Silicon carbon negative electrode material, and preparation method therefor and use thereof

By coating the silicon carbon material with a cross-linked network structure of lithium polyacrylate compounds, cross-linking agents and conductive materials, the volume expansion and cycle performance problems of silicon carbon anode materials in lithium-ion batteries are solved, and higher performance is achieved. Battery cycle performance and feasibility of industrial production.

WO2024221285A1PCT designated stage expired Publication Date: 2024-10-31WUXI LINGYI FUTURE RES INST OF NEW MATERIALS TECH CO LTD

Patent Information

Application Number
PCT/CN2023/090920
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2023-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing silicon-carbon anode materials suffer from volume expansion and cycle performance failure in lithium-ion batteries, especially the reduction in electrochemical performance due to the crushing of silicon particles and separation from current collectors. The traditional process is complex and unfavorable for industrial production.

Method used

Lithium polyacrylate compounds, cross-linking agents and conductive materials are used as the coating layer to improve the conductivity by forming a cross-linked network structure, restrain the volume expansion of the silicon carbon material, inhibit the growth of the SEI film, and improve the cycle performance.

Benefits of technology

The cycle performance and battery electrical performance of the silicon-carbon anode material are significantly improved, especially the cycle performance. The process is safe and environmentally friendly, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023090920-FTAPPB-I100001
    Figure PCTCN2023090920-FTAPPB-I100001
  • Figure PCTCN2023090920-FTAPPB-I100002
    Figure PCTCN2023090920-FTAPPB-I100002
Patent Text Reader

Abstract

A silicon carbon negative electrode material comprises a silicon carbon material and a coating layer with which the silicon carbon material is coated; the materials of the coating layer comprise a lithium polyacrylate compound, a crosslinking agent, and a conductive material. The lithium polyacrylate compound, the crosslinking agent, and the conductive material are blended to serve as the materials of the coating layer, so that the coating layer has excellent electric conductivity and lithium conduction performance, can effectively inhibit the volume expansion of the silicon carbon material, and can also inhibit the growth of an SEI film on the surface of the silicon carbon material, thereby effectively improving the cycle performance of a battery comprising the silicon carbon negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

A silicon-carbon negative electrode material and its preparation method and application Technical Field

[0001] The present application belongs to the field of lithium battery technology, for example, a silicon-carbon negative electrode material and its preparation method and application. Background Art

[0002] Anode materials, as carriers of lithium ions and electrons during the charging process of lithium batteries, play a role in energy storage and release. Currently, commercial lithium battery anode materials are primarily modified natural graphite and artificial graphite. Despite mature preparation technology, their theoretical specific capacity is only 372 mAh / g, which remains insufficient to meet market demand for high-capacity lithium-ion batteries. High-capacity anode materials can effectively improve the energy density of the entire battery. In a graphite anode, six carbon atoms are required to store one lithium ion, while each silicon atom can bind to four lithium ions. As a result, a silicon anode material can store 10 times the charge of a graphite anode material of the same volume. In other words, silicon anode materials can directly increase the battery's energy density by an order of magnitude. Therefore, the research and development of silicon-based anodes with higher gram capacities has become a priority. However, due to the large lithium storage capacity of silicon-based materials, the crystal lattice expands during lithium insertion and collapses during lithium removal. This leads to significant volume changes during cycling, causing silicon particles to shatter and detach from the current collector, resulting in a loss of electrochemical performance. Moreover, due to the volume effect of silicon, the SEI film on its surface will continue to grow, continuously consuming lithium ions, causing the capacity to decay rapidly, and affecting the cycle performance of silicon negative electrode materials in lithium-ion batteries.

[0003] Silicon-carbon negative electrode material is a new type of negative electrode material with carbon as the dispersed matrix and silicon as the active material. However, due to its high volume expansion and the side reaction with the electrolyte, it accelerates the capacity decay. In practical applications, it is still necessary to further improve its own insufficient conductivity and the performance degradation caused by the non-negligible volume expansion. At present, in order to solve the problems of volume expansion and cycle performance failure faced by silicon-carbon negative electrode materials, on the one hand, the silicon-carbon negative electrode is pre-treated by nano-sizing, composite, porous, alloying, pre-lithiation, etc., to alleviate the adverse effects of volume change on the electrode to a certain extent and improve the cycle performance of the material; on the other hand, by surface modification of silicon-based materials, including carbon coating and polymer coating, the first charge reversible capacity, cycle stability and battery rate performance of the negative electrode material are improved.

[0004] CN110931744A discloses a method for preparing a silicon-carbon anode material. The method involves adding a polymer monomer and a catalyst to a silicon source to react and obtain a polymer nanobelt-coated silicon material. The material is then carbonized in an inert atmosphere to obtain a silicon-carbon anode material. The material is formed by polymerizing and carbonizing low-steric aldehyde monomers such as formaldehyde and acetaldehyde with phenolic monomers in the silicon source to form a high-porosity network-like coating structure. This effectively mitigates the volume expansion of silicon during lithium insertion and extraction, thereby extending the cycle life of lithium-ion batteries. However, this method requires the use of large amounts of small-molecule monomers such as formaldehyde and acetaldehyde, which are highly toxic and carcinogenic, limiting its industrial application.

[0005] CN115732664A discloses a silicon-carbon composite material, its preparation method, and a secondary battery. The invention includes a silicon-carbon composite core and a carbon coating layer that coats the silicon-carbon composite core. The multiple closed pores dispersed in the silicon-carbon composite core can effectively alleviate the huge volume effect generated by silicon during lithium insertion and removal. At the same time, the silicon-carbon composite core and the carbon coating layer can further alleviate the volume effect generated by silicon during lithium insertion and removal, thereby improving the material's cycling performance. However, the coating process is complex, requiring the preparation of a nano-silicon dispersion, the preparation of two precursors, and then carbon coating. Furthermore, a UV / ozone device is required to surface treat the polymer material. The process is extremely complex and is not conducive to industrial production.

[0006] CN111081976A discloses a method for preparing a silicon-carbon-polymer composite electrode for a lithium secondary battery. The electrode comprises a core-shell structure formed by chemically coating nanosilicon with cyclized conductive polyacrylonitrile, which is then composited with a graphite carbon material. Micronized silicon and polyacrylonitrile are ball-milled to form a nanocomposite. The resulting composite, along with graphite, is then added to a PAN solution in dimethylformamide, stirred uniformly, and dried to yield the final product. However, this method fails to effectively suppress the negative effects of silicon's volume expansion, hindering cycling performance. Furthermore, the production process requires a large amount of organic solvent to dissolve the PAN, increasing process costs.

[0007] Therefore, developing a silicon-carbon negative electrode material with excellent electrical conductivity and lithium conductivity and the ability to effectively inhibit the volume expansion of silicon-carbon materials is a technical problem that urgently needs to be solved.

[0008] Summary of the Invention

[0009] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0010] The present application provides a silicon-carbon negative electrode material, a preparation method, and an application thereof. The silicon-carbon negative electrode material includes a silicon-carbon material and a coating layer coated on the outside of the silicon-carbon material. The material of the coating layer includes a lithium polyacrylate compound, a cross-linking agent, and a conductive material. By selecting the above three materials as the material of the coating layer, the obtained coating layer has excellent electrical conductivity and lithium conductivity, and can effectively restrain the volume expansion of the silicon-carbon material and inhibit the continuous growth of the SEI film on the surface of the silicon-carbon material, thereby effectively improving the electrical performance of the battery containing the silicon-carbon negative electrode material, especially the cycle performance.

[0011] This application adopts the following technical solutions:

[0012] In a first aspect, an embodiment of the present application provides a silicon-carbon negative electrode material, wherein the silicon-carbon negative electrode material comprises a silicon-carbon material and a coating layer coated on the outside of the silicon-carbon material;

[0013] The materials of the coating layer include lithium polyacrylate compounds, a cross-linking agent and a conductive material.

[0014] The silicon-carbon negative electrode material provided in the embodiment of the present application includes a silicon-carbon material and a coating layer coated on the outside of the silicon-carbon material, and the material of the coating layer includes a lithium polyacrylate compound, a cross-linking agent and a conductive material. On the one hand, by selecting a combination of a lithium polyacrylate compound, a cross-linking agent and a conductive material as the material of the coating layer, and utilizing the good lithium ion conductivity of the lithium polyacrylate compound, further combining the cross-linking agent can form a cross-linked network structure in the coating layer, which is conducive to improving the conductive material to form a more stable conductive network therein, so that the obtained coating layer has excellent electrical conductivity and lithium conductivity; on the other hand, the coating layer formed by the above three materials can effectively restrain the silicon-carbon material and reduce its volume expansion, thereby avoiding or reducing the problem of the silicon-carbon negative electrode material losing its electrochemical performance due to the breakage of silicon particles and the separation of the current collector, and also effectively inhibiting the continuous growth of the SEI film on the surface of the obtained silicon-carbon negative electrode material, reducing its sensitivity to lithium ions (Li + ) is consumed continuously, thereby effectively improving the electrical performance of the battery, especially the cycle performance.

[0015] In one embodiment, the structure of the silicon-carbon material includes any one of a single-layer core-shell structure, a multi-layer core-shell structure, a sandwich structure, or an embedded structure, or a combination of at least two thereof, but is not limited to the above structures.

[0016] The single-layer core-shell structure is a single-layer core-shell structure of carbon-coated silicon.

[0017] In one embodiment, the particle size of the silicon-carbon material is 50 nm to 20 μm, for example, 100 nm, 500 nm, 1 μm, 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm or 18 μm.

[0018] As an optional technical solution for an embodiment of the present application, the particle size of the silicon-carbon material is limited to 50nm~20μm, so that it has a smaller particle size and more inter-particle gaps, which makes it easier to buffer the stress and deformation generated by silicon during the process of lithium ion insertion and extraction; in addition, silicon-carbon material particles with a particle size of 50nm~20μm can shorten the diffusion distance of lithium ions and increase the lithium storage capacity of silicon materials. This is because there is a critical particle size of about 150nm for the lithiation of a single silicon particle. When the particle size is lower than this critical particle size, the particle will not break during the first lithiation, so the particle size of the optional silicon-carbon material is 50nm~20μm.

[0019] In one embodiment, the specific surface area of ​​the silicon-carbon material is 0.5 to 2.5 m 2 / g, for example 0.7m 2 / g, 0.9m 2 / g, 1.1m 2 / g, 1.3m 2 / g, 1.5m 2 / g, 1.7m 2 / g, 1.9m 2 / g, 2.1m 2 / g or 2.3m 2 / g, etc.

[0020] In one embodiment, the mass percentage of the coating layer in the silicon-carbon negative electrode material is 0.1-10%, for example, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%.

[0021] As an optional technical solution of the embodiment of the present application, the mass percentage of the coating layer in the silicon-carbon negative electrode material is limited to 0.1-10%, which can not only play a good coating and binding effect on the silicon-carbon material, but also will not reduce the content of effective ingredients in the silicon-carbon negative electrode material due to the excessive mass proportion of the coating layer, and will not reduce the energy density of the silicon-carbon negative electrode material.

[0022] In one embodiment, the mass percentage of the conductive material in the coating layer is 1-20%, for example, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16% or 18%.

[0023] In one embodiment, the conductive material includes any one of graphene, acetylene black, carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes, or flake graphite, or a combination of at least two thereof.

[0024] In one embodiment, the total mass percentage of the lithium polyacrylate compound and the cross-linking agent in the coating layer material is 80-99%, for example, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96% or 98%.

[0025] In one embodiment, the number average molecular weight of the lithium polyacrylate compound is 200-300,000, for example, 500, 1,000, 5,000, 10,000, 50,000, 100,000 or 200,000.

[0026] In one embodiment, the cross-linking agent has a number average molecular weight of 200 to 200,000, for example, 500, 1,000, 5,000, 10,000, 50,000, 100,000 or 150,000.

[0027] As an optional technical solution of the embodiment of the present application, it is necessary to limit the number average molecular weight of the lithium polyacrylate compound to 200-300,000, and the number average molecular weight of the cross-linking agent to 200-200,000. If the number average molecular weights of the two are lower than the above-mentioned respective limited ranges, the flexibility of the two will be poor, and if the number average molecular weights of the two are higher than the above-mentioned respective limited ranges, the water solubility of the two will be poor.

[0028] In one embodiment, based on the total mass of the lithium polyacrylate compound and the cross-linking agent as 100%, the mass percentage of the lithium polyacrylate compound is 50-99.8%, for example, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90% or 95%, etc.

[0029] In one embodiment, the cross-linking agent includes any one or a combination of at least two of cellulose and its derivatives, polysaccharides and their derivatives, polyethylene glycol and its derivatives, polyvinyl alcohol and its derivatives, or plant gum and its derivatives.

[0030] In one embodiment, the cellulose and its derivatives include any one of hydroxymethyl cellulose, sulfonated cellulose, hydroxypropyl cellulose or carboxymethyl cellulose, or a combination of at least two thereof.

[0031] In one embodiment, the polysaccharide and its derivatives include any one of glucose, polylactose or arabinose, or a combination of at least two of them.

[0032] In one embodiment, the polyethylene glycol and its derivatives include any one of polyethylene glycol, polyethylene glycol monomethyl ether or polyethylene glycol monolaurate, or a combination of at least two thereof.

[0033] In one embodiment, the polyvinyl alcohol and its derivatives include any one of polyvinyl alcohol, polyvinyl titanate or polyvinyl formal, or a combination of at least two thereof.

[0034] In one embodiment, the plant seed gum and its derivatives include any one of locust bean gum, guar gum or carboxylated locust bean gum, or a combination of at least two thereof.

[0035] In one embodiment, the raw materials for preparing the lithium polyacrylate compound include reactive monomers and lithium salts, and the reactive monomers include acrylic acid first monomers.

[0036] In one embodiment, the acrylic first monomer includes acrylic acid and / or methacrylic acid.

[0037] In one embodiment, the reactive monomer further includes a second monomer, and the second monomer includes any one or a combination of at least two of methyl methacrylate, styrene, acrylonitrile, 2-hydroxyethyl acrylate, or acrylamide.

[0038] As an optional technical solution of the embodiment of the present application, the purpose of limiting the reaction monomer to also include a second monomer is to improve the toughness of the formed coating layer and prevent the coating layer from being easily broken and losing the restraint of the silicon-carbon material.

[0039] In one embodiment, the mass percentage of the acrylic acid first monomer in the reactive monomers is not less than 60%, for example, 65%, 70%, 75%, 80%, 85%, 90% or 95%.

[0040] In one embodiment, the lithium salt includes lithium hydroxide.

[0041] In a second aspect, an embodiment of the present application provides a method for preparing the silicon-carbon negative electrode material as described in the first aspect, the preparation method comprising: mixing a lithium polyacrylate compound, a cross-linking agent and a conductive material in water, adding the silicon-carbon material and continuing to mix, and drying to obtain the silicon-carbon negative electrode material.

[0042] In one embodiment, the drying specifically includes any one of stirring drying, vacuum drying, oven drying or spray drying, or a combination of at least two thereof.

[0043] In one embodiment, the drying temperature is 80-200°C, for example, 100°C, 120°C, 140°C, 160°C or 180°C.

[0044] As an optional technical solution of an embodiment of the present application, the drying temperature will affect the cross-linking degree of the polymer cross-linking reaction; if the temperature is too low, the cross-linking reaction degree is low, and a cross-linked network structure is not formed, resulting in poor strength of the coating layer; and if the reaction temperature is too high, it will lead to an excessively high degree of cross-linking reaction, excessive curing, and the material of the coating layer becomes brittle.

[0045] In a third aspect, an embodiment of the present application provides a negative electrode slurry, which includes the silicon-carbon negative electrode material as described in the first aspect.

[0046] In one embodiment, the negative electrode slurry further includes a conductive agent and a binder.

[0047] In a fourth aspect, an embodiment of the present application provides a negative electrode plate, wherein the raw materials for preparing the negative electrode plate include the negative electrode slurry described in the third aspect.

[0048] In one embodiment, the negative electrode plate further includes copper foil.

[0049] In a fifth aspect, an embodiment of the present application provides a battery, comprising the silicon-carbon negative electrode material as described in the first aspect.

[0050] This application has the following beneficial effects:

[0051] (1) The silicon-carbon negative electrode material provided in the present application includes a silicon-carbon material and a coating layer coated on the outside of the silicon-carbon material, wherein the material of the coating layer includes a lithium polyacrylate compound, a cross-linking agent and a conductive material. By coating the surface of the silicon-carbon material with a coating layer composed of a lithium polyacrylate compound, a cross-linking agent and a conductive material, the coating layer can effectively restrain the silicon-carbon material, reduce its volume expansion, and effectively reduce its consumption of electrolyte during the cycle.

[0052] (2) The materials of the coating layer in the silicon-carbon negative electrode material provided in the present application include polyacrylate lithium compounds, cross-linking agents and conductive materials. The polyacrylate lithium compounds and cross-linking agents can form a cross-linked network structure, which is conducive to the formation of a stable conductive network between the conductive material and the polymer, thereby effectively improving the conductivity and ion conductivity of the coating layer.

[0053] (3) The silicon-carbon negative electrode material provided in this application also has the advantages of safe and environmentally friendly production process, low energy consumption, and easy industrial scale-up.

[0054] (4) The silicon-carbon negative electrode material provided in the present application can effectively improve the cycle performance of the button battery containing the same. Specifically, the peel strength of the negative electrode plate made using the silicon-carbon negative electrode material provided in the present application is 80.1 to 94.5 N / m, and the cycle capacity retention rate of the battery further prepared is 75.2 to 83.8%, and the full-charge expansion rate of the plate is 180 to 226%.

[0055] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION

[0056] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.

[0057] The structure of the silicon-carbon materials selected in the specific embodiment of the present application is an embedded structure with carbon material as the matrix, a particle size of 8 to 10 μm, and a specific surface area of ​​25 m 2 / g.

[0058] Preparation Example 1

[0059] A lithium polyacrylate compound A1 is prepared by the following steps: dissolving 7.5 g of acrylic acid in 150 g of water, introducing nitrogen, setting the stirring speed to 300 rpm, heating to 70° C., adding 2 g of styrene, 0.5 g of methyl methacrylate, and 1 g of acrylonitrile, and mixing them uniformly, adding them dropwise at a uniform speed for 10 minutes, maintaining the temperature at 70° C. for 10 minutes, adding 0.05 g of azobisisobutylcyanide initiator dropwise, reacting at 70° C. for 6 hours, cooling to room temperature, adding 4.1 g of an aqueous solution of lithium hydroxide monohydrate (the molar concentration of lithium hydroxide monohydrate is 0.1 mol / L) to the system, and stirring at room temperature for 1 hour to obtain the lithium polyacrylate compound A1.

[0060] Preparation Example 2

[0061] A lithium polyacrylate compound A2 is prepared by dissolving 7.5 g of acrylic acid in 150 g of water, introducing nitrogen, setting the stirring speed to 300 rpm, heating to 70° C., adding 1.5 g of 2-hydroxyethyl acrylate, 0.5 g of methyl methacrylate, and 1 g of acrylonitrile, and mixing them uniformly, adding them dropwise at a uniform speed for 10 minutes, keeping the temperature at 70° C. for 10 minutes, adding 0.05 g of azobisisobutyl cyanide initiator dropwise, reacting at 70° C. for 8 hours, cooling to room temperature, adding 4.1 g of an aqueous solution of lithium hydroxide monohydrate (the molar concentration of lithium hydroxide monohydrate is 0.1 mol / L) to the system, and stirring at room temperature for 1 hour to obtain the lithium polyacrylate compound A2.

[0062] Preparation Example 3

[0063] A lithium polyacrylate compound A3 is prepared by dissolving 7.5 g of acrylic acid in 150 g of water, introducing nitrogen, setting the stirring speed to 300 rpm, heating to 70° C., adding 1 g of acrylonitrile and mixing uniformly, adding dropwise at a uniform speed for 10 minutes, maintaining the temperature at 70° C. for 10 minutes, adding dropwise 0.05 g of azobisisobutylcyanide initiator, reacting at 70° C. for 8 hours, cooling to room temperature, adding 4.1 g of an aqueous solution of lithium hydroxide monohydrate (the molar concentration of lithium hydroxide monohydrate is 0.1 mol / L) to the system, and stirring at room temperature for 1 hour to obtain the lithium polyacrylate compound A3.

[0064] Preparation Example 4

[0065] A lithium polyacrylate compound A4 is prepared by dissolving 7.5 g of acrylic acid in 150 g of water, introducing nitrogen, setting the stirring speed to 300 rpm, heating to 70° C. and maintaining the temperature for 10 minutes, dropwise adding 0.05 g of azobisisobutylcyanide initiator, reacting at 70° C. for 6 hours, cooling to room temperature, adding 4.1 g of an aqueous solution of lithium hydroxide monohydrate to the system, and stirring at room temperature for 1 hour to obtain the lithium polyacrylate compound A4.

[0066] Example 1

[0067] A silicon-carbon negative electrode material, comprising 100 g of a silicon-carbon material and a coating layer coated on the silicon-carbon material, wherein the coating layer comprises 2.4 g of a lithium polyacrylate compound A1 (Preparation Example 1), 0.55 g of polyvinyl alcohol (number average molecular weight of 25,000), and 0.05 g of graphene;

[0068] The preparation method includes: dissolving a lithium polyacrylate compound A1, graphene and polyvinyl alcohol in 120g of water, stirring at a rotation speed of 1800rpm for 0.5h to obtain a coating slurry; then, adding a silicon-carbon material thereto, reducing the rotation speed to 1500rpm and stirring for 0.5h, and drying at 100°C for 12h to crush and disperse the product to obtain the silicon-carbon negative electrode material.

[0069] Example 2

[0070] A silicon-carbon negative electrode material is different from Example 1 only in that polyethylene glycol (number average molecular weight is 20,000) is used to replace polyvinyl alcohol, and other components, amounts and preparation methods are the same as those in Example 1.

[0071] Example 3

[0072] A silicon-carbon negative electrode material is provided, which differs from Example 1 only in that single-walled carbon nanotubes are used instead of graphene, and other components, amounts and preparation methods are the same as those in Example 1.

[0073] Example 4

[0074] A silicon-carbon negative electrode material, which differs from Example 1 only in that the lithium polyacrylate compound A2 (Preparation Example 2) is used to replace the lithium polyacrylate compound A1 obtained in Preparation Example 1, and the other components, amounts and preparation methods are the same as those in Example 1.

[0075] Example 5

[0076] A silicon-carbon negative electrode material, which differs from Example 1 only in that the lithium polyacrylate compound A3 (Preparation Example 3) is used to replace the lithium polyacrylate compound A1 obtained in Preparation Example 1, and the other components, amounts and preparation methods are the same as those in Example 1.

[0077] Example 6

[0078] A silicon-carbon negative electrode material, which differs from Example 1 only in that the lithium polyacrylate compound A4 (Preparation Example 4) is used to replace the lithium polyacrylate compound A1 obtained in Preparation Example 1, and the other components, amounts and preparation methods are the same as those in Example 1.

[0079] Example 7

[0080] A silicon-carbon negative electrode material, which differs from Example 1 only in that the material of the coating layer includes 2g of lithium polyacrylate compound A1, 0.95g of polyvinyl alcohol and 0.05g of graphene, and the other components, amounts and preparation methods are the same as those in Example 1.

[0081] Example 8

[0082] A silicon-carbon negative electrode material is different from Example 1 only in that the amount of silicon-carbon material used is 25 g, and the other components, amounts and preparation methods are the same as those in Example 1.

[0083] Comparative Example 1

[0084] A silicon-carbon negative electrode material is directly a silicon-carbon material without any coating layer.

[0085] Comparative Example 2

[0086] A silicon-carbon negative electrode material, which differs from Example 1 only in that the material of the coating layer does not include polyvinyl alcohol, but only includes 2.95g of lithium polyacrylate compound A1 and 0.05g of graphene. Other components, amounts and preparation methods are the same as those in Example 1.

[0087] Comparative Example 3

[0088] A silicon-carbon negative electrode material, which differs from Example 1 only in that the material of the coating layer does not include graphene, but only includes 2.45g of lithium polyacrylate compound A1 and 0.55g of polyvinyl alcohol, and the other components, amounts and preparation methods are the same as those in Example 1.

[0089] Performance testing:

[0090] Preparation of button batteries: Silicon-carbon negative electrode material, conductive carbon black, sodium carboxymethyl cellulose and polyacrylic acid (number average molecular weight of 100,000) are prepared into a negative electrode slurry in a mass ratio of 70:15:5:10, and the slurry is evenly coated on copper foil and dried to form a negative electrode plate. The negative electrode plate is placed in an argon atmosphere glove box to make a button battery. A polypropylene microporous membrane is used as a separator. The electrolyte used is 1 mol / L lithium hexafluorophosphate (the solvent is a mixture of ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate and fluoroethylene carbonate in a volume ratio of 30:30:30:10), and the counter electrode used is a metal lithium sheet.

[0091] (1) Peel strength: The negative electrode is subjected to a peel strength test according to GB / T 2790-1995.

[0092] (2) Negative electrode full charge expansion rate and cycle capacity retention rate: button cells were cycled for 50 cycles with a voltage range of 0.005 to 1.5 V and a charge and discharge rate of 0.5 C. The cycle capacity retention rate was calculated after the cycle test. The button cells were disassembled, and the thickness of the negative electrode plate was measured when fully charged to calculate the negative electrode full charge expansion rate.

[0093] Among them, the 50-week cycle capacity retention rate = the 50th cycle discharge capacity / the first week discharge capacity × 100%, and the full-charge expansion rate of the negative electrode plate = (the thickness of the electrode plate after full charge - the thickness of the uncharged electrode plate) / the thickness of the uncharged electrode plate × 100%.

[0094] The button batteries prepared from the silicon-carbon negative electrode materials provided in Examples 1 to 8 and Comparative Examples 1 to 3 were tested according to the above test method. The test results are shown in Table 1:

[0095] Table 1

[0096] According to the data in Table 1, we can see that:

[0097] The peel strength of the negative electrode sheets made of the silicon-carbon negative electrode materials provided in Examples 1 to 8 is 80.1 to 94.5 N / m, the cycle capacity retention rate of the batteries further prepared is 75.2 to 83.8%, and the full-charge expansion rate of the sheets is 180 to 226%.

[0098] By comparing Example 1 with Comparative Examples 1 to 3, it can be seen that the silicon-carbon negative electrode material provided in Comparative Example 1 without a coating layer, the silicon-carbon negative electrode material provided in Comparative Example 2 with no cross-linking agent added to the coating layer, and the silicon-carbon negative electrode material provided in Comparative Example 3 with no conductive material added to the coating layer all have low peel strength after being made into pole pieces, and the cycle capacity retention rate of the batteries further made is poor, and the full-charge expansion rate of the pole pieces is also very high.

[0099] Comparing Example 1 and Example 6, it can be seen that the failure to add a second monomer in the preparation of the lithium polyacrylate compound will also have an adverse effect on the peel strength of the final silicon-carbon negative electrode material after it is made into a pole piece, as well as the cycle capacity retention rate and full-charge expansion rate of the pole piece after it is made into a battery.

[0100] Further comparison of Example 1 and Example 7 shows that the proportion of lithium polyacrylate compounds in the coating layer is relatively low, which will also affect the peel strength of the silicon-carbon negative electrode material after it is made into a pole piece, as well as the cycle capacity retention rate and full-charge expansion rate of the pole piece after it is made into a battery.

[0101] Finally, by comparing Example 1 and Example 8, it can be seen that the overall proportion of the coating layer is too high. Although it will increase the peel strength of the silicon-carbon negative electrode material after it is made into a pole piece, the cycle capacity retention rate after further making it into a battery is very low, and the pole piece expansion rate when fully charged is very high.

[0102] The applicant declares that this application uses the above-mentioned embodiments to illustrate a silicon-carbon negative electrode material, its preparation method, and application, but this application is not limited to the above-mentioned embodiments, that is, it does not mean that this application must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvements to this application, equivalent replacement of various raw materials of the product of this application, addition of auxiliary components, selection of specific methods, etc., all fall within the scope of protection and disclosure of this application.

Claims

1. A silicon-carbon negative electrode material, comprising a silicon-carbon material and a coating layer coated outside the silicon-carbon material; The materials of the coating layer include lithium polyacrylate compounds, a cross-linking agent and a conductive material.

2. The silicon-carbon negative electrode material according to claim 1, wherein: The structure of the silicon-carbon material includes any one of a single-layer core-shell structure, a multi-layer core-shell structure, a sandwich structure or an embedded structure, or a combination of at least two thereof; Optionally, the particle size of the silicon-carbon material is 50 nm to 20 μm; Optionally, the specific surface area of ​​the silicon-carbon material is 0.5 to 2.5 m 2 / g.

3. The silicon-carbon negative electrode material according to claim 1 or 2, wherein: The mass percentage of the coating layer in the silicon-carbon negative electrode material is 0.1 to 10%; Optionally, the mass percentage of the conductive material in the coating layer is 1 to 20%; Optionally, the conductive material includes any one of graphene, acetylene black, carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes or flake graphite, or a combination of at least two of them.

4. The silicon-carbon negative electrode material according to any one of claims 1 to 3, wherein: The total mass percentage of the lithium polyacrylate compound and the cross-linking agent in the coating layer material is 80-99%; Optionally, the number average molecular weight of the lithium polyacrylate compound is 200 to 300,000; Optionally, the number average molecular weight of the cross-linking agent is 200 to 200,000.

5. The silicon-carbon negative electrode material according to any one of claims 1 to 4, wherein: Taking the total mass of the lithium polyacrylate compound and the cross-linking agent as 100%, the mass percentage of the lithium polyacrylate compound is 50 to 99.8%; Optionally, the cross-linking agent includes any one or a combination of at least two of cellulose and its derivatives, polysaccharides and their derivatives, polyethylene glycol and its derivatives, polyvinyl alcohol and its derivatives, or plant gum and its derivatives; Optionally, the cellulose and its derivatives include any one or a combination of at least two of hydroxymethyl cellulose, sulfonated cellulose, hydroxypropyl cellulose or carboxymethyl cellulose; Optionally, the polysaccharide and its derivatives include any one or a combination of at least two of glucose, polylactose or arabinose; Optionally, the polyethylene glycol and its derivatives include any one or a combination of at least two of polyethylene glycol, polyethylene glycol monomethyl ether or polyethylene glycol monolaurate; Optionally, the polyvinyl alcohol and its derivatives include any one of polyvinyl alcohol, polyvinyl alcohol titanate or polyvinyl alcohol formal or a combination of at least two thereof; Optionally, the plant seed gum and its derivatives include any one or a combination of at least two of locust bean gum, guar gum or carboxylated locust bean gum; Optionally, the raw materials for preparing the lithium polyacrylate compound include a reaction monomer and a lithium salt, and the reaction monomer includes an acrylic acid first monomer; Optionally, the acrylic first monomer includes acrylic acid and / or methacrylic acid; Optionally, the reactive monomer further comprises a second monomer, and the second monomer comprises any one or a combination of at least two of methyl methacrylate, styrene, acrylonitrile, 2-hydroxyethyl acrylate or acrylamide; Optionally, the mass percentage of the acrylic acid first monomer in the reaction monomer is not less than 60%; Optionally, the lithium salt comprises lithium hydroxide.

6. A method for preparing the silicon-carbon negative electrode material according to any one of claims 1 to 5, the method comprising: The lithium polyacrylate compound, the cross-linking agent and the conductive material are mixed in water, the silicon-carbon material is added and continued to be mixed, and then dried to obtain the silicon-carbon negative electrode material.

7. The preparation method according to claim 6, wherein: The drying specifically includes any one of stirring drying, vacuum drying, oven drying or spray drying, or a combination of at least two thereof; Optionally, the drying temperature is 80-200°C.

8. A negative electrode slurry, comprising the silicon-carbon negative electrode material according to any one of claims 1 to 5. 9 . A negative electrode sheet, wherein the raw material for preparing the negative electrode sheet comprises the negative electrode slurry according to claim 8 .

10. A battery, comprising the silicon-carbon negative electrode material according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Double-layer coated silicon-based composite negative electrode material and preparation method thereof

    CN111048769A

  • Anode material and electrochemical device including same and electronic device

    CN111146422A

  • Silicon-based composite material for negative active material, negative plate and lithium ion battery

    CN112002883A

  • Negative electrode for lithium ion secondary battery and lithium ion secondary battery

    CN112823440A

  • Silicon-oxygen negative electrode material with surface connected with binder, and preparation method and application of silicon-oxygen negative electrode material

    CN115799488A

Cited By

  • Lithium ion battery silicon-based negative electrode material and preparation method and application thereof

    CN119133422A

  • Preparation method of copper-doped bi-crosslinked asphalt-based porous carbon and product and application of copper-doped bi-crosslinked asphalt-based porous carbon

    CN119637845A

  • Silicon-carbon negative electrode material based on nanocellulose as well as preparation method and application of silicon-carbon negative electrode material

    CN119911895A

  • Lithium-ion battery negative electrode material and preparation method therefor

    WO2026108205A1