Positive electrode sheet, battery, and electric device

By using a combination of first and second positive active materials in the upper and lower film layers of the positive electrode sheet, the problem of poor low-temperature rate performance in the existing technology is solved, the low-temperature power and fast charging performance of the battery are improved, the battery life is extended, and Improved cycle life.

WO2024221337A1PCT designated stage expired Publication Date: 2024-10-31CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/091177
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing lithium iron phosphate cathode active materials have poor low-temperature rate performance under low-temperature conditions and insufficient conductivity, resulting in short battery life; ternary cathode active materials are prone to undervoltage when using high-current discharge under low-temperature conditions, and cannot meet high-temperature requirements. magnification and fast charging performance requirements.

Method used

A combination of the first cathode active material compound LiaAbMn1-cBcP1-dRdO4-nDn and the second cathode active material compound LixNiyCozMkMepOrEm is used. By using these materials in the upper and lower film layers of the cathode plate respectively, the lithium ion conduction rate and cycle life are improved, and enhanced Low temperature power and fast charging performance of the battery.

Benefits of technology

It significantly improves the battery's low-temperature power and low-temperature rate performance, extends the battery life under low-temperature conditions, improves the battery's fast-charging performance and cycle life, and at the same time enhances the safety of the positive electrode piece.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023091177_31102024_PF_FP_ABST
    Figure CN2023091177_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a positive electrode sheet, a battery, and an electric device. The positive electrode sheet of the present application comprises a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a first positive electrode film layer provided on the surface of the positive electrode current collector and a second positive electrode film layer provided on the surface of the first positive electrode film layer. The first positive electrode film layer comprises a first positive electrode active material, and the second positive electrode film layer comprises a second positive electrode active material; and the first positive electrode active material comprises compound LiaAbMn1-cBcP1-dRdO4-nDn, and the second positive electrode active material comprises compound LixNiyCozMkMepOrEm.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode sheet, battery and power-using device Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode sheet, a battery, and an electrical device. Background Art

[0002] In recent years, the application of secondary batteries has become increasingly widespread. They are widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As secondary batteries have achieved significant development, higher requirements have been placed on their rate performance, power, fast charging performance, and cycle performance.

[0003] Summary of the Invention

[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide a positive electrode plate, a battery and an electrical device. The positive electrode plate of the present application improves the low-temperature power, low-temperature rate performance, fast charging performance and cycle life of the battery.

[0005] To achieve the above-mentioned object, the present application provides a positive electrode sheet in a first aspect, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a first positive electrode film layer disposed on the surface of the positive electrode current collector and a second positive electrode film layer disposed on the surface of the first positive electrode film layer; the first positive electrode film layer comprises a first positive electrode active material, and the second positive electrode film layer comprises a second positive electrode active material;

[0006] The first positive electrode active material comprises a compound Li a A b Mn 1-c B c P 1-d R d O 4-n D n ,in,

[0007] The A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W;

[0008] The B includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge;

[0009] R includes one or more elements selected from B, Si, N, S, F, Cl and Br;

[0010] Said D comprises one or more elements selected from S, F, Cl and Br;

[0011] a is 0.9 to 1.1, and may be 0.977 to 1; b is 0 to 0.1, and may be 0 to 0.001; c is 0.001 to 0.9, and may be 0.1 to 0.9 or 0.001 to 0.6; d is 0 to 0.1, and may be 0 to 0.001 or 0.001 to 0.1; n is 0 to 0.1, and may be 0 to 0.001 or 0.001 to 0.1;

[0012] The second positive electrode active material comprises a compound Li x Ni y Co z M k Me p O r E m ; wherein, the M includes one or two elements of Mn and Al; the Me includes one or more elements of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W and Nb; the E includes one or more elements of N, F, S and Cl; 0.85≤x≤1.15; 0<y≤1; 0≤z<1; 0<k<1; 0≤p≤0.1; 1≤r≤2, 0≤m≤1, and m+r≤2.

[0013] The present application combines the first positive electrode active material with the second positive electrode active material, thereby improving the low-temperature power and low-temperature rate performance (low-temperature discharge capacity retention rate) of the battery and extending the battery life under low-temperature conditions; and, including the second positive electrode active material and the first positive electrode active material in the upper and lower adjacent second and first positive electrode film layers, respectively, is beneficial to improving the lithium ion conduction rate of the positive electrode sheet, thereby improving the fast charging performance of the battery and improving the cycle life of the battery.

[0014] In any embodiment, the B comprises one or more elements selected from the group consisting of Fe, Ti, V, Ni, Co, and Mg; and / or

[0015] The R includes any one of B, Si, N, and S elements.

[0016] In any embodiment, the mass ratio of the first positive electrode active material to the second positive electrode active material is 5%-90%, and optionally 10%-50%. This helps to leverage the combined advantages of the first and second positive electrode active materials, further improving the battery's low-temperature power and low-temperature rate performance, and further improving the battery's fast charging performance and cycle life.

[0017] In any embodiment, the lithium ion diffusion coefficient of the second positive electrode active material is greater than the lithium ion diffusion coefficient of the first positive electrode active material, thereby increasing the lithium ion conduction rate of the positive electrode sheet and thus improving the fast charging performance of the battery.

[0018] In any embodiment, the compaction density of the second positive electrode active material under 3 tons of pressure is greater than the compaction density of the first positive electrode active material under 3 tons of pressure. This facilitates stable bonding between the first and second positive electrode film layers, reduces the resistance of the positive electrode sheet, and facilitates processing of the positive electrode sheet.

[0019] In any embodiment, the second positive electrode active material is a single crystal or quasi-single crystal material; and / or the Dv10 particle size of the positive electrode active material is 0.3-2.5 μm, optionally 0.5-1.5 μm. This makes the positive electrode plate easier to process, reducing problems such as cold pressing roller sticking and plate cracking and demolding.

[0020] In any embodiment, the lithium ion diffusion coefficient of the first positive electrode active material at 25° C. is 10 -16 -10 -12 cm 2 ·s -1 , which can be 10 -15 -10 -13 cm 2 ·s -1 and / or,

[0021] The powder resistivity of the first positive electrode active material at 20 MPa is 2000-10000 Ω·cm, and can be optionally 3000-6000 Ω·cm; and / or,

[0022] The compaction density of the first positive electrode active material under a pressure of 3 tons is 1.9-3.1 g / cm 3 , optional 2.2-2.9g / cm 3 .

[0023] In any embodiment, the lithium ion solid phase diffusion coefficient of the second positive electrode active material at 25° C. is 10 -12 -10 -8 cm 2 ·s -1 , which can be 10 -11 -10 -9 cm 2 ·s -1 and / or,

[0024] The powder resistivity of the second positive electrode active material at 20 MPa is 100-700 Ω·cm, optionally 200-550 Ω·cm; and / or,

[0025] The compaction density of the second positive electrode active material under a pressure of 3 tons is 3-4.2 g / cm3, and can be optionally 3.6-3.75 g / cm3.

[0026] The lithium ion diffusion coefficients of the first positive electrode active material and the second positive electrode active material are within the above range and the lithium ion diffusion coefficient of the second positive electrode active material is greater than the lithium ion diffusion coefficient of the first positive electrode active material, which is beneficial to improving the lithium ion conduction rate of the positive electrode sheet, thereby improving the fast charging performance of the battery; in addition, when the positive electrode sheet breaks due to accidental fracture, the first positive electrode active material is closer to the positive electrode current collector, and heat will be transferred to the first positive electrode active material first. The lithium ion diffusion coefficient of the first positive electrode active material is lower, and accordingly its high temperature stability is better, which can delay the transfer of heat to the second positive electrode active material, thereby improving the overall safety of the battery.

[0027] The powder resistivity of the first positive electrode active material and the second positive electrode active material is within the above range and the powder resistivity of the first positive electrode active material is greater than the powder resistivity of the second positive electrode active material, which is beneficial to improving the lithium ion conduction rate of the positive electrode sheet, thereby improving the fast charging performance of the battery.

[0028] The compaction density of the first positive electrode active material and the second positive electrode active material is within the above range and the compaction density of the second positive electrode active material is greater than the compaction density of the first positive electrode active material; on the one hand, it is beneficial to reduce the ductility of the first positive electrode active material, so as to alleviate the rupture of the current collector caused by the inconsistent ductility between the positive electrode active material and the positive electrode collector, thereby improving the safety and reliability of the positive electrode sheet; on the other hand, during the cold pressing process, the second positive electrode active material contacts the cold pressing roller and has a higher compaction density, and it is not easy for material particles to break.

[0029] In any embodiment, the thickness ratio of the first positive electrode film layer to the second positive electrode film layer is 0.08-1.53, optionally 0.1-1.2, and more optionally 0.15-0.93; and / or,

[0030] The thickness of the positive electrode film layer is 60-300 μm.

[0031] This is beneficial to giving full play to the combined advantages of the first positive electrode active material and the second positive electrode active material, further improving the low-temperature power and low-temperature rate performance of the battery, and further improving the fast charging performance and cycle life of the battery.

[0032] In any embodiment, the power capability m of the positive electrode plate is calculated according to the following formula, and m is 2.93-87.62, optionally 3-13, and more optionally 3.81-12.67;

[0033] in,

[0034] PD A represents the compaction density of the first positive electrode active material under a pressure of 3 tons, in g / cm 3 ;

[0035] C A represents the lithium ion diffusion coefficient of the first positive electrode active material at 25°C, in cm 2 ·s -1 ;

[0036] N A represents the powder resistivity of the first positive electrode active material at 20 MPa, in Ω·cm;

[0037] PD B represents the compaction density of the second positive electrode active material under 3 tons of pressure, in g / cm 3 ;

[0038] C B represents the lithium ion diffusion coefficient of the second positive electrode active material at 25°C, in cm 2 ·s -1 ;

[0039] N B represents the powder resistivity of the second positive electrode active material at 20 MPa, in Ω·cm.

[0040] M represents the mass ratio of the first positive electrode active material to the second positive electrode active material.

[0041] Therefore, the power capability m parameter of the positive electrode sheet helps to quantify the differences when different first positive electrode active materials are combined with second positive electrode active materials, and to compare and distinguish the overall power capability of the positive electrode substrate. The power capability of the positive electrode sheet within the above range is beneficial to improving the low-temperature power and low-temperature rate capability of the battery, and improving the fast charging performance and cycle life of the battery.

[0042] In any embodiment, the first positive electrode active material includes a core and a coating layer covering the core, and the core includes the compound Li a A b Mn 1-c B c P 1-d R d O 4-n D n , the coating layer includes one or more of pyrophosphate, phosphate and carbon.

[0043] Therefore, the coating layer in the first positive electrode active material is beneficial to improving the electrical conductivity of the material and increasing the lithium ion conduction rate of the material.

[0044] In any embodiment, the second positive electrode active material includes a core and a coating layer covering the core, and the core includes the compound Li x Ni y Co z M k Me p O r E m The coating layer includes one or more elements of Al, Ba, Zn, Ti, Co, W, Y, Si, Sn, B and P.

[0045] Therefore, the coating layer in the second positive electrode active material is beneficial to suppressing the disproportionation reaction and improving the cycle performance and low-temperature rate performance of the material.

[0046] The second aspect of the present application provides a battery, comprising the positive electrode sheet of the first aspect of the present application.

[0047] In this application, batteries include but are not limited to secondary batteries, battery packs, battery modules, etc.

[0048] The third aspect of the present application provides an electrical device, comprising the positive electrode sheet of the first aspect of the present application or the battery of the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application.

[0050] FIG. 2 is an exploded view of the secondary battery according to the embodiment of the present application shown in FIG. 1 .

[0051] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application.

[0052] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application.

[0053] FIG. 5 is an exploded view of the battery pack shown in FIG. 4 according to an embodiment of the present application.

[0054] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0055] Explanation of reference numerals: 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 housing; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION

[0056] Below, the embodiments of the positive electrode sheet, secondary battery, battery module, battery pack and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0057] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0058] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0059] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0060] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a method includes steps (a) and (b), which indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a method may further include step (c), which indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.

[0061] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may indicate that other components not listed may also be included or that only the listed components are included.

[0062] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0063] Unless otherwise specified, in the present application, the term "single crystal / quasi-single crystal particle" means a single particle (ie, a primary particle).

[0064] If not otherwise specified, in this application, the terms "secondary particles" and "polycrystalline material particles" generally have similar meanings, which refer to particles formed by the agglomeration of more than 100 primary particles with an average particle size in the range of 50-800 nm.

[0065] Unless otherwise specified, in the present application, the term "Dv10 particle size" refers to a particle size at which the cumulative volume reaches 10% from the smallest particle size side in a volume-based particle size distribution.

[0066] [Secondary battery]

[0067] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged to activate the active materials after discharge and continue to be used.

[0068] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. During the battery's charge and discharge process, active ions (such as lithium ions) are embedded and released back and forth between the positive and negative electrode sheets. The separator is set between the positive and negative electrode sheets, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte between the positive and negative electrode sheets mainly plays the role of conducting active ions.

[0069] [Positive electrode]

[0070] One embodiment of the present application provides a positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a first positive electrode film layer disposed on the surface of the positive electrode current collector and a second positive electrode film layer disposed on the surface of the first positive electrode film layer; the first positive electrode film layer comprises a first positive electrode active material, and the second positive electrode film layer comprises a second positive electrode active material;

[0071] The first positive electrode active material comprises a compound Li a A b Mn 1-c B c P 1-d R d O 4-n D n ,in,

[0072] The A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W;

[0073] The B includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge;

[0074] R includes one or more elements selected from B, Si, N, S, F, Cl and Br;

[0075] Said D comprises one or more elements selected from S, F, Cl and Br;

[0076] The a is 0.9 to 1.1, and can be selected from 0.977 to 1, such as 0.95, 0.97, 1, 1.05, 1.1, and the range consisting of any of the above values; the b is 0 to 0.1, and can be selected from 0 to 0.001, such as 0, 0.001, 0.003, 0.005, 0.008, 0.1, and the range consisting of any of the above values; the c is 0.001 to 0.9, and can be selected from 0.1 to 0.9 or 0.001 to 0.6, such as 0.005, 0.01, 0.0 5, 0.1, 0.2, 0.3, 0.5, 0.7, 0.8, 0.9 and the range consisting of any of the above values; the d is 0 to 0.1, and can be selected from 0 to 0.001 or 0.001 to 0.1, for example, 0, 0.01, 0.05, 0.07, 0.1 and the range consisting of any of the above values; the n is 0 to 0.1, and can be selected from 0 to 0.001 or 0.001 to 0.1, for example, 0, 0.01, 0.05, 0.07, 0.1 and the range consisting of any of the above values;

[0077] The second positive electrode active material comprises a compound Li x Ni yCo z M k Me p O r E m ; Wherein, the M includes one or two elements of Mn and Al; the Me includes one or more elements of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W and Nb; the E includes one or more elements of N, F, S and Cl; 0.85≤x≤1.15, for example, x is 0.9, 0.95, 1, 1.05, 1.1, 1.15 and the range consisting of any of the above values; 0<y≤1, for example, y is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 and the range consisting of any of the above values; 0≤z<1, for example, z is 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99, and any range consisting of the above values; 0<k<1, for example, k is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99, and any range consisting of the above values; 0≤p≤0.1, for example, p is 0, 0.01, 0.02, 0.03, 0.05, 0.07, 0.08, 0.09, 0.1, and any range consisting of the above values; 1≤r≤2, for example, r is 1, 1.1, 1.3, 1.5, 1.7, 1.8, 2, and any range consisting of the above values, 0≤m≤1, for example, m is 0, 0.1, 0.2, 0.5, 0.7, 0.8, 1, and any range consisting of the above values, and m+r≤2, can be optionally equal to 2.

[0078] Existing lithium iron phosphate positive electrode active materials have poor low-temperature rate performance and poor conductivity, poor capacity utilization under low-temperature conditions, and short battery life; existing ternary positive electrode active materials have low low-temperature power and are prone to undervoltage when using large current discharge under low-temperature conditions.

[0079] Although the mechanism is still unclear, the applicant unexpectedly discovered that the present application combines the first positive electrode active material with the second positive electrode active material, which improves the low-temperature power and low-temperature rate performance of the battery and extends the battery life under low-temperature conditions. In addition, including the second positive electrode active material and the first positive electrode active material in the upper and lower adjacent second and first positive electrode film layers, respectively, is beneficial to improving the lithium ion conduction rate of the positive electrode sheet, thereby improving the fast charging performance of the battery and improving the cycle life of the battery.

[0080] In some embodiments, the B comprises one or more elements selected from the group consisting of Fe, Ti, V, Ni, Co, and Mg; and / or,

[0081] The R includes any one of B, Si, N, and S elements.

[0082] In some embodiments, the mass ratio of the first positive electrode active material to the second positive electrode active material is 5%-90%, optionally 10%-50%, for example, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, and any range thereof. This is beneficial for leveraging the combined advantages of the first positive electrode active material and the second positive electrode active material, further improving the low-temperature power and low-temperature rate performance of the battery, and further improving the fast charging performance and cycle life of the battery.

[0083] In some embodiments, the lithium ion diffusion coefficient of the second positive electrode active material is greater than the lithium ion diffusion coefficient of the first positive electrode active material, thereby increasing the lithium ion conduction rate of the positive electrode sheet and thus improving the fast charging performance of the battery.

[0084] In some embodiments, the compaction density of the second positive electrode active material under a pressure of 3 tons is greater than the compaction density of the first positive electrode active material under a pressure of 3 tons. This facilitates stable bonding between the first positive electrode film layer and the second positive electrode film layer, reduces the resistance of the positive electrode sheet, and facilitates processing of the positive electrode sheet.

[0085] In some embodiments, the second cathode active material is a single crystal or quasi-single crystal material; and / or,

[0086] The Dv10 particle size of the second positive electrode active material is 0.3-2.5 μm, and can be optionally 0.5-1.5 μm, for example, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 1 μm, 1.2 μm, 1.3 μm, 1.5 μm, 1.7 μm, 1.9 μm, 2 μm, 2.3 μm, 2.5 μm and the range consisting of any of the above values.

[0087] As a result, the positive electrode plates are easier to process, reducing problems such as cold pressing sticking to the rollers and cracking and demolding of the plates.

[0088] In some embodiments, the crystal type can be tested by scanning electron microscopy. For example, if the number and average particle size of the primary particles in 50% or more (including 50%) of the collected agglomerated particles meet the above definition of "polycrystalline material particles", then the positive electrode active material is a polycrystalline material; otherwise, it is a single crystal or a quasi-single crystal material.

[0089] In some embodiments, the particle size Dv10 is measured using conventional methods in the art, for example, a laser particle size analyzer (Malvern Mastersizer 2000E) can be used for measurement, the solvent used for the measurement is water, and ultrasound is used for dispersion.

[0090] In some embodiments, the lithium ion diffusion coefficient of the first positive electrode active material at 25° C. is 10 -16 -10 -12 cm 2 ·s -1 , which can be 10 -15 -10 -13 cm 2 ·s -1 , for example 10 -16 cm 2 ·s -1 , 10 -15 cm 2 ·s -1 , 10 -14 cm 2 ·s -1 , 10 -13 cm 2 ·s -1 , 10 -12 cm 2 ·s -1 and any range of the above values; and / or,

[0091] The powder resistivity of the first positive electrode active material at 20 MPa is 2000-10000 Ω·cm, optionally 3000-6000 Ω·cm, for example, 2000 Ω·cm, 3000 Ω·cm, 4000 Ω·cm, 5000 Ω·cm, 6000 Ω·cm, 7000 Ω·cm, 8000 Ω·cm, 9000 Ω·cm, 10000 Ω·cm, or any range consisting of the above values; and / or,

[0092] The compaction density of the first positive electrode active material under a pressure of 3 tons is 1.9-3.1 g / cm 3 , optional 2.2-2.9g / cm 3 , for example 1.9 g / cm 3 , 2g / cm 3 , 2.1g / cm 3 , 2.2g / cm 3 , 2.3g / cm 3 , 2.5g / cm 3 , 2.6g / cm 3 , 2.7g / cm 3 , 2.8g / cm 3 , 2.9g / cm 3 , 3.0g / cm 3 , 3.1g / cm 3 and ranges consisting of any of the above numerical values.

[0093] In some embodiments, the lithium ion diffusion coefficient of the second positive electrode active material at 25° C. is 10 -12 -10 -8 cm 2 ·s -1 , which can be 10 -11 -10 -9 cm 2 ·s -1 , for example, 10 -12 cm 2 ·s -1 , 10 -11 cm 2 ·s -1 , 10 -10 cm 2 ·s -1 , 10 -9 cm 2 ·s -1 , 10 -8 cm 2 ·s -1 and any range of the above values; and / or,

[0094] The powder resistivity of the second positive electrode active material at 20 MPa is 100-700 Ω·cm, optionally 200-550 Ω·cm, for example, 100 Ω·cm, 200 Ω·cm, 300 Ω·cm, 400 Ω·cm, 500 Ω·cm, 600 Ω·cm, 700 Ω·cm, and any range consisting of the above values; and / or,

[0095] The compaction density of the second positive electrode active material under a pressure of 3 tons is 3-4.2 g / cm 3 , optional 3.6-3.75g / cm 3 , for example 3g / cm 3 , 3.1g / cm 3 , 3.3g / cm 3 , 3.5g / cm 3 、3.6g / cm 3 、3.8g / cm 3 、3.9g / cm 3 , 4.0g / cm 3 , 4.1g / cm 3 , 4.2g / cm 3 and ranges consisting of any of the above numerical values.

[0096] The lithium ion diffusion coefficients of the first positive electrode active material and the second positive electrode active material are within the above range and the lithium ion diffusion coefficient of the second positive electrode active material is greater than the lithium ion diffusion coefficient of the first positive electrode active material, which is beneficial to improving the lithium ion conduction rate of the positive electrode sheet, thereby improving the fast charging performance of the battery; in addition, when the positive electrode sheet breaks due to accidental fracture, the first positive electrode active material is closer to the positive electrode current collector, and heat will be transferred to the first positive electrode active material first. The lithium ion diffusion coefficient of the first positive electrode active material is lower, and accordingly its high temperature stability is better, which can delay the transfer of heat to the second positive electrode active material, thereby improving the overall safety of the battery.

[0097] The powder resistivity of the first positive electrode active material and the second positive electrode active material is within the above range and the powder resistivity of the first positive electrode active material is greater than the powder resistivity of the second positive electrode active material, which is beneficial to improving the lithium ion conduction rate of the positive electrode sheet, thereby improving the fast charging performance of the battery.

[0098] The compaction density of the first positive electrode active material and the second positive electrode active material is within the above range and the compaction density of the second positive electrode active material is greater than the compaction density of the first positive electrode active material; on the one hand, it is beneficial to reduce the ductility of the first positive electrode active material, so as to alleviate the rupture of the current collector caused by the inconsistent ductility between the positive electrode active material and the positive electrode collector, thereby improving the safety and reliability of the positive electrode sheet; on the other hand, during the cold pressing process, the second positive electrode active material contacts the cold pressing roller and has a higher compaction density, and it is not easy for material particles to break.

[0099] In some embodiments, the lithium ion diffusion coefficient is measured using conventional methods in the art, such as the methods described in “Xie et al., Solid State Ionics, 2007, 178: 1218–1224; Yang et al., Electrochimica Acta, 2012, 66: 88–93”.

[0100] In some embodiments, the powder resistivity is tested using conventional methods in the art. For example, a suitable amount of powder can be placed in a sample chamber of a powder resistivity tester with a depth of 20 mm and a cross-sectional area of ​​1 cm. 2 , then apply pressure to 20 MPa and record the powder resistivity test results at 20 MPa.

[0101] In some embodiments, the compaction density under 3 tons of pressure is tested using conventional methods in the art. For example, a powder of the material to be tested with a density of ω (g) can be placed in a mold of an electronic pressure testing machine with a bottom area of ​​α (cm 2) Adjust the pressure to 3 tons, maintain the pressure for 30 seconds, read the height h (cm) of the resulting powder block, and calculate the compaction density PD of the material under 3 tons of pressure according to the following formula: PD = ω / (α×h).

[0102] In some embodiments, the thickness ratio of the first positive electrode film layer to the second positive electrode film layer is 0.08-1.53, optionally 0.1-1.2, and more optionally 0.15-0.93, for example, 0.08, 0.1, 0.12, 0.3, 0.5, 0.6, 0.7, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, and the range consisting of any of the above values; and / or,

[0103] The thickness of the positive electrode film layer is 60-300 μm, for example, 70 μm, 80 μm, 100 μm, 120 μm, 150 μm, 170 μm, 200 μm, 220 μm, 250 μm, 270 μm, 290 μm, 300 μm and any range consisting of the above values.

[0104] This is beneficial to giving full play to the combined advantages of the first positive electrode active material and the second positive electrode active material, further improving the low-temperature power and low-temperature rate performance of the battery, and further improving the fast charging performance and cycle life of the battery.

[0105] In some embodiments, the thickness of the positive electrode film layer is tested using conventional methods in the art, for example, using a micrometer.

[0106] In some embodiments, the power capability m of the positive electrode sheet is calculated according to the following formula, and m is 2.93-87.62, optionally 3-13, more optionally 3.81-12.67, for example, 2.93, 3, 5, 8, 10, 11, 12, 13, 14, 15, 16, 17, 20, 25, 30, 35, 40, 50, 60, 70, 75, 80, 85, 87, 87.62 and the range of any of the above values;

[0107] in,

[0108] PD A represents the compaction density of the first positive electrode active material under a pressure of 3 tons, in g / cm 3 ;

[0109] C A represents the lithium ion diffusion coefficient of the first positive electrode active material at 25°C, in cm 2 ·s -1 ;

[0110] N Arepresents the powder resistivity of the first positive electrode active material at 20 MPa, in Ω·cm;

[0111] PD B represents the compaction density of the second positive electrode active material under 3 tons of pressure, in g / cm 3 ;

[0112] C B represents the lithium ion diffusion coefficient of the second positive electrode active material at 25°C, in cm 2 ·s -1 ;

[0113] N B represents the powder resistivity of the second positive electrode active material at 20 MPa, in Ω·cm.

[0114] M represents the mass ratio of the first positive electrode active material to the second positive electrode active material.

[0115] Therefore, the power capability m parameter of the positive electrode sheet helps to quantify the differences when different first positive electrode active materials are combined with second positive electrode active materials, and to compare and distinguish the overall power capability of the positive electrode substrate. The power capability of the positive electrode sheet within the above range is beneficial to improving the low-temperature power and low-temperature rate capability of the battery, and improving the fast charging performance of the battery.

[0116] In some embodiments, the first positive electrode active material includes a core and a coating layer coating the core, wherein the core includes the compound Li a A b Mn 1-c B c P 1-d R d O 4-n D n , the coating layer includes one or more of pyrophosphate, phosphate and carbon.

[0117] Therefore, the coating layer in the first positive electrode active material is beneficial to improving the electrical conductivity of the material and increasing the lithium ion conduction rate of the material.

[0118] In some embodiments, the second positive electrode active material includes a core and a coating layer coating the core, wherein the core includes the compound Li x Ni y Co z M k Me p O r E m The coating layer includes one or more elements of Al, Ba, Zn, Ti, Co, W, Y, Si, Sn, B and P.

[0119] Therefore, the coating layer in the second positive electrode active material is beneficial to suppressing the disproportionation reaction and improving the cycle performance and low-temperature rate performance of the material.

[0120] In some embodiments, the method for preparing the first positive electrode active material of the present application comprises the following steps:

[0121] (1) dissolving a manganese source, a source of element B, and an acid in a solvent and stirring to generate a suspension of a manganese salt doped with element B, filtering the suspension and drying the filter cake to obtain a manganese salt doped with element B;

[0122] (2) adding a lithium source, a phosphorus source, a source of element A, a source of element R, a source of element D, a solvent, and the manganese salt doped with element B obtained in step (1) into a reaction container, grinding and mixing to obtain a slurry;

[0123] (3) transferring the slurry obtained in step (2) to a spray drying device for spray drying and granulation to obtain granules;

[0124] (4) Sintering the particles obtained in step (3).

[0125] In some embodiments, the source of element A is selected from at least one of a simple substance, oxide, phosphate, oxalate, carbonate, and sulfate of element A; the source of element B is selected from at least one of a simple substance, oxide, phosphate, oxalate, carbonate, and sulfate of element B; the source of element R is selected from at least one of a sulfate, borate, nitrate, and silicate of element R; and the source of element D is selected from at least one of a simple substance and an ammonium salt of element D. By selecting the source of each doping element, the uniformity of the distribution of the doping element can be improved, thereby improving the performance of the material.

[0126] In some embodiments, the acid is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and organic acids such as oxalic acid, for example, oxalic acid. In some embodiments, the acid is a dilute acid with a concentration of 60% by weight or less.

[0127] In some embodiments, the manganese source may be a manganese-containing substance known in the art that can be used to prepare lithium manganese phosphate. For example, the manganese source may be selected from elemental manganese, manganese dioxide, manganese phosphate, manganese oxalate, manganese carbonate, or a combination thereof.

[0128] In some embodiments, the lithium source may be a lithium-containing material known in the art that can be used to prepare lithium manganese phosphate. For example, the lithium source may be selected from lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, or a combination thereof.

[0129] In some embodiments, the phosphorus source may be a phosphorus-containing substance known in the art that can be used to prepare lithium manganese phosphate. For example, the phosphorus source may be selected from diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, and phosphoric acid, or a combination thereof.

[0130] The amount of each source of elements A, B, R, and D added depends on the target doping amount, and the ratio of the amount of lithium source, manganese source, and phosphorus source used conforms to the stoichiometric ratio.

[0131] In some embodiments, the solvents in step (1) and step (2) can each independently be a solvent conventionally used by those skilled in the art in the preparation of manganese salts and lithium manganese phosphate, for example, they can each independently be selected from at least one of ethanol and water (e.g., deionized water).

[0132] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0133] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0134] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0135] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0136] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0137] [Negative electrode]

[0138] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0139] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0140] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0141] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0142] In some embodiments, the negative electrode film layer may further include a binder. For example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0143] In some embodiments, the negative electrode film layer may further include a conductive agent. For example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0144] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0145] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0146] [Electrolytes]

[0147] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0148] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.

[0149] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0150] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0151] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0152] [Isolation film]

[0153] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0154] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0155] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0156] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0157] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0158] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.

[0159] In some embodiments, referring to FIG2 , the outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0160] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0161] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0162] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0163] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0164] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0165] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0166] As an electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0167] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0168] [Example]

[0169] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0170] Example 1

[0171] (1) First positive electrode active material: LiMn 0.4 Fe 0.6 PO4.

[0172] (2) Second positive electrode active material: LiNi 0.55 Co 0.1 Mn0.35 O2.

[0173] (3) Preparation of positive electrode sheet:

[0174] The first positive electrode active material, the binder polyvinylidene fluoride (PVDF), and the conductive agent acetylene black are dissolved in the solvent N-methylpyrrolidone (NMP) in a mass ratio of 90:5:5, and the mixture is fully stirred and evenly mixed to prepare a first positive electrode slurry; the second positive electrode active material, the binder polyvinylidene fluoride (PVDF), and the conductive agent acetylene black are dissolved in the solvent N-methylpyrrolidone (NMP) in a mass ratio of 90:5:5, and the mixture is fully stirred and evenly mixed to prepare a second positive electrode slurry; the first positive electrode slurry is evenly coated on the positive electrode collector aluminum foil, and after drying, a positive electrode collector coated with the first positive electrode film layer is obtained, and then the second positive electrode slurry is evenly coated on the surface of the first positive electrode film layer, and then dried, cold pressed, and cut to obtain a positive electrode sheet.

[0175] (4) Preparation of negative electrode sheets: artificial graphite, a conductive agent, acetylene black, a binder, styrene-butadiene rubber (SBR), and a thickener, sodium carboxymethyl cellulose (CMC-Na), are dissolved in deionized water at a mass ratio of 95:2:1:2, and the mixture is stirred thoroughly to prepare a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector copper foil, and then dried, cold pressed, and cut to obtain a negative electrode sheet.

[0176] (5) Isolation film: PE film is used as the isolation film.

[0177] (6) Preparation of electrolyte: Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1, and LiPF6 was uniformly dissolved in the above solution to obtain an electrolyte. The concentration of LiPF6 in the electrolyte was 1 mol / L.

[0178] (7) Preparation of secondary batteries: The positive electrode sheets, separators, and negative electrode sheets are stacked and wound in order to obtain a battery cell; the battery cell is placed in an outer package, and the electrolyte prepared above is added. After packaging, standing, formation, aging, and other processes, a secondary battery is obtained.

[0179] The secondary battery preparation methods of Examples 2-36 and Comparative Examples are similar to those of Example 1, but the parameters are adjusted. The different parameters are detailed in Table 1.

[0180] LiMn used in Examples 1-5, 12-23, and 30-35 of this application 0.4 Fe 0.6 PO4 was purchased from Defang Nano with the product number LMFP-D2.

[0181] LiMn used in Examples 6-11 of this application0.4 Fe 0.6 PO4 was purchased from Defang Nanotechnology with product numbers LMFP-D1, LMFP-D3, LMFP-D4, LMFP-D5, LMFP-D6, and LMFP-D7.

[0182] LiMn used in Examples 24-29 and 36 of this application 0.4 Fe 0.6 PO4 was purchased from Defang Nanotechnology with product numbers LMFP-D8, LMFP-D9, LMFP-D10, LMFP-D11, LMFP-D12, LMFP-D13, and LMFP-D14.

[0183] LiNi used in Examples 1-3, 6-11, 21-22, and 24-29 of this application 0.55 Co 0.1 Mn 0.35 O2 was purchased from Rongbai Technology, item number N1.

[0184] LiNi used in Examples 4-5, 12-16 of this application 0.55 Co 0.1 Mn 0.35 O2 was purchased from Rongbai Technology, with product numbers N2-N8.

[0185] LiNi used in Examples 17 and 36 of this application 0.55 Co 0.1 Mn 0.35 O2 was purchased from Rongbai Technology, the product number is N9.

[0186] LiNi used in Example 18 of this application 0.34 Co 0.33 Mn 0.33 O2 was purchased from Rongbai Technology, the product number is N17.

[0187] LiNi used in Example 19 of this application 0.83 Co 0.07 Mn 0.1 O2 was purchased from Rongbai Technology, item number N18.

[0188] LiNi used in Example 20 of this application 0.9 Mn 0.1 O2 was purchased from Rongbai Technology, item number N19.

[0189] LiNi used in Example 23 of this application 0.55 Co 0.1 Mn 0.35 O2 was purchased from Rongbai Technology, the product number is N10.

[0190] LiNi used in Examples 30-35 of this application 0.55 Co 0.1 Mn 0.35 O2 was purchased from Rongbai Technology, with product numbers N11-N16.

[0191] Test Case

[0192] (1) Test of lithium ion diffusion coefficient of positive electrode active material:

[0193] The conventional methods in this field such as the CV method, EIS method, GITT method, and PITT method can be used for testing, and the results can be calculated based on Fick's first and second laws.

[0194] Taking the GITT method as an example, the steps for testing the lithium ion diffusion coefficient of the first positive electrode active material or the second positive electrode active material are as follows:

[0195] The first cathode active material or the second cathode active material was ground into a powder microelectrode; the powder microelectrode was connected to an electrochemical workstation and coulometric titration was performed. A pulse current of 20 μA was used, the titration time was 1 hour, the rest time was 4 hours, and the test temperature was 25°C (Note: To compare the effects of pulse current and time, a parallel experiment of 10 μA and 10 minutes can be performed). After obtaining the GITT curve, the lithium ion diffusion coefficient was calculated using the following formula:

[0196] Where D is the lithium ion diffusion coefficient; I0 ​​is the pulse current used, 20 μA; Vm is the molar volume of the positive electrode active material; F is the Faraday constant; A is the electrode surface area; n is the charge number of the lithium ion, where n is 1; dE / dx is the slope of the coulometric titration curve, which is the slope of the open circuit potential versus the lithium concentration at a certain concentration; and (dE) / (dt1 / 2) is the slope of the polarization voltage versus t1 / 2 curve. For more information, please refer to: Xie et al., Solid State Ionics, 2007, 178:1218–1224; Yang et al., Electrochimica Acta, 2012, 66:88–93.

[0197] (2) Test of compaction density of positive electrode active material:

[0198] Weigh 2.0g of positive electrode active material powder and place it in the mold of the UTM7305 electronic pressure testing machine. Adjust the pressure to 3 tons. After maintaining the pressure for 30 seconds, read the height of the positive electrode active material powder block. Calculate the compaction density (PD) of the positive electrode active material under 3 tons of pressure using the following formula: PD = ω / (α×h)

[0199] Where ω is the mass of the positive electrode active material powder (g); α is the bottom area of ​​the mold (cm 2 ); h is the height of the positive electrode active material powder block (cm).

[0200] (3) Test of the powder resistivity of the positive electrode active material:

[0201] The powder of the positive electrode active material was dried and an appropriate amount of powder was weighed and placed in the sample chamber of a powder resistivity tester (Suzhou Jingge, model ST2722). The sample chamber had a depth of 20 mm and a cross-sectional area of ​​1 cm. 2 , then slowly apply pressure from small to large until it reaches 20MPa, and record the powder resistivity test results at 20MPa.

[0202] (4) Crystal type test:

[0203] The positive electrode active material is tested using a scanning electron microscope. The sample and magnification are adjusted so that there are more than 10 agglomerated particles in the field of view. The number of primary particles making up each agglomerated particle is measured, and the length dimension of the primary particles is measured with a ruler and recorded as the particle size. The particle size of the primary particles in each agglomerated particle is sorted from large to small. The 1 / 10th of the largest particle size data and the 1 / 10th of the smallest particle size data are removed, and the average of the remaining particle size data is taken as the average particle size of the primary particles in the agglomerated particle. If the number and average particle size of the primary particles in more than 50% (including 50%) of the agglomerated particles meet the definition of "polycrystalline material particles", the positive electrode active material is determined to be a polycrystalline material; otherwise, it is determined to be a single crystal material.

[0204] (5) Dv10 particle size test:

[0205] The test was conducted using a laser particle size analyzer (Malvern Mastersizer 2000E), the solvent used in the test was water, and ultrasound was used for dispersion.

[0206] (6) Test of the thickness of the positive electrode film:

[0207] The thickness of the positive electrode film layer was measured using a micrometer (Mitutoyo MDH-25MB).

[0208] (7) Low temperature power test:

[0209] Refer to the methods in GB / T 19596 and GB / T 31486, use a battery charger and discharge machine + high and low temperature box to test the power of the battery at 253K and 5% SOC.

[0210] (8) Fast charging time test:

[0211] In a constant temperature environment of 25 °C, charge the soft-pack laminated battery at different rates (C1 < C2 < C3 < C4 < …… < Cn). During the test, the charging rate increases from small to large. During the charging process, it is necessary to simultaneously monitor the full battery voltage and the negative electrode voltage of the soft-pack laminated battery. The specific process is as follows: Charge the soft-pack laminated battery at C1 until the full charge voltage of 4.4 V or the negative electrode voltage reaches 0 V, obtain the SOC value of the battery at the end of charging, and then discharge it at 0.33C until the full discharge voltage of 2.5 V; repeat the above process according to the charging rate increasing from small to large, and the SOC values at the end of charging at different rates can be obtained. Fit the SOC values at the end of charging with the corresponding rate values to obtain the relationship between the SOC and the rate value at the end of charging. Substitute 100% SOC into the relationship to obtain the corresponding Ci. The time consumed for constant current and constant voltage charging to the cut-off voltage at Ci as the charging rate is the fast charging time.

[0212] (9) Test of cycle performance:

[0213] Charge the battery in a constant temperature environment of 25 °C from 2.5 V to 4.25 - 4.3 V at 0.5C, then charge it at a constant voltage of 4.25 - 4.3 V until the current ≤ 0.05 mA, let it stand for 5 minutes, and then discharge it at 0.5C to 2.5 V. Record the discharge capacity of the first cycle of the battery as D1; repeat the above operation, and record the discharge capacity of each cycle as D n (n = 2, 3 ……); Calculate the attenuation degree (State of health SOH) of the battery cell according to the following formula, and record the number of cycles n when the attenuation degree reaches 80% SOH; The attenuation degree of the battery cell = 100% × D n / D3.

[0214] (10) Test of low-temperature discharge capacity retention rate:

[0215] In a constant temperature environment of 25 °C, let the battery stand for 30 minutes, discharge it at a constant current of 0.33C to the lower cut-off voltage of 2.5 V, let it stand for 5 minutes, charge it at a constant current of 0.33C to the upper cut-off voltage of 4.4 V, charge it at a constant voltage until the current < 0.05C, let it stand for 5 minutes, and discharge it at a constant current of 0.33C to the lower cut-off voltage of 2.5 V. Record the discharge capacity at this time, which is the initial discharge capacity C0.

[0216] Operate the battery at -5 °C according to the above process, and record the discharge capacity Cn. Calculate the low-temperature discharge capacity retention rate of the battery at -5 °C according to the following formula. Low-temperature discharge capacity retention rate = 100% × Cn / C0

[0217] The above results are shown in Table 2.

[0218] Table 2: Performance test results of Examples 1 - 36 and Comparative Examples “ / ” means not tested.

[0219] According to the above results, we can know that:

[0220] Compared with the comparative example, the fast charging time of the battery in Examples 1-36 of the present application is shorter and the cycle life is longer.

[0221] Compared with Example 24 of the present application, the fast charging time of the battery of Examples 1-20 of the present application is shorter, the low-temperature discharge capacity retention rate is higher, and the cycle life of Examples 2-19 of the present application is longer.

[0222] Compared with Example 25 of the present application, the batteries of Examples 1-20 of the present application have higher low-temperature power, longer cycle life, and higher low-temperature discharge capacity retention rate.

[0223] Compared with Example 26 of the present application, the low-temperature power of the batteries of Examples 2-6, 8-11, and 13-20 of the present application is higher, and the cycle life of the battery of Example 2-19 of the present application is longer.

[0224] Compared with Example 27 of the present application, the batteries of Examples 1-2, 4-5, 7-11, and 14-19 of the present application have shorter fast charging times and higher low-temperature discharge capacity retention rates, and the batteries of Examples 1-19 of the present application have longer cycle lives.

[0225] Compared with Example 28 of the present application, the fast charging time of the batteries of Examples 1-2, 7-12, and 15-19 of the present application is shorter, and the cycle life of Examples 2-19 of the present application is longer.

[0226] Compared with Example 29 of the present application, the low-temperature power of the batteries of Examples 2-6, 9-11, 13-14, and 16-20 of the present application is higher, and the cycle life of the batteries of Examples 1-19 of the present application is longer.

[0227] Compared with Example 30 of the present application, the batteries of Examples 1-19 of the present application have higher low-temperature power, longer cycle life, and higher low-temperature discharge capacity retention rate.

[0228] Compared with Example 31 of the present application, the batteries of Examples 1-20 of the present application have shorter fast charging time and longer cycle life.

[0229] Compared with Example 32 of the present application, the fast charging time of the batteries of Examples 1-5, 7-12, and 14-20 of the present application is shorter, and the cycle life of the batteries of Examples 2-19 of the present application is longer.

[0230] Compared with Example 33 of the present application, the low-temperature power of the batteries of Examples 2-6, 8-11, and 13-20 of the present application is higher, and the cycle life of the battery of Example 2-19 of the present application is longer.

[0231] Compared with Example 36 of the present application, the batteries of Examples 1-19 of the present application have shorter fast charging time and longer cycle life.

[0232] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises a first positive electrode film layer disposed on the surface of the positive electrode current collector and a second positive electrode film layer disposed on the surface of the first positive electrode film layer; the first positive electrode film layer comprises a first positive electrode active material, and the second positive electrode film layer comprises a second positive electrode active material; The first positive electrode active material comprises a compound Li a A b Mn 1-c B c P 1-d R d O 4-n D n ,in, A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; The B includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; The R includes one or more elements selected from the group consisting of B, Si, N, S, F, Cl and Br; The D comprises one or more elements selected from the group consisting of S, F, Cl and Br; a is 0.9 to 1.1; b is 0 to 0.1; c is 0.001 to 0.9; d is 0 to 0.1; n is 0 to 0.1; The second positive electrode active material comprises a compound Li x Ni y Co z M k Me p O r E m ; wherein, the M includes one or two elements of Mn and Al; the Me includes one or more elements of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W and Nb; the E includes one or more elements of N, F, S and Cl; 0.85≤x≤1.15; 0<y≤1; 0≤z<1; 0<k<1; 0≤p≤0.1; 1≤r≤2, 0≤m≤1, and m+r≤2.

2. The positive electrode sheet according to claim 1, wherein: The B includes one or more elements selected from Fe, Ti, V, Ni, Co and Mg; and / or, The R includes any one of B, Si, N and S elements.

3. The positive electrode sheet according to claim 1 or 2, wherein: The mass ratio of the first positive electrode active material to the second positive electrode active material is 5%-90%, and can be optionally 10%-50%.

4. The positive electrode sheet according to any one of claims 1 to 3, wherein: The second positive electrode active material has a lithium ion diffusion coefficient greater than a lithium ion diffusion coefficient of the first positive electrode active material.

5. The positive electrode sheet according to any one of claims 1 to 4, wherein: The compaction density of the second positive electrode active material under a pressure of 3 tons is greater than the compaction density of the first positive electrode active material under a pressure of 3 tons.

6. The positive electrode sheet according to any one of claims 1 to 5, wherein: The second positive electrode active material is a single crystal or a quasi-single crystal material; and / or, The Dv10 particle size of the second positive electrode active material is 0.3-2.5 μm, and can be 0.5-1.5 μm.

7. The positive electrode sheet according to any one of claims 1 to 6, wherein: The lithium ion diffusion coefficient of the first positive electrode active material at 25° C. is 10 -16 -10 -12 cm 2 ·s -1 , optional 10 -15 -10 -13 cm 2 ·s -1 and / or, The powder resistivity of the first positive electrode active material at 20 MPa is 2000-10000 Ω·cm, and can be 3000-6000 Ω·cm; and / or, The compaction density of the first positive electrode active material under a pressure of 3 tons is 1.9-3.1 g / cm 3 , optional: 2.2-2.9g / cm 3 .

8. The positive electrode sheet according to any one of claims 1 to 7, wherein: The lithium ion diffusion coefficient of the second positive electrode active material at 25°C is 10 -12 -10 -8 cm 2 ·s -1 , optional 10 -11 -10 -9 cm 2 ·s -1 and / or, The powder resistivity of the second positive electrode active material at 20 MPa is 100-700 Ω·cm, and can be 200-550 Ω·cm; and / or, The compaction density of the second positive electrode active material under a pressure of 3 tons is 3-4.2 g / cm 3 , optional: 3.6-3.75g / cm 3 .

9. The positive electrode sheet according to any one of claims 1 to 8, wherein: The thickness ratio of the first positive electrode film layer to the second positive electrode film layer is 0.08-1.53, optionally 0.1-1.2, more optionally 0.15-0.93; and / or, The thickness of the positive electrode film layer is 60-300 μm.

10. The positive electrode sheet according to any one of claims 1 to 9, wherein: The power capacity m of the positive electrode plate is calculated according to the following formula, and m is 2.93-87.62, optionally 3-13, and more optionally 3.81-12.67; in, PD A represents the compaction density of the first positive electrode active material under a pressure of 3 tons, in g / cm 3 ; C A represents the lithium ion diffusion coefficient of the first positive electrode active material at 25°C, in cm 2 ·s -1 ; N A represents the powder resistivity of the first positive electrode active material at 20 MPa, in Ω·cm; PD B represents the compaction density of the second positive electrode active material under 3 tons of pressure, in g / cm 3 ; C B represents the lithium ion diffusion coefficient of the second positive electrode active material at 25°C, in cm 2 ·s -1 ; N B represents the powder resistivity of the second positive electrode active material at 20 MPa, in Ω·cm. M represents the mass ratio of the first positive electrode active material to the second positive electrode active material.

11. The positive electrode sheet according to any one of claims 1 to 10, wherein: The first positive electrode active material comprises a core and a coating layer covering the core, wherein the core comprises the compound Li a A b Mn 1-c B c P 1-d R d O 4-n D n , the coating layer includes one or more of pyrophosphate, phosphate and carbon.

12. The positive electrode sheet according to any one of claims 1 to 11, wherein: The second positive electrode active material comprises a core and a coating layer covering the core, wherein the core comprises the compound Li x Ni y Co z M k Me p O r E m The coating layer includes one or more elements of Al, Ba, Zn, Ti, Co, W, Y, Si, Sn, B and P.

13. A battery comprising the positive electrode sheet according to any one of claims 1 to 12. 。。。。 14. An electrical device comprising the positive electrode sheet according to any one of claims 1 to 12 or the battery according to claim 13.

Citation Information

Patent Citations

  • Battery

    CN111200132A

  • Battery

    CN111200159A

  • Secondary battery and device thereof

    CN111446488A