Method for manufacturing electrode assembly for secondary battery and method for manufacturing secondary battery comprising same
The method of forming electrode assemblies with varying active material densities on both sides of the current collector addresses the issue of non-uniformity in secondary battery electrode assemblies, resulting in improved energy density and lifespan by ensuring uniform active material distribution during the winding process.
Patent Information
- Application Number
- PCT/KR2024/005283
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
AI Technical Summary
Secondary battery electrode assemblies with jelly-roll configurations often experience non-uniform active material density due to winding, leading to uneven energy density and lifespan characteristics.
A method of manufacturing an electrode assembly with a preliminary electrode formed by coating active material layers of different densities on both sides of a current collector, where the lower active material layer has a lower density than the upper layer, and the density difference between the wound layers is minimized to ensure uniform energy density and lifespan.
The method achieves uniform active material distribution and density within the electrode assembly, preventing cracking and peeling, thereby enhancing the energy density and lifespan of secondary batteries.
Smart Images

Figure KR2024005283_24102024_PF_FP_ABST
Abstract
Description
Method for manufacturing an electrode assembly for a secondary battery and method for manufacturing a secondary battery including the same
[0001] The present disclosure relates to a method for manufacturing an electrode assembly for a secondary battery and a method for manufacturing a secondary battery including the electrode assembly for a secondary battery. More specifically, the present disclosure relates to a method for manufacturing an electrode assembly for a secondary battery having active material layers formed on both sides of a current collector and a secondary battery including the electrode assembly for a secondary battery.
[0002]
[0003] Secondary batteries, which can be repeatedly charged and discharged, are widely used as power sources for portable electronic communication devices such as camcorders, mobile phones, and laptops, thanks to the advancements in the information and communication and display industries. Furthermore, battery packs containing secondary batteries are being developed and applied as power sources for eco-friendly vehicles such as hybrid vehicles.
[0004] Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, and nickel-hydrogen batteries. Among these, lithium secondary batteries are being actively developed and applied due to their high operating voltage and energy density per unit weight, and their advantages in charging speed and weight reduction.
[0005] For example, a secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator, and an electrolyte that impregnates the electrode assembly. The secondary battery may further include an outer packaging material, for example, in the form of a pouch, that accommodates the electrode assembly and the electrolyte.
[0006] The above electrode assembly may have, for example, a jelly-roll shape in which the positive and negative electrodes are wound with a separator interposed therebetween.
[0007] However, the jelly roll-shaped electrode assembly may have a non-uniform active material density due to winding, which may result in non-uniform energy density and lifespan characteristics.
[0008]
[0009] An object of the present disclosure is to provide a method for manufacturing an electrode assembly for a secondary battery having improved life characteristics and energy density.
[0010] One object of the present disclosure is to provide a secondary battery including the electrode assembly for the secondary battery.
[0011]
[0012] In a method for manufacturing an electrode assembly for a secondary battery according to exemplary embodiments, an electrode current collector may be prepared. An upper active material layer may be formed on an upper surface of the electrode current collector, and a lower active material layer having a lower density than the upper active material layer may be formed on a lower surface of the electrode current collector to form a preliminary electrode. The preliminary electrode may be wound with the lower active material layer facing inward, thereby forming a wound electrode including a wound upper active material layer and a wound lower active material layer.
[0013] In some embodiments, the density of the upper active material layer may be less than the density of the upper active material layer, and the density of the lower active material layer may be greater than the density of the lower active material layer.
[0014] In some embodiments, the density difference between the upper active material layer and the lower active material layer may be smaller than the density difference between the upper active material layer and the lower active material layer.
[0015] In some embodiments, the density difference between the upper active material layer and the lower active material layer is 0.1 g / cm 3 It could be as follows:
[0016] In some embodiments, forming the upper active material layer and the lower active material layer may include coating an upper slurry and a lower slurry containing a solvent and an active material, respectively, on the upper and lower surfaces of the electrode current collector, and the solvent used in the upper slurry may be different from the solvent used in the lower slurry.
[0017] In some embodiments, forming the preliminary electrode may include forming at least one of the upper active material layer and the lower active material layer into a multi-layer structure having different densities.
[0018] In some embodiments, forming the multilayer structure may include forming a first active material layer on a surface of the electrode current collector, and forming a second active material layer on the first active material layer, the second active material layer being spaced apart from the electrode current collector and the first active material layer and having a different density from the first active material layer.
[0019] In some embodiments, forming the first active material layer may include applying a first slurry comprising a first solvent and a first active material, and forming the second active material layer may include applying a second slurry comprising a second solvent and a second active material that are different from the first solvent on the first active material layer.
[0020] In some embodiments, the second solvent may comprise a solvent that is phase-separable from the first solvent.
[0021] In some embodiments, the upper active material layer may include the first active material layer and the second active material layer, and the density of the second active material layer may be greater than the density of the first active material layer.
[0022] In some embodiments, the lower active material layer may include the first active material layer and the second active material layer, and the density of the first active material layer may be greater than the density of the second active material layer.
[0023] In some embodiments, the first active material and the second active material may be the same active material.
[0024] In some embodiments, the first solvent and the second solvent may have different solubilities for the active material.
[0025] In some embodiments, the device may further include positioning the spare electrode on each of the first and second surfaces facing the separator, and the separator may be wound together with the spare electrode.
[0026] A method for manufacturing a secondary battery according to exemplary embodiments can prepare an electrode assembly manufactured according to the method for manufacturing an electrode assembly for a secondary battery. The electrode assembly can be accommodated in a case.
[0027]
[0028] According to exemplary embodiments, the active material loading amount and density of the lower active material layer disposed inward during the winding operation can be relatively reduced. Accordingly, the density of the winding active material layers disposed on the outer and inner sides of the winding can be substantially uniformly controlled, and electrode cracking / peeling due to variations in the distribution of the active material within the jelly roll can be prevented, thereby uniformizing the energy density and life characteristics.
[0029] In some embodiments, the active material layer is formed by including a first active material layer and a second active material layer sequentially formed on the electrode current collector, and the density of the active material layer disposed innerward among the first active material layer and the second active material layer may be lower. By utilizing a multi-layer structure, the density difference in the active material layer of the above-described preliminary electrode can be more easily implemented. In addition, by using different solvents in the slurries for forming the first active material layer and the second active material layer, mixing of the active materials and density disturbance between the first active material layer and the second active material layer can be prevented.
[0030] The method for manufacturing an electrode assembly for a secondary battery of the present disclosure and the secondary battery manufactured according to the method for manufacturing a secondary battery can be widely applied in green technology fields such as electric vehicles, battery charging stations, and other fields utilizing batteries, such as solar power generation and wind power generation. The negative active material for a lithium secondary battery of the present disclosure, the method for manufacturing the same, and the lithium secondary battery including the same can be used in eco-friendly electric vehicles, hybrid vehicles, etc. to prevent climate change by suppressing air pollution and greenhouse gas emissions.
[0031]
[0032] FIG. 1 and FIG. 2 are drawings for explaining a method for manufacturing an electrode assembly for a secondary battery according to exemplary embodiments.
[0033] Figures 3 and 4 are schematic cross-sectional views showing a spare electrode according to some exemplary embodiments.
[0034] FIG. 5 is a schematic plan view showing a secondary battery according to exemplary embodiments.
[0035]
[0036] Embodiments of the present disclosure provide a method for manufacturing an electrode assembly for a secondary battery, which includes winding a spare electrode having a density variation of active material layers disposed on both sides of an electrode current collector. In addition, a method for manufacturing a secondary battery including the electrode assembly for a secondary battery is provided.
[0037] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the drawings. However, the following drawings attached to this disclosure illustrate preferred embodiments of the present disclosure and serve to further understand the technical concepts of the present disclosure. Therefore, this disclosure should not be interpreted as being limited to the matters described in such drawings.
[0038] The terms “upper”, “lower”, “top surface”, “lower surface”, etc. used in this disclosure are used in a relative sense to distinguish the positions of the components, and do not specify absolute positions.
[0039] FIG. 1 and FIG. 2 are drawings for explaining a method for manufacturing an electrode assembly for a secondary battery according to exemplary embodiments.
[0040] Referring to FIG. 1, a preliminary electrode (50) may be formed by forming an active material layer (110) on an electrode current collector (105). The active material layer (110) may include an active material that provides charge / discharge activity to the electrode of a secondary battery. For example, the active material may be dispersed in the active material layer (110) in the form of particles, as indicated by black dots in FIG. 1.
[0041] According to exemplary embodiments, an upper active material layer (112) may be formed on the upper surface of an electrode current collector (105), and a lower active material layer (114) having a lower density than the upper active material layer (112) may be formed on the lower surface of the electrode current collector (105).
[0042] The active material layer (110) can be formed by coating a slurry containing an active material on an electrode current collector (105), followed by drying and rolling. For example, the slurry can be prepared by mixing the active material with a binder, a conductive agent, and / or a dispersant in a solvent.
[0043] In some embodiments, the upper active material layer (112) may be formed by coating an upper slurry containing the active material on the upper surface of the electrode current collector (105), followed by drying and rolling. In addition, the lower active material layer (114) may be formed by coating a lower slurry containing the active material on the lower surface of the electrode current collector (105), followed by drying and rolling.
[0044] The polar aprotic solvent may include, for example, N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), acetonitrile, butylene carbonate, propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethylene carbonate (EC), ethyl bromide, tetrahydrofuran (THF), acetone, and the like.
[0045] The polar proton solvent may include, for example, deionized water, distilled water, ethanol, isopropanol, methanol, n-propanol, t-butanol, etc.
[0046] The above non-polar solvent may include, for example, hexane, heptane, carbon tetrachloride, benzene, toluene, ethylbenzene, xylene, 1,4-dioxane, etc. These may be used alone or in combination of two or more.
[0047] In some embodiments, the solvent used in the upper slurry may be different from the solvent used in the lower slurry. For example, the polarity of the solvent used in the upper slurry may be different from that of the solvent used in the lower slurry.
[0048] In one embodiment, the solubility of the active material in the solvent used in the upper slurry may be greater than the solubility of the active material in the solvent used in the lower slurry. In this case, the amount of the active material contained in the upper slurry may be greater than the amount of the active material contained in the lower slurry. Accordingly, the density of the upper active material layer (112) may be greater than the density of the lower active material layer (114).
[0049] In some embodiments, the spare electrode (50) may be a spare electrode for the anode.
[0050] For example, the density of the upper active material layer of the positive electrode is 2.85 to 3.75 g / cm 3 , or 3.0 to 3.7 g / cm 3 The density of the lower active material layer of the positive electrode pre-electrode may be 2.75 to 3.65 g / cm 3 , or 2.8 to 3.4 g / cm 3 In the above range, the active material layers of the positive electrode pre-electrode can be rolled at a high density, thereby preventing the active material layers of the positive electrode pre-electrode from being separated from each other.
[0051] When the reserve electrode (50) is a reserve electrode for a positive electrode, the active material included in the reserve electrode (50) may include a compound capable of reversibly intercalating and deintercalating lithium ions. The active material may include lithium-transition metal composite oxide particles. For example, the lithium-transition metal composite oxide particles include nickel (Ni) and may further include at least one of cobalt (Co) and manganese (Mn).
[0052] For example, the lithium-transition metal composite oxide particles can be represented by the following chemical formula 1.
[0053] [Chemical Formula 1]
[0054] Li x Ni 1-y M y O 2+z
[0055] In chemical formula 1, 0.9≤x≤1.1, y may be 0≤y≤0.7, and z may be -0.1≤z≤0.1. M may represent one or more elements selected from Na, Mg, Ca, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Co, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, or Zr.
[0056] The positive electrode binder may include, for example, an organic binder such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, or an aqueous binder such as styrene-butadiene rubber (SBR). The positive electrode binder may be used together with a thickener such as carboxymethyl cellulose (CMC), for example.
[0057] For example, a PVDF series binder can be used as a positive electrode binder. In this case, the amount of binder for forming a positive electrode active material layer can be reduced and the amount of positive electrode active material can be relatively increased, thereby improving the output and capacity of the secondary battery (200).
[0058] The positive electrode collector (135) may include, for example, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof. For example, the positive electrode collector (135) may include aluminum or an aluminum alloy.
[0059] A cathode conductive material may be included to promote electron transfer between active material particles. For example, the cathode conductive material may include a carbon-based conductive material such as graphite, carbon black, graphene, carbon nanotubes, and / or a metal-based conductive material including a perovskite material such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3.
[0060] In some embodiments, the spare electrode (50) may be a spare electrode for the cathode.
[0061] For example, the density of the upper active material layer of the negative electrode reserve electrode is 1.25 to 1.8 g / cm 3 , or 1.5 to 1.7 g / cm 3 The density of the lower active material layer of the negative electrode reserve electrode may be 1.15 to 1.7 g / cm 3 , or 1.4 to 1.6 g / cm 3 In the above range, the active material layers of the negative electrode reserve electrode can be rolled at a high density, thereby preventing the active material layers of the negative electrode reserve electrode from being separated from each other.
[0062] When the reserve electrode (50) is a reserve electrode for a negative electrode, the active material included in the reserve electrode (50) may include a compound capable of adsorbing and desorbing lithium ions. For example, it may include a carbon-based material such as crystalline carbon, amorphous carbon, a carbon composite, or carbon fiber, a lithium alloy, a silicon (Si)-based compound, or tin.
[0063] The amorphous carbon may include, for example, hard carbon, coke, mesocarbon microbeads (mesocarbon pitch-based carbon fiber: MPCF), etc. The crystalline carbon may include, for example, graphite-based carbon such as natural graphite, artificial graphite, coke, graphitized MCMB, etc. The elements included in the lithium alloy may include, for example, aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, indium, etc. The silicon-based compound may include, for example, silicon oxide (SiO x ) or a silicon-carbon composite oxide such as carbide (SiC).
[0064] The negative electrode binder may include, for example, an aqueous binder such as styrene-butadiene rubber (SBR) for compatibility with the carbon-based active material. The negative electrode binder may be used together with a thickener such as, for example, carboxymethyl cellulose (CMC).
[0065] The negative electrode current collector (145) may include gold, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof. For example, the negative electrode current collector (145) may include copper or a copper alloy.
[0066] The cathode conductive material may include a carbon-based conductive material such as carbon nanotubes, carbon black, Super P, etc.
[0067] Referring to FIG. 2, a spare electrode (50) can be wound to form an electrode assembly (100) including a wound electrode.
[0068] According to exemplary embodiments, the spare electrode (50) can be wound in a jelly roll shape with the upper active material layer (112) of the electrode current collector (105) on the outer side of the winding and the lower active material layer (114) on the inner side of the winding. Accordingly, a wound electrode including a wound upper active material layer and a wound lower active material layer can be formed.
[0069] In some embodiments, the density of the upper active material layer may be lower than that of the upper active material layer (112). The upper active material layer (112) may be stretched when a winding tension is applied. Accordingly, the density of the active material may decrease when a tension is applied to the upper active material layer (112) having a relatively high density.
[0070] In some embodiments, the lower active material layer may have a density greater than that of the lower active material layer (114). The lower active material layer (114) may be compressed when a winding shrinkage force is applied. Accordingly, the density of the active material may increase when a shrinkage force is applied to the lower active material layer (114) having a relatively low density.
[0071] As described above, the density of the upper active material layer of the winding may decrease and the density of the lower active material layer of the winding may increase.
[0072] In some embodiments, the density difference between the upper active material layer and the lower active material layer may be smaller than the density difference between the upper active material layer (112) and the lower active material layer (114). Accordingly, the unevenness of energy density / lifespan characteristics due to the deviation in the active material distribution of the upper active material layer and the lower active material layer can be suppressed.
[0073] In one embodiment, the density difference between the upper winding active material layer and the lower winding active material layer is 0.1 g / cm 3 or less, or 0.05 g / cm 3It may be as follows. In the above range, peeling and cracking of the active material layer due to differences in electrode expansion according to deviations in active material distribution in the state of the electrode assembly (100) can be suppressed.
[0074] The above-described winding electrode may include an anode (130) and a cathode (140). In some embodiments, a separator (120) may be placed between the anode (130) and the cathode (140), and the anode (130) and the cathode (140) may be wound together using the separator (120).
[0075] The positive electrode (130) may include a positive electrode current collector (135) and an upper positive electrode active material layer (132) and a lower positive electrode active material layer (134) positioned with the positive electrode current collector (135) interposed therebetween. For example, the lower positive electrode active material layer (134) may be positioned on the inner side of the winding, and the upper positive electrode active material layer (132) may be positioned on the outer side of the winding.
[0076] The density of the upper positive electrode active material layer (132) is 2.8 to 3.7 g / cm 3 , or 2.9 to 3.6 g / cm 3 The density of the lower positive electrode active material layer (134) may be 2.8 to 3.7 g / cm 3 , or 2.9 to 3.5 g / cm 3 It can be. In the above range, cracks in the positive electrode active material layer (132, 134) can be prevented, and the energy density of the secondary battery can be improved.
[0077] The negative electrode (140) may include a negative electrode current collector (145) and an upper negative electrode active material layer (142) and a lower negative electrode active material layer (144) positioned with the negative electrode current collector (145) interposed therebetween. For example, the lower negative electrode active material layer (144) may be positioned on the inner side of the winding, and the upper negative electrode active material layer (142) may be positioned on the outer side of the winding.
[0078] The density of the upper negative electrode active material layer (142) is 1.2 to 1.75 g / cm 3 , or 1.45 to 1.65 g / cm3 It can be. The density of the lower negative active material layer (144) is 1.2 to 1.75 g / cm 3 , or 1.45 to 1.65 g / cm 3 It can be. In the above range, cracks in the negative active material layer (142, 144) can be prevented, and the energy density of the secondary battery can be improved.
[0079] The separator (120) may include a porous polymer film made of a polyolefin polymer, such as, for example, an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc. The separator (120) may also include a nonwoven fabric formed of high-melting-point glass fibers, polyethylene terephthalate fibers, etc.
[0080] Figures 3 and 4 are schematic cross-sectional views illustrating a preliminary electrode according to some exemplary embodiments. Detailed descriptions of structures / processes substantially identical or similar to those described with reference to Figures 1 and 2 are omitted.
[0081] Referring to FIG. 3, the density can also gradually increase within the active material layer (110).
[0082] In one embodiment, the density of the active material may gradually increase from the bottom to the top of the upper active material layer (112) and the lower active material layer (114). Accordingly, density uniformity may be achieved within the upper active material layer and the lower active material layer of the wound electrode.
[0083] Referring to FIG. 4, a first active material layer is formed on an electrode current collector (105), and a second active material layer having a different density from the first active material layer is formed on the first active material layer, thereby forming an active material layer (110) having a multi-layer structure having different densities.
[0084] For example, the second active material layer may be formed spaced apart from the electrode current collector (105) with the first active material layer therebetween.
[0085] According to exemplary embodiments, at least one of the upper active material layer (112) and the lower active material layer (114) may be formed as an active material layer (110) having a multi-layer structure with different densities.
[0086] In some embodiments, the upper active material layer (112) includes an upper first active material layer (112a) and an upper second active material layer (112b), and the density of the upper second active material layer (112b) may be greater than the density of the upper first active material layer (112a).
[0087] In one embodiment, the upper first active material layer (112a) may be the upper first active material layer of the positive electrode reserve electrode, and the upper second active material layer (112b) may be the upper second active material layer of the positive electrode reserve electrode.
[0088] In this case, the density of the upper first active material layer of the positive electrode reserve electrode is 2.85 to 3.75 g / cm 3 , or 3.0 to 3.7 g / cm 3 The density of the upper second active material layer of the above-mentioned positive electrode may be 2.9 to 3.75 g / cm 3 , or 3.1 to 3.7 g / cm 3 It can be. In the above range, cracking of the active material during the winding process can be prevented.
[0089] In one embodiment, the upper first active material layer (112a) may be the upper first active material layer of a reserve electrode for a negative electrode, and the upper second active material layer (112b) may be the upper second active material layer of a reserve electrode for a negative electrode.
[0090] In this case, the density of the upper first active material layer of the negative electrode reserve electrode is 1.25 to 1.8 g / cm 3 , or 1.5 to 1.7 g / cm 3 The density of the upper second active material layer of the above-mentioned negative electrode may be 1.3 to 1.8 g / cm 3 , or 1.6 to 1.8 g / cm 3It can be. In the above range, cracking of the active material during the winding process can be prevented.
[0091] In one embodiment, the density difference between the upper first active material layer (112a) and the upper second active material layer (112b) is 0.03 to 0.2 g / cm 3 , or 0.05 to 0.1 g / cm 3 It can be. In the above range, separation of the upper first active material layer (112a) and the upper second active material layer (112b) due to density deviation can be prevented.
[0092] In some embodiments, the lower active material layer (114) includes a lower first active material layer (114a) and a lower second active material layer (114b), and the density of the lower first active material layer (114a) may be greater than the density of the lower second active material layer (114b).
[0093] In one embodiment, the lower first active material layer (114a) may be the lower first active material layer of the positive electrode reserve electrode, and the lower second active material layer (114b) may be the lower second active material layer of the positive electrode reserve electrode.
[0094] In this case, the density of the lower first active material layer of the positive electrode reserve electrode is 2.75 to 3.65 g / cm 3 , or 2.8 to 3.4 g / cm 3 The density of the lower second active material layer of the above-mentioned positive electrode may be 2.75 to 3.55 g / cm 3 , or 2.8 to 3.3 g / cm 3 It can be. In the above range, cracking of the active material during the winding process can be prevented.
[0095] In one embodiment, the lower first active material layer (114a) may be the lower first active material layer of the negative electrode reserve electrode, and the lower second active material layer (114b) may be the lower second active material layer of the negative electrode reserve electrode.
[0096] In this case, the density of the lower first active material layer of the negative electrode reserve electrode is 1.2 to 1.75 g / cm 3 , or 1.45 to 1.65 g / cm 3 The density of the lower second active material layer of the above-mentioned negative electrode may be 1.2 to 1.65 g / cm 3 , or 1.45 to 1.55 g / cm 3 It can be. In the above range, cracking of the active material during the winding process can be prevented.
[0097] In one embodiment, the density difference between the lower first active material layer (114a) and the upper second active material layer (114b) is 0.03 to 0.2 g / cm 3 , or 0.05 to 0.1 g / cm 3 It can be. In the above range, separation of the lower first active material layer (114a) and the lower second active material layer (114b) due to density deviation can be prevented.
[0098] In some embodiments, the first active material layer may be formed by coating a first slurry containing an active material on an electrode current collector (105), followed by drying and rolling. For example, the first slurry may be prepared by mixing the active material with a binder, a conductive agent, and / or a dispersant in a first solvent.
[0099] In some embodiments, the second active material layer may be formed by coating a second slurry containing an active material on the first active material layer, followed by drying and rolling. For example, the second slurry may be prepared by mixing the active material with a binder, a conductive agent, and / or a dispersant in a second solvent.
[0100] In one embodiment, the active material included in the first slurry may be the same active material as the active material included in the second slurry.
[0101] In some embodiments, the first solvent may be a different solvent from the second solvent. For example, the first solvent and the second solvent may have different solubilities for the active material.
[0102] In one embodiment, the second solvent may comprise a solvent that is phase-separable from the first solvent.
[0103] For example, the first solvent and the second solvent may have different polarities. Accordingly, the first slurry phase may be formed by the phase separation of the second slurry due to the difference in polarity between the first solvent and the second solvent.
[0104] For example, the density of the first solvent may be greater than that of the second solvent. Accordingly, the second slurry may be formed by phase separation on the first slurry due to the difference in density between the first solvent and the second solvent.
[0105] In some embodiments, the first slurry may include an upper first slurry forming an upper first active material layer (112a) and a lower first slurry forming a lower first active material layer (114a). The second slurry may include an upper second slurry forming an upper second active material layer (112b) and a lower second slurry forming a lower second active material layer (114b).
[0106] In one embodiment, the loading amount of the upper first slurry may be greater than the loading amount of the lower second slurry. For example, the difference in the loading amounts of the upper first slurry and the lower second slurry may be 0.07 to 1.3 mg / cm 2 , or 0.1 to 1.0 mg / cm 2 It could be.
[0107] In one embodiment, the loading amount of the upper second slurry may be greater than the loading amount of the lower first slurry. For example, the difference in the loading amounts of the upper second slurry and the lower first slurry may be 0.07 to 1.3 mg / cm 2 , or 0.1 to 1.0 mg / cm 2 It could be.
[0108] In some embodiments, the first solvent may include an upper first solvent included in the upper first slurry and a lower first solvent included in the lower first slurry. The second solvent may include an upper second solvent included in the upper second slurry and a lower second solvent included in the lower second slurry.
[0109] In one embodiment, the solubility of the active material in the upper first solvent may be less than the solubility of the active material in the upper second solvent. In this case, the amount of the active material included in the upper first slurry may be less than the amount of the active material included in the upper second slurry. Accordingly, the density of the upper first active material layer (112a) may be less than the density of the upper second active material layer (112b).
[0110] In one embodiment, the solubility of the active material in the lower first solvent may be greater than the solubility of the active material in the lower second solvent. In this case, the amount of the active material contained in the lower first slurry may be greater than the amount of the active material contained in the lower second slurry. Accordingly, the density of the lower first active material layer (114a) may be greater than the density of the lower second active material layer (114b).
[0111] FIG. 5 is a schematic plan view showing a secondary battery (200) according to exemplary embodiments.
[0112] Referring to FIG. 5, a secondary battery (200) can be manufactured by preparing an electrode assembly (100) and housing the electrode assembly (100) in an external case (210).
[0113] A secondary battery (200) may be defined by housing an electrode assembly (100) together with an electrolyte within an outer case (210). According to exemplary embodiments, a non-aqueous electrolyte may be used as the electrolyte.
[0114] The non-aqueous electrolyte contains a lithium salt as an electrolyte and an organic solvent, and the lithium salt is, for example, Li + X - is expressed as and the anion of the lithium salt (X - ) as F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It may include:
[0115] The organic solvent may include, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethylmethyl carbonate (EMC), methylpropyl carbonate, dipropyl carbonate, dimethylsulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, and tetrahydrofuran. These may be used alone or in combination of two or more.
[0116] As illustrated in FIG. 5, electrode tabs may protrude from the electrode current collectors belonging to each electrode cell and extend to one side of the outer case (210). The electrode tabs may be fused together with the one side of the outer case (210) and connected to electrode leads (160, 170) that extend or are exposed to the outside of the outer case (210).
[0117] The above lithium secondary battery (200) can be manufactured in a cylindrical, square, pouch or coin shape using a can, for example.
[0118] Hereinafter, specific experimental examples are presented to help understand the present disclosure, but these are only illustrative of the present invention and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the examples are possible within the scope and technical idea of the present disclosure, and it is natural that such changes and modifications fall within the scope of the appended claims.
[0119]
[0120] Examples and Comparative Examples
[0121] Example 1
[0122] 1) Manufacturing of cathode
[0123] A lower anode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive CNT in a solvent. The lower anode slurry was applied, dried, and rolled onto the first side of a Cu foil current collector to obtain a thickness of 1.55 g / cm. 3 A lower negative electrode active material layer having an active material density of was formed. Distilled water was used as the solvent.
[0124] The upper negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive CNT in a solvent. The upper negative electrode slurry was applied, dried, and rolled on the second side of the Cu foil current collector on which the upper negative electrode active material layer was formed to obtain a thickness of 1.65 g / cm. 3 A negative electrode for a secondary battery was manufactured by forming an upper negative electrode active material layer having an active material density of . Propylene carbonate (PC) was used as the solvent.
[0125] 2) Manufacturing of cylindrical cells
[0126] Lithium foil was used as the above-mentioned negative electrode and counter electrode, and a polyethylene (PE) separator was introduced between the negative electrode and counter electrode. Afterwards, the outermost portion was wound with a curvature of 2 and the first negative electrode active material layer was positioned inward, and an electrolyte was injected to produce a cylindrical cell.
[0127] Example 2
[0128] 1) Manufacturing of cathode
[0129] A lower first negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive CNT in a lower first solvent. The lower first negative electrode slurry was applied, dried, and rolled onto the first side of a Cu foil current collector to obtain a thickness of 1.58 g / cm. 3 A lower first negative electrode active material layer having an active material density of was formed. N-methyl-2-pyrrolidone (NMP) was used as the lower first solvent.
[0130] A lower second negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber (SBR), and 1 wt% of conductive CNT in a lower second solvent. The lower second negative electrode slurry was applied, dried, and rolled onto the lower first negative electrode active material layer to obtain a density of 1.5 g / cm. 3 A lower second negative electrode active material layer having an active material density of was formed. Ethanol was used as the lower second solvent.
[0131] 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive CNT were mixed in the upper first solvent to prepare an upper first negative electrode slurry. The upper first negative electrode slurry was applied to the second surface of a Cu foil current collector on which the lower first negative electrode active material layer and the lower second negative electrode active material layer were formed, dried, and rolled to obtain a thickness of 1.62 g / cm. 3 A second negative electrode active material layer having an active material density of was formed. The upper first solvent used was propylene carbonate (PC).
[0132] The upper second negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive CNT in the upper second solvent. The upper second negative electrode slurry was applied, dried, and rolled onto the upper first negative electrode active material layer to obtain a density of 1.7 g / cm. 3 A negative electrode for a secondary battery was manufactured by forming an upper second negative electrode active material layer having an active material density of . Distilled water was used as the upper second solvent.
[0133] 2) Manufacturing of cylindrical cells
[0134] Lithium foil was used as the above-mentioned negative electrode and counter electrode, and a polyethylene (PE) separator was introduced between the negative electrode and counter electrode. Afterwards, the outermost portion was wound with a curvature of 2 and the first negative electrode active material layer and the third negative electrode active material layer were positioned inward, and an electrolyte was injected to manufacture a cylindrical cell.
[0135] Example 3
[0136] The active material density of the lower first negative electrode active material layer is 1.6 g / cm 3 , the active material density of the upper first negative electrode active material layer is 1.65 g / cm 3 , the active material density of the lower second negative electrode active material layer is 1.55 g / cm 3 And the active material density of the upper second negative electrode active material layer is 1.7 g / cm 3 A cylindrical cell was manufactured in the same manner as in Example 2, except that the cathode slurry was applied, dried, and rolled.
[0137] Example 4
[0138] The active material density of the lower first negative electrode active material layer is 1.7 g / cm 3 , the active material density of the upper first negative electrode active material layer is 1.7 g / cm 3 , the active material density of the lower second negative electrode active material layer is 1.6 g / cm 3And the active material density of the upper second negative electrode active material layer is 1.8 g / cm 3 A cylindrical cell was manufactured in the same manner as in Example 2, except that the cathode slurry was applied, dried, and rolled.
[0139] Example 5
[0140] A cylindrical cell was manufactured in the same manner as in Example 2, except that the curvature of the outermost part was set to 1 during winding.
[0141] Example 6
[0142] A cylindrical cell was manufactured in the same manner as in Example 2, except that the curvature of the outermost part was set to 3 during winding.
[0143] Example 7
[0144] A cylindrical cell was manufactured in the same manner as in Example 2, except that the active materials mixed in the upper first slurry and the upper second slurry were 23 wt% natural graphite, 68 wt% artificial graphite, and 3 wt% carbide (SiC).
[0145] Comparative Example 1
[0146] 1) Manufacturing of cathode
[0147] A negative electrode slurry was prepared by mixing 24 wt% of natural graphite, 70 wt% of artificial graphite, 1 wt% of carboxymethyl cellulose (CMC), 4 wt% of styrene butadiene rubber, and 1 wt% of conductive CNT in distilled water. The negative electrode slurry was applied to a Cu foil current collector, dried, and rolled to obtain a density of 1.6 g / cm. 3 A negative electrode for a secondary battery was manufactured by forming a negative electrode active material layer having an active material density of .
[0148] 2) Manufacturing of cylindrical cells
[0149] Lithium foil was used as the cathode and counter electrode, and a polyethylene (PE) separator was introduced between the cathode and counter electrode. Afterwards, the cell was wound so that the curvature of the outermost part was 2, and an electrolyte was injected to produce a cylindrical cell.
[0150] Comparative Example 2
[0151] The active material density of the negative active material is 1.7 g / cm 3 A cylindrical cell was manufactured in the same manner as in Comparative Example 1, except that the cathode slurry was applied, dried, and rolled.
[0152] Comparative Example 3
[0153] The active material density of the negative active material is 1.5 g / cm 3 A cylindrical cell was manufactured in the same manner as in Comparative Example 1, except that the cathode slurry was applied, dried, and rolled.
[0154] Comparative Example 4
[0155] A cylindrical cell was manufactured in the same manner as in Comparative Example 1, except that the active material mixed in the negative electrode slurry was 23 wt% natural graphite, 68 wt% artificial graphite, and 3 wt% carbide (SiC).
[0156] The active materials used in the examples, the curvature of the outermost part, and the active material density before winding are shown in Table 1 below.
[0157] Cathode active material curvature average active material density (g / cm) 3) Lower (first) active material layer Upper (first) active material layer Lower second active material layer Upper second active material layer Example 1 Natural graphite and artificial graphite 21.55 1.65 -- Example 2 Natural graphite and artificial graphite 21.58 1.62 1.51.7 Example 3 Natural graphite and artificial graphite 21.6 1.65 1.55 1.7 Example 4 Natural graphite and artificial graphite 21.7 1.7 1.6 1.8 Example 5 Natural graphite and artificial graphite 11.58 1.62 1.51.7 Example 6 Natural graphite and artificial graphite 31.58 1.62 1.51.7 Example 7 Natural graphite, artificial graphite and carbide (SiC) 21.55 1.55 1.51.6
[0158] Experimental example
[0159] (1) Measurement of the density of the active material in the negative electrode active material layers after winding
[0160] After winding, the thickness, length, and width of the electrode were measured using a micrometer to calculate the volume of the wound cylindrical cell, and the active material density for the active material layer was measured using the active material weight value.
[0161] (2) Energy density measurement
[0162] The capacity measured by charging (CC-CV 1.0C 4.2V 0.05C CUT-OFF) and discharging (CC 1.0C 2.7V CUT-OFF) once for the battery cells according to the examples and comparative examples was converted into energy density.
[0163] (3) Measurement of life characteristics
[0164] For the battery cells according to the examples and comparative examples, charging (CC-CV 1.0C 4.2V CUT OFF) and discharging (1.0C 2.7V CUT-OFF) were repeated, and the number of cycles until a discharge capacity of 60% or less compared to the initial discharge capacity was measured was measured.
[0165] The evaluation results are shown in Table 2 below.
[0166] Average active material density (g / cm) 3) Energy density (Wh / L) Life characteristics (cycle) Lower (first) active material layer Upper (first) active material layer Lower second active material layer Upper second active material layer Example 11.61.6--500800 Example 21.61.61.65001,000 Example 31.611.621.61.635301,000 Example 41.721.651.71.7550800 Example 51.591.591.571.61500900 Example 61.611.611.591.63500900 Example 71.61.51.61.5550800 Comparative example 11.661.545--500500Comparative Example 21.761.645--550300Comparative Example 31.5551.44--450700Comparative Example 41.661.545--550300
[0167] Referring to Table 2, in examples where the density of the active material layer of the preliminary electrode increases from the center to the periphery using different solvents, the difference in density between the active material layers of the wound negative electrode is maintained small, thereby improving the life characteristics.
[0168] In Examples 3 to 7, in which the active material layers on both sides of the negative electrode collector were formed in two layers each, both the energy density and life characteristics were improved.
[0169] In Example 3, where the density difference between the active material layers of the preliminary negative electrode was configured to be constant, both the energy density and life characteristics were improved.
[0170] The difference in the density of the active material between the lower first active material layer and the upper first active material layer is 0.07 g / cm 3 In Examples 4 and 7, the life characteristics were somewhat deteriorated.
[0171] The difference in the density of the active material between the lower first active material layer and the upper first active material layer is 0.1 g / cm 3 In comparative examples exceeding , the life characteristics were deteriorated.
Claims
1. Step of preparing the electrode collector; A step of forming a preliminary electrode by forming an upper active material layer on the upper surface of the electrode current collector and forming a lower active material layer having a lower density than the upper active material layer on the lower surface of the electrode current collector; and A method for manufacturing an electrode assembly for a secondary battery, comprising the step of forming a rolled electrode including a rolled upper active material layer and a rolled lower active material layer by rolling the preliminary electrode with the lower active material layer facing inward.
2. A method for manufacturing an electrode assembly for a secondary battery according to claim 1, wherein the density of the upper active material layer is lower than the density of the upper active material layer, and the density of the lower active material layer is higher than the density of the lower active material layer.
3. A method for manufacturing an electrode assembly for a secondary battery, wherein, in claim 1, the difference in density between the upper active material layer and the lower active material layer is smaller than the difference in density between the upper active material layer and the lower active material layer.
4. In claim 3, the difference in density between the upper winding active material layer and the lower winding active material layer is 0.1 g / cm 3 Below, a method for manufacturing an electrode assembly for a secondary battery.
5. In claim 1, forming the upper active material layer and the lower active material layer includes coating the upper slurry and the lower slurry containing a solvent and an active material, respectively, on the upper surface and the lower surface of the electrode current collector, A method for manufacturing an electrode assembly for a secondary battery, wherein the solvent used in the upper slurry is different from the solvent used in the lower slurry.
6. A method for manufacturing an electrode assembly for a secondary battery, wherein the step of forming the preliminary electrode according to claim 1 comprises forming at least one of the upper active material layer and the lower active material layer into a multi-layer structure having different densities.
7. In claim 6, forming the multi-layer structure comprises; Forming a first active material layer on the surface of the electrode current collector; and A method for manufacturing an electrode assembly for a secondary battery, comprising forming a second active material layer on the first active material layer, the second active material layer being spaced apart from the electrode current collector and the first active material layer and having a different density from the first active material layer.
8. In claim 7, forming the first active material layer includes applying a first slurry containing a first solvent and a first active material, A method for manufacturing an electrode assembly for a secondary battery, wherein forming the second active material layer includes applying a second slurry containing a second solvent different from the first solvent and a second active material on the first active material layer.
9. A method for manufacturing an electrode assembly for a secondary battery, wherein the second solvent comprises a solvent that is phase-separable from the first solvent in claim 8.
10. In claim 8, the upper active material layer includes the first active material layer and the second active material layer, A method for manufacturing an electrode assembly for a secondary battery, wherein the density of the second active material layer is greater than the density of the first active material layer.
11. In claim 8, the lower active material layer includes the first active material layer and the second active material layer, A method for manufacturing an electrode assembly for a secondary battery, wherein the density of the first active material layer is greater than the density of the second active material layer.
12. A method for manufacturing an electrode assembly for a secondary battery according to claim 8, wherein the first active material and the second active material are the same active material.
13. A method for manufacturing an electrode assembly for a secondary battery according to claim 12, wherein the first solvent and the second solvent have different solubilities for the active material.
14. In claim 1, further comprising a step of arranging the spare electrodes on the first and second faces of the separator, which face each other, A method for manufacturing an electrode assembly for a secondary battery, wherein the separator is wound together with the spare electrode.
15. A step of preparing an electrode assembly manufactured according to claim 1; and A method for manufacturing a secondary battery, comprising the step of housing the electrode assembly within a case.
Citation Information
Patent Citations
Power storage device, secondary battery, and electrode manufacturing method
JP2014102896A
Nonaqueous electrolyte secondary battery having wound electrode body
JP2017130317A
Non-aqueous electrolyte secondary battery
JP5884039B2
Electrode having porous coating layer and electrochemical device containing the same
KR1020130114926A
Electrode structure and lithium battery including the same
KR1020150133554A