Binder for secondary battery, preparation method therefor, secondary battery, and electrical apparatus

By using a binder with a core layer and shell structure in the battery cell, the problem of the gap between the pole piece and the separator is solved, the cycle performance and hardness of the battery are improved, and more efficient electrochemical performance is achieved.

WO2024221564A1PCT designated stage expired Publication Date: 2024-10-31CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/099989
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2023-06-13
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

There is an opening problem in the battery cell, and a gap is easily formed between the pole piece and the separator, resulting in poor battery cycle performance.

Method used

A binder is used that includes a core structure and a shell structure. The core structure is composed of a rigid polymer, and the shell structure is composed of an acrylic copolymer. The crystallinity of the rigid polymer ranges from 32% to 94%. To improve the bonding performance of the binder and the hardness of the battery core.

Benefits of technology

By improving the adhesion between the pole piece and the separator, the dynamic performance of the battery is improved, the electrochemical impedance is reduced, and the cycle performance of the secondary battery is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023099989_31102024_PF_FP_ABST
    Figure CN2023099989_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of secondary batteries, and particularly relates to a binder for a secondary battery, a preparation method therefor, a secondary battery, and an electrical apparatus. The binder comprises a core layer structure and a shell layer structure provided on the surface of the core layer structure. The shell layer structure comprises an acrylate copolymer, and the core layer structure comprises a rigid polymer, the value range of the crystallinity of the rigid polymer being 32-94%. Since the binder of the core-shell structure comprises the core layer structure containing the rigid polymer, during a cold pressing process of battery cells, the rigid polymer serving as a support enables the structure of binder particles to be stable, that is, the rigid polymer achieves a supporting effect so that the overall rigidity of the binder is improved. Therefore, during cold pressing of battery cells, the dimensional stability of the binder is improved, avoiding complete deformation, thereby improving the hardness of battery cells while improving the cold-pressing bonding force of battery cells.
Need to check novelty before this filing date? Find Prior Art

Description

Binder for secondary battery, preparation method thereof, secondary battery and electrical device

[0001] Related applications

[0002] This application claims priority to Chinese patent application No. 202310447245.8 filed on April 24, 2023, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the technical field of secondary batteries, and in particular to a binder for secondary batteries and a preparation method thereof, a secondary battery, and an electrical device. Background Art

[0004] With the rapid growth of portable electronic devices and electric vehicles, the demand for power batteries is also growing. Among them, the electrochemical performance of batteries is also attracting more and more attention.

[0005] At present, there is an opening problem in battery cells, that is, a gap is easily formed between the electrode and the diaphragm, resulting in poor battery cycle performance.

[0006] Summary of the Invention

[0007] The main purpose of this application is to provide an adhesive, which aims to improve the adhesion between the electrode and the separator, thereby improving battery performance.

[0008] To achieve the above-mentioned purpose, the present application proposes a binder for secondary batteries, which includes a core layer structure and a shell layer structure arranged on the surface of the core layer structure, the shell layer structure includes an acrylic copolymer, and the core layer structure includes a rigid polymer, and the crystallinity range of the rigid polymer is 32% to 94%.

[0009] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the electrode after cold pressing.

[0010] Rigid polymers have a crystallinity range of 32% to 94% and possess properties such as high strength, impact resistance, heat resistance, hardness, and aging resistance. Rigid polymers are difficult to deform during the cold pressing process of the battery cell. It is understood that rigid polymers exhibit minimal or no deformation during the cold pressing process.

[0011] The core-shell structure adhesive includes a core layer structure of a rigid polymer. During the cold pressing process of the battery cell, the rigid polymer acts as a support to stabilize the adhesive particle structure, that is, the rigid polymer plays a supporting role, and the overall rigidity of the adhesive is improved. When the battery cell is cold pressed, the dimensional stability of the adhesive is improved so that it will not be completely deformed. While improving the cold pressing bonding strength of the battery cell, the hardness of the battery cell is improved.

[0012] It is understandable that without the rigid polymer of the core layer as support, the probability of the binder being flattened increases, and during the flattening process, the pores between the binders are compressed and blocked, which is not conducive to the penetration of electrolyte and the transmission of ions.

[0013] Since rigid polymers are difficult to deform, the binder can maintain a certain shape during the cold pressing process, thereby improving the problem of clogging the pores between the binder particles due to the deformation of the binder during the flattening process.

[0014] Since the binder of the present application is supported by a rigid polymer, the binder particles are difficult to completely deform during cold pressing so as not to block the pores between the binder particles. These unblocked pores become channels for electrolyte infiltration, which is beneficial to the transmission of ions. At the same time, it also increases the hardness of the battery cell, improves the dynamic performance of the secondary battery, reduces the electrochemical impedance, and can improve the cycle performance of the secondary battery.

[0015] It is understandable that during the cold pressing process of the battery cell, the core layer structure of the adhesive does not deform or undergoes slight deformation, reducing the probability of the adhesive particles being flattened. The shell structure includes acrylic copolymers, which can provide better viscosity and improve the cold pressing adhesion of the battery cell. It is understandable that during the cold pressing process, the acrylic copolymers in the shell structure are deformed by the extrusion force, so that the shell structure can be inserted into the gaps between the diaphragm and the electrode, thereby improving the adhesion.

[0016] Optionally, the rigid polymer has a crystallinity value in the range of 40% to 80%.

[0017] In order to improve the hardness of the rigid polymer, preferably, the crystallinity of the rigid polymer is greater than or equal to 40%. At the same time, considering that too high crystallinity is difficult to implement in the process, therefore, preferably, the crystallinity of the rigid polymer is less than or equal to 80%.

[0018] Optionally, the rigid polymer includes at least one of polyethylene, polypropylene, polystyrene, polymethyl methacrylate, and polyamide.

[0019] Rigid polymers include commonly used engineering plastics. Engineering plastics refer to industrial plastics used as industrial parts or housing materials, and have good strength, impact resistance, heat resistance, hardness, and aging resistance. For example, they include at least one of polyethylene, polypropylene, polystyrene, polymethyl methacrylate, and polyamide. The rigid polymers of this application can be selected from the rigid polymers listed above, and of course, other rigid polymers not listed in this application can also be selected. Engineering plastics have a relatively high degree of crystallinity, generally ranging from 32% to 94%. Using the above-mentioned rigid polymers as the core layer structure is beneficial to improving the cold pressing performance of the adhesive.

[0020] Optionally, the shape of the binder includes a spherical shape.

[0021] The spherical shape facilitates uniform dispersion during the stirring of the slurry, which is conducive to uniform coating.

[0022] Optionally, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm. Preferably, the volume particle size distribution Dv50 of the binder is 1 μm to 12 μm.

[0023] In order to improve the permeability of lithium ions (taking lithium ion batteries as an example, of course it can also be other types of secondary batteries) on the diaphragm and improve the energy density of the battery, the volume particle size distribution Dv50 of the binder is 1μm to 15μm, preferably 1μm to 12μm.

[0024] Optionally, the ratio of the volume particle size distribution Dv50 of the acrylic copolymer to the volume particle size distribution Dv50 of the rigid polymer is 1:(1-50).

[0025] In order to effectively arrange the acrylic copolymer on the surface of the core layer structure to form a core-shell structure, the volume particle size distribution Dv50 of the acrylic copolymer is smaller than the volume particle size distribution Dv50 of the rigid polymer. Specifically, the ratio of the volume particle size distribution Dv50 of the acrylic copolymer to the volume particle size distribution Dv50 of the rigid polymer is 1:(1~50).

[0026] Optionally, the volume particle size distribution Dv50 of the rigid polymer is 0.1 μm to 5 μm, preferably, the volume particle size distribution Dv50 of the rigid polymer is 0.5 μm to 2 μm;

[0027] And / or, the volume particle size distribution Dv50 of the acrylic ester copolymer is 100 nm to 200 nm, preferably, the volume particle size distribution Dv50 of the acrylic ester copolymer is 130 nm to 180 nm. It is understood that in order to obtain a core-shell structured adhesive and improve the adhesive's adhesion, the volume particle size distribution Dv50 of the rigid polymer is 0.1 μm to 5 μm, preferably 0.5 μm to 2 μm, and the volume particle size distribution Dv50 of the acrylic ester copolymer is 100 nm to 200 nm, preferably 130 nm to 180 nm.

[0028] It can be understood that the binder of the core-shell structure can be a binder in which the shell structure completely covers the core structure, or a binder in which the shell structure does not completely cover the shell structure.

[0029] Optionally, the ratio of the mass of the shell structure to the mass of the core structure is 1:(0.1-10). Preferably, the ratio of the mass of the shell structure to the mass of the core structure is 1:(0.1-5).

[0030] In order to improve the problem of reduced adhesive performance of the adhesive caused by excessive mass of the rigid polymer; and to improve the problem of reduced overall hardness of the adhesive caused by insufficient mass of the rigid polymer, which affects the subsequent battery performance, the ratio of the mass of the shell structure to the mass of the core layer structure is 1:(0.1~10). Preferably, the ratio of the mass of the shell structure to the mass of the core layer structure is 1:(0.1~5).

[0031] Optionally, the monomers constituting the acrylic ester copolymer include at least two of acrylic ester monomers, acrylonitrile monomers, and acrylamide monomers.

[0032] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the electrode after cold pressing.

[0033] It is understood that acrylate monomers can improve the polymer's anti-swelling ability and, as flexible monomer segments within the molecular chain, can adjust the polymer's glass transition temperature, improving the adhesive's toughness during application and contributing to effective bonding. Acrylonitrile monomers, with their highly polar cyano groups, help improve ionic conductivity. Acrylamide monomers serve to regulate molecular weight.

[0034] When the constituent monomers of the acrylic ester copolymer include two of the acrylic ester monomers, acrylonitrile monomers, and acrylamide monomers, the bonding performance is better. When the constituent monomers include all three of the above monomers, the performance is even better.

[0035] Optionally, the acrylic acid ester monomer includes at least one of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate;

[0036] And / or, the acrylonitrile monomer includes at least one of acrylonitrile or methacrylonitrile;

[0037] And / or, the acrylamide monomer includes at least one of acrylamide, N-hydroxymethyl acrylamide and N-butoxymethyl acrylamide.

[0038] By using any one or more of the above-mentioned acrylate monomers, the glass transition temperature of the polymer can be adjusted and the anti-swelling ability of the polymer can be improved. The above is an enumeration of acrylate monomers. The acrylate monomers used in this application can be the substances listed above or other acrylate monomers other than those in this application.

[0039] The use of any one or more of the above-mentioned acrylonitrile monomers can improve the ionic conductivity of the binder. The above is an enumeration of acrylonitrile monomers. The acrylonitrile monomers used in this application can be the above-mentioned substances or other acrylonitrile monomers other than those in this application.

[0040] Using any one or more of the above-mentioned acrylamide monomers can regulate the molecular weight of the polymer. A molecular weight within a certain range of the adhesive helps improve adhesion. The above is an example of acrylamide monomers. The acrylamide monomers used in this application can be any of the above-mentioned substances or other acrylamide monomers not mentioned in this application.

[0041] Optionally, the constituent monomers of the acrylic ester copolymer include acrylic ester monomers, acrylonitrile monomers, and acrylamide monomers, and the mass ratio of the acrylic ester monomers, the acrylonitrile monomers, and the acrylamide monomers is 1:(0.01-0.8):(0.01-0.15). Preferably, the mass ratio of the acrylic ester monomers, the acrylonitrile monomers, and the acrylamide monomers is 1:(0.1-0.6):(0.06-0.12).

[0042] By controlling the mass ratio of the three monomers within the above range, the molecular weight and glass transition temperature of the polymer can be controlled, thereby improving the bonding properties of the adhesive.

[0043] The present application also provides a method for preparing a binder for a secondary battery, comprising:

[0044] preparing an acrylic copolymer emulsion;

[0045] The acrylic copolymer emulsion is blended with a rigid polymer and spray-dried to obtain a core-shell structure adhesive.

[0046] An acrylic copolymer emulsion is prepared by emulsion polymerization, the acrylic copolymer emulsion is blended with a rigid polymer, and spray-dried to obtain a core-shell structure adhesive.

[0047] During spray drying, the acrylic copolymer particles are small and sticky, and will be adsorbed on the surface of non-sticky rigid particles to coat them, thereby forming a core-shell structure.

[0048] In the step of forming the core-shell adhesive, spray drying provides better coating of rigid particles with acrylic copolymers than emulsion polymerization. Furthermore, emulsion polymerization is difficult to control during polymerization, so spray drying is used to prepare the core-shell adhesive, resulting in an adhesive with better bonding properties.

[0049] During the spray drying process, the shell structure is formed by the accumulation of spherical particles on the surface of the core structure. The spherical particles are in point contact with each other, creating channels and voids in the shell, which facilitates electrolyte infiltration. The support of the core structure reduces the probability of binder particles flattening during cold pressing, thus reducing the possibility of channels and voids in the shell being squeezed and blocked. This increases the porosity of the adhesive layer, allowing the electrolyte to penetrate into the binder through the gaps between the acrylic copolymer particles.

[0050] At the same time, some rigid polymer materials also have rich functional groups on their surfaces, which can improve electrolyte wettability, accelerate ion transport, and enhance the electrochemical performance of batteries. For example, rigid polymers composed of polymethyl methacrylate have ester groups, which can improve the wettability of solvents in the electrolyte, such as ethylene carbonate, propylene carbonate, and ethyl methyl carbonate.

[0051] Optionally, the step of preparing the acrylic copolymer emulsion includes:

[0052] Stirring and emulsifying water, an emulsifier, and monomers constituting an acrylic copolymer to obtain a pre-emulsion of the monomers;

[0053] The emulsifier and water are stirred and emulsified, the pre-emulsion and the initiator are added under heating conditions, and the temperature is increased to obtain an acrylic copolymer emulsion.

[0054] In the step of preparing the acrylic copolymer emulsion, the steps of pre-emulsification and then polymerization reaction are adopted to make the monomers more evenly mixed, and the obtained acrylic copolymer particles are more uniform and have more stable performance.

[0055] The present application also provides a separator, comprising a base film and an adhesive layer provided on at least one side of the base film, wherein the adhesive layer comprises the adhesive for secondary batteries as described above;

[0056] Alternatively, the adhesive layer includes an adhesive prepared by the method for preparing an adhesive for a secondary battery.

[0057] The present application also provides a secondary battery, which includes the separator as described above.

[0058] The present application also provides an electrical device, which includes the secondary battery as described above. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0060] FIG1 is a scanning electron microscope image of the adhesive provided in Example 1 of the present application;

[0061] FIG2 is a schematic flow chart of a method for preparing a binder provided in an embodiment of the present application;

[0062] FIG3 is a schematic diagram of a secondary battery provided in an embodiment of the present application;

[0063] FIG4 is an exploded view of the secondary battery provided by the embodiment of the present application shown in FIG3 ;

[0064] FIG5 is a schematic diagram of a battery module provided in an embodiment of the present application;

[0065] FIG6 is a schematic diagram of a battery pack provided in an embodiment of the present application;

[0066] FIG7 is an exploded view of the battery pack provided by the embodiment of the present application shown in FIG6 ;

[0067] FIG8 is a schematic diagram of an electrical device using a secondary battery provided in an embodiment of the present application as a power source.

[0068] Description of Figure Numbers:

[0069] The realization of the objectives, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0070] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0071] Below, the binder and its preparation method of the present application, as well as the embodiments of the diaphragm, electrode assembly, battery cell, battery and electrical device containing the binder are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0072] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0073] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0074] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0075] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0076] There is an opening problem in the battery cell, that is, a gap is easily formed between the electrode and the diaphragm, resulting in poor battery cycle performance.

[0077] For example, polyvinylidene fluoride (PVDF), the most commonly used binder, is widely used in separators, but its current cost is high. Coating PVDF polymer on the surface of secondary battery separators can partially address the separator's high-temperature shrinkage problem. After winding, battery cells undergo cold pressing, but conventional PVDF is a homopolymer with a crystallinity of approximately 50%, resulting in insufficient adhesion to the positive and negative electrodes, often leading to cell opening problems and failing to meet the performance requirements of coated separators for power secondary batteries.

[0078] Specifically, coating the battery separator with polyvinylidene fluoride (PVDF) polymer can partially address the separator's high-temperature shrinkage problem. After winding, the battery cell undergoes cold pressing, but conventional PVDF is a homopolymer with a crystallinity of approximately 50%, resulting in insufficient adhesion to the positive and negative electrode sheets, often leading to cell openings. These openings create gaps between the electrode sheets and the separator, loosening the overall cell structure and reducing its rigidity, leading to poor cycling performance.

[0079] The battery cell is formed by bonding the positive and negative electrode sheets and the separator. The battery cell has a certain hardness. That is, because the bonded positive and negative electrode sheets and the separator adhere to each other and support each other, a structure with a certain thickness is formed. A structure with a certain thickness has a certain hardness. The negative electrode will expand during the charge and discharge process. If the bonding force is weak, a gap will form between the positive and negative electrode sheets and the separator. The positive and negative electrode sheets and the separator cannot adhere to each other and support each other, resulting in a loose battery cell and a lower hardness. At this time, the power performance of the battery cell will deteriorate. For example, the rate performance will be reduced, and the cycle performance will also deteriorate. For example, in electric vehicles, loose battery cells will cause the battery charging speed to slow down, and the battery cycle performance will deteriorate, which will directly shorten the battery life. Electric vehicles need to frequently replace batteries, and consumers' costs for electric vehicles increase.

[0080] Based on this, the present application proposes an adhesive for secondary batteries, which includes a core layer structure and a shell layer structure arranged on the surface of the core layer structure. The shell layer structure includes an acrylic copolymer, and the core layer structure includes a rigid polymer. The crystallinity range of the rigid polymer is 32% to 94%.

[0081] Binder refers to a material with adhesive properties that is used to bond different substances together.

[0082] The core-shell structure consists of a central core and an outer shell.

[0083] In the core-shell structure, the core layer structure is located inside and is covered by the outer shell.

[0084] In the core-shell structure, the shell structure is located on the outside and the structure covering the surface of the core structure is the shell structure.

[0085] The core-shell structure can be observed through a transmission electron microscope. Specifically, due to the different materials of the core-shell structure, there will be a difference in brightness (thickness contrast) between the core layer structure and the shell layer structure in the transmission electron microscope image. The thickness contrast is due to the differences in thickness and mass of different areas on the sample surface. Since different parts of the sample have different electron scattering abilities, the number of transmitted electrons passing through the objective lens is also different, and thus the electron beam intensity will be different. The image of the area with strong scattering and less transmitted electrons is dark, and vice versa.

[0086] Acrylate copolymers, acrylic copolymers are a general term for polymers produced by copolymerization of acrylic monomers and other comonomers.

[0087] The acrylic ester monomer has an acrylate group in its structure, for example, methyl acrylate, ethyl acrylate, and n-butyl acrylate.

[0088] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the electrode after cold pressing.

[0089] Crystallinity, crystallinity is used to indicate the proportion of crystalline regions in a polymer. Crystallinity is an ordered arrangement of molecular chains.

[0090] Crystallinity can be measured using DSC (Differential Scanning Calorimetry). For example, the crystallinity test for polypropylene involves using DSC to determine crystallinity. A uniform value for the heat of fusion, ΔH0, of a fully crystalline polymer is used to minimize the impact on the sample's test results. The procedure is as follows: Under nitrogen at a flow rate of 20 mL / min, place a 5 mg sample in a DSC (Differential Scanning Calorimeter (DSC): Model SDT2960, TA Instruments, USA). The temperature is raised from room temperature to 210°C at a rate of 15°C / min, held at that temperature for 5 minutes to eliminate thermal history, and then cooled to room temperature at a constant rate of 5°C / min. The process is recorded and the crystallinity is calculated.

[0091] Rigid polymers, with a crystallinity range of 32% to 94%, offer high strength, impact resistance, heat resistance, hardness, and aging resistance. Examples include polyethylene and polypropylene. Rigid polymers are lighter than inorganic particles and can increase battery energy density.

[0092] During the cold pressing process of the battery cell, the rigid polymer is difficult to deform. It is understandable that the rigid polymer does not deform or undergoes minimal deformation during the cold pressing process. It is understandable that the cold pressure range during the cold pressing process is 1MPa to 10MPa. Within this range, the rigid polymer does not deform or undergoes minimal deformation.

[0093] The core-shell structure adhesive includes a core layer structure of a rigid polymer. During the cold pressing process of the battery cell, the rigid polymer acts as a support to stabilize the adhesive particle structure, that is, the rigid polymer plays a supporting role, and the overall rigidity of the adhesive is improved. When the battery cell is cold pressed, the dimensional stability of the adhesive is improved so that it will not be completely deformed. While improving the cold pressing bonding strength of the battery cell, the hardness of the battery cell is improved.

[0094] It is understandable that without the rigid polymer of the core layer as support, the probability of the binder being flattened increases, and during the flattening process, the pores between the binders are compressed and blocked, which is not conducive to the penetration of electrolyte and the transmission of ions.

[0095] Since rigid polymers are difficult to deform, the binder can maintain a certain shape during the cold pressing process, thereby improving the problem of clogging the pores between the binder particles due to the deformation of the binder during the flattening process.

[0096] Since the binder of the present application is supported by a rigid polymer, the binder particles are difficult to completely deform during cold pressing so as not to block the pores between the binder particles. These unblocked pores become channels for electrolyte infiltration, which is beneficial to the transmission of ions. At the same time, it also increases the hardness of the battery cell, improves the dynamic performance of the secondary battery, reduces the electrochemical impedance, and can improve the cycle performance of the secondary battery.

[0097] It can be understood that during the cold pressing process of the battery cell, the core layer structure of the adhesive does not deform or undergoes slight deformation, reducing the probability of the adhesive particles being flattened. The shell layer structure includes acrylic copolymers, which can provide better viscosity and improve the cold pressing adhesion of the battery cell.

[0098] In the above-mentioned 32% to 94%, the values ​​include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 32%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 94%, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0099] In one embodiment, the rigid polymer has a crystallinity ranging from 40% to 80%.

[0100] In order to improve the hardness of the rigid polymer, preferably, the crystallinity of the rigid polymer is greater than or equal to 40%. At the same time, considering that too high crystallinity is difficult to implement in the process, therefore, preferably, the crystallinity of the rigid polymer is less than or equal to 80%.

[0101] In the above 40% to 80%, the values ​​include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, etc., as well as the range values ​​between any two of the above point values.

[0102] In one embodiment, the rigid polymer includes at least one of polyethylene, polypropylene, polystyrene, polymethyl methacrylate, and polyamide.

[0103] Rigid polymers include commonly used engineering plastics. Engineering plastics refer to industrial plastics used as industrial parts or housing materials, and have good strength, impact resistance, heat resistance, hardness, and aging resistance. For example, they include at least one of polyethylene, polypropylene, polystyrene, polymethyl methacrylate, and polyamide. The rigid polymers of this application can be selected from the rigid polymers listed above, and of course, other rigid polymers not listed in this application can also be selected. Engineering plastics have a relatively high degree of crystallinity, generally ranging from 32% to 94%. Using the above-mentioned rigid polymers as the core layer structure is beneficial to improving the cold pressing performance of the adhesive.

[0104] In one embodiment, the shape of the binder includes a spherical shape.

[0105] The spherical shape facilitates uniform dispersion during the stirring of the slurry, which is conducive to uniform coating.

[0106] In one embodiment, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm. Preferably, the volume particle size distribution Dv50 of the binder is 1 μm to 12 μm.

[0107] Dv50: Among the sample particles, 50% of the total volume of the particles have a particle size larger than this value, and another 50% of the total volume of the particles have a particle size smaller than this value; Dv50 can represent the median particle size of the sample.

[0108] The volume particle size distribution Dv50 of the binder can be measured using methods known in the art. For example, GB / T 19077-2016 can be used for characterization testing using a Malvern laser particle size analyzer, such as a Malvern Mastersizer-3000.

[0109] In order to improve the permeability of lithium ions (taking lithium ion batteries as an example, of course it can also be other types of secondary batteries) on the diaphragm and improve the energy density of the battery, the volume particle size distribution Dv50 of the binder is 1μm to 15μm, preferably 1μm to 12μm.

[0110] In the above-mentioned 1μm to 15μm, the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0111] In the above-mentioned 1μm to 15μm, the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0112] Theoretically, the volume particle size distribution Dv50 of the acrylic copolymer and the volume particle size distribution Dv50 of the rigid polymer in the binder can be obtained by measurement using a projection electron microscope and a scanning electron microscope.

[0113] The size of the core structure can be measured by the binder image obtained by projection electron microscopy, and the size of the shell particles can be measured by the image obtained by scanning electron microscopy.

[0114] In one embodiment, the ratio of the volume particle size distribution Dv50 of the acrylic copolymer to the volume particle size distribution Dv50 of the rigid polymer is 1:(1-50).

[0115] In order to effectively arrange the acrylic copolymer on the surface of the core layer structure to form a core-shell structure, the volume particle size distribution Dv50 of the acrylic copolymer is smaller than the volume particle size distribution Dv50 of the rigid polymer. Specifically, the ratio of the volume particle size distribution Dv50 of the acrylic copolymer to the volume particle size distribution Dv50 of the rigid polymer is 1:(1~50).

[0116] In the above 1:(1~50), the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1:1, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, etc., as well as the range values ​​between any two of the above point values.

[0117] In one embodiment, the volume particle size distribution Dv50 of the rigid polymer is 0.1 μm to 5 μm, preferably, the volume particle size distribution Dv50 of the rigid polymer is 0.5 μm to 2 μm; and / or, the volume particle size distribution Dv50 of the acrylic copolymer is 100 nm to 200 nm, preferably, the volume particle size distribution Dv50 of the acrylic copolymer is 130 nm to 180 nm.

[0118] It can be understood that in order to obtain a core-shell structured adhesive; and to improve the bonding properties of the adhesive, the volume particle size distribution Dv50 of the rigid polymer is 0.1 μm to 5 μm, preferably 0.5 μm to 2 μm, and the volume particle size distribution Dv50 of the acrylic copolymer is 100 nm to 200 nm, preferably 130 nm to 180 nm.

[0119] In the above 0.1μm to 5μm, the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 0.1μm, 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, etc., as well as the range values ​​between any two of the above point values.

[0120] In the above-mentioned 0.5μm to 2μm, the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 0.5μm, 0.7μm, 0.9μm, 1μm, 1.2μm, 1.4μm, 1.5μm, 1.7μm, 1.9μm, 2μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0121] In the above-mentioned 100nm to 200nm, the values ​​include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 18nm, 190nm, 200nm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0122] In the above-mentioned 130nm to 180nm, the values ​​include the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 130nm, 140nm, 150nm, 160nm, 170nm, 18nm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0123] It can be understood that the binder of the core-shell structure can be a shell structure that completely covers the core structure, or a shell structure that does not completely cover the shell structure, and there is no specific limitation.

[0124] In one embodiment, the ratio of the mass of the shell structure to the mass of the core structure is 1:(0.1-10). Preferably, the ratio of the mass of the shell structure to the mass of the core structure is 1:(0.1-5).

[0125] The mass ratio test method is as follows: during the preparation of the adhesive, the mass of the rigid polymer used to prepare the core layer structure is recorded as m, and the mass of the acrylic copolymer used to prepare the shell layer structure is recorded as n. The mass ratio of the core layer structure to the shell layer structure is m:n.

[0126] In order to improve the problem of reduced adhesive performance of the adhesive caused by excessive rigid polymer mass; and to improve the problem of reduced overall hardness of the adhesive caused by insufficient rigid polymer mass, which affects the subsequent battery performance, the ratio of the mass of the shell structure to the mass of the core structure is 1:(0.1~10), preferably 1:(0.1~5).

[0127] In the above 1:(0.1~10), the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1:0.1, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc., as well as the range values ​​between any two of the above point values.

[0128] In the above 1:(0.1~5), the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1:0.1, 1:1, 1:2, 1:3, 1:4, 1:5, etc., as well as the range values ​​between any two of the above point values.

[0129] In one embodiment, the monomers constituting the acrylic ester copolymer include at least two of acrylic ester monomers, acrylonitrile monomers, and acrylamide monomers.

[0130] Acrylate monomers, the structure of which includes an acrylate group, for example, its structural formula is Wherein, R1 includes a hydrogen atom or an alkyl group with 1 to 12 carbon atoms, and R2 includes an alkyl group with 1 to 12 carbon atoms. In one embodiment, the acrylic acid ester monomer includes methyl acrylate, ethyl acrylate, n-butyl acrylate, etc.

[0131] Acrylonitrile monomers, which have unsaturated cyano groups in their structures, for example, have the structural formula Wherein, R3 comprises a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. In one embodiment, the acrylonitrile monomer comprises acrylonitrile, methacrylonitrile, etc.

[0132] Acrylamide monomers, the structure of which includes unsaturated amide groups, for example, its structural formula is Wherein, R4 comprises a hydrogen atom or an alkyl group of 1-6 carbon atoms, and R5 comprises a hydrogen atom, an alkyl group of 1-6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1-6 carbon atoms. In one embodiment, the acrylamide monomer includes acrylamide, N-hydroxymethyl acrylamide, and N-butoxymethyl acrylamide.

[0133] It is understandable that acrylate monomers can improve the anti-swelling ability of the polymer, and as flexible monomer segments in the molecular chain segments, they can adjust the glass transition temperature of the polymer, improve the toughness of the adhesive during application, and help to exert a good bonding effect.

[0134] Acrylonitrile monomers, which have a highly polar cyano group, help to improve ionic conductivity.

[0135] Acrylamide monomers play a role in regulating molecular weight.

[0136] When the constituent monomers of the acrylic copolymer include two of the acrylic monomers, acrylonitrile monomers, and acrylamide monomers, for example, when including acrylic monomers and acrylonitrile monomers, and when including acrylic monomers and acrylamide monomers, the bonding performance is better. When including the above three monomers at the same time, the performance is even better.

[0137] In one embodiment, the acrylate monomer includes at least one of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate; and / or, the acrylonitrile monomer includes at least one of acrylonitrile or methacrylonitrile; and / or, the acrylamide monomer includes at least one of acrylamide, N-hydroxymethyl acrylamide, and N-butoxymethyl acrylamide.

[0138] By using any one or more of the above-mentioned acrylate monomers, the glass transition temperature of the polymer can be adjusted and the anti-swelling ability of the polymer can be improved. The above is an enumeration of acrylate monomers. The acrylate monomers used in this application can be the substances listed above or other acrylate monomers other than those in this application.

[0139] The use of any one or more of the above-mentioned acrylonitrile monomers can improve the ionic conductivity of the binder. The above is an enumeration of acrylonitrile monomers. The acrylonitrile monomers used in this application can be the above-mentioned substances or other acrylonitrile monomers other than those in this application.

[0140] Using any one or more of the above-mentioned acrylamide monomers can regulate the molecular weight of the polymer. A molecular weight within a certain range of the adhesive helps improve adhesion. The above is an example of acrylamide monomers. The acrylamide monomers used in this application can be any of the above-mentioned substances or other acrylamide monomers not mentioned in this application.

[0141] In one embodiment, the constituent monomers of the acrylic ester copolymer include acrylic ester monomers, acrylonitrile monomers, and acrylamide monomers, and the mass ratio of the acrylic ester monomers, acrylonitrile monomers, and acrylamide monomers is 1:(0.01-0.8):(0.01-0.15). Preferably, the mass ratio of the acrylic ester monomers, acrylonitrile monomers, and acrylamide monomers is 1:(0.1-0.6):(0.06-0.12).

[0142] By controlling the mass ratio of the three monomers within the above range, the molecular weight and glass transition temperature of the polymer can be controlled, thereby improving the bonding properties of the adhesive.

[0143] In the above 1:(0.01~0.8):(0.01~0.15), the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1:0.01:0.01, 1:0.1:0.01, 1:0.4:0.01, 1:0.8:0.01, 1:0.01:0.05, 1:0.01:0.1, 1:0.01:0.15, 1:0.1:0.01, 1:0.1:0.05, 1:0.1:0.15, 1:0.4:0.01, 1:0.4:0.05, 1:0.4:0.15, 1:0.8:0.01, 1:0.8:0.05, 1:0.8:0.15, etc., and the range values ​​between any two of the above point values.

[0144] In the above 1: (0.1~0.6): (0.06~0.12), the values ​​include the minimum and maximum values ​​of the range, and every value between this minimum and maximum value. Specific examples include but are not limited to the point values ​​in the embodiments and 1:0.1:0.06, 1:0.4:0.06, 1:0.6:0.06, 1:0.1:0.1, 1:0.1:0.12, etc., as well as the range values ​​between any two of the above point values.

[0145] In one embodiment, the present application also provides a method for preparing a binder for a secondary battery, comprising: preparing an acrylic copolymer emulsion; blending the acrylic copolymer emulsion with a rigid polymer, and spray drying the mixture to obtain a core-shell structured binder.

[0146] Spray drying, through mechanical action, disperses the material to be dried (a mixture of acrylic copolymer emulsion and rigid polymer) into very fine mist-like particles (increasing the water evaporation area and accelerating the drying process). When in contact with hot air, most of the water is removed instantly, and the solid matter in the material is dried into powder.

[0147] The core-shell structure adhesive is obtained through a spray drying process.

[0148] During spray drying, the acrylic copolymer particles are small and sticky, and will be adsorbed on the surface of non-sticky rigid particles to coat them, thereby forming a core-shell structure.

[0149] In the step of forming the core-shell adhesive, spray drying provides better coating of rigid particles with acrylic copolymers than emulsion polymerization. Furthermore, emulsion polymerization is difficult to control during polymerization, so spray drying is used to prepare the core-shell adhesive, resulting in an adhesive with better bonding properties.

[0150] During the spray drying process, the shell structure is formed by the accumulation of spherical particles on the surface of the core structure. The spherical particles are in point contact with each other, creating channels and voids in the shell, which facilitates electrolyte infiltration. The support of the core structure reduces the probability of binder particles flattening during cold pressing, thus reducing the possibility of channels and voids in the shell being squeezed and blocked. This increases the porosity of the adhesive layer, allowing the electrolyte to penetrate into the binder through the gaps between the acrylic copolymer particles.

[0151] Understandably, traditional secondary battery separators are mostly polyolefin separators. Multilayer separators have the function of blocking ion transmission at high temperatures by closing pores, thus ensuring battery safety. The PP (polypropylene) layer on the separator surface further improves the separator's antioxidant capacity. Compared with traditional single-layer separators, these multilayer polyolefin composite separators have improved battery cycle performance and safety to a certain extent. However, the characteristics of polyolefin separators, such as poor electrolyte wettability and low thermal decomposition temperature, still exist, and the performance of multilayer polyolefin separators is gradually failing to meet the growing social needs.

[0152] The rigid polymers described in this application possess low density and excellent thermal and chemical stability. Furthermore, some rigid polymer materials also possess a rich surface functional group, which can enhance electrolyte wettability, accelerate ion transport, and improve the electrochemical performance of the battery. For example, a rigid polymer composed of polymethyl methacrylate has ester groups, which can improve the wettability of electrolyte solvents such as ethylene carbonate, propylene carbonate, and ethyl methyl carbonate.

[0153] In one embodiment, the steps of preparing an acrylic copolymer emulsion include: stirring and emulsifying water, an emulsifier, and monomers constituting the acrylic copolymer to obtain a pre-emulsion of the monomers; stirring and emulsifying the emulsifier and water, adding the pre-emulsion and an initiator under heating conditions, and raising the temperature to obtain the acrylic copolymer emulsion.

[0154] Pre-emulsion is a solution obtained by pre-emulsifying the monomers. Emulsification is the process of evenly dispersing a liquid in another immiscible liquid in the form of extremely small droplets. Water, an emulsifier, and the monomers constituting the acrylic copolymer are blended and stirred so that the monomers constituting the acrylic copolymer are dispersed in water under the action of the emulsifier.

[0155] Emulsion polymerization is a process in which monomers are dispersed in water with the help of emulsifiers and mechanical stirring to form an emulsion, and then an initiator is added to initiate monomer polymerization.

[0156] Emulsifiers are substances that can transform mutually incompatible oil and water into an emulsion that is difficult to separate. Emulsifiers are usually surfactants that have both hydrophilic polar groups and hydrophobic (lipophilic) non-polar groups.

[0157] Initiators are substances that can initiate polymerization reactions of monomers. For example, free radical initiators are compounds that readily decompose into free radicals (i.e., primary free radicals) upon exposure to heat. They can be used to initiate free radical polymerization and copolymerization reactions of olefins and dienes.

[0158] In the preparation of the acrylic copolymer emulsion, pre-emulsification followed by polymerization allows for more uniform monomer mixing, resulting in more uniform acrylic copolymer particles with more stable performance. This helps ensure that the acrylic copolymer particles are effectively deposited on the core layer during the spray drying process.

[0159] It is understood that, in the specific operation process, two containers can be used for the test operation. In the first container, water, emulsifier, and monomers constituting the acrylic copolymer are added and stirred and emulsified to obtain a monomer pre-emulsion. In the second container, emulsifier and water are again added and stirred and emulsified. The pre-emulsion and initiator solution are then added under heating conditions, and the temperature is raised to obtain an acrylic copolymer emulsion.

[0160] For example, in one embodiment, the volume particle size distribution (Dv50) of the acrylic copolymer obtained through emulsion polymerization ranges from 0.1 μm to 0.11 μm, showing relatively uniform particle size. The volume particle size distribution (Dv50) of the rigid polymer is approximately 1 μm ± 0.2 μm. Spray drying allows the acrylic copolymer to effectively adhere to the surface of the rigid polymer.

[0161] An embodiment of the present application also provides a diaphragm, which includes a base film and an adhesive layer provided on at least one side of the base film, the adhesive layer including the adhesive for secondary batteries as described above; or, the adhesive layer including an adhesive prepared by the preparation method of the adhesive for secondary batteries as described above.

[0162] An embodiment of the present application further provides a secondary battery, which includes the separator as described above.

[0163] Secondary batteries include battery modules, battery cells, battery packs, and other forms. When the secondary battery is a battery cell, the battery cell includes the aforementioned separator; when the secondary battery is a battery module, the battery module includes the aforementioned separator; and when the secondary battery is a battery pack, the battery pack includes the aforementioned separator.

[0164] An embodiment of the present application further provides an electrical device, which includes the aforementioned secondary battery.

[0165] In addition, the electrode assembly, battery cell, battery, and electric device of the present application will be described below with reference to the accompanying drawings as appropriate.

[0166] In one embodiment of the present application, an electrode assembly is provided.

[0167] Typically, an electrode assembly includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery's charge and discharge process, active ions are embedded in and released from the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator is located between the positive and negative electrodes, primarily preventing a short circuit between the positive and negative electrodes while allowing ions to pass through. The separator is the separator described above in this application.

[0168] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.

[0169] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0170] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0171] In some embodiments, when the electrode assembly is a lithium-ion battery, the positive electrode active material may be a positive electrode active material for lithium-ion batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0172] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0173] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0174] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0175] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0176] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0177] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0178] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0179] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0180] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0181] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0182] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0183] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. This application has no specific restrictions on the type of electrolyte, and it can be selected according to needs.

[0184] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0185] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0186] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0187] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0188] In some embodiments, the electrode assembly further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0189] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0190] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0191] In some embodiments, the electrode assembly may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0192] In some embodiments, the outer packaging of the electrode assembly may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the electrode assembly may be a soft shell, such as a bag-type soft shell. The soft shell may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0193] The present application has no particular limitation on the shape of the electrode assembly, which may be cylindrical, square, or any other shape. For example, FIG3 shows a secondary battery 5 having a square structure as an example.

[0194] In some embodiments, referring to FIG4 , the outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the diaphragm can be formed into a secondary battery 52 through a winding process or a lamination process. The secondary battery 52 is encapsulated in the receiving cavity. The electrolyte is immersed in the secondary battery 52. ​​The number of secondary batteries 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0195] In some embodiments, the electrode assemblies may be assembled into a battery module. The number of electrode assemblies contained in the battery module may be one or more. The specific number may be selected by those skilled in the art based on the application and capacity of the battery module.

[0196] Figure 5 shows an example battery module 4. Referring to Figure 5 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0197] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0198] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0199] Figures 6 and 7 illustrate an example battery pack 1. Referring to Figures 6 and 7 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0200] In addition, the present application also provides an electrical device, which includes at least one of the electrode assembly, battery module, or battery pack provided in the present application. The electrode assembly, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0201] As an electrical device, an electrode assembly, battery module or battery pack can be selected according to its usage requirements.

[0202] Figure 8 shows an example of an electric device. This device can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the electrode assembly, a battery pack or battery module can be used.

[0203] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use an electrode assembly as a power source.

[0204] Example

[0205] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0206] Example 1

[0207] Preparation of acrylic copolymers

[0208] Preparation Example 1

[0209] (1) To a 500 ml three-necked flask, 150 g of deionized water and 3.6 g of sodium dodecylsulfonate were added, and the mixture was stirred for 15 min for emulsification. Then, 91.74 g of ethyl acrylate, 0.92 g of acrylonitrile, and 7.34 g of N-hydroxymethyl acrylamide were added in a mass ratio of 1:0.01:0.08, for a total of 100 g of monomers. The mixture was stirred for 60 min to obtain a pre-emulsion of the monomers, which was then taken out for later use.

[0210] (2) Add 100 ml of deionized water and 0.15 g of sodium dodecylbenzenesulfonate to a 500 ml three-necked flask, heat to 75 ° C, and emulsify at a speed of 2000 r / min for 15 min to fully emulsify the system. Then slowly dropwise add the pre-emulsion prepared in the step and the initiator solution (0.2 g of potassium persulfate as an initiator is dissolved in 30 g of deionized water to form a solution). After the addition is complete, heat to 90 ° C and keep warm for 0.5 h, then cool to 40 ° C; adjust the pH to 7 with ammonia water, stop stirring, filter, and discharge to obtain an acrylic copolymer emulsion. The volume particle size distribution Dv50 of the acrylic copolymer is 0.1 μm ± 0.01 μm (the volume particle size distribution Dv50 of the shell structure polymer in each embodiment is 0.1 μm ± 0.01 μm).

[0211] Preparation Example 2 to Preparation Example 10

[0212] On the basis of Preparation Example 1, the types and mass ratios of the monomers added were changed to obtain Preparation Examples 2 to 10.

[0213] Preparation of binder

[0214] Example 1

[0215] The acrylic copolymer emulsion (containing 100 g of acrylic copolymer) prepared in Preparation Example 1 was mixed with 100 g of polypropylene particles having a volume particle size distribution (Dv50) of 1 μm and dispersed at high speed for 60 minutes. After stirring, the mixture was spray-dried to obtain a core-shell adhesive. The spray-drying parameters were: inlet air temperature of 110°C and outlet air temperature of 50°C.

[0216] Examples 2 to 31

[0217] Based on Example 1, the polymer types and mass ratios of the core layer structure and the shell layer structure, the volume particle size distribution Dv50 of the core layer structure, and the volume particle size distribution Dv50 of the binder were adjusted to obtain Examples 2 to 31.

[0218] Comparative Example 1

[0219] On the basis of Example 1, the mass ratio of the shell structure to the core structure was adjusted to 1:0, that is, there was no core layer structure, to obtain Comparative Example 1.

[0220] Preparation of battery cells and batteries

[0221] 1. Preparation of Isolation Membrane

[0222] A commercially available PE microporous film with a thickness of 7 μm and an average pore size of 80 nm (from Zhuo Gao Electronic Technology Co., Ltd.) was used as the substrate. The binder prepared above was stirred and mixed uniformly in deionized water to obtain a slurry (solid content of 20%). The slurry was evenly coated on both surfaces of the substrate and dried to remove the solvent. The coating density of the coating composition on the substrate was 1.5 g / m 2 , and obtain an isolation film.

[0223] 2. Preparation of positive electrode sheet

[0224] Polyvinylidene fluoride (PVDF), lithium iron phosphate (LFP), conductive carbon black, and N-methylpyrrolidone (NMP) were mixed in a mass ratio of 1.2:58.38:0.42:40 and stirred thoroughly to prepare a positive electrode slurry. 2 The loading amount is evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed and cut to obtain the positive electrode sheet.

[0225] 3. Preparation of negative electrode sheet

[0226] Artificial graphite, conductive agent acetylene black, binder styrene butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na) were added into deionized water in a mass ratio of 96.2:1.0:1.6:1.2, and stirred thoroughly to prepare a negative electrode slurry (solid content of 63%). 2The loading amount is coated on the negative electrode current collector copper foil, and then dried, cold pressed and cut to obtain the negative electrode sheet.

[0227] 4. Preparation of Electrolyte

[0228] At 25°C, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a mixed solvent, and then LiPF6 is dissolved in the above mixed solvent to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.

[0229] 5. Preparation of Secondary Batteries

[0230] The positive electrode sheet, separator, and negative electrode sheet are stacked in sequence, wound, and cold-pressed (during which the separator is bonded to the electrode sheet) to obtain a battery cell; the battery cell is placed in an outer package, and the above-prepared electrolyte is added. After packaging, standing, formation, aging and other processes, a secondary battery is obtained.

[0231] Performance Testing

[0232] 1. Cold pressing bonding:

[0233] The battery negative electrode sheet and separator were stacked together and placed on a hot press. Pressing parameters were set at 25°C, 10t pressure, and 30s to produce a bonded separator / positive electrode sheet sample. The separator / negative electrode sheet sample was cut into 150mm x 20mm rectangular strips. The electrode sheet side of the strip was affixed to a steel plate using double-sided tape. At one end of the strip, the separator and electrode sheet were separated by 2cm along the length to produce the test specimen.

[0234] The steel plate was held horizontally and secured with the lower clamp of a universal testing machine (Xie Qiang Instrument Manufacturing (Shanghai) Co., Ltd., Model CTM2100). The peeled end of the separator, as described above, was secured with the upper clamp of the universal testing machine and connected to a tensile testing machine. The test conditions were set to a tensile rate of 20 mm / min and a horizontal pull of 10 cm. Once the tensile force stabilized, the tensile force was recorded. The ratio of the tensile force to the sample width was used to determine the adhesion strength between the separator and the electrode.

[0235] 2. Battery core hardness:

[0236] Place the battery cell on a table with both ends horizontal, fix the middle hollow part to be 12 cm wide, let the battery cell lie flat naturally, and measure the deviation of the center position of the battery cell from the horizontal reference line to evaluate the hardness of the battery cell.

[0237] 3. EIS data:

[0238] Using a Shanghai Chenhua CHI660D electrochemical workstation, a small-amplitude sinusoidal voltage signal with a frequency of W1 is applied to the battery system. The system generates a sinusoidal current response with a frequency of W2. The change in the ratio of the excitation voltage to the response current is the impedance spectrum of the electrochemical system. In the AC impedance test, the test frequency range is 10mHz to 100kHz, with an amplitude of 5mV. This test can obtain information such as the real and imaginary parts of the impedance at different frequencies.

[0239] 4. Cycle performance of lithium-ion batteries:

[0240] Using the LAND battery testing system, at 25°C, the prepared battery was charged at a constant current of 1 / 3C to 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C, left for 5 minutes, and then discharged at 1 / 3C to 2.5V. The resulting discharge capacity was recorded as the initial capacity C0. The above steps were repeated for the same battery, and the discharge capacity Cn of the battery after the 500th cycle was recorded at the same time. The battery capacity retention rate after each cycle, Pn, = (Cn / C0) × 100%. The battery capacity retention rate at a specific number of cycles can be used to reflect the difference in cycle performance.

[0241] Table 1 Preparation parameters of acrylic copolymer emulsion

[0242] Table 2 Binder preparation parameters

[0243] It can be seen from the above data that the application of an adhesive comprising a shell structure of an acrylic copolymer and a core structure of a rigid polymer in a battery improves the cold pressing bonding strength of the battery cell and increases the hardness of the battery cell, while helping to reduce the electrochemical impedance and improve the cycle performance of the secondary battery.

[0244] The above is only a preferred embodiment of the present application and does not limit the patent scope of the present application. All equivalent structural transformations made based on the contents of the present application specification and drawings, or direct / indirect application in other related technical fields, are included in the patent protection scope of the present application.

Claims

1. A binder for a secondary battery, wherein: The adhesive comprises a core layer structure and a shell layer structure arranged on the surface of the core layer structure, the shell layer structure comprises an acrylic copolymer, the core layer structure comprises a rigid polymer, and the crystallinity of the rigid polymer ranges from 32% to 94%.

2. The binder for secondary batteries according to claim 1, wherein The rigid polymer has a crystallinity value ranging from 40% to 80%.

3. The binder for secondary batteries according to claim 1 or 2, wherein The rigid polymer includes at least one of polyethylene, polypropylene, polystyrene, polymethyl methacrylate, and polyamide.

4. The secondary battery binder according to any one of claims 1 to 3, wherein The shape of the binder includes a spherical shape.

5. The secondary battery binder according to any one of claims 1 to 4, wherein The volume particle size distribution Dv50 of the binder is 1 μm to 15 μm. Preferably, the volume particle size distribution Dv50 of the binder is 1 μm to 12 μm.

6. The binder for secondary batteries according to any one of claims 1 to 5, wherein The ratio of the volume particle size distribution Dv50 of the acrylic copolymer to the volume particle size distribution Dv50 of the rigid polymer is 1:(1-50).

7. The binder for secondary batteries according to claim 6, wherein The volume particle size distribution Dv50 of the rigid polymer is 0.1 μm to 5 μm, preferably, the volume particle size distribution Dv50 of the rigid polymer is 0.5 μm to 2 μm; And / or, the volume particle size distribution Dv50 of the acrylic ester copolymer is 100 nm to 200 nm, preferably, the volume particle size distribution Dv50 of the acrylic ester copolymer is 130 nm to 180 nm.

8. The secondary battery binder according to any one of claims 1 to 7, wherein The ratio of the mass of the shell structure to the mass of the core structure is 1:(0.1-10). Preferably, the ratio of the mass of the shell structure to the mass of the core structure is 1:(0.1-5).

9. The binder for secondary batteries according to any one of claims 1 to 8, wherein The monomers constituting the acrylic ester copolymer include at least two of acrylic ester monomers, acrylonitrile monomers and acrylamide monomers.

10. The binder for secondary batteries according to claim 9, wherein The acrylic acid ester monomers include at least one of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate and 2-hydroxypropyl methacrylate; And / or, the acrylonitrile monomer includes at least one of acrylonitrile or methacrylonitrile; And / or, the acrylamide monomer includes at least one of acrylamide, N-hydroxymethyl acrylamide and N-butoxymethyl acrylamide.

11. The secondary battery binder according to any one of claims 1 to 10, wherein The constituent monomers of the acrylic ester copolymer include acrylic ester monomers, acrylonitrile monomers, and acrylamide monomers. The mass ratio of the acrylic ester monomers, the acrylonitrile monomers, and the acrylamide monomers is 1:(0.01-0.8):(0.01-0.15). Preferably, the mass ratio of the acrylic ester monomers, the acrylonitrile monomers, and the acrylamide monomers is 1:(0.1-0.6):(0.06-0.12).

12. A method for preparing a binder for a secondary battery according to any one of claims 1 to 11, wherein: include: preparing an acrylic copolymer emulsion; The acrylic copolymer emulsion is blended with a rigid polymer and spray-dried to obtain a core-shell structure adhesive.

13. The method for preparing a binder for a secondary battery according to claim 12, wherein: The steps of preparing the acrylic copolymer emulsion include: Stirring and emulsifying water, an emulsifier, and monomers constituting an acrylic copolymer to obtain a pre-emulsified solution of the monomers; The emulsifier and water are stirred and emulsified, and the pre-emulsion and initiator are added under heating conditions, and the temperature is increased to obtain an acrylic copolymer emulsion.

14. A diaphragm, wherein: The separator comprises a base film and a bonding layer provided on at least one side of the base film, wherein the bonding layer comprises the secondary battery binder according to any one of claims 1 to 11; Alternatively, the adhesive layer includes an adhesive prepared by the method for preparing an adhesive for a secondary battery as claimed in claim 12 or 13.

15. A secondary battery, wherein: The secondary battery includes the separator according to claim 14 .

16. An electrical device, wherein: The electric device comprises the secondary battery as claimed in claim 15 .

Citation Information

Patent Citations

  • Binder composition for lithium-ion secondary battery electrode

    CN107112540A

  • Fluoropolymer binder coating for use in electrochemical devices

    CN112055883A

  • Ion-conducting functional resin and lithium battery diaphragm containing ion-conducting functional resin

    CN113381125A

  • Core-shell resin material and preparation method thereof, water-based polymer coating, battery diaphragm and secondary battery

    CN114716696A

  • Core-shell structure polymer, preparation method and application thereof, positive electrode slurry, secondary battery, battery module, battery pack and electric device

    CN115117356A