Positive electrode sheet, secondary battery, and electric device

By adopting an alternately stacked layered oxide and phosphate material structure in the lithium-ion battery cathode sheet, and using fluorinated monomers to suppress the gelation of the slurry, the problems of insufficient peeling force and low cycle performance of the cathode sheet are solved. problem, improving the overall performance of the battery.

WO2024221229A1PCT designated stage expired Publication Date: 2024-10-31CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/090630
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode plates have insufficient peeling force during cycling, resulting in a decline in battery cell cycle performance, and the alkalinity of the layered oxide material causes the slurry to gel, affecting coating performance.

Method used

Adopting an alternately stacked first active layer and a second active layer structure, the first active layer contains a layered oxide active material and a first copolymer binder, and the second active layer contains a phosphate cathode active material and fluorine It is a monomer homopolymer binder that inhibits the cross-linking reaction by adjusting the ratio of C-F bonds and C-H bonds to prevent gelation of the slurry.

Benefits of technology

It improves the peeling force of the positive electrode film and the cycle performance of the battery core, ensures the coatability and bonding effect of the slurry, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023090630_31102024_PF_FP_ABST
    Figure CN2023090630_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a positive electrode sheet, a secondary battery, and an electric device. The positive electrode sheet comprises a positive electrode current collector and a positive electrode film layer provided on at least one side of the positive electrode current collector; the positive electrode film layer comprises one or more first active layers and one or more second active layers arranged in the thickness direction of the positive electrode current collector; the first active layers and the second active layers are alternately stacked; each first active layer comprises a layered oxide active material and a first binder; the first binder comprises a first copolymer; each second active layer comprises a phosphate-based positive electrode active material and a second binder; the second binder comprises a fluorinated monomer homopolymer and / or a second copolymer; and the monomers forming the first copolymer and the monomers forming the second copolymer each independently comprise a fluorinated monomer. The peel force of the positive electrode sheet is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode sheet, secondary battery and electrical device Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a positive electrode sheet, a secondary battery, and an electrical device. Background Art

[0002] Lithium-ion batteries have high energy density and a long lifespan, making them an ideal energy source for electric vehicles and other power tools. Currently, there are numerous methods for improving the cycling performance of lithium-ion batteries. These include modifying the positive electrode material by doping or coating it to mitigate the deterioration of its crystal structure during cycling; or combining positive electrode materials with different advantages to leverage their strengths and overcome their weaknesses to improve the battery's cycling performance and energy density. For example, lithium iron phosphate-based positive electrode materials can be combined with layered oxides, typically ternary positive electrode materials. Specifically, the two can be mixed with a binder, conductive agent, or other materials to form a slurry, which can then be applied. Alternatively, the two can be mixed with a binder and conductive agent to form separate slurries, which can then be applied in multiple layers.

[0003] Summary of the Invention

[0004] The present application provides a positive electrode sheet, a secondary battery, and an electrical device to improve the peeling force of the positive electrode sheet.

[0005] The first aspect of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode film layer arranged on at least one side of the positive electrode collector, the positive electrode film layer includes one or more first active layers and one or more second active layers arranged along the thickness direction of the positive electrode collector, the first active layers and the second active layers are alternately stacked, the first active layer includes a layered oxide active material and a first binder, the first binder includes a first copolymer; the second active layer includes a phosphate-based positive electrode active material and a second binder, the second binder includes a fluorinated monomer homopolymer and / or a second copolymer, and the monomers forming the first copolymer and the second copolymer each independently include a fluorinated monomer.

[0006] Fluorinated monomers are typically unsaturated compounds formed by replacing one or more H in an unsaturated compound with fluorine, and contain C-F bonds. Since C-F bonds are easily broken in an alkaline environment to produce free F ions, when a homopolymer contains a large number of both C-F and C-H bonds, the free F ions produced by the CF bond breakage combine with the free hydrogen formed by the C-H bond breakage to form HF and carbon-carbon double bonds, resulting in crosslinks within or between the molecular chains of the homopolymer, thereby causing the slurry to gel. The first and second copolymers of the fluorinated monomers use the fluorinated monomers to provide good adhesion, while the ratio of C-F bonds to C-H bonds is adjusted by combining the fluorinated monomers with other monomers to suppress the reaction of forming HF and carbon-carbon double bonds, thereby making it difficult for the positive electrode slurry used to coat the first active layer to gel. The suppression of positive electrode slurry gelation ensures the coatability of the positive electrode slurry while fully utilizing the adhesive effect of the binder. Therefore, the use of the first copolymer effectively improves the peeling strength of the positive electrode film layer and the cycling performance of the battery cell.

[0007] The second aspect of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode film layer arranged on at least one side of the positive electrode collector, the positive electrode film layer includes one or more first active layers and one or more second active layers arranged along the thickness direction of the positive electrode collector, the first active layers and the second active layers are alternately stacked, the first active layer includes a first positive electrode active material and a first binder, the first binder includes a first copolymer, the first positive electrode active material is mixed with water to form a mixed slurry with a mass content of 10%, and the pH value is between 11-13; the second active layer includes a second positive electrode active material and a second binder, the second binder includes a fluorinated monomer homopolymer and / or a second copolymer, the second positive electrode active material is mixed with water to form a mixed slurry with a mass content of 10%, which is alkaline and has a pH value below 10, and the monomers forming the first copolymer and the second copolymer each independently include a fluorinated monomer.

[0008] Fluorinated monomers are typically unsaturated compounds formed by replacing one or more hydrogen atoms in an unsaturated compound with fluorine, and contain C—F bonds. Because C—F bonds are more likely to break in a highly alkaline environment, producing free F ions, when a homopolymer contains a high concentration of both C—F and C—H bonds, the free F ions generated by the CF bond breakage combine with the free hydrogen formed by the C—H bond breakage to form HF and carbon-carbon double bonds, leading to crosslinking within or between the homopolymer's molecular chains, which in turn causes the slurry to gel. The first and second copolymers of the fluorinated monomers utilize the fluorinated monomers to provide good adhesion, while the ratio of C—F bonds to C—H bonds is adjusted using a combination of the fluorinated monomers and other monomers to suppress the aforementioned reactions that form HF and carbon-carbon double bonds. When this first copolymer is used in combination with a first positive electrode active material having a higher pH value, the positive electrode slurry used to coat the first active layer is less likely to gel. Suppressing the gelation of the positive electrode slurry ensures the coatability of the positive electrode slurry while fully utilizing the binding effect of the binder. Therefore, the use of this first copolymer effectively improves the peeling strength of the positive electrode film layer and the cycling performance of the battery cell.

[0009] In any embodiment of the first and second aspects, the fluorinated monomers forming the first and second copolymers each independently include any one or more selected from the group consisting of vinyl fluoride, vinylidene fluoride, trifluoroethylene, tetrafluoroethylene, hexafluoropropylene, and perfluoroalkyl vinyl ether, thereby maximizing the adhesive properties of the adhesive containing the fluorinated monomers.

[0010] In any embodiment of the first aspect and the second aspect, the first copolymer and the second copolymer each independently include one or more selected from the group consisting of vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-ethylene oxide copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer.

[0011] In any embodiment of the first and second aspects, the fluorinated monomers of the first and second copolymers contain vinylidene fluoride; the first and second copolymers each independently comprise one or more selected from the group consisting of vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-ethylene oxide copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer. The vinylidene fluoride monomer is used to improve the adhesive properties of the copolymers, and other monomers such as hexafluoropropylene in the copolymers are used to adjust the ratio of C—H bonds to C—H bonds, particularly adjusting the C—H bond content to be significantly greater than the C—H bond content, thereby improving the adhesive properties of the copolymers while better preventing the generation of HF.

[0012] The molar content of the structural units corresponding to the vinylidene fluoride monomer in the first copolymer and the second copolymer is independently 50% to 95%, thereby improving the gelation of the slurry while increasing the bonding strength as much as possible.

[0013] In any embodiment of the first and second aspects, the second binder is a fluorinated monomer homopolymer; optionally, the fluorinated monomer homopolymer is a vinylidene fluoride homopolymer. Experiments have shown that when a vinylidene fluoride copolymer is used as the second binder, the second positive electrode slurry actually undergoes slight gelation. Therefore, using a vinylidene fluoride homopolymer can avoid gelation caused by the copolymer.

[0014] In any embodiment of the first aspect and the second aspect, optionally, the weight average molecular weight of the first copolymer, the second copolymer and the fluorinated monomer homopolymer is each independently 100,000 Da to 1,000,000 Da.

[0015] In any embodiment of the first aspect and the second aspect, the positive electrode sheet satisfies any one or more of the following conditions:

[0016] The mass content of the first binder in the first active layer is 0.5% to 2.5%;

[0017] The mass content of the second binder in the second active layer is 0.5% to 2.5%;

[0018] The first active layer and the second active layer each independently include a conductive agent. The aforementioned content limits ensure sufficient bonding strength while avoiding the reduction in energy density of the resulting positive electrode film due to excessive amounts of binder. The conductive agent is used to improve the conductivity of the positive electrode film.

[0019] In any embodiment of the first aspect, the pH value of the mixed slurry formed by mixing the layered oxide active material with water to form a 10% by mass content is between 11 and 13.

[0020] In any embodiment of the second aspect, the first positive electrode active material includes a layered oxide active material.

[0021] In any embodiment of the first aspect and the second aspect, the above-mentioned layered oxide active material includes a ternary positive electrode material and / or a quaternary positive electrode material, and optionally the layered oxide active material includes one or more selected from the group consisting of a nickel cobalt manganese oxide positive electrode active material, a nickel cobalt aluminum oxide positive electrode active material, a nickel cobalt manganese aluminum oxide positive electrode active material, a doped or coated nickel cobalt manganese oxide positive electrode active material, a doped or coated nickel cobalt aluminum oxide positive electrode active material, and a doped or coated nickel cobalt manganese aluminum oxide positive electrode active material.

[0022] In any embodiment of the first and second aspects, the surface of the layered oxide active material has a first coating layer, and the first coating layer comprises one or more coating layers selected from carbon, conductive graphene, a conductive polymer material, or an oxide. This further enhances the conductivity of the layered oxide active material, increases the lithium ion migration rate, and thereby improves the rate performance of the battery.

[0023] In any embodiment of the first aspect, the pH value of the mixed slurry formed by mixing the phosphate-based positive electrode active material with water to form a 10% by mass content is between 8 and 10.

[0024] In any embodiment of the second aspect, the pH value of the mixed slurry formed by mixing the second positive electrode active material with water and forming a 10% by mass content is between 8 and 10. Optionally, the second positive electrode active material is a phosphate-based positive electrode active material.

[0025] In any embodiment of the first aspect and the second aspect, the phosphate-based positive electrode active material may include at least one of the following materials: LiMn 1-y Fe y PO4, y is any value in the range of 0.001 to 0.5; Li 1+t Mn 1- c Fe c P 1-z R z O4, t is any value in the range of -0.100 to 0.100, c is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, and R includes one or more elements selected from B, S, Si and N; Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n, wherein A comprises one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W, E comprises one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, R comprises one or more elements selected from B, S, Si, and N, D comprises one or more elements selected from S, F, Cl, and Br, w is any value in the range of -0.100 to 0.100, m is any value in the range of 0.001 to 0.1, u is any value in the range of 0.001 to 0.500, a is any value in the range of 0.001 to 0.100, n is any value in the range of 0.001 to 0.1, and Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n It is electrically neutral. Doping can improve the cycling performance or rate performance of the material.

[0026] In any embodiment of the first aspect and the second aspect, the surface of the phosphate-based positive electrode active material has a second coating layer, and the second coating layer includes a single coating layer or multiple coating layers of pyrophosphate, phosphate, and carbon.

[0027] In any embodiment of the first and second aspects, if the first active layer is one layer and the second active layer is two layers, the first active layer is located between the two second active layers; and / or if the first active layer is two layers and the second active layer is one layer, the second active layer is located between the two first active layers. The first active layer containing the layered oxide active material in each of the above-mentioned positive electrode films exhibits significantly improved film uniformity and peel strength compared to a film containing the same amount of vinylidene fluoride homopolymer.

[0028] In any embodiment of the first and second aspects, the ratio of the thickness of the first active layer to the thickness of the second active layer is 0.9:1 to 1.1:1. Optionally, the thickness of the first active layer is 60 μm to 65 μm, and the thickness of the second active layer is 60 μm to 65 μm. The thickness of the first and second active layers can be adjusted within this thickness range to adjust the ratio of the two active materials and thereby adjust the performance of the battery cell.

[0029] The third aspect of the present application provides a secondary battery comprising a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises any one of the positive electrode sheets of the first aspect, and the positive electrode sheet has good cycle performance.

[0030] A fourth aspect of the present application provides an electrical device comprising a secondary battery, wherein the secondary battery comprises any one of the above-mentioned secondary batteries. The secondary battery of the electrical device has a long service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0032] FIG1 is a schematic diagram of the cross-sectional structure of a positive electrode sheet provided in one embodiment of the present application.

[0033] FIG2 is a schematic diagram of the cross-sectional structure of a positive electrode sheet provided in one embodiment of the present application.

[0034] FIG3 is a schematic diagram of the cross-sectional structure of a positive electrode sheet provided in one embodiment of the present application.

[0035] FIG4 is a schematic diagram of the cross-sectional structure of a positive electrode sheet provided in one embodiment of the present application.

[0036] FIG5 is a schematic diagram of the cross-sectional structure of a positive electrode sheet provided in one embodiment of the present application.

[0037] FIG6 is a schematic diagram of the cross-sectional structure of a positive electrode sheet provided in one embodiment of the present application.

[0038] FIG. 7 is a schematic diagram of a secondary battery according to an embodiment of the present application.

[0039] FIG. 8 is an exploded view of the secondary battery according to the embodiment of the present application shown in FIG. 7 .

[0040] FIG9 is a schematic diagram of a battery module according to an embodiment of the present application.

[0041] FIG10 is a schematic diagram of a battery pack according to an embodiment of the present application.

[0042] FIG. 11 is an exploded view of the battery pack shown in FIG. 10 according to an embodiment of the present application.

[0043] FIG. 12 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0044] In the drawings, the drawings are not drawn to scale.

[0045] Explanation of reference numerals: positive electrode current collector 10; first active layer 21; second active layer 22; 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 housing; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION

[0046] The following detailed description of the embodiments of the present application is provided in conjunction with the accompanying drawings and examples. The following detailed description of the embodiments and the accompanying drawings are used to illustrate the principles of the present application, but are not intended to limit the scope of the present application, that is, the present application is not limited to the described embodiments.

[0047] Below, the embodiments of the positive electrode slurry composition, positive electrode sheet, secondary battery and electric device of the present application are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0048] The "ranges" disclosed herein are defined in terms of lower and upper limits, where a given range is defined by selecting a lower limit and an upper limit, and the selected lower and upper limits define the boundaries of the particular range. Ranges defined in this manner can be inclusive or exclusive of the end values ​​and can be combined arbitrarily, i.e., any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60 to 120 and 80 to 110 are listed for a particular parameter, it is understood that ranges of 60 to 110 and 80 to 120 are also contemplated. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, the following ranges are all contemplated: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5. In this application, unless otherwise indicated, the numerical range "a to b" is a shorthand representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0049] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0050] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0051] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0052] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0053] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0054] [Secondary battery]

[0055] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged to activate the active materials after discharge and continue to be used.

[0056] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and an optional separator (if it is a solid-state battery, a separator may not be provided, and if it is a liquid battery, a separator is provided). During the charge and discharge process of the battery, active ions (such as lithium ions or sodium ions) are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte is between the positive electrode sheet and the negative electrode sheet, mainly to conduct active ions.

[0057] [Positive electrode]

[0058] As described in the background art, combining lithium iron phosphate-based positive electrode materials and layered oxides is a way to improve the performance of positive electrode materials. When the two are combined, whether forming a mixed slurry or an independent slurry, the same form of binder is usually selected. During the application process, the peeling force of the positive electrode sheet is insufficient. After research, it was found that compared with the positive electrode slurry containing lithium iron phosphate-based positive electrode materials, the positive electrode slurry containing layered oxides is more likely to form chemical gel during the stirring process, resulting in a serious decrease in the filterability and adhesion of the slurry, affecting the coating performance of the slurry, reducing the processability of the positive electrode sheet, and also causing the peeling force of the positive electrode sheet to decrease, ultimately affecting the cycle performance of the battery cell. The reason may be that there is more residual alkali on the surface of the layered oxide, so its alkalinity is relatively strong, resulting in an increase in viscosity when using it as a positive electrode active material to prepare a slurry, and a gel phenomenon occurs. In severe cases, the slurry has no coating performance at all.

[0059] In order to solve this problem, the applicant has tried many ways, such as reducing the alkalinity of the layered oxide by coating, etc., but this method is technically complex. When a copolymer of vinylidene fluoride is used as a layered oxide binder, the slurry is relatively stable and not easy to gel. Therefore, the first embodiment of the present application provides a positive electrode plate, the positive electrode plate includes a positive electrode collector and a positive electrode film layer arranged on at least one side of the positive electrode collector, the positive electrode film layer includes one or more first active layers and one or more second active layers arranged along the thickness direction of the positive electrode collector, the first active layer and the second active layer are alternately stacked, the first active layer includes a layered oxide active material and a first binder, the first binder includes a first copolymer; the second active layer includes a phosphate-based positive electrode active material and a second binder, the second binder includes a fluorinated monomer homopolymer and / or a second copolymer, and the monomers forming the first copolymer and the second copolymer each independently include a fluorinated monomer.

[0060] The above-mentioned scheme of alternatingly stacking the first active layer and the second active layer includes but is not limited to any one of the following schemes:

[0061] A scheme in which a first active layer and a second active layer are stacked, a scheme in which a first active layer is arranged between two second active layers, a scheme in which a second active layer is arranged between two first active layers, and a scheme in which both the first active layer and the second active layer are multiple layers and alternately stacked.

[0062] Fluorinated monomers are typically unsaturated compounds formed by replacing one or more H in an unsaturated compound with fluorine, and contain C-F bonds. Since C-F bonds are more likely to break in an alkaline environment to produce free F ions, when a homopolymer contains a large number of both C-F and C-H bonds, the free F ions produced by the CF bond breakage combine with the free hydrogen formed by the C-H bond breakage to form HF and carbon-carbon double bonds, resulting in crosslinks within or between the molecular chains of the homopolymer, which in turn causes the slurry to gel. When the first and second copolymers of the fluorinated monomers are used as binders, the fluorinated monomers are used to provide good adhesion, and the ratio of C-F bonds to C-H bonds is adjusted by combining the fluorinated monomers with other monomers to suppress the reaction of forming HF and carbon-carbon double bonds, thereby making it difficult for the positive electrode slurry used to form the first active layer to gel. The suppression of positive electrode slurry gelation ensures the coatability of the positive electrode slurry while fully utilizing the binding effect of the binder. Therefore, the use of the first copolymer effectively improves the peeling strength of the positive electrode film layer and the cycling performance of the battery cell.

[0063] Even in the preparation of other positive electrode sheets containing multiple positive electrode active materials, when the pH value of the positive electrode active material is higher, the gelation problem is more serious, the coating is more difficult, and the peeling force of the positive electrode sheet after application is more seriously affected. In order to solve this problem, the second embodiment of the present application provides a positive electrode sheet, which includes a positive electrode collector and a positive electrode film layer arranged on at least one side of the positive electrode collector, the positive electrode film layer includes one or more first active layers and one or more second active layers arranged along the thickness direction of the positive electrode collector, the first active layer and the second active layer are interlaced. The first active layer includes a first positive electrode active material and a first binder, the first binder includes a first copolymer, and the first positive electrode active material is mixed with water to form a mixed slurry with a mass content of 10%, and the pH value is between 11 and 13; the second active layer includes a second positive electrode active material and a second binder, the second binder includes a fluorinated monomer homopolymer and / or a second copolymer, the second positive electrode active material is mixed with water to form a mixed slurry with a mass content of 10%, which is alkaline and has a pH value below 10, and the monomers forming the first copolymer and the second copolymer each independently include a fluorinated monomer.

[0064] Fluorinated monomers are typically unsaturated compounds formed by replacing one or more H in an unsaturated compound with fluorine, and contain C-F bonds. Since C-F bonds are more likely to break in a highly alkaline environment to produce free F ions, when a homopolymer contains a large number of both C-F and C-H bonds, the free F ions produced by the CF bond breakage combine with the free hydrogen formed by the C-H bond breakage to form HF and carbon-carbon double bonds, resulting in crosslinks within or between the molecular chains of the homopolymer, which in turn leads to gelation of the slurry. The first and second copolymers of the fluorinated monomers use the fluorinated monomers to provide good adhesion, while the ratio of C-F bonds to C-H bonds is adjusted by combining the fluorinated monomers with other monomers to suppress the reaction of forming HF and carbon-carbon double bonds. When this first copolymer is used in combination with a first positive electrode active material with a higher pH value, the positive electrode slurry used to coat the first active layer is less likely to gel. The suppression of positive electrode slurry gelation ensures the coatability of the positive electrode slurry while fully utilizing the binding effect of the binder. Therefore, the use of the first copolymer effectively improves the peeling strength of the positive electrode film layer and the cycling performance of the battery cell.

[0065] The pH value can be measured as follows: Weigh 5g of sample powder into an Erlenmeyer flask. Add 45g of deionized water to the flask at a ratio of 1:9 powder to solvent. Place the flask in a magnetic rotor and seal with parafilm. Place the prepared solution on the center of the magnetic stirrer platform and stir for 30 minutes. After stirring, let it stand for 1.5 hours. Immerse the pH electrode glass bulb completely in the solution and wait for at least 1 minute for the pH reading to stabilize.

[0066] The first copolymer and the second copolymer used in the present application can both be formed by conventional copolymers with fluorinated monomers or conventional copolymerization methods. In some embodiments, the fluorinated monomers forming the first copolymer and the second copolymer each independently include any one or more of the group consisting of vinyl fluoride, vinylidene fluoride, trifluoroethylene, tetrafluoroethylene, hexafluoropropylene and perfluoroalkyl vinyl ether. Thereby improving the bonding performance of the adhesive containing it as much as possible. The above-mentioned "the fluorinated monomers forming the first copolymer and the second copolymer each independently include any one or more of the group consisting of vinyl fluoride, vinylidene fluoride, trifluoroethylene, tetrafluoroethylene, hexafluoropropylene and perfluoroalkyl vinyl ether" means that the fluorinated monomers forming the first copolymer and the second copolymer can not only be selected from the group consisting of vinyl fluoride, vinylidene fluoride, trifluoroethylene, tetrafluoroethylene, hexafluoropropylene and perfluoroalkyl vinyl ether, but can also include other types of fluorinated monomers.

[0067] In some embodiments, the first copolymer and the second copolymer each independently include one or more selected from the group consisting of vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-ethylene oxide copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer.

[0068] In some embodiments, the fluorinated monomers of the first and second copolymers must contain vinylidene fluoride; the first and second copolymers each independently comprise one or more selected from the group consisting of vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-ethylene oxide copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer. The vinylidene fluoride monomer is used to improve the adhesive properties of the copolymers, and other monomers such as hexafluoropropylene in the above copolymers are used to adjust the ratio of C—H bonds to C—H bonds, particularly adjusting the C—H bond content to be much greater than the C—H bond content, thereby improving the adhesive properties of the copolymers while better preventing the occurrence of HF generation reactions.

[0069] The higher the content of vinylidene fluoride structural units in the copolymer, the better the adhesion. In order to improve the gelation of the slurry while increasing the adhesion as much as possible, in some embodiments, the molar content of the structural units corresponding to the vinylidene fluoride monomer in the first copolymer and the second copolymer is independently 50% to 95%.

[0070] The second binder can be a vinylidene fluoride homopolymer and / or a vinylidene fluoride copolymer. Due to the high cost of vinylidene fluoride copolymer, in some embodiments, the second binder may include a vinylidene fluoride homopolymer. Experiments have found that when a vinylidene fluoride copolymer is used as the second binder, due to the generally small particle size of the lithium iron manganese phosphate material, small particles in the vinylidene fluoride copolymer system entangle and agglomerate with the vinylidene fluoride copolymer, resulting in gelation. Therefore, using a vinylidene fluoride homopolymer can avoid gelation caused by the copolymer.

[0071] As a general rule, whether it is a homopolymer or a copolymer, the larger the molecular weight, the greater the viscosity, but polymers within the molecular weight range used as binders can be used in this application. In some embodiments, the weight average molecular weight of the first copolymer, the second copolymer and the fluorinated monomer homopolymer are optionally each independently 100,000 Da to 1,000,000 Da.

[0072] The amounts of the first and second binders used in this application can refer to the amounts of binders used in conventional positive electrode films. In some embodiments, the mass content of the first binder in the first active layer is 0.5% to 2.5%, and / or the mass content of the second binder in the second active layer is 0.5% to 2.5%. This ensures sufficient bonding strength while avoiding the reduction in energy density of the resulting positive electrode film due to excessive binder usage.

[0073] To improve the conductivity of the formed positive electrode film, in some embodiments, the first active layer and the second active layer each independently include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0074] In some embodiments, the first positive electrode active material includes a layered oxide active material. The amount of the layered oxide active material in the first positive electrode slurry can also refer to the prior art. For example, in some embodiments, the mass content of the layered oxide active material in the first active layer is 95% to 98.8%.

[0075] The layered oxide active material used in the present application can be a conventional layered oxide used for positive electrode materials in the art. In order to avoid the alkalinity of the layered oxide active material being too high, in some embodiments, the pH value of the mixed slurry formed by mixing the above-mentioned layered oxide active material with water to form a mass content of 10% is controlled to be between 11 and 13. For example, conventional binary layered oxides such as lithium cobaltate, lithium manganate, and lithium nickelate, conventional ternary positive electrode materials, and conventional quaternary positive electrode materials. In some embodiments, the above-mentioned layered oxide active material includes a ternary positive electrode material and / or a quaternary positive electrode material, and the layered oxide active material optionally includes one or more selected from the group consisting of a lithium nickel cobalt manganate positive electrode active material, a lithium nickel cobalt aluminum oxide positive electrode active material, a lithium nickel cobalt manganate aluminum oxide positive electrode active material, a doped or coated lithium nickel cobalt manganate positive electrode active material, and a doped or coated lithium nickel cobalt manganese aluminum oxide positive electrode active material.

[0076] In some embodiments, the layered oxide active material includes Li element, transition metal element, and optionally Al element, wherein the transition metal element includes any one or more selected from the group consisting of Ni, Co, Mn, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb.

[0077] In some embodiments, the surface of the layered oxide active material has a first coating layer, and the first coating layer includes a coating layer or multiple coating layers of carbon, conductive graphene, conductive polymer material, or oxide. To further improve the conductivity of the layered oxide active material, increase the lithium ion migration rate, and thus improve the rate performance of the battery. The conductive polymer material includes but is not limited to any one or more of modified or unmodified polypyrrole (PPy), modified or unmodified poly 3,4-ethylenedioxythiophene (PEDOT), and modified or unmodified polyamide (PI). The oxides include but are not limited to Li2ZrO3, LiNbO3, Li4Ti5O 12 , Li2TiO3, Li3VO4, LiSnO3, Li2SiO3 and LiAlO2. The above layered oxides are all derived from layered oxides known in the prior art or are prepared using a preparation method known in the prior art, which will not be described in detail in this application.

[0078] In some embodiments, the pH of a 10% by weight slurry formed by mixing the second positive electrode active material with water is between 8 and 10. Optionally, the second positive electrode active material is a phosphate-based positive electrode active material. The amount of the phosphate-based positive electrode active material in the second active layer can also refer to the prior art. For example, in some embodiments, the phosphate-based positive electrode active material in the second active layer has a weight content of 95% to 98.8%.

[0079] In some embodiments, the pH of a 10% by weight slurry of a phosphate-based positive electrode active material mixed with water is between 8 and 10, effectively alleviating the problem of slurry gelation caused by excessive alkalinity of the phosphate-based positive electrode active material. The pH test method is consistent with the test method for the layered oxide active material described above.

[0080] Optionally, the phosphate-based positive electrode active material includes at least one of the following materials: LiMn 1-y Fe y PO4, y is any value in the range of 0.001 to 0.5; Li 1+t Mn 1-c Fe c P 1-z R z O4, t is any value in the range of -0.100 to 0.100, c is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, and R includes one or more elements selected from B, S, Si and N; Li 1+w A m Mn 1-u E u P 1-a Ra O 4- n D n , wherein A comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W, E comprises one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, R comprises one or more elements selected from the group consisting of B, S, Si, and N, D comprises one or more elements selected from the group consisting of S, F, Cl, and Br, w is any value within the range of -0.100 to 0.100, m is any value within the range of 0.001 to 0.1, u is any value within the range of 0.001 to 0.500, a is any value within the range of 0.001 to 0.100, n is any value within the range of 0.001 to 0.1, and Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n It is electrically neutral. Doping can improve the cycling performance or rate performance of the material.

[0081] Doping element A at the manganese position of lithium manganese phosphate helps reduce the lattice change rate of lithium manganese phosphate during lithium insertion and extraction, improving the structural stability of the lithium manganese phosphate cathode material, significantly reducing manganese dissolution and reducing oxygen activity on the particle surface. Doping element R at the phosphorus position helps change the difficulty of the Mn-O bond length change, thereby reducing the lithium ion migration barrier, promoting lithium ion migration, and improving the rate performance of the secondary battery.

[0082] Doping at the P and O sites also affects the Mn dissolution and kinetic properties of antisite defects. Therefore, doping reduces the concentration of antisite defects in the material, improves the kinetic properties and gram capacity of the material, and can also change the morphology of the particles, thereby increasing the compaction density. In summary, by doping specific elements at the Li, Mn, P and O sites of the compound LiMnPO4 at specific amounts at the same time, significantly improved rate performance can be obtained, while significantly reducing the dissolution of Mn and Mn-site doping elements, obtaining significantly improved cycle performance and / or high temperature stability, and the gram capacity and compaction density of the material can also be improved.

[0083] The M in the cathode material LiMPO4 designed in this scheme may include Mn and Fe elements. As a possible implementation method, LiMPO4 may be a compound LiMn 1-y Fe y PO4.

[0084] For example, the compound LiMn0.50 Fe 0.50 The preparation method of PO4 includes:

[0085] Step S1: preparing Fe-doped manganese oxalate.

[0086] 574.7g of manganese carbonate and 579.3g of ferrous carbonate were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours until the reaction terminated and no bubbles were generated, resulting in an Fe-doped manganese oxalate suspension. The suspension was then filtered, dried at 120°C, and sand-milled to obtain ferromanganese oxalate particles with a particle size of 100nm.

[0087] Step S2: Preparation of LiMn 0.50 Fe 0.50 PO4.

[0088] Take the manganese oxalate iron (C2O4Mn 0.50 Fe 0.50 1791.4 g of 1,000 g of 1,000 g of 1,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 4,000 g of 1,000 g of 2,000 g of 1 ...1,000 g of 2,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 1,000 g of 2,000 g of 1,000 g of 1,000 g of 1,000 g of 1,000

[0089] The positive electrode active material may be a material having the chemical formula Li 1+t Mn 1-c Fe c P 1-z R z O4 compound, wherein t is any value in the range of -0.100 to 0.100, c is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, and R includes one or more elements selected from B (boron), S, Si and N. Wherein, the values ​​of t, c and z satisfy the following conditions: the entire compound remains electrically neutral. The ratio of c to 1-c is 1:10 to 1:1, and can be optionally 1:4 to 1:1. Here c represents the sum of the stoichiometric numbers of the Mn-site doping element Fe. In some embodiments, the ratio of z to 1-z is 1:9 to 1:999, and can be optionally 1:499 to 1:249. Here z represents the sum of the stoichiometric numbers of the P-site doping element R.

[0090] Compound Li 1+t Mn1-c Fe c P 1-z R z The preparation method of O4 may include the following steps:

[0091] (1) dissolving a manganese source, an iron source, and an acid in a solvent and stirring to generate a suspension of a manganese salt doped with elemental Fe, filtering the suspension and drying the filter cake to obtain a manganese salt doped with elemental Fe; (2) adding a lithium source, a phosphorus source, a source of elemental R, a solvent, and the manganese salt doped with elemental Fe obtained in step (1) into a reaction vessel, grinding and mixing to obtain a slurry; (3) transferring the slurry obtained in step (2) to a spray drying device for spray drying and granulation to obtain particles; (4) sintering the particles obtained in step (3) to obtain a positive electrode active material.

[0092] In any embodiment, the manganese source can be a manganese-containing substance known in the art that can be used to prepare lithium manganese phosphate, such as a manganese source selected from one or a combination of elemental manganese, manganese dioxide, manganese phosphate, manganese oxalate, and manganese carbonate. The iron source is selected from at least one of elemental iron, oxides, phosphates, oxalates, carbonates, and sulfates. The acid is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and organic acids such as oxalic acid, and can be, for example, oxalic acid. The source of element R is selected from at least one of sulfates, borates, nitrates, and silicates of element R.

[0093] For example, the compound Li 1.001 Mn 0.999 Fe 0.001 P 0.999 Si 0.001 The preparation method of O4 includes:

[0094] Step S1: preparing Fe-doped manganese oxalate.

[0095] 1148.2g of manganese carbonate and 1.2g of ferrous carbonate were added to a mixer and thoroughly mixed for 6 hours. The resulting mixture was then transferred to a reactor, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added. The mixture was heated to 80°C and stirred at 500 rpm for 6 hours, mixing until the reaction terminated and no bubbles were generated, resulting in an Fe-doped manganese oxalate suspension. The suspension was then filtered, dried at 120°C, and sand-milled to obtain ferromanganese oxalate particles with a particle size of 100nm.

[0096] Step S2: Preparation of Li 1.001 Mn 0.999 Fe 0.001 P 0.999 Si 0.001 O4.

[0097] Take the manganese oxalate iron (C2O4Mn0.999 Fe 0.001 1789.6 g of 2H2O (calculated as 2H2O), 369.8 g of lithium carbonate, 1148.9 g of ammonium dihydrogen phosphate, and 0.8 g of silicic acid were added to 20 L of deionized water, stirred thoroughly, and uniformly mixed at 80°C for 10 hours to obtain a slurry. The slurry was transferred to a spray dryer for spray drying and granulation, and then dried at 250°C to obtain a powder. The powder was sintered in a roller kiln at 700°C for 4 hours in a protective atmosphere (90% nitrogen and 10% hydrogen).

[0098] In other embodiments, the positive electrode active material may be a material having the chemical formula Li 1+w C m Mn 1-u Fe u P 1- a R a O 4-n D n A compound wherein C comprises one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W, R comprises one or more elements selected from B (boron), S, Si, and N, D comprises one or more elements selected from S, F, Cl, and Br, w is any value in the range of -0.100 to 0.100, u is any value in the range of 0.001 to 0.500, a is any value in the range of 0.001 to 0.100, n is any value in the range of 0.001 to 0.1, and m is any value in the range of 0.9 to 1.1. Similarly, the values ​​of w, u, a, and m satisfy the following condition: the entire compound remains electrically neutral.

[0099] Compound Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n The preparation method may include the following steps:

[0100] (1) dissolving a manganese source, an iron source, and an acid in a solvent and stirring to generate a suspension of a manganese salt doped with element E, filtering the suspension and drying the filter cake to obtain a manganese salt doped with element E; (2) adding a lithium source, a phosphorus source, a source of element A, a source of element R, a source of element D, a solvent, and the manganese salt doped with element E obtained in step (1) into a reaction vessel, grinding and mixing to obtain a slurry; (3) transferring the slurry obtained in step (2) to a spray drying device for spray drying and granulation to obtain particles; (4) sintering the particles obtained in step (3) to obtain a positive electrode active material.

[0101] In any embodiment, the source of element A is selected from at least one of a simple substance, oxide, phosphate, oxalate, carbonate and sulfate of element A. The manganese source can be a manganese-containing substance known in the art that can be used to prepare lithium manganese phosphate, for example, the manganese source can be selected from one or a combination of simple manganese, manganese dioxide, manganese phosphate, manganese oxalate and manganese carbonate. The iron source is selected from at least one of a simple substance, oxide, phosphate, oxalate, carbonate and sulfate of iron. The acid is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, an organic acid such as oxalic acid, etc., for example, oxalic acid. The source of element R is selected from at least one of sulfate, borate, nitrate and silicate of element R, and the source of element D is selected from at least one of a simple substance and an ammonium salt of element D.

[0102] The positive electrode active material may contain Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D nAn embodiment of the present invention, wherein the size of w is affected by the valence of E and R and the size of y and z to ensure that the entire system is electrically neutral. If the value of w is too small, the lithium content of the entire system will be reduced, affecting the gram capacity of the material. The u value will limit the total amount of all doping elements. If u is too small, that is, the doping amount is too little, the doping element will not work. If u exceeds 0.5, the Mn content in the system will be low, affecting the voltage platform of the material. The R element is doped in the position of P. Since the PO tetrahedron is relatively stable, and a value that is too large will affect the stability of the material, the a value is limited to 0.001 to 0.100. More specifically, w is any value in the range of -0.100 to 0.100, m is any value in the range of 0.001 to 0.1, u is any value in the range of 0.001 to 0.500, a is any value in the range of 0.001 to 0.100, and n is any value in the range of 0.001 to 0.1. For example, the 1+w is selected from the range of 0.9 to 1.1, for example, 0.97, 0.977, 0.984, 0.988, 0.99, 0.991, 0.992, 0.993, 0.994, 0.995, 0.996, 0.997, 0.998, 1.01, the m is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, the u is selected from the range of 0.001 to 0.5, for example, 0.001, 0.005, 0.02, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.34, 0.345, 0.349, 0.35, 0.4, wherein a is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, 0.08, 0.1, and n is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, 0.08, 0.1, and the positive electrode active material is electrically neutral.

[0103] Unless otherwise specified, in the above chemical formulas, when a doping site has two or more elements, the above limits on the numerical ranges of w, u, a, m, or n are not only limits on the stoichiometric number of each element as the site, but also limits on the sum of the stoichiometric numbers of the elements as the site. For example, when the chemical formula is Li 1+t Mn 1-c Fe c P 1-z R zFor compounds containing O4, when R is two or more elements R1, R2, ..., Rn, the stoichiometric numbers z1, z2, ..., zn of R1, R2, ..., Rn must each fall within the numerical range specified for z in this application, and the sum of z1, z2, ..., zn must also fall within this numerical range. Similarly, for the case where A is two or more elements, the numerical range of the stoichiometric number of A specified in this application also has the above meaning.

[0104] In some embodiments, the phosphate-based positive electrode active material optionally further includes a coating layer, which is optionally one or more layers of pyrophosphate, phosphate, and carbon. Since the migration barrier of transition metals in pyrophosphate is relatively high (>1eV), the dissolution of transition metals can be effectively suppressed. Phosphate has excellent lithium ion conductivity and can reduce the surface impurity lithium content. The carbon layer can effectively improve the electrical conductivity and desolvation ability of LiMnPO4, and can also act as a "barrier" to further hinder the migration of manganese ions into the electrolyte and reduce the corrosion of the electrolyte on the active material; at the same time, the above-mentioned carbon layer can also optimize the conductive network around the ternary positive electrode material in the mixture, thereby improving the mixing uniformity of the phosphate-based positive electrode material and the ternary positive electrode material.

[0105] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0106] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0107] The following description of the positive electrode film layer is a description of the positive electrode film layer on either side of the current collector. If there are positive electrode film layers on both sides of the current collector, the two positive electrode film layers are designed relatively independently.

[0108] In some embodiments, as shown in Figures 1 to 6, the positive electrode film includes one or more first active layers 21 and one or more second active layers 22 arranged along the thickness direction of the positive electrode current collector 10. The first active layers 21 and the second active layers 22 are alternately stacked. Each first active layer 21 is independently formed by applying a first positive electrode slurry and then drying it, and each second active layer 22 is independently formed by applying a second positive electrode slurry and then drying it. The first active layer 21 in the above-mentioned positive electrode film can serve as the active layer closest to the positive electrode current collector 10, or the second active layer 22 can serve as the active layer closest to the positive electrode current collector 10.

[0109] In some embodiments, the first active layer 21 and the second active layer 22 in the positive electrode film layer are both one layer. Referring to Figures 1 to 3, in Figure 1, the first active layer 21 and the second active layer 22 in the positive electrode film layer on both sides of the positive electrode current collector 10 are arranged away from the positive electrode current collector 10 in sequence; in Figure 2, in the positive electrode film layer on both sides of the positive electrode current collector 10, the second active layer 22 and the first active layer 21 are arranged away from the positive electrode current collector 10 in sequence; in Figure 3, the first active layer 21 and the second active layer 22 in the positive electrode film layer on one side of the positive electrode current collector 10 are arranged away from the positive electrode current collector 10 in sequence, and the second active layer 22 and the first active layer 21 in the positive electrode film layer on the other side are arranged away from the positive electrode current collector 10 in sequence.

[0110] In some embodiments, the first active layer 21 is one layer and the second active layer 22 is two layers, then the first active layer 21 is between the two layers of the second active layer 22; and / or the first active layer 21 is two layers and the second active layer 22 is one layer, then the second active layer 22 is between the two layers of the first active layer 21. Referring to Figures 4 to 6, in Figure 4, the second active layer 22, the first active layer 21, and the second active layer 22 in the positive electrode film layers on both sides of the positive electrode current collector 10 are sequentially away from the positive electrode current collector 1 0 setting; in Figure 5, the first active layer 21, the second active layer 22, and the first active layer 21 in the positive electrode film layer on both sides of the positive electrode current collector 10 are arranged away from the positive electrode current collector 10 in sequence; in Figure 6, the second active layer 22, the first active layer 21, and the second active layer 22 in the positive electrode film layer on one side of the positive electrode current collector 10 are arranged away from the positive electrode current collector 10 in sequence; the first active layer 21, the second active layer 22, and the first active layer 21 in the positive electrode film layer on the other side are arranged away from the positive electrode current collector 10 in sequence.

[0111] In addition, the positive electrode film layer on either side of FIG. 1 to FIG. 3 and the positive electrode film layer on the opposite side in FIG. 4 to FIG. 6 may also be combined to form the positive electrode film layers on both sides of the positive electrode current collector 10 .

[0112] The above-mentioned positive electrode films with different structures can be prepared by adjusting the coating order of the first positive electrode slurry and the second positive electrode slurry. After coating, the positive electrode sheet can be obtained through drying, cold pressing and other processes. As an example, the organic solvent used to form the first positive electrode slurry and the second positive electrode slurry can include one or more of N-methylpyrrolidone, N-dimethylformamide, and dimethyl sulfoxide.

[0113] The film uniformity and peeling strength of the active layer containing the layered oxide active material in each of the above-mentioned positive electrode film layers are significantly improved compared with when the PVDF homopolymer with the same content is used.

[0114] The thickness of the positive electrode film layer in the positive electrode sheet of this application can refer to the existing technology. In some embodiments, the ratio of the thickness of the first active layer to the thickness of the second active layer is 0.9:1 to 1.1:1. Optionally, the thickness of the first active layer is 60μm to 65μm, and the thickness of the second active layer is 60μm to 65μm. The thickness of the first and second active layers can be adjusted within this thickness range to adjust the ratio of the two active materials and thus adjust the performance of the battery cell.

[0115] [Negative electrode]

[0116] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0117] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0118] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0119] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0120] In some embodiments, the negative electrode film layer may further include a binder. For example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0121] In some embodiments, the negative electrode film layer may further include a conductive agent. For example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0122] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0123] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0124] [Electrolytes]

[0125] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0126] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.

[0127] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0128] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0129] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0130] [Isolation film]

[0131] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0132] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0133] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0134] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0135] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0136] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG7 shows a secondary battery 5 having a square structure as an example.

[0137] In some embodiments, referring to Figure 8, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0138] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0139] Figure 9 shows an example battery module 4. Referring to Figure 9 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0140] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0141] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0142] Figures 10 and 11 illustrate an exemplary battery pack 1. Referring to Figures 10 and 11 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0143] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0144] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0145] Figure 12 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0146] [Example]

[0147] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0148] The sources and compositions of the PVDF copolymers or PVDF homopolymers used in the following examples are shown in Table 1.

[0149] Table 1

[0150] Cathode slurry composition:

[0151] First positive electrode slurry A: LiNi 0.8 Co 0.1 Mn 0.1 O2(LiNi 0.8 Co 0.1 Mn 0.1O2 is mixed with water to form a mixed slurry with a mass content of 10% (the pH value is about 12.4), the binder PVDF-1 and the conductive agent Super P conductive carbon black are mixed in a mass ratio of 97.0wt%:1.5wt%:1.5wt% to form a first mixed material, and the first mixed material is dispersed in N-methylpyrrolidone to prepare a first positive electrode slurry A, wherein the mass volume ratio of the first mixed material to N-methylpyrrolidone is 3:1.

[0152] First positive electrode slurry B: PVDF-2 is used to replace the PVDF-1 in the first positive electrode slurry A as a binder, and the rest is the same as the first positive electrode slurry A to prepare the first positive electrode slurry B.

[0153] First positive electrode slurry C: PVDF-3 is used to replace the PVDF-1 in the first positive electrode slurry A as a binder, and the rest is the same as the first positive electrode slurry A to prepare the first positive electrode slurry C.

[0154] First positive electrode slurry D: PVDF-4 is used to replace the PVDF-1 in the first positive electrode slurry A as a binder, and the rest is the same as the first positive electrode slurry A to prepare the first positive electrode slurry D.

[0155] First positive electrode slurry E: PVDF-5 is used to replace the PVDF-1 in the first positive electrode slurry A as a binder, and the rest is the same as the first positive electrode slurry A to prepare the first positive electrode slurry E.

[0156] First positive electrode slurry F: PVDF-6 is used to replace the PVDF copolymer in the first positive electrode slurry A as a binder, and the rest is the same as the first positive electrode slurry A to prepare the first positive electrode slurry F.

[0157] First positive electrode slurry G: adjust LiNi 0.8 Co 0.1 Mn 0.1 O2, binder PVDF-1, and conductive agent Super P conductive carbon black are mixed in a mass ratio of 98.0wt%:0.5wt%:1.5wt% to form a first mixed material, and the first mixed material is dispersed in N-methylpyrrolidone to prepare a first positive electrode slurry G.

[0158] First positive electrode slurry H: adjust LiNi 0.8 Co 0.1 Mn 0.1 O2, binder PVDF-1, and conductive agent Super P conductive carbon black are mixed in a mass ratio of 96.0wt%:2.5wt%:1.5wt% to form a first mixed material, and the first mixed material is dispersed in N-methylpyrrolidone to prepare a first positive electrode slurry H.

[0159] First positive electrode slurry I: PVDF-7 in Table 1 was used to replace PVDF-1 in the first positive electrode slurry A as a binder, and the rest was the same as the first positive electrode slurry A to prepare the first positive electrode slurry I.

[0160] The first positive electrode slurry J: using LiNi 0.65 Co 0.07 Mn 0.28 O2(LiNi 0.65 Co 0.07 Mn 0.28 O2 is mixed with water to form a mixed slurry with a mass content of 10% and a pH value of about 11.2) to replace the LiNi in the first positive electrode slurry A 0.8 Co 0.1 Mn 0.1 O2 is used as the active material, and the rest is the same as the first positive electrode slurry A to prepare the first positive electrode slurry J.

[0161] The first positive electrode slurry K: using LiAl 0.05 Ni 0.75 Co 0.1 Mn 0.1 O2(LiAl 0.05 Ni 0.75 Co 0.1 Mn 0.1 O2 is mixed with water to form a mixed slurry with a mass content of 10% and a pH value of about 12.8) to replace the LiNi in the first positive electrode slurry A 0.8 Co 0.1 Mn 0.1 O2 is used as the active material, and the rest is the same as the first positive electrode slurry A to prepare the first positive electrode slurry K.

[0162] First positive electrode slurry L: PVDF-8 is used to replace the PVDF copolymer in the first positive electrode slurry A as a binder, and the rest is the same as the first positive electrode slurry to prepare the first positive electrode slurry L.

[0163] Second positive electrode slurry A: LiMn 0.5 Fe 0.5 PO4 (the pH value of a mixed slurry with a mass content of 10% formed by mixing with water is about 9.6), a binder homopolymer PVDF-8, and a conductive agent Super P conductive carbon black are mixed in a mass ratio of 97.0wt%:1.5wt%:1.5wt% to form a second mixed material, and the second mixed material is dispersed in N-methylpyrrolidone to prepare a second positive electrode slurry A, wherein the mass volume ratio of the second mixed material to N-methylpyrrolidone is 3:1.

[0164] Second positive electrode slurry B: LiMn 0.5 Fe 0.5PO4, binder PVDF-1, and conductive agent Super P conductive carbon black are mixed in a mass ratio of 97.0wt%:1.5wt%:1.5wt% to form a second mixed material, and the second mixed material is dispersed in N-methylpyrrolidone to prepare a second positive electrode slurry B.

[0165] The testing method for the cathode material used is as follows: Weigh 5g of sample powder into an Erlenmeyer flask. Add 45g of deionized water to the flask at a ratio of 1:9 powder to solvent. Place a magnetic rotor in the flask and seal with parafilm. Place the prepared solution on the center of the magnetic stirrer platform and stir for 30 minutes. After stirring, let it stand for 1.5 hours. Immerse the pH electrode glass bulb completely in the solution and wait for at least 1 minute for the pH reading to stabilize.

[0166] The filtration performance and viscosity tests of the above slurries were performed as follows: Filtration performance test: 300 mL of slurry was poured into a beaker with a 100-mesh filter, and the time it took for the slurry to completely pass through the filter was recorded.

[0167] Viscosity test method: Place the slurry in a beaker after 48 hours and measure it using a NDJ-79 rotary viscometer.

[0168] The test results are recorded in Table 2.

[0169] Table 2

[0170] As can be seen from the table above, after different types of positive electrode materials are made into slurries using different types of PVDF, there are significant differences in their slurry filtration performance and the state after standing for 48 hours. The NCM material with PVDF copolymer has the best slurry filtration performance. For example, the filtration of 300mL of the first positive electrode slurry A can be completed in just 15s, and the viscosity of the slurry is also low after standing for 48 hours, without any gel phenomenon. However, the slurry filtration performance of the NCM material with PVDF homopolymer is poor. The same 300mL of the first positive electrode slurry K takes 160s to filter, which is 10 times the time required for the slurry made by stirring the PVDF copolymer. In addition, the viscosity of the slurry is significantly higher after standing for 48 hours, and the verified serious gel phenomenon occurs, making it more difficult to filter and the fluidity deteriorates seriously. The slurry filtration performance and viscosity after standing for 48 hours of LFMP material with PVDF homopolymer are similar to those of NCM with PVDF copolymer, which also shows that the PVDF type that LFMP material is more suitable for is PVDF homopolymer. If LFMP material is paired with PVDF copolymer, its slurry filtration performance and viscosity after standing for 48 hours will also increase compared to when it is paired with PVDF homopolymer. The slurry state will slightly deteriorate and slight gel will appear.

[0171] Example 1

[0172] Positive electrode:

[0173] The first positive electrode slurry A was applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A was applied to the first coating layer to form a second coating layer. After drying, the positive electrode sheet Q1 was obtained. The active material layer of the positive electrode sheet Q1 consisted of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight. The average thickness of the first coating layer was 60 μm, and the average thickness of the second coating layer was 60 μm.

[0174] Negative electrode sheet: The negative electrode active material graphite, the conductive agent Super P conductive carbon black, and the binder styrene-butadiene rubber (SBR) are dissolved in the solvent deionized water in a weight ratio of 92:4:4, and mixed evenly to prepare the negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting.

[0175] Separator film: PE film with ceramic coating.

[0176] Electrolyte: lithium hexafluorophosphate LiPF6 is used as the electrolyte, and its content in the electrolyte is 10%. A mixture of EC+PC (ethylene carbonate+propylene carbonate) with a volume ratio of 3:7 is used as the solvent.

[0177] The positive electrode Q1, negative electrode, and separator are combined to form a bare cell. The bare cell is then insulated and encased in an aluminum shell. The top cover is then welded to form a dry cell. The dry cell is then baked, injected with electrolyte, and subjected to formation and aging to produce the hard-shell battery X1.

[0178] Example 2

[0179] Positive electrode sheet: The first positive electrode slurry B is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A is applied to the surface of the first coating layer to obtain positive electrode sheet Q2. The active material layer of positive electrode sheet Q2 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0180] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X2.

[0181] Example 3

[0182] Positive electrode sheet: The first positive electrode slurry C is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A is applied to the surface of the first coating layer to obtain positive electrode sheet Q3. The active material layer of positive electrode sheet Q3 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0183] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, and a hard shell battery X3 is obtained.

[0184] Example 4

[0185] Positive electrode sheet: The first positive electrode slurry D is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A is then applied to the surface of the first coating layer to obtain positive electrode sheet Q4. The active material layer of positive electrode sheet Q4 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0186] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X4.

[0187] Example 5

[0188] Positive electrode sheet: The first positive electrode slurry E was applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A was then applied to the surface of the first coating layer to produce positive electrode sheet Q5. The active material layer of positive electrode sheet Q5 consisted of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0189] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X5.

[0190] Example 6

[0191] Positive electrode sheet: The first positive electrode slurry F is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A is then applied to the surface of the first coating layer to produce positive electrode sheet Q6. The active material layer of positive electrode sheet Q6 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0192] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard shell battery X6.

[0193] Example 7

[0194] Positive electrode sheet: The first positive electrode slurry G is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A is applied to the surface of the first coating layer to obtain positive electrode sheet Q7. The active material layer of positive electrode sheet Q7 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0195] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard shell battery X7.

[0196] Example 8

[0197] Positive electrode sheet: The first positive electrode slurry H is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A is then applied to the surface of the first coating layer to produce a positive electrode sheet Q8. The active material layer of the positive electrode sheet Q8 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0198] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X8.

[0199] Example 9

[0200] Positive electrode sheet: The first positive electrode slurry I was applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A was then applied to the surface of the first coating layer to obtain positive electrode sheet Q9. The active material layer of positive electrode sheet Q9 consisted of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0201] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard shell battery X9.

[0202] Example 10

[0203] Positive electrode sheet: The first positive electrode slurry J was applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A was then applied to the surface of the first coating layer to produce positive electrode sheet Q10. The active material layer of positive electrode sheet Q10 consisted of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0204] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X10.

[0205] Example 11

[0206] Positive electrode sheet: The first positive electrode slurry K is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A is then applied to the surface of the first coating layer to produce a positive electrode sheet Q11. The active material layer of the positive electrode sheet Q11 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each comprising 50% by weight.

[0207] The negative electrode sheet, separator, and electrolyte composition were the same as those in Example 1, to obtain a hard-shell battery X11.

[0208] Example 12

[0209] Positive electrode sheet: The first positive electrode slurry A is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry B is applied to the surface of the first coating layer to obtain positive electrode sheet Q12. The active material layer of positive electrode sheet Q12 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0210] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X12.

[0211] Example 13

[0212] Positive electrode:

[0213] The second positive electrode slurry A was applied to both sides of the aluminum foil to form a first coating layer. The first positive electrode slurry A was applied to the first coating layer to form a second coating layer. After drying, the positive electrode sheet Q13 was obtained. The active material layer of the positive electrode sheet Q13 consisted of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0214] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X13.

[0215] Comparative Example 1

[0216] Positive electrode sheet: The first positive electrode slurry L is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry A is then applied to the surface of the first coating layer to produce a positive electrode sheet Q14. The active material layer of the positive electrode sheet Q14 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each comprising 50% by weight.

[0217] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X14.

[0218] Comparative Example 2

[0219] Positive electrode sheet: The first positive electrode slurry L is applied to both sides of the aluminum foil to form a first coating layer. The second positive electrode slurry B is then applied to the surface of the first coating layer to produce a positive electrode sheet Q15. The active material layer of the positive electrode sheet Q15 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each accounting for 50% by weight.

[0220] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard-shell battery X15.

[0221] Comparative Example 3

[0222] Positive electrode sheet: The second positive electrode slurry A is applied to both sides of the aluminum foil to form a first coating layer. The first positive electrode slurry L is then applied to the surface of the first coating layer to produce a positive electrode sheet Q16. The active material layer of the positive electrode sheet Q16 consists of lithium nickel cobalt manganese oxide and lithium manganese iron phosphate, each comprising 50% by weight.

[0223] The negative electrode sheet, separator, and electrolyte composition are the same as those in Example 1, to obtain a hard shell battery X16.

[0224] The negative electrode is subjected to a peeling force test. The test method is as follows:

[0225] 1. Take the electrode to be tested and use a blade to cut a sample with a width of 30mm and a length of 100-160mm.

[0226] 2. Stick the special double-sided tape on the steel plate, with the tape width 20mm and length 90-150mm.

[0227] 3. Stick the electrode sample cut in step 1 on the double-sided tape with the test surface facing down, and then roll it three times in the same direction with a pressure roller.

[0228] 4. Insert a paper tape with a width equal to the electrode and a length 80-200 mm greater than the sample length under the electrode and secure it with wrinkle glue.

[0229] 5. Use Sansi tensile testing machine to perform peeling force test.

[0230] The test results are recorded in Table 3.

[0231] The hard shell batteries obtained in each embodiment were subjected to cycle performance tests, and the test method is as follows:

[0232] At 25°C, the hard-shell battery was first fully discharged at 1C before testing. The test process was as follows: the hard-shell battery was charged at a constant current of 1 / 3C to a voltage of 4.25V, then charged at a constant voltage of 4.25V to a current of 0.02C. After standing for 10 minutes, the lithium-ion battery was discharged at a constant current of 1 / 3C to a voltage of 2.8V. This constituted one charge-discharge cycle, and the discharge capacity was the discharge capacity of the first cycle. The hard-shell battery was subjected to 400 cycles of charge and discharge testing using the above method, and the discharge capacity retention rate was recorded.

[0233] The test results are recorded in Table 3.

[0234] Table 3

[0235] As can be seen from Table 3, the positive electrode Q1 has a maximum peeling force of 0.8 MPa because the NCM layer uses a PVDF copolymer and the LFMP layer uses a PVDF homopolymer. Once the NCM layer is paired with a homopolymer PVDF, such as the electrodes Q9 and Q10, their cathode peeling forces are significantly smaller than those of the electrode Q1.

[0236] As can be seen from Table 3, the NCM layer of Example 1 uses copolymerized PVDF, and the LFMP layer uses homopolymerized PVDF. In the long-term cycle process, the capacity of Example 1 is stable, and the capacity retention rate is 92% after 400 cycles.

[0237] The battery of Comparative Example 1 has a faster capacity decay during long-term cycling. After 400 cycles, the capacity retention rate is 77%. The reason is that the binders used for the two layers of different types of active materials are not classified and matched. The PVDF homopolymer has poor compatibility with NCM, and the cohesion of the positive electrode is not bad. During the cycling process, the binder cannot bind the particles well, resulting in their isolation and additional capacity loss.

[0238] Comparative Example 2 achieved a capacity retention rate of 75% after 400 cycles. The NCM-containing active layer in Comparative Example 2 used a PVDF homopolymer binder, while the LFMP-containing active layer used a PVDF copolymer binder. Due to the poor compatibility between PVDF homopolymer and NCM materials, the electrode peel force was relatively low. Therefore, the cycle improvement effect was significantly worse than that in Example 1.

[0239] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and components may be substituted with equivalents without departing from the scope of the present application. In particular, the various technical features described in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.

Claims

1. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode film layer comprises one or more first active layers and one or more second active layers arranged along the thickness direction of the positive electrode current collector, wherein the first active layers and the second active layers are alternately stacked, The first active layer includes a layered oxide active material and a first binder, wherein the first binder includes a first copolymer; The second active layer includes a phosphate-based positive electrode active material and a second binder, the second binder includes a fluorinated monomer homopolymer and / or a second copolymer, and the monomers forming the first copolymer and the second copolymer each independently include a fluorinated monomer.

2. The positive electrode sheet according to claim 1, wherein: The fluorinated monomers forming the first copolymer and the second copolymer each independently include any one or more selected from the group consisting of vinyl fluoride, vinylidene fluoride, trifluoroethylene, tetrafluoroethylene, hexafluoropropylene and perfluoroalkyl vinyl ether; optionally, the first copolymer and the second copolymer each independently include one or more selected from the group consisting of vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-ethylene oxide copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer.

3. The positive electrode sheet according to claim 1 or 2, wherein: The fluorinated monomer of the first copolymer and the second copolymer contains vinylidene fluoride; the first copolymer and the second copolymer each independently include one or more selected from the group consisting of vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-ethylene oxide copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-vinyl fluoride copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer; Optionally, the molar contents of the structural units corresponding to the vinylidene fluoride monomer in the first copolymer and the second copolymer are independently 50 to 95%.

4. The positive electrode sheet according to any one of claims 1 to 3, wherein: The second binder is a fluorinated monomer homopolymer; optionally, the fluorinated monomer homopolymer is a vinylidene fluoride homopolymer.

5. The positive electrode sheet according to any one of claims 1 to 4, wherein: The weight average molecular weights of the first copolymer, the second copolymer and the fluorinated monomer homopolymer are each independently 100,000 Da to 1,000,000 Da.

6. The positive electrode sheet according to any one of claims 1 to 4, wherein: The positive electrode sheet satisfies any one or more of the following conditions: The mass content of the first binder in the first active layer is 0.5% to 2.5%; The mass content of the second binder in the second active layer is 0.5% to 2.5%; The first active layer and the second active layer each independently include a conductive agent.

7. The positive electrode sheet according to any one of claims 1 to 6, wherein: The pH value of the mixed slurry formed by mixing the layered oxide active material with water and forming a 10% by mass content is between 11 and 13; optionally, the layered oxide active material includes a ternary positive electrode material and / or a quaternary positive electrode material, and optionally, the layered oxide active material includes one or more selected from the group consisting of nickel cobalt manganese oxide positive electrode active material, nickel cobalt aluminum oxide positive electrode active material, nickel cobalt manganese aluminum oxide positive electrode active material, doped or coated nickel cobalt manganese oxide positive electrode active material, doped or coated nickel cobalt aluminum oxide positive electrode active material, and doped or coated nickel cobalt manganese aluminum oxide positive electrode active material.

8. The positive electrode sheet according to claim 7, wherein: The surface of the layered oxide active material has a first coating layer, and the first coating layer includes a single coating layer or multiple coating layers selected from the group consisting of carbon, conductive graphene, conductive polymer material, and oxide.

9. The positive electrode sheet according to any one of claims 1 to 8, wherein: The pH value of the mixed slurry formed by mixing the phosphate-based positive electrode active material with water and having a mass content of 10% is between 8 and 10; optionally, the phosphate-based positive electrode active material includes at least one of the following materials: LiMn 1-y Fe y PO4,y is any value in the range of 0.001 to 0.5; Li 1+t Mn 1-c Fe c P 1-z R z O4, t is any value in the range of -0.100 to 0.100, c is any value in the range of 0.001 to 0.500, z is any value in the range of 0.001 to 0.100, and R includes one or more elements selected from B, S, Si and N; Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n , wherein A comprises one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W, E comprises one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, R comprises one or more elements selected from B, S, Si and N, D comprises one or more elements selected from S, F, Cl and Br, w is any value in the range of -0.100 to 0.100, m is any value in the range of 0.001 to 0.1, u is any value in the range of 0.001 to 0.500, a is any value in the range of 0.001 to 0.100, n is any value in the range of 0.001 to 0.1, and Li 1+w A m Mn 1-u E u P 1-a R a O 4-n D n It is electrically neutral.

10. The positive electrode sheet according to claim 9, wherein: The surface of the phosphate-based positive electrode active material has a second coating layer, and the second coating layer includes a single coating layer or multiple coating layers of pyrophosphate, phosphate, and carbon.

11. The positive electrode sheet according to any one of claims 1 to 10, wherein: The arrangement of the positive electrode film layer includes any one of the following methods: The first active layer and the second active layer are both one layer; The first active layer is one layer and the second active layer is two layers, and the first active layer is arranged between the second active layers; The first active layer is two layers and the second active layer is one layer, and the second active layer is arranged between the first active layers.

12. The positive electrode sheet according to any one of claims 1 to 11, wherein: The ratio of the thickness of the first active layer to the thickness of the second active layer is 0.9:1 to 1.1:

1.

13. A secondary battery, comprising a positive electrode sheet and a negative electrode sheet, wherein: The positive electrode sheet comprises the positive electrode sheet according to any one of claims 8 to 11.

14. An electrical device comprising a secondary battery, wherein: The secondary battery includes the secondary battery according to claim 13.

Citation Information

Patent Citations

  • Lithium manganese oxide and manufacturing method thereof, lithium secondary cell and positive active materials

    CN101140987A

  • Electrode slice and electrochemical energy storage apparatus

    CN105703010A

  • LiMn1-XFexPO4 positive electrode material having core-shell structure, and preparation method thereof, and lithium ion battery

    CN106058225A

  • Positive pole piece and preparation method thereof, and lithium ion secondary battery

    CN111092194A

  • Positive plate and high-safety lithium ion battery thereof

    CN112768702A

Cited By

  • Positive electrode sheet, battery including same, and electrical apparatus

    WO2026214102A1