Method for manufacturing lithium secondary battery electrode and method for manufacturing secondary battery including lithium secondary battery electrode
The method of forming and drying active material layers on electrode current collectors for secondary batteries addresses the issue of natural agitation, improving cohesion and reducing resistance, thereby enhancing the performance and lifespan of secondary batteries.
Patent Information
- Application Number
- PCT/KR2024/005279
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
AI Technical Summary
Secondary batteries with active material layers in a multi-layer structure often experience increased resistance and deteriorated lifespan due to natural agitation between the layers, leading to reduced performance and capacity.
A method of manufacturing electrodes with a multi-layer active material structure involves forming a first and second coating layer on an electrode current collector, with preliminary drying followed by bulk drying at higher temperatures, using different solvents to minimize natural agitation and enhance cohesion between layers.
This approach improves the cohesion between active material layers, reduces electrode resistance, and enhances cycle performance, resulting in more uniform energy density and extended lifespan characteristics.
Smart Images

Figure KR2024005279_24102024_PF_FP_ABST
Abstract
Description
Method for manufacturing an electrode for a lithium secondary battery and method for manufacturing a secondary battery including the same
[0001] The present disclosure relates to a method for manufacturing an electrode for a secondary battery and a method for manufacturing a secondary battery including the electrode for a secondary battery. More specifically, the present disclosure relates to a method for manufacturing an electrode for a secondary battery including an active material layer having a multi-layer structure and a method for manufacturing a secondary battery including the electrode for a secondary battery.
[0002]
[0003] Secondary batteries, which can be repeatedly charged and discharged, are widely used as power sources for portable electronic communication devices such as camcorders, mobile phones, and laptops, thanks to the advancements in the information and communication and display industries. Furthermore, battery packs containing secondary batteries are being developed and applied as power sources for eco-friendly vehicles such as hybrid vehicles.
[0004] Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, and nickel-hydrogen batteries. Among these, lithium secondary batteries are being actively developed and applied due to their high operating voltage and energy density per unit weight, and their advantages in charging speed and weight reduction.
[0005] For example, a secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator, and an electrolyte that impregnates the electrode assembly. The secondary battery may further include an outer packaging material, for example, in the form of a pouch, that accommodates the electrode assembly and the electrolyte.
[0006] The above electrode may include, for example, a multi-layered active material layer. However, a secondary battery including a multi-layered active material layer may experience increased resistance and deteriorated life characteristics due to natural stirring between the active material layers of each layer.
[0007]
[0008] One object of the present disclosure is to provide a method for manufacturing an electrode for a secondary battery having improved life characteristics.
[0009] One object of the present disclosure is to provide a secondary battery including the electrode for the secondary battery.
[0010]
[0011] In a method for manufacturing an electrode for a secondary battery according to exemplary embodiments, a first active material slurry may be applied onto an electrode current collector to form a first coating layer. The first coating layer may be preliminarily dried to form a first preliminary active material layer. A second active material slurry may be applied onto the first preliminary active material layer to form a second coating layer. The first preliminary active material layer and the second coating layer may be converted into a first active material layer and a second active material layer, respectively, through bulk drying performed at a temperature higher than the preliminarily drying.
[0012] In some embodiments, the pre-drying may include exposing the first coating layer to warm air of 40 to 60° C.
[0013] In some embodiments, the pre-drying is performed 1 cm above the first coating layer. 2 This may include exposure to hot air for 5 to 20 seconds.
[0014] In some embodiments, the first active material slurry may be supplied onto the electrode current collector through the first coating portion, the second active material slurry may be supplied onto the first pre-active material layer through the second coating portion, and the second coating portion may be spaced apart from the first coating portion along the coating progress direction.
[0015] In some embodiments, the pre-drying may be performed through a first drying unit, the bulk drying may be performed through a second drying unit, and the first drying unit may be disposed between the first coating unit and the second coating unit along the coating progress direction.
[0016] In some embodiments, the second coating portion may be disposed between the first drying portion and the second drying portion along the coating progress direction.
[0017] In some embodiments, the first active material slurry may include a first active material and a first solvent, and the second active material slurry may include a second solvent that is phase-separable from the second active material and the first solvent.
[0018] In some embodiments, the density of the first solvent may be greater than the density of the second solvent.
[0019] In some embodiments, the first active material and the second active material may be the same active material.
[0020] In some embodiments, the amount of the first active material included in the first active material layer and the amount of the second active material included in the second active material layer may be different.
[0021] A method for manufacturing a secondary battery according to exemplary embodiments may prepare a secondary battery electrode manufactured according to the method for manufacturing a secondary battery electrode. The secondary battery electrode may be wound to form an electrode assembly. The electrode assembly may be accommodated in a case.
[0022] In some embodiments, the density of the active material layer disposed inside in the winding direction of the electrode for the secondary battery may be lower.
[0023] In some embodiments, forming the electrode assembly may further include arranging the secondary battery electrode on each of the first and second faces of the separator, which face each other, and winding the separator together with the secondary battery electrode.
[0024]
[0025] According to exemplary embodiments, the active material layer of the electrode may include a multilayer structure. When forming the active material layer having the multilayer structure, the method may include pre-drying a first coating layer formed on an electrode current collector. Accordingly, when forming a second coating layer on the first preliminary active material layer formed by pre-drying the first coating layer, appropriate natural stirring can be induced. Accordingly, the cohesion between the active material layers can be improved. In addition, the resistance of the electrode can be reduced, and the cycle performance for the same capacity can be improved.
[0026] In some embodiments, the solvents included in the slurries for forming the multilayer active material layers may be different from each other. Accordingly, excessive mixing of the multilayer active material layers can be suppressed, thereby reducing the resistance of the secondary battery and improving cycle performance.
[0027] According to exemplary embodiments, the density of the active material layer disposed inwardly during the winding operation can be relatively reduced compared to the density of the active material layer disposed outwardly during the winding operation. Accordingly, the density of the winding active material layers disposed in the outer and inner winding can be substantially uniformly controlled. Accordingly, electrode cracking / peeling due to variations in the distribution of the active material within the jelly roll can be prevented, thereby uniformizing the energy density and life characteristics.
[0028] The method for manufacturing an electrode for a secondary battery of the present disclosure and the secondary battery manufactured according to the method for manufacturing the secondary battery can be widely applied in green technology fields such as electric vehicles, battery charging stations, and other fields utilizing batteries, such as solar power generation and wind power generation. The negative active material for a lithium secondary battery of the present disclosure, the method for manufacturing the same, and the lithium secondary battery including the same can be used in eco-friendly electric vehicles, hybrid vehicles, etc. to prevent climate change by suppressing air pollution and greenhouse gas emissions.
[0029]
[0030] FIGS. 1 to 3 are cross-sectional views illustrating a method for manufacturing an electrode for a secondary battery according to exemplary embodiments.
[0031] FIGS. 4 and 7 are drawings for explaining a method of manufacturing a secondary battery according to exemplary embodiments, respectively.
[0032]
[0033] Embodiments of the present disclosure provide a method for manufacturing an electrode including an active material layer having a multi-layer structure. In addition, a method for manufacturing a secondary battery including the electrode for the secondary battery is provided.
[0034] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the drawings. However, the following drawings attached to this disclosure illustrate preferred embodiments of the present disclosure and serve to further understand the technical concepts of the present disclosure. Therefore, this disclosure should not be interpreted as being limited to the matters described in such drawings.
[0035] The terms “upper”, “lower”, “top surface”, “lower surface”, etc. used in this disclosure are used in a relative sense to distinguish the positions of the components, and do not specify absolute positions.
[0036] FIGS. 1 to 3 are cross-sectional views illustrating a method for manufacturing an electrode for a secondary battery according to exemplary embodiments.
[0037] For convenience of explanation, in FIGS. 1 to 3, the first coating layer (70), the first preliminary active material layer (73), and the second coating layer (80) are shown as being formed only on one side of the electrode current collector (60), but they may be formed on both sides of the electrode current collector (60).
[0038] Referring to Fig. 1, an electrode current collector (60) may be provided through a supply roll (50). For example, the electrode current collector (60) may be continuously provided while the supply roll (50) rotates in a horizontal direction. The horizontal direction may be, for example, the direction of an arrow.
[0039] According to exemplary embodiments, a first active material slurry may be applied onto an electrode current collector (60) to form a first coating layer. For example, the first active material slurry may be prepared by mixing the first active material with a binder, a conductive agent, and / or a dispersant in a first solvent.
[0040] In some embodiments, the first active material slurry may be applied onto the electrode current collector (60) by the first coating unit (53) to form a first coating layer (70). The first coating unit (53) may be, for example, a coater including a slot die.
[0041] In one embodiment, the first active material slurry may be introduced through one end (e.g., a slot die) of the first coating portion (53) and may flow out through the other end (e.g., a slot die head). Accordingly, the first active material slurry may be applied onto the electrode current collector (60).
[0042] In one embodiment, the electrode current collector (60) may be moved in a horizontal direction (e.g., in the direction of an arrow) so that a first coating layer (70) may be formed on the electrode current collector (60) through the first coating portion (53). The horizontal direction may be the same direction as the movement direction of the electrode current collector (60) by the supply roll (50). Accordingly, the first coating portion (53) may continuously form the first coating layer (70) on the electrode current collector (60) without moving.
[0043] According to exemplary embodiments, the first coating layer (70) may be pre-dried to form the first preliminary active material layer (73). For example, the first solvent of the first coating layer (70) may be partially evaporated to form the first preliminary active material layer (73).
[0044] In some embodiments, the first coating layer (70) may be exposed to warm air. Accordingly, the first coating layer (70) may be pre-dried.
[0045] The above-mentioned warm air may be, for example, 30 to 70°C, preferably 40 to 60°C. Within this range, the first coating layer (70) may be pre-dried without being excessive. Accordingly, the first pre-active material layer (73) may undergo a certain amount of natural stirring with the second coating layer (80) described below, thereby improving the cohesiveness of the first active material layer (75) and the second active material layer (85).
[0046] The first coating layer (70) is, for example, 1 cm on the upper surface of the first coating layer (70). 2 The secondary battery may be exposed to the hot air for 3 to 30 seconds, preferably 5 to 20 seconds. Within this range, the first coating layer (70) may be sufficiently pre-dried. Accordingly, excessive natural stirring between the first pre-active material layer (73) and the second coating layer (80) may be suppressed, thereby reducing the resistance of the secondary battery and improving the capacity retention rate.
[0047] In some embodiments, the pre-drying may be performed through a first drying unit (55). The first drying unit (55) may be a dryer capable of supplying hot air. For example, the first drying unit (55) may be, for example, a hot air heater, a heat pump hot air dryer, an electric hot air dryer, etc.
[0048] In one embodiment, when the electrode current collector (60) having the first coating layer (70) formed thereon enters the first drying section (55), the movement of the electrode current collector (60) having the first coating layer (70) formed thereon may be stopped for a predetermined period of time. For example, the supply of the electrode current collector (60) from the supply roll (50) may be stopped for the predetermined period of time.
[0049] The above-described predetermined time may be, for example, 5 to 30 seconds, or 10 to 20 seconds. Accordingly, the degree of drying of the first preliminary active material layer (73) can be controlled. Accordingly, the cohesion of the first active material layer (75) and the second active material layer (85) can be improved while suppressing excessive natural stirring with the second coating layer (80).
[0050] In one embodiment, the electrode current collector (60) having the first coating layer (70) formed thereon may be pre-dried by the first drying unit (55) while moving in a horizontal direction (e.g., in the direction of the arrow). The horizontal direction may be the same direction as the direction in which the first coating layer (70) is formed. Accordingly, the first coating layer (70) may be continuously pre-dried without movement of the first drying unit (55), thereby forming the first pre-active material layer (73).
[0051] Referring to FIG. 2, a second active material slurry may be applied on a first preliminary active material layer (73) to form a second coating layer. For example, the second active material slurry may be prepared by mixing the second active material with a binder, a conductive agent, and / or a dispersant in a second solvent.
[0052] The first solvent forming the first active material slurry described above and the second solvent forming the second active material slurry may be, for example, a polar aprotic solvent, a polar protic solvent, or a nonpolar solvent.
[0053] The polar aprotic solvent may include, for example, N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), acetonitrile, butylene carbonate, propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethylene carbonate (EC), ethyl bromide, tetrahydrofuran (THF), acetone, and the like.
[0054] The polar proton solvent may be, for example, deionized water, distilled water, ethanol, isopropanol, methanol, n-propanol, t-butanol, etc.
[0055] The above non-polar solvent may include, for example, hexane, heptane, carbon tetrachloride, benzene, toluene, ethylbenzene, xylene, 1,4-dioxane, etc. These may be used alone or in combination of two or more.
[0056] In some embodiments, the first solvent and the second solvent may be different solvents.
[0057] In one embodiment, the first solvent may be a solvent having a higher density than the second solvent. In one embodiment, the first solvent may be a solvent having a different polarity from the second solvent. Accordingly, the first pre-active material layer (73) can be prevented from being excessively stirred with the second coating layer (80).
[0058] In some embodiments, the first active material and the second active material may be the same active material. Accordingly, even if a multi-layered active material layer is formed, the resistance between the active material layers due to the difference in the active materials can be reduced.
[0059] According to exemplary embodiments, the electrode current collector (60) on which the first preliminary active material layer (73) is formed may move in the direction of the arrow while the second active material slurry is applied on the first preliminary active material layer (73) to form a second coating layer (80).
[0060] In some embodiments, the second active material slurry may be applied onto the first pre-active material layer (73) by a second coating unit (57) to form a second coating layer (80). The second coating unit (57) may be, for example, a coater including a slot die.
[0061] In one embodiment, the second active material slurry may be introduced through one end (e.g., a slot die) of the second coating portion (57) and may be discharged through the other end (e.g., a slot die head). Accordingly, the second active material slurry may be applied onto the first preliminary active material layer (73).
[0062] In some embodiments, the second coating layer (80) may be formed to entirely cover the first preliminary active material layer (73). Accordingly, the movement of lithium ions between the first active material layer (75) and the second active material layer (85) may be prevented from being interrupted, thereby inhibiting an increase in resistance.
[0063] Referring to FIG. 3, the first preliminary active material layer (73) and the second coating layer (80) can be dried together.
[0064] According to exemplary embodiments, the first pre-active material layer (73) and the second coating layer (80) may be bulk dried to be converted into the first active material layer (75) and the second active material layer (85), respectively. For example, the first solvent and the second solvent of the first pre-active material layer (73) and the second coating layer (80), respectively, may be evaporated to be converted into the first active material layer (75) and the second active material layer (85).
[0065] In some embodiments, the bulk drying may be performed at a higher temperature than the pre-drying.
[0066] The above bulk drying can be performed, for example, at a temperature of 100 to 120°C, or 105 to 115°C, for 60 to 120 seconds, or 80 to 100 seconds. In this range, the first pre-active material layer (73) and the second coating layer (80) can suppress additional natural stirring between the first active material layer (75) and the second active material layer (85) formed by completing drying, respectively.
[0067] In some embodiments, the bulk drying may be performed through a second drying unit (59). The second drying unit (59) may be, for example, a hot air heater, a heat pump hot air dryer, an electric hot air dryer, etc.
[0068] In some embodiments, the first coating portion (53) may be formed at a constant interval from the second coating portion (57). In addition, the first drying portion (55) may be formed at a constant interval from the second drying portion (59).
[0069] In this case, the first drying unit (55) may be arranged between the first coating unit (53) and the second coating unit (57). In addition, the second coating unit (57) may be arranged between the first drying unit (55) and the second drying unit (59). Accordingly, the formation of the above-described coating layers, preliminary drying, and bulk drying can be performed continuously through a single process.
[0070] According to exemplary embodiments, the first active material layer (75) and the second active material layer (85) may be formed on the upper and lower surfaces of the electrode current collector (60), respectively.
[0071] For example, the active material layer (75, 85) may be formed on the upper surface of the electrode current collector (60) and then formed on the lower surface of the electrode current collector (60). For example, the active material layers (75, 85) may be formed simultaneously on the upper surface and the lower surface of the electrode current collector (60).
[0072] In this case, the method of forming the active material layer (75, 85) on the lower surface of the electrode current collector (60) may be substantially the same as or similar to the method of forming the active material layer (60) on the upper surface of the electrode current collector (60).
[0073] Accordingly, an electrode can be formed in which a multi-layer structure of active material layers including a first active material layer (75) and a second active material layer (85) are formed on both sides of an electrode current collector (60).
[0074] The electrode for a secondary battery manufactured as described above can be provided as a positive electrode (90) for a secondary battery or a negative electrode (110) for a secondary battery.
[0075] In some embodiments, the electrode may be a positive electrode. In this case, the active material included in the positive electrode active material layer (100) of the positive electrode (90) may include a compound capable of reversibly intercalating and deintercalating lithium ions. The active material may include lithium-transition metal composite oxide particles. For example, the lithium-transition metal composite oxide particles include nickel (Ni) and may further include at least one of cobalt (Co) and manganese (Mn).
[0076] For example, the lithium-transition metal composite oxide particles can be represented by the following chemical formula 1.
[0077] [Chemical Formula 1]
[0078] Li x Ni 1-y M y O 2+z
[0079] In chemical formula 1, 0.9≤x≤1.1, y may be 0≤y≤0.7, and z may be -0.1≤z≤0.1. M may represent one or more elements selected from Na, Mg, Ca, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Co, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, or Zr.
[0080] The positive electrode binder may include, for example, an organic binder such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, or an aqueous binder such as styrene-butadiene rubber (SBR). The positive electrode binder may be included together with a thickener such as carboxymethyl cellulose (CMC), for example.
[0081] For example, a PVDF-based binder can be used as a positive electrode binder. In this case, the amount of binder required to form the positive electrode active material layer can be reduced and the amount of positive electrode active material can be relatively increased, thereby improving the output and capacity of the secondary battery.
[0082] The positive electrode collector (95) may include, for example, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof. For example, the positive electrode collector (95) may include aluminum or an aluminum alloy.
[0083] A cathode conductive material may be included to promote electron transfer between active material particles. For example, the cathode conductive material may include a carbon-based conductive material such as graphite, carbon black, graphene, carbon nanotubes, and / or a metal-based conductive material including a perovskite material such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3.
[0084] In some embodiments, the electrode may be a negative electrode. In this case, the active material included in the negative electrode active material layer (115) of the negative electrode (110) may include a compound capable of adsorbing and desorbing lithium ions. For example, the active material may include a carbon-based material such as crystalline carbon, amorphous carbon, a carbon composite, or carbon fiber, a lithium alloy, a silicon (Si)-based compound, or tin.
[0085] The amorphous carbon may include, for example, hard carbon, coke, mesocarbon microbeads (mesocarbon pitch-based carbon fiber: MPCF), etc. The crystalline carbon may include, for example, graphite-based carbon such as natural graphite, artificial graphite, coke, graphitized MCMB, etc. The elements included in the lithium alloy may include, for example, aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, indium, etc. The silicon-based compound may include, for example, silicon oxide (SiO x ) or a silicon-carbon composite oxide such as carbide (SiC).
[0086] The negative electrode binder may include, for example, an aqueous binder such as styrene-butadiene rubber (SBR) for compatibility with the carbon-based active material. The negative electrode binder may be included together with a thickener such as, for example, carboxymethyl cellulose (CMC).
[0087] The negative electrode current collector (115) may include gold, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof. For example, the negative electrode current collector (115) may include copper or a copper alloy.
[0088] The cathode conductive material may include a carbon-based conductive material such as carbon nanotubes, carbon black, Super P, etc.
[0089] FIGS. 4 to 7 are drawings for explaining a method of manufacturing a secondary battery according to exemplary embodiments, respectively.
[0090] Referring to Fig. 4, the electrode for a secondary battery manufactured as described with reference to Figs. 1 to 3 can be prepared. The electrode for a secondary battery may have an active material layer (75, 85) formed on both sides of an electrode current collector (60). For example, the active material may be dispersed in the active material layer (75, 85) in the form of particles, as indicated by black dots in Fig. 4.
[0091] According to exemplary embodiments, the amount of the first active material included in the first active material layer (75) and the amount of the second active material included in the second active material layer (85) may be different from each other. Accordingly, an electrode may be formed in which the densities of the first active material layer (75) and the second active material layer (85) formed on the upper and lower surfaces of the electrode current collector (60) are different from each other. For example, as described below, when the electrode is wound, the amounts of the first active material included in the first active material layer (75) and the second active material included in the second active material layer (85) may be adjusted so that the density of the active material layer disposed inward in the winding direction may be small.
[0092] In some embodiments, the electrode may be wound with the second active material layer (85) formed on the lower surface of the electrode current collector (60) facing the inner side of the winding. In this case, the average density of the active material layer (75, 85) formed on the upper surface of the electrode current collector (60) may be higher than the average density of the active material layer (75, 85) formed on the lower surface of the electrode current collector (60).
[0093] In one embodiment, the amount of the first active material included in the first active material layer (75) formed on the upper surface of the electrode current collector (60) may be less than the amount of the second active material included in the second active material layer (85) formed on the first active material layer (75). Accordingly, the density of the first active material layer (75) formed on the upper surface of the electrode current collector (60) may be lower than the density of the second active material layer (85) formed on the first active material layer (75).
[0094] In one embodiment, the amount of the first active material included in the first active material layer (75) formed on the lower surface of the electrode current collector (60) may be greater than the amount of the second active material included in the second active material layer (85) formed on the first active material layer (75). Accordingly, the density of the first active material layer (75) formed on the lower surface of the electrode current collector (60) may be higher than the density of the second active material layer (85) formed on the first active material layer (75).
[0095] In some embodiments, the electrode may be wound with the second active material layer (85) formed on the upper surface of the electrode current collector (60) facing the inner side of the winding. In this case, the average density of the active material layer (75, 85) formed on the upper surface of the electrode current collector (60) may be lower than the average density of the active material layer (75, 85) formed on the lower surface of the electrode contactor (60).
[0096] In one embodiment, the amount of the first active material included in the first active material layer (75) formed on the upper surface of the electrode current collector (60) may be greater than the amount of the second active material included in the second active material layer (85) formed on the first active material layer (75). Accordingly, the density of the first active material layer (75) formed on the upper surface of the electrode current collector (60) may be higher than the density of the second active material layer (85) formed on the first active material layer (75).
[0097] In one embodiment, the amount of the first active material included in the first active material layer (75) formed on the lower surface of the electrode current collector (60) may be less than the amount of the second active material included in the second active material layer (85) formed on the first active material layer (75). Accordingly, the density of the first active material layer (75) formed on the lower surface of the electrode current collector (60) may be lower than the density of the second active material layer (85) formed on the first active material layer (75).
[0098] Referring to FIG. 5, a wound electrode can be formed by winding an electrode including a first active material layer (75) and a second active material layer (85) having different densities formed on the upper and lower surfaces of an electrode current collector (60), respectively.
[0099] In some embodiments, the electrode may be wound with the second active material layer (85) formed on the upper surface of the electrode current collector (60) as the outer side of the winding. In addition, the second active material layer (85) formed on the lower surface of the electrode current collector (60) may be wound in a jelly roll shape with the inner side of the winding, thereby forming a wound electrode. Accordingly, an upper wound active material layer and a lower wound active material layer may be formed.
[0100] In one embodiment, the upper winding active material layer including the active material layer (75, 85) formed on the upper surface of the electrode current collector (60) may have a relatively high density. The upper winding active material layer may be stretched when a winding tension is applied. Accordingly, the density of the active material may decrease when a tensile force is applied to the upper winding active material layer having a relatively high density.
[0101] In one embodiment, the lower winding active material layer including the active material layer (75, 85) formed on the lower surface of the electrode current collector (60) may have a relatively low density. The lower winding active material layer may be compressed when a winding shrinkage force is applied. Accordingly, the density of the active material may increase when a shrinkage force is applied to the lower winding active material layer having a relatively low density.
[0102] In some embodiments, the electrode may be wound with the second active material layer (85) formed on the upper surface of the electrode current collector (60) as the inner side of the winding. In addition, the second active material layer (85) formed on the lower surface of the electrode current collector (60) may be wound in a jelly roll shape with the outer side of the winding, thereby forming a wound electrode. Accordingly, an upper wound active material layer and a lower wound active material layer may be formed.
[0103] In one embodiment, the lower winding active material layer including the active material layer (75, 85) formed on the lower surface of the electrode current collector (60) may have a relatively high density. The lower winding active material layer may be stretched when a winding tension is applied. Accordingly, the density of the active material may decrease when a tensile force is applied to the lower winding active material layer having a relatively high density.
[0104] In one embodiment, the upper winding active material layer including the active material layer (75, 85) formed on the upper surface of the electrode current collector (60) may have a relatively low density. The lower winding active material layer may be compressed when a winding shrinkage force is applied. Accordingly, the density of the active material may increase when a shrinkage force is applied to the upper winding active material layer having a relatively low density.
[0105] As described above, the density of the upper active material layer of the winding electrode may decrease, and the density of the lower active material layer of the winding electrode may increase. Accordingly, the densities of the upper active material layer and the lower active material layer of the winding electrode may be the same overall.
[0106] Referring to FIG. 6, the electrodes described with reference to FIGS. 4 and 5 are placed on the opposing first and second surfaces of the separator, respectively, and the separator (130) can be wound together with the electrodes.
[0107] For convenience of explanation, in FIG. 6, the active material layer is shown as being formed as a single layer on both sides of the electrode current collector (60), but the active material layer may be a multi-layered active material layer including a first active material layer (75) and a second active material layer (85).
[0108] According to exemplary embodiments, a separator (130) may be placed between the positive electrode (90) and the negative electrode (110), and the positive electrode (130) and the negative electrode (140) may be wound together using the separator (130). Accordingly, a wound electrode assembly (140) may be manufactured.
[0109] The positive electrode (90) may include a positive electrode current collector (95) and a positive electrode active material layer (100) disposed between the positive electrode current collector (95).
[0110] For example, the density of the positive electrode active material layer (100) disposed on the lower surface of the positive electrode current collector (95) may be relatively low. In this case, the positive electrode active material layer (100) disposed on the lower surface of the positive electrode current collector (95) may be disposed on the inner side of the winding, and the positive electrode active material layer (100) disposed on the upper surface of the positive electrode current collector (95) may be disposed on the outer side of the winding.
[0111] For example, the density of the positive electrode active material layer (100) disposed on the upper surface of the positive electrode current collector (95) may be relatively low. In this case, the positive electrode active material layer (100) disposed on the upper surface of the positive electrode current collector (95) may be disposed on the inner side of the winding, and the positive electrode active material layer (100) disposed on the lower surface of the positive electrode current collector (95) may be disposed on the outer side of the winding.
[0112] Accordingly, the density of the positive electrode active material layer (100) disposed on both sides of the positive electrode current collector (95) can be substantially the same.
[0113] The negative electrode (110) may include a negative electrode current collector (115) and a negative electrode active material layer (120) disposed between the negative electrode current collector (115).
[0114] For example, the density of the negative active material layer (120) disposed on the lower surface of the negative current collector (115) may be relatively low. In this case, the negative active material layer (120) disposed on the lower surface of the negative current collector (115) may be disposed on the inner side of the winding, and the negative active material layer (120) disposed on the upper surface of the negative current collector (115) may be disposed on the outer side of the winding.
[0115] For example, the density of the negative active material layer (120) disposed on the upper surface of the negative current collector (115) may be relatively low. In this case, the negative active material layer (120) disposed on the upper surface of the negative current collector (115) may be disposed on the inner side of the winding, and the negative active material layer (120) disposed on the lower surface of the negative current collector (115) may be disposed on the outer side of the winding.
[0116] Accordingly, the density of the negative electrode active material layer (120) arranged on both sides of the negative electrode current collector (115) can be substantially the same.
[0117] The separator (130) may include a porous polymer film made of a polyolefin polymer, such as, for example, an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc. The separator (130) may also include a nonwoven fabric formed of high-melting-point glass fibers, polyethylene terephthalate fibers, etc.
[0118] Referring to FIG. 7, a secondary battery (160) can be manufactured by preparing an electrode assembly (140) described with reference to FIG. 6 and housing the electrode assembly (140) in a case (150).
[0119] An electrode assembly (140) may be housed together with an electrolyte within a case (150) to define a secondary battery (160). According to exemplary embodiments, a non-aqueous electrolyte may be used as the electrolyte.
[0120] The non-aqueous electrolyte contains a lithium salt as an electrolyte and an organic solvent, and the lithium salt is, for example, Li + X - is expressed as and the anion of the lithium salt (X - ) as F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4- , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF-SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It may include:
[0121] The organic solvent may include, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethylmethyl carbonate (EMC), methylpropyl carbonate, dipropyl carbonate, dimethylsulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, and tetrahydrofuran. These may be used alone or in combination of two or more.
[0122] As illustrated in Fig. 7, electrode tabs may protrude from the electrode collectors belonging to each electrode cell and extend to one side of the case (150). The electrode tabs may be fused together with the one side of the case (150) and connected to electrode leads (97, 117) that extend or are exposed to the outside of the case (150).
[0123] The above lithium secondary battery (160) can be manufactured in a cylindrical, square, pouch or coin shape using a can, for example.
[0124] Hereinafter, specific experimental examples are presented to help understand the present disclosure, but these are only illustrative of the present disclosure and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the examples are possible within the scope and technical idea of the present disclosure, and it is also natural that such changes and modifications fall within the scope of the appended claims.
[0125]
[0126] Examples and Comparative Examples
[0127] Example 1
[0128] 1) Manufacturing of cathode
[0129] A first negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive carbon nanotubes (CNTs) in a solvent. The first negative electrode slurry was applied onto a Cu foil current collector to form a first negative electrode coating layer. Thereafter, the first negative electrode coating layer was preliminarily dried through a first drying unit to form a first preliminary negative electrode active material layer. Propylene carbonate (PC) was used as the solvent.
[0130] The first drying unit supplied warm air of 45°C to the first cathode coating layer to preliminarily dry the first cathode coating layer. In addition, the first cathode coating layer was dried by supplying warm air at a distance of 1 cm from the first cathode coating layer. 2 It was exposed for 10 seconds.
[0131] A second negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber (SBR), and 1 wt% of conductive carbon nanotubes (CNT) in a solvent. The second negative electrode slurry was applied onto the first preliminary negative electrode active material layer to form a second negative electrode coating layer. Thereafter, the first preliminary negative electrode active material layer and the second negative electrode coating layer were bulk-dried and rolled together through a second drying unit to form a first negative electrode active material layer and a second negative electrode active material layer. Distilled water was used as the solvent.
[0132] 2) Manufacturing of the anode
[0133] LiNi as positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, carbon black and carbon nanotubes (CNT) as a cathode conductive agent, and polyvinylidene fluoride (PVDF) as a cathode binder were mixed in a solvent at a weight ratio of 94:2:4 to prepare a first cathode slurry. The first cathode slurry was applied onto an Al foil current collector to form a first cathode coating layer. Thereafter, the first cathode coating layer was preliminarily dried through a first drying unit to form a first preliminary cathode active material layer. Propylene carbonate (PC) was used as the solvent.
[0134] The first drying unit supplied warm air of 45°C to the first anode coating layer to preliminarily dry the first anode coating layer. In addition, the first anode coating layer was dried by supplying warm air at a distance of 1 cm from the first anode coating layer. 2 It was exposed for 10 seconds.
[0135] LiNi as positive electrode active material0.8 Co 0.1 Mn 0.1 O2, carbon black and carbon nanotubes (CNT) as a cathode conductive agent, and polyvinylidene fluoride (PVDF) as a cathode binder were mixed in a solvent at a weight ratio of 94:2:4 to prepare a second cathode slurry. The second cathode slurry was applied onto the first preliminary cathode active material layer to form a second cathode coating layer. Thereafter, the first preliminary cathode active material layer and the second cathode coating layer were bulk dried and rolled together through a second drying unit to form the first cathode active material layer and the second cathode active material layer. Distilled water was used as the solvent.
[0136] 3) Cell manufacturing
[0137] A polyethylene (PE) separator was introduced between the cathode and the anode. Thereafter, an electrolyte was injected to fabricate a cell.
[0138] Example 2
[0139] The first cathode coating layer and the first anode coating layer are each supplied from the first drying unit to the warm air, and the first cathode coating layer and the first anode coating layer are each 1 cm apart. 2 Cells were prepared in the same manner as in Example 1, except that they were exposed for 5 seconds.
[0140] Example 3
[0141] The first cathode coating layer and the first anode coating layer are each supplied from the first drying unit to the warm air, and the first cathode coating layer and the first anode coating layer are each 1 cm apart. 2 Cells were prepared in the same manner as in Example 1, except that they were exposed for 30 seconds.
[0142] Example 4
[0143] A cell was manufactured in the same manner as in Example 1, except that the warm air supplied to the first cathode coating layer and the first anode coating layer in the first drying section was each 60°C.
[0144] Example 5
[0145] A cell was manufactured in the same manner as in Example 2, except that the warm air supplied to the first cathode coating layer and the first anode coating layer in the first drying section was each 60°C.
[0146] Comparative Example 1
[0147] The solvents of the first cathode slurry, the second cathode slurry, the first anode slurry, and the second anode slurry were all propylene carbonate (PC).
[0148] The first cathode coating layer was not pre-dried, and the first cathode coating layer and the second cathode coating layer were bulk-dried together.
[0149] In addition, the first anode coating layer and the second anode coating layer were bulk-dried together without pre-drying the first anode coating layer.
[0150] Except for the above-described points, the cell was manufactured in the same manner as in Example 1.
[0151] Comparative Example 2
[0152] A cell was manufactured in the same manner as in Comparative Example 1, except that the solvent used in the first cathode slurry and the first anode slurry was propylene carbonate (PC), and the solvent used in the second cathode slurry and the second anode slurry was distilled water.
[0153]
[0154] Experimental example
[0155] (1) Bonding strength of the negative electrode current collector and the first negative electrode active material layer
[0156] A double-sided tape was attached to a glass plate, and the negative electrodes manufactured according to the examples and comparative examples were attached to the double-sided tape. Thereafter, force was applied until the negative electrode active material layer was peeled off from the negative electrode current collector, and the bonding strength between the negative electrode current collector and the first negative electrode active material layer was measured.
[0157] (2) Cohesion of the first negative electrode active material layer and the second negative electrode active material layer
[0158] According to the examples and comparative examples, the cohesive force of the first negative electrode active material layer and the second negative electrode active material layer was measured by applying force until the second negative electrode active material layer was peeled off from the first negative electrode active material layer.
[0159] (3) Resistance performance evaluation
[0160] The average resistance for 10 seconds at 1C was measured when the SOC (State of Charge) of the secondary battery module according to the examples and comparative examples was set to 50%.
[0161] (4) Cycle performance evaluation
[0162] For the battery cells according to the examples and comparative examples, charging (CC-CV 1.0C 4.2V CUT OFF) and discharging (1.0C 2.7V CUT-OFF) were repeated, and the number of cycles until the first negative electrode active material layer and the second negative electrode active material layer were detached was measured.
[0163] The evaluation results are shown in Table 1 below.
[0164]
[0165] Current collector-active material layer cohesion (N)First active material layer-second active material layer cohesion (N)Cell capacity (Ah)Cell resistance performance (mΩ)Cell cycle performance (cycle)Example 14025500.952500Example 24015501.151500Example 33020501.11800Example 43020501.091900Example 54020501.02000Comparative example 13020501.02000Comparative example 23010501.21000
[0166] Referring to Table 2, in the examples in which different solvents were used but pre-dried, the bonding strength between the electrode current collector and the first negative electrode active material layer, the cohesion between the first negative electrode active material layer and the second negative electrode active material layer, and the cell cycle performance were all improved, and the cell resistance was reduced, compared to Comparative Example 2 in which different solvents were used but pre-dried.
[0167] In Example 1, in which the first negative electrode slurry was pre-dried at 45°C for 10 seconds, the bonding strength between the negative electrode current collector and the active material layer, the cohesion between the first negative electrode active material layer and the second negative electrode active material layer, and the cell cycle performance were improved, and the cell resistance was reduced, compared to Comparative Example 1, in which one solvent was used.
[0168] In Example 2, where the pre-drying time was reduced to 5 seconds, the bonding strength and cell cycle performance of the first negative electrode active material layer and the second negative electrode active material layer decreased, and the cell resistance increased, compared to Example 1.
[0169] In Example 3, where the pre-drying time was increased to 30 seconds, the bonding force between the negative current collector and the first negative active material layer, the cohesion between the first negative active material layer and the second negative active material layer, and the cell cycle performance decreased compared to Example 1, and the cell resistance increased.
[0170] In Example 4, where the pre-drying temperature was increased to 60°C in Example 1, the bonding force between the negative current collector and the first negative electrode active material layer, the cohesion between the first negative electrode active material layer and the second negative electrode active material layer, and the cell cycle performance decreased compared to Example 1, and the cell resistance increased.
[0171] In Example 5, where the pre-drying temperature was increased to 60°C in Example 2, the cohesion between the first negative electrode active material layer and the second negative electrode active material layer and the cell cycle performance were improved, and the cell resistance was reduced compared to Example 2.
[0172] In Comparative Example 2, where a different solvent was used but pre-drying was not performed, the bonding force between the negative current collector and the first negative active material layer, the cohesion between the first negative active material layer and the second negative active material layer, and the cell cycle performance decreased, and the cell resistance increased.
Claims
1. A step of forming a first coating layer by applying a first active material slurry on an electrode current collector; A step of preliminarily drying the first coating layer to form a first preliminary active material layer; A step of forming a second coating layer by applying a second active material slurry on the first preliminary active material layer; and A method for manufacturing an electrode for a secondary battery, comprising a step of converting the first pre-active material layer and the second coating layer into a first active material layer and a second active material layer, respectively, through bulk drying performed at a temperature higher than the pre-drying.
2. A method for manufacturing an electrode for a secondary battery according to claim 1, wherein the pre-drying comprises exposing the first coating layer to warm air of 40 to 60°C.
3. In claim 2, the pre-drying is performed on the upper surface of the first coating layer by 1 cm. 2 A method for manufacturing an electrode for a secondary battery, comprising exposing the electrode to hot air for 5 to 20 seconds.
4. In claim 1, the first active material slurry is supplied onto the electrode current collector through the first coating portion, and the second active material slurry is supplied onto the first preliminary active material layer through the second coating portion. A method for manufacturing an electrode for a secondary battery, wherein the second coating portion is spaced apart from the first coating portion along the coating progress direction.
5. In claim 4, the preliminary drying is performed through a first drying unit, and the bulk drying is performed through a second drying unit. A method for manufacturing an electrode for a secondary battery, wherein the first drying unit is disposed between the first coating unit and the second coating unit along the coating progress direction.
6. A method for manufacturing an electrode for a secondary battery according to claim 5, wherein the second coating portion is disposed between the first drying portion and the second drying portion along the coating progress direction.
7. A method for manufacturing an electrode for a secondary battery according to claim 1, wherein the first active material slurry includes a first active material and a first solvent, and the second active material slurry includes a second solvent that is phase-separable from the first solvent.
8. A method for manufacturing an electrode for a secondary battery according to claim 7, wherein the density of the first solvent is greater than the density of the second solvent.
9. A method for manufacturing an electrode for a secondary battery according to claim 7, wherein the first active material and the second active material are the same active material.
10. A method for manufacturing an electrode for a secondary battery, wherein, in claim 7, the amount of the first active material included in the first active material layer and the amount of the second active material included in the second active material layer are different.
11. A step of preparing an electrode for a secondary battery manufactured according to claim 1; A step of forming an electrode assembly by winding the electrode for the secondary battery; and A method for manufacturing a secondary battery, comprising the step of accommodating the electrode assembly in a case.
12. A method for manufacturing a secondary battery, wherein the density of the active material layer disposed on the inside in the winding direction of the electrode for the secondary battery is smaller in claim 11.
13. In claim 11, the step of forming the electrode assembly comprises: A step of arranging the secondary battery electrodes on the first and second sides of the separator, which are opposite to each other; and A method for manufacturing a secondary battery, comprising a step of winding the separator together with the electrode for the secondary battery.
Citation Information
Patent Citations
Method for manufacturing battery
JP2015015156A
Apparatus for producing lithium polymer battery using continuous roll-to-roll system by direct solution casting technology and method for producing lithium polymer battery using the sam ...
KR1020130071333A
Anode for lithium secondary battery, preparation method thereof and lithium secondary battery comprising the same
KR1020150043769A
Flexible Electrode, Method of Preparing the Same, and Secondary Battery Comprising the Same
KR1020180127921A
KR20220009280A
Cited By
Method and apparatus for producing a multilayer coating for battery electrodes
DE102025116735A1