amount in the first region (I) of the electrode current collector (105) of the second active material layer (110b) may be greater than the active material loading amount in the second region (II) of the electrode current collector (105).
[0089] In some embodiments, the active material loading amount of the second active material layer (110b) in the intermediate region (III) may be smaller than that of the first region (I) and larger than that of the second region (II). Accordingly, the active material loading amount of the second active material layer (110b) may sequentially decrease from the first region (I) to the second region (II).
[0090] In one embodiment, the active material loading amount of the second active material layer (110b) may gradually decrease from the first region (I) toward the second region (II). In this case, the active material loading amount of the second active material layer (110b) may also gradually decrease within the first region (I), the second region (II), and / or the intermediate region (III).
[0091] In some embodiments, the first active material layer (110a) may be formed so that the thickness in the first region (I) of the electrode current collector is smaller than the thickness in the second region (II). In this case, the thickness of the first active material layer (110a) may gradually increase from the first region (I) toward the second region (II).
[0092] In some embodiments, the second active material layer (110b) may be formed so that the thickness in the first region (I) of the electrode current collector (105) is greater than the thickness in the second region (II). In this case, the thickness of the second active material layer (110b) may gradually decrease from the first region (I) toward the second region (II).
[0093] The thickness increase rate of the first active material layer (110a) from the first region (I) to the second region (II) may be substantially the same as the thickness decrease rate of the second active material layer (110b) from the first region (I) to the second region (II). In this case, the sum of the thicknesses of the first active material layer (110a) and the second active material layer (110b) may be substantially the same from the first region (I) to the second region (II). Accordingly, it is possible to suppress excessive variations in the active material loading amounts in the first region (I) and the second region (II) due to changes in the thicknesses of the first active material layer (110a) and the second active material layer (110b).
[0094] In some embodiments, the density of the first active material layer (110a) can be increased compared to the density of the second active material layer (110b). In this case, the density of the active material layer (110) can be easily controlled simply by adjusting the thicknesses of the first active material layer (110a) and the second active material layer (110b).
[0095] According to exemplary embodiments, a multi-layered active material layer (110) including a first active material layer (110a) and a second active material layer (110b) may be formed on the upper and lower surfaces of the electrode current collector (105), respectively.
[0096] In some embodiments, the first active material layer (110a) may be formed by coating a first slurry containing an active material on an electrode current collector (105), followed by drying and rolling. For example, the first slurry may be prepared by mixing the active material with a binder, a conductive agent, and / or a dispersant in a first solvent.
[0097] In some embodiments, the second active material layer (110b) may be formed by coating a second slurry containing an active material on the first active material layer (110a), followed by drying and rolling. For example, the second slurry may be prepared by mixing the active material with a binder, a conductive agent, and / or a dispersant in a second solvent.
[0098] In one embodiment, the active material included in the first slurry may be the same active material as the active material included in the second slurry.
[0099] In some embodiments, the first solvent may be a different solvent from the second solvent. For example, the first solvent may have a different polarity from the second solvent.
[0100] In one embodiment, the density of the first solvent may be greater than that of the second solvent. Accordingly, the second slurry may be separated and formed on the first slurry due to the density difference between the first solvent and the second solvent.
[0101] In one embodiment, the solubility of the active material in the first solvent may be greater than the solubility of the active material in the second solvent. In this case, the amount of the active material contained in the first slurry may be greater than the amount of the active material contained in the second slurry. Accordingly, the density of the first active material layer (110a) may be greater than the density of the second active material layer (110b).
[0102] Referring to FIG. 4, the active material loading amount of the first active material layer (110a) may increase stepwise from the first region (I) to the second region (II), and the active material loading amount of the second active material layer (110b) may decrease stepwise.
[0103] FIG. 5 is a schematic plan view showing a secondary battery (200) according to exemplary embodiments.
[0104] Referring to FIG. 5, a secondary battery (200) can be manufactured by preparing an electrode assembly (100) and housing the electrode assembly (100) in an external case (210).
[0105] A secondary battery (200) may be defined by housing an electrode assembly (100) together with an electrolyte within an outer case (210). According to exemplary embodiments, a non-aqueous electrolyte may be used as the electrolyte.
[0106] The non-aqueous electrolyte contains a lithium salt as an electrolyte and an organic solvent, and the lithium salt is, for example, Li + X - is expressed as and the anion of the lithium salt (X - ) as F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH -, (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It may include:
[0107] The organic solvent may include, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethylmethyl carbonate (EMC), methylpropyl carbonate, dipropyl carbonate, dimethylsulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, and tetrahydrofuran. These may be used alone or in combination of two or more.
[0108] As illustrated in FIG. 5, electrode tabs may protrude from the electrode current collectors belonging to each electrode cell and extend to one side of the outer case (210). The electrode tabs may be fused together with the one side of the outer case (210) and connected to electrode leads (160, 170) that extend or are exposed to the outside of the outer case (210).
[0109] The secondary battery (200) can be manufactured in a cylindrical, square, pouch or coin shape using, for example, a can.
[0110] Hereinafter, specific experimental examples are presented to help understand the present invention, but these are only illustrative of the present invention and do not limit the scope of the appended claims. It is obvious to those skilled in the art that various changes and modifications to the examples are possible within the scope and technical idea of the present invention, and it is also natural that such changes and modifications fall within the scope of the appended claims.
[0111]
[0112] Examples and Comparative Examples
[0113] Example 1
[0114] 1) Manufacturing of cathode
[0115] A negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive carbon nanotubes (CNTs) in a solvent. The negative electrode slurry was applied onto a Cu foil current collector with increasing loading from the first region to the second region. Thereafter, drying and rolling were performed to form a negative electrode active material layer. Distilled water was used as the solvent.
[0116] The average active material density in the first region of the lower negative active material layer formed on the lower surface of the negative active material layer is 1.4 g / cm 3 , the average active material density in the second region is 1.6 g / cm 3 The above loading amount was increased to .
[0117] The average active material density in the first region of the upper negative electrode active material layer formed on the upper surface of the negative electrode active material layer is 1.5 g / cm 3 , the average active material density in the second region is 1.7 g / cm 3 The above loading amount was increased to .
[0118] 2) Manufacturing of the anode
[0119] LiNi as positive electrode active material 0.8 Co 0.1 Mn0.1 O2, carbon black and carbon nanotubes (CNTs) as a cathode conductive agent, and polyvinylidene fluoride (PVDF) as a cathode binder were mixed in a solvent at a weight ratio of 94:2:4 to prepare a cathode slurry. The cathode slurry was applied onto an Al foil current collector with increasing loading from the first region to the second region. Thereafter, drying and rolling were performed to form a cathode active material layer. Distilled water was used as the solvent.
[0120] The average active material density in the first region of the lower positive electrode active material layer formed on the lower surface of the positive electrode active material layer is 2.8 g / cm 3 , the average active material density in the second region is 3.4 g / cm 3 The above loading amount was increased to .
[0121] The average active material density in the first region of the upper positive electrode active material layer formed on the upper surface of the positive electrode active material layer is 3.0 g / cm 3 , the average active material density in the second region is 3.7 g / cm 3 The above loading amount was increased to .
[0122] 3) Manufacturing of cylindrical cells
[0123] A polyethylene (PE) separator was introduced between the above-described negative electrode and the above-described positive electrode. Afterwards, the outermost portion was wound with a curvature of 2 and the first negative electrode active material layer and the first positive electrode active material layer positioned inward, and an electrolyte was injected to produce a cylindrical cell.
[0124] Example 2
[0125] 1) Manufacturing of cathode
[0126] A first negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive carbon nanotubes (CNTs) in a solvent. The first negative electrode slurry was applied onto a Cu foil current collector with increasing loading from the first region to the second region. Thereafter, drying and rolling were performed to form a first negative electrode active material layer. Propylene carbonate (PC) was used as the solvent.
[0127] A second negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber (SBR), and 1 wt% of conductive carbon nanotubes (CNT) in a solvent. The second negative electrode slurry was applied onto the first negative electrode active material layer while decreasing the loading amount from the first region to the second region. Thereafter, the second negative electrode active material layer was formed by drying and rolling. Distilled water was used as the solvent.
[0128] The average density of the first negative electrode active material layer and the second negative electrode active material layer of the lower negative electrode active material layer formed on the lower surface of the above negative electrode active material layer is 1.4 g / cm in the first region. 3 , the density of the active material in the second region is 1.6 g / cm 3 It was loaded like this.
[0129] The average density of the first negative electrode active material layer and the second negative electrode active material layer of the upper negative electrode active material layer formed on the upper surface of the above negative electrode active material layer is 1.5 g / cm at the start of the winding. 3 , the density of the active material at the end of the winding is 1.7 g / cm 3 It was loaded like this.
[0130] 2) Manufacturing of the anode
[0131] LiNi as positive electrode active material 0.8 Co 0.1 Mn 0.1A first cathode slurry was prepared by mixing O2, carbon black and carbon nanotubes (CNTs) as cathode conductive agents, and polyvinylidene fluoride (PVDF) as cathode binder in a solvent at a weight ratio of 94:2:4. The first cathode slurry was applied onto an Al foil current collector with increasing loading from the first region to the second region. Thereafter, drying and rolling were performed to form a first cathode active material layer. Propylene carbonate (PC) was used as the solvent.
[0132] LiNi as positive electrode active material 0.8 Co 0.1 Mn 0.1 A second cathode slurry was prepared by mixing O2, carbon black and carbon nanotubes (CNTs) as cathode conductive agents, and polyvinylidene fluoride (PVDF) as cathode binder in a solvent at a weight ratio of 94:2:4. The second cathode slurry was applied onto the first cathode active material layer while decreasing the loading amount from the first region to the second region. Thereafter, drying and rolling were performed to form the second cathode active material layer. Distilled water was used as the solvent.
[0133] The average density of the first positive electrode active material layer and the second positive electrode active material layer of the lower positive electrode active material layer formed on the lower surface of the positive electrode active material layer is 2.8 g / cm at the start of the winding. 3 , the density of the active material at the end of the winding is 3.4 g / cm 3 The above loading was done so that it becomes possible.
[0134] The average density of the first positive electrode active material layer and the second positive electrode active material layer formed on the upper surface of the positive electrode active material layer is 3.0 g / cm in the first region. 3 , the density of the active material in the second region is 3.7 g / cm 3 It was loaded like this.
[0135] 3) Manufacturing of cylindrical cells
[0136] A polyethylene (PE) separator was introduced between the above-described negative electrode and the above-described positive electrode. Afterwards, the outermost portion was wound with a curvature of 2 and the first negative electrode active material layer and the first positive electrode active material layer positioned inward, and an electrolyte was injected to produce a cylindrical cell.
[0137] Example 3
[0138] A cylindrical cell was manufactured in the same manner as in Example 2, except that the curvature of the outermost part was set to 1 during winding.
[0139] Example 4
[0140] A cylindrical cell was manufactured in the same manner as in Example 2, except that the curvature of the outermost part was set to 3 during winding.
[0141] Comparative Example 1
[0142] 1) Manufacturing of cathode
[0143] A negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive CNT in distilled water. The negative electrode slurry was applied to a Cu foil current collector, dried, and rolled to obtain a density of 1.6 g / cm. 3 A negative electrode for a secondary battery was manufactured by forming a negative electrode active material layer having an active material density of .
[0144] 2) Manufacturing of cylindrical cells
[0145] Lithium foil was used as the cathode and counter electrode, and a polyethylene (PE) separator was introduced between the cathode and counter electrode. Afterwards, the cell was wound so that the curvature of the outermost part was 2, and an electrolyte was injected to produce a cylindrical cell.
[0146] Comparative Example 2
[0147] The active material density of the negative active material is 1.7 g / cm 3A cylindrical cell was manufactured in the same manner as in Comparative Example 1, except that the cathode slurry was applied, dried, and rolled.
[0148] Comparative Example 3
[0149] The active material density of the negative active material is 1.5 g / cm 3 A cylindrical cell was manufactured in the same manner as in Comparative Example 1, except that the cathode slurry was applied, dried, and rolled.
[0150] The slurry loading amounts of Examples 1 and 2 are shown in Table 1 below.
[0151] Electrode type Slurry type Loading amount (mg / cm) 2 ) Winding start point (one end) 1 / 4 point from the winding start point Collector center 3 / 4 point from the winding start point Winding end point (other end) Example 1 Anode Lower Anode slurry 16.0 17.5 19.0 20.5 2.0 Upper Anode slurry 17.0 18.7 20.4 22.1 23.8 Cathode Lower Anode slurry 6.5 7.2 5 8.0 8.7 5 9.5 Upper Anode slurry 7.5 8.2 5 9.0 9.7 5 10.5 Example 2 Anode Lower First Anode slurry 0.05 5 11.0 16.5 2.0 Upper First Anode slurry 1.06 25 11.5 16.7 5 2.0 Lower Second Anode slurry 16.0 12.0 8.0 4.0 0.0 Upper Second Anode slurry 16.012.458.95.351.8Cathode Lower first cathode slurry 0.02.3754.757.1259.5Upper first cathode slurry 1.03.1255.257.3759.5Lower second cathode slurry 6.54.8753.251.6250.0Upper second cathode slurry 6.55.1253.752.3751.0
[0152] Experimental example
[0153] (1) Measurement of the density of the active material in the negative electrode active material layers after winding
[0154] After winding, a portion of the cylindrical cell was cut from the outermost part to the center, and the thickness, length, and width of the electrode were measured using a micrometer, and the active material density for the active material layer was measured using the active material weight value.
[0155] (2) Measurement of life characteristics
[0156] For the battery cells according to the examples and comparative examples, charging (CC-CV 1.0C 4.2V CUT OFF) and discharging (1.0C 2.7V CUT-OFF) were repeated, and the number of cycles until a discharge capacity of 60% or less compared to the initial discharge capacity was measured was measured.
[0157] The evaluation results are shown in Table 2 below.
[0158] Average density of active material (g / cm) 3 ) Life characteristics (cycle) Winding start (one end) 1 / 4 point from the winding start point Collector center 3 / 4 point from the winding start point Winding end (other end) Example 11.541.541.551.561.561,050 Example 21.541.541.551.561.561,500 Example 31.521.531.551.571.581,400 Example 41.551.551.551.551.551,400 Comparative example 11.311.391.471.511.59500 Comparative example 21.361.441.521.61.68300 Comparative example 31.211.291.371.411.49700
[0159] Referring to Table 2, in examples where the density of the active material before winding was gradually increased from the start of winding (one end) to the end of winding (the other end) by giving a difference in loading amount, the difference in density after winding was maintained small, thereby improving the life characteristics.
[0160] In Examples 2 to 4, in which the active material layers on both sides of the collector were formed in two layers each, the life characteristics were improved.
[0161] In Example 3, where the curvature at the outermost part was reduced to 1 during winding, the energy density was somewhat reduced.
[0162] In Example 4, where the curvature at the outermost part was increased to 3 during winding, the energy density was somewhat reduced.
[0163] The difference in loading amount is not given, so the density difference between the center and the periphery of the winding electrode is 0.2 g / cm. 3 In the above comparative examples, the energy density was reduced.
Claims
1. Step of preparing the electrode collector; A step of forming a preliminary electrode by forming an active material layer including a first region on one end of the electrode current collector and a second region having a higher active material loading amount and density than the first region on the other end of the electrode current collector; and A method for manufacturing an electrode assembly for a secondary battery, comprising a step of forming a wound electrode including a wound active material layer by winding the spare electrode together with the active material layer around the one end of the electrode current collector.
2. A method for manufacturing an electrode assembly for a secondary battery according to claim 1, wherein the active material layer is formed between the first region and the second region and includes an intermediate region having a greater active material loading amount and density than the first region and a smaller active material loading amount and density than the second region.
3. A method for manufacturing an electrode assembly for a secondary battery, wherein the active material layer is formed so that the loading amount and density of the active material gradually or stepwise increase in the direction of the second region in the first region.
4. A method for manufacturing an electrode assembly for a secondary battery, wherein the loading amount and density of the active material of the winding active material layer are uniform over the entire area of the electrode current collector in claim 1.
5. A method for manufacturing an electrode assembly for a secondary battery, wherein the thickness of the active material layer included in the preliminary electrode is uniform over the entire area of the electrode current collector in claim 1.
6. In claim 1, forming the active material layer includes forming an upper active material layer and a lower active material layer on the upper and lower surfaces of the electrode current collector, respectively. A method for manufacturing an electrode assembly for a secondary battery, wherein the average active material loading amount and average density of the lower active material layer are smaller than those of the upper active material layer.
7. A method for manufacturing an electrode assembly for a secondary battery, wherein winding the preliminary electrode according to claim 6 includes winding the lower active material layer inward.
8. In claim 1, forming the active material layer comprises: Forming a first active material layer on the surface of the electrode current collector; and A method for manufacturing an electrode assembly for a secondary battery, comprising forming a second active material layer on the first active material layer, with the electrode current collector and the first active material layer interposed therebetween.
9. In claim 8, the active material loading amount in the first region of the first active material layer is smaller than the active material loading amount in the second region, A method for manufacturing an electrode assembly for a secondary battery, wherein the loading amount of active material in the first region of the second active material layer is greater than the loading amount of active material in the second region.
10. In claim 9, the thickness of the first active material layer in the first region is smaller than the thickness in the second region, A method for manufacturing an electrode assembly for a secondary battery, wherein the thickness of the second active material layer in the first region is greater than the thickness in the second region.
11. In claim 9, the active material loading amount of the first active material layer gradually or stepwise increases from the first region to the second region, A method for manufacturing an electrode assembly for a secondary battery, wherein the active material loading amount of the second active material layer gradually or stepwise decreases from the first region to the second region.
12. In claim 9, forming the first active material layer includes applying a first slurry containing a first solvent and the active material, A method for manufacturing an electrode assembly for a secondary battery, wherein forming the second active material layer includes applying a second slurry containing a second solvent different from the first solvent and the active material on the first active material layer.
13. A method for manufacturing an electrode assembly for a secondary battery according to claim 12, wherein the density of the first solvent is greater than the density of the second solvent.
14. In claim 1, further comprising a step of arranging the spare electrodes on the first and second faces of the separator, which face each other, A method for manufacturing an electrode assembly for a secondary battery, wherein the separator is wound together with the spare electrode.
15. A step of preparing an electrode assembly manufactured according to claim 1; and A method for manufacturing a secondary battery, comprising the step of housing the electrode assembly within a case.
Citation Information
Patent Citations
Jelly rolls with active material layers in varying amounts
JP2010521793A
Electrode structure and lithium battery including the same
KR1020150134162A
Electrode Assembly Comprising Electrode Having Gradient in Loading Amount of Active Material
KR1020170022289A
A hydrophobic pattern forming method
KR1020220109222A
Photomask, the method of manufacturing photomask, photomask blank and the method of manufacturing display device
KR102195658B1