Electrode assembly and method for manufacturing same
The electrode assembly with an adhesive-coated single-sided anode and zigzag-folded separators, manufactured at low pressure and temperature, effectively addresses battery life degradation and resistance issues, ensuring efficient energy storage and extended battery life.
Patent Information
- Application Number
- PCT/KR2024/095750
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-24
AI Technical Summary
The challenge is to manufacture an electrode assembly with a single-sided anode at low pressure and temperature to prevent battery life degradation due to Li-precipitation and resistance increase, while maintaining the energy density and cycle life of lithium secondary batteries.
The electrode assembly includes a single-sided anode with an adhesive coating layer and a zigzag-folded separator, where n+1 cathodes and n anodes are alternately arranged between 2n second separators, and the assembly is manufactured at temperatures below 90°C and pressures below 6.5 MPa, using a polyvinylidene-based resin as the polymer binder to ensure adhesion and prevent curling.
This method prevents battery life deterioration and resistance increase by maintaining the structural integrity and adhesion of the electrodes at low assembly conditions, improving manufacturing efficiency and extending battery life.
Smart Images

Figure KR2024095750_24102024_PF_FP_ABST
Abstract
Description
Electrode assembly and method for manufacturing the same
[0001] This invention claims the benefit of patent application No. 10-2023-0052674 filed with the Korean Intellectual Property Office on April 21, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to an electrode assembly and a method for manufacturing the same, and more particularly, to an electrode assembly comprising a cross-sectional positive electrode and manufacturing the electrode assembly at low pressure and temperature to prevent degradation of battery life due to Li precipitation and resistance increase, and a method for manufacturing the same.
[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions. Recently, lithium secondary batteries have become widely used due to their high energy density and voltage, long cycle life, and wide range of applications. With the increasing demand for electric vehicles and energy storage devices, development is underway on materials and structures to maximize capacity and energy density.
[0004] A secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and may be manufactured by housing the electrode assembly in a case together with an electrolyte. Secondary batteries may be classified into pouch-type, cylindrical, square, coin-type, etc. depending on the shape of the case in which the electrode assembly is housed, and may be classified into jelly-roll type, stack type, etc. depending on the manufacturing method or shape of the electrode assembly.
[0005] Recently, a zigzag stacking (ZZS) electrode assembly has been developed, which folds a long sheet-shaped separator in a zigzag shape and alternately places positive and negative electrodes between adjacent folds. For example, a zigzag electrode assembly can be manufactured by tilting or swinging a table on which electrode assemblies are stacked, or by reciprocating a feed roll that transports the separator, to fold the separator in a zigzag shape and place each electrode between the folds when a long sheet-shaped separator is supplied wound on a cylinder. Zigzag stacking has the advantage of being simple in process and thus highly productive compared to other types.
[0006] Meanwhile, one method to increase the energy density of a battery is to place single-sided positive electrodes at both ends of the battery. However, single-sided positive electrodes are very curled, so assembling them requires pressing at very high pressure and temperature for a long time. In this case, the pores of the electrodes and separator can become clogged due to the high pressure and temperature, resulting in poor wettability and increased resistance in the battery. Furthermore, if the battery is manufactured under weak conditions, the single-sided positive electrodes at both ends of the battery will curl, and as the cycle is repeated, the gap between the electrodes will rise, causing lithium precipitation in the affected area and increased resistance, resulting in deterioration of the battery life.
[0007] Accordingly, there was a need for a method to solve the above problem even under low pressure and temperature conditions while using a single-sided anode.
[0008] The technical problem to be achieved by the present invention is to provide an electrode assembly including a cross-sectional positive electrode and a method for manufacturing the same, which can prevent degradation of battery life due to Li precipitation and resistance increase by manufacturing the electrode assembly at low pressure and temperature.
[0009] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.
[0010] One embodiment of the present invention provides an electrode assembly including a cross-sectional anode provided at both ends and a unit electrode assembly provided between the cross-sectional anodes, and a first separator provided between the cross-sectional anodes and the unit electrode assembly, wherein the unit electrode assembly has n+1 cathodes and n anodes alternately arranged between 2n second separators (n is a positive integer), and an outer portion of a surface of the cross-sectional anode facing the first separator is provided with an adhesive coating layer including a first polymer binder on at least a portion thereof.
[0011] According to one embodiment of the present invention, the first separator and the second separator may be formed as a single separator folded in a zigzag pattern.
[0012] According to one embodiment of the present invention, the area of the adhesive coating layer provided on the cross-sectional anode may be 10% or more and 20% or less of the total area of the surface of the cross-sectional anode facing the first separator.
[0013] According to one embodiment of the present invention, the thickness of the adhesive coating layer may be 10% or more and 100% or less of the thickness of the first separator.
[0014] According to one embodiment of the present invention, the entire surface of the cross-sectional anode facing the first separator may be provided with an adhesive coating layer in a predetermined pattern.
[0015] According to one embodiment of the present invention, the first polymer binder may be a polyvinylidene resin.
[0016] According to one embodiment of the present invention, the first polymer binder may be a copolymer of polyvinylidene propylene and hexafluoropropylene.
[0017] According to one embodiment of the present invention, the substitution rate of the hexafluoropropylene in the first polymer binder may be 20% or more.
[0018] According to one embodiment of the present invention, the cross-sectional anode includes a second polymer binder, the separator is provided on at least one surface, and includes a porous coating layer including a third polymer binder and inorganic particles, and each of the second polymer binder and the third polymer binder included in the cross-sectional anode and the porous coating layer may be the same as the first polymer binder included in the adhesive coating layer.
[0019] One embodiment of the present invention provides a method for manufacturing an electrode assembly, comprising: a step of providing 2n second separators between first separators at both ends; a step of preparing a laminate by providing n+1 cathodes and n anodes alternately between the first separators and the second separators, and providing a single-sided anode having an adhesive coating layer on an outer portion on the first separators at both ends; and a step of manufacturing an electrode assembly by applying heat and pressure to the laminate.
[0020] According to one embodiment of the present invention, the step of manufacturing the electrode assembly may be to assemble the electrode assembly at a temperature of less than 90°C and a pressure of less than 6.5 MPa.
[0021] According to one embodiment of the present invention, the step of providing the separator may be to provide one separator by folding it in a zigzag pattern.
[0022] An electrode assembly according to one embodiment of the present invention includes a cross-sectional positive electrode including an adhesive coating layer, thereby preventing degradation of battery life due to Li precipitation and resistance increase even when the electrode assembly is assembled at low pressure and temperature.
[0023] A method for manufacturing an electrode assembly according to an embodiment of the present invention can prevent degradation of battery life due to Li precipitation and resistance increase by manufacturing the electrode assembly at low pressure and temperature, and can increase manufacturing ease by shortening the battery manufacturing time.
[0024] Figure 1 is a schematic diagram of an electrode assembly of a comparative example.
[0025] Figure 2 is a schematic diagram of Li precipitation occurring at the cross-sectional anode of Comparative Example 2.
[0026] Figure 3 is a schematic diagram of a cross-sectional anode having an adhesive coating layer according to one embodiment of the present invention.
[0027] Figure 4 is a schematic diagram of an electrode assembly according to one embodiment of the present invention.
[0028] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0029] In this specification, “A and / or B” means “A and B, or A or B.”
[0030] The term "comprises" as used herein is used to list materials, compositions, devices, and methods useful in the present invention, but is not limited to the listed examples.
[0031] In this specification, when it is said that a component is “provided on”, this does not exclude other components being placed in between, unless otherwise specifically stated, and it means that other components may be further placed.
[0032] Hereinafter, an embodiment of the present invention will be described in detail with reference to the attached drawings. The drawings may be exaggerated, omitted, or schematically illustrated to explain or emphasize the contents of an embodiment of the present invention.
[0033]
[0034] One embodiment of the present invention provides an electrode assembly (100) including a cross-sectional anode (110) provided at both ends and a unit electrode assembly (130) provided between the cross-sectional anode (110), and a first separator (111) provided between the cross-sectional anode (110) and the unit electrode assembly (130), wherein the unit electrode assembly (130) has n+1 cathodes (135) and n anodes (137) alternately arranged between 2n second separators (133, n is a positive integer), and an outer portion of a surface of the cross-sectional anode (110) facing the first separator (111) is provided with an adhesive coating layer (113) including a first polymer binder at least in a portion thereof.
[0035] An electrode assembly according to one embodiment of the present invention includes a cross-sectional positive electrode including an adhesive coating layer, so that the cross-sectional positive electrode has adhesive strength, and thus even when the electrode assembly is assembled at low pressure and temperature, degradation of battery life due to Li precipitation and resistance increase can be prevented.
[0036] According to one embodiment of the present invention, the unit electrode assembly may be manufactured by thermally compressing a laminate in which the positive electrode and the negative electrode are alternately arranged between zigzag-folded separators.
[0037] According to one embodiment of the present invention, the separator (meaning the first separator (111) and / or the second separator (133)) may mean a functional separator in which a porous coating layer including an inorganic substance and a binder (third polymer binder) is formed on at least one surface of a porous polymer substrate such as a polyolefin substrate or a non-woven fabric, but is not limited thereto. The separator may also refer to a free-standing separator formed of an inorganic substance and a binder (third polymer binder) without a porous polymer substrate.
[0038] According to one embodiment of the present invention, the separator (meaning the first separator and / or the second separator) electrically insulates the positive electrode and the negative electrode to prevent a short circuit, while providing pores through which lithium ions can pass. The separator may have resistance to the electrolyte of the electrochemical device, which is an organic solvent. For example, the separator may include a porous polymer substrate, and specifically, the porous polymer substrate may include a polymer resin such as a polyolefin-based resin such as polyethylene, polypropylene, and polybutene, polyvinyl chloride, polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, polyaramid, polycycloolefin, nylon, polytetrafluoroethylene, and copolymers or mixtures thereof, but is not limited thereto.
[0039] According to one embodiment of the present invention, a slurry may be applied and dried on at least one surface of the separator (meaning the first separator and / or the second separator) to form a porous coating layer. The slurry may include a polymer binder (a third polymer binder), inorganic particles, a dispersion medium, etc. The porous coating layer may include inorganic particles for improving the mechanical properties and insulating properties of the separator and a polymer binder for improving the adhesive force between the electrode and the separator. The polymer binder may provide adhesive force between the electrode and the separator, and may bind adjacent inorganic particles and maintain the bond. The inorganic particles may bind to adjacent inorganic particles to provide an interstitial volume, which is a void between the inorganic particles, and lithium ions may move through the interstitial volume.
[0040] According to one embodiment of the present invention, the polymer binder (third polymer binder) may be any binder known in the art, such as an acrylic binder or a fluorine-based binder. As described below, preferably, the polymer binder (third polymer binder) may be a fluorine-based binder.
[0041] According to one embodiment of the present invention, the inorganic particles may be those known in the art that can have one or more of the following properties: lithium ion transfer capability, piezoelectricity, and flame retardancy. Specifically, the inorganic particles may be BaSO4, BaTiO3, Pb(Zr, Ti)O3(PZT), b1-xLaxZr1-yTiyO3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), boehmite (AlO(OH)) and combinations thereof, but this is only an example and is not limited thereto.
[0042] According to one embodiment of the present invention, the total content of the inorganic particles may be greater than 75 parts by weight with respect to 100 parts by weight of the adhesive coating layer, but is not limited thereto.
[0043] According to one embodiment of the present invention, the unit electrode assembly (130) has n+1 cathodes (135) and n anodes (137) alternately arranged between 2n second separators (133, where n is a positive integer). Specifically, since the anodes (137) and the cathodes (135) have second separators (133) adhered to both surfaces, 2n second separators (133) are formed. In addition, since the single-sided anodes (110) adjacent to the first separator (111) are provided at both ends of the electrode assembly (100), the unit electrode assembly (130) provided between the single-sided anodes (110) provided at both ends has cathodes (135) positioned at both ends. Accordingly, the unit electrode assembly (130) is arranged with n+1 cathodes (135) and n anodes (137) alternately.
[0044] According to one embodiment of the present invention, the positive electrode and the negative electrode may mean that an electrode active material is applied to at least one surface of a material having conductivity without causing a chemical change in the electrochemical device and then dried. The types of the material and the electrode active material are not limited as long as they can be used in an electrochemical device.
[0045] According to one embodiment of the present invention, the thickness of the positive electrode (137) may be 90 ㎛ or more and 130 ㎛ or less. Specifically, the thickness of the positive electrode may be 90 ㎛ or more and 125 ㎛ or less, 90 ㎛ or more and 120 ㎛ or less, 90 ㎛ or more and 115 ㎛ or less, 90 ㎛ or more and 110 ㎛ or less, or 95 ㎛ or more and 105 ㎛ or less. By controlling the thickness of the positive electrode within the above-described range, the ease of assembly of the electrode assembly can be increased, the desired capacity of the battery can be secured, and performance degradation of the battery can be prevented.
[0046] According to one embodiment of the present invention, the thickness of the negative electrode (135) may be 100 ㎛ or more and 150 ㎛ or less. Specifically, the thickness of the negative electrode may be 105 ㎛ or more and 145 ㎛ or less, 110 ㎛ or more and 140 ㎛ or less, 115 ㎛ or more and 135 ㎛ or less, 120 ㎛ or more and 135 ㎛ or less, or 125 ㎛ or more and 135 ㎛ or less. By controlling the thickness of the negative electrode within the above-described range, the ease of assembly of the electrode assembly can be increased, the desired capacity of the battery can be secured, and at the same time, performance degradation of the battery can be prevented.
[0047] According to one embodiment of the present invention, the thickness of the cross-sectional positive electrode (110) may be 50 ㎛ or more and 70 ㎛ or less. Specifically, the thickness of the cross-sectional positive electrode may be 55 ㎛ or more and 65 ㎛ or less. By controlling the thickness of the cross-sectional positive electrode within the above-described range, the ease of assembly of the electrode assembly can be increased and the performance degradation of the battery can be prevented.
[0048] According to one embodiment of the present invention, an adhesive coating layer including a first polymer binder is provided on at least a portion of the outer surface of the surface facing the first separator in the single-sided positive electrode. Fig. 1 is a schematic diagram of an electrode assembly (10) of a comparative example. According to Fig. 1, an adhesive coating layer is not provided on the single-sided positive electrode (11). Fig. 2 is a schematic diagram of Li precipitation occurring in the single-sided positive electrode (11) of comparative example 2. According to Fig. 2, when the adhesive coating layer is not provided on the single-sided positive electrode and a battery is manufactured under weak conditions, the single-sided positive electrodes at both ends of the battery curl, and as the cycle is repeated, the gap between the electrodes becomes lifted, resulting in deterioration of the battery life due to Li precipitation and an increase in resistance in that portion.
[0049] Meanwhile, Fig. 3 is a schematic diagram of a single-sided positive electrode (110) provided with an adhesive coating layer (113) of Example 1 according to an embodiment of the present invention. Fig. 4 is a schematic diagram of an electrode assembly (100) according to an embodiment of the present invention. According to Figs. 3 and 4, unlike Comparative Example 1, it can be seen that an adhesive coating layer is formed on the single-sided positive electrode. As described above, since the outer portion of the surface facing the first separator in the single-sided positive electrode is provided with an adhesive coating layer including the first polymer binder on at least a portion thereof, even when the electrode assembly is assembled at low pressure and temperature, degradation of battery life due to Li precipitation and resistance increase can be prevented.
[0050] According to one embodiment of the present invention, the first separator (111) and the second separator (133) may be formed as a single separator folded in a zigzag pattern. Specifically, the single separator may be folded in a zigzag pattern at a predetermined interval. In this case, the first separator and the second separator are not separate, independent components, but are connected as a single separator and are only defined differently depending on the position. The interval is not limited as long as it can prevent the positive electrode and the negative electrode from contacting each other, but is preferably a constant interval. The electrodes are laminated with both sides covered by the separator, and can be bonded to the adjacent separator by the thermal compression. The fact that the positive electrode and the negative electrode are bonded to the adjacent separator respectively means that the electrode and the separator are bonded within a single electrode assembly. As described above, the first separator and the second separator are formed as a single separator folded in a zigzag pattern and manufactured in a zigzag stacking manner, thereby enabling a more stable electrode assembly to be realized.
[0051] According to one embodiment of the present invention, the area of the adhesive coating layer (113) provided on the single-sided positive electrode (110) may be 10% or more and 20% or less of the total area of the surface of the single-sided positive electrode (110) facing the first separator (111). Specifically, the area of the adhesive coating layer provided on the single-sided positive electrode may be 10% or more and 20% or less, 11% or more and 19% or less, 12% or more and 18% or less, 13% or more and 17% or less, or 14% or more and 16% or less of the total area of the surface of the single-sided positive electrode facing the first separator. By controlling the area ratio of the adhesive coating layer within the above-described range, curling of the single-sided positive electrode can be prevented and degradation of battery life due to partial Li precipitation and resistance increase can be prevented.
[0052] According to one embodiment of the present invention, the thickness of the adhesive coating layer (113) may be 10% or more and 100% or less of the thickness of the first separator (111). Specifically, the thickness of the adhesive coating layer may be 15% or more and 95% or less, 20% or more and 90% or less, 25% or more and 85% or less, 30% or more and 80% or less, 35% or more and 75% or less, 40% or more and 70% or less, 45% or more and 65% or less, or 50% or more and 60% or less. As described above, by controlling the thickness of the adhesive coating layer with respect to the thickness of the first separator, the assembly of the electrode assembly can be facilitated, and the single-sided positive electrode and the first separator can be uniformly adhered to prevent degradation of the battery life due to Li precipitation and resistance increase.
[0053] According to one embodiment of the present invention, the thickness of the adhesive coating layer (113) may be 1 ㎛ or more and 20 ㎛ or less. Specifically, the thickness of the adhesive coating layer may be 2 ㎛ or more and 19 ㎛ or less, 3 ㎛ or more and 18 ㎛ or less, 4 ㎛ or more and 17 ㎛ or less, 5 ㎛ or more and 16 ㎛ or less, 6 ㎛ or more and 15 ㎛ or less, 7 ㎛ or more and 14 ㎛ or less, 8 ㎛ or more and 13 ㎛ or less, 9 ㎛ or more and 12 ㎛ or less, or 10 ㎛ or more and 11 ㎛ or less. By controlling the thickness of the adhesive coating layer within the above-described range, the thickness of the single-sided positive electrode can be controlled while exerting adhesive force, thereby preventing degradation of the battery life due to Li precipitation and resistance increase even when the electrode assembly is assembled at low pressure and temperature.
[0054] According to one embodiment of the present invention, the thickness of the first separator (111) may be 5 ㎛ or more and 30 ㎛ or less. Specifically, the thickness of the first separator may be 10 ㎛ or more and 25 ㎛ or less or 15 ㎛ or more and 20 ㎛ or less, and preferably 15 ㎛. By controlling the thickness of the first separator within the above-described range, the volume of the electrode assembly can be minimized, and the positive and negative electrodes can be electrically insulated.
[0055] Furthermore, the thickness of the second separator (133) may be the same as the thickness of the first separator (111). In addition, if the first separator and the second separator are formed as a single separator folded in a zigzag pattern, it is obvious that the thicknesses of the first separator and the second separator are the same.
[0056] In one embodiment of the present invention, the thickness of the separator and the adhesive coating layer can be measured using a contact thickness measuring device. For example, the contact thickness measuring device can be the VL-50S-B from Mitutoyo.
[0057] According to one embodiment of the present invention, the entire surface of the cross-sectional positive electrode (110) facing the first separator (111) may be provided with an adhesive coating layer (113) in a predetermined pattern. According to FIGS. 3 and 4, the adhesive coating layer (113) provided on the cross-sectional positive electrode (110) has a certain shape, but this is merely an example and is not limited thereto. As described above, the entire surface of the cross-sectional positive electrode facing the first separator is provided with an adhesive coating layer in a predetermined pattern, thereby increasing the adhesive strength between the cross-sectional positive electrode and the first separator and preventing degradation of battery life due to Li precipitation and resistance increase.
[0058] According to one embodiment of the present invention, the first polymer binder may be a polyvinylidene-based resin. As described above, by selecting the first polymer binder as a polyvinylidene-based resin, the porosity of the first polymer separator can be maintained, and even if the coating layer is wetted by the electrolyte after activation of the battery, the adhesive strength can be maintained. Furthermore, the stiffness of the battery can be improved, and bending of the single-sided positive electrode can be prevented, thereby preventing degradation of the battery life due to Li precipitation and increased resistance.
[0059] According to one embodiment of the present invention, the first polymer binder may be a copolymer of polyvinylidene propylene and hexafluoropropylene.
[0060] According to one embodiment of the present invention, the substitution rate of the hexafluoropropylene in the first polymer binder may be 20% or more. Specifically, the substitution rate of the hexafluoropropylene in the first polymer binder may be 20% or more by weight and 50% or less by weight, 25% or more by weight and 45% or less by weight, or 30% or more by weight and 40% or less by weight. As described above, by selecting the substitution rate of the hexafluoropropylene in the first polymer binder to be 20% or more, the adhesion between the single-sided positive electrode and the first separator can be increased while maintaining the porosity of the separator, and the adhesion can be maintained even when the coating layer is wetted by the electrolyte after activation of the battery.
[0061] According to one embodiment of the present invention, the single-sided positive electrode includes a second polymer binder, the separator is provided on at least one surface, and includes a porous coating layer including a third polymer binder and inorganic particles, and each of the second and third polymer binders included in the single-sided positive electrode and the porous coating layer may be the same as the first polymer binder included in the adhesive coating layer. As described above, by configuring the first polymer binder, the second polymer binder, and the third polymer binder to be the same, the adhesive strength of the adhesive coating layer and the single-sided positive electrode and the adhesive coating layer and the first separator is increased, so that even when the battery assembly is assembled at low pressure and temperature, degradation of the battery life due to Li precipitation and resistance increase can be prevented.
[0062] According to one embodiment of the present invention, the electrode assembly (100) can be applied to an electrochemical device. The electrochemical device can be manufactured by inserting the electrode assembly into a pouch or case, injecting an electrolyte, and then sealing the pouch or case.
[0063] According to one embodiment of the present invention, the electrolyte may be a non-aqueous electrolyte containing a lithium salt. The electrolyte is composed of an electrolyte and a lithium salt, and a non-aqueous organic solvent, an organic solid electrolyte, an inorganic solid electrolyte, etc. may be used as the electrolyte.
[0064] According to one embodiment of the present invention, the shape of the case or pouch for inserting the electrode assembly is not limited. For example, the electrochemical device may be a cylindrical, square, coin-shaped, or pouch-shaped lithium secondary battery. The lithium secondary battery may be packaged or modularized as a unit cell and used in small devices such as computers, mobile phones, and power tools; power tools that are powered by an electric motor and move; electric vehicles including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and medium to large devices such as power storage systems.
[0065] One embodiment of the present invention provides a method for manufacturing an electrode assembly, including the steps of: providing 2n second separators (133) between first separators (111) at both ends; providing n+1 cathodes (135) and n anodes (137) alternately between the first separators (111) and the second separators (133), and providing a single-sided anode (110) having an adhesive coating layer (113) provided on the outer portion on the first separators (111) at both ends to prepare a laminate; and applying heat and pressure to the laminate to manufacture an electrode assembly (100). In the description of the method for manufacturing the electrode assembly, the same content as the description of the electrode assembly described above is replaced with the description of the preceding embodiment.
[0066] A method for manufacturing an electrode assembly according to an embodiment of the present invention can prevent degradation of battery life due to Li precipitation and resistance increase by manufacturing the electrode assembly at low pressure and temperature, and can increase manufacturing ease by shortening the battery manufacturing time.
[0067] According to one embodiment of the present invention, a step of providing 2n second separators between first separators at both ends is included. Since the positive electrode and the negative electrode are bonded with second separators on both sides, the 2n second separators are required.
[0068] According to one embodiment of the present invention, the second separator may form a unit electrode assembly by stacking each cut separator in the order of second separator, cathode, second separator, anode, second separator, cathode, second separator (when n=1), but this is merely an example and is not limited thereto.
[0069] According to one embodiment of the present invention, a step of preparing a laminate is provided, wherein n+1 cathodes and n anodes are alternately provided between the first separator and the second separator, and single-sided anodes are provided on the first separator at both ends. Specifically, the thickness of the laminate may be 2 mm or more and 9.5 mm or less. Specifically, the thickness of the laminate may be 2.5 mm or more and 9 mm or less, 3 mm or more and 8.5 mm or less, 3.5 mm or more and 8 mm or less, 4 mm or more and 7.5 mm or less, 4.5 mm or more and 7 mm or less, or 5 mm or more and 6.5 mm or less. By controlling the thickness of the laminate within the above-described range, all electrodes and separators constituting the laminate can implement uniform adhesive strength through thermocompression.
[0070] According to one embodiment of the present invention, a step of manufacturing an electrode assembly by applying heat and pressure to the laminate is included. Specifically, by applying heat and pressure to the laminate, the positive electrode and the separator are bonded, and the negative electrode and the separator are bonded, thereby manufacturing a single unit electrode assembly. The thermocompression bonding may be performed by compressing the uppermost and lowermost ends of the laminate using a press device. The type of the press device is not limited as long as it can simultaneously or simultaneously apply heat and pressure to one or both sides of the laminate while maintaining the alignment of the separator and the electrode included in the laminate to bond the separator and the electrode.
[0071] According to one embodiment of the present invention, a step of preparing an adhesive coating layer including a first polymer binder before the step of preparing the laminate or on the outer portion of the single-sided positive electrode may be further included. As described above, by further including a step of preparing an adhesive coating layer including a first polymer binder before the step of preparing the laminate or on the outer portion of the single-sided positive electrode, even when the electrode assembly is assembled at low pressure and temperature due to adhesive force on the single-sided positive electrode, degradation of battery life due to Li precipitation and resistance increase can be prevented.
[0072] According to one embodiment of the present invention, in the step of preparing the laminate, the single-sided anode including an adhesive coating layer on the outer portion on the first separator at both ends may be provided such that the first separator and the outer portion face each other. By providing the single-sided anode as described above, since the single-sided anode has adhesive strength, even when the electrode assembly is assembled at low pressure and temperature, degradation of the battery life due to Li precipitation and resistance increase can be prevented.
[0073] According to one embodiment of the present invention, the step of manufacturing the electrode assembly may be to assemble the electrode assembly at a temperature of less than 90°C and a pressure of less than 6.5 MPa.
[0074] Specifically, the temperature may be 45°C or more and less than 90°C, 50°C or more and 85°C or less, 55°C or more and 85°C or less, or 60°C or more and 85°C or less. Specifically, the pressure may be 3 MPa or more and less than 6.5 MPa, 3 MPa or more and 6.0 MPa or less, or 3 MPa or more and 5.5 MPa or less. If it is less than the above range, the position of the electrode is not fixed, and the electrodes may deviate from the set position during the handling of the laminate. If it is more than the above range, the coating layer formed on the electrode may be destroyed, or the pore structure formed on the separator may collapse, which may cause problems with the air permeability and electrical resistance of the separator.
[0075] By controlling the temperature and pressure conditions of thermocompression within the above-described range, the adhesion of the separator and electrodes constituting the laminate can be achieved without causing damage to the laminate, thereby preventing degradation of battery life due to Li precipitation and resistance increase.
[0076] According to one embodiment of the present invention, the step of providing the separator may be to prepare a separator by folding it in a zigzag pattern. Furthermore, a laminate may be prepared by alternately arranging positive and negative electrodes between the folds formed by folding the separator in a zigzag pattern. The step of manufacturing an electrode assembly by applying heat and pressure to the laminate may be identical to the above procedure.
[0077] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0078]
[0079] <Example 1>
[0080] A 15 ㎛ thick separator coated with a slurry containing an inorganic substance and a binder was prepared, and 30 and 31 100 ㎛ thick anodes and 130 ㎛ thick cathodes were prepared, respectively. The separator was folded in a zigzag pattern at 98.5 mm intervals, and the anodes and cathodes were alternately arranged between the separators, and a single-sided anode (60 ㎛ thick) having an adhesive coating layer (5 ㎛ thick) provided on the separator at both ends was prepared to prepare a laminate.
[0081] The above laminate was placed on a press device and subjected to thermal compression once at 60°C and a pressure of 4.5 MPa for 20 seconds to manufacture an electrode assembly.
[0082]
[0083] <Example 2>
[0084] The same laminate as in Example 1 was prepared.
[0085] The above laminate was placed on a press device and subjected to thermal compression once at 70°C and a pressure of 5.5 MPa for 10 seconds to manufacture an electrode assembly.
[0086]
[0087] <Example 3>
[0088] The same laminate as in Example 1 was prepared.
[0089] The above laminate was placed on a press device and subjected to thermal compression once at 85°C and a pressure of 3.0 MPa for 10 seconds to manufacture an electrode assembly.
[0090]
[0091] <Comparative Example 1>
[0092] A laminate was prepared in the same manner as in Example 1, except that a single-sided anode without an adhesive coating layer was used.
[0093] The above laminate was placed on a press device and subjected to thermal compression once at 90°C and a pressure of 6.5 MPa for 20 seconds to manufacture an electrode assembly.
[0094]
[0095] Comparative Example 2
[0096] A laminate was prepared in the same manner as in Example 1, except that a single-sided anode without an adhesive coating layer was used.
[0097] The above laminate was placed on a press device and subjected to thermal compression once at 60°C and a pressure of 4.5 MPa for 20 seconds to manufacture an electrode assembly.
[0098]
[0099] Experimental Example 1
[0100] The manufacturing process of the electrode assembly manufactured in the above examples and comparative examples, the time required for manufacturing the electrode assembly, and whether lithium (Li) was precipitated after manufacturing are summarized in Table 1 below.
[0101]
[0102] Experimental Example 2
[0103] Electrical resistance was measured by fabricating a cell using the electrode assembly manufactured in the above examples and comparative examples, leaving the cell at room temperature for one day, and then measuring the resistance of the electrode assembly separator using an impedance measurement method. The measured resistance values (mΩ) are summarized in Table 1 below.
[0104]
[0105] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Temperature (℃) 60 70 85 90 60 Pressure (MPa) 4.5 5.5 36.5 4.5 Manufacturing time (sec) 20 10 10 20 20 Resistance of the membrane (mΩ) 1.3 0 1.3 5 1.3 0 2.1 0 2.8 Whether Li is precipitated after manufacturing XXXXO
[0106]
[0107] Figure 2 is a schematic diagram of Li precipitation occurring on the cross-sectional anode of Comparative Example 2. According to Figure 2, it can be seen that Li precipitation occurs when the adhesive coating layer is not provided on the cross-sectional anode and the battery is manufactured under weak conditions.
[0108] Meanwhile, Fig. 3 is a schematic diagram of a cross-sectional positive electrode provided with an adhesive coating layer according to Examples 1 to 3. Fig. 4 is a schematic diagram of an electrode assembly according to Examples 1 to 3. According to Figs. 3 and 4, unlike the comparative example, since an adhesive coating layer is provided on the cross-sectional positive electrode, Li precipitation does not occur even when the electrode assembly is assembled at low pressure and temperature.
[0109] <Explanation of symbols>
[0110] 10, 100: Electrode assembly
[0111] 11, 110: Single-sided anode
[0112] 13, 130: Unit electrode assembly
[0113] 1, 111: First membrane
[0114] 113: Adhesive coating layer
[0115] 3, 133: Second membrane
[0116] 5, 135: Cathode
[0117] 7, 137: Bipolar
Claims
1. An electrode assembly comprising a cross-sectional anode provided at both ends and a unit electrode assembly provided between the cross-sectional anodes, and a first separator provided between the cross-sectional anodes and the unit electrode assembly, The above unit electrode assembly is formed by alternately arranging n+1 cathodes and n anodes between 2n second separators (n is a positive integer). An electrode assembly, wherein the outer surface of the surface facing the first separator in the above cross-sectional anode is provided with an adhesive coating layer including a first polymer binder on at least a portion thereof.
2. In claim 1, An electrode assembly wherein the first separator and the second separator are formed as a single separator folded in a zigzag pattern.
3. In claim 1, An electrode assembly, wherein the area of the adhesive coating layer provided on the cross-sectional anode is 10% or more and 20% or less of the total area of the surface of the cross-sectional anode facing the first separator.
4. In claim 1, An electrode assembly, wherein the thickness of the adhesive coating layer is 10% or more and 100% or less of the thickness of the first separator.
5. In claim 1, An electrode assembly, wherein the entire surface of the cross-sectional anode facing the first separator is provided with an adhesive coating layer in a predetermined pattern.
6. In claim 1, An electrode assembly, wherein the first polymer binder is a polyvinylidene resin.
7. In claim 1, An electrode assembly, wherein the first polymer binder is a copolymer of polyvinylidene propylene and hexafluoropropylene.
8. In claim 1, An electrode assembly, wherein the substitution rate of the hexafluoropropylene in the first polymer binder is 20% or more.
9. In claim 1, The above cross-sectional positive electrode comprises a second polymer binder, The above separator comprises a porous coating layer provided on at least one surface and including a third polymer binder and inorganic particles, An electrode assembly, wherein each of the second polymer binder and the third polymer binder included in the cross-sectional positive electrode and the porous coating layer is the same as the first polymer binder included in the adhesive coating layer.
10. A step of providing 2n second separators between the first separators at both ends; A step of preparing a laminate by providing n+1 cathodes and n anodes alternately between the first separator and the second separator, and providing a single-sided anode having an adhesive coating layer on the outer portion on the first separator at both ends; and A method for manufacturing an electrode assembly, comprising: a step of manufacturing an electrode assembly by applying heat and pressure to the laminate; 11. In claim 10, A method for manufacturing an electrode assembly, wherein the step of manufacturing the electrode assembly is performed at a temperature of less than 90°C and a pressure of less than 6.5 MPa.
12. In claim 10, A method for manufacturing an electrode assembly, wherein the step of providing the above separator is to provide one separator by folding it in a zigzag pattern.
Citation Information
Patent Citations
An electrode assembly and a method of manufacturing the same
KR1020240156121A
Electrode assembly having separator and electrode adhesive layers, and electrochemical devices comprising the same
KR1020140026009A
Electrode-separator assembly, secondary battery comprising the same, and manufacturing method thereof
KR1020160042666A
Rebound stopper of shock absorber for vehicle
KR1020210140994A
Door hinge
KR102241346B1
Cited By
Electrode assembly and manufacturing method thereof
JP2025537361A